Additional manufacturing material, additional manufacturing method, and additional manufacturing device

A dual-powder additive manufacturing material with controlled liquid phase ratios and temperature ranges addresses shape retention and defect issues in metal sintering, achieving high-density molded articles.

JP2024135253APending Publication Date: 2024-10-04RICOH CO LTD +2
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023045849
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Additive manufacturing of metals, particularly aluminum, faces challenges in maintaining shape and preventing defects such as voids and poor solidification due to inadequate control of the melted metal amount and oxide film destruction during the sintering process.

Method used

A material for additive manufacturing comprising at least two types of powders, A and B, where powder A contains an alloy or pure metal, and powder B has a different composition, with specific liquid phase ratios and temperature ranges to control melting, ensuring high density and shape retention.

Benefits of technology

The material enables easy additive manufacturing of high-density molded articles with excellent shape retention by precise temperature control and reduced sintering defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135253000001_ABST
    Figure 2024135253000001_ABST
Patent Text Reader

Abstract

To provide an additional manufacturing material easily manufactured additionally and capable of manufacturing a compact highly sealed and excellent in shape retention.SOLUTION: This additional manufacturing material contains at least powder A and powder B. The powder A contains an alloy or a pure metal. The powder B contains an alloy different in composition from the powder A. There is a temperature range in which the liquid-phase ratio of the powder A to the total mass of the powder A is 30 mass% or lower and the liquid-phase ratio of the powder B to the total mass of the powder B is 70 mass% or higher.SELECTED DRAWING: Figure 9A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to additive manufacturing materials, additive manufacturing methods, and additive manufacturing devices. [Background technology]

[0002] In recent years, additive manufacturing technology, which produces high-resolution three-dimensional objects made of metals and ceramics, has been attracting attention. Examples of additive manufacturing for metals include the powder bed fusion method, in which a laser or electron beam is irradiated onto metal powder evenly spread on a stage to melt and solidify the metal powder locally and selectively, the directed energy deposition method, in which metal powder is directly supplied to the irradiation position of the laser or electron beam, and the binder jetting method (BJT), in which a hardening liquid is ejected onto a powder bed by inkjet to solidify it, to produce a shaped object called a sintered precursor, which is then heat-treated to volatilize the resin components (called the "debinding process") and then further heated to bond the core powder particles together to produce a sintered body, which is the final part (called the "sintering process").

[0003] Metal additive manufacturing is a new manufacturing technology that is expected to continue to develop in the future. Aluminum (Al) in particular has a lower melting point and requires less energy to manufacture than iron and other materials, making it suitable for additive manufacturing. However, because the metal powder is partially melted and solidified to form the product, there is also the issue that defects such as voids and poor solidification tend to occur during solidification.

[0004] Therefore, for example, in order to suppress defects such as voids and poor solidification, it has been proposed to mix a base metal powder with a metal powder having a higher melting point than the base metal powder, and to solidify the base metal powder by using the metal powder with the higher melting point as a solidification nucleus, thereby suppressing defects in the molded body (see, for example, Patent Document 1). Summary of the Invention [Problem to be solved by the invention]

[0005] If too much metal is melted, the compact will not be able to maintain its shape, and conversely, if too little is melted, the oxide film will not be sufficiently destroyed, resulting in poor bonding and defects such as voids. For this reason, high precision is required in controlling the temperature of the metal powder during molding.

[0006] The present invention aims to provide a material for additive manufacturing that can be easily additively manufactured and can produce molded bodies that have high density and excellent shape retention. [Means for solving the problem]

[0007] The additive manufacturing material of the present invention, as a means for solving the above-mentioned problems, is an additive manufacturing material containing at least powder A and powder B, wherein powder A contains an alloy or pure metal, and powder B contains an alloy having a different composition from powder A, and is characterized in that a liquid phase ratio of powder A to the total mass of powder A is 30 mass% or less, and there is a temperature range in which the liquid phase ratio of powder B to the total mass of powder B is 70 mass% or more. Effect of the Invention

[0008] According to the present invention, it is possible to provide a material for additive manufacturing that can be easily additively manufactured and can produce a molded body that has high density and excellent shape retention. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a schematic cross-sectional view of a BJT additive manufacturing apparatus in accordance with one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic side view of the additive manufacturing apparatus of FIG. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing a modeling portion of the additive manufacturing apparatus of FIG. [Figure 4] FIG. 4 is a schematic perspective view of the additive manufacturing apparatus of FIG. [Figure 5A] FIG. 5A is a schematic perspective view of a powder bath of the additive manufacturing apparatus of FIG. 1. [Figure 5B]5B is a schematic perspective view of the supply tank and the model tank of the additive manufacturing apparatus of FIG. 1. [Figure 6] FIG. 6 is a block diagram illustrating a control unit of a BJT additive manufacturing device in accordance with one embodiment of the present invention. [Figure 7A] FIG. 7A is a schematic cross-sectional view showing the flow of a modeling operation in a modeling unit of a BJT additive manufacturing apparatus according to one embodiment of the present invention. [Figure 7B] FIG. 7B is a schematic cross-sectional view showing the flow of a modeling operation in a modeling unit of a BJT additive manufacturing apparatus according to one embodiment of the present invention. [Figure 7C] FIG. 7C is a schematic cross-sectional view showing the flow of a modeling operation in a modeling unit of a BJT additive manufacturing apparatus according to one embodiment of the present invention. [Figure 7D] FIG. 7D is a schematic cross-sectional view showing the flow of a modeling operation in a modeling unit of a BJT additive manufacturing apparatus according to one embodiment of the present invention. [Figure 7E] FIG. 7E is a schematic cross-sectional view showing the flow of a modeling operation in a modeling unit of a BJT additive manufacturing apparatus according to one embodiment of the present invention. [Figure 8] 8 is a graph showing the relationship between the progress of the debinding and sintering steps in a BJT additive manufacturing method according to an embodiment of the present invention and the temperature of the additive manufacturing material according to an embodiment of the present invention. The vertical axis shows the temperature of the additive manufacturing material (° C.), and the horizontal axis shows time (h). [Figure 9A] 9A is a graph showing the results of calculations, using thermodynamic calculation software (CaTCalc), of the change in liquid phase ratio versus temperature for Powder A (pure Al) and Powder B (AlSi12) in Example 1. The vertical axis represents the liquid phase ratio (%), and the horizontal axis represents the temperature (°C). [Figure 9B] 9B is a graph showing the results of calculations, using thermodynamic calculation software (CaTCalc), of the change in the liquid phase ratio with respect to temperature for Powder A (AlSi4) and Powder B (AlSi5) in Comparative Example 2. The vertical axis represents the liquid phase ratio (%), and the horizontal axis represents the temperature (°C). [Figure 10A] FIG. 10A is a schematic perspective view showing the shapes of the sintered precursors shaped in Examples 1 to 14 and Comparative Examples 1 and 2. FIG. [Figure 10B]FIG. 10B is a schematic front view showing the shapes of the sintered precursors shaped in Examples 1 to 14 and Comparative Examples 1 and 2. [Figure 10C] FIG. 10C is a schematic front view showing the shapes of the sintered bodies of Examples 1 to 14 and Comparative Examples 1 and 2, and is an explanatory diagram of a method for evaluating the amount of deformation of the sintered bodies. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] (Materials for Additive Manufacturing) The additive manufacturing material of the present invention is an additive manufacturing material containing at least powder A and powder B, wherein powder A contains an alloy or pure metal, powder B contains an alloy having a different composition from powder A, and there exists a temperature range in which the liquid phase ratio of powder A to the total mass of powder A is 30 mass% or less, and the liquid phase ratio of powder B to the total mass of powder B is 70 mass% or more.

[0011] In additive manufacturing, when sintering a sintering precursor, if too much metal is melted, the shape of the sintered body cannot be maintained, and conversely, if too little is melted, not enough liquid phase will spread between the solid particles, and especially in the case of aluminum (Al), the oxide film will not be destroyed sufficiently, resulting in poor sintering. Therefore, high precision is required in controlling the sintering temperature.

[0012] The melting point of a metal can be changed by adding other elements, even if it is the same metal. Specifically, the melting point can be changed by the type and amount of the added element. Therefore, the inventors have found that by mixing a high-melting-point metal powder in which the type or amount of the added element is changed and a low-melting-point metal powder in which the type or amount of the added element is changed, only the low-melting-point metal powder can be melted during sintering, and sintering can be performed without high-precision temperature control and without causing sintering defects. When heated to the same temperature, a metal with a high melting point has a low liquid phase ratio, and a metal with a low melting point has a high liquid phase ratio. Therefore, the additive manufacturing material of the present invention can be easily additively manufactured, and can produce a molded body with high density and excellent shape retention.

[0013] The present invention is not limited to the embodiments described below, but may be modified within the scope of what a person skilled in the art can imagine, such as other embodiments, additions, modifications, or deletions, and is within the scope of the present invention as long as the functions and effects of the present invention are achieved in any aspect.

[0014] <Powder A> The powder A contains an alloy or a pure metal. In the present invention, "pure metal" means a single metal, and "alloy" means a metal-like material containing multiple elements.

[0015] The pure metal as the powder A is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include aluminum (Al), tungsten (W), titanium (Ti), molybdenum (Mo), niobium (Nb), silicon (Si), copper (Cu), tin (Sn), magnesium (Mg), iron (Fe), manganese (Mn), nickel (Ni), zinc (Zn), chromium (Cr), etc. Among these, the pure metal as the powder A is preferably aluminum.

[0016] The alloy as the powder A is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include alloys consisting of two or more metals selected from the group consisting of aluminum (Al), tungsten (W), titanium (Ti), molybdenum (Mo), niobium (Nb), silicon (Si), copper (Cu), tin (Sn), magnesium (Mg), iron (Fe), manganese (Mn), nickel (Ni), zinc (Zn), and chromium (Cr). Among these, the alloy as the powder A is preferably an aluminum alloy, more preferably an aluminum alloy containing at least one selected from the group consisting of silicon, magnesium, iron, and copper, and further preferably an Al-Cu alloy, an Al-Mn alloy, an Al-Mg alloy, an Al-Si alloy, an Al-Si-Mg alloy, an Al-Si-Cu alloy, an Al-Zn-Mg alloy, an Al-Li alloy, and an Al-Fe alloy, and particularly preferably an Al-Si alloy and an Al-Fe alloy.

[0017] When the powder A is the aluminum alloy, the content of the aluminum relative to the total mass of the aluminum alloy is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 96% by mass to 99% by mass, and more preferably 97% by mass to 99% by mass. When the content of the aluminum relative to the total mass of the aluminum alloy as the powder A is 96% by mass to 99% by mass, it becomes easier to control the liquid phase ratio at a low level compared to an aluminum alloy containing a high content of metals other than aluminum, and the shape retention of the sintered body can be improved.

[0018] When the powder A is the aluminum alloy, the content of the metal other than aluminum relative to the total mass of the aluminum alloy is not particularly limited, and can be appropriately selected depending on the purpose, as long as there is a temperature range in which the liquid phase ratio of the powder A relative to the total mass of the powder A is 30 mass% or less, and the liquid phase ratio of the powder B relative to the total mass of the powder B is 70 mass% or more.

[0019] When the aluminum alloy as the powder A is an Al-Si alloy, the content of the silicon relative to the total mass of the Al-Si alloy is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1% by mass to 4% by mass, and more preferably 1% by mass to 3% by mass. When the content of the silicon relative to the total mass of the Al-Si alloy as the powder A is 1% by mass to 4% by mass, it becomes easier to control the liquid phase ratio at a low level compared to an Al-Si alloy with a high Si composition, and the shape retention of the sintered body can be improved.

[0020] When the aluminum alloy as the powder A is an Al-Fe alloy, the content of the iron relative to the total mass of the Al-Fe alloy is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1% by mass to 3% by mass, and more preferably 1% by mass to 2% by mass. When the content of the iron relative to the total mass of the Al-Fe alloy as the powder A is 1% by mass to 3% by mass, it becomes easier to control the liquid phase ratio at a low level compared to an Al-Fe alloy with a high Fe composition, and the shape retention of the sintered body can be improved.

[0021] <Powder B> The powder B contains an alloy having a different composition from that of the powder A. The alloy as the powder B is not particularly limited as long as it is an alloy having a different composition from that of the powder A, and can be appropriately selected depending on the purpose. For example, an alloy consisting of two or more metals selected from the group consisting of aluminum (Al), tungsten (W), titanium (Ti), molybdenum (Mo), niobium (Nb), silicon (Si), copper (Cu), tin (Sn), magnesium (Mg), iron (Fe), manganese (Mn), nickel (Ni), zinc (Zn), and chromium (Cr) can be mentioned. Among these, the alloy as the powder B is preferably an aluminum alloy, more preferably an aluminum alloy containing at least one selected from the group consisting of silicon, magnesium, iron, and copper, further preferably an Al-Cu alloy, an Al-Mn alloy, an Al-Mg alloy, an Al-Si alloy, an Al-Si-Mg alloy, an Al-Si-Cu alloy, an Al-Zn-Mg alloy, an Al-Li alloy, or an Al-Fe alloy, and particularly preferably an Al-Si alloy, an Al-Cu alloy, or an Al-Si-Mg alloy.

[0022] When the powder B is the aluminum alloy, the content of the aluminum relative to the total mass of the aluminum alloy is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 86% by mass to 92% by mass, more preferably 88% by mass to 90% by mass, relative to the total mass of the aluminum alloy. When the content of the aluminum relative to the total mass of the aluminum alloy as the powder B is 86% by mass to 92% by mass, complete melting occurs at a lower temperature, making it easier to densify the sintered body.

[0023] When Powder B is the aluminum alloy, the content of the metal other than aluminum relative to the total mass of the aluminum alloy is not particularly limited, and can be appropriately selected depending on the purpose, as long as there is a temperature range in which the liquid phase ratio of Powder A relative to the total mass of Powder A is 30 mass% or less, and the liquid phase ratio of Powder B relative to the total mass of Powder B is 70 mass% or more.

[0024] When the aluminum alloy as the powder B is an Al-Si alloy or an Al-Si-Mg alloy, the content of the silicon relative to the total mass of the Al-Si alloy or Al-Si-Mg alloy is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 8% by mass to 14% by mass, more preferably 10% by mass to 12% by mass. When the content of the silicon relative to the total mass of the Al-Si alloy or Al-Si-Mg alloy as the powder B is 8% by mass to 14% by mass, complete melting occurs at a lower temperature, and the sintered body can be easily densified.

[0025] When the aluminum alloy is an Al-Cu alloy, the content of copper relative to the total mass of the Al-Cu alloy is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 25% by mass to 35% by mass, and more preferably 30% by mass to 33% by mass. When the content of copper relative to the total mass of the Al-Cu alloy as powder B is 25% by mass to 35% by mass, complete melting occurs at a lower temperature, making it easier to densify the sintered body.

[0026] When the aluminum alloy is an Al-Si-Mg alloy, the content of the magnesium relative to the total mass of the Al-Si-Mg alloy is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.1% by mass to 3% by mass, and more preferably 0.2% by mass to 1% by mass. When the content of the magnesium relative to the total mass of the Al-Si-Mg alloy as the powder B is 0.1% by mass to 3% by mass, the sintered body is easily densified because it is completely melted at a lower temperature. Furthermore, the mechanical strength is increased compared to alloys that do not contain magnesium.

[0027] In addition, it is preferable that at least one of the powder A and the powder B of the additive manufacturing material contains the aluminum alloy or consists of the aluminum alloy, in terms of reducing the weight of the sintered part and improving the thermal conductivity.

[0028] <<Liquid phase ratio>> The additive manufacturing material has a temperature range in which the liquid phase ratio of powder A relative to the total mass of powder A is 30 mass% or less, and the liquid phase ratio of powder B relative to the total mass of powder B is 70 mass% or more.

[0029] The additive manufacturing material is made by mixing the powder A, in which the liquid phase ratio of the powder A is 30% by mass or less relative to the total mass of the powder A, with the powder B, in which the liquid phase ratio of the powder B is 70% by mass or more relative to the total mass of the powder B, so that during sintering, a state in which the powder B starts to melt but the powder A is hardly melted can be easily created without high-precision control of the sintering temperature, making it difficult for molding defects and sintering defects to occur. As described above, the powder A and the powder B only need to have different melting states during sintering, so there is no particular limit to the lower limit of the liquid phase ratio of the powder A relative to the total mass of the powder A, and it may be 0% by mass. Similarly, there is no particular limit to the upper limit of the liquid phase ratio of the powder B relative to the total mass of the powder B, and it may be 100% by mass.

[0030] In the present invention, the liquid phase ratios of the powder A and the powder B can be obtained by simulation using thermodynamic calculation software (CaTCalc, manufactured by the Institute of Computational Thermodynamics, Inc.). Specifically, the liquid phase ratios of the powder A and the powder B can be calculated by inputting the metal composition, temperature range, and pressure of the additive manufacturing material into the thermodynamic calculation software. For example, when "Al: 100 mass%" is input as a parameter for the powder A as the metal composition, "Al: 88 mass%" and "Si: 12 mass%" are input as parameters for the powder B, "550°C to 700°C" is input as the temperature range, and "101,325 Pa" is input as the pressure, the calculation result shown in FIG. 9A can be obtained.

[0031] As a method for determining the liquid phase ratio of the powder A and the powder B without using the simulation, there is a method in which the liquid phase portion is fixed by rapidly solidifying a metal in a semi-molten state, and the liquid phase ratio is calculated by observing the cross-sectional structure under a microscope. However, this method requires very fast cooling to fix the cross-sectional structure, making it difficult to measure with high accuracy. Furthermore, it has the disadvantage that it cannot be applied to metals whose liquid phase portion cannot be clearly determined from the cross-sectional structure, and that it takes a lot of man-hours to obtain the desired data. On the other hand, the simulation can calculate the liquid phase ratio quickly and accurately for any metal. Therefore, it is optimal to determine the liquid phase ratio of the powder A and the powder B in the present invention by the simulation.

[0032] <<particle size>> The ratio of the powder having a particle size of 106 μm or more in the powder A is not particularly limited and can be appropriately selected according to the purpose, but is preferably less than 10 mass%. When the ratio of the powder having a particle size of 106 μm or more in the powder A is less than 10 mass%, it is possible to mold the sintered precursor with a narrow lamination pitch, and the dimensional accuracy of the sintered body is improved. Furthermore, since the ratio of large particle diameter particles is small, the number of particle contact points in the sintered precursor increases, and the relative density of the sintered body increases. Thus, the ratio of the powder having a particle size of 106 μm or more in the powder A is preferably as small as possible, so the lower limit of the ratio of the powder having a particle size of 106 μm or more in the powder A is not particularly limited and may be 0 mass%.

[0033] The ratio of the powder having a particle size of 106 μm or more in the powder B is not particularly limited and can be appropriately selected according to the purpose, but is preferably less than 10 mass%. When the ratio of the powder having a particle size of 106 μm or more in the powder B is less than 10 mass%, it is possible to mold the sintered precursor with a narrow lamination pitch, and the dimensional accuracy of the sintered body is improved. Furthermore, since the ratio of large particle diameter particles is small, the number of particle contact points in the sintered precursor increases, and the relative density of the sintered body increases. Thus, the ratio of the powder having a particle size of 106 μm or more in the powder B is preferably as small as possible, so the lower limit of the ratio of the powder having a particle size of 106 μm or more in the powder B is not particularly limited and may be 0 mass%.

[0034] It is more preferable that the proportion of powder having a particle size of 106 μm or more in the powder A is less than 10 mass %, and the proportion of powder having a particle size of 106 μm or more in the powder B is less than 10 mass %. Since the proportion of powder having a particle size of 106 μm or more in both the powder A and the powder B is less than 10 mass %, it is possible to mold the sintered precursor with a narrow layer pitch, and the dimensional accuracy of the sintered body is improved. Furthermore, since the proportion of large particle diameter particles is small, the number of particle contact points in the sintered precursor increases, and the relative density of the sintered body increases.

[0035] The proportion of powder having a particle size of 106 μm or more in the powder A and the proportion of powder having a particle size of 106 μm or more in the powder B can be confirmed, for example, by a sieve test.

[0036] In the present invention, the "relative density" of the sintered precursor and the sintered body is a relative density measured by the Archimedes method.

[0037] The particle size of the powder A is not particularly limited and can be appropriately selected according to the purpose, but the median diameter (d50) is preferably 25 μm or more and 80 μm or less, more preferably 35 μm or more and 55 μm or less, and even more preferably 45 μm or more and 55 μm or less. When the median diameter of the powder A is 25 μm or more, there is an advantage that the fluidity of the powder A during recoating is improved and the relative density of the sintered precursor is easily improved. In addition, when the median diameter of the powder A is 80 μm or less, there is an advantage that the sintered precursor can be molded with a narrow layer pitch and the dimensional accuracy of the sintered body is improved. Furthermore, when the median diameter of the powder A is 80 μm or less, the number of particle contacts in the sintered precursor increases, and the relative density of the sintered body increases.

[0038] The particle size of the powder B is not particularly limited and can be appropriately selected according to the purpose, but the median diameter (d50) is preferably 20 μm or more and 80 μm or less, more preferably 20 μm or more and 50 μm or less, and even more preferably 20 μm or more and 30 μm or less. When the median diameter of the powder B is 20 μm or more, there is an advantage that the fluidity of the powder B during recoating is improved and the relative density of the sintered precursor is easily improved. In addition, when the median diameter of the powder B is 80 μm or less, there is an advantage that the sintered precursor can be molded with a narrow layer pitch and the dimensional accuracy of the sintered body is improved. Furthermore, when the median diameter of the powder B is 80 μm or less, the number of particle contacts in the sintered precursor increases, and the relative density of the sintered body increases.

[0039] The median diameter (d50) of the powder A and the powder B can be measured, for example, by a particle size distribution measuring device (for example, Microtrac MT3000II series, manufactured by Microtrac Bell).

[0040] -First aspect (median diameter of powder A>median diameter of powder B)- In the first aspect, it is preferable that the median diameter of the powder A is larger than that of the powder B. When the median diameter of the powder A is larger than that of the powder B, the relative density of the sintered body is increased when the powder B is arranged between the powders A and the additive manufacturing material is sintered. In addition, the relative density and dimensional accuracy of the sintered body are improved by uniformly arranging the powder B, which generates a liquid phase.

[0041] The ratio of the median diameter of the powder A to the median diameter of the powder B [median diameter of powder A: median diameter of powder B] is not particularly limited and can be appropriately selected according to the purpose, but is preferably 1:0.3 to 1:0.7. When the ratio [median diameter of powder A: median diameter of powder B] is 1:0.3 to 1:0.7, when the powder B is arranged between the powders A and the additive manufacturing material is sintered, the relative density of the sintered body becomes higher. In addition, by uniformly arranging the powder B that generates a liquid phase, the relative density and dimensional accuracy of the sintered body are further improved.

[0042] Furthermore, it is preferable that the median diameter of the powder A is 45 μm or more and 55 μm or less, and the median diameter of the powder B is 20 μm or more and 30 μm or less. As a result, when the powder B is arranged between the powders A and the additive manufacturing material is sintered, the relative density of the sintered body is further increased. Furthermore, by uniformly arranging the powder B, which generates a liquid phase, the relative density and dimensional accuracy of the sintered body are further improved.

[0043] -Second embodiment (median diameter of powder A<median diameter of powder B)- In a second aspect, the median diameter of the powder B is preferably larger than that of the powder A. When the median diameter of the powder B is larger than that of the powder A, the oxide film thickness relative to the particle volume of the powder B is relatively thin, so that the oxide film is easily broken when the powder B is liquidized, and when the additive manufacturing material is sintered, the relative density of the sintered body is high.

[0044] <<Content>> The volume of the powder B relative to the total volume of the additive manufacturing material is not particularly limited and can be appropriately selected according to the purpose, but is preferably 5% by volume or more, more preferably 10% by volume or more, and even more preferably 15% by volume or more and 25% by volume or less. When the volume of the powder B relative to the total volume of the additive manufacturing material is 5% by volume or more, the content ratio of the powder B that generates a liquid phase increases, and when the additive manufacturing material is sintered, the relative density of the sintered body increases when the additive manufacturing material is sintered, and when the volume is 10% by volume or more, the liquid phase generated during sintering increases, so that when the additive manufacturing material is sintered, the relative density of the sintered body increases, and when the volume is 15% by volume or more and 25% by volume or less, the relative density of the sintered body increases further when the additive manufacturing material is sintered. In addition, when the volume of the powder B relative to the total volume of the additive manufacturing material is 25% by volume or less, the liquid phase generated during sintering does not become too large, and the shape of the sintered body can be favorably maintained.

[0045] <Other ingredients> The other components are not particularly limited as long as they do not impair the effects of the present invention and can be appropriately selected depending on the purpose, and examples thereof include additives such as deterioration inhibitors, fluidizing agents, reinforcing agents, flame retardants, plasticizers, thermal stability additives, crystal nucleating agents, polymer particles such as amorphous resins, etc. These may be used alone or in combination of two or more.

[0046] The content of the other components in the additive manufacturing material is not particularly limited as long as it does not impair the effects of the present invention, and can be appropriately selected depending on the purpose.

[0047] (Additive manufacturing method and additive manufacturing device) The additive manufacturing method of the present invention includes a powder layer formation step of forming a powder layer using the additive manufacturing material of the present invention containing at least powder A and powder B, a powder layer solidification step of applying a resin liquid containing at least a resin to the powder layer and solidifying the powder layer, a sintered precursor preparation step of repeating the powder layer formation step and the powder layer solidification step to prepare a sintered precursor, and a sintering step of sintering the sintered precursor in a temperature range where the liquid phase ratio of powder A to the total mass of powder A is 30 mass% or less and the liquid phase ratio of powder B to the total mass of powder B is 70 mass% or more, and further includes other steps as necessary. The additive manufacturing method of the present invention is suitably carried out by the additive manufacturing apparatus of the present invention.

[0048] The additive manufacturing apparatus of the present invention comprises a powder layer forming means for forming a powder layer using the additive manufacturing material of the present invention containing at least powder A and powder B, a powder layer solidifying means for applying a resin liquid containing at least a resin to the powder layer and solidifying the powder layer, and a sintering means for sintering the sintering precursor within a temperature range in which the liquid phase ratio of powder A to the total mass of powder A is 30 mass% or less and the liquid phase ratio of powder B to the total mass of powder B is 70 mass% or more, and further comprises other means as necessary.

[0049] The additive manufacturing apparatus of the present invention will be described below in conjunction with the additive manufacturing method of the present invention.

[0050] <Powder layer forming step and powder layer forming means> The powder layer formation step is a step of forming a powder layer using the additive manufacturing material of the present invention containing at least Powder A and Powder B. The powder layer forming means is a means for forming a powder layer using the additive manufacturing material of the present invention containing at least Powder A and Powder B. The powder layer forming step is suitably carried out by the powder layer forming means. The powder layer is preferably formed on a support.

[0051] -Support- The support is not particularly limited as long as it is capable of supporting the additive manufacturing material, and can be appropriately selected depending on the purpose. For example, a table having a surface for supporting the additive manufacturing material, a base plate, etc. can be mentioned.

[0052] The surface of the support, i.e., the surface on which the additive manufacturing material is placed, may be, for example, a smooth surface or a rough surface, and may be a flat surface or a curved surface, but it is preferable that the surface has low affinity with the resin when the resin in the additive manufacturing material dissolves.

[0053] It is preferable that the affinity between the mounting surface and the dissolved resin is lower than the affinity between the additive manufacturing material and the dissolved resin, in that the resulting additive product can be easily removed from the mounting surface.

[0054] << Formation of powder layer >> The method for disposing the additive manufacturing material on the support is not particularly limited and can be appropriately selected depending on the purpose. For example, suitable methods for disposing the additive manufacturing material in a thin layer include a method using a known counter rotation mechanism (counter roller) used in a selective laser sintering method; a method of spreading the additive manufacturing material into a thin layer using a member such as a brush, roller, or blade; a method of pressing the surface of the additive manufacturing material using a pressing member to spread it into a thin layer; and a method of using a known powder additive manufacturing device.

[0055] The additive manufacturing material can be deposited in a thin layer on the support using the counter-rotating mechanism (counter roller), the brush or blade, the pressing member, etc., for example, as follows. That is, the additive manufacturing material is placed on the support arranged in an outer frame (sometimes called a "mold", "hollow cylinder", "cylindrical structure", etc.) so as to be able to move up and down while sliding on the inner wall of the outer frame, using the counter rotation mechanism (counter roller), the brush, the roller, the blade, the pressing member, etc. In this case, when a support that can move up and down within the outer frame is used, the support is placed slightly below the upper end opening of the outer frame, that is, positioned below by the thickness of the powder layer, and the additive manufacturing material is placed on the support. In this way, the additive manufacturing material can be placed in a thin layer on the support.

[0056] <Powder layer solidification step and powder layer solidification means> The powder layer solidification step is a step of applying a resin liquid (hereinafter, sometimes referred to as a "modeling liquid") containing at least a resin to the powder layer, and solidifying the powder layer. The powder layer solidifying means is a means for applying a resin liquid containing at least a resin onto the powder layer, thereby solidifying the powder layer. The powder layer solidification step is suitably carried out by the powder layer solidification means.

[0057] In the powder layer solidifying step, the resin liquid is applied to the powder layer, thereby solidifying the powder layer.

[0058] -Resin liquid (modeling liquid)- The resin liquid is not particularly limited as long as it contains at least a resin, and can be appropriately selected depending on the purpose, and further contains other components as necessary. The resin liquid is used as a binder when sintering the additive manufacturing material and is also referred to as a "build liquid."

[0059] --resin-- The resin is not particularly limited and can be appropriately selected from known resins that can be used for sintering, and examples thereof include vinyl resins such as polyvinyl acetate resin, partially saponified polyvinyl acetate resin, polyvinyl butyral resin, etc. These may be used alone or in combination of two or more.

[0060] The content of the resin is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 5.0% by mass or more, more preferably 7.0% by mass or more, even more preferably 10.0% by mass or more, and particularly preferably 11.0% by mass or more, based on the total mass of the resin liquid. The content of the resin is preferably 30.0% by mass or less, more preferably 25.0% by mass or less, and even more preferably 20.0% by mass or less, based on the total mass of the resin liquid. When the content of the resin is 5.0% by mass or more and 30.0% by mass or less, the viscosity of the resin liquid can be made suitable for ejection by an inkjet method.

[0061] --Other ingredients-- The other components in the resin liquid are not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include surfactants, drying inhibitors, viscosity adjusters, penetrants, defoamers, pH adjusters, preservatives, antifungal agents, colorants (dyes, pigments, etc.), preservatives, stabilizers, etc. These may be used alone or in combination of two or more. As the other components, conventionally known materials can be used. The content of the other components is not particularly limited and can be appropriately selected depending on the purpose, but it is preferable that the total content of the other components is 10% by mass or less based on the total mass of the resin liquid.

[0062] ---solvent--- Examples of the solvent include n-octane, m-xylene, solvent naphtha, diisobutyl ketone, 3-heptanone, 2-octanone, acetylacetone, butyl acetate, amyl acetate, n-hexyl acetate, n-octyl acetate, ethyl butyrate, ethyl valerate, ethyl caprylate, ethyl octanoate, ethyl acetoacetate, ethyl 3-ethoxypropionate, diethyl oxalate, diethyl malonate, diethyl succinate, diethyl adipate, bis-2-ethylhexyl maleate, and triacetin. , tributyrin, propylene glycol monomethyl ether acetate, ethylene glycol monobutyl ether acetate, dibutyl ether, 1,2-dimethoxybenzene, 1,4-dimethoxybenzene, diethylene glycol monobutyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, 2-methoxy-1-methylethyl acetate, γ-butyrolactone, propylene carbonate, cyclohexanone, and butyl cellosolve. These may be used alone or in combination of two or more.

[0063] The content of the solvent is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 60.0% by mass or more and 95.0% by mass or less, and more preferably 70.0% by mass or more and 95.0% by mass or less, based on the total mass of the resin liquid. When the content of the solvent is 60.0% by mass or more and 95.0% by mass or less, the solubility of the resin is improved, and the viscosity of the resin liquid can be reduced accordingly, so that the resin liquid can be appropriately discharged, for example, by an inkjet method. In addition, the resin liquid is prevented from drying in the powder layer solidification means, and a resin liquid with excellent discharge stability can be provided.

[0064] <<Applying resin liquid to powder layer>> The method of applying the resin liquid to the powder layer is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include a dispenser method, a spray method, an inkjet method, etc. In addition, in order to carry out these methods, known devices can be suitably used as the powder layer solidifying means.

[0065] The dispenser method is excellent in terms of the quantity of droplets, but the coating area may become narrow. The spray method can easily form fine droplets, has a wide coating area, and is excellent in coating properties, but the quantity of droplets may be poor and the additive manufacturing material may be scattered by the spray flow. For this reason, the inkjet method is particularly preferred as a method for applying the resin liquid to the powder layer. The inkjet method is preferred in that it has the advantages of being able to apply droplets more quantitatively than the spray method, being able to apply a larger area than the dispenser method, and being able to form a complex three-dimensional shape with high precision and efficiency.

[0066] In the case of the application method using the inkjet method, the powder layer solidifying means may be a nozzle capable of applying the resin liquid to the powder layer by the inkjet method, or an inkjet printer having the nozzle. As the nozzle, a nozzle (ejection head) in a known ink jet printer can be suitably used. A suitable example of the inkjet printer is the SG7100 manufactured by Ricoh Co., Ltd. The inkjet printer is preferred in that a large amount of resin liquid can be dropped from the head at one time and the coating area is large, making it possible to increase the coating speed.

[0067] <Sintered precursor preparation step and sintered precursor preparation means> The sintered precursor preparation step is a step of repeating the powder layer formation step and the powder layer solidification step to prepare a sintered precursor. The sintered precursor producing means is a means for producing a sintered precursor by repeatedly carrying out the powder layer forming means and the powder layer solidifying means. The sintered precursor preparation step is suitably carried out by the sintered precursor preparation means.

[0068] The additive manufacturing material is placed in a thin layer on the sintered precursor (solidified material) of the thin layer obtained in the powder layer forming process in the same manner as described above, and the resin liquid is applied to the additive manufacturing material (powder layer) placed on the thin layer, causing hardening. Hardening at this time occurs not only in the additive manufacturing material (powder layer) placed on the thin layer, but also between the additive manufacturing material (powder layer) and the sintered precursor (solidified material) of the thin layer that was previously hardened and exists below it. As a result, a solidified material (sintered precursor) having a thickness of about two layers of the additive manufacturing material (powder layer) placed on the thin layer is obtained.

[0069] The additive manufacturing material can also be deposited in a thin layer on the support in an automated and convenient manner using the known powder additive manufacturing apparatus. The powder additive manufacturing apparatus generally includes a recoater, a mobile supply tank, and a mobile molding tank. The recoater deposits the additive manufacturing material. The mobile supply tank supplies the additive manufacturing material onto the support. The mobile molding tank deposits and deposits the additive manufacturing material in a thin layer. In the powder additive manufacturing apparatus, the surface of the movable supply tank can always be slightly higher than the surface of the movable molding tank by raising the movable supply tank or lowering the movable molding tank, or both, and the additive manufacturing material can be deposited in a thin layer from the movable supply tank side using the recoater, and thin layers of additive manufacturing material can be deposited by repeatedly moving the recoater.

[0070] The thickness of the additive manufacturing material layer is not particularly limited and can be appropriately selected depending on the purpose, but the average thickness per layer is preferably 20 μm or more and less than 200 μm, and more preferably 60 μm or more and 100 μm or less. When the average thickness of the additive manufacturing material layer is 20 μm or more, the strength of the solidified material (sintered precursor) of the additive manufacturing material layer formed by applying the resin liquid to the additive manufacturing material is sufficient, and problems such as deformation do not occur during subsequent processing or handling such as sintering. In addition, when the average thickness of the additive manufacturing material layer is less than 200 μm, the dimensional accuracy of the solidified material (sintered precursor) of the additive manufacturing material layer formed by applying the resin liquid to the additive manufacturing material is improved, and the stacking step does not become too large, making it difficult for sintering defects to occur.

[0071] The average thickness of the additive manufacturing material layer can be adjusted by inputting values ​​into the additive manufacturing device. The method for measuring the average thickness of the additive manufacturing material layer is not particularly limited and can be measured according to a known method.

[0072] <Degreasing process and degreasing means> The degreasing step is a step of degreasing the resin in the sintering precursor. The degreasing means is a means for degreasing the resin in the sintering precursor. The degreasing step is suitably carried out by the degreasing means.

[0073] By carrying out the degreasing step, the resin component in the solidified powder layer (sintered precursor) formed in the powder layer solidifying step is degreased. The resin component does not have to be completely degreased, i.e., the amount of the resin component remaining in the sintering precursor may be greater than 0% by mass. However, the closer the amount of the resin component remaining in the sintering precursor is to 0% by mass, the more preferable it is in terms of improving the density of the sintered body after sintering.

[0074] The degreasing means may be, for example, a known degreasing furnace.

[0075] The temperature in the degreasing step will be described with reference to FIG. FIG. 8 is a graph showing the relationship between the progress of the debinding and sintering steps in an additive manufacturing method according to an embodiment of the present invention and the temperature of a material for additive manufacturing according to an embodiment of the present invention. In the degreasing process, the resin component contained in the resin liquid is decomposed at a temperature higher than the thermal decomposition temperature of the resin and lower than the melting point or solidus temperature of the alloy or pure metal as the powder A in the additive manufacturing material and the alloy as the powder B. Depending on the resin component used, it is also possible to set multiple heating and holding temperatures. In addition, a degreasing method using solvent extraction in which the resin is extracted by immersing the sintering precursor in a solvent instead of heating can also be applied.

[0076] <Sintering process and sintering means> The sintering step is a step of sintering the degreased sintering precursor in a temperature range in which the liquid phase ratio of powder A relative to the total mass of powder A is 30 mass% or less, and the liquid phase ratio of powder B relative to the total mass of powder B is 70 mass% or more. The sintering means is a means for sintering the degreased sintering precursor in a temperature range in which the liquid phase ratio of powder A to the total mass of powder A is 30 mass% or less, and the liquid phase ratio of powder B to the total mass of powder B is 70 mass% or more. The sintering step is preferably carried out by the sintering means.

[0077] By carrying out the sintering step, the solidified powder layer (sintered precursor) formed in the powder layer solidifying step can be made into an integrated sintered metal body with increased density.

[0078] The sintering means may be, for example, a known sintering furnace. The degreasing step and the sintering step may be carried out continuously using the same degreasing / sintering furnace, or may be carried out in separate degreasing furnaces and sintering furnaces. However, in the sintering step, in order to adjust the temperature range so that the liquid phase ratio of Powder A relative to the total mass of Powder A is 30 mass% or less and the liquid phase ratio of Powder B relative to the total mass of Powder B is 70 mass% or more, each of the degreasing / sintering furnace, the degreasing furnace, and the sintering furnace must be temperature adjustable.

[0079] The temperature in the baking step will be described with reference to FIG. The temperature range of the firing step is a temperature range in which the liquid phase ratio of the powder A to the total mass of the powder A is 30 mass% or less, and the liquid phase ratio of the powder B to the total mass of the powder B is 70 mass% or more. The sintered precursor after the debinding step is heated to the above temperature range at a rate of 1°C / hour to 200°C / hour (the heating rate can be changed during the process), and then the temperature is maintained for about 1 hour to 10 hours. After heating and maintaining in the firing step in this manner, the inside of the furnace is cooled to obtain a fired body.

[0080] The atmospheric conditions for carrying out the degreasing step and the firing step are not particularly limited and can be appropriately selected depending on the purpose. However, it is preferable to carry out the steps under atmospheric conditions such as vacuum, argon (Ar), hydrogen (H2), or nitrogen (N2).

[0081] By carrying out the sintering process and the sintering means and sintering the sintering precursor within a temperature range in which the liquid phase ratio of powder A to the total mass of powder A is 30 mass% or less and the liquid phase ratio of powder B to the total mass of powder B is 70 mass% or more, the obtained additive product (sintered body) has high density and excellent shape retention.

[0082] <Other steps and other means> Examples of the other steps include a drying step, a surface protection treatment step, and a coating step. Examples of the other means include powder containing means, resin liquid containing means, drying means, surface protection treatment means, and coating means.

[0083] <<Powder Containing Means>> The powder containing means is a means for containing the additive manufacturing material. There are no particular limitations on the size, shape, material, etc. of the powder containing means, and these may be appropriately selected depending on the purpose. Examples of the powder containing means include a reservoir, a bag, a cartridge, and a tank.

[0084] <<Means for containing resin liquid>> The resin liquid containing means is a means for containing the resin liquid. The size, shape, material, etc. of the resin liquid containing means are not particularly limited and may be appropriately selected depending on the purpose. Examples of the resin liquid containing means include a reservoir, a bag, a cartridge, and a tank.

[0085] <<Drying process and drying means>> The drying step is a step of drying the solidified material (sintering precursor) obtained in the powder layer solidification step. In the drying step, not only the moisture contained in the solidified material but also organic matter may be removed (degreased).

[0086] The drying means is a means for drying the solidified material (sintering precursor) obtained in the powder layer solidification step. The drying means may be, for example, a known dryer.

[0087] <<Surface protection treatment process and surface protection treatment means>> The surface protection treatment step is a step of forming a protective layer on the surface of the solidified material (sintered precursor) formed in the powder layer solidification step. By carrying out this surface protection treatment step, it is possible to impart durability, etc., to the surface of the solidified material (sintered precursor), which allows the solidified material (sintered precursor) to be used as is, for example.

[0088] Specific examples of the protective layer include a water-resistant layer, a weather-resistant layer, a light-resistant layer, a heat-insulating layer, and a gloss layer.

[0089] The surface protection treatment means is a means for forming a protective layer on the surface of the solidified material (sintering precursor) formed in the powder layer solidification step.

[0090] The surface protection treatment means may be a known surface protection treatment device, such as a spray device or a coating device.

[0091] <<Painting process and painting method>> The coating process is a process for coating the solidified material (sintered precursor) formed in the powder layer solidification process. By carrying out the coating process, the solidified material (sintered precursor) can be colored in a desired color.

[0092] The coating means is a means for coating the solidified material (sintered precursor) formed in the powder layer solidification step.

[0093] The coating means may be a known coating device, such as a spray, roller, or brush coating device.

[0094] Here, an embodiment of the additive manufacturing material of the present invention and an additive manufacturing method and an additive manufacturing device for a BJT using the additive manufacturing material will be described in detail with reference to the drawings. Note that the BJT is an example of an additive manufacturing method, and additive manufacturing in the present invention is not limited to the BJT. In addition, in each drawing, the same components are denoted by the same reference numerals, and duplicated explanations may be omitted. Furthermore, the number, position, shape, etc. of the following components are not limited to the present embodiment, and may be any number, position, shape, etc. that is preferable for implementing the present invention.

[0095] Figure 1 is a schematic cross-sectional view of an additive manufacturing apparatus according to an embodiment of the present invention. Figure 2 is a schematic side view of the additive manufacturing apparatus of Figure 1. Figure 3 is a schematic cross-sectional view of a modeling section of the additive manufacturing apparatus of Figure 1. Figure 4 is a schematic perspective view of the additive manufacturing apparatus of Figure 1. Figure 5A is a schematic perspective view of a powder bath of the additive manufacturing apparatus of Figure 1. Figure 5B is a schematic perspective view of a supply bath and a modeling bath of the additive manufacturing apparatus of Figure 1.

[0096] The additive manufacturing apparatus, also known as a powder modeling apparatus, includes a modeling section 1 in which a modeling layer 30, which is a layered object formed by combining additive manufacturing materials (containing at least powder A and powder B), is formed, and a modeling unit 5 that ejects modeling liquid (resin liquid) 10 onto the powder layer 31 spread in layers in the modeling section 1 to form an additive product.

[0097] The modeling section 1 includes a powder tank 11 and a flattening roller 12 as a rotating body that is a flattening member (recoater). The flattening member may be, for example, a plate-like member (blade) instead of the rotating body.

[0098] The powder tank 11 has a supply tank 21 and a modeling tank 22. The supply tank 21 supplies the additive manufacturing material 20. In the modeling tank 22, modeling layers 30 are stacked to form an additive product. The bottom of the supply tank 21 serves as a supply stage 23 and can be raised and lowered in the vertical direction (height direction). Similarly, the bottom of the modeling tank 22 serves as a modeling stage 24 and can be raised and lowered in the vertical direction (height direction). An additive product is formed by stacking modeling layers 30 on the modeling stage 24. For example, as shown in FIG. 4, the supply stage 23 is raised and lowered in the direction of the arrow Z (height direction) by a motor 27, and the modeling stage 24 is similarly raised and lowered in the direction of the arrow Z by a motor 28.

[0099] As shown in Fig. 5A, a powder drop port 29 having a concave shape with an open top is provided around the powder tank 11 (omitted in Figs. 1 to 3). Excess additive manufacturing material 20 from the additive manufacturing material 20 supplied by the flattening roller 12 when forming the powder layer 31 falls into the powder drop port 29. The excess additive manufacturing material 20 that has fallen into the powder drop port 29 is returned to a powder supply device 554 (described later) that supplies additive manufacturing material to the supply tank 21.

[0100] 6 is placed on the supply tank 21. During the initial operation of modeling or when the amount of powder in the supply tank 21 decreases, the additive manufacturing material 20 in the tank constituting the powder supply device 554 is supplied to the supply tank 21. Examples of powder transport methods for supplying the additive manufacturing material include a screw conveyor method using a screw and a pneumatic transport method using air.

[0101] The flattening roller 12 supplies the additive manufacturing material 20 supplied onto the supply stage 23 of the supply tank 21 to the modeling tank 22, and flattens and smooths the material by the flattening roller 12, which is a flattening member, to form a powder layer 31. The flattening roller 12 is disposed so as to be movable back and forth relative to the stage surface in the direction of arrow Y in FIG. 4 along the stage surface (the surface on which the additive manufacturing material 20 is loaded) of the modeling stage 24, and is moved by a reciprocating mechanism 25. The flattening roller 12 is also driven to rotate by a motor 26.

[0102] 3, a powder removal plate 13 is disposed in contact with the circumferential surface of the flattening roller 12, which is a powder removal member for removing additive manufacturing material 20 adhering to the flattening roller 12. The powder removal plate 13 moves together with the flattening roller 12 while in contact with the circumferential surface of the flattening roller 12. The powder removal plate 13 is disposed in a state in which it is in a counter direction when the flattening roller 12 rotates in the rotation direction in which the flattening roller 12 performs flattening.

[0103] In this embodiment, the powder tank 11 of the modeling section 1 is configured to have two tanks, a supply tank 21 and a modeling tank 22, but it can also be configured to have only the modeling tank 22, with additive manufacturing material supplied to the modeling tank 22 from a powder supply device and flattened by a flattening means.

[0104] The modeling unit 5 includes a liquid discharge unit 50. The liquid discharge unit 50 discharges modeling liquid 10 onto the powder layer 31 on the modeling stage 24. The modeling unit 5 has a slider portion 72 movably held by a guide member 71 disposed on the base member 7, and the entire modeling unit 5 can reciprocate in a Y direction (sub-scanning direction) perpendicular to the X direction. The entire modeling unit 5 is reciprocated in the Y direction by a Y-direction scanning mechanism 552, which will be described later.

[0105] 1, the liquid ejection unit 50 includes a carriage 51 and two (or may be one or more) liquid ejection heads (hereinafter, may be simply referred to as "heads") 52a and 52b mounted on the carriage 51. The liquid ejection unit 50 is arranged so as to be able to rise and fall in the direction of the arrow Z in FIG. 2 together with guide members 54 and 55, and is raised and lowered in the Z direction by a Z-direction lifting mechanism 551 described later.

[0106] The two heads 52a and 52b (hereinafter, when there is no need to distinguish between them, they may be simply referred to as "heads 52") each have two nozzle rows in which a plurality of nozzles that eject the modeling liquid are arranged. Note that the head configuration is not limited to this. A tank 60 containing the modeling liquid is attached to the tank attachment portion 56, and the modeling liquid is supplied to the heads 52a and 52b via a supply tube or the like.

[0107] An overview of the control unit of an additive manufacturing device will be described with reference to Fig. 6. Fig. 6 is a block diagram showing the control unit of an additive manufacturing device according to an embodiment of the present invention. The control unit 500 includes a main control unit 500A including a CPU 501 that controls the entire additive manufacturing apparatus, a ROM 502 that stores programs including programs for causing the CPU 501 to execute control of additive manufacturing operations including the control according to the present invention and other fixed data, and a RAM 503 that temporarily stores modeling data and the like. The control unit 500 also includes a non-volatile memory (NVRAM) 504 for retaining data even when the power to the apparatus is cut off.

[0108] The control unit 500 includes an ASIC 505 that processes input / output signals for image processing that performs various signal processing on image data and other control of the entire device. The control unit 500 also includes an I / F 506 that transmits and receives data and signals used when receiving shaping data from an external shaping data creation device 600. The shaping data creation device 600 is a device that creates shaping data in which a final shaped object is sliced ​​into each shaping layer, and is configured with an information processing device such as a personal computer. The control unit 500 also includes an I / O 507 that receives detection signals from various sensors. The control unit 500 also includes a head drive control unit 508 that drives and controls the heads 52a and 52b of the liquid ejection unit 50.

[0109] The control unit 500 includes a motor drive unit 510 that drives a motor constituting an X-direction scanning mechanism 550 that moves the carriage 51 of the liquid discharge unit 50 in the X-direction (main scanning direction), and a motor drive unit 512 that drives a motor constituting a Y-direction scanning mechanism 552 that moves the modeling unit 5 in the Y-direction (sub-scanning direction). The control unit 500 includes a motor drive unit 511 that drives a motor constituting a Z-direction lifting mechanism 551 that moves (lifts and lowers) the carriage 51 of the liquid discharge unit 50 in the Z-direction. Note that the lifting in the arrow Z direction may be configured to lift and lower the entire modeling unit 5. The control unit 500 includes a motor drive unit 513 that drives a motor 27 that lifts and lowers the supply stage 23, and a motor drive unit 514 that drives a motor 28 that lifts and lowers the modeling stage 24. The control unit 500 includes a motor drive unit 515 that drives the motor 553 of the reciprocating mechanism 25 that moves the flattening roller 12 , and a motor drive unit 516 that drives the motor 26 that drives the flattening roller 12 to rotate.

[0110] The control unit 500 also includes a supply system drive unit 517 that drives a powder supply device 554 that supplies additive manufacturing material 20 to the supply tank 21, and a maintenance drive unit 518 that drives a maintenance mechanism 61 of the liquid discharge unit 50. Detection signals from a temperature and humidity sensor 560 that detects temperature and humidity as environmental conditions of the device and other sensors are input to the I / O 507 of the control unit 500. An operation panel 522 for inputting and displaying information required for this device is connected to the control unit 500. The modeling data creation device 600 and the additive manufacturing device (powder additive manufacturing device) 601 constitute an additive manufacturing system as an additive manufacturing device according to the present invention.

[0111] Next, the flow of modeling will be described with reference to Figures 7A to 7E. Figures 7A to 7E are schematic cross-sectional views showing the flow of modeling operations in a modeling unit of an additive manufacturing apparatus according to one embodiment of the present invention. The following description will start from a state where the first modeling layer 30 is formed on the modeling stage 24 of the modeling tank 22. When forming the next modeling layer 30 on this modeling layer 30, as shown in FIG. 7A, the supply stage 23 of the supply tank 21 is raised in the Z1 direction, and the modeling stage 24 of the modeling tank 22 is lowered in the Z2 direction. At this time, the lowering distance of the modeling stage 24 is set so that the interval between the upper surface (powder layer surface) of the modeling tank 22 and the lower part (lower tangent part) of the flattening roller 12 is Δt1. This interval Δt1 corresponds to the thickness of the powder layer 31 to be formed next. The interval Δt1 is preferably 20 μm or more and less than 200 μm.

[0112] Next, as shown in Figure 7B, the additive manufacturing material 20 located above the top surface level of the supply tank 21 is transported and supplied to the modeling tank 22 by moving the flattening roller 12 in the Y2 direction (towards the modeling tank 22) while rotating in the forward direction (the direction of the arrow in Figure 7B).

[0113] Furthermore, as shown in FIG. 7C, the flattening roller 12 is moved parallel to the stage surface of the modeling stage 24 of the modeling tank 22, and as shown in FIG. 7D, a powder layer 31 having a predetermined thickness Δt1 is formed on the modeling layer 30 of the modeling stage 24 (powder layer forming process). After forming the powder layer 31, the flattening roller 12 is moved in the Y1 direction and returned to the initial position, as shown in FIG. 7D. Here, the flattening roller 12 is adapted to move while maintaining a constant distance from the upper surface levels of the modeling tank 22 and the supply tank 21. Since the flattening roller 12 can move while maintaining a constant distance from the upper surface levels of the modeling tank 22 and the supply tank 21, the flattening roller 12 can transport the additive manufacturing material 20 onto the modeling tank 22, while forming a powder layer 31 of a uniform thickness Δt1 on the modeling tank 22 or on the already formed modeling layer 30.

[0114] After that, as shown in FIG. 7E, droplets of the modeling liquid 10 are discharged from the head 52 of the liquid discharge unit 50 to form a modeling layer 30 on the next powder layer 31 (powder layer solidification process). The modeling layer 30 is formed, for example, when the modeling liquid 10 ejected from the head 52 is mixed with the additive manufacturing material 20, causing the adhesive contained in the additive manufacturing material 20 to dissolve, and the dissolved adhesives bond together to bond the additive manufacturing material 20.

[0115] Next, the above-mentioned process of forming the powder layer 31 by supplying powder and flattening (powder layer forming process) and the process of discharging the modeling liquid by the head 52 (powder layer solidifying process) are repeated to form a new modeling layer 30. At this time, the new modeling layer 30 and the modeling layer 30 below it are integrated to form a part of the three-dimensional shaped object.

[0116] (Powder container) The powder-containing container of the present invention is formed by filling the additive manufacturing material of the present invention into the container. The container is not particularly limited, and its shape, structure, size, material, etc. can be appropriately selected depending on the purpose. Examples of the container include a powder-containing bag, a powder-containing cartridge, a powder-containing tank, etc., formed of an aluminum laminate film, a resin film, etc. EXAMPLES

[0117] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these examples. In the following examples and comparative examples, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".

[0118] <<How to measure d50 of powder>> In the following Examples 1 to 14 and Comparative Examples 1 and 2, the median diameters (d50) of Powder A and Powder B were measured with a particle size distribution measuring device (Microtrac MT3000II series, manufactured by Microtrac Bell). The results are shown in the following Tables 1 to 4.

[0119] <<Method for measuring the percentage of powder particles with particle sizes of 106 μm or more>> In the following Examples 1 to 14 and Comparative Examples 1 and 2, the proportion of powder A and powder B having a particle size of 106 μm or more was measured by a sieve test. The sieve test was carried out based on the method specified in ISO 2591-1:1988 (Test sieving - Part 1). A sieve with 106 μm openings (test sieve, manufactured by Kansai Wire Mesh Co., Ltd.) was placed on top of the powder receiver. The test powder was placed on top of the sieve and covered. The sieve was attached to a sieving device (low tap type sieve shaker, manufactured by Iida Seisakusho Co., Ltd.), and the device was operated at a rotation speed of 60 Hz for 10 minutes to perform sieving. The mass ratio of the powder remaining on the 106 μm opening sieve to the total powder charged was defined as the "ratio of powder with a particle size of 106 μm or more." The results are shown in Tables 1 to 4 below.

[0120] <<Changes in liquid phase ratio with temperature for powder A and powder B>> In the following Examples 1 to 14 and Comparative Examples 1 and 2, a simulation of the change in the liquid phase ratio with respect to the temperature of Powder A and Powder B was carried out using thermodynamic calculation software (CaTCalc, manufactured by Computational Thermodynamics Institute, Inc.). Specifically, the composition of the metal of the additive manufacturing material, the temperature range, and the pressure were inputted into the thermodynamic calculation software, and the liquid phase ratio was calculated. In the calculation in Example 1, as the metal composition, "Al: 100 mass%" was inputted as a parameter for Powder A, "Al: 88 mass%" and "Si: 12 mass%" were inputted as parameters for Powder B, "550°C to 700°C" was inputted as a temperature range, and "101,325 Pa" was inputted as a pressure. In Examples 2 to 13 and Comparative Examples 1 to 3, calculations were performed in the same manner, except that the parameters for Powder A and the parameters for Powder B were changed to parameters based on the compositions shown in Tables 1 to 4 below. The results are shown in Tables 1 to 4 below.

[0121] <<Evaluation of sintered precursors and sintered bodies>> In the following Examples 1 to 14 and Comparative Examples 1 and 2, the "relative density of the sintered precursor," the "relative density of the fired body," and the "deformation amount of the fired body" were evaluated by the following methods. The results are shown in Table 5 below.

[0122] -Method for measuring the relative density of sintered precursors and sintered bodies- The relative densities of the sintered precursor and the sintered body were measured by the Archimedes method.

[0123] -Evaluation of deformation of sintered body- FIG. 10A is a schematic oblique view showing the shapes of the sintered precursors formed in Examples 1 to 14 and Comparative Examples 1 to 2, FIG. 10B is a schematic front view showing the shapes of the sintered precursors formed in Examples 1 to 14 and Comparative Examples 1 to 2, and FIG. 10C is a schematic front view showing the shapes of the sintered bodies of Examples 1 to 14 and Comparative Examples 1 to 2, and is an explanatory diagram of a method for evaluating the deformation amount of the sintered bodies. 10A and 10B, when the sintered precursor having blocks 102 attached to both ends of a thin and long pipe portion 101 formed in Examples 1 to 14 and Comparative Examples 1 and 2 was sintered, the pipe portion 101 was bent downward due to its own weight. As shown in Fig. 10C, the amount of bending Δh of the pipe portion 101 was used as an index of the deformation amount (mm) of the sintered body. The deflection amount Δh was expressed as the absolute value of the length between imaginary lines U and L drawn as follows, measured using a dial gauge (ID-C125XB, manufactured by Mitutoyo Corporation). (1) When observing the object from directly in front, the height of an imaginary line U connecting the uppermost end 101a of the pipe section 101 that contacts one block section 102 and the uppermost end 101b of the pipe section 101 that contacts the other block section 102 was set to "0 mm." (2) The imaginary line L is the line that passes through the point 101c at the top end of the pipe section 101 where the deflection occurs, the point 101c being the maximum distance from the imaginary line U, and is parallel to the imaginary line U.

[0124] Example 1 <Production of materials for additive manufacturing> A mixed powder of the following powder A and powder B was used as the additive manufacturing material. Powder A: Pure Al (manufactured by Toyo Aluminum Co., Ltd., d50: 35 μm, the proportion of powder with a particle size of 106 μm or more is less than 0.1 mass%) Powder B: AlSi12 (manufactured by Toyo Aluminum Co., Ltd., d50: 35 μm, the proportion of powder with a particle size of 106 μm or more is less than 0.1% by mass) In addition, "AlSi12" refers to "Al-12% by mass Si alloy." Below, other alloy types are also denoted in the same way.

[0125] Powder A and powder B were placed in a bead mill (DYNO-MILL, manufactured by Shinmaru Enterprises, Inc.) so that the ratio of powder B to the total volume of the mixed powder of powder A and powder B was 20 volume %. The mill was operated at 100 rpm for 5 minutes to prepare [Additive Manufacturing Material 1].

[0126] <Preparation of modeling liquid> 88% by mass of partially saponified polyvinyl acetate resin (JMR-10LL, manufactured by Nippon Vinylon Co., Ltd.) as a binder (indicating the total amount, not the resin solids content) and 12% by mass of triethylene glycol dimethyl ether were mixed and dissolved by stirring with a magnetic stirrer for 2 hours while heating at 80 °C. After stirring, the solution was passed through a 1-μm filter to prepare a shaping liquid.

[0127] <Manufacture of Sintering Precursor> [Additive Manufacturing Material 1] was leveled by recoating so that the layer thickness (also referred to as "lamination pitch") became 84 μm (powder layer formation step). Next, the shaping liquid prepared in the shaping region was dropped by a liquid ejection head (powder layer solidification step). The powder layer formation step and the powder layer solidification step were repeated to shape [Sintering Precursor 1] in the shape where block portions 102 of a cube with a side length of 20 mm were attached to both ends of an elongated pipe portion 101 with a length of 80 mm and a diameter of 4 mm as shown in FIGS. 10A and 10B.

[0128] <Manufacture of Sintered Body> Thereafter, while [Sintering Precursor 1] was buried in the excess mixed powder that had not been cured (hereinafter sometimes referred to as "excess powder"), it was placed in a vacuum dryer (DP610P, manufactured by Yamato Scientific Co., Ltd.) and heated at 100 °C in a reduced-pressure atmosphere (gauge pressure -0.1 MPa). The dried sintering precursor was blasted with air to remove the adhering excess powder. The sintering precursor from which the excess powder had been removed was placed in a small vacuum sintering furnace (manufactured by DOWA Thermotech Co., Ltd.) and degreased by holding at a temperature equal to or higher than the temperature at which the binder thermally decomposes and lower than the eutectic temperature (577 °C) of AlSi12. The temperature was further raised and sintered by holding at 600 °C within the temperature range of 577 °C < T < 660 °C to form [Sintered Body 1].

[0129] -Evaluation Results- Figure 9A is a graph showing the results of calculating the change in the liquid-phase ratio with respect to temperature for powder A (pure Al) and powder B (AlSi12) of Example 1 using thermodynamic calculation software (CaTCalc). From this calculation, the temperature T at which the liquid-phase ratio of powder A (pure Al) is 30 mass% or less and the liquid-phase ratio of powder B (AlSi12) is 70 mass% or more was in the range of 577 °C < T < 660 °C. From this, it was found that by setting the sintering temperature within the above range, most of powder A (pure Al) acts as a solid-phase skeleton, while most of powder B (AlSi12) liquefies and fills the voids between the skeletons. Also, the liquid-phase ratio of pure Al at the sintering temperature of 600 °C of [Sintered Body 1] was 0 mass%, and the liquid-phase ratio of AlSi12 at the sintering temperature of 600 °C of [Sintered Body 1] was 100 mass%.

[0130] The relative density of the pre-sintered body in Example 1 was 56%, and the relative density of the sintered body was 92%. Since the sintered body had a high density, at the sintering temperature, the effect that AlSi12 liquefied and filled the voids between pure Al, densifying the sintered body was shown.

[0131] The amount of deformation of the sintered body in Example 1 was as small as 0.2 mm. From this, at the sintering temperature, while AlSi12 liquefied, pure Al remained in the solid phase and acted as a skeleton, showing the effect of suppressing sintering deformation.

[0132] (Comparative Example 1) In the <Manufacture of Material for Additive Manufacturing> of Example 1, [Material for Additive Manufacturing 15] was prepared in the same manner as in Example 1, except that only powder A (pure Al, manufactured by Toyo Aluminum Co., Ltd., d50: 35 μm, the ratio of powder with a particle size of 106 μm or more being less than 0.1 mass%) was used instead of using the mixed powder of powder A and powder B, and [Pre-sintered Body 15] and [Sintered Body 15] were formed using this [Material for Additive Manufacturing 15].

[0133] -Evaluation Results- The relative density of [Sintered body 15] did not change from the relative density of [Sintered precursor 15], and sintering did not proceed. Therefore, it was shown that the sintered body does not become densified if the additive manufacturing material does not contain an alloy powder that generates a liquid phase.

[0134] Since sintering did not proceed, the amount of deformation of the sintered body was not evaluated.

[0135] Comparative Example 2 In the <Production of additive manufacturing material> of Example 1, except that the type of mixed powder of powder A and powder B was changed to the following, [additive manufacturing material 16] was prepared in the same manner as in Example 1, and this [additive manufacturing material 16] was used to form [sintered precursor 16] and [sintered body 16]. Powder A: AlSi4 (manufactured by Toyo Aluminum Co., Ltd., d50: 35 μm, the proportion of powder with a particle size of 106 μm or more is less than 0.1 mass%) Powder B: AlSi5 (manufactured by Toyo Aluminum Co., Ltd., d50: 35 μm, the proportion of powder with a particle size of 106 μm or more is less than 0.1 mass %)

[0136] -Evaluation results- FIG. 9B is a graph showing the results of calculations using thermodynamic calculation software (CaTCalc) of the change in the liquid phase ratio with respect to temperature for Powder A (AlSi4) and Powder B (AlSi5) in Comparative Example 2. From this calculation, there was no temperature range in which the liquid phase ratio of Powder A (AlSi4) was 30 mass% or less and the liquid phase ratio of Powder B (AlSi5) was 70 mass% or more. Therefore, no matter how the sintering temperature was set, there was no part that acted as a skeleton, and a liquid phase was generated throughout the shaped object. In addition, the liquid phase ratio of AlSi4 in [Sintered Body 16] at a sintering temperature of 600°C was 35 mass%, and the liquid phase ratio of AlSi5 in [Sintered Body 16] at a sintering temperature of 600°C was 47 mass%.

[0137] The deformation of the sintered body (deflection Δh) was as large as 0.6 mm. This indicates that sintering deformation becomes significant when there is no part that acts as a skeleton during sintering.

[0138] Example 2 In the <manufacture of additive manufacturing materials> of Example 1, except that the type of the mixed powder of Powder A and Powder B was changed to the following and the sintering temperature was changed from 600 °C to 580 °C in the <manufacture of sintered body>, [additive manufacturing material 2] was prepared in the same manner as in Example 1, and [sintering precursor 2] and [sintered body 2] were formed using this [additive manufacturing material 2]. · Powder A: AlSi3 (manufactured by Toyo Aluminum Co., Ltd., d50: 35 μm, the proportion of powder with a particle size of 106 μm or more is less than 0.1 mass%) · Powder B: AlSi10 (manufactured by Toyo Aluminum Co., Ltd., d50: 35 μm, the proportion of powder with a particle size of 106 μm or more is less than 0.1 mass%)

[0139] -Evaluation Results- From the calculation results, the temperature T at which the liquid phase ratio of Powder A (AlSi3) is 30 mass% or less and the liquid phase ratio of Powder B (AlSi10) is 70 mass% or more was in the range of 577 °C < T < 610 °C. Also, the liquid phase ratio of AlSi3 at the sintering temperature of 580 °C of [sintered body 2] was 14 mass%, and the liquid phase ratio of AlSi10 at the sintering temperature of 580 °C of [sintered body 2] was 80 mass%.

[0140] In addition, as a result of the evaluation of the sintering precursor and the sintered body, an effect of achieving both density improvement and deformation suppression was observed, similar to Example 1.

[0141] (Example 3) In the <manufacture of additive manufacturing materials> of Example 1, except that the type of the mixed powder of Powder A and Powder B was changed to the following and the sintering temperature was changed from 600 °C to 590 °C in the <manufacture of sintered body>, [additive manufacturing material 3] was prepared in the same manner as in Example 1, and [sintering precursor 3] and [sintered body 3] were formed using this [additive manufacturing material 3]. · Powder A: AlSi4 (manufactured by Toyo Aluminum Co., Ltd., d50: 35 μm, the proportion of powder with a particle size of 106 μm or more is less than 0.1 mass%) · Powder B: AlSi8 (manufactured by Toyo Aluminum Co., Ltd., d50: 35 μm, the proportion of powder with a particle size of 106 μm or more is less than 0.1 mass%)

[0142] -Evaluation Results- From the calculation results, the temperature T at which the liquid phase ratio of powder A (AlSi4) is 30% by mass or less and the liquid phase ratio of powder B (:AlSi8) is 70% by mass or more was in the range of 589 °C < T < 593 °C. Also, the liquid phase ratio of AlSi4 at the sintering temperature of 590 °C for [Sintered Body 3] was 29% by mass, and the liquid phase ratio of AlSi8 at the sintering temperature of 590 °C for [Sintered Body 3] was 71% by mass.

[0143] Also, as a result of the evaluation of the sintering precursor and the sintered body, an effect of achieving both density improvement and deformation suppression was observed, similar to Example 1.

[0144] (Example 4) In <Manufacture of Material for Additive Manufacturing> of Example 1, [Material for Additive Manufacturing 3] was prepared in the same manner as in Example 1, except that the types of the mixed powders of powder A and powder B were changed to the following, and [Sintering Precursor 3] and [Sintered Body 3] were formed using this [Material for Additive Manufacturing 3]. · Powder A: Pure Al (manufactured by Toyo Aluminum Co., Ltd., d50: 80 μm, the ratio of powder with a particle size of 106 μm or more is 14.0% by mass) · Powder B: AlSi12 (manufactured by Toyo Aluminum Co., Ltd., d50: 80 μm, the ratio of powder with a particle size of 106 μm or more is 14.0% by mass)

[0145] -Evaluation Results- The ratio of particles with a particle size larger than the layer pitch of 84 μm was large, and a certain proportion of those large particles was recoated to the excess powder receiver. As a result, the amount of powder particles in the layer pitch decreased, and the relative density of the sintering precursor decreased compared to Example 1. Accordingly, the relative density of the sintered body also decreased compared to Example 1.

[0146] (Example 5) In the <Production of additive manufacturing material> of Example 1, the ratio of powder B to the total volume of the mixed powder of powder A and powder B was changed from 20 volume% to 5 volume%. Except for this, [Additive manufacturing material 5] was prepared in the same manner as in Example 1, and this [Additive manufacturing material 5] was used to form [sintered precursor 5] and [sintered body 5].

[0147] -Evaluation results- When the ratio of Powder B to the total volume of the mixed powder of Powder A and Powder B was reduced, the relative density of the sintered body decreased compared to Example 1. It was shown that the densification effect is improved by increasing the addition ratio of the alloy powder that becomes a liquid phase during sintering.

[0148] Example 6 In the <Production of additive manufacturing material> of Example 1, the ratio of powder B to the total volume of the mixed powder of powder A and powder B was changed from 20 volume% to 25 volume%. Except for this, [Additive manufacturing material 6] was prepared in the same manner as in Example 1, and this [Additive manufacturing material 6] was used to form [sintered precursor 6] and [sintered body 6].

[0149] -Evaluation results- It was confirmed that increasing the ratio of Powder B to the total volume of the mixed powder of Powder A and Powder B had the effect of improving the relative density of the sintered body compared to Example 1. It was shown that the densification effect was improved by increasing the addition ratio of the alloy powder that becomes a liquid phase during sintering.

[0150] Example 7 In the <Production of additive manufacturing material> of Example 1, the ratio of powder B to the total volume of the mixed powder of powder A and powder B was changed from 20 volume% to 30 volume%. Except for this, [Additive manufacturing material 7] was prepared in the same manner as in Example 1, and this [Additive manufacturing material 7] was used to form [sintered precursor 7] and [sintered body 7].

[0151] -Evaluation results- It was confirmed that increasing the ratio of Powder B to the total volume of the mixed powder of Powder A and Powder B had the effect of improving the relative density of the sintered body compared to Example 1. It was shown that the densification effect was improved by increasing the addition ratio of the alloy powder that becomes a liquid phase during sintering.

[0152] Example 8 In the <Production of additive manufacturing material> of Example 1, [Additive manufacturing material 8] was prepared in the same manner as in Example 1, except that the type of mixed powder of powder A and powder B was changed to the following, and this [Additive manufacturing material 8] was used to form [sintered precursor 8] and [sintered body 8]. Powder A: Pure Al (manufactured by Toyo Aluminum Co., Ltd., d50: 50 μm, the proportion of powder with a particle size of 106 μm or more is less than 0.1 mass%) Powder B: AlSi12 (manufactured by Toyo Aluminum Co., Ltd., d50: 50 μm, the proportion of powder with a particle size of 106 μm or more is less than 0.1 mass %)

[0153] -Evaluation results- Increasing the median diameter of Powder A and Powder B improved the flowability of the additive manufacturing material and enhanced the packing of the powder bed. As a result, the relative density of the sintered precursor was improved compared to Example 1.

[0154] Example 9 In the <Production of additive manufacturing material> of Example 8, except that powder B was changed to the following, [Additive manufacturing material 9] was prepared in the same manner as in Example 8, and this [Additive manufacturing material 9] was used to form [Sintered precursor 9] and [Sintered body 9]. Powder B: AlSi12 (manufactured by Toyo Aluminum Co., Ltd., d50: 25 μm, the proportion of powder with a particle size of 106 μm or more is less than 0.1 mass%)

[0155] -Evaluation results- By disposing small-grained AlSi12 between large-grained pure Al particles, the relative density of the sintered precursor was improved compared to Example 8. In addition, the inclusion of small-grained AlSi12 increased the number of particle contacts, sintering was promoted, and the relative density of the sintered body was improved compared to Example 8. Furthermore, by improving the relative density of the sintered precursor, sintering shrinkage was reduced, and the amount of deformation of the sintered body was reduced compared to Example 8.

[0156] Example 10 In the <Production of additive manufacturing material> of Example 8, except that powder A was changed to the following, [additive manufacturing material 10] was prepared in the same manner as in Example 8, and this [additive manufacturing material 10] was used to form [sintered precursor 10] and [sintered body 10]. Powder A: Pure Al (manufactured by Toyo Aluminum Co., Ltd., d50: 25 μm, the proportion of powder with a particle size of 106 μm or more is less than 0.1 mass%)

[0157] -Evaluation results- The large grain size of AlSi12 is advantageous for densification because the oxide film thickness is relatively thin relative to the particle volume and the oxide film is easily broken when liquefied. As a result, the sintered density was improved compared to Example 8.

[0158] Example 11 In the <Production of additive manufacturing material> of Example 1, powder B was changed to the following, and the debinding temperature was changed from a temperature above the temperature at which the binder thermally decomposes and below the eutectic temperature of AlSi12 (577°C) to a temperature above the temperature at which the binder thermally decomposes and below the eutectic temperature of AlCu33 (548°C). Except for this, [additive manufacturing material 11] was prepared in the same manner as in Example 1, and this [additive manufacturing material 11] was used to form [sintered precursor 11] and [sintered body 11]. Powder B: AlCu33 (manufactured by Toyo Aluminum Co., Ltd., d50: 35 μm, the proportion of powder with a particle size of 106 μm or more is less than 0.1 mass %)

[0159] -Evaluation results- The temperature range in which the liquid phase ratio of powder A (pure Al) is 30 mass% or less and the liquid phase ratio of powder B (AlCu33) is 70 mass% or more was 548 °C < T < 660 °C. As a result, a densification effect similar to that of Example 1 was confirmed.

[0160] (Example 12) In the <manufacture of additive manufacturing material> of Example 1, powder B was changed to the following, and the debinding temperature was changed from a temperature equal to or higher than the temperature at which the binder thermally decomposes and lower than the eutectic temperature (577 °C) of AlSi12 to a temperature equal to or higher than the temperature at which the binder thermally decomposes and lower than the solidus temperature (567 °C) of AlSi10Mg0.4. Except for this, [additive manufacturing material 12] was prepared in the same manner as in Example 1, and [sintering precursor 12] and [sintered body 12] were formed using this [additive manufacturing material 12]. · Powder B: AlSi10Mg0.4 (manufactured by Toyo Aluminum Co., Ltd., d50: 35 μm, ratio of powder with a particle size of 106 μm or more is less than 0.1 mass%)

[0161] -Evaluation results- The temperature range in which the liquid phase ratio of powder A (pure Al) is 30 mass% or less and the liquid phase ratio of powder B (AlSi10Mg0.4) is 70 mass% or more was 578 °C < T < 660 °C. As a result, the reduction effect of the Mg oxide film was manifested, and a sintered body with a higher density than that of Example 1 was obtained.

[0162] (Example 13) In the <manufacture of additive manufacturing material> of Example 1, [additive manufacturing material 13] was prepared in the same manner as in Example 1 except that powder A was changed to the following, and [sintering precursor 13] and [sintered body 13] were formed using this [additive manufacturing material 13]. · Powder A: AlFe1 (manufactured by Toyo Aluminum Co., Ltd., d50: 35 μm, ratio of powder with a particle size of 106 μm or more is less than 0.1 mass%)

[0163] -Evaluation results- The temperature T at which the liquid phase ratio of powder A (AlFe1) is 30 mass% or less and the liquid phase ratio of powder B (AlSi12) is 70 mass% or more was in the range of 577 °C < T < 653 °C. As a result, a densification effect similar to that of Example 1 was confirmed.

[0164] (Example 14) The <manufacture of the material for additive manufacturing> of Example 1 was changed as follows to prepare [Material for Additive Manufacturing 14]. [Sintering precursor 14] and [Sintered body 14] were formed in the same manner as in Example 1 except that [Material for Additive Manufacturing 14] was used.

[0165] <Manufacture of the material for additive manufacturing> As the material for additive manufacturing, a mixed powder of the following powder A, powder B, and powder C was used. · Powder A: Pure Al (manufactured by Toyo Aluminum Co., Ltd., d50: 35 μm, the proportion of powder with a particle size of 106 μm or more is less than 0.1 mass%) · Powder B: AlSi12 (manufactured by Toyo Aluminum Co., Ltd., d50: 35 μm, the proportion of powder with a particle size of 106 μm or more is less than 0.1 mass%) · Powder C: AlSi1Mg0.4 (manufactured by Toyo Aluminum Co., Ltd., d50: 35 μm, the proportion of powder with a particle size of 106 μm or more is less than 0.1 mass%)

[0166] Powder A, powder B, and powder C were put into a bead mill (DYNO-MILL, manufactured by Shinmaru Enterprises Co., Ltd.) so that the ratio of powder A, powder B, and powder C to the total volume of the mixed powder of powder A, powder B, and powder C was powder A: powder B: powder C = 40:20:40 (volume%). It was operated at 100 rpm for 5 minutes to prepare [Material for Additive Manufacturing 14].

[0167] -Evaluation results- The temperature T at which the liquid phase ratio of powder A (pure Al) is 30 mass% or less and the liquid phase ratio of powder B (AlSi12) is 70 mass% or more was in the range of 577 °C < T < 660 °C. As a result, a densification effect was confirmed in the same manner as in Example 1.

[0168] [Table 1]

[0169] [Table 2]

[0170] [Table 3]

[0171] [Table 4]

[0172] [Table 5]

[0173] Examples of aspects of the present invention include the following. <1> A material for additive manufacturing comprising at least powder A and powder B, The powder A contains an alloy or a pure metal, The powder B contains an alloy having a different composition from that of the powder A, This is a material for additive manufacturing, characterized in that there exists a temperature range in which the liquid phase ratio of powder A relative to the total mass of powder A is 30 mass% or less, and the liquid phase ratio of powder B relative to the total mass of powder B is 70 mass% or more. <2> The ratio of powder having a particle size of 106 μm or more in the powder A is less than 10 mass %, and the ratio of powder having a particle size of 106 μm or more in the powder B is less than 10 mass %. <1> It is a material for additive manufacturing described in <3> The volume of the powder B relative to the total volume of the additive manufacturing material is 10 volume % or more; <2> It is a material for additive manufacturing described in <4> The volume of the powder B relative to the total volume of the additive manufacturing material is 15% by volume or more and 25% by volume or less; <3> It is a material for additive manufacturing described in <5> The median diameter of the powder A is larger than the median diameter of the powder B. <1> from <3> The additive manufacturing material according to any one of claims 1 to 5, <6> The ratio of the median diameter of the powder A to the median diameter of the powder B [median diameter of the powder A:median diameter of the powder B] is 1:0.3 to 1:0.7. <5> It is a material for additive manufacturing described in <7> The median diameter of the powder A is 45 μm or more and 55 μm or less, and the median diameter of the powder B is 20 μm or more and 30 μm or less. <6> It is a material for additive manufacturing described in <8> The median diameter of the powder B is larger than the median diameter of the powder A. <1> from <3> The additive manufacturing material according to any one of claims 1 to 5, <9> At least one of the powder A and the powder B contains an aluminum alloy. <1> from <8> The additive manufacturing material according to any one of claims 1 to 5, <10> The aluminum alloy contains at least one selected from the group consisting of silicon, magnesium, iron, and copper. <9> It is a material for additive manufacturing described in <11> Powder B is the aluminum alloy containing silicon, The content of the silicon relative to the total mass of the aluminum alloy is 8 mass% or more and 14 mass% or less. <10> It is a material for additive manufacturing described in <12> The above-mentioned composition containing at least powder A and powder B <1> from <11> A powder layer forming step of forming a powder layer using the additive manufacturing material according to any one of the above items; a powder layer solidification step of applying a resin liquid containing at least a resin to the powder layer to solidify the powder layer; a sintered precursor preparation step of repeating the powder layer forming step and the powder layer solidifying step to prepare a sintered precursor; a degreasing step of degreasing the resin in the sintering precursor; a sintering step of sintering the degreased sintering precursor in a temperature range in which the liquid phase ratio of the powder A relative to the total mass of the powder A is 30 mass% or less and the liquid phase ratio of the powder B relative to the total mass of the powder B is 70 mass% or more; The additive manufacturing method is characterized by comprising: <13> The above-mentioned composition containing at least powder A and powder B <1> from <11> A powder layer forming means for forming a powder layer using the additive manufacturing material according to any one of the preceding claims; a powder layer solidifying means for applying a resin liquid containing at least a resin to the powder layer and solidifying the powder layer; a sintered precursor producing means for producing a sintered precursor by repeatedly executing the powder layer forming means and the powder layer solidifying means; A degreasing means for degreasing the resin in the sintering precursor; a sintering means for sintering the degreased sintering precursor in a temperature range in which the liquid phase ratio of the powder A relative to the total mass of the powder A is 30 mass% or less and the liquid phase ratio of the powder B relative to the total mass of the powder B is 70 mass% or more; The additive manufacturing device is characterized by having:

[0174] The above <1> from <11> The additive manufacturing material according to any one of the preceding claims. <12> The additive manufacturing method according to <13> The additive manufacturing apparatus described above can solve the above-mentioned problems in the conventional art and achieve the object of the present invention. [Explanation of symbols]

[0175] 1 Modeling Department 5 Modeling Unit 7 Base material 10 Modeling liquid (resin liquid) 11 Powder tank 12 Flattening roller 13 Powder removal plate 20 Additive Manufacturing Materials 21 Supply tank 22 Modeling tank 23 Supply Stage 24 Modeling Stage 25 Reciprocating mechanism 26 Motor 27 Motor 28 Motor 29 Powder Drop Hole 30 Modeling layer 31 Powder layer 50 Liquid discharge unit 51 Carriage 52 Head 52a Head 52b Head 54 Guide member 55 Guide member 56 Tank mounting part 60 Tank 61 Maintenance Organization 71 Guide member 72 Slider section 101 Pipe section 101a: Uppermost end of pipe section 101 101b Uppermost end of pipe section 101 101c: The uppermost end of the pipe section 101, the point at which the distance from the imaginary line U is maximum 102 Block section 500 Control section 500A Main control unit 504 Non-volatile memory (NVRAM) 508 Head drive control unit 510 Motor drive unit 511 Motor drive unit 512 Motor drive unit 513 Motor drive unit 514 Motor drive unit 515 Motor drive unit 517 Supply system drive unit 518 Maintenance Drive Unit 522 Operation Panel 550 x-direction scanning mechanism 551 z-direction scanning mechanism 552 y-direction scanning mechanism 553 Motor 554 Powder feeding device 560 Temperature and Humidity Sensor [Prior art documents] [Patent documents]

[0176] [Patent Document 1] JP 2019-85604 A

Claims

1. A material for additive manufacturing comprising at least powder A and powder B, The powder A contains an alloy or a pure metal, The powder B contains an alloy having a different composition from that of the powder A, A temperature range exists in which the liquid phase ratio of the powder A relative to the total mass of the powder A is 30% by mass or less, and the liquid phase ratio of the powder B relative to the total mass of the powder B is 70% by mass or more. A material for additive manufacturing.

2. 2. The additive manufacturing material of claim 1, wherein the proportion of powder having a particle size of 106 μm or more in powder A is less than 10% by mass, and the proportion of powder having a particle size of 106 μm or more in powder B is less than 10% by mass.

3. The additive manufacturing material according to claim 2 , wherein the volume of the powder B relative to the total volume of the additive manufacturing material is 10% by volume or more.

4. The additive manufacturing material according to claim 3 , wherein the volume of the powder B relative to the total volume of the additive manufacturing material is 15 vol.% or more and 25 vol.% or less.

5. 2. The additive manufacturing material of claim 1 , wherein the median diameter of Powder A is larger compared to the median diameter of Powder B.

6. The additive manufacturing material of claim 5, wherein the ratio of the median diameter of the powder A to the median diameter of the powder B [median diameter of powder A: median diameter of powder B] is 1:0.3 to 1:0.

7.

7. 7. The additive manufacturing material of claim 6, wherein the median diameter of Powder A is 45 μm to 55 μm, and the median diameter of Powder B is 20 μm to 30 μm.

8. 2. The additive manufacturing material of claim 1 , wherein a median diameter of Powder B is larger compared to a median diameter of Powder A.

9. 2. The additive manufacturing material of claim 1 , wherein at least one of Powder A and Powder B contains an aluminum alloy.

10. 10. The additive manufacturing material of claim 9, wherein the aluminum alloy contains at least one selected from the group consisting of silicon, magnesium, iron, and copper.

11. The powder B is the aluminum alloy containing silicon, 11. The additive manufacturing material of claim 10, wherein the silicon content is equal to or greater than 8% by weight and equal to or less than 14% by weight relative to the total weight of the aluminum alloy.

12. A powder layer forming step of forming a powder layer using the additive manufacturing material according to claim 1 containing at least powder A and powder B; a powder layer solidification step of applying a resin liquid containing at least a resin to the powder layer to solidify the powder layer; a sintered precursor preparation step of repeating the powder layer forming step and the powder layer solidifying step to prepare a sintered precursor; a degreasing step of degreasing the resin in the sintering precursor; a sintering step of sintering the degreased sintering precursor in a temperature range in which a liquid phase ratio of the powder A relative to the total mass of the powder A is 30 mass% or less and a liquid phase ratio of the powder B relative to the total mass of the powder B is 70 mass% or more; An additive manufacturing method comprising:

13. A powder layer forming means for forming a powder layer using the additive manufacturing material according to claim 1 containing at least powder A and powder B; a powder layer solidifying means for applying a resin liquid containing at least a resin to the powder layer and solidifying the powder layer; a sintered precursor producing means for producing a sintered precursor by repeatedly executing the powder layer forming means and the powder layer solidifying means; A degreasing means for degreasing the resin in the sintering precursor; a sintering means for sintering the degreased sintering precursor in a temperature range in which the liquid phase ratio of the powder A relative to the total mass of the powder A is 30 mass% or less and the liquid phase ratio of the powder B relative to the total mass of the powder B is 70 mass% or more; An additive manufacturing apparatus comprising:

Citation Information

Patent Citations

  • Powder for three-dimensional printing containing foreign nuclear particles, shaped body using the same, and method for producing the shaped body

    JP2019085604A