Method for manufacturing resin-metal bonded body of polyetheretherketone carbon fiber reinforced resin and aluminum material

The method of hydrolyzing silane coupling agents and pressing polyetheretherketone resin against treated aluminum achieves strong bonding and molding, addressing bonding challenges and enabling complex shape formation.

JP2024135016APending Publication Date: 2024-10-04WASEDA UNIV
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023045504
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing methods struggle to achieve sufficient bonding strength between polyetheretherketone resin, which is chemically stable and has poor bonding properties, and aluminum materials without using bolts, rivets, or adhesives, while also addressing the issue of structural changes due to high molding temperatures.

Method used

A method involving hydrolyzing amino group- or isocyanate group-containing silane coupling agents, applying a silane coupling treatment to the aluminum surface, and pressing the polyetheretherketone resin against the treated aluminum at a temperature conducive to superplasticity, allowing direct bonding and molding.

Benefits of technology

This method enables strong bonding between polyetheretherketone resin and aluminum without additional joining members, leveraging superplastic properties for complex shape molding and improved strength, while maintaining recyclability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135016000007
    Figure 2024135016000007
  • Figure 2024135016000008
    Figure 2024135016000008
  • Figure 2024135016000009
    Figure 2024135016000009
Patent Text Reader

Abstract

To provide a method for manufacturing a resin-metal bonded body in which sufficient bonding strength can be obtained without using bolts, rivets, or other bonding materials or adhesives when joining a resin material using polyetheretherketone resin as the base material which has poor bonding properties because it is chemically very stable, and an aluminum material.SOLUTION: A method for manufacturing a resin-metal bonded body includes the processes of hydrolyzing a silane coupling agent containing amino or isocyanate groups to obtain a hydrolyzed product, performing a silane coupling treatment using the hydrolyzed product on the surface of the aluminum material, and joining the joint parts of the resin material having the polyetheretherketone as a base material, which has been heated to a molten state, and the joint part of the aluminum material, which has been subjected to the silane coupling treatment, by pressing the joint parts in a direction in which they approach each other.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a resin-metal bonded body between a polyether ether ketone carbon fiber reinforced resin and an aluminum material. [Background technology]

[0002] Carbon fiber reinforced plastic (CFRP) is known as a composite material of carbon fiber and resin. CFRP includes thermosetting CFRP, which uses a thermosetting resin as the matrix, and thermoplastic carbon fiber reinforced plastic (CFRTP), which uses a thermoplastic resin as the matrix.

[0003] These CFRPs are lightweight and strong, and are therefore widely used in parts for aircraft, automobiles, and other applications. In response to the recent demand for carbon neutrality, there is an increasing demand for CFRPs to replace metal materials in order to reduce the weight of mechanical structures. In particular, in the automotive field, there is a trend toward multi-materialization, where various materials are used in the right places, and the use of CFRTP, which uses thermoplastic resin as a base material, is expanding from the perspective of formability and recyclability. CFRTP has excellent storage and mass production properties, is easy to post-process, and is recyclable, making it inexpensive to manufacture.

[0004] When CFRP is used as a material for parts of aircraft, automobiles, etc., it is necessary to join it to other parts made of metal materials. For example, in aircraft, joining members such as bolts and rivets are often used to join CFRP parts to metal materials. However, joining using such joining members not only impedes the weight of the bolts and rivets themselves, which is a factor that hinders the weight reduction benefits of using CFRP, but also makes the bolt holes prone to becoming the starting point of damage, so in recent years there has been a demand for boltless joining of resins such as CFRP and metal materials.

[0005] The inventors have previously developed a technology that can firmly bond CFRTP to metal materials. In Patent Document 1, they propose a technology in which a nanostructure and chemical treatment are applied to the surface of a metal material, and the metal material is bonded to thermoplastic resins such as polyamide resins and composite materials thereof by thermal welding.

[0006] Polyether ether ketone resin (PEEK resin), one of the super engineering plastics, has advantages in that it has excellent heat resistance, the molded products are lightweight, and it can improve strength, sliding properties, etc. However, it is chemically very stable compared to other thermoplastic resins, so it has poor bonding properties. Silane coupling agents are known as a means of improving the bonding strength of the interface, but PEEK resin has poor reactivity because it is chemically very stable.

[0007] In addition, the molding temperature of PEEK resin is around 400°C, so there was an issue of structural changes due to heat in metal materials.

[0008] Non-Patent Document 1 proposes a technology for joining titanium alloys to PEEK composite materials by chemically treating the titanium alloys with aminosilane, but does not consider specific means for obtaining sufficient joining strength with aluminum alloys or means suitable for molding. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Patent No. 6809680

[0010] [Non-Patent Document 1] Chunming Ji et al., Effect of different preparation methods on mechanical behaviors of carbon fiber-reinforced PEEK-Titanium hybrid laminates, Polymer Testing, Volume 85, May 2020, 106462 Summary of the Invention [Problem to be solved by the invention]

[0011] The present invention has been made in consideration of the above-mentioned circumstances, and an object of the present invention is to provide a method for producing a resin-metal joined body that can obtain sufficient joining strength when joining an aluminum material to a resin material containing a polyether ether ketone resin as a base material, which is very chemically stable and therefore has poor joining properties, without using any joining members such as bolts or rivets or adhesives. [Means for solving the problem]

[0012] In order to solve the above problems, the present invention provides a method for producing a resin-metal bonded body, which is a method for producing a resin-metal bonded body between a resin material containing polyether ether ketone as a base material and an aluminum material, comprising the steps of: A step of hydrolyzing an amino group- or isocyanate group-containing silane coupling agent to obtain a hydrolysate of the amino group- or isocyanate group-containing silane coupling agent; A step of subjecting the surface of the aluminum material to a silane coupling treatment using the hydrolyzate; and A process of joining the joint parts of the resin material having the polyether ether ketone as a base material, which has been heated to a molten state, and the joint part of the aluminum material, which has been subjected to the silane coupling treatment, by pressing the joint parts in a direction in which they approach each other. The present invention is characterized in that it includes: In a preferred aspect of the method for producing a resin-metal bonded body, a polyether ether ketone resin film is interposed between a bonding portion of the resin material having polyether ether ketone as a base material and a bonding portion of the aluminum material subjected to the silane coupling treatment. In another preferred embodiment of the method for producing a resin-metal bonded body, the resin material containing polyether ether ketone as a base material is a carbon fiber reinforced resin, and a woven material is used as the carbon fibers of the carbon fiber reinforced resin. In another preferred embodiment of the method for producing a resin-metal bonded body, the pressing process is performed at a temperature at which the aluminum material exhibits superplastic properties using upper and lower dies having pressing surfaces corresponding to a desired shape of the resin-metal bonded body to be obtained, and the aluminum material is molded into the desired shape together with the resin material having polyether ether ketone as a base material. Effect of the Invention

[0013] According to the present invention, when joining an aluminum material to a resin material based on polyether ether ketone resin, which is very chemically stable and therefore has poor bonding properties, sufficient bonding strength can be obtained without using bonding members such as bolts or rivets or adhesives. In addition, by utilizing the fact that the joining temperature of resin materials based on polyether ether ketone resin is close to the temperature at which aluminum alloys exhibit their superplastic properties, the company is able to directly join the two and at the same time provide a molding processing technology that allows for large deformation. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a diagram showing an outline of the shape of a test piece used in Example 1. [Diagram 2] 1 is a photograph of a fracture surface after a tensile shear test in the case where aminosilane was used in Example 1. [Diagram 3] 4 is a photograph of the central portion of the fracture surface of (a) CFRTP and (b) Al after a tensile shear test in Example 1 when aminosilane was used, observed by FE-SEM. [Figure 4] FIG. 13 is a graph showing the relationship between the hydrolysis time of (a) aminosilane and (b) isocyanatesilane and the bond strength in Example 2. [Diagram 5] FIG. 13 is a graph showing the relationship between the passage of time and (a) the methanol concentration in an aqueous aminosilane solution and (b) the ethanol concentration in an aqueous isocyanatesilane solution in Example 2. [Figure 6] FIG. 13 is a graph showing the relationship between the hydrolysis time of isocyanate silane and the bonding strength in Example 6. [Figure 7] 13 is a photograph of the center of a fracture surface of Al after a tensile shear test in Example 6, observed by FE-SEM. [Figure 8] 13 is a graph showing the results of a tensile shear test of a joint between CFRTP and an aluminum alloy in Example 7. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, the embodiment of the present invention will be specifically described. The method for producing a resin-metal bonded body of the present invention is a method for producing a resin-metal bonded body between an aluminum material and a resin material containing polyether ether ketone as a base material, and includes the following steps (A) to (C). (A) A step of hydrolyzing an amino group- or isocyanate group-containing silane coupling agent to obtain a hydrolyzate of the amino group- or isocyanate group-containing silane coupling agent. (B) A step of subjecting the surface of the aluminum material to a silane coupling treatment using the hydrolyzate. (C) A process of joining the joint parts of the resin material having the polyether ether ketone as a base material, which has been molten by heating, and the joint part of the aluminum material which has been subjected to the silane coupling treatment, by pressing the joint parts in a direction in which they approach each other.

[0016] Examples of resin materials having polyether ether ketone as a base material include those using reinforcing materials such as fibers, such as carbon fiber reinforced resin and glass fiber reinforced resin, but they may also be polyether ether ketone alone without using any reinforcing materials. Of these, polyetheretherketone carbon fiber reinforced resin uses polyetheretherketone resin as the base material that encases the carbon fibers. Polyetheretherketone resin has a linear polymer structure in which benzene rings are bonded by ether and ketone, and is a crystalline plastic that has a high melting point of 334°C and excellent heat resistance, as well as excellent mechanical properties, making it one of the super engineering plastics.

[0017] Carbon fibers can be used without any particular restrictions, including those that have been conventionally used in CFRP, such as PAN-based fibers made from PAN (polyacrylonitrile) and pitch-based fibers made from pitch obtained from petroleum or coal. Also usable are UD materials in which carbon fibers are aligned in one direction, and woven materials woven warp and weft. Woven materials can be classified into plain weave, twill weave, satin weave, etc., depending on the weaving method.

[0018] Examples of the aluminum material include aluminum alloys containing aluminum as a main component, pure aluminum, and the like. The aluminum alloy is not particularly limited, and for example, A2024, A5052, and the like can be used. The shape of the aluminum material is not particularly limited, and may be an appropriate shape such as a plate material. An aluminum material as rolled can be used, but it may also be one that has been subjected to a surface treatment. The surface treatment is not particularly limited, and examples thereof include surface roughening treatments such as anodizing treatment, etching treatment, and surface treatments in combination thereof, laser processing treatment, polishing treatment, corona treatment, flame treatment, etc. Among these, anodizing treatment, etching treatment, and surface treatments in combination thereof, and laser processing treatment are preferred. Anodizing and etching can form a one-tiered (OT) structure, which is a single-layer spike-shaped surface nanostructure, or a multi-tiered (MT) structure, which is multi-layered and porous. In a surface treatment that combines anodizing and etching, for example, a degreased aluminum material is anodized in an acidic electrolyte to form a porous alumina layer, which is a porous oxide film, on the surface of the aluminum material, and then an etching process is performed to remove the porous alumina layer with numerous pores formed by the anodizing process. In the laser processing, a laser is applied to the surface of the aluminum material in a desired microstructure pattern, forming the microstructure in the form of, for example, a grid or groove.

[0019] Process (A) In step (A), the amino group- or isocyanate group-containing silane coupling agent achieves higher adhesive strength to the polyether ether ketone resin than conventional adhesives.

[0020] The amino group or isocyanate group-containing silane coupling agent is not particularly limited. Examples of amino group-containing silane coupling agents include N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, and N-phenyl-γ-aminopropyltrimethoxysilane. Examples of isocyanate group-containing silane coupling agents include 3-isocyanatepropyltriethoxysilane. The amino group-containing silane coupling agent may be reacted with isocyanate after hydrolysis.

[0021] Hydrolysis of the amino group- or isocyanate group-containing silane coupling agent can be carried out in an aqueous solution, and the concentration and time are appropriately set according to the type of silane coupling agent. The concentration depends on the type of silane coupling agent, but is, for example, about 1 to 10% by mass. The hydrolysis time is considered because hydrolysis tends to proceed quickly in amino group-containing silane coupling agents and slower in isocyanate group-containing silane coupling agents. As for the time, the hydrolysis proceeds and the bonding strength increases shortly after the hydrolysis time, but after that, when the dehydration condensation reaction between silanols proceeds, the number of reactions between the aluminum alloy and the silane coupling agent decreases due to the increase in hydrolysis. It is preferable to set the hydrolysis time as a guide so that the dehydration condensation reaction between silanols is reduced while silanols are generated by hydrolysis, and the number of dehydration condensation reactions between aluminum alloys and silane coupling agents is maximized.

[0022] Process (B) The silane coupling treatment on the surface of the aluminum material is carried out by contacting the aluminum material with a hydrolyzate of a silane coupling agent. For example, the aluminum material is immersed in an aqueous solution of a hydrolyzed silane coupling agent, and the silane coupling agent is attached to the surface of the aluminum material, followed by drying. Drying is preferably carried out at a temperature at which a dehydration condensation reaction occurs, and is carried out under appropriate conditions according to the type of silane coupling agent, for example, at about 100°C or higher.

[0023] Process (C) In step (C), the joining parts of the polyether ether ketone carbon fiber reinforced resin in a molten state by heating and the joining part of the aluminum material treated with silane coupling are pressed in a direction to approach each other, thereby joining the respective joining parts. Specific examples of the process of pressing while heating include hot pressing and blow molding. In the hot pressing process, the aluminum material to which the silane coupling agent is applied to the joining part is heated by a method such as placing it on a hot plate, the joining part of the resin is superimposed on the joining part to melt the resin, and the resin is cooled and solidified while pressing the resin toward the aluminum material, thereby joining the aluminum material and the resin. The temperature condition of the hot pressing process is set to a temperature equal to or higher than the glass transition temperature of the base resin and lower than a temperature at which the desired shape can be maintained. As an example, the pressing temperature is 390°C or higher, and the pressing pressure is 0.1 to 10 MPa.

[0024] The bonding strength can be increased by interposing a polyether ether ketone resin film between the bonding portion of the polyether ether ketone carbon fiber reinforced resin and the bonding portion of the silane coupling treated aluminum material. The thickness of the polyether ether ketone resin film is preferably about 0 to 200 μm.The molecular weight of polyether ether ketone is preferably low from the viewpoint of melt viscosity.

[0025] Furthermore, by using a woven material as the carbon fiber of the polyetheretherketone carbon fiber reinforced resin, the bonding strength can be increased. In this case, there is a tendency that sufficient strength can be obtained even without the interposition of a polyetheretherketone resin film.

[0026] The method for producing a resin-metal bonded body of the present invention can also be applied to molding. Using upper and lower dies having pressing surfaces corresponding to the desired shape of the resin-metal bonded body to be obtained, a pressing process is performed while heating the aluminum material at a temperature at which the aluminum material exhibits superplastic properties, for example, a hot press process, to mold the aluminum material together with a polyether ether ketone carbon fiber reinforced resin into the desired shape.

[0027] By taking advantage of the fact that aluminum alloys exhibit superplastic properties at a specific temperature, steps (A) to (C) above allow for strong dissimilar bonding with composite materials whose base material is the super engineering plastic PEEK resin, which has been difficult to bond up until now. Furthermore, by taking advantage of the fact that the bonding temperature is close to the temperature at which aluminum alloys exhibit their superplastic properties, it is possible to directly bond aluminum alloys and plastic-based composite materials while simultaneously performing molding processing that allows for large deformations. Despite being dissimilar materials, molding processing of complex shapes is possible, which not only reduces the number of parts, but also makes it possible to reduce the weight of aluminum alloys, improve their strength, and create coatings with excellent sliding properties.

[0028] Here, superplasticity is a phenomenon where a solid material shows huge plastic deformation under certain conditions, that is, when a solid is deformed at a certain strain rate in a high temperature range, it elongates by several hundred percent or more. There are two types of superplasticity: transformation superplasticity caused by phase transformation of the material, and fine-grained superplasticity that occurs in polycrystalline materials with grain sizes of a few micrometers or less. In fine-grained superplasticity, the strain rate sensitivity index (m value), which corresponds to the slope of the logarithmic strain rate-stress curve, is high, and the criterion for the occurrence of superplastic behavior is generally a m value of 0.3 or more and a fracture elongation of 200% or more. Aluminum alloys are one of the representative practical superplastic materials, and statically recrystallized aluminum alloys are known. When the superplastic phenomenon occurs, the flow stress also decreases, and a method of plastic processing such as forging that utilizes this phenomenon has been put into practical use for high-strength, difficult-to-process materials. The use of aluminum alloys in body panels is becoming more widespread with the aim of reducing the weight of automobiles, but the press formability of aluminum alloys is generally inferior to that of steel materials, and improving this has been a major challenge. One method of improving this is high-temperature forming, and when an alloy with a fine grain structure with crystal grains of several μm or less is deformed at high temperatures, a phenomenon called superplasticity appears, resulting in significantly improved formability.

[0029] According to the manufacturing method of the resin-metal bonded body of the present invention described above, it is possible to directly bond only CFRTP and metal, and it is possible to apply it to PEEK resin, which is difficult to bond while being highly recyclable, and it is also possible to realize bonding and molding at the same time. It is expected to be implemented and applied to parts where superplastic technology of aluminum alloys is applied, for example, it can be applied to aircraft parts, automobile parts, cryogenic tanks, etc. EXAMPLES

[0030] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the following description, polyether ether ketone and carbon fiber are sometimes abbreviated as PEEK and CF, respectively. The aluminum alloys used were A2024 and A5052. The composition (mass%) of the aluminum alloy A2024 was Si: 0.50, Fe: 0.50, Cu: 3.8-4.9, Mn: 0.30-0.9, Mg: 1.2-1.8, Cr: 0.10, Zn: 0.25, Ti: 0.15, and Al: Bal. The composition (mass%) of the aluminum alloy A5052 was Si: 0.25, Fe: 0.40, Cu: 0.10, Mn: 0.10, Mg: 2.2-2.8, Cr: 0.15-0.35, Zn: 0.10, Ti: 0.15, Al: 0.15, Other: 0.15, and Al: Bal. Before the silane coupling treatment, the aluminum alloy was appropriately cleaned and exposed to UV light to make the bonding surface hydrophilic.

[0031] <Example 1> The effect of silane coupling treatment on the bonding strength between aluminum alloy A2024 and CF / PEEK laminate (hereafter referred to as CFRTP) was evaluated.

[0032] CFRTP Specifications Matrix resin: PEEK resin Melting point: 343℃ Fiber volume ratio 58.6% Carbon Fiber Quasi-Isotropic Composite Laminates PEEK film specifications Shin-Etsu Sepla Film Thickness: 150μm

[0033] Silane Coupling Agent 1) Aminosilane N-2-(aminoethyl)-3-aminopropyltrimethoxysilane [ka] 2) Isocyanate silane 3-Isocyanatopropyltriethoxysilane [ka] 3) Aminophenyl + phenyl isocyanate In order to prevent thermal decomposition, the aluminum alloy pieces were immersed in a 1 mass% aqueous solution of hydrolyzed 3-aminophenyltrimethoxysilane at 60°C for 2 hours, then dried at 130°C for 60 minutes, and then immersed in a 25 mol / L aqueous solution of phenyl isocyanate for 24 hours to obtain aluminum alloy pieces treated with the following chemical structure. [ka]

[0034] Among the silane coupling agents, aminosilane was added to water to form a 10% by mass aqueous solution, and hydrolyzed for 20 minutes. Isocyanatesilane was added to water to form a 1% by mass aqueous solution, and hydrolyzed for 20 minutes.

[0035] The silane coupling treatment was carried out by immersing one side of the rectangular aluminum alloy piece in an aqueous solution of hydrolyzed silane coupling agent for 10 minutes, removing it, and drying it in an oven at 130° C. for 60 minutes.

[0036] The test specimen shape was prepared according to JIS K 6850. The aluminum alloy and CFRTP were laminated as shown in Figure 1 with a PEEK film (thickness 150 μm) inserted between the joining surfaces. The lower part of the hot press was heated to 390°C, and the upper part of the hot press, heated to 100°C, was pressurized at 6.27 MPa for 20 minutes. The specimens were then slowly cooled in the furnace while still under pressure to obtain test pieces.

[0037] The tensile shear test was carried out at 1 mm / min, and the bond strength was calculated using the following formula. Bonding strength [MPa] = breaking load [N] / bonding area [mm 2 ] Aminosilane, isocyanate silane, and aminophenyl + phenyl isocyanate were all used to bond PEEK-based CFRTP to aluminum alloy, and the bond strengths were 15.92 MPa, 3.13 MPa, and 2.81 MPa, respectively.

[0038] The fracture surface of a test piece that used aminosilane was observed after a tensile shear test (Figure 2). It was confirmed that some carbon fibers were attached to the test piece that used aminosilane. Figure 3 is a photograph of the center of the fracture surface of a test piece that used aminosilane, observed with an FE-SEM. Fractures were observed at the carbon fiber / resin interface and inside the resin, confirming strong chemical bonds. It is believed that the formation of covalent bonds with PEEK by amino groups affects strength expression.

[0039] <Example 2> The effect of the hydrolysis time of the silane coupling agent on the bond strength was evaluated. The CFRTP used the quasi-isotropic material in Example 1 as the carbon fiber, and the PEEK film in Example 1. The silane coupling agent used was (a) hydrolyzate of aminosilane (concentration 10% by mass, drying temperature after hydrolysis 130°C, drying time 60 minutes) or (b) hydrolyzate of isocyanatesilane (concentration 1% by mass, drying temperature after hydrolysis 130°C, drying time 60 minutes). The aluminum alloy used was A2024 in Example 1, and hot press processing was performed at a press pressure of 6.27 MPa, a bonding temperature of 390°C, and a bonding time of 20 minutes, followed by slow cooling in the furnace.

[0040] Figure 4 shows the relationship between the hydrolysis time and bond strength for (a) aminosilane and (b) isocyanatesilane. The hydrolysis time has a significant effect on bond strength, and while aminosilane hydrolyzes in a short time, isocyanatesilane takes time to hydrolyze and has an optimal treatment time.

[0041] The amount of methanol and ethanol produced in the aminosilane-isocyanate silane aqueous solution (1 mass%) was measured every 30 minutes using a gas chromatograph. Figure 5 shows the relationship between time and (a) the methanol concentration in the aminosilane aqueous solution and (b) the ethanol concentration in the isocyanate silane aqueous solution. Aminosilane is unstable and hydrolyzes quickly, whereas isocyanate silane is hydrolyzed slowly. This is consistent with the results in Figure 4.

[0042] <Example 3> The effect of drying temperature on the dehydration condensation of silane coupling agents was evaluated. The CFRTP used the quasi-isotropic material in Example 1 as the carbon fiber, and the PEEK film in Example 1. The silane coupling agent used was a hydrolyzate of aminosilane (concentration 10% by mass, hydrolysis time 20 minutes, drying temperature 100°C, 110°C, or 130°C, drying time 60 minutes). The aluminum alloy used was A2024 in Example 1, and hot press processing was performed at a press pressure of 6.27 MPa, a bonding temperature of 390°C, and a bonding time of 20 minutes, and then slowly cooled in a furnace. The bonding strength of the obtained test piece was measured and found to be 0 MPa (drying temperature 100°C), 2.59 MPa (drying temperature 110°C), and 15.1 MPa (drying temperature 130°C). It was suggested that a high temperature is necessary because the dehydration condensation reaction of aminosilane is difficult to occur.

[0043] <Example 4> The effect of the inserted PEEK film was evaluated. The CFRTP used the quasi-isotropic material in Example 1 as the carbon fiber, and the PEEK films used were (1) no film, (2) Shin-Etsu Sepla Film (thickness 3 μm), and (3) Shin-Etsu Sepla Film (thickness 150 μm). The silane coupling agent used was an aminosilane hydrolyzate (concentration 10 mass%, hydrolysis time 20 minutes, drying temperature 130 ° C, drying time 60 minutes). The aluminum alloy used was A2024 in Example 1, and hot press processing was performed at a press pressure of 6.27 MPa, a bonding temperature of 390 ° C, and a bonding time of 20 minutes, and then slowly cooled in a furnace. The bonding strength of the obtained test pieces was measured, and (1) was 1.73 MPa, (2) was 2.29 MPa, and (3) was 15.1 MPa. It was suggested that the bonding strength would be improved if there was a sufficient amount of resin on the bonding surface.

[0044] <Example 5> We investigated the types of CFRTP. For the CFRTP, a woven material (without a release agent) was used as the carbon fiber, and no PEEK film was used. The CFRTP and aluminum alloy were directly stacked together and hot-pressed. The silane coupling agent used was a hydrolyzate of isocyanate silane (concentration 1 mass%, hydrolysis time 90 minutes, drying temperature 130°C, drying time 60 minutes). Two types of aluminum alloys were used: (1) A2024 and (2) A5052. The hot-press process was performed with a press pressure of 6.27 MPa, a bonding temperature of 400°C, and a bonding time of 5 minutes, and the material was slowly cooled in a furnace. The bonding strength of the obtained test pieces was measured, and it was 15.43 MPa for (1) and 18.17 MPa for (2).

[0045] When a woven material was used as the carbon fiber, high bonding strength was achieved without the use of a PEEK film. The surface of the woven CFRTP was covered with a slightly thick layer of PEEK resin of several microns. It was suggested that the pseudo-isotropic CFRTP in Example 1 had little PEEK resin on the surface, so it was necessary to use a PEEK film to obtain bonding strength. The aluminum alloy was applicable to A5052 as well as A2024.

[0046] <Example 6> The CFRTP used a woven material (without a release agent) as the carbon fiber, and no PEEK film was used. The CFRTP and aluminum alloy were directly stacked together and hot-pressed. The silane coupling agent used was a hydrolyzate of isocyanate silane (concentration 1 mass%, drying temperature after hydrolysis 100°C, drying time 60 minutes). The aluminum alloy used was A5052. The hot-press process was performed with a press pressure of 6 MPa, a bonding temperature of 400°C, and a bonding time of 5 minutes, and then slowly cooled in the furnace. Figure 6 shows the relationship between the hydrolysis time of isocyanate silane and the bond strength. The hydrolysis time was 10 to 130 minutes. With a hydrolysis time of 10 minutes, the maximum bond strength was 17.7 MPa. As the hydrolysis progressed, the bond strength decreased, but increased again at 130 minutes.

[0047] The fracture surface of the test piece using isocyanate was observed after the tensile shear test. Figure 7 shows a photograph of the center of the fracture surface of the test piece using isocyanate after 10 minutes of hydrolysis, observed by FE-SEM. For each hydrolysis time, the observation of the fracture surface confirmed that the higher the bonding strength, the more PEEK resin adhered to the aluminum alloy surface, and cohesive failure occurred at the interface. Although not shown in the figure, the results of FTIR measurements showed that the number of isocyanate functional groups first decreased and then increased over time. It also showed that the number of hydroxyl groups due to hydrolysis first increased and then decreased. It is believed that as the added water decomposes, a dehydration condensation reaction occurs between the silane coupling agent molecules, forming a dimer. It is believed that the decrease in isocyanate groups reduces the number of reactions with the PEEK resin, resulting in a decrease in the initial adhesive strength. The results of NMR measurements suggest that the number of dimer molecules formed by dehydration condensation of the silane coupling agent molecules gradually increases from the time of hydrolysis.

[0048] <Example 7> The effect of laser processing on the aluminum alloy surface on bonding strength was evaluated. Laser processing was performed on the bonding surface of aluminum alloy A5052. Two types of lattice structures with grid widths of 30 μm and 100 μm were formed by laser processing using computer-aided design software with a scan speed of 100 mm / s, output of 5 W, frequency of 100 kHz, and 20 processing times. The surface shape after processing was confirmed by a laser confocal microscope. For the CFRTP, a woven material (without a release agent) was used as the carbon fiber. When a PEEK film was used, it was placed between the CFRTP and the aluminum alloy, and when a PEEK film was not used, the CFRTP and the aluminum alloy were directly stacked on top of each other and hot pressed. The silane coupling agent used was an aminosilane hydrolysate (concentration 10% by mass, hydrolysis time 10 minutes, drying temperature after hydrolysis 130°C, drying time 60 minutes). Hot pressing was performed at a pressure of 6 MPa and a bonding temperature of 400°C, and the material was slowly cooled in the furnace.

[0049] The results are shown in Figure 8. The test pieces in Figure 8 are as follows, from the left: No silane coupling treatment Laser processing of aluminum alloy: Grid width 30μm PEEK film used No silane coupling treatment Laser processing of aluminum alloy: Grid width 100μm PEEK film used - Silane coupling treatment applied Laser processing on aluminum alloy: No PEEK film used -Silane coupling treatment applied Laser processing of aluminum alloy: Grid width 30μm PEEK film used -Silane coupling treatment applied Laser processing of aluminum alloy: Grid width 100μm PEEK film used -Silane coupling treatment applied Laser processing on aluminum alloy: Grid width 30μm No PEEK film

[0050] Compared to silane coupling treatment alone, the bonding strength increased by 28% to 78% for laser processing of aluminum alloy with a grid width of 30 μm and by 78% to 97% for laser processing of aluminum alloy with a grid width of 100 μm. Compared to laser processing only the microstructure created by laser processing, silane coupling treatment increased the bonding strength by 85% to 158% for laser processing of aluminum alloy with a grid width of 30 μm and by 41% to 55% for laser processing of aluminum alloy with a grid width of 100 μm. An improvement in bonding strength was observed by combining the interfacial microstructure created by laser processing with silane coupling treatment. An improvement in bonding strength was observed by sandwiching a PEEK film. It was suggested that the shape of the interfacial microstructure changes the structural surface area and structural width / depth, which affect the silane coupling effect and anchor effect, respectively.

[0051] <Example 8> The effect of the microstructure of the aluminum alloy surface on the interlaminar fracture toughness was evaluated. The aluminum alloy A5052 was used, and its joining surface was subjected to laser processing in the same manner as in Example 7 to form a groove structure consisting of straight lines with a width of 10 μm. The surface shape after processing was confirmed by a laser confocal microscope. In addition, aluminum alloy A5052 was used, and the bonding surfaces were subjected to anodizing and etching under the conditions shown in Table 1.

[0052] [Table 1]

[0053] For the CFRTP, a woven material (without a release agent) was used as the carbon fiber. When a PEEK film was used, it was placed between the CFRTP and the aluminum alloy, and when a PEEK film was not used, the CFRTP and the aluminum alloy were directly stacked on top of each other and hot pressed. The silane coupling agent used was an aminosilane hydrolysate (concentration 10% by mass, hydrolysis time 10 minutes, drying temperature after hydrolysis 130°C, drying time 60 minutes). Hot pressing was performed at a pressure of 7 MPa and a bonding temperature of 390°C, and the material was slowly cooled in the furnace.

[0054] The bonding conditions for each test piece were as follows: Si-AR No surface structure No PEEK film Silane coupling treatment Si-Laser Laser processing PEEK film available Silane coupling treatment available Si-MT Anodizing and etching treatment No PEEK film Silane coupling treatment

[0055] A DCB (Double Cantilever Beam) static tensile test was performed on each specimen. A pre-crack was introduced by static tension at a static load of 0.5 mm / min, and after multiple crack propagations, the constants α0 and α1 were obtained from the following equation. [ka]

[0056] Static fracture toughness G C was calculated from the following formula: [ka]

[0057] Static fracture toughness G C , Si-AR is 0.3212 kJ / m 2 , Si-Laser is 1.2221kJ / m 2 , Si-MT is 1.8742 kJ / m 2 In the thermal welding with CF / PEEK, the effect of the structure imparted to the A5052 surface on the interlaminar fracture toughness value was 3.8 times that of a test piece with no structure for the groove structure created by laser processing, and 5.8 times that of a test piece with no structure for the nanostructure created by anodizing and etching.

Claims

1. A method for producing a resin-metal joined body between a resin material having a polyether ether ketone base material and an aluminum material, comprising the steps of: A step of hydrolyzing an amino group- or isocyanate group-containing silane coupling agent to obtain a hydrolysate of the amino group- or isocyanate group-containing silane coupling agent; A step of subjecting the surface of the aluminum material to a silane coupling treatment using the hydrolyzate; and A process of joining the joint parts of the resin material having the polyether ether ketone as a base material, which has been heated to a molten state, and the joint part of the aluminum material, which has been subjected to the silane coupling treatment, by pressing the joint parts in a direction in which they approach each other. The method for producing a resin-metal bonded body comprising the steps of:

2. 2. The method for producing a resin-metal joined body according to claim 1, further comprising the step of: interposing a polyether ether ketone resin film between a joining portion of the resin material having a polyether ether ketone base material and a joining portion of the aluminum material subjected to the silane coupling treatment.

3. 2. The method for producing a resin-metal joined body according to claim 1, wherein the resin material containing polyether ether ketone as a base material is a carbon fiber reinforced resin, and a woven material is used as the carbon fibers of the carbon fiber reinforced resin.

4. 3. The method for producing a resin-metal joined body according to claim 1, wherein the pressing process is performed at a temperature at which the aluminum material exhibits superplastic properties using upper and lower dies having pressing surfaces corresponding to a desired shape of the resin-metal joined body to be obtained, and the aluminum material is molded into the desired shape together with the resin material having polyether ether ketone as a base material.

Citation Information

Patent Citations

  • Laminate, methods for its manufacture and its use

    DE102011082697A1

  • Method of manufacturing connector of carbon fiber composite material

    JP2012187861A

  • Aluminum-resin composite, aluminum insulated wire, flat cable and method for producing them

    JP2014218050A

  • Silicon-containing aluminium alloy resin composite material and manufacturing method therefor

    JP2018171749A

  • Manufacturing method of resin-metal joined body and resin-metal joined body

    JP2019166638A