Resin composition, semiconductor device, and circuit board with heat sink

A resin composition with controlled epoxy resin, curing agent, and inorganic filler content and size improves polishability, addressing polishability issues in pre-molding resin compositions, enhancing semiconductor device manufacturing efficiency and reliability.

JP2024135038AInactive Publication Date: 2024-10-04SUMITOMO BAKELITE CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023045530
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The polishability of pre-molding resin compositions used in power semiconductor modules decreases when unnecessary resin is removed by polishing, leading to damage to polishing tools and uneven surfaces.

Method used

A resin composition comprising an epoxy resin, a curing agent, and an inorganic filler, with specific content ratios and particle sizes, is used to improve polishability and surface flatness, ensuring the top surfaces of circuit patterns and sealing bodies are flush.

Benefits of technology

The resin composition enhances polishability, reduces tool damage, and improves adhesion and filling properties, resulting in higher productivity and reliability of semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135038000001_ABST
    Figure 2024135038000001_ABST
Patent Text Reader

Abstract

To provide a resin composition for pre-molding which can improve polishing property.SOLUTION: A resin composition for pre-molding contains an epoxy resin, a curing agent (B), and an inorganic filler (C), wherein the content of the inorganic filler (C) is 50 mass% or more and 75 mass% or less with respect to the total amount of the resin composition.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition, a semiconductor device, and a circuit board with a heat sink. More specifically, the present invention relates to a resin composition, a semiconductor device and a method for producing the same, a circuit board with a heat sink, and a method for producing the same. [Background technology]

[0002] The market for power modules, which have power semiconductor elements mounted on a metal circuit board, is expanding. It is known that a lead frame having a plurality of independent patterns is used as the electrical wiring for such power modules in order to meet the demand for high density wiring.

[0003] Patent Document 1 discloses a lead frame having a plurality of independent patterns and a resin bonding material that fills the gaps between adjacent patterns and connects the adjacent patterns. Patent Document 1 discloses that after filling and curing the resin bonding material, if any resin bonding material remains on the upper surface of the lead frame, it is removed by a known means such as buff polishing. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2009 / 110376 Summary of the Invention [Problem to be solved by the invention]

[0005] The present inventors have noticed that when a premolding resin as disclosed in Patent Document 1 is used, after the premolding resin is filled and cured, when unnecessary resin is polished away, there is a problem that polishing ability decreases and a polishing tool is damaged. [Means for solving the problem]

[0006] As a result of intensive research aimed at solving the above problems, the present inventors discovered that it is effective to control the blending of the resin components and inorganic filler used in the resin composition used in premold molding, and thus completed the present invention.

[0007] According to the present invention, there are provided the following resin composition for premold molding, a semiconductor device and a method for producing the same, a circuit board with a heat sink and a method for producing the same.

[0008] [1] A resin composition comprising an epoxy resin (A), a curing agent (B), and an inorganic filler (C), A resin composition for premold molding, wherein the content of the inorganic filler (C) is 50% by mass or more and 75% by mass or less based on the total amount of the resin composition. [2] The resin composition according to [1], A resin composition, wherein D90 is a particle diameter corresponding to a cumulative 90% of the particle diameter in a volume-based integrated fraction of the inorganic filler (C) measured by a laser diffraction scattering method, and D90 is 5.0 to 80 μm. [3] The resin composition according to [1] or [2], The resin composition, wherein the inorganic filler (C) is one or more selected from the group consisting of fused silica, spherical silica, crystalline silica, alumina, silicon nitride and aluminum nitride. [4] The resin composition according to any one of [1] to [3], A resin composition having a flexural modulus of 12,000 MPa or less, as measured by the following procedure. Procedure: The resin composition is cured at 175° C. and 9.8 MPa, and the flexural strength of the resulting test piece is measured at 25° C. in accordance with JIS K-6911. [5] The resin composition according to any one of [1] to [4], A resin composition, wherein an equivalent ratio, which is a ratio of an epoxy equivalent of the epoxy resin (A) to an active hydroxyl group equivalent of the curing agent (B), is 1.4 or more and 2.0 or less. [6] An insulating layer provided on one surface of the heat sink; A circuit pattern provided on the insulating layer; a first sealing body embedded between the circuit patterns; A heat sink-equipped circuit board comprising: The first sealing body is a premolded product made of the resin composition according to any one of [1] to [5]. [7] In the circuit board with a heat sink according to [6], an upper surface of the circuit pattern and an upper surface of the first sealing body are substantially flush with each other; [8] In the circuit board with a heat sink according to [6] or [7], The circuit board with a heat sink, wherein the surface roughness Ra of the upper surface of the first sealing body is 0.7 μm or less. [9] A circuit board with a heat sink according to any one of [6] to [8], a semiconductor chip mounted on the circuit board with a heat sink; A second sealing body that covers the semiconductor chip; Equipped with The semiconductor device has an interface between the first encapsulant and the second encapsulant.

[10] The semiconductor device according to [9], The semiconductor device, wherein the first sealing body and the second sealing body are formed from different resin materials.

[11] depositing an insulating layer on one side of the heat sink; disposing a lead frame having a plurality of independent circuit patterns on the insulating layer; [1] to [5], a step of embedding the resin composition according to any one of the above between the circuit patterns; removing a portion of the resin composition and the convex bridge to expose an upper surface of the circuit pattern; A method for manufacturing a circuit board with a heat sink, comprising:

[12] A method for producing a circuit board with a heat sink according to

[11] , comprising the steps of: After the step of exposing the top surface of the circuit pattern, The method for manufacturing a circuit board with a heat sink further comprises a step of applying an antioxidant to the exposed circuit pattern.

[13] A method for producing a circuit board with a heat sink according to

[11] or

[12] , comprising the steps of: A method for manufacturing a circuit board with a heat sink, wherein the lead frame has a convex bridge arranged to span between adjacent circuit patterns.

[14] A method for producing a circuit board with a heat sink according to any one of

[11] to

[13] , comprising the steps of: A method for manufacturing a circuit board with a heat sink, wherein the step of exposing the upper surface of the circuit pattern is performed by polishing or cutting.

[15] A method for manufacturing a semiconductor device using a circuit board with a heat sink obtained by the method for manufacturing a circuit board with a heat sink according to any one of

[11] to

[14] , comprising the steps of: mounting a semiconductor chip on the exposed top surface of the circuit pattern; encapsulating the semiconductor chip with a second resin composition; A method for manufacturing a semiconductor device comprising the steps of: Effect of the Invention

[0009] According to the present invention, there can be provided a resin composition for premold molding capable of improving polishability, a semiconductor device using the same and a method for producing the same, and a circuit board with a heat sink and a method for producing the same. [Brief description of the drawings]

[0010] [Figure 1] 5A to 5C are cross-sectional views each showing a schematic process of a method for manufacturing a circuit board with a heat sink according to an embodiment. [Diagram 2] 1 is a cross-sectional view showing a schematic diagram of a lead frame used in a circuit board with a heat sink according to an embodiment. [Diagram 3] 1 is a cross-sectional view that illustrates a semiconductor device that uses a circuit board with a heat sink according to an embodiment. [Figure 4]11 is a cross-sectional view showing a schematic diagram of a modified example of a circuit board with a heat sink according to an embodiment. FIG. [Diagram 5] 11 is a cross-sectional view showing a schematic diagram of a modified example of a semiconductor device using a circuit board with a heat sink according to an embodiment. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. In all drawings, the same components are denoted by the same reference numerals, and the description thereof will be omitted as appropriate. Note that the drawings are for explanatory purposes only. The shapes and dimensional ratios of the components in the drawings do not necessarily correspond to the actual products.

[0012] In this specification, the expression "a to b" in the explanation of a numerical range means from a to b, unless otherwise specified. For example, "1 to 5% by mass" means "1% by mass to 5% by mass."

[0013] <Premolding resin composition> The resin composition for premold molding of this embodiment (hereinafter also referred to as "resin composition (P1)") contains an epoxy resin (A), a curing agent (B), and an inorganic filler (C), and the content of the inorganic filler (C) is 50 mass% or more and 75 mass% or less with respect to the total amount of the resin composition (P1). This allows for good polishing after filling and curing using the resin composition (P1) of this embodiment. That is, when unnecessary resin is polished away after filling and curing the premolding resin, it is possible to reduce the occurrence of a decrease in polishing power and damage to the polishing tool. In addition, by reducing the unevenness of the polishing surface and making it flatter, it is possible to prevent gaps from occurring at the interface with the premolding surface during overmolding, and to improve adhesion and filling properties.

[0014] [Application] The term "for premolding" refers to a use in which a molded product is obtained by using the resin composition (P1) of this embodiment, and then another resin composition is used to perform overmolding to obtain a final product. By improving the polishability of the premolded product, the productivity of the final product can be improved, and the adhesion between the premolded product and the overmolded product can be improved. For example, in order to obtain a semiconductor device, the resin composition (P1) is filled between the circuits of a lead frame, and the lead frame is further encapsulated using another resin composition to obtain a semiconductor device. As described later, the resin composition (P1) of this embodiment is suitable for use in pre-molding to obtain a circuit board with a heat sink and a semiconductor device using the same.

[0015] [Flexural modulus] The resin composition (P1) preferably has a flexural modulus of 12000 MPa or less, more preferably 10000 MPa or less, as measured by the following procedure. By making the flexural modulus equal to or less than the above upper limit, polishability is improved and flatness is easily improved.

[0016] Procedure: The resin composition (P1) is cured at 175° C. and 9.8 MPa to obtain a test piece, and the bending strength at 25° C. is measured in accordance with JIS K-6911.

[0017] On the other hand, the lower limit of the flexural modulus is not particularly limited, but is preferably 500 MPa or more in order to maintain good moldability.

[0018] [Loss tangent (tanδ)] Furthermore, for a test piece obtained by curing resin composition (P1) at 175°C and 9.8 MPa, the maximum value of loss tangent (tan δ) determined by dynamic viscoelasticity measurement in the range of 30 to 350°C under conditions of a heating rate of 5°C / min, a frequency of 10 Hz, and a load of 800 g is preferably 0.30 or more, more preferably 0.40 or more, and even more preferably 0.50 or more. That is, the cured product of the resin composition (P1) can convert much of the mechanical energy into thermal energy and can absorb a lot of energy, so that it has an appropriate hardness against the load during polishing, improves polishability, and makes it easier to achieve good flatness.

[0019] The components constituting the resin composition (P1) of this embodiment will be described below.

[0020] [Epoxy resin (A)] As the epoxy resin (A), a known epoxy resin used in an encapsulating epoxy resin composition can be used.

[0021] Specific examples of the epoxy resin (A) include crystalline epoxy resins such as biphenyl-type epoxy resins, bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, and tetramethylbisphenol F-type epoxy resins, stilbene-type epoxy resins, and hydroquinone-type epoxy resins; novolac-type epoxy resins such as cresol novolac-type epoxy resins, phenol novolac-type epoxy resins, and naphthol novolac-type epoxy resins; aralkyl-type epoxy resins such as phenylene-skeleton-containing phenol aralkyl-type epoxy resins, biphenylene-skeleton-containing phenol aralkyl-type epoxy resins, phenylene-skeleton-containing naphthol aralkyl-type epoxy resins, and alkoxynaphthalene-skeleton-containing phenol aralkyl-type epoxy resins; trifunctional epoxy resins such as triphenol methane-type epoxy resins and alkyl-modified triphenol methane-type epoxy resins; modified phenol-type epoxy resins such as dicyclopentadiene-modified phenol-type epoxy resins and terpene-modified phenol-type epoxy resins; and heterocyclic-containing epoxy resins such as triazine-nucleus-containing epoxy resins. These may be used alone or in combination of two or more.

[0022] The content of the epoxy resin (A) is preferably 5 mass% or more, more preferably 8 mass% or more, even more preferably 10 mass% or more, and particularly preferably 15 mass% or more, based on the total amount of the resin composition (P1), in order to obtain good fluidity, filling property, and adhesion. On the other hand, the content of the epoxy resin (A) is preferably 30 mass% or less, more preferably 25 mass% or less, and even more preferably 20 mass% or less, based on the total amount of the resin composition (P1), from the viewpoint of improving high-temperature reliability and reflow resistance.

[0023] The epoxy equivalent weight of the total epoxy resin (A) is preferably 100 g / eq or more, more preferably 180 g / eq or more, and further preferably 200 g / eq or more. On the other hand, the epoxy equivalent weight of the total epoxy resin (A) is preferably 500 g / eq or less, more preferably 480 g / eq or less, and further preferably 450 g / eq or less.

[0024] [Hardening agent (B)] As the curing agent (B), a known curing agent used in an encapsulating epoxy resin composition can be used. Specific examples of the curing agent (B) include phenol-based curing agents and amine-based curing agents (curing agents having an amino group).

[0025] Examples of the phenol-based curing agent include novolak-type phenolic resins obtained by condensing or co-condensing phenols such as phenol, cresol, resorcin, catechol, bisphenol A, bisphenol F, phenylphenol, and aminophenol, and / or naphthols such as α-naphthol, β-naphthol, and dihydroxynaphthalene, with compounds having an aldehyde group such as formaldehyde, benzaldehyde, and salicylaldehyde, under an acidic catalyst; polyfunctional phenolic resins such as triphenylmethane-type phenolic resins and biphenylene skeleton-containing polyfunctional phenolic resins; phenol aralkyl-type phenolic resins such as biphenylene skeleton-containing polyfunctional phenolic resins synthesized from phenols and / or naphthols and dimethoxyparaxylene or bis(methoxymethyl)biphenyl; dicyclopentadiene-type phenolic resins, and terpene-modified phenolic resins.

[0026] Examples of the amine curing agent include linear aliphatic diamines having 2 to 20 carbon atoms, such as ethylenediamine, trimethylenediamine, tetramethylenediamine, and hexamethylenediamine, metaphenylenediamine, paraphenylenediamine, paraxylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylpropane, 4,4'-diaminodiphenylether, 4,4'-diaminodiphenylsulfone, 4,4'-diaminodicyclohexane, bis(4-aminophenyl)phenylmethane, 1,5-diaminonaphthalene, metaxylenediamine, paraxylenediamine, 1,1-bis(4-aminophenyl)cyclohexane, and dicyanodiamide.

[0027] Other examples of the curing agent (B) include polyoxystyrenes such as polyparaoxystyrene; alicyclic acid anhydrides such as hexahydrophthalic anhydride (HHPA) and methyltetrahydrophthalic anhydride (MTHPA), and aromatic acid anhydrides such as trimellitic anhydride (TMA), pyromellitic anhydride (PMDA), and benzophenonetetracarboxylic acid (BTDA); polymercaptan compounds such as polysulfides, thioesters, and thioethers; isocyanate compounds such as isocyanate prepolymers and blocked isocyanates; and organic acids such as carboxylic acid-containing polyester resins. These may be used alone or in combination of two or more.

[0028] Among these, from the viewpoint of obtaining adhesion and high-temperature reliability while maintaining good polishability, it is preferable to contain one or two of a polyfunctional phenol resin and a phenol aralkyl phenol resin, and it is more preferable to contain a triphenylmethane phenol resin or a biphenylene skeleton-containing polyfunctional phenol resin.

[0029] The content of the curing agent (B) is preferably 1 mass % or more, more preferably 2 mass % or more, and even more preferably 5 mass % or more, based on the total amount of the resin composition (P1), in order to obtain appropriate fluidity, filling property, and adhesion while maintaining good polishability. On the other hand, the content of the curing agent (B) is preferably 20 mass % or less, more preferably 15 mass % or less, and even more preferably 10 mass % or less, based on the total amount of the resin composition (P1), from the viewpoint of improving high-temperature reliability and reflow resistance.

[0030] The equivalent ratio, which is the ratio of the epoxy equivalent of the epoxy resin (A) to the active hydroxyl group equivalent of the curing agent (B), is preferably 0.8 to 2.0, more preferably 0.9 to 1.8, and further preferably 1.0 to 1.5.

[0031] [Inorganic filler (C)] The inorganic filler (C) is used to reduce the decrease in strength that occurs with curing of the resin composition (P1) and to control the abrasiveness.

[0032] Examples of the inorganic filler (C) include silicates such as talc, calcined clay, uncalcined clay, mica, and glass; oxides such as titanium oxide, alumina, boehmite, and silica; carbonates such as calcium carbonate, magnesium carbonate, and hydrotalcite; hydroxides such as aluminum hydroxide, magnesium hydroxide, and calcium hydroxide; sulfates or sulfites such as barium sulfate, calcium sulfate, and calcium sulfite; borates such as zinc borate, barium metaborate, aluminum borate, calcium borate, and sodium borate; nitrides such as aluminum nitride, boron nitride, silicon nitride, and carbon nitride; titanates such as strontium titanate and barium titanate. These may be used alone or in combination of two or more.

[0033] Among these, the inorganic filler (C) is preferably one or more selected from fused silica, spherical silica, crystalline silica, alumina, silicon nitride and aluminum nitride, and more preferably fused silica and spherical silica.

[0034] (Particle size of inorganic filler (C)) When the particle size D90 corresponds to a cumulative 90% of the volume-based integrated fraction of the inorganic filler (C) measured by a laser diffraction scattering method, D90 is preferably 5.0 to 80 μm, more preferably 10 to 70 μm, and further preferably 30 to 60 μm. By controlling the D90 in the particle size distribution of the inorganic filler (C), the influence of inorganic fillers (C) having large particle sizes on the reduction in polishing properties can be effectively suppressed.

[0035] Furthermore, when the particle size D50 of the inorganic filler (C) corresponding to a cumulative 50% in the volume-based integrated fraction measured by the laser diffraction scattering method is taken as the particle size D50, it is preferable that the particle size D50 is 0.8 to 40 μm, more preferably 5.0 to 35 μm, and further preferably 10 to 30 μm.

[0036] In addition, the inorganic filler (C) may have two or more peaks in the volume-based particle size distribution measured by the laser diffraction scattering method. In other words, it is preferable to contain two or more kinds of inorganic fillers (C) having different particle sizes. This allows particles with smaller particle sizes to enter between particles with larger particle sizes, making it easier to improve the filling property.

[0037] The content of the inorganic filler (C) is 50% by mass or more, preferably 55% by mass or more, more preferably 60% by mass or more, and even more preferably 65% ​​by mass or more, based on the total amount of the resin composition (P1). By making the content of the inorganic filler (C) equal to or more than the above lower limit, the resin composition (P1) portion is prevented from becoming lower than the surroundings (e.g., the copper layer) during polishing, and thus the occurrence of gaps at the interface with the premolded surface during the subsequent overmolding can be prevented, resulting in good adhesion. On the other hand, the content of the inorganic filler (C) is 75% by mass or less, preferably 74% by mass or less, more preferably 73% by mass or less, and even more preferably 72% by mass or less, based on the total amount of the resin composition (P1). By making the content of the inorganic filler (C) equal to or less than the above upper limit, so-called bite damage is reduced, and polishability is easily improved.

[0038] The resin composition (P1) of the present invention may contain a curing accelerator, a coupling agent, etc. in addition to the epoxy resin (A), the curing agent (B) and the inorganic filler (C).

[0039] [Cure accelerator] The curing accelerator is used to promote the reaction between the epoxy groups of the epoxy resin (A) and the reactive groups of the curing agent (B).

[0040] Examples of the curing accelerator include phosphorus-containing compounds such as organic phosphines, tetra-substituted phosphonium compounds, phosphobetaine compounds, adducts of phosphine compounds and quinone compounds, or adducts of phosphonium compounds and silane compounds; amidine compounds such as 1,8-diazabicyclo(5,4,0)undecene-7 and imidazole; nitrogen-containing compounds such as tertiary amines, amidinium salts, or ammonium salts, such as benzyldimethylamine; phenol compounds such as phenol, bisphenol A, nonylphenol, and 2,3-dihydroxynaphthalene. Examples of the organic phosphines include triphenylphosphine, tri-p-tolylphosphine, tetraphenylphosphonium tetraphenylborate, tetraphenylphosphonium 4,4'-sulfonyldiphenolate, triphenylphosphine triphenylborane, and 1,2-bis-(diphenylphosphino)ethane.

[0041] When a curing accelerator is used, its content is preferably from 0.01 to 2 mass %, and more preferably from 0.1 to 1.0 mass %, based on the total amount of the resin composition (P1).

[0042] [Coupling agent] The coupling agent is used to improve the adhesion between the epoxy resin (A) and the inorganic filler (C).

[0043] As the coupling agent, for example, various silane-based compounds such as epoxysilane, mercaptosilane, aminosilane, alkylsilane, ureidosilane, and vinylsilane; titanium-based compounds; aluminum chelates; aluminum / zirconium-based compounds and other known coupling agents can be used.

[0044] The aminosilane is not particularly limited, but examples thereof include γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropylmethyldimethoxysilane, N-phenylγ-aminopropyltriethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropyltriethoxysilane, N-6-(aminohexyl)3-aminopropyltrimethoxysilane, and N-(3-(trimethoxysilylpropyl)-1,3-benzenedimethanamine).

[0045] The content of the coupling agent is preferably from 0.01 to 10 parts by mass, and more preferably from 0.05 to 5 parts by mass, based on 100 parts by mass of the inorganic filler (C).

[0046] [others] Furthermore, in addition to the above components, the resin composition (P1) of the present embodiment may contain various additives, such as thermosetting resins such as phenolic resins, unsaturated polyester resins, melamine resins, and polyurethanes (excluding the epoxy resin (A)); colorants such as carbon black; release agents such as natural waxes, synthetic waxes, higher fatty acids or metal salts thereof, paraffin, and polyethylene oxide; ion scavengers such as hydrotalcite; stress reduction agents such as silicone oil and silicone rubber; flame retardants such as aluminum hydroxide; and antioxidants.

[0047] [Shape of resin composition (P1)] The shape of the resin composition (P1) of this embodiment can be selected depending on the molding method of the resin composition (P1), and examples thereof include particulate shapes such as tablets, powders, and granules; and sheets.

[0048] [Method for producing resin composition (P1)] The resin composition (P1) of this embodiment is obtained by a known method, and can be prepared as a varnish-like composition, for example, by dissolving, mixing, and stirring the above-mentioned components in a solvent using various mixers such as those used for ultrasonic dispersion, high-pressure collision dispersion, high-speed rotation dispersion, bead mill, high-speed shear dispersion, or rotation-revolution dispersion.

[0049] Hereinafter, an example will be described in which the resin composition (P1) of this embodiment is used in a circuit board with a heat sink, but the use of the resin composition (P1) of this embodiment is not limited to this.

[0050] <Circuit board with heat sink> 1(c), the heatsink-fitted circuit board 50 according to this embodiment includes an insulating layer 20 provided on one surface of the heatsink 10, a circuit pattern 30 provided on the insulating layer 20, and a first sealing body 40 embedded between the circuit patterns 30. The upper surface of the circuit pattern 30 and the upper surface of the first sealing body 40 are approximately flush with each other. The heat sink-equipped circuit board 50 of this embodiment can then be used in the semiconductor device 100 described below.

[0051] The components of the heat sink-fitted circuit board 50 will be described in detail below.

[0052] [First sealing body] The first sealing body 40 is used to fill the spaces between the circuits that constitute the circuit pattern 30. The first sealing body 40 is formed from the above-mentioned premolding resin composition (P1). In other words, the first sealing body 40 is obtained by filling the above-mentioned resin composition (P1) between the circuits of the circuit pattern 30, and then polishing and removing unnecessary resin composition (P1) so that the upper surface of the circuit pattern 30 and the upper surface of the first sealing body 40 are approximately flush with each other. By making the upper surface of the circuit pattern 30 and the upper surface of the first sealing body 40 approximately flush with each other, it becomes easier to suppress the occurrence of gaps and voids on the upper surface of the first sealing body 40 during the subsequent overmolding.

[0053] The first sealing body 40 may be in either a B-stage state or a C-stage state, and is preferably semi-cured after molding such as transfer or compression.

[0054] The surface roughness Ra of the upper surface of the first sealing body 40 is preferably 0.7 μm or less, more preferably 0.5 μm or less, and further preferably 0.3 μm or less, which can prevent gaps from being generated at the interface with the overmold resin. On the other hand, the lower limit of the surface roughness Ra of the upper surface of the first sealing body 40 is not particularly limited, but may be set to, for example, 0.0001 μm or more in order to maintain good productivity.

[0055] On the surface of first sealing body 40, the upper surface of an element mounting portion and the upper surface of a circuit, which will be described later, are exposed.

[0056] [Circuit pattern] The circuit pattern 30 is a circuit formed by etching a part of a lead frame 35 (described later) or the like, and includes an element mounting portion on which a semiconductor chip is placed. The circuit pattern 30 is formed on the heat sink 10 via an insulating layer 20. In this embodiment, the heat sink-fitted circuit board 50 includes a plurality of circuit patterns 30 which are independent of each other.

[0057] The arrangement of the circuit patterns 30 in plan view is set appropriately, but it is preferable that the area surrounded by the outermost edge of the circuit patterns 30 is included in the area covered by the insulating layer 20. That is, it is preferable that all the circuit patterns 30 are arranged within the area of ​​the insulating layer 20, i.e., on the insulating layer 20. This allows the circuit patterns 30 and the insulating layer 20 to be more reliably adhered to each other.

[0058] [Insulation layer] The insulating layer 20 is disposed between the circuit pattern 30 and the heat sink 10, and serves to provide insulation so that electricity passed through the circuit pattern 30 does not leak to the heat sink 10. The insulating layer 20 also has good thermal conductivity and excellent heat dissipation properties.

[0059] The thermal conductivity (25°C) of the insulating layer 20 in the thickness direction is preferably higher than the thermal conductivity (25°C) of the cured body of the resin composition (P1) of this embodiment, and specifically, is preferably 7.5 W / m·K or more.

[0060] Furthermore, the insulating layer 20 is formed in a process different from that of the first sealing body 40. That is, an interface exists between the insulating layer 20 and the first sealing body 40.

[0061] Furthermore, the outer peripheral edge of the insulating layer 20 is covered with the first sealing body 40. This makes it easier to improve the reliability of the circuit board 50 with a heat sink.

[0062] The thickness of the insulating layer 20 is preferably 50 μm or more and 500 μm or less. By making the thickness of the insulating layer 20 equal to or more than the above-mentioned lower limit, good insulation properties can be maintained. On the other hand, by making the thickness of the insulating layer 20 equal to or less than the above-mentioned upper limit, the overall thickness of the heat sink-equipped circuit board 50 can be prevented from becoming too thick.

[0063] In this embodiment, the specific gravity of the sheet-like insulating layer 20 in the B-stage state is preferably 1.0 to 2.0. This allows more appropriate pressure to be applied in the manufacturing process of the heatsink-fitted circuit board 50, making it easier to improve adhesion between the heatsink 10 and the circuit pattern 30.

[0064] (Resin composition (p)) The insulating layer 20 is made of a resin composition (p) containing a thermosetting resin. The resin composition (p) is a material different from the resin composition (P1) that forms the first sealing body 40.

[0065] Specifically, the resin composition (p) preferably contains a thermosetting resin and boron nitride particles. This provides good thermal conductivity and insulation. In addition, the insulating layer 20 can efficiently improve thermal conductivity and adhesion by dispersing boron nitride particles when pressure is applied during the manufacturing process of the heat sink-equipped circuit board 50.

[0066] The thermosetting resin includes the same epoxy resin as the epoxy resin (A) and a cyanate resin. Among them, one or more selected from epoxy resins having a dicyclopentadiene skeleton, epoxy resins having a biphenyl skeleton, epoxy resins having an adamantane skeleton, epoxy resins having a phenol aralkyl skeleton, epoxy resins having a biphenyl aralkyl skeleton, epoxy resins having a naphthalene aralkyl skeleton, epoxy resins having a naphthalene skeleton, epoxy resins having a methoxynaphthalene aralkyl skeleton, and cyanate resins are preferred, which makes it easier to improve the dispersibility of boron nitride particles.

[0067] As the cyanate resin, a cyanate ester resin can be used. Specific examples of the cyanate ester resin include bisphenol A dicyanate, polyphenol cyanate (oligo(3-methylene-1,5-phenylene cyanate), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanate phenylmethane), bis(4-cyanate-3,5 bifunctional cyanate resins such as 1,3-bis(4-cyanatephenyl-1-(methylethylidene))benzene, bis(4-cyanatephenyl)thioether, and bis(4-cyanatephenyl)ether; polyfunctional cyanate resins derived from phenol novolac, cresol novolac, and phenol resins containing a dicyclopentadiene structure; and prepolymers in which the above-listed cyanate ester resins are partially converted to triazine.

[0068] As commercially available cyanate ester resins, for example, PT30, BA230, DT-4000, DT-7000, etc. manufactured by Lonza Japan can be used.

[0069] The content of the thermosetting resin is preferably from 1 to 30% by mass, and more preferably from 5 to 20% by mass, based on the total amount of the resin composition (p) (solid content).

[0070] The boron nitride particles are preferably agglomerated particles formed by agglomerating primary particles. The primary particles of the boron nitride particles may be plate-like, scaly, or spherical, and are preferably scaly. In particular, agglomerated particles of scaly boron nitride are preferred. This allows the boron nitride particles to be aligned, making it easier to improve thermal conductivity.

[0071] The average longitudinal length of the scaly (or plate-like) primary particles of boron nitride (the maximum length in the direction perpendicular to the thickness direction of the scales) is, for example, 1 to 100 μm, preferably 3 to 90 μm. The average longitudinal length of the boron nitride particles is preferably 5 μm or more, more preferably 10 μm or more, even more preferably 20 μm or more, particularly preferably 30 μm or more, and even more preferably 40 μm or more, while it is preferably 100 μm or less, more preferably 90 μm or less.

[0072] The average thickness of the primary particles of the scaly boron nitride (the length of the flakes in the thickness direction, that is, the length of the particles in the shorter direction) is, for example, 0.01 to 20 μm, and preferably 0.1 to 15 μm.

[0073] The aspect ratio (length in the longitudinal direction / thickness) of the primary particles of the scaly boron nitride is, for example, 2 to 10,000, and preferably 10 to 5,000.

[0074] The average primary particle size measured by the light scattering method is a volume average particle size measured by a dynamic light scattering particle size distribution measuring device. If the average primary particle size of the boron nitride particles measured by the light scattering method is not within the above range, the insulating layer 20 may become brittle and the handling properties may be reduced.

[0075] Specific examples of commercially available boron nitride particles include the "PT" series (e.g., "PT-110") manufactured by Momentive Performance Materials Japan, Inc., and the "Sho-B-N UHP" series (e.g., "Sho-B-N UHP-1") manufactured by Showa Denko KK.

[0076] The content of the boron nitride particles is 60 to 80 mass %, more preferably 65 to 75 mass %, based on the total amount of the resin composition (p) (solid content). The content by volume of the boron nitride particles is preferably 50 to 70% by volume, and more preferably 55 to 65% by volume, based on the total volume of the resin composition (p) (solid content).

[0077] The resin composition (p) may further contain components other than the above-mentioned thermosetting resin and boron nitride particles. For example, when an epoxy resin is used as the thermosetting resin, it is preferable to use a curing agent, which may be the above-mentioned curing agent (B), preferably a phenol-based curing agent, and a curing catalyst.

[0078] Examples of the curing catalyst include organic metal salts such as zinc naphthenate, cobalt naphthenate, tin octoate, cobalt octoate, bisacetylacetonate cobalt (II), and trisacetylacetonate cobalt (III); tertiary amines such as triethylamine, tributylamine, and 1,4-diazabicyclo[2.2.2]octane; 2-phenyl-4-methylimidazole, 2-ethyl-4-methylimidazole, 2,4-diethylimidazole, and 2-phenyl-4-methyl-5-hydroxyimidazole. imidazoles such as phenylalanine, 2-phenyl-4,5-dihydroxymethylimidazole, etc.; organic phosphorus compounds such as triphenylphosphine, tri-p-tolylphosphine, tetraphenylphosphonium tetraphenylborate, triphenylphosphine triphenylborane, 1,2-bis-(diphenylphosphino)ethane, etc.; phenolic compounds such as phenol, bisphenol A, nonylphenol, etc.; organic acids such as acetic acid, benzoic acid, salicylic acid, p-toluenesulfonic acid, etc.; etc., or mixtures thereof.

[0079] When a curing catalyst is used, the content thereof is preferably 0.001 part by mass or more and 1 part by mass or less based on the total amount of the resin composition (p) (solid content).

[0080] The content of the curing agent is preferably from 0.1% by mass to 30% by mass, and more preferably from 0.3% by mass to 15% by mass, based on the total amount of the resin composition (p) (solid content).

[0081] The material constituting the insulating layer 20 may further include a leveling agent, a coupling agent, an antioxidant, and the like.

[0082] The leveling agent may be an acrylic copolymer, etc. The leveling agent is preferably used in an amount of 2% by mass or less, more preferably 0.01% by mass or more and 1.0% by mass or less, based on the total amount of the resin composition (p) (solid content).

[0083] As the coupling agent, an epoxy silane coupling agent, a cationic silane coupling agent, an amino silane coupling agent, a titanate-based coupling agent, a silicone oil-type coupling agent, or the like can be used. The amount of the coupling agent is preferably from 0.1 to 10 parts by mass, and particularly preferably from 0.5 to 7 parts by mass, per 100 parts by mass of the boron nitride particles.

[0084] (Method of producing resin composition (p)) The resin composition (p) (solid content) constituting the insulating layer 20 of this embodiment can be prepared by blending the above-mentioned thermosetting resin, boron nitride particles, other components, and solvent in the above-mentioned ratios and stirring and mixing them by a known method.

[0085] Examples of the solvent include organic solvents such as ketones such as acetone and methyl ethyl ketone, esters such as ethyl acetate, and amides such as N,N-dimethylformamide, etc. Examples of the solvent also include aqueous solvents such as water and alcohols such as methanol, ethanol, propanol, and isopropanol.

[0086] The insulating layer 20 of the present embodiment can be produced by forming it into a sheet in a B-stage state. That is, the insulating layer 20 is completely cured when it is integrated with the heat sink 10 and the circuit pattern 30 under heat and pressure during the manufacturing process of the heat sink-fitted circuit board 50. For example, the material in the form of a varnish can be applied to a substrate, which can then be heat-treated and dried to form a sheet. The substrate can be, for example, a metal foil that constitutes a heat dissipation member, a lead frame, a peelable carrier material, or the like, but it may also be applied directly to the heat sink 10. The heat treatment for drying the coating film is carried out under conditions of, for example, 80 to 150° C. and 5 minutes to 1 hour.

[0087] [heat sink] The heat sink 10 has a function of dissipating heat generated in the circuit pattern 30 and the like to the outside. The thickness of the heat sink 10 can be appropriately set depending on the application, but is preferably, for example, 0.2 to 5 mm.

[0088] The heat sink 10 is preferably made of at least one material selected from copper and aluminum, and from the standpoint of improving thermal conductivity, workability, and the like, copper is more preferable.

[0089] <Method of manufacturing a circuit board with a heat sink> Next, a method for manufacturing the circuit board 50 fitted with a heat sink according to this embodiment will be described with reference to FIG. The method for manufacturing the circuit board 50 with a heat sink of this embodiment includes the following steps. [Step 1] A step of laminating an insulating layer 20 on one surface of a heat sink 10. [Step 2] A step of arranging a lead frame 35 on the insulating layer 20, the lead frame 35 having a plurality of independent circuit patterns 30 and a convex bridge 31 provided so as to straddle adjacent circuit patterns 30. [Step 3] A step of embedding the first sealing body 40 between the circuit patterns 30. [Step 4] A step of removing a part of the first sealing body 40 and the convex bridge 31 to expose the upper surface of the circuit pattern 30.

[0090] Each step will be described in detail below.

[0091] [Process 1] The above-mentioned materials can be used as the heat sink 10. Next, an insulating layer 20 is laminated on one surface of the heat sink 10 by a known method.

[0092] [Process 2] 1(a), there is prepared a lead frame 35 having a plurality of independent circuit patterns 30 and a convex bridge 31 provided so as to straddle adjacent circuit patterns 30. Here, the lead frame 35 will be described in detail.

[0093] (Lead frame) Fig. 2 is a perspective view showing an example of a lead frame. As shown in Fig. 2, a lead frame 35 has a surface on which a plurality of circuit patterns are formed (later circuit patterns 30) and a convex bridge 31 connecting these surfaces. The lead frame 35 is formed using a metal plate having good electrical and thermal conductivity, and is preferably made of, for example, an aluminum plate or a copper plate, and more preferably a copper plate from the viewpoint of low thermal resistance. The lead frame 35 may be subjected to a surface treatment from the viewpoint of preventing oxidation of copper, etc., and may be subjected to, for example, nickel plating or solder plating. The thickness of the lead frame 35 is adjusted as appropriate, but is preferably, for example, 0.3 to 1.0 mm.

[0094] The convex bridge 31 may be made of the same material as the circuit pattern 30 or a different material, but from the viewpoint of productivity, it is preferable that the convex bridge 31 is made of the same material. Also, it is preferable that the convex bridge 31 is integrally formed with the circuit pattern 30. There are multiple convex bridges 31, and the directions in which they cross over one another are parallel to each other. That is, the convex bridges are in the same direction as each other.

[0095] The convex bridge 31 of this embodiment is formed as follows. First, the metal plate that is the material of the lead frame 35 is bent at the portion that will become the convex bridge 31. At this time, the degree of curvature is set to be about the same as the thickness of the metal plate. After that, the plate is pressed and punched to form a plurality of independent circuit patterns 30, thereby obtaining the lead frame 35 shown in FIG. In this embodiment, by making the connecting portion protrude above the circuit pattern 30, it is possible to remove the convex bridge 31 together with a part of the first sealing body 40 in step 4, thereby improving production efficiency.

[0096] The connecting parts in this embodiment will then become the convex bridges 31. The connecting parts may be of a known shape, but preferably have a length of 0.5 to 2 mm and a width of 0.5 to 2 mm. In addition, the connecting parts are preferably provided in parallel to each other so that they can be molded and processed together.

[0097] Lead frame 35 is then placed on insulating layer 20 in a known manner with convex bridge 31 on top.

[0098] [Process 3] 1(b), a first sealing body 40 is embedded between the circuits constituting the circuit pattern 30. For example, a resin composition (P1) for the first sealing body 40 is used, and the resin composition (P1) is filled between the circuits by using a method selected from a transfer molding method, a compression molding method, an injection molding method, or the like, to embed the first sealing body 40. At this time, the first sealing body 40 may be embedded so as to cover the entirety of the convex bridge 31, the insulating layer 20, and the circuit pattern 30.

[0099] [Step 4] A part of the first sealing body 40 and the convex bridge 31 are removed to match the height of the circuit pattern 30, thereby exposing the upper surface of the circuit pattern 30 (FIG. 1(c)). That is, the removal is stopped when the upper surface of the circuit pattern 30 is exposed. This makes it possible to make the upper surface of the first sealing body 40 and the upper surface of the circuit pattern 30 flush while removing the convex bridge 31, thereby improving productivity.

[0100] The removal method may be a known method, for example, polishing or cutting. Specifically, mechanical polishing (diamond tool, grindstone, buff, polishing roll, etc.) or chemical mechanical polishing (CMP) may be used, but mechanical polishing is preferred from the viewpoint of obtaining a significant polishing improvement effect.

[0101] After the circuit surface is exposed, it is preferable to apply an antioxidant to the upper surface of the circuit pattern 30. This can prevent the circuit from being oxidized.

[0102] <Semiconductor device> As shown in FIG. 3(b), the semiconductor device 100 of this embodiment includes a heat sink 10, an insulating layer 20 laminated on one side of the heat sink 10, a circuit pattern 30 arranged on the insulating layer 20, a first sealing body 41 (cured product of resin composition (P1)) embedded between the circuits constituting the circuit pattern 30 and configured so that its upper surface is approximately flush with the upper surface of the circuit pattern 30, a semiconductor chip 81 mounted on the circuit pattern 30 exposed on the upper surface of the first sealing body 40, and a second sealing body 42 (cured product of resin composition (P2)) covering the semiconductor chip 81, and there is an interface between the first sealing body 41 and the second sealing body 42. In addition, the semiconductor chip 81 is connected to the lead frame 35 via wires 83 .

[0103] The interface between the first sealing body 41 and the second sealing body 42 is a boundary that is generated when the first sealing body 41 and the second sealing body 42 are bonded to each other after being obtained by different processes. The interface may be visible, but is not limited to being visible. In this embodiment, the interface is a substantially horizontal surface. The second sealing body 42 can be obtained by using a known sealing resin material (also referred to as "resin composition (P2)"). The first sealing body 41 and the second sealing body 42 may be formed of different resin materials or may be formed of the same material, but are preferably formed of different resin materials.

[0104] In this embodiment, when the linear expansion coefficient of the first sealing body 41 (cured product of the resin composition (P1): 175°C for 3 minutes) at 40°C to 80°C is α1 (ppm / °C) and the linear expansion coefficient of the second sealing body 42 (cured product of the resin composition (P2): 175°C for 3 minutes) at 40°C to 80°C is α2 (ppm / °C), (α1 / α2) is preferably 0.7 to 1.5, and more preferably 0.8 to 1.2. That is, the smaller the difference between α1 and α2, the more effectively it is possible to suppress interface peeling caused by the difference in the linear expansion coefficient between the first sealing body 41 and the second sealing body 42, peeling from the circuit pattern 30 due to warping, and the like.

[0105] In this embodiment, α1 and α2 are appropriately adjusted depending on the structure of the semiconductor module and the thickness of the sealing resin portion, but are preferably 8 to 20 ppm / ° C., and more preferably 12 to 18 ppm / ° C., respectively. This makes it possible to suppress warping and peeling within the semiconductor device 100 and improve reliability.

[0106] <Method of Manufacturing Semiconductor Device> 3A to 3C are cross-sectional views that diagrammatically show a method for manufacturing the semiconductor device 100 of the present embodiment. A manufacturing method for the semiconductor device 100 includes a step of using a heat sink-fitted circuit board 50 to mount a semiconductor chip 81 on a circuit pattern 30 exposed on the heat sink-fitted circuit board 50, and a step of encapsulating the semiconductor chip 81 with a second encapsulating resin (resin composition (P2)) to form a second encapsulating body 42. The step of mounting the semiconductor chip 81 and the step of forming the second sealing body 42 can both be performed using known methods.

[0107] The semiconductor device 100 of this embodiment uses the circuit board 50 with a heat sink, and therefore has improved processability, manufacturing stability, positional accuracy, and the like, and is therefore excellent in reliability and durability.

[0108] Although the embodiments of the present invention have been described above with reference to the drawings, these are merely examples of the present invention, and various configurations other than those described above can also be adopted.

[0109] <Modification> 4 and 5, the heat sink 10 of a circuit board 51 with a heat sink and a semiconductor device 101 may have fins 12. Details will be described below.

[0110] The heat sink 10 may include a flat base plate 11 and a plurality of fins 12 protruding from the surface of the base plate 11 opposite to the insulating layer 20. The flat base plate 11 and the fins 12 may be joined by a known method, or may be integrally molded.

[0111] The thickness of the base plate 11 can be appropriately set depending on the application, but is preferably, for example, 0.2 to 1.5 mm. Furthermore, by making the thickness of the base plate 11 0.5 to 1.5 times the thickness of the circuit pattern 30, warping of the entire heat sink-attached circuit board 51 can be suppressed, and adhesion can be easily improved.

[0112] In this embodiment, the heat sink 10 has a plurality of fins 12 standing upright from one surface of the base plate 11, thereby increasing the surface area of ​​the heat sink 10 and improving the heat dissipation efficiency. The plurality of fins 12 are flush. The heights of the plurality of fins 12 are uniform, and the upper surfaces of the fins 12 are flat, forming a surface, so that the heat sink-fitted circuit board 51 can be manufactured stably.

[0113] The shape of the fin 12 is not particularly limited, and may be, for example, a polygonal columnar shape such as a square or hexagonal columnar shape, or a cylindrical shape. The above-mentioned quadrangular columnar shape may be a columnar shape having a square cross-sectional shape, a rectangular columnar shape, a rhombus columnar shape, a parallelogram columnar shape, etc. The above-mentioned cylindrical shape may be a columnar shape having a circular, elliptical, oval, etc. cross-sectional shape.

[0114] The number of the multiple fins 12 is not particularly limited and is set appropriately from the viewpoints of the application, mechanical strength, etc. The shapes of the multiple fins 12 may be the same as or different from each other, or may differ only partially.

[0115] Although the arrangement of the multiple fins 12 is not particularly limited, it is preferable that the area surrounded by the outline connecting the outer ends of the fins 12 is included in the area covered by the insulating layer 20 of the base plate 11. It is also preferable that the base plate 11 does not have fins 12 at the outer peripheral end. This makes it possible to improve adhesion while maintaining mechanical strength against pressure applied during the manufacturing process of the circuit board 51 fitted with a heat sink.

[0116] The distance between the fins 12 is not particularly limited, but is preferably 0.5 to 2.0 mm. By setting the distance between the fins 12 to 0.5 mm or more, the cutting process of the fins 12 can be performed efficiently, and the mechanical strength can be maintained against the pressing force during the manufacturing process of the heat sink-fitted circuit board 50. Furthermore, by setting the distance between the fins 12 to 2.0 mm or less, the heat dissipation performance of the heat sink 10 can be further improved. EXAMPLES

[0117] The present invention will be described below with reference to examples, but the present invention is not limited to these.

[0118] (1) Preparation of premolding resin composition (P1) The following raw materials were used and mixed in a mixer to obtain the contents (parts by mass) shown in Table 1. The resulting mixture was then kneaded with a roll, cooled, and pulverized to obtain a granular resin composition (P1).

[0119] [Raw materials] (Epoxy resin (A)) Epoxy resin (A1): Phenol aralkyl type epoxy resin containing biphenylene skeleton, "NC3000H" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent 286 Epoxy resin (A2): Triphenolmethane type epoxy resin, Mitsubishi Chemical Corporation "1032H60", epoxy equivalent 171 Epoxy resin (A3): Phenol aralkyl type epoxy resin containing biphenylene skeleton, "NC3000" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent 277

[0120] (Hardening agent (B)) Hardener (B1): Phenol aralkyl resin containing biphenylene skeleton, Meiwa Kasei's "MEH-7851H", active hydroxyl equivalent 199 Hardener (B2): Triphenolmethane type phenolic resin, Meiwa Kasei's "MEH-7500", active hydroxyl equivalent 97

[0121] (Inorganic filler (C)) Inorganic filler (C1): Fused spherical silica, particle size (D50): 28 μm

[0122] (Cure accelerator) Curing accelerator: Tetraphenylphosphonium 4,4'-sulfonyldiphenolate

[0123] (Coupling Agent) Coupling agent: N-phenyl-3-aminopropyltrimethoxysilane, Toray Dow Corning "CF4083"

[0124] (others) Flame retardant: Aluminum hydroxide, Sumitomo Chemical "CL303" Particle size: 4μm Low stress agent: Epoxy polyether modified silicone oil, Toray Dow Corning "FZ-3730" Colorant: Carbon black, Mitsubishi Chemical "Carbon #5"

[0125] (2) Manufacturing of circuit boards with heat sinks A metal substrate (copper foil with a thickness of 500 μm) was punched to produce a lead frame having a circuit pattern and a convex bridge. The obtained lead frame was filled with the obtained resin composition (P1) using a low pressure transfer molding machine under conditions of a mold temperature of 175°C, an injection pressure of 10.0 MPa, and a curing time of 2 minutes, and then cured. Subsequently, a part of the sealing body and the convex portion of the convex bridge were polished with a diamond bit to expose the upper surface of the circuit pattern, thereby obtaining a circuit board with a heat sink.

[0126] (3) Measurement The resin composition (P1) was subjected to the following measurements.

[0127] (Gel Time) Using a low pressure transfer molding machine (KOTAKISEIKI Co., Ltd., "KTS-15"), the resin composition (P1) of each Example and Comparative Example was injected into a spiral flow measurement mold conforming to ANSI / ASTM D 3123-72 under conditions of 175°C, injection pressure of 6.9 MPa, and pressure retention time of 120 seconds. The time from the start of injection until the resin composition (P1) hardened and no longer flowed was measured and taken as the gel time.

[0128] [Creating test specimens] Using a low-pressure transfer molding machine (KTS-30, manufactured by Kotaki Seiki Co., Ltd.), the resin composition (P1) was injected and molded under conditions of a mold temperature of 175°C, an injection pressure of 9.8 MPa, and a curing time of 120 seconds to obtain a molded product having a length of 80 mm, a width of 10 mm, and a thickness of 4 mm. The molded product was then further heat-treated at 200°C for 4 hours to post-cure it, and used as a test specimen.

[0129] (Glass transition temperature (Tg), coefficient of linear expansion (CTE)) Using the test piece, measurements were performed with a thermomechanical analyzer (Seiko Instruments Inc., TMA / SS6000) at a temperature range of 0°C to 320°C and a heating rate of 5°C / min. From the measurement results, the glass transition temperature Tg (°C), the linear expansion coefficient below the glass transition temperature (α1), and the linear expansion coefficient above the glass transition temperature (α2) were calculated. α1 was the linear expansion coefficient at 40°C to 80°C, and α2 was the linear expansion coefficient at 190°C to 230°C.

[0130] (Flexural modulus, flexural strength) The test pieces were used to measure the flexural modulus and flexural strength in accordance with JIS K 6911 at an ambient temperature of 25°C.

[0131] (storage modulus, loss modulus, tan δ) The test pieces were used to measure the storage modulus, loss modulus, and tan δ with a dynamic viscoelasticity measuring device (manufactured by A&D Co., Ltd., "DDV-25GP") (heating rate: 5°C / min, frequency: 10 Hz, load: 800 g, temperature range: 30 to 350°C).

[0132] (Water absorption rate) The test piece was subjected to a humidification treatment in a boiling environment for 24 hours, the weights before and after the humidification treatment were measured, and the rate of weight change was calculated as the water absorption rate (%).

[0133] (4) Evaluation [Abrasive; Bite damage] The resin composition (P1) was injected and molded using a low-pressure transfer molding machine (KTS-30 manufactured by Kotaki Seiki Co., Ltd.) at a mold temperature of 175°C, injection pressure of 9.8MPa, and curing time of 120 seconds to obtain a molded product with a diameter of 50 mmΦ and a thickness of 3 mm. The molded product was then post-cured at 175°C for 4 hours to prepare a test specimen. The upper surface of the obtained test piece was subjected to a polishing test (processing depth 10 μm) using a semi-automatic cutting and flattening processing device (DAS8930, manufactured by DISCO Corporation). The polishing speed during processing and the polishing jig after polishing were visually confirmed and evaluated as follows. ·standard 〇: No loss of polishing power during processing, and minimal damage to polishing jigs △: Either the decrease in polishing power during processing or damage to the polishing jig is small, but the other is large. ×: The polishing power during processing is reduced, or the polishing tool is damaged.

[0134] [Flatness] The surface roughness Ra of the upper surface (exposed surface, polished surface) of the first sealing body was measured in accordance with JIS B 0601 and evaluated according to the following criteria. The measurement was performed using a laser microscope (OLS3000, manufactured by Olympus Corporation). Standard (roughness after polishing) ○:Ra less than 0.5μm △: Ra0.5 or more, less than 1.0μm ×: Ra1.0μm or more

[0135] [Table 1] [Explanation of symbols]

[0136] 10 Heatsink 11 Base plate 12 fins 20 insulating layers 30 Circuit Patterns 31 Convex Bridge 35 lead frame 40 sealing resin 41 First sealing body 42 Second sealing body 50 Circuit board with heat sink 51 Circuit board with heat sink 81 Semiconductor chips 83 Wire 100 Semiconductor device 101 Semiconductor device

Claims

1. A resin composition comprising an epoxy resin (A), a curing agent (B), and an inorganic filler (C), A resin composition for premold molding, wherein the content of the inorganic filler (C) is 50% by mass or more and 75% by mass or less based on the total amount of the resin composition.

2. The resin composition according to claim 1, The resin composition has a particle size D90 of 5.0 to 80 μm, where D90 is a particle size corresponding to a cumulative 90% of the volume-based integrated fraction of the inorganic filler (C) measured by a laser diffraction scattering method.

3. The resin composition according to claim 1 or 2, The resin composition, wherein the inorganic filler (C) is one or more selected from the group consisting of fused silica, spherical silica, crystalline silica, alumina, silicon nitride and aluminum nitride.

4. The resin composition according to claim 1 or 2, A resin composition having a flexural modulus of 12,000 MPa or less, as measured by the following procedure. Procedure: The resin composition is cured at 175° C. and 9.8 MPa, and the flexural strength of the resulting test piece is measured at 25° C. in accordance with JIS K-6911.

5. The resin composition according to claim 1 or 2, A resin composition, wherein an equivalent ratio, which is a ratio of an epoxy equivalent of the epoxy resin (A) to an active hydroxyl group equivalent of the curing agent (B), is 1.4 or more and 2.0 or less.

6. an insulating layer provided on one surface of the heat sink; A circuit pattern provided on the insulating layer; a first sealing body embedded between the circuit patterns; A heat sink-equipped circuit board comprising: The first sealing body is a premolded body made of the resin composition according to claim 1 .

7. 7. The circuit board with a heat sink according to claim 6, a top surface of the circuit pattern and a top surface of the first sealing body are substantially flush with each other;

8. 7. The circuit board with a heat sink according to claim 6, A circuit board with a heat sink, wherein the surface roughness Ra of the upper surface of the first sealing body is 0.7 μm or less.

9. The circuit board with a heat sink according to claim 6 ; a semiconductor chip mounted on the circuit board with a heat sink; a second sealing body covering the semiconductor chip; Equipped with The semiconductor device has an interface between the first encapsulant and the second encapsulant.

10. 10. The semiconductor device according to claim 9, The semiconductor device, wherein the first sealing body and the second sealing body are formed from different resin materials.

11. depositing an insulating layer on one side of the heat sink; disposing a lead frame having a plurality of independent circuit patterns on the insulating layer; A step of embedding the resin composition according to claim 1 or 2 between the circuit patterns; removing a portion of the resin composition and the convex bridge to expose an upper surface of the circuit pattern; A method for manufacturing a circuit board with a heat sink, comprising:

12. A method for manufacturing a circuit board with a heat sink according to claim 11, comprising the steps of: After the step of exposing the top surface of the circuit pattern, The method for manufacturing a circuit board with a heat sink further comprises a step of applying an antioxidant to the exposed circuit pattern.

13. A method for manufacturing a circuit board with a heat sink according to claim 11, comprising the steps of: A method for manufacturing a circuit board with a heat sink, wherein the lead frame has a convex bridge arranged to span between adjacent circuit patterns.

14. A method for manufacturing a circuit board with a heat sink according to claim 11, comprising the steps of: A method for manufacturing a circuit board with a heat sink, wherein the step of exposing the upper surface of the circuit pattern is performed by polishing or cutting.

15. A method for manufacturing a semiconductor device using a heat sink-fitted circuit board obtained by the method for manufacturing a heat sink-fitted circuit board according to claim 11, comprising the steps of: mounting a semiconductor chip on the exposed top surface of the circuit pattern; encapsulating the semiconductor chip with a second resin composition; A method for manufacturing a semiconductor device comprising the steps of:

Citation Information

Patent Citations

  • Leadframe substrate, semiconductor module and method for manufacturing leadframe substrate

    WO2009110376A1