Pyrochlore oxide powder
By controlling the atomic ratios and refining the particle size of pyrochlore oxide powder through dispersion treatment, the issues of impurity phases and environmental impact in BRO oxide catalysts are addressed, resulting in improved catalytic activity and battery performance.
Patent Information
- Application Number
- JP2023046557
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
The presence of bismuth-containing impurity phases in BRO oxide catalysts affects the performance of secondary batteries, reducing their lifespan and catalytic activity due to the formation of micro short circuits and dendrites, and conventional methods to remove these impurities increase environmental impact and manufacturing costs.
A pyrochlore oxide powder with controlled particle size distribution and reduced impurity phases is produced by adjusting the atomic ratios of bismuth and ruthenium/manganese in the raw material solution, followed by dispersion treatment to refine the powder particles, eliminating the need for pickling steps.
The resulting pyrochlore oxide powder exhibits improved catalytic activity and dispersibility, enhancing the performance of secondary batteries while reducing environmental impact and manufacturing costs.
Smart Images

Figure 2024135725000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a powder of a pyrochlore oxide (hereinafter, this type of composite oxide may be referred to as "BRO oxide") that has a crystal structure of a bismuth (Bi)-ruthenium (Ru)-oxygen (O) type pyrochlore oxide and contains bismuth and ruthenium, or bismuth, ruthenium and manganese (Mn) as its constituent metal elements. [Background technology]
[0002] BRO oxide is a material that is expected to be used as a positive electrode catalyst in air secondary batteries and hydrogen production processes through water electrolysis.
[0003] Patent Document 1 describes a manganese-containing BRO oxide catalyst (Claim 1). It is said that the inclusion of manganese provides effects such as improved catalytic activity. In an experiment to evaluate the properties of the oxide catalyst, an aqueous NaOH solution is added to an aqueous solution containing a metal salt of the raw material at a specified ratio, and the solution is stirred for 24 hours while aerating oxygen at 75°C to obtain an oxidation reaction product, which is then dried, calcined at 600°C, suction filtered using distilled water, and then dried. The material obtained is used as a sample (paragraphs 0027 and 0041). According to the description in paragraph 0027 and Table 2, the Bi / (Ru+Mn) atomic ratio in the blending ratio of the raw material in the aqueous solution is calculated to be 0.82 (Example 1), 0.93 (Examples 2 and 3), and 1.00 (Examples 4 to 6).
[0004] Patent Documents 2 to 5 describe BRO oxide catalysts and air secondary batteries using the same. According to the disclosure of Patent Document 2, metal components (mainly bismuth) in the by-products formed in the manufacturing process of BRO oxide undergo dissolution and precipitation reactions during the charge and discharge cycle of the battery, and grow as dendrites on the electrode plate, which causes micro-short circuits and reduces battery performance and battery life (paragraph 0012). In order to remove these by-products (see paragraph 0030), the manufacturing method disclosed in Patent Document 2 involves immersing the washed and dried fired BRO oxide in an aqueous nitric acid solution for acid treatment (paragraphs 0051-0053). It is also described that in the preparation of the initial aqueous solution used in the reaction before firing, a bismuth-containing salt and a ruthenium-containing salt are added to have the same concentration (paragraphs 0051 and 0077).
[0005] In Patent Document 3, in order to further improve the energy efficiency and increase the output of air secondary batteries (see paragraph 0009), a method is adopted in which a secondary heat treatment is performed to form ruthenium oxide on the surface of the catalyst (paragraphs 0053-0056). In the process of obtaining a water-washed and dried product of BRO oxide to be subjected to the secondary heat treatment, an acid treatment is performed by immersing the product in an aqueous nitric acid solution to remove by-products, as in Patent Document 2 (paragraph 0052). In Patent Document 3, in the preparation of the initial aqueous solution used in the reaction before calcination, a bismuth-containing salt and a ruthenium-containing salt are also added to have the same concentration (paragraphs 0045, 0082).
[0006] In the manufacturing process of the BRO oxide catalyst disclosed in Patent Document 4, similarly to Patent Document 2, an acid treatment is performed by immersing in an aqueous nitric acid solution to remove by-products (paragraphs 0041 to 0043), and in preparing the initial aqueous solution used in the reaction before calcination, a bismuth-containing salt and a ruthenium-containing salt are added to have the same concentration (paragraphs 0040 and 0065).
[0007] In Patent Document 5, in order to further improve the energy efficiency and increase the output of air secondary batteries (see paragraph 0012), a method is adopted in which an aqueous sodium hydroxide solution is added to a powdered precursor, the precursor is dried, and then the precursor is fired (paragraphs 0046-0047). In the manufacturing process, as in Patent Document 2, an acid treatment is performed by immersing the precursor in an aqueous nitric acid solution to remove by-products (paragraphs 0041-0043), and in the preparation of the initial aqueous solution used in the reaction before firing, a bismuth-containing salt and a ruthenium-containing salt are added so that they have the same concentration (paragraphs 0046, 0074). [Prior art documents] [Patent documents]
[0008] [Patent Document 1] International Publication No. 2020 / 153401 [Patent Document 2] JP 2019-179592 A [Patent Document 3] JP 2020-80291 A [Patent Document 4] JP 2020-126754 A [Patent Document 5] Patent Publication No. 2021-99914 Summary of the Invention [Problem to be solved by the invention]
[0009] As described in Patent Documents 2 to 5, by-products containing raw metals (such as bismuth) generated in the manufacturing process of BRO oxide are factors that reduce the performance and lifespan of secondary batteries using the BRO oxide as a catalyst. In order to prevent such by-products from remaining in the catalyst material, it was necessary to subject the synthesized BRO oxide to an acid pickling treatment, such as immersing it in an aqueous nitric acid solution. The addition of an acid pickling treatment step increases the environmental load and the manufacturing cost of the BRO oxide catalyst.
[0010] In order to use BRO oxide as a catalyst for electrochemical reactions, in many cases, a powder product of BRO oxide is dispersed in a specific liquid medium to make a suspension or paste, and then the suspension or paste is supported on a conductor. In this process, BRO oxide can exhibit catalytic activity by contacting with substances involved in electrochemical reactions (such as electrolytes and oxygen gas). Therefore, it is expected that the larger the contact area with these substances, the higher the catalytic activity will be, so it is preferable that the specific surface area of BRO oxide is large. BRO oxide powder particles usually exist as secondary particles formed by agglomeration of many primary particles. In general, one of the methods for improving the specific surface area of powder particles is to reduce the particle size (secondary particle diameter) of the powder particles. In addition, reducing the secondary particle diameter is expected to lead to the dispersion stability of BRO oxide in liquid media (when the liquid medium is left to stand, the smaller the particles, the more they will maintain the dispersed state without settling), which is advantageous in terms of production.
[0011] Conventionally, finishing BRO oxide into a powder product consisting of fine particles, for example, having an average particle size on the submicron order, by final dispersion treatment has not been generally performed, as can be seen from the examples of Patent Documents 1 to 5. It is also not known what residual behavior the above-mentioned by-products exhibit after the final dispersion treatment. An object of the present invention is to provide a BRO oxide powder which has a particle size distribution controlled to be advantageous for improving dispersibility in a liquid medium and in which the presence of impurity phases is significantly reduced. [Means for solving the problem]
[0012] According to the research of the inventors, when the BRO oxide synthesized by the conventional process of calcining a precursor formed by a wet oxidation reaction is subjected to a final dispersion treatment to reduce the powder particles, it has been found that the presence of impurity phases containing bismuth (mainly basic carbonates of bismuth) that were not observed before the dispersion treatment becomes apparent. Since basic carbonates of bismuth are thermally decomposed at a temperature lower than the calcination temperature and are therefore considered not to be present in the BRO oxide powder after calcination, it is presumed that the impurity phases that become apparent after the dispersion treatment are formed as carbonates by the excess bismuth components (bismuth hydroxide, bismuth oxide, etc.) that existed between the primary particles being exposed to the surface during the dispersion treatment and reacting with carbon dioxide in the air. If such excess bismuth components are present on the catalyst surface, they may impair the catalytic activity by hindering the movement of substances involved in the electrochemical reaction. Therefore, the inventors have found, as a result of detailed investigation, that by slightly reducing the atomic ratio of bismuth used as a raw material to the total atomic number of ruthenium and manganese, it is possible to significantly prevent the appearance of impurity phases containing bismuth after dispersion treatment. In addition, in Patent Document 1, the atomic ratio of bismuth used as a raw material is set to a range of 0.82 to 1.00 relative to the total atomic number of ruthenium and manganese (as described above). However, no final dispersion treatment is performed to refine the particles, and Patent Document 1 does not teach a method for achieving both refinement and prevention of impurity phase formation.
[0013] The above object can be achieved by the following invention. [1] A powder composed of particles having a crystal structure of a bismuth-ruthenium-oxygen pyrochlore oxide and containing bismuth and ruthenium, or bismuth, ruthenium and manganese as metal elements, in which the cumulative 50% particle size D50 in a volume-based particle size distribution measured by a laser diffraction / scattering method is 3.0 μm or less, and no bismuth-containing phase different from the crystal structure of the pyrochlore oxide is detected in the X-ray diffraction pattern. [2] The pyrochlore oxide powder according to the above [1], in which the atomic ratio of Mn / (Ru+Mn), which represents the atomic ratio of manganese to the total amount of ruthenium and manganese, is 0 or more and 0.35 or less. Effect of the Invention
[0014] The pyrochlore oxide powder according to the present invention is advantageous in improving catalytic activity and dispersibility in a liquid medium because the particle size is controlled to be fine, and the inclusion of impurity phases is significantly reduced, which is advantageous in improving the performance of devices such as secondary batteries using the powder as a catalyst. According to the method for producing pyrochlore oxide powder of the present invention, an acid washing process for removing impurity phases is not required, so that an increase in environmental load is suppressed. In addition, it is possible to significantly increase the amount of metal salt raw material mixed per 1 L of the initial aqueous solution used in the reaction (hereinafter sometimes referred to as the "feed concentration") compared to the feed concentration generally used in laboratory experiments. Therefore, the present invention contributes to the industrial spread of pyrochlore oxide powder. [Brief description of the drawings]
[0015] [Figure 1] FIG. 2 is a diagram illustrating the particle size distribution of the BRO oxide powder obtained in Comparative Example 1 before and after the dispersion treatment. [Diagram 2] FIG. 2 is a diagram illustrating X-ray diffraction patterns of the BRO oxide powder obtained in Comparative Example 1 before and after dispersion treatment. [Diagram 3] The diffraction pattern in Figure 2 is enlarged in the peak height direction. [Figure 4] FIG. 2 is a diagram illustrating the particle size distribution of the BRO oxide powder obtained in Example 1 before and after the dispersion treatment. [Diagram 5] FIG. 2 is a diagram illustrating X-ray diffraction patterns of the BRO oxide powder obtained in Example 1 before and after the dispersion treatment. [Figure 6] The diffraction pattern of Figure 5 enlarged in the peak height direction. [Figure 7]FIG. 4 is a diagram illustrating the particle size distribution of the BRO oxide powder obtained in Example 2 before and after the dispersion treatment. [Figure 8] FIG. 2 is a diagram illustrating X-ray diffraction patterns of the BRO oxide powder obtained in Example 2 before and after dispersion treatment. [Figure 9] FIG. 9 is an enlarged view of the diffraction pattern in FIG. 8 in the peak height direction. [Figure 10] FIG. 1 is a diagram illustrating the particle size distribution of the BRO oxide powder obtained in Example 3 before and after wet dispersion. [Figure 11] FIG. 1 is a diagram illustrating X-ray diffraction patterns of the BRO oxide powder before and after wet dispersion obtained in Example 3. [Figure 12] FIG. 12 is an enlarged view of the diffraction pattern in FIG. 11 in the peak height direction. [Figure 13] FIG. 1 is a diagram illustrating the particle size distribution of the BRO oxide powder obtained in Example 4 before and after wet dispersion. [Figure 14] FIG. 1 is a diagram illustrating X-ray diffraction patterns of the BRO oxide powder before and after wet dispersion obtained in Example 4. [Figure 15] FIG. 15 is an enlarged view of the diffraction pattern in FIG. 14 in the peak height direction. [Figure 16] FIG. 1 is a diagram illustrating X-ray diffraction patterns of BRO oxide powders (obtained in Comparative Example 2 and Examples 5 and 6) having an Mn / (Ru+Mn) atomic ratio of 0.30 before dispersion treatment. [Figure 17] Photographs substituting for drawings showing the appearance of slurries of the BRO oxide powder before and after the dispersion treatment produced in Example 2 at the start of standing. [Figure 18] 18 is a photograph showing the appearance of the liquid in FIG. 17 after it was left to stand for 15 hours. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] [Pyrochlore oxide] The typical formula for pyrochlore oxides is A2B2O xThe term "bismuth-ruthenium-oxygen pyrochlore oxide" refers to a pyrochlore oxide in which the A site is bismuth (Bi) and the B site is ruthenium (Ru). The pyrochlore oxide (BRO oxide) of the present invention has a crystal structure in which diffraction peaks from each crystal plane of the "bismuth-ruthenium-oxygen pyrochlore oxide" are observed in the X-ray diffraction pattern. When manganese is contained as a metal element, it is generally considered to exhibit an atomic arrangement in which a part of the ruthenium atom occupying the B site is replaced by a manganese atom. In addition, an atomic arrangement in which an atom other than bismuth, ruthenium, or manganese replaces a part of the bismuth atom occupying the A site or a part of the ruthenium atom occupying the B site, or enters an interstitial position, is also acceptable as long as it does not impair the effects of the present invention. For example, sodium (Na) atoms, which may be introduced into the liquid during the manufacturing process, are considered to exist in the crystal lattice by replacing a part of the bismuth atom occupying the A site or entering an interstitial position. When manganese or the above-mentioned sodium is present in the crystal lattice, the crystal plane spacing may vary slightly compared to a pure "bismuth-ruthenium-oxygen pyrochlore oxide."
[0017] As described above, manganese can be used as an element to replace a part of ruthenium in BRO oxide, and is useful for saving expensive ruthenium. The Mn / (Ru+Mn) atomic ratio, which represents the atomic ratio of manganese to the total amount of ruthenium and manganese, can be set in the range of 0 to 0.35, and may be controlled to 0.3 or less. When manganese is not contained, the Mn / (Ru+Mn) atomic ratio is 0. When manganese is contained, it is effective to set the Mn / (Ru+Mn) atomic ratio to 0.05 or more, and more effective to set it to 0.1 or more.
[0018] [Particle size distribution] The BRO oxide powder of the present invention has a particle size distribution controlled to a minute average particle size. Specifically, the cumulative 50% particle size D50 in the volume-based particle size distribution by the laser diffraction / scattering method is 3.0 μm or less. Such a small average particle size BRO powder is advantageous in terms of exhibiting good catalytic activity and dispersion maintenance characteristics in a liquid medium. The above D50 is more preferably 2.0 μm or less, and even more preferably 1.0 μm or less. The BRO powder particles can be made fine by, for example, a dispersion treatment using a bead mill, as described later. Excessively making the particles fine leads to a decrease in catalytic activity or a decrease in productivity due to the collapse of the crystal structure. Usually, the above D50 can be adjusted to a range of 0.05 μm or more.
[0019] [Impurity phase] If a bismuth-containing impurity phase exists on the particle surface of the BRO oxide powder, it may hinder the performance improvement of devices such as secondary batteries using the BRO oxide as a catalyst. In the BRO oxide powder of the present invention, no bismuth-containing phase different from the crystal structure of the "bismuth-ruthenium-oxygen pyrochlore oxide" is detected in the X-ray diffraction pattern. A representative example of a bismuth-containing phase different from the crystal structure of the "bismuth-ruthenium-oxygen pyrochlore oxide" is basic carbonate of bismuth (Bi2O2CO3). Such an impurity phase containing bismuth is easily manifested by the final fineness by the dispersion treatment. In addition, if such an impurity phase exists on the surface of the "bismuth-ruthenium-oxygen pyrochlore oxide", it is concerned that the catalytic activity will be reduced. As described later, the formation of the above impurity phase can be prevented by adjusting the blending of the metal salt raw material in the metal salt-containing liquid preparation process.
[0020] [Production method of BRO oxide powder] The BRO oxide powder of the present invention can be obtained by a manufacturing process including, in the above order, a metal salt-containing liquid preparation step, an oxidation step, a drying step, a calcination step, and a dispersion treatment step.
[0021] [Raw material solution preparation process] As raw materials, a bismuth-containing salt (e.g., bismuth (III) nitrate hydrate) and a ruthenium-containing salt (e.g., ruthenium (III) chloride hydrate) are prepared. When manganese is to be added, a manganese-containing salt (e.g., manganese (II) nitrate hydrate) is also prepared. These are mixed in an aqueous solvent to prepare a metal salt-containing liquid. This initial metal salt-containing liquid is referred to as a "raw material solution" in this specification. An aqueous solvent is a liquid medium whose main component is water (i.e., the mass ratio of water is 50% or more). Since the solubility of the bismuth-containing salt and the ruthenium-containing salt in water is low, when they are mixed with water, most of them do not dissolve and exist in the water as a solid, and when they are stirred, they become a slurry state. Therefore, in the present invention, it is preferable to use an aqueous solvent in which an organic substance that serves as a dispersant is dissolved as a secondary component other than water. An example of a dispersant is tetra-n-propylammonium bromide.
[0022] Since the stoichiometric atomic ratio of the A site and the B site of the BRO oxide is 1:1, if it is assumed that bismuth occupies the entire A site and ruthenium and manganese occupy the entire B site, when the raw metal salts are blended so that the Bi / (Ru+Mn) atomic ratio is 1.000, the A site and the B site can be theoretically occupied by each of the above elements without excess or deficiency. However, when the raw material solution is prepared with such a blending, it was found that an impurity phase containing bismuth is formed by performing a final dispersion treatment. Therefore, the inventors conducted detailed studies. As a result, the problem of the impurity phase formation could be solved by setting the Bi / (Ru+Mn) atomic ratio to 0.990 or less when preparing the raw material solution. If the Bi / (Ru+Mn) atomic ratio is too low, the amount of surplus ruthenium increases, which impairs economy. Usually, the Bi / (Ru+Mn) atomic ratio may be set in the range of 0.900 or more, and may be controlled in the range of 0.940 or more.
[0023] When manganese is contained, the Mn / (Ru+Mn) atomic ratio can be set to a range of 0.35 or less, and may be controlled to 0.3 or less. In these cases, it is effective to set the Mn / (Ru+Mn) atomic ratio to 0.05 or more, and more effective to set it to 0.1 or more.
[0024] In preparing the raw material solution, the concentration of the metal salt (molar concentration of the metal salt contained per 1 L of the liquid containing the raw material and the dispersant) is preferably set so that the bismuth content as the number of atoms is 0.1 mol / L or more from the viewpoint of productivity, and more effectively set to 0.3 mol / L or more. If the concentration of the metal salt is too high, the amount of alkali added in the oxidation step described below increases, and the cooling load of the equipment increases and the rate of alkali addition is restricted in order to suppress the heat generation at that time. Usually, the concentration of the metal salt is preferably set so that the bismuth content as the number of atoms is 0.5 mol / L or less. When a dispersant is used, for example, in the case of tetra-n-propylammonium bromide, the dispersant concentration in the raw material solution may be adjusted to a range of 0.05 to 0.50 mol / L.
[0025] [Oxidation process] An alkali is added to the raw material solution, and an oxidation reaction is carried out while supplying oxygen to the liquid, forming a solid reaction product. The higher the liquid temperature, the more favorable it is for the progress of the dissolution-precipitation reaction. On the other hand, from the viewpoint of ensuring safety during work, it is desirable for the liquid temperature to be below the boiling point. Therefore, the liquid temperature is preferably in the range of 50 to 99°C. For example, sodium hydroxide can be used as the alkali. The amount of alkali added is equal to or more than the amount required to react with all of the anions supplied from the metal-containing salts mixed in the liquid (bismuth-containing salt and ruthenium-containing salt, but if manganese-containing salt is mixed, the bismuth-containing salt, ruthenium-containing salt, and manganese-containing salt) mixed in the liquid. The alkali is added by adding all at once, intermittently, or continuously while stirring the liquid so that the liquid temperature does not exceed the above temperature range depending on the cooling capacity of the reaction vessel. Thereafter, the liquid temperature is maintained within the above temperature range, and stirring is continued while oxygen is supplied to the liquid. Oxygen can be supplied by blowing (bubbling) oxygen gas or air into the liquid. At this time, a reaction product is slowly formed as the dissolution and precipitation reaction proceeds. The stirring time under oxygen supply is preferably 1 to 72 hours. The supply of oxygen may be started before the addition of the alkali. In this way, the oxidation reaction proceeds to form a solid reaction product containing bismuth and ruthenium, or further manganese. It is believed that this reaction product is mainly composed of oxyhydroxides of the above metals.
[0026] (Example of a method for calculating the amount of alkali required to react with all of the anions provided by the bismuth-containing salt, the ruthenium-containing salt, and the manganese-containing salt) For example, if NaOH is used as the alkali, in a liquid containing 0.95 mol of Bi(NO3)3·5H2O, 0.7 mol of RuCl3·nH2O, and 0.3 mol of Mn(NO3)2·6H2O, the Na ions, NO3 ions, and Cl ions are all monovalent, so the amount of alkali required to react with all of the anions supplied by the bismuth-containing salt, ruthenium-containing salt, and manganese-containing salt is 3×0.95+3×0.7+2×0.3=5.55 mol.
[0027] [Drying process] The reaction product generated by the oxidation reaction is collected and then dried. One embodiment of the method for collecting the reaction product includes a method in which the liquid containing the reaction product is left to stand for, for example, 24 hours or more to allow the solid content of the reaction product to settle and generate a supernatant, and then the supernatant is removed. If necessary, a sedimentation promotion operation such as centrifugation may be added. It is effective to remove the amount of the supernatant at a volume ratio of, for example, 70% or more relative to the liquid containing the reaction product. The drying can be performed by exposing the reaction product (solid content) together with the remaining liquid components to air at, for example, 80 to 140°C. In this way, a precursor substance is formed. Thereafter, for example, the product can be crushed until it passes through a sieve with an opening of 100 μm, and then dried at a temperature of 180 to 250°C.
[0028] [Firing process] The obtained precursor material is heated in an oxidizing gas atmosphere to be calcined, and an oxide powder composed of particles having a crystal structure of a bismuth-ruthenium-oxygen pyrochlore oxide is synthesized. The calcination temperature is preferably set to 400 to 700°C, and the calcination time is preferably set in the range of 0.1 to 12 hours. Air under atmospheric pressure can be used as the oxidizing gas atmosphere.
[0029] Conventionally, the BRO oxide synthesized by firing is generally subjected to washing and crushing to remove adhering salts as appropriate, and is then used in various applications as a final powder product. In the present invention, the BRO oxide is further subjected to a dispersion treatment after the above steps.
[0030] [Dispersion processing process] The oxide powder synthesized in the firing process and, if necessary, washed with water or crushed to pass through a sieve with a mesh size of, for example, 100 μm is subjected to a dispersion treatment using an aqueous solvent. A bead mill is preferably used as the means. For the beads, ceramic spheres such as zirconia (ZrO2) are preferably used. From the viewpoint of efficiently obtaining pyrochlore oxide powder with a small D50, the average particle size of the beads is preferably 0.03 mm to 10 mm, and more preferably 0.1 mm to 5 mm. This dispersion treatment crushes coarse secondary particles to obtain a powder composed of fine secondary particles. In addition to adjusting the particle size, this dispersion treatment has the effect of washing out impurity components remaining between the primary particles (for example, metal components that are surplus to the formation of BRO oxide crystals, dispersants, and sodium salts derived from the raw materials (sodium chloride, sodium bromide, etc.)). If there is an excess bismuth component (bismuth hydroxide, bismuth oxide, etc.), an impurity phase such as basic carbonate is generated, which is problematically formed on the surface of the particles after the dispersion treatment. In the present invention, the atomic ratio of bismuth is slightly less than equal to the total number of ruthenium and manganese atoms in the raw solution preparation step, thereby avoiding the problem of the formation of the impurity phase. The fine particles obtained by this dispersion treatment provide good catalytic activity and good dispersion retention properties in a liquid medium.
[0031] As described above, the final particle size distribution of the BRO oxide is preferably such that the cumulative 50% particle size D50 in the volume-based particle size distribution by the laser diffraction / scattering method is 3.0 μm or less. The above D50 is more preferably 2.0 μm or less, and even more preferably 1.0 μm or less. Usually, the above D50 can be adjusted to a range of 0.05 μm or more. BRO oxide powder having such a desired particle size distribution can be obtained directly by the above dispersion treatment, but the particle size can also be adjusted by performing a classification operation after the dispersion treatment as necessary. EXAMPLES
[0032] [Comparative Example 1] (Raw material solution preparation process) A 10L separable beaker (manufactured by Asahi Seisakusho) was set on a mantle heater (manufactured by Asahi Seisakusho), and 2500g of pure water was added and heated to 75°C while stirring. An anchor blade was used for stirring, and the stirring speed was set to 200 rpm. 0.521 mol (141.5g) of tetra-n-propylammonium bromide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was dissolved in 500g of pure water and added while stirring. Furthermore, 2.083 mol (1015g) of bismuth (III) nitrate pentahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 2.083 mol (466.3g) of ruthenium (III) chloride n-hydrate (manufactured by Tanaka Kikinzoku Kogyo Co., Ltd.) were prepared as slurries in which they were uniformly mixed in 2000g of pure water and added. The total amount of pure water used was 7000g. After each substance was added, the mixture was stirred for 1 hour at a liquid temperature of 75°C. Since bismuth (III) nitrate pentahydrate and ruthenium (III) chloride n-hydrate have low solubility in water, they could not be completely dissolved even at 75°C, and a slurry-like raw solution was obtained. In this example, no manganese-containing salt was mixed, and the Bi / (Ru+Mn) atomic ratio in this raw solution = Bi / Ru atomic ratio is 1.000. The concentration of the raw metal salts was 0.2976 mol / L in terms of the bismuth content as the number of atoms. This feed concentration was calculated based on the liquid volume being 7 L, which is the total amount of pure water used.
[0033] (oxidation process) A sodium hydroxide solution with a concentration of 18 mol / L was prepared and added to the above raw material solution. The amount of sodium hydroxide added was set to provide an atomic ratio of 1.08 times the amount of sodium required to react with the total amount of anions provided by bismuth (III) nitrate pentahydrate and ruthenium (III) chloride n-hydrate. The entire amount of sodium hydroxide was added over 7.5 minutes to prevent excessive temperature rise. The temperature of the solution during the addition of sodium hydroxide was maintained at approximately 75°C using a temperature controller.
[0034] Next, while blowing pure oxygen gas into the liquid in the reaction vessel, the temperature was maintained at 75°C and stirring was continued for 18 hours to form a solid reaction product. The pure oxygen gas was supplied at a rate of about 100 mL / min per 1 L of liquid in the reaction vessel, calculated as a gas volume at room temperature and atmospheric pressure.
[0035] (Drying process) The liquid in the reaction tank after the stirring (slurry in which the reaction product was suspended) was left to stand for 5 days, and then the supernatant was removed. Finally, by centrifuging, 70% or more of the supernatant was removed relative to the volume of the "liquid in the reaction tank" to recover the reaction product. The recovered reaction product was dried together with the remaining liquid components by holding them in air at 120°C for 18 hours to form a precursor substance.
[0036] This precursor material was crushed into powder, sieved through a sieve with 100 μm openings, dried by keeping the sieve in air at 200° C. for 2 hours, and then crushed in a mortar to prepare a precursor material for firing.
[0037] (Firing process) The above precursor material was calcined in air at 600°C for 1 hour to synthesize BRO oxide.
[0038] The synthesized BRO oxide was stirred and washed with water to remove adhering salts, and then the solid matter was recovered by suction filtration and dried in air at 120°C to obtain BRO oxide powder.
[0039] (Dispersion processing process) 300 g of the obtained BRO oxide powder was subjected to dispersion treatment using a wet bead mill (Imex Co., Ltd., 1 / 2G-SG, vessel capacity 2 L used). Water was used as the solvent for dispersion treatment, and zirconia (ZrO2) beads with a diameter of 1 mm were used as the beads for wet dispersion. The amount of solvent was about 700 g and the amount of zirconia beads was 1200 g for 300 g of BRO oxide powder to be treated, and dispersion treatment was performed for 6 hours at a rotation speed of 1500 rpm, a rotation radius of 45 mm, and a tip peripheral speed of 7 m / s. During the treatment, the solvent temperature was maintained at about 25°C by cooling the container using a chiller. The liquid after the dispersion treatment was subjected to suction filtration to recover the solid matter, which was then dried in air at 100°C to obtain a BRO oxide powder composed of particles refined by the dispersion treatment.
[0040] (Measurement of particle size distribution) The BRO oxide powder before and after the dispersion treatment was added to an aqueous solution containing 0.2% by weight of sodium hexametaphosphate as a dispersant, and ultrasonic cleaning was performed for 5 minutes using an ultrasonic cleaner (AUC-06L, manufactured by AS ONE Corporation). After that, the volume-based particle size distribution was measured using a wet laser diffraction particle size distribution analyzer (MT3300EX, manufactured by Microtrack Bell Corporation) with water as the solvent and a refractive index of the powder of 1.9, by the laser diffraction / scattering method. As a result, the cumulative 50% particle diameter D50 was 7.4 μm before the dispersion treatment and 0.5 μm after the dispersion treatment. The particle size distribution measurements, including D10 and D90, are shown in Table 1 (the same applies to each of the following examples).
[0041] FIG. 1 illustrates the particle size distribution of the BRO oxide powder obtained in this example before and after the dispersion treatment.
[0042] (X-ray diffraction pattern measurement) The X-ray diffraction patterns of the BRO oxide powder before and after the dispersion treatment were measured using an X-ray diffractometer (Rigaku, Ultima IV) under the conditions of Cu-Kα radiation, tube voltage of 40 kV, tube current of 40 mA, measurement step of 0.02 degrees, and scan speed of 0.5 degrees / min.
[0043] Figure 2 shows the X-ray diffraction patterns of the BRO oxide powder obtained in this example before and after the dispersion process. Before the dispersion process, in addition to the diffraction peaks representing the crystal structure of the bismuth-ruthenium-oxygen pyrochlore oxide, no peaks of the bismuth-containing phase different from the crystal structure were observed. However, after the dispersion process, a diffraction peak due to Bi2O2CO3 was observed at the location indicated by the arrow in Figure 2. Figure 3 shows the diffraction pattern in Figure 2 enlarged in the peak height direction. It can be seen that after dispersion treatment, a new diffraction peak (a diffraction peak due to Bi2O2CO3) appears at the diffraction angle 2θ position shown by the dashed line, as indicated by the arrow. In this example, it was not possible to realize a pyrochlore oxide powder in which the cumulative 50% particle size D50 was refined to 3.0 μm or less and in which the bismuth-containing phase was not detected. The results are shown in Table 1 (the same applies to each of the following examples).
[0044] (Measurement of the amount of salt adhering) The adhering salt components were measured for the BRO oxide powder before and after the dispersion process. Br derived from the dispersant tetra-n-propylammonium bromide and Cl derived from the raw material ruthenium (III) chloride n-hydrate were measured using an ion chromatograph (Tosoh Corporation, IC-2100). Na derived from sodium hydroxide was measured using an atomic absorption spectrophotometer (Hitachi High-Tech, ZA3300). The measurement subject was a liquid obtained by adding 50 mL of ultrapure water to 1 g of BRO oxide powder, extracting the adhering components into the liquid, and then filtering it. The amount of attached salts was 640 ppm for Na, 87 ppm for Br, and 103 ppm for Cl before the dispersion treatment, and 160 ppm for Na, 14 ppm for Br, and 18 ppm for Cl after the dispersion treatment.
[0045] [Example 1] In the raw solution preparation step, 0.521 mol of tetra-n-propylammonium bromide, 2.083 mol of bismuth (III) nitrate pentahydrate, and 2.126 mol of ruthenium (III) chloride n-hydrate were mixed to set the Bi / (Ru+Mn) atomic ratio in the raw solution = Bi / Ru atomic ratio to 0.980, except that the BRO oxide powder was produced under the same conditions as in Comparative Example 1. The substances used were the same products as in Comparative Example 1 (the same applies to Comparative Example 2 below). The concentration of the raw metal salt in the raw solution before the addition of alkali prepared was 0.2976 mol / L in terms of the bismuth content as the number of atoms. Measurement of particle size distribution and X-ray diffraction pattern were performed in the same manner as in Comparative Example 1.
[0046] The particle size distribution of the BRO oxide powder obtained in this example before and after the dispersion treatment is illustrated in Figure 4. The cumulative 50% particle size D50 was 7.4 μm before the dispersion treatment and 0.9 μm after the dispersion treatment. Figure 5 shows the X-ray diffraction patterns of the BRO oxide powder obtained in this example before and after the dispersion treatment. Figure 6 shows the diffraction pattern in Figure 5 enlarged in the peak height direction. No peaks of the bismuth-containing phase were observed even after the dispersion treatment. In this example, it was possible to realize a pyrochlore oxide powder in which the cumulative 50% particle size D50 was refined to 3.0 μm or less, in which no bismuth-containing phase was detected.
[0047] [Example 2] In the raw solution preparation step, 0.521 mol of tetra-n-propylammonium bromide, 2.083 mol of bismuth (III) nitrate pentahydrate, and 2.192 mol of ruthenium (III) chloride n-hydrate were mixed to set the Bi / (Ru+Mn) atomic ratio=Bi / Ru atomic ratio in the raw solution to 0.950, and the BRO oxide powder was produced under the same conditions as in Comparative Example 1. The concentration of the raw metal salt in the raw solution before the addition of the alkali prepared was 0.2976 mol / L in terms of the bismuth content as the number of atoms. The particle size distribution and the X-ray diffraction pattern were measured in the same manner as in Comparative Example 1.
[0048] The particle size distribution of the BRO oxide powder obtained in this example before and after the dispersion treatment is illustrated in Figure 7. The cumulative 50% particle size D50 was 7.4 μm before the dispersion treatment and 0.9 μm after the dispersion treatment. Figure 8 shows the X-ray diffraction patterns of the BRO oxide powder obtained in this example before and after the dispersion treatment. Figure 9 shows the diffraction pattern in Figure 8 enlarged in the peak height direction. No peaks of the bismuth-containing phase were observed even after the dispersion treatment. In this example, it was possible to realize a pyrochlore oxide powder in which the cumulative 50% particle size D50 was refined to 3.0 μm or less, in which no bismuth-containing phase was detected.
[0049] [Example 3] In the raw solution preparation step, 0.521 mol of tetra-n-propylammonium bromide, 2.083 mol of bismuth (III) nitrate pentahydrate, and 2.314 mol of ruthenium (III) chloride n-hydrate were mixed to set the Bi / (Ru+Mn) atomic ratio=Bi / Ru atomic ratio in the raw solution to 0.900, and the BRO oxide powder was produced under the same conditions as in Comparative Example 1. The concentration of the raw metal salt in the raw solution before the addition of the alkali prepared was 0.2976 mol / L in terms of the bismuth content as the number of atoms. The particle size distribution and the X-ray diffraction pattern were measured in the same manner as in Comparative Example 1.
[0050] The particle size distribution of the BRO oxide powder obtained in this example before and after the dispersion treatment is illustrated in Figure 10. The cumulative 50% particle size D50 was 4.9 μm before the dispersion treatment and 0.5 μm after the dispersion treatment. Figure 11 shows the X-ray diffraction patterns of the BRO oxide powder obtained in this example before and after the dispersion treatment. Figure 12 shows the diffraction pattern in Figure 11 enlarged in the peak height direction. No peaks of the bismuth-containing phase were observed even after the dispersion treatment. In this example, it was possible to realize a pyrochlore oxide powder in which the cumulative 50% particle size D50 was refined to 3.0 μm or less, in which no bismuth-containing phase was detected.
[0051] [Example 4] In the raw solution preparation step, 0.521 mol of tetra-n-propylammonium bromide, 2.083 mol of bismuth (III) nitrate pentahydrate, and 2.604 mol of ruthenium (III) chloride n-hydrate were mixed to set the Bi / (Ru+Mn) atomic ratio=Bi / Ru atomic ratio in the raw solution to 0.800, and the BRO oxide powder was produced under the same conditions as in Comparative Example 1. The concentration of the raw metal salt in the raw solution before the addition of the alkali prepared was 0.2976 mol / L in terms of the bismuth content as the number of atoms. The particle size distribution and the X-ray diffraction pattern were measured in the same manner as in Comparative Example 1.
[0052] The particle size distribution of the BRO oxide powder obtained in this example before and after the dispersion treatment is illustrated in Figure 13. The cumulative 50% particle size D50 was 4.9 μm before the dispersion treatment and 0.5 μm after the dispersion treatment. Figure 14 shows the X-ray diffraction patterns of the BRO oxide powder obtained in this example before and after the dispersion treatment. Figure 15 shows the diffraction pattern in Figure 14 enlarged in the peak height direction. No peaks of the bismuth-containing phase were observed even after the dispersion treatment. In this example, it was possible to realize a pyrochlore oxide powder in which the cumulative 50% particle size D50 was refined to 3.0 μm or less, in which no bismuth-containing phase was detected.
[0053] [Comparative Example 2] (Raw material solution preparation process) A 1L separable beaker (manufactured by Asahi Seisakusho) was set on a mantle heater (manufactured by Asahi Seisakusho), and 150g of pure water was added and heated to 75°C while stirring. An anchor blade was used for stirring, and the stirring speed was set to 300 rpm. 0.0521 mol (14.15g) of tetra-n-propylammonium bromide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was dissolved in 50g of pure water and added while stirring. Furthermore, 0.2083 mol (101.5g) of bismuth (III) nitrate pentahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 0.1458 mol (32.64g) of ruthenium (III) chloride n-hydrate (manufactured by Tanaka Kikinzoku Kogyo Co., Ltd.) were prepared as slurries in which they were uniformly mixed in 200g of pure water and added. Furthermore, 0.0625 mol (17.94 g) of manganese (II) nitrate hexahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was dissolved in 100 g of pure water and added. The total amount of pure water used was 700 g. After each substance was added, the mixture was stirred for 1 hour at a liquid temperature of 75°C. Since bismuth (III) nitrate pentahydrate and ruthenium (III) chloride n-hydrate have low solubility in water, they could not be completely dissolved even at 75°C, and a slurry-like raw material solution was obtained. In this example, a manganese-containing salt was mixed, and the Bi / (Ru+Mn) atomic ratio in this raw material solution was 1.000 and the Mn / (Ru+Mn) atomic ratio was 30. The concentration of the raw material metal salt was 0.2976 mol / L in terms of the bismuth content as the number of atoms. This feed concentration was calculated based on the liquid volume being 0.7 L, which is the total amount of pure water used.
[0054] (oxidation process) A sodium hydroxide solution with a concentration of 18 mol / L was prepared and added to the above raw material solution. The amount of sodium hydroxide added was set to provide an atomic ratio of 1.08 times the amount of sodium required to react with the total amount of anions provided by bismuth (III) nitrate pentahydrate, ruthenium (III) chloride n-hydrate, and manganese (II) nitrate hexahydrate. The total amount of sodium hydroxide was added over 7.5 minutes to prevent excessive temperature rise. The temperature of the solution during the addition of sodium hydroxide was maintained at approximately 75°C using a temperature controller.
[0055] Next, while blowing pure oxygen gas into the liquid in the reaction vessel, the temperature was maintained at 75°C and stirring was continued for 18 hours to form a solid reaction product. The pure oxygen gas was supplied at a rate of about 100 mL / min per 1 L of liquid in the reaction vessel, calculated as a gas volume at room temperature and atmospheric pressure.
[0056] Using this reaction product, the steps after the "drying step" described in Comparative Example 1 were carried out in the same manner as in Comparative Example 1 to produce BRO oxide powder. Measurement of particle size distribution and measurement of X-ray diffraction pattern were carried out in the same manner as in Comparative Example 1.
[0057] The cumulative 50% particle size D50 of the BRO oxide powder obtained in this example was 12.2 μm before the dispersion treatment. FIG. 16 shows examples of X-ray diffraction patterns before dispersion treatment for a BRO oxide powder with an Mn / (Ru+Mn) atomic ratio of 0.30 when the Bi / (Ru+Mn) atomic ratio of the raw material solution is 1.000 (this example), 0.980 (Example 5 described below), and 0.950 (Example 6 described below). In the BRO oxide powder obtained in this example, a diffraction peak due to Bi2O2CO3 was observed at the location indicated by the arrow in FIG. 16 before the dispersion treatment.
[0058] [Example 5] In the raw material solution preparation step, 0.0521 mol of tetra-n-propylammonium bromide, 0.2083 mol of bismuth (III) nitrate pentahydrate, 0.1488 mol of ruthenium (III) chloride n-hydrate, and 0.0638 mol of manganese (II) nitrate hexahydrate were mixed to set the Bi / (Ru+Mn) atomic ratio in the raw material solution to 0.980, so that the BRO oxide powder was prepared under the same conditions as in Comparative Example 2. The substances used were the same products as in Comparative Example 2. The concentration of the raw material metal salt in the prepared raw material solution was 0.2976 mol / L in terms of the bismuth content as the number of atoms. The particle size distribution and the X-ray diffraction pattern were measured in the same manner as in Comparative Example 1.
[0059] In the X-ray diffraction pattern for the BRO oxide powder obtained in this example after the dispersion treatment, no peak of the bismuth-containing phase was observed, similar to that before the dispersion treatment (see FIG. 16). In this example, it was possible to realize a pyrochlore oxide powder in which the cumulative 50% particle size D50 was refined to 3.0 μm or less, in which no bismuth-containing phase was detected.
[0060] [Example 6] In the raw solution preparation step, 0.0521 mol of tetra-n-propylammonium bromide, 0.2083 mol of bismuth (III) nitrate pentahydrate, 0.1535 mol of ruthenium (III) chloride n-hydrate, and 0.0658 mol of manganese (II) nitrate hexahydrate were mixed to set the Bi / (Ru+Mn) atomic ratio in the raw solution to 0.950, to produce BRO oxide powder under the same conditions as in Comparative Example 2. The concentration of the raw metal salt in the prepared raw solution was 0.2976 mol / L in terms of the bismuth content as the number of atoms. Measurement of particle size distribution and measurement of X-ray diffraction pattern were performed in the same manner as in Comparative Example 1.
[0061] The cumulative 50% particle size D50 of the BRO oxide powder obtained in this example was 3.9 μm before the dispersion treatment and 0.33 μm after the dispersion treatment. In the X-ray diffraction pattern for the BRO oxide powder obtained in this example after the dispersion treatment, no peak of the bismuth-containing phase was observed, similar to that before the dispersion treatment (see FIG. 16). In this example, it was possible to realize a pyrochlore oxide powder in which the cumulative 50% particle size D50 was refined to 3.0 μm or less, in which no bismuth-containing phase was detected.
[0062] [Table 1]
[0063] [Comparison of BRO oxide powder dispersibility in liquid before and after dispersion treatment] For the BRO oxide powder before and after the dispersion treatment produced in Example 2, sodium hexametaphosphate was added to the dispersant, and ultrasonic cleaning was performed for 5 minutes using an ultrasonic cleaner (AUC-06L, manufactured by AS ONE Corporation) to produce a slurry-like liquid, which was then allowed to stand at room temperature. Figure 17 shows an example of the appearance of the liquid at the start of the standing, and Figure 18 shows an example of the appearance of the liquid after standing for 15 hours. It can be seen that the dispersibility of the BRO oxide powder in the liquid is significantly improved by refining the particles by the dispersion treatment.
Claims
1. The pyrochlore oxide powder has a crystal structure of a bismuth-ruthenium-oxygen pyrochlore oxide and is composed of particles containing bismuth and ruthenium, or bismuth, ruthenium and manganese as metal elements, wherein the cumulative 50% particle diameter D50 in a volume-based particle size distribution measured by a laser diffraction / scattering method is 3.0 μm or less, and no bismuth-containing phase different from the crystal structure of the pyrochlore oxide is detected in an X-ray diffraction pattern.
2. 2. The pyrochlore oxide powder according to claim 1, wherein the atomic ratio of Mn / (Ru+Mn), which represents the atomic ratio of manganese to the total amount of ruthenium and manganese, is 0 or more and 0.35 or less.
Citation Information
Patent Citations
Manufacturing method of catalyst for air secondary battery, manufacturing method of air secondary battery, catalyst for air secondary battery, and air secondary battery
JP2019179592A
Air electrode catalyst for air secondary battery, manufacturing method of air electrode catalyst, and air secondary battery
JP2020080291A
Air electrode catalyst for air secondary battery and air secondary battery
JP2020126754A
Air electrode catalyst for air secondary battery, manufacturing method thereof, and air secondary battery
JP2021099914A
Oxygen catalyst and electrode using said oxygen catalyst
WO2020153401A1
Cited By
Secondary battery and electronic device
CN121905862A
マンガン含有パイロクロア酸化物粉体およびその製造方法
JP2026184162A