Coil component, circuit board and method for manufacturing coil component

By bonding metal magnetic particles with varying surface resistances, the coil component addresses insulation and miniaturization challenges, facilitating high-density packaging and efficient insulation without additional insulating layers.

JP2024134992APending Publication Date: 2024-10-04TAIYO YUDEN KK

Patent Information

Application Number
JP2023045471
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Conventional coil components face challenges in achieving high-density packaging due to the need for thick insulating layers and adherence of insulating material to the bottom electrode, which impedes miniaturization and increases component spacing.

Method used

A coil component is formed by bonding metal magnetic particles with an insulating material, featuring varying surface resistances across different surfaces to ensure insulation without the need for additional insulating coats, allowing for high-density mounting.

Benefits of technology

The coil component achieves high-density packaging by optimizing surface resistances and electrode placement, enabling miniaturization and efficient insulation without expanding component size.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134992000001_ABST
    Figure 2024134992000001_ABST
Patent Text Reader

Abstract

To provide a coil component capable of high-density mounting.SOLUTION: A coil component according to an aspect comprises: a magnetic part comprising metallic magnetic particles bonded with an insulating material, and having first and second surfaces adjacent to each other as surfaces, the surface resistance of the second surface being higher than the surface resistance of the first surface; a conductor inside or on the surface of the magnetic part; and an external electrode provided on the first surface and connected to the conductor.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coil component, a circuit board, and a method for manufacturing a coil component. [Background technology]

[0002] Conventionally, mobile phones are known as a representative example of high-performance electronic devices. Electronic components used in mobile phones are required to be not only high-performance but also compact. Some electronic devices require an increased number of components, so high-density packaging is used to package components at a high density. To achieve high-density packaging, components must be miniaturized and the pitch between components must be narrowed.

[0003] In designing electronic components to accommodate narrower component pitches, a structure in which external electrodes are provided only on the mounting surface is often adopted, and technical studies on this structure have been conducted in the past. In addition, there is a technological trend to replace magnetic materials from ferrite with metallic magnetic materials to improve the performance of small coil components. The replacement of magnetic materials in coil components corresponds to the current load, and the replacement of materials changes the saturation characteristics with respect to the current, making it possible to reduce the size of coil components even with the same current load.

[0004] As the use of metallic magnetic materials in coil components increases, there is also a demand for improved productivity. For example, Patent Document 1 proposes a method of adopting part of the conventional lamination process to form a sheet shape and then cutting it to the component size, thereby improving both miniaturization and productivity. However, the coil component in Patent Document 1 requires the formation of external electrodes on the end faces, which are the cut surfaces, which hinders narrowing the pitch between components and ultimately hinders high-density mounting.

[0005] In response to this, for example, Patent Document 2 proposes a coil array component in which extraction electrodes are covered with an insulating layer on the end faces of the element body. Thus, conventionally, metallic magnetic materials have been used to meet the demands for high performance and miniaturization, while insulating layers have been used to meet the demands for narrower pitches. Combinations of these approaches have also been proposed. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2016-92422 A [Patent Document 2] JP 2020-17621 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, when an insulating layer is provided, the insulating layer needs to be sufficiently thick to ensure insulation, and it is necessary to prevent the insulating material from adhering to the electrodes on the bottom side. These factors restrict the miniaturization of electronic components and ultimately hinder high-density mounting. In view of the above circumstances, an object of the present invention is to provide a coil component that can be mounted at high density. [Means for solving the problem]

[0008] In order to solve the above problems, a coil component according to one embodiment of the present invention comprises a magnetic portion formed by bonding metal magnetic particles with an insulating material, having a first surface and a second surface adjacent to each other as surfaces, the surface resistance of the second surface being higher than the surface resistance of the first surface, a conductor portion provided inside or on the surface of the magnetic portion, and an external electrode provided on the first surface and connected to the conductor portion.

[0009] In addition, in a coil component according to one embodiment of the present invention, the magnetic portion has a third surface opposite to the second surface and adjacent to the first surface, and the surface resistance of the third surface is higher than the surface resistance of the first surface. Furthermore, in a coil component according to one embodiment of the present invention, the magnetic portion has a fourth surface and a fifth surface adjacent to both the first surface and the second surface, and the surface resistance of each of the fourth surface and the fifth surface is higher than the surface resistance of the first surface.

[0010] In addition, in the coil component according to an aspect of the present invention, the surface resistance of the third surface, the fourth surface, and the fifth surface has an error of 10% or less with respect to the surface resistance of the second surface. In addition, in a coil component according to an aspect of the present invention, the magnetic portion has a sixth surface opposite to the first surface, and the surface resistance of the sixth surface is higher than the surface resistance of the first surface.

[0011] In addition, in the coil component according to an aspect of the present invention, the error in the surface resistance of the third surface to the sixth surface is within 10% of the error in the surface resistance of the second surface. In addition, in a coil component according to an aspect of the present invention, the external electrodes are provided within an outer periphery of the first surface when viewed in a direction perpendicular to the first surface. In addition, in a coil component according to an aspect of the present invention, the external electrode is spaced apart from the second surface, the third surface, the fourth surface, and the fifth surface.

[0012] A circuit board according to an aspect of the present invention includes any one of the coil components described above, and a substrate on which the coil component is mounted. In addition, a manufacturing method for a coil component according to one embodiment of the present invention includes a molding step of obtaining a molded body having six molded surfaces using raw material particles of a metal magnetic material and an insulating binder that bonds the raw material particles, a processing step of processing at least one surface of the six molded bodies to remove the raw material particles and the binder to obtain a processed surface, and an electrode formation step of forming an external electrode on the processed surface by plating. Effect of the Invention

[0013] According to the present invention, a coil component that can be mounted at high density can be obtained. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a perspective view showing a coil component according to an embodiment of the present invention. [Diagram 2] 1 is a cross-sectional view showing a coil component according to an embodiment of the present invention. [Diagram 3] FIG. 2 is a bottom view showing the coil component according to the embodiment of the present invention. [Figure 4] 13A and 13B are diagrams illustrating other examples of the arrangement of external electrodes. [Diagram 5] 1A and 1B are diagrams illustrating an example of high-density mounting of coil components. [Figure 6] 1 is a flowchart showing an example of a manufacturing method of a coil component. [Figure 7] FIG. 2 is a diagram showing a schematic diagram of a microscopic structure of a molding surface. [Figure 8] FIG. 2 is a diagram showing a schematic diagram of a microscopic structure of a processed surface. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, the embodiments of the present invention will be described in detail with reference to the accompanying drawings. Note that the following embodiments do not limit the present invention, and not all of the combinations of features described in the embodiments are necessarily essential to the configuration of the present invention. The configuration of the embodiments may be appropriately modified or changed depending on the specifications of the device to which the present invention is applied and various conditions (such as usage conditions and usage environment).

[0016] The technical scope of the present invention is defined by the claims and is not limited by the following individual embodiments. The drawings used in the following description may differ in scale and shape from the actual structure in order to make each configuration easier to understand. The components shown in the drawings described above may be appropriately referenced in the description of the drawings that follow.

[0017] <Coil component structure> 1 to 3 are diagrams showing a coil component according to one embodiment of the present invention, in which FIG. 1 shows a perspective view, FIG. 2 shows a cross section taken along line AA in FIG. 1, and FIG. 3 shows a bottom view.

[0018] The coil component 1 is mounted on a substrate 2a. The substrate 2a is provided with, for example, two land portions 3. The coil component 1 has one magnetic base (magnetic portion) 11 and two external electrodes 12. The coil component 1 is mounted on the substrate 2a by joining each external electrode 12 and the land portion 3 with solder 4. When viewed in the H-axis direction, the area of ​​the land portion 3 is 1.6 times or less the area of ​​the external electrode 12. More preferably, when viewed in the H-axis direction, the area of ​​the land portion 3 is 1.3 times or less the area of ​​the external electrode 12.

[0019] A circuit board 2 according to an embodiment of the present invention includes a coil component 1 and a substrate 2a on which the coil component 1 is mounted. The circuit board 2 is included in various electronic devices. Examples of electronic devices that include the circuit board 2 include electrical equipment for automobiles, servers, board computers, and various other electronic devices.

[0020] The coil component 1 may be an inductor, a filter, a reactor, or any other of various coil components. The coil component 1 may be a coupled inductor, a transformer, a choke coil, or any other of various magnetically coupled coil components. The coil component 1 may be, for example, an inductor used in a DC / DC converter.

[0021] In this specification, unless otherwise understood in the context, the directions are described based on the "L axis" direction, the "W axis" direction, and the "H axis" direction in Figure 1, and are referred to as the "length" direction, the "width" direction, and the "height" direction, respectively. The coil component 1 has a rectangular parallelepiped outer shape. That is, the coil component 1 has end faces 1a and 1b at both ends in the length direction L, a top face 1c and a bottom face 1d at both ends in the height direction H, and a front face 1e and a rear face 1f at both ends in the width direction W. The bottom face 1d is a mounting face that faces the board 2a when the coil component 1 is mounted on the board 2a.

[0022] The dimensions of each side of the rectangular coil component 1 may be such that the maximum side in the outer dimensions is smaller than 5.0 mm, or smaller than 2.5 mm, or even smaller than 2.0 mm. The area of ​​the external electrodes of the coil component 1 may be smaller than 20% or even smaller than 10% of the surface area of ​​the coil component 1. The weight per unit volume of the coil component 1 is 0.6 g / mm 3 Greater than or equal to 0.65g / mm 3 Larger, even 0.70g / mm 3 The weight per unit area of ​​the external electrodes of the coil component 1 is 0.025 g / mm 2 Greater than or equal to 0.027g / cm 2 Larger, even 0.029g / cm 2 It could be larger.

[0023] The outer surfaces of the coil component 1 may be flat or curved, and the eight corners and 12 ridges of the coil component 1 may be rounded or chamfered. In this specification, even when the outer surface of the coil component 1 is partially curved or when the corners or ridges of the coil component 1 are rounded, such a shape may be referred to as a "rectangular parallelepiped shape." In other words, in this specification, the terms "rectangular parallelepiped" or "rectangular parallelepiped shape" do not mean a "rectangular parallelepiped" in the strict mathematical sense.

[0024] The coil component 1 in the first embodiment of the present invention has a magnetic base (magnetic portion) 11 and an external electrode 12, and has a coil conductor (conductor portion) 14 inside the magnetic base 11. The magnetic base 11 has six faces, and one of its external shapes is a rectangular parallelepiped shape, and the end faces 1a, 1b, top face 1c, bottom face 1d, front face 1e, and rear face 1f of the magnetic base 11 are substantially the end faces 1a, 1b, top face 1c, bottom face 1d, front face 1e, and rear face 1f of the coil component 1. As one example, the bottom face 1d is the first face, the end faces 1a, 1b are the second and third faces, the front face 1e, and rear face 1f are the fourth and fifth faces, and the top face 1c is the sixth face. The first face is adjacent to the second, third, fourth, and fifth faces, and is back-to-back with the sixth face. Adjacent means that the adjacent faces are perpendicular to each other, and back-to-back means that the faces face outward in opposite directions.

[0025] The magnetic base 11 in this embodiment is a magnetic body formed of a metal magnetic material and a binder. The binder bonds the metal magnetic material together and has high insulating properties to prevent electrical conduction. The binder is used to make the surface resistance of the magnetic base 11 10 5 A binder with a resistivity of 10 Ω / sq. or more is used. Since the metal magnetic material, which is mainly composed of Fe, has a low resistance, it is desirable to adjust the composition and mixing ratio of the binder to match the metal magnetic material. For example, a binder with a resistivity of 10 8 A material having a resistivity of Ωcm or more is selected, and in order to enhance the insulating properties, a resin is included as the binder, and glass or metal oxide can be selected as a component other than the resin.

[0026] The magnetic substrate 11 has a very high internal resistivity, and the same is true for the surface, where a binder is also present. The metal magnetic material is a metal magnetic particle containing one or more of Fe, Ni, and Co. In addition to the metal magnetic particles, the metal magnetic material may also contain ceramic magnetic particles of one or more of Mg, Mn, and Ni, or non-magnetic particles such as silica. The metal magnetic particles may contain one or more of Si, Cr, Al, B, and P in addition to the Fe, Ni, and Co components, and multiple types of metal magnetic particles may be combined.

[0027] The magnetic material has a particle size of 1 μm or more and 60 μm or less. When the metal magnetic material further contains other materials such as metal fine particles, metal oxides, and ceramic materials in addition to the metal magnetic particles, the particle size of the other materials is 0.01 to 1 μm on average, which is smaller than that of the metal magnetic particles. When materials other than the metal magnetic particles are contained, it is possible to, for example, reduce voids or compensate for mechanical strength rather than improving the magnetic function. The magnetic base 11 has a filling rate of the metal magnetic material of 80 vol % or more and 88 vol % or less, with the remainder being other than the metal magnetic material and including an insulator or voids.

[0028] The conductor 14 is made of a metal material with excellent electrical conductivity. For example, one or more of Cu, Al, Ni, and Ag, or an alloy containing any of these metals, may be used as the metal material for the coil conductor 14. The coil conductor 14 may be a wound metal conductor with an insulating film on its surface, or may be formed on the surface of a substrate, sheet, or the like by plating or printing.

[0029] The coil conductor 14 of this embodiment has a winding portion 41 that winds one or more times. The number of turns of the winding portion 41 is, for example, 1.5 turns or more and 10.5 turns or less. When the dimension of the coil component 1 in the length direction L is, for example, 1.0 to 2.5 mm, the number of turns of the winding portion 41 is, for example, 1.5 turns or more and 6.5 turns or less. The shape of the winding portion 41 may be planar or spiral. The winding portion 41 may be, for example, an assembly of two turns facing each other at the upper and lower sides. Furthermore, the coil conductor 14 may be linear or stepped without the winding portion 41.

[0030] The conductor 14 may be divided into a plurality of elements. A plurality of elements means that each element is insulated from the others and functions as a coil. Examples of the coil component 1 in which the conductor 14 is divided into a plurality of elements include an array type in which the elements are arranged in parallel, and a type in which the elements are magnetically coupled to each other. Specific examples of the coil component 1 in which the conductor 14 is divided into a plurality of elements include a transformer, a common mode choke coil, and a coupled inductor.

[0031] The coil conductor 14 has an extraction portion 42 for electrical conduction with the outside. The extraction portions 42 are provided on both ends of the winding portion 41, and connect the external electrodes 12 to the coil conductor 14. The coil conductor 14 can be manufactured by any of the processes of winding, thin film, and lamination, without any particular limitation.

[0032] 2 illustrates a so-called horizontally wound winding portion 41 that winds around the bottom surface 1d and the top surface 1c of the magnetic base 11. The coil conductor 14 may have a so-called vertically wound winding portion that winds around the end surfaces 1a and 1b of the magnetic base 11. The coil component 1 has a pair of external electrodes 12 on the bottom surface 1d, which corresponds to the first surface of the magnetic base 11. In this specification, "provided on the surface" and "provided on the surface" mean that the electrodes are present at locations that are visible when the surface is viewed, and may be provided to extend inward from the surface or to protrude outward. In addition, the case where the magnetic base 11 has a protrusion on its surface and the external electrodes 12 are provided to cover the protrusion also corresponds to "provided on the surface" and "provided on the surface".

[0033] The external electrode 12 is formed using a general metal material, and has a metal layer made of one or more metals selected from the group consisting of Ag, Cu, Ti, Ni, and Sn. The metal layer has a thickness of, for example, 0.01 to 5 μm. The external electrode 12 may also be formed by combining a plurality of metal layers, with a total thickness of 5 to 10 μm. The external electrode 12 may also be partially combined with a resin layer containing resin, with a total thickness of 10 to 20 μm.

[0034] The external electrodes 12 have an area that matches the outer dimensions of the coil component 1 or the outer circumferential dimensions of the bottom surface 1d, and have an area necessary for mounting on the substrate 2a. For example, the area ratio of the external electrodes 12 to the area of ​​the bottom surface 1d calculated from the outer dimensions of the coil component 1 is 50% or less. In this embodiment, a pair of external electrodes 12 are provided, and therefore the area of ​​one external electrode 12 is 25% or less of the area of ​​the bottom surface 1d.

[0035] The external electrode 12 is provided within the outer periphery of the bottom surface 1d, and does not protrude onto the end surfaces 1a, 1b, front surface 1e, or rear surface 1f. This prevents the external electrode 12 from increasing the outer dimensions of the coil component 1, making it possible to maximize the magnetic base 11. The external electrode 12 can be provided up to the same plane as the end surfaces 1a, 1b, front surface 1e, and rear surface 1f without affecting the outer dimensions of the coil component 1, making it possible to maximize the external electrode 12 on the bottom surface 1d.

[0036] In this embodiment, the external electrodes 12 are provided at positions away from the outer periphery of the bottom surface 1d. That is, the external electrodes 12 do not reach the end faces 1a, 1b, the front surface 1e, and the rear surface 1f. Due to the arrangement of the external electrodes 12 shown in Fig. 3, the solder 4 during mounting is contained within the outer periphery of the bottom surface 1d, and the area required for mounting the coil component 1 is small, which contributes to high-density mounting.

[0037] The arrangement of the external electrodes 12 is not limited to the arrangement shown in Fig. 3. The external electrodes 12 may be arranged, for example, as shown in Fig. 4. In the example shown in Fig. 4, the external electrodes 12 are arranged at a position where one end is flush with, for example, the end faces 1a and 1b. Even when the external electrodes 12 are arranged at the position shown in Fig. 4, the increase in the external dimensions of the coil component 1 due to the presence of the external electrodes 12 is suppressed, and the area required for mounting the coil component 1 is small, which contributes to high-density mounting.

[0038] FIG. 5 is a diagram showing an example of high-density mounting of the coil component 1. In FIG. The surface resistance of the magnetic base 11 is higher at the end faces 1a and 1b than at the bottom face 1d. The end faces 1a and 1b are adjacent to the bottom face 1d in the length direction L, and the pair of external electrodes 12 are arranged at an interval in the length direction L. In the length direction L, the distance between the external electrodes 12 and other electronic components is likely to be closer when mounted than in other directions. However, since the surface resistance of the end faces 1a and 1b adjacent to the bottom face 1d in the length direction L is higher, it is possible to reduce (i.e., narrow the pitch) the interval D1 between the coil components 1 or the interval D1 between the coil component 1 and other electronic components. In addition, the difference in surface resistance between the end faces 1a and 1b is within 10%. Therefore, it is not necessary to adjust the interval between the coil components 1 and other electronic components adjacent to each other in the length direction L.

[0039] Furthermore, the surface resistance of the magnetic base 11 is higher on the front surface 1e and rear surface 1f than on the bottom surface 1d. This allows the component intervals to be narrowed in the width direction W as well. The difference in surface resistance of the end surface 1b, front surface 1e, and rear surface 1f relative to the surface resistance of the end surface 1a is within 10%. This allows the component intervals to be narrowed regardless of the direction in which the component is adjacent to other electronic components, and also eliminates the need to adjust the component intervals depending on the direction in which the component is adjacent.

[0040] Furthermore, the surface resistance of the magnetic base 11 is higher on the top surface 1c than on the bottom surface 1d. Therefore, in a mounting form in which multiple substrates 2a are arranged in the height direction H, it is possible to reduce the distance D2 between the top surface 1c and other substrates 2a. In addition, the difference in surface resistance between the end surface 1b, the front surface 1e, the rear surface 1f, and the top surface 1c relative to the surface resistance of the end surface 1a is within 10%. Therefore, the pitch of the component intervals can be narrowed regardless of the direction in which the component is adjacent to other electronic components, and it is not necessary to adjust the component intervals depending on the direction in which the component is adjacent and the vertical direction. Since the magnetic base 11 or the coil component 1 can obtain insulation without being provided with an insulating coating, the coil component 1 can be made smaller, and high-density mounting can be achieved.

[0041] Next, a method for manufacturing the coil device 1 will be described. FIG. 6 is a flowchart showing an example of a method for manufacturing the coil device 1. In step S101, raw material particles forming a metal magnetic material and a binder forming an insulating material are mixed to prepare a composite material. In step S102, a conductor member that becomes the coil conductor 14 is formed. The conductor member may be formed, for example, by a conductive wire, or may be formed by printing or plating a conductor material. The conductor member is formed, for example, by processes such as winding, lamination, and thin film.

[0042] Step S103 is a molding process, in which a conductive member is placed in a metal mold, and a molded body integrated with the conductive member is obtained by, for example, filling the metal mold with a heated composite material, compressing it, and cooling it (molding). The metal mold may have a resin component present on a portion of its surface during the molding stage. This resin component is preferably a resin that does not soften at the heating temperature during molding. For example, a thermosetting resin component is selected as the resin component. The molded body obtained in step S103 corresponds to the magnetic base 11 in one coil component 1, and the molded body is, for example, a hexahedron.

[0043] FIG. 7 is a diagram showing a schematic diagram of the microscopic structure of the molding surface. FIG. 7 shows, as an example, a molding surface 50 corresponding to the end surface 1b. When the composite material is filled in the mold and compressed, it is compressed at a pressure lower than 10 MPa, for example. This keeps the amount of deformation of the raw material particles 54 small, and the change in the aspect ratio of the metal magnetic particles 51 obtained from the raw material particles 54 can be kept within a range of less than 10%.

[0044] During filling, the composite material is heated to a high temperature equal to or higher than the softening temperature of the binder 52, so that the binder 52 becomes easily movable, and after compression, the binder 52 is cooled to a temperature lower than the softening temperature of the binder 52, so that the binder 52 does not move, and the molded body 58 is obtained. That is, in the molding process, the binder 52 is made to exist on the surface of the raw material particles 54 by combining heating and cooling without relying on pressure as in the conventional method, and the molded body 58 can be taken out. As a result, the binder 52 is present evenly on the entire outer surface of the molded body 58, and the insulating material 56 formed from the binder 52 is also present evenly on the entire molding surface 50. Therefore, the surface area of ​​the raw material particles 54 exposed on the surface of the molded body 58 is small, and the number of exposed raw material particles 54 can be reduced. The surface resistance of this molding surface 50 is high, and the difference in surface resistance between the molding surfaces 50 is small. The surface resistivity of the molding surface 50 varies depending on the size and filling rate of the raw material particles 54, the resistivity of the binder, etc., but is generally within the range of 10 8 Ω / sq. or less. In other words, a compact 58 is obtained in which the surfaces of raw material particles 54 are covered with binder 52, and the magnetic base 11 obtained from such compact 58 has the surfaces of metal magnetic particles 51 covered with insulating material 56.

[0045] Returning to FIG. 6, the explanation will be continued. Step S104 is a processing step, in which one surface of the outer surface (i.e., molding surface 50) of molded body 58 on which external electrode 12 is provided is subjected to surface processing to expose lead-out portion 42 of coil conductor 14. In this surface processing, a process is performed to lower the resistance compared to the molding surface to the extent that the external electrode 12 can be formed. In the case where external electrode 12 is, for example, a two-surface electrode that reaches from bottom surface 1d to part of end surface 1b, surface processing is also performed on part of the surface corresponding to end surface 1b. However, the surface processing is limited to part of the surface corresponding to end surface 1b, and most of the surface corresponding to end surface 1b remains as the molding surface.

[0046] In step S104, the surface of the compact 58 may be treated by a method of removing the binder 52 from the surface of the compact 58, or may be treated by a method of removing the raw material particles 54. As a surface treatment method for removing the binder 52, a method may be used in which a laser, sandblasting, or the like is used to damage the binder 52, and the binder 52 is first removed, thereby removing the raw material particles 54. As a surface treatment method for removing the raw material particles 54, a method may be used in which a load is applied to the raw material particles 54 using polishing, and the raw material particles 54 is first removed, thereby removing the binder 52.

[0047] FIG. 8 is a diagram showing a schematic diagram of the microscopic structure of the processed surface. 8 shows an example of a machined surface 55 corresponding to the bottom surface 1d. The surfaces of the raw material particles 54 are also covered with the binder 52 on the machined surface 55, but the amount of the binder 52 has been reduced by the surface processing, and the surface resistance of the machined surface 55 is smaller than that of the molding surface 50. Note that Figures 7 and 8 show the molding surface 50 and the processed surface 55 of the molding 58, but the surfaces of the magnetic base 11 obtained from the molding 58 and the metal magnetic particles 51 obtained from the raw material particles 54 have a similar structure.

[0048] In the surface processing by the method of removing the binder 52, the surface resistance decreases due to damage to the binder 52, and the surface resistance of the processed surface 55 becomes smaller than the surface resistance of the molding surface 50. In the surface processing by the method of removing the raw material particles 54, the surface resistance decreases due to loss of the binder on the processed surface 55 and exposure of the metal surfaces of the raw material particles 54, and the surface resistance of the processed surface 55 becomes smaller than the surface resistance of the molding surface 50. The rate of decrease in surface resistance is greater in the surface processing by the method of removing the binder 52 than in the surface processing by the method of removing the raw material particles 54.

[0049] On the processed surface 55, some of the raw material particles 54 have been removed to form recesses 53, and therefore the surface roughness of the processed surface 55 is greater than that of the molding surface 50. Conversely, since the molding surface 50 has not been subjected to a surface treatment, the surface roughness of the molding surface 50 is less than that of the processed surface 55. This provides high handleability, such as transportation, on the molding surface 50, and also prevents the raw material particles 54 from falling off the molding surface 50. This is also true for the magnetic base 11, and makes it easier to maintain the state of the molding surface 50.

[0050] 6, a surface-processed molded body 58 is obtained, and in step S105, a base electrode made of a metal film is formed on the processed surface 55 by sputtering or vapor deposition as a part of the external electrode 12. The base electrode is formed in the formation range of the external electrode 12; for example, in the case of a one-surface electrode, it is formed only on the bottom surface 1d, or in the case of a two-surface electrode, it is formed from the bottom surface 1d to a part of the end surface 1b.

[0051] In step S106 of FIG. 6, an insulation treatment is performed to improve the insulation of the surface of the compact 58. For example, an acid treatment or a substitution treatment is used as the insulation treatment. In the acid treatment, the raw material particles 54 present on the surface of the compact 58 are selectively removed. In the substitution treatment, for example, a phosphoric acid treatment is used, and the metal surfaces of the raw material particles 54 present on the surface of the compact 58 are replaced with an insulator by substitution. In both the acid treatment and the substitution treatment, the external dimensions of the magnetic base 11 obtained from the compact 58 after the insulation treatment are not larger than the external dimensions of the compact 58. In addition, the external dimensions of the compact 58 after the insulation treatment are not larger than the external dimensions of the compact 58 before the insulation treatment. In particular, since the raw material particles 54 exposed on the surface of the compact 58 are subjected to the insulation treatment on the molding surface 50, the external dimensions do not change, and the external dimensions can be made smaller than when an insulator is provided on the entire molding surface 50.

[0052] As described above, the surface resistance of the molding surface 50 is greater than the surface resistance of the processing surface 55. If the insulation treatment in step S106 is not performed, the surface resistivity of the processing surface 55 is 10 5 Ω / sq. or more, and the surface resistivity of the insulated processed surface 55 is 10 6 Ω / sq. or more. When not insulated, the surface resistivity (rate) of molding surface 50 is 10 times or more the surface resistivity (rate) of machined surface 55, and when insulated, the surface resistivity (rate) of molding surface 50 is 2 times or more the surface resistivity (rate) of machined surface 55. Since there is more binder 52 on the surface of molding surface 50 than on machined surface 55, there is a difference in the effects of insulation treatment on molding surface 50 and machined surface 55, and the increase in surface resistivity of molding surface 50 is smaller than that of machined surface 55.

[0053] In step S107, as an example, an intermediate layer made of a conductive resin material is provided by printing or coating on the outside of the base electrode, and a metal layer is provided by electrolytic plating on the outside of the intermediate layer to form the external electrode 12. The external electrode 12 is formed within the range of the base electrode, and for example, in the case of a one-surface electrode, it is formed only on the bottom surface 1d, or in the case of a two-surface electrode, it is formed from the bottom surface 1d to a part of the end surface 1b. The coil component 1 is completed by forming the external electrodes 12.

[0054] 6, the molding process in step S103 results in a molded body 58 having a molding surface 50 with high surface resistance or a small difference in surface resistance between the molding surfaces 50, so that the surface processing in step S104 easily produces a processed surface 55 with a lower surface resistance than the molding surface 50. Therefore, a coil component 1 including a magnetic base 11 having a processed surface 55 with a lower surface resistance than the molding surface 50 can be easily obtained. [Explanation of symbols]

[0055] 1 Coil parts 1a, 1b end face 1c top surface 1d Bottom 1e front 1f rear 2 Circuit Board 2a board 3 Land Section 4 Solder 11 Magnetic base (magnetic part) 12 External electrode 14 Coil conductor (conductor part) 41 Orbital Division 42 Drawer section 50 Molding surface 51 Metal magnetic particles 52 Binding material 53 Recess 54 Raw material particles 55 Machining surface 56 Insulation Materials 58 Molded body

Claims

1. a magnetic portion formed by bonding metal magnetic particles with an insulating material, the magnetic portion having a first surface and a second surface adjacent to each other as surfaces, the surface resistance of the second surface being higher than the surface resistance of the first surface; A conductor portion provided inside or on a surface of the magnetic portion; an external electrode provided on the first surface and connected to the conductor portion; A coil component comprising:

2. The coil component according to claim 1, characterized in that the magnetic portion has a third surface opposite to the second surface and adjacent to the first surface, and the surface resistance of the third surface is higher than the surface resistance of the first surface.

3. 3. The coil component according to claim 2, wherein the magnetic portion has a fourth surface and a fifth surface adjacent to both the first surface and the second surface, and the surface resistance of each of the fourth surface and the fifth surface is higher than the surface resistance of the first surface.

4. 4. The coil component according to claim 3, wherein the surface resistances of the third surface, the fourth surface and the fifth surface have an error of 10% or less with respect to the surface resistance of the second surface.

5. The coil component according to claim 1 , wherein the magnetic portion has a sixth surface opposite to the first surface, and a surface resistance of the sixth surface is higher than a surface resistance of the first surface.

6. 6. The coil component according to claim 5, wherein the surface resistance of the third surface to the sixth surface has an error of 10% or less with respect to the surface resistance of the second surface.

7. The coil component according to claim 1 , wherein the external electrodes are provided within an outer periphery of the first surface when viewed in a direction perpendicular to the first surface.

8. The coil component according to claim 3 , wherein the external electrodes are spaced apart from the second surface, the third surface, the fourth surface, and the fifth surface.

9. A coil component according to any one of claims 1 to 8; a substrate on which the coil component is mounted.

10. a molding step of obtaining a green body having six molding surfaces by using raw material particles of a metal magnetic material and an insulating binder that bonds the raw material particles; a processing step of performing a process for removing the raw material particles and the binder from at least one of the six molding surfaces to obtain a processed surface; an electrode forming step of forming an external electrode on the processed surface by plating; A method for manufacturing a coil component comprising the steps of:

Citation Information

Patent Citations

  • Coil component assembly, coil component, and method of manufacturing the same

    JP2016092422A

  • Coil array component

    JP2020017621A

Cited By

  • Package board for image sensor and camera module including the same

    KR1020240145429A

  • Substrate for image sensor

    US12335589B2