Nitride semiconductor light emitting device

By employing a first AlN layer with a mole fraction of 0.42 or less and an uneven surface, the nitride semiconductor light emitting device achieves improved ohmic characteristics and reduced power consumption, addressing the limitations of existing devices.

JP2024135643APending Publication Date: 2024-10-04MEIJO UNIVERSITY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023046430
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing nitride semiconductor light emitting devices face challenges in achieving ohmic characteristics due to limitations in heat treatment temperatures, leading to suboptimal current-voltage characteristics and increased power consumption.

Method used

The device incorporates a first AlN composition layer with a mole fraction of 0.42 or less, thinner than a second layer, and an uneven exposed surface to facilitate better electrode contact, allowing for improved ohmic characteristics and reduced power consumption.

Benefits of technology

The configuration enables efficient current flow at lower voltages, approximating ohmic characteristics and reducing stress, thereby enhancing light emission while minimizing power consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135643000001_ABST
    Figure 2024135643000001_ABST
Patent Text Reader

Abstract

To provide a nitride semiconductor light emitting device having characteristics close to ohmic characteristics.SOLUTION: A nitride semiconductor light emitting device 1 includes a first n-AlGaN layer 12B having one side in the stacking direction L formed as an exposed surface Es, a Ti / Pt / Au electrode Ne stacked on the exposed surface Es, and a second n-AlGaN layer 12C stacked on the side opposite the Ti / Pt / Au electrode Ne across the first n-AlGaN layer 12B, and the molar fraction of AlN in the first n-AlGaN layer 12B is smaller than the molar fraction of AlN in the second n-AlGaN layer 12C.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a nitride semiconductor light emitting device. [Background technology]

[0002] Patent Document 1 discloses a nitride semiconductor device capable of lasing ultraviolet light. In this device, a composition gradient layer and a p-type semiconductor layer are laminated in this order on the surface of an upper guide layer and crystal growth is performed, and the part of the p-type semiconductor layer close to the upper guide layer is given the function of blocking electrons moving from the active layer toward the surface side. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2021-184456 Summary of the Invention [Problem to be solved by the invention]

[0004] For GaN-based light-emitting devices, there is a method for fabricating a thin-film structure device that can pass current vertically (in the stacking direction) by peeling off GaN-based nitride semiconductor crystals from a sapphire substrate using laser lift-off (LLO) technology and forming an n-electrode on the back surface (nitrogen polarity surface). Using this method, a device that can pass current vertically was fabricated using AlGaN-based nitride semiconductor crystals. In this structure, the AlGaN-based nitride semiconductor crystals with p-electrodes and pad electrodes formed on the surface of the support are eutectic-bonded to the support substrate using a metal such as AuSn, and then peeled off from the sapphire substrate using LLO technology. Then, an n-electrode is formed on the exposed surface that is exposed after peeling. The heat treatment temperature after the n-electrode formation cannot be very high, at most about 300°C, in order to prevent cracks from occurring in the crystal. As the n-electrode for nitrogen-polarity AlGaN, we investigated V / Al / Ti / Au electrodes, which have a proven track record on the metal polarity surface of AlGaN, and Cr / Ni / Au and Ti / Pt / Au electrodes, which are non-alloyed and provide ohmic characteristics on the metal polarity surface or nitrogen polarity surface of GaN in GaN-based devices. As a result, within the constraints of a heat treatment temperature of up to 300°C, the best results were obtained when using Ti / Pt / Au electrodes, but the characteristics were Schottky characteristics. For this reason, further improvement is desired to achieve ohmic characteristics. Ohmic characteristics mean that the current-voltage characteristics show characteristics that are roughly linear. Schottky characteristics mean that the degree of change in the current value changes significantly at a certain voltage value.

[0005] The present invention has been made in view of the above-mentioned conventional circumstances, and an object of the present invention is to provide a nitride semiconductor light-emitting device having characteristics close to ohmic characteristics. [Means for solving the problem]

[0006] The nitride semiconductor light-emitting device of the present invention comprises: A first layer having one side in the stacking direction formed as an exposed surface; an electrode laminated on the exposed surface; a second layer laminated on the opposite side of the electrode with the first layer interposed therebetween; Equipped with The mole fraction of AlN in the first layer is smaller than the mole fraction of AlN in the second layer.

[0007] According to this configuration, it is possible to approach the characteristic (ohmic characteristic) in which a current flows satisfactorily even when a small voltage is applied, and it is possible to emit light satisfactorily while suppressing power consumption. [Brief description of the drawings]

[0008] [Figure 1] 1 is a schematic diagram showing the structure of a nitride semiconductor light-emitting device according to Example 1. FIG. [Diagram 2] FIG. 2 is a schematic diagram showing the structure of a nitride semiconductor light-emitting device before LLO is performed. [Diagram 3] (A) shows the nitride semiconductor light-emitting element of Example 1 after chemical mechanical polishing to expose the exposed surface of the first n-AlGaN layer, (B) shows a state in which a SiO2 layer is laminated on the exposed surface to expose the central portion of the exposed surface, (C) shows a state in which a protrusion is formed on the exposed surface, and (D) shows a state in which an n-electrode is provided on the exposed surface with the protrusion formed. [Figure 4] 1 is a graph showing the turn-on voltage and differential resistance value versus the molar fraction of AlN in the samples of Example 1 and Comparative Examples 1 and 2. [Diagram 5] 1 is a graph showing current-voltage characteristics of samples of Example 1 and Comparative Examples 1 and 2. [Figure 6] 4 is a partially enlarged schematic view showing the structure of the nitride semiconductor light-emitting device of Example 2. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] A preferred embodiment of the present invention will now be described.

[0010] In the nitride semiconductor light emitting device of the present invention, the molar fraction of AlN in the first layer may be 0.42 or less. In this case, even if a small voltage is applied, the current can flow easily. In other words, the current-voltage characteristics can be made closer to ohmic characteristics.

[0011] The thickness of the first layer in the stacking direction of the nitride semiconductor light-emitting device of the present invention can be made thinner than the thickness of the second layer in the stacking direction. In this case, since the thickness of the first layer is made thinner than the thickness of the second layer, stress on the device caused by the first layer can be reduced.

[0012] The first layer of the nitride semiconductor light emitting device of the present invention may be a first AlN composition layer having an AlN molar fraction of 0.42 or less and a second AlN composition layer having an AlN molar fraction of more than 0.42, alternately stacked in the stacking direction. In this case, the stress on the device caused by the first layer can be reduced more effectively.

[0013] The exposed surface of the first layer of the nitride semiconductor light emitting device of the present invention may be formed to have projections and recesses. In this case, the first AlN composition layer having an AlN mole fraction of 0.42 or less can be reliably exposed to allow an electrode to come into contact with this layer.

[0014] Next, a first embodiment of the nitride semiconductor light emitting device of the present invention will be described with reference to the drawings.

[0015] <Example 1> As shown in Fig. 1, the nitride semiconductor light emitting device 1 of Example 1 includes a first n-AlGaN layer 12B as a first layer, a second n-AlGaN layer 12C as a second layer, a first guide layer 13A, a double quantum well active layer 13B, a second guide layer 13C as a guide layer, an electron blocking layer 14, a cladding layer 15, a p-AlGaN layer 16, a p-GaN layer 17, a Ni / Pt / Au electrode Pe, and a Ti / Pt / Au electrode Ne. The nitride semiconductor light emitting device 1 of Example 1 is grown as a crystal by stacking layers using MOVPE (metal organic vapor phase epitaxy). The nitride semiconductor light emitting device 1 is an ultraviolet semiconductor laser device that lases ultraviolet light in the UV-B wavelength range.

[0016] [Manufacturing procedures for nitride semiconductor light-emitting devices] Next, a manufacturing procedure of the nitride semiconductor light emitting device 1 will be described. First, a sapphire substrate 10A is prepared with the C-plane ((0001) plane) as the surface (the front is the upper side in FIG. 2, the same applies below). Then, a first AlN layer 10B is laminated on the surface of the sapphire substrate 10A by using a sputtering method. The thickness of the first AlN layer 10B is 450 nm. After the first AlN layer 10B is laminated, annealing is performed at 1700° C. for 3 hours in an N2 (nitrogen) atmosphere. In this way, an AlN template substrate 10 having the sapphire substrate 10A and the first AlN layer 10B is fabricated by using a sputtering method. After that, a layer structure is formed by using an MOVPE method.

[0017] The AlN template substrate 10 is placed in a reactor capable of carrying out the MOVPE method (hereinafter, simply referred to as the reactor), and while NH3 (ammonia), which is an N (nitrogen) raw material, is flowed onto the surface of the AlN template substrate 10 (the surface of the first AlN layer 10B) (hereinafter, the supply is not stopped), the temperature of the AlN template substrate 10 is raised to 1200°C in an H2 (hydrogen) atmosphere, and then maintained for 10 minutes.

[0018] Next, the second AlN layer 11 is laminated on the surface of the first AlN layer 10B for crystal growth. The thickness of the second AlN layer 11 is 1550 nm. The second AlN layer 11 is formed by supplying TMAl (trimethylaluminum), an Al (aluminum) raw material, into a reactor while the temperature of the AlN template substrate 10 is set to 1200°C. The total thickness of the first AlN layer 10B and the second AlN layer 11 is 2000 nm.

[0019] Next, a convex portion forming process is performed to form a plurality of convex portions 11A extending in a columnar shape in the stacking direction L on the surface of the second AlN layer 11. Specifically, a SiO2 layer is stacked to a thickness of 420 nm on the surface of the second AlN layer 11 using a sputtering device. Then, a resin for nanoimprinting is applied to the surface of the SiO2 layer to form a resin film, and then a fine pattern with a pitch of 1000 nm and an outer diameter of 500 nm is formed on the resin film using a nanoimprinting device. Then, an ICP device is used to perform inductively coupled plasma etching on the SiO2 layer with CF4 gas, and then, buffered hydrofluoric acid is used to remove the residue of the SiO2 layer. Then, using Cl2 gas, inductively coupled plasma etching is performed on the surface side of the second AlN layer 11 to a depth of 300 nm. After that, the SiO2 layer and the resist film used as a mask are removed using hydrofluoric acid. In this manner, the convex portion forming process is performed.

[0020] Next, a u-AlGaN layer 12A is laminated on the surface of the second AlN layer 11 on which the protrusions 11A are formed, and crystals are grown. Specifically, the AlN template substrate 10 on which the protrusions 11A are formed is placed in a reactor again. Then, the temperature of the AlN template substrate 10 is raised to 1200°C, and when it reaches a predetermined temperature, H2, TMGa (trimethylgallium), TMAl, and NH3, which are raw materials for Ga (gallium), are supplied into the reactor so that the mole fraction of AlN becomes 0.68. The thickness of the u-AlGaN layer 12A is 3 μm. By making the thickness of the u-AlGaN layer 12A 3 μm, the surface of the second AlN layer 11 on which the protrusions 11A are formed can be buried and flattened. The u-AlGaN layer 12A is not doped with impurities such as Si or Mg, but the u-AlGaN layer 12A may be replaced with an n-AlGaN layer doped with Si or the like. Here, the thickness of the u-AlGaN layer 12A is the dimension from the base end of the protrusion 11A to the surface of the u-AlGaN layer 12A.

[0021] Next, the first n-AlGaN layer 12B is laminated on the surface of the u-AlGaN layer 12A and crystal growth is performed. Specifically, while continuing to supply H2, TMGa, TMAl, and NH3 into the reactor, SiH4 is supplied into the reactor. The Si concentration in the first n-AlGaN layer 12B is 6×10 18 cm -3 The supply flow rates of the raw materials are adjusted so that the thickness of the first n-AlGaN layer 12B is, for example, 1 μm. The thickness of the first n-AlGaN layer 12B is preferably 1 μm or more and 2 μm or less. The mole fraction of AlN in the first n-AlGaN layer 12B is 0.42.

[0022] Next, the 2n-AlGaN layer 12C is stacked on the surface of the 1n-AlGaN layer 12B to grow crystals. The concentration of Si added in the 2n-AlGaN layer 12C is the same as that in the 1n-AlGaN layer 12B. The thickness of the 2n-AlGaN layer 12C is, for example, 3 μm. That is, the thickness of the 1n-AlGaN layer 12B in the stacking direction L is thinner than the thickness of the 2n-AlGaN layer 12C in the stacking direction L. The supply flow rate of the raw material is adjusted so that the mole fraction of AlN in the 2n-AlGaN layer 12C is 0.62. That is, the mole fraction of AlN in the 1n-AlGaN layer 12B is smaller than the mole fraction of AlN in the 2n-AlGaN layer 12C.

[0023] Next, the first guide layer 13A and the double quantum well active layer 13B are laminated in this order on the surface of the second n-AlGaN layer 12C to grow crystals. Specifically, the temperature of the AlN template substrate 10 is lowered to 1050°C. Then, TMGa is switched to TEGa (triethylgallium). Then, when the temperature of the AlN template substrate 10 reaches a predetermined temperature, the double quantum well active layer 13B is laminated, which is composed of two laminated sets of the first guide layer 13A (the molar fraction of AlN is 0.45) having a thickness of 50 nm, a well layer (the molar fraction of AlN is 0.35) having a thickness of 4 nm, and a barrier layer (the molar fraction of AlN is 0.45) having a thickness of 8 nm.

[0024] Next, while maintaining the temperature of the AlN template substrate 10 at the condition for depositing the double quantum well active layer 13B, the second guide layer 13C is deposited on the surface of the double quantum well active layer 13B, which is the active layer, for crystal growth. The flow rate of the raw material supplied into the reactor is adjusted so that the molar fraction of AlN in the second guide layer 13C is 0.45. The thickness of the second guide layer 13C is 55 nm. In this manner, the second guide layer 13C (the molar fraction of AlN is 0.45) is deposited.

[0025] Next, the electron block layer 14 that blocks the flow of electrons from the double quantum well active layer 13B side is laminated on the surface of the second guide layer 13C and crystal growth is performed. Specifically, only group III raw materials are supplied into the reactor and held for a predetermined time. The flow rate of the raw materials supplied into the reactor is adjusted so that the molar fraction of AlN in the electron block layer 14 is 0.9. The group III raw materials supplied at this time are TMGa and TMAl. In this way, the electron block layer 14 (the molar fraction of AlN is 0.9) with a thickness of 5 nm is laminated on the surface of the second guide layer 13C.

[0026] Next, the cladding layer 15 is laminated on the surface of the electron blocking layer 14 to grow crystals. Specifically, the flow rate of the raw material supplied into the reactor is adjusted so that the molar fraction of AlN in the cladding layer 15 becomes 0.9. The flow rate of the raw material supplied into the reactor is then adjusted so that the molar fraction of AlN gradually changes from 0.9 to 0.6 over a predetermined time. In this way, the cladding layer 15 having a thickness of 320 nm is laminated on the surface of the electron blocking layer 14. The molar fraction of AlN in the cladding layer 15 thus laminated has a composition gradient that decreases in the direction away from the double quantum well active layer 13B in the lamination direction L.

[0027] Next, a p-AlGaN layer 16 is laminated on the surface of the cladding layer 15 for crystal growth. Specifically, after the crystal growth of the cladding layer 15 is completed, the flow rate of the raw material supplied into the reactor is adjusted so that the molar fraction of AlN is gradually changed from 0.6 to 0 over a predetermined time. In this way, a p-AlGaN layer 16 having a thickness of 75 nm is laminated on the surface of the cladding layer 15. The cladding layer 15 and the p-AlGaN layer 16 have different rates of change in the molar fraction of AlN per unit thickness in the lamination direction L.

[0028] Next, a p-GaN layer 17 that functions as a contact layer with the Ni / Pt / Au electrode Pe is laminated on the surface of the p-AlGaN layer 16 and crystal grown. Then, the supply of TMGa and TMAl into the reactor is stopped to terminate the crystal growth, and the temperature of the AlN template substrate 10 is lowered to room temperature while flowing H2 and NH3 into the reactor. After the temperature of the AlN template substrate 10 has reached room temperature, the reactor is thoroughly purged, and the AlN template substrate 10 is removed from the reactor.

[0029] Next, a p-electrode pattern is formed on the surface of the p-GaN layer 17 using a resist film, Ni / Pt / Au (10 nm / 10 nm / 40 nm) are sequentially evaporated and lifted off, and then a heat treatment is performed in an oxygen atmosphere at 700° C. for 1 minute to form a Ni / Pt / Au electrode Pe. Then, a pad electrode pattern is formed using a resist film, and Ti / Au (50 nm / 800 nm) is evaporated and lifted off to form a pad electrode (not shown).

[0030] Next, after mirror polishing the back surface of the sapphire substrate, the nitride semiconductor light emitting element is attached to the support substrate with AuSn via a pad electrode. Then, laser lift-off (LLO) is performed to peel off the u-AlGaN layer 12A from the second AlN layer 11. Specifically, a laser beam with a wavelength of 257 nm and an energy density of 0.53 J / cm is applied from the back surface side of the nitride semiconductor light emitting element 1 bonded to the support substrate (i.e., the back surface side of the sapphire substrate 10A). 2The laser light is irradiated evenly onto the entire back surface. This makes it possible to peel off the u-AlGaN layer 12A from the second AlN layer 11.

[0031] Next, as shown in FIG. 3(A), the exposed surface of the u-AlGaN layer 12A that is peeled off from the second AlN layer 11 is chemically and mechanically polished to expose the 1n-AlGaN layer 12B as the exposed surface Es. The 1n-AlGaN layer 12B has one side in the stacking direction L formed as the exposed surface Es. The exposed surface Es is a nitrogen polarity surface. Next, the exposed surface Es of the exposed 1n-AlGaN layer 12B is patterned with resist, and then a SiO2 layer 18 is stacked to a thickness of 420 nm using a sputtering device and lifted off. Thus, the center of the exposed surface Es of the 1n-AlGaN layer 12B is exposed (see FIG. 3(B)).

[0032] Then, an n-electrode is formed on the exposed surface Es of the first n-AlGaN layer 12B exposed from the SiO2 layer 18. A Ti / Pt / Au electrode Ne is laminated as the n-electrode by using a vacuum deposition method (see FIG. 3(D)). Specifically, after patterning with a resist, Ti / Pt / Au (50 nm / 50 nm / 100 nm) is deposited and lifted off by using a vacuum deposition method. When the n-electrode is formed by the lift-off method, the electrode deposition portion is exposed to a developer. When a 2.38% TMAH aqueous solution is used as the developer, the exposed surface Es of the first n-AlGaN layer 12B is formed in an uneven shape as shown in FIG. 3(C). Specifically, a plurality of mountain-shaped protrusions C are formed on the exposed surface Es. The dimension of the protrusions C in the lamination direction L is approximately 200 nm. In this way, the nitride semiconductor light-emitting device 1 shown in FIG. 1 is completed. As shown in FIG. 3D, the second n-AlGaN layer 12C is laminated on the opposite side to the Ti / Pt / Au electrode Ne with the first n-AlGaN layer 12B interposed therebetween.

[0033] Next, the results of measuring the electrical characteristics of the nitride semiconductor light-emitting device 1 thus completed will be described. The pattern for measuring the electrical characteristics was a pattern for TLM measurement, which is a test pattern for measuring the contact resistance with the first n-AlGaN layer 12B. To compare with the nitride semiconductor light-emitting device 1, samples of Comparative Examples 1 and 2 were prepared in which the molar fractions of AlN in the first n-AlGaN layer 12B were set to 0.51 and 0.62. The samples of Comparative Examples 1 and 2 have the same configuration as the nitride semiconductor light-emitting device 1, except for the molar fraction of AlN in the first n-AlGaN layer 12B. As shown in FIGS. 4 and 5, the voltage (rise voltage) at which a current starts to flow in the sample of Comparative Example 2 (AlN molar fraction 0.62) was about 2.4V. The voltage (rise voltage) at which a current starts to flow in the sample of Comparative Example 1 (AlN molar fraction 0.51) was about 1V. The voltage (rise voltage) at which a current starts to flow in the nitride semiconductor light-emitting device 1 (AlN molar fraction 0.42) was about 0.2V.

[0034] That is, it was found that as the molar fraction of AlN in the first n-AlGaN layer 12B decreases, the voltage at which current starts to flow (start-up voltage) decreases, and the current-voltage characteristics approach ohmic characteristics. Focusing on the graph of the voltage at which current starts to flow versus the molar fraction of AlN in the first n-AlGaN layer 12B in Fig. 4, it is considered that the voltage at which current starts to flow can be set to 0V (i.e., ohmic characteristics) by setting the molar fraction of AlN in the first n-AlGaN layer 12B to approximately 0.38. Therefore, by setting the molar fraction of AlN in the first n-AlGaN layer 12B to 0.42 or less, the current-voltage characteristics of the nitride semiconductor light-emitting device 1 can be improved.

[0035] The differential resistance value of the sample of Comparative Example 2 is approximately 1.0 × 10 2 The differential resistance value of the sample of Comparative Example 1 was approximately 6.0×10 1 The differential resistance of the nitride semiconductor light-emitting element 1 was approximately 4.1×10 1In other words, it was found that the differential resistance value decreased as the molar fraction of AlN in the first n-AlGaN layer 12B decreased.

[0036] Next, the operation of the above embodiment will be described. The nitride semiconductor light emitting element 1 includes a first n-AlGaN layer 12B having one side in the stacking direction L formed as an exposed surface Es, a Ti / Pt / Au electrode Ne stacked on the exposed surface Es, and a second n-AlGaN layer 12C stacked on the opposite side of the Ti / Pt / Au electrode Ne across the first n-AlGaN layer 12B, where the mole fraction of AlN in the first n-AlGaN layer 12B is smaller than the mole fraction of AlN in the second n-AlGaN layer 12C. This configuration makes it possible to approach the characteristic of good current flow even when a small applied voltage is applied (ohmic characteristic), and good light emission can be achieved while suppressing power consumption.

[0037] In the nitride semiconductor light emitting device 1, the molar fraction of AlN in the first n-AlGaN layer 12B is 0.42 or less. In this case, even if a small voltage is applied, the current can flow easily. In other words, the current-voltage characteristics can be made to approach ohmic characteristics.

[0038] The thickness of the first n-AlGaN layer 12B in the stacking direction L of the nitride semiconductor light emitting device 1 is thinner than the thickness of the second n-AlGaN layer 12C in the stacking direction L. In this case, since the thickness of the first n-AlGaN layer 12B is made smaller than the thickness of the second n-AlGaN layer 12C, it is possible to reduce stress on the element caused by the first n-AlGaN layer 12B having a small mole fraction of AlN.

[0039] <Example 2> Next, a nitride semiconductor light emitting element 2 according to Example 2 will be described with reference to Fig. 6. The nitride semiconductor light emitting element 2 according to Example 2 differs from Example 1 in that the first n-AlGaN layer 112B has first AlN composition layers 112D and second AlN composition layers 112E having different AlN mole fractions stacked alternately in the stacking direction L. The same reference numerals are used for the same components as in Example 1, and descriptions of the structures, functions and effects will be omitted.

[0040] As shown in FIG. 6, the first n-AlGaN layer 112B has a first AlN composition layer 112D and a second AlN composition layer 112E. The first AlN composition layer 112D and the second AlN composition layer 112E are formed of AlGaN. The molar fraction of AlN in the first AlN composition layer 112D is 0.3, which is equal to or less than 0.42. The molar fraction of AlN in the second AlN composition layer 112E is 0.62, which is greater than 0.42. The first AlN composition layer 112D and the second AlN composition layer 112E are alternately stacked in a stacking direction L. The thickness of each of the first AlN composition layer 112D and the second AlN composition layer 112E is, for example, 25 nm. The number of stacked first AlN composition layers 112D and second AlN composition layers 112E is, for example, 40 layers. The first AlN composition layer 112D and the second AlN composition layer 112E have a so-called superlattice structure.

[0041] As in Example 1, when the Ti / Pt / Au electrode Ne is provided on the exposed surface Es of the first n-AlGaN layer 112B exposed by chemical mechanical polishing, the exposed surface Es is etched by being exposed to a TMAH aqueous solution (2.38%) as a developer. In this case, a plurality of mountain-shaped protrusions C are formed on the exposed surface Es of the exposed first n-AlGaN layer 112B. When focusing on the slope of each protrusion C, both the first AlN composition layer 112D and the second AlN composition layer 112E are exposed. This ensures that the Ti / Pt / Au electrode Ne is in contact with the first AlN composition layer 112D and the second AlN composition layer 112E. The Ti / Pt / Au electrode Ne is in contact with the first AlN composition layer 112D, which is a low AlN mole fraction layer, and current can be passed more smoothly.

[0042] The first n-AlGaN layer 112B of the nitride semiconductor light emitting device 2 is formed by alternately stacking a first AlN composition layer 112D having an AlN molar fraction of 0.42 or less and a second AlN composition layer 112E having an AlN molar fraction of more than 0.42 in the stacking direction L. In this case, the stress on the element caused by the first layer can be reduced more effectively.

[0043] The exposed surface Es of the first n-AlGaN layer 112B of the nitride semiconductor light emitting element 2 is formed in an uneven shape. In this case, the first AlN composition layer 112D having an AlN mole fraction of 0.42 or less can be reliably exposed and the Ti / Pt / Au electrode Ne can be brought into contact with this layer.

[0044] The present invention is not limited to the first embodiment described above with reference to the drawings, and the following embodiments are also included within the technical scope of the present invention. (1) In the first embodiment, Si is added as an n-type impurity, but the n-type impurity may be Ge, Te, etc. Also, Mg, Zn, Be, Ca, Sr, Ba, etc. may be added as a p-type impurity. (2) In the first embodiment, a sapphire substrate is used, but an AlN layer may be laminated on another substrate such as an AlN substrate for crystal growth. (3) In the first embodiment, the AlN layer formed by sputtering is included, but instead of sputtering, only the AlN layer grown by MOVPE may be used. (4) Unlike the first embodiment, the exposed surface may not be formed unevenly, and a Ti / Pt / Au electrode may be provided. (5) The present invention may be applied to a light-emitting diode that uses a nitride semiconductor. (6) The exposed surface may be etched with an alkaline liquid such as an aqueous KOH solution. (7) The number of the first AlN composition layers and the second AlN composition layers stacked is not limited to 40. In addition, the thickness of the first AlN composition layer and the second AlN composition layer is not limited to 25 nm. [Explanation of symbols]

[0045] 1...Nitride semiconductor light emitting device 12B, 112B…1st n-AlGaN layer (1st layer) 12C…2nd n-AlGaN layer (2nd layer) 112D…first AlN composition layer 112E…Second AlN composition layer Es…exposed surface L…Lamination direction Ne…Ti / Pt / Au electrode (electrode)

Claims

1. A first layer having one side in a stacking direction formed as an exposed surface; an electrode laminated on the exposed surface; a second layer laminated on the opposite side of the electrode with the first layer interposed therebetween; Equipped with A nitride semiconductor light-emitting device, wherein a mole fraction of AlN in the first layer is smaller than a mole fraction of AlN in the second layer.

2. The nitride semiconductor light emitting device according to claim 1 , wherein a mole fraction of AlN in said first layer is 0.42 or less.

3. 3 . The nitride semiconductor light-emitting element according to claim 1 , wherein a thickness of said first layer in said stacking direction is smaller than a thickness of said second layer in said stacking direction. 4 .

4. 3. The nitride semiconductor light-emitting device according to claim 2, wherein the first layer is formed by alternately stacking in the stacking direction a first AlN composition layer having an AlN molar fraction of 0.42 or less and a second AlN composition layer having an AlN molar fraction of more than 0.

42.

5. The nitride semiconductor light emitting element according to claim 4 , wherein the exposed surface of the first layer is formed unevenly.

Citation Information

Patent Citations

  • Nitride semiconductor laser diode

    JP2021184456A