Structure and design method therefor
By integrating stress-absorbing and fastening reinforcing layers with specific fiber orientations, the structure enhances the fastening strength of laminated UD sheets, addressing stress concentration issues and improving durability.
Patent Information
- Application Number
- JP2023046575
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Reinforcing materials made by laminating and fusing UD sheets face issues with fastening strength when subjected to external forces, as stress concentration can lead to destruction at fastening points, and increasing the number of fastening members does not always improve strength.
Incorporating stress-absorbing layers with reinforcing fibers oriented at ±60°±15° and fastening reinforcing layers with fibers oriented at 0°±15° within the laminate structure to distribute and absorb stress effectively, thereby enhancing fastening strength.
The proposed structure and design method increase the fastening strength of reinforcing materials by distributing stress, preventing destruction at fastening points even when external forces are applied.
Smart Images

Figure 2024135736000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a structure and a design method thereof. [Background technology]
[0002] A thin-film fiber-reinforced resin (hereinafter, simply referred to as "Uni-Directional (UD) sheet") is known, which contains a plurality of reinforcing fibers oriented in one direction and a resin composition (matrix resin) impregnated into the reinforcing fibers. This UD sheet is lighter than metal and has high mechanical strength, and therefore, it is being considered to use it as a reinforcing material by laminating a plurality of sheets, fusing them together, and placing them on the surface of the mating member to be reinforced. The placement on the surface of the mating member may be performed by fastening (for example, Patent Document 1, etc.). In addition, by stacking and fusing multiple UD sheets with the orientation direction of the reinforcing fibers changed for each layer, the strength of the reinforcing material in multiple directions can be increased (for example, Patent Document 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-114139 A [Patent Document 2] JP 2022-103810 A Summary of the Invention [Problem to be solved by the invention]
[0004] Incidentally, a member (structure) reinforced by a reinforcing material formed by laminating and fusing UD sheets may itself be used as a reinforcing member for a moving body, etc. According to the findings of the present inventors, such a reinforcing member has a problem that the fastening portion of the reinforcing member with the mating member may be easily broken when subjected to an external force. When an attempt was made to distribute the stress at the fastening portion by increasing the number of fastening members, the breakage of the reinforcing member in the fastening region with the mating member was sometimes suppressed and sometimes not suppressed, and the fastening strength was not always improved.
[0005] The present invention has been made in consideration of the above problems, and has an object to provide a structure in which a reinforcing material made of laminated and fused UD sheets is fastened to a mating member, and in which the fastening strength of the reinforcing material to the mating member can be increased when the fastening strength of the reinforcing material to the mating member cannot be increased even by increasing the number of fastening members, and a method for designing such a structure. [Means for solving the problem]
[0006] One aspect of the present invention for solving the above problems relates to the following structures [1] to [9]. [1] A stress member that generates stress when subjected to an external force; a reinforcing member fastened to the stress member by a fastening member; The reinforcing material is a laminate formed by fusing a fiber-reinforced resin containing a plurality of reinforcing fibers oriented in one direction and a matrix resin, The laminate has a stress absorbing layer in which the reinforcing fibers are oriented at an angle of ±60°±15° with respect to the direction of stress generated at the position of the fastening member of the stress member when an external force is applied, and a fastening reinforcement layer in which the reinforcing fibers are oriented at an angle of 0°±15°. structure. [2] When the stress member is subjected to an external force, a first stress having the largest amount of energy is generated, and a second stress having an amount of energy smaller than the first stress is generated at the position of the fastening member; The laminate has a stress absorbing layer in which the reinforcing fibers are oriented at an angle of ±60°±15° with respect to the direction of the second stress, and a fastening reinforcement layer in which the reinforcing fibers are oriented at an angle of 0°±15°, [1] The structure described in. [3] When the stress member is subjected to an external force, the second stress is generated at the position of the fastening member in a direction different from that of the first stress. [2] The structure described in. [4] The fastening reinforcement layer is disposed as the outermost layer of the reinforcement material. The structure according to any one of [1] to [3]. [5] The stress absorption layer is a layer in which the reinforcing fibers are oriented at +60°±15° and a layer in which the reinforcing fibers are oriented at -60°±15°, which are continuously arranged in the stacking direction. The structure according to any one of [1] to [4]. [6] A columnar structure. The fastening member is disposed on the side surface of the columnar member. The structure according to any one of [1] to [5]. [7] A structure having a hat-shaped cross section having a top surface portion, a side surface portion, and a flange portion, The fastening member is disposed on the side surface portion or the flange portion, The structure according to any one of [1] to [6]. [8] A columnar structure. The fastening member is disposed at an end portion of the column in the longitudinal direction. The structure according to any one of [1] to [7]. [9] A pillar in an automobile. The structure according to any one of [1] to [8].
[0007] Another aspect of the present invention for solving the above problem relates to a method for designing a structure as described below in
[10] .
[10] A process of analyzing the direction of stress generated at the position of the fastening member of a structure having a stress member that generates stress when subjected to an external force and a reinforcing material fastened to the stress member by a fastening member, the reinforcing material being a laminate formed by fusing a fiber-reinforced resin containing a plurality of reinforcing fibers oriented in one direction and a matrix resin; A step of determining whether the laminate includes a stress absorbing layer in which the reinforcing fibers are oriented at an angle of ±60°±15° with respect to the direction of stress generated at the position of the fastening member of the stress member when an external force is applied; When it is determined that the stress absorption layer is included, a step of determining that the laminate is provided with a fastening reinforcement layer in which the reinforcing fibers are oriented at 0°±15° with respect to the direction of the stress generated at the position of the fastening member; A method for designing a structure comprising the steps of: Effect of the Invention
[0008] According to the present invention, there is provided a structure in which a reinforcing material made by stacking and fusing UD sheets is fastened to a mating member, and when the fastening strength of the reinforcing material to the mating member cannot be increased even by increasing the number of fastening members, there is provided a structure that can increase the fastening strength of the reinforcing material to the mating member, and a method for designing this structure. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is an external view showing a schematic configuration of a structure according to a first embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing the direction of stress generated in the columnar member shown in FIG. 1 when the top surface of the columnar member receives an impact in the direction opposite to the Z direction in the figure. [Diagram 3] FIG. 3 is a schematic diagram illustrating the layer structure of the reinforcing material. [Figure 4] FIG. 4 is a schematic diagram showing another configuration and layer configuration of a structure having columnar members (stress members), reinforcing materials, and fastening members. [Diagram 5]FIG. 5 is a schematic diagram showing another configuration and layer configuration of a structure having columnar members (stress members), reinforcing materials, and fastening members. [Figure 6] FIG. 6 is a schematic diagram showing another configuration and layer configuration of a structure having columnar members (stress members), reinforcing materials, and fastening members. [Figure 7] FIG. 7 is a flowchart showing a method for designing a structure. [Figure 8] FIG. 8 is a schematic diagram showing the arrangement of the test specimen and the aluminum plate in the examples. [Figure 9] 9A to 9D are schematic diagrams showing fastening positions in an embodiment. [Figure 10] FIG. 10 is a graph showing the results of Experiment 1. [Figure 11] FIG. 11 is a graph showing the results of Experiment 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] [Structure configuration] 1 is an external view showing a schematic configuration of a structure according to a first embodiment of the present invention. The structure 100 has a columnar member 110, a reinforcing member 120 disposed on the surface of the columnar member 110, and a plurality of fastening members 130 for fastening the reinforcing member 120 to the columnar member 110.
[0011] The columnar member 110 has a generally rectangular top surface portion 112 extending in one direction (Y direction in the figure), side surface portions 114 extending vertically in the same direction (opposite to the Z direction in the figure) from both ends (both ends in the X direction in the figure) of the top surface portion 112, and a pair of flange portions 116 extending laterally (in the X direction and the opposite direction in the figure) from the lower ends of the side surface portion 114. The top surface portion 112, the side surface portion 114, and the flange portions 116 are metal or resin plate-like portions having the same thickness, and are connected at their respective X direction ends, so that the cross section parallel to the X direction as a whole has a hat shape.
[0012] In the columnar member 110 shown in Fig. 1, the top surface portion 112, the side surface portion 114, and the flange portion 116 all have the same length in the Y direction, but these may vary. In the columnar member 110 shown in Fig. 1, the height in the Z direction of the side surface portion 114 is constant throughout the Y direction, but these may vary depending on the location. In the columnar member shown in Fig. 1, the width in the X direction of the top surface portion 112 and the flange portion 116 is constant throughout the Y direction, but these may vary depending on the location.
[0013] The reinforcing material 120 is formed by laminating and fusing together a plurality of thin-film fiber-reinforced resin sheets (UD sheets) containing a plurality of reinforcing fibers oriented in one direction and a resin composition (matrix resin) impregnated into the reinforcing fibers. The reinforcing material 120 is disposed on the surface of the top surface portion 112 side (Z direction side) of the flange portion 116, and is fastened to the flange portion 116 by a plurality of fastening members 130.
[0014] There are no particular limitations on the planar shape and thickness of the reinforcing material 120, and any shape may be used depending on the application. The thickness of the reinforcing material 120 is preferably 1 mm or more and 4 mm or less.
[0015] In this embodiment, the fastening member 130 is a self-piercing rivet that penetrates the reinforcing member 120 and is inserted into the columnar member 110. However, the type of the fastening member 130 is not limited to this, and may be another type of rivet, a bolt and nut, or a screw without a nut.
[0016] The columnar member 110 is itself a reinforcing member, and is used to receive and absorb the load of an impact when the top surface portion 112 receives the impact in the direction opposite to the Z direction in the figure, thereby preventing other members from being destroyed. When the columnar member 110 receives an impact (external force), it generates stress within the member to mitigate the external force. The columnar member 110 is an example of a stress member in this embodiment.
[0017] Fig. 2 is a schematic diagram showing the direction of stress generated in the columnar member 110 shown in Fig. 1 when the columnar member 110 receives an impact on the top surface in the opposite direction to the Z direction in the figure. As shown in Fig. 2, when the columnar member 110 receives an external force EF on the top surface portion 112 in the opposite direction to the Z direction in the figure, a first stress F1 is generated in the entire columnar member 110 (top surface portion 112, side surface portion 114, and flange portion 116) in the column extension direction (Y direction in the figure). The first stress F1 is the stress with the largest amount of energy generated inside the columnar member 110 by the external force EF.
[0018] On the other hand, when the columnar member 110 receives an external force EF, the top surface portion 112 bends downward (the opposite direction to the Z direction in the figure), and the pair of side portions 114 and the pair of flange portions 116 are deformed so as to move away from each other. At this time, stress is generated in the side portion 114 and the flange portion 116 in the direction of moving away from each other (the X direction in the figure and the opposite direction). If the fastening member 130 is present at the location where this stress is generated, the stress tends to concentrate at the position of the fastening member 130 (the stress generated at the position of the fastening member 130 in this way is referred to as stress F2). The magnitude of the second stress F2 is smaller than the first stress F1.
[0019] FIG. 3 is a schematic diagram illustrating the layer structure of the reinforcing material 120. As shown in FIG.
[0020] In the reinforcing material 120, a plurality of UD sheets are laminated so that the reinforcing fibers are oriented at a predetermined angle (±30°±15° in this embodiment) with respect to the direction of the first stress F1 (Y direction in the figure) so as to enhance the reinforcing effect against the first stress F1 having the largest energy amount. As a result, a plurality of UD sheets are laminated and fused to each other so that the reinforcing fibers are oriented in a direction of ±60°±15° with respect to the direction of the second stress F2 (X direction in the figure). As shown in FIG. 3, in the reinforcing material 120 of this embodiment, a layer 124 in which the reinforcing fibers are oriented at +60° with respect to the direction of the second stress F2 and a layer 126 in which the reinforcing fibers are oriented at -60° with respect to the direction of the second stress F2 are laminated in a plurality of layers. The layer 124 and the layer 126 are examples of stress absorbing layers for enhancing the stress absorption of the reinforcing material 120.
[0021] However, depending on layers 124 and 126 in which reinforcing fibers are oriented at a predetermined angle with respect to the direction of first stress F1 (Y direction and the opposite direction in the figure), the strength against second stress F2 (stress in X direction and the opposite direction in the figure) may not be increased. If second stress F2 in X direction and the opposite direction in the figure is generated by external force EF and this stress is concentrated at the position where fastening member 130 penetrates reinforcing material 120, reinforcing material 120 may be destroyed at the position of fastening member 130.
[0022] According to the findings of the inventors, when the orientation angle of the reinforcing fibers in the stress absorbing layer included in the reinforcing material 120 is ±60°±15° with respect to the direction of the second stress F2 (X direction in the figure), the fastening strength cannot be increased even by increasing the number of fastening members 130. The reason for this is unclear, but it is thought that it is probably because when the reinforcing fibers are oriented in a direction that is ±60°±15° with respect to the direction of the second stress F2, the reinforcing material is easily stretched by the second stress F2 and is unable to fully absorb the stress.
[0023] Therefore, in this embodiment, the reinforcing material 120 is provided with layers 122 and 128 in which the reinforcing fibers are oriented at an angle of 0°±15° with respect to the direction of the second stress F2 (the X direction in the figure and the opposite direction). These layers 122 and 128 are examples of fastening reinforcement layers that prevent the reinforcing material 120 from being destroyed by the second stress F2 generated at the position of the fastening member 130, thereby increasing the fastening strength.
[0024] The position of the fastening reinforcement layer is not limited, and it may be disposed as the outermost layer (layer 122 and / or layer 128) of the reinforcement material 120, or may be disposed sandwiched between other layers inside the stacking direction of the reinforcement material 120. When the fastening reinforcement layer is disposed inside the stacking direction of the reinforcement material 120, it is preferable that the fastening reinforcement layer is disposed in the center of the stacking direction of the reinforcement material 120. In other words, it is preferable that the number of stress absorption layers disposed on one side of the fastening reinforcement layer in the stacking direction is the same as the number of stress absorption layers disposed on the other side of the stacking direction.
[0025] The number of fastening layers is not limited, and may be one or more. According to the knowledge of the inventors, even one fastening layer can sufficiently increase the fastening strength. Therefore, it is preferable to arrange the fastening layers one layer above and one layer below the outermost layer of the reinforcing material 120, or one layer in the center of the layering direction of the foot race.
[0026] The number of stress absorbing layers is not particularly limited, and can be determined according to the stress absorbing property required for the reinforcing material 120. The arrangement of the stress absorbing layers is not particularly limited, but in order to prevent bias in the stress absorbing property, it is preferable that the layer 124 in which the reinforcing fibers are oriented at +60°±15° with respect to the direction of the second stress F2 and the layer 126 in which the reinforcing fibers are oriented at -60°±15° with respect to the direction of the second stress F2 are arranged continuously in the stacking direction. In addition, it is preferable that more than half of the layers constituting the reinforcing material 120 are stress absorbing layers in which the reinforcing fibers are oriented at ±60°±15°, and it is more preferable that all layers except the fastening reinforcement layer are stress absorbing layers in which the reinforcing fibers are oriented at ±60°±15°.
[0027] Fig. 4 is a schematic diagram showing another configuration and layer configuration of a structure 400 having a columnar member 410 (stress member), a reinforcing member 420, and a fastening member 430. Fig. 5 is a schematic diagram showing another configuration and layer configuration of a structure 500 having a columnar member 510 (stress member), a reinforcing member 520, and a fastening member 530.
[0028] In FIG. 4, a columnar reinforcement member 420 (since FIG. 4 is a plan view, it is shown in a rectangular shape) extending in one direction is fastened to a columnar member 410 at its short side end by a plurality of fastening members 430. In FIG. 5, a columnar reinforcement member 520 (since FIG. 5 is a plan view, it is shown in a rectangular shape) extending in one direction is fastened to a columnar member 510 at its long side end by a plurality of fastening members 530. In both FIG. 4 and FIG. 5, the direction of the first stress F1 is the vertical direction in the figure. However, the direction of the second stress F2 is the vertical direction in the figure like the first stress F1 in FIG. 4, and is the horizontal direction in the figure unlike the first stress F1 in FIG. 5. Note that, as shown in FIG. 4 and FIG. 5, the direction of the second stress F2 at the position of the fastening member may be the direction connecting the fastening member and the end of the reinforcing member 120 closest to the fastening member, but is not limited thereto.
[0029] Even in these cases, when the reinforcing material 420 and the reinforcing material 520 have layers 424 and 426, and layers 524 and 526, which are stress absorbing layers in which a plurality of UD sheets are laminated and fused to each other so that the reinforcing fibers are oriented in a direction of ±60°±15° with respect to the direction of the second stress F2, the fastening strength cannot be increased even by increasing the number of fastening members 430 or fastening members 530. Therefore, in these cases, the fastening strength of the reinforcing material 120 can be increased by providing layers 422 and 428, and layers 522 and 528, which are fastening reinforcing layers in which the reinforcing fibers are oriented at an angle of 0°±15° with respect to the direction of the second stress F2.
[0030] The fastening reinforcement layer may be provided when a layer is formed in which the reinforcing fibers are oriented in a direction that is ±60°±15° relative to the direction of the second stress F2, as in each of the above-mentioned embodiments, or when only layers in which the reinforcing fibers are oriented in a direction that is ±60°±15° relative to the direction of the second stress F2 are stacked. When there is no layer oriented in this way, the fastening reinforcement layer does not need to be provided.
[0031] In addition, as shown in Figures 3 and 5, when the direction of the first stress F1 generated in the stress member by the external force EF differs from the direction of the first stress F3 generated in the fastening portion by the external force EF, the fastening portion is likely to be destroyed, and the effect of improving the fastening strength by the fastening reinforcement layer is remarkable.
[0032] Fig. 6 is a schematic diagram showing yet another configuration and layer configuration of a structure having a columnar member 610 (stress member), a reinforcing member 620, and a fastening member 630. The structure 600 shown in Fig. 6 has a shape in which the columnar member 610 is bent halfway. The columnar member 610 is fastened to the columnar member 610 by a plurality of fastening members 630 at the end of the columnar member 610 in the short side direction in a plan view. In the structure 600 shown in Fig. 6, a second stress F2 in a different direction is generated at each position where the plurality of fastening members 630 are arranged.
[0033] In this case, depending on the orientation direction of the reinforcing fibers of the UD sheet constituting the reinforcing material 620 (usually determined according to the direction of the first stress F1), the reinforcing material 620 may include a stress absorbing layer in which the reinforcing fibers are oriented in a direction of ±60°±15° with respect to the direction of the second stress F2 at any of the positions of the fastening members 630. For example, in the structure 600 shown in FIG. 6, the reinforcing material 620 includes layers 624 and 626, which are stress absorbing layers in which the reinforcing fibers are oriented in a direction of ±60°±15° with respect to the direction of the second stress F2 at the position of the fastening member 630a. In this case, the reinforcing material 620 may include layers 622 and 628, which are fastening reinforcement layers in which the reinforcing fibers are oriented at an angle of 0°±15° with respect to the direction of the second stress F2 at the position of the fastening member 630a.
[0034] The UD sheets forming each layer each contain a plurality of reinforcing fibers 210 oriented in one direction, and a matrix resin 220 impregnated into the reinforcing fibers 210.
[0035] There is no particular limitation on the material of the reinforcing fiber 210. For example, carbon fiber, glass fiber, aramid fiber, alumina fiber, silicon carbide fiber, boron fiber, metal fiber, etc. can be used as the reinforcing fiber. Among these, carbon fiber and glass fiber are preferable.
[0036] From the viewpoint of sufficiently enhancing the effect of improving the strength by the reinforcing fibers 210, the average diameter of the reinforcing fibers 210 is preferably 1 μm or more and 20 μm or less, and more preferably 4 μm or more and 10 μm or less.
[0037] The length of the reinforcing fiber 210 is usually 15 mm or more. The lower limit of the length of the reinforcing fiber 210 is preferably 20 mm or more, more preferably 100 mm or more, and even more preferably 500 mm or more. The maximum upper limit of the length of the reinforcing fiber 210 is, for example, 50 m.
[0038] Furthermore, the reinforcing fibers 210 may be subjected to a sizing treatment using a sizing agent.
[0039] The sizing agent is not particularly limited, but is preferably a modified polyolefin, more preferably a modified polyolefin containing a metal carboxylate. The modified polyolefin is, for example, a polyolefin in which a carboxylic acid group, a carboxylic anhydride group or a carboxylic ester group is grafted onto the polymer chain of an unmodified polyolefin, and a salt is formed between the functional group and a metal cation.
[0040] The unmodified polyolefin is preferably an ethylene-based polymer having 50 mol% or more of structural units derived from ethylene, or a propylene-based polymer having 50 mol% or more of structural units derived from propylene. Examples of the ethylene-based polymer include ethylene homopolymers and copolymers of ethylene and α-olefins having 3 to 10 carbon atoms. Examples of the propylene-based polymer include propylene homopolymers and copolymers of propylene and ethylene or α-olefins having 4 to 10 carbon atoms. The unmodified polyolefin is preferably homopolypropylene, homopolyethylene, ethylene-propylene copolymer, propylene-1-butene copolymer, or ethylene-propylene-1-butene copolymer. The α-olefins constituting these unmodified polyolefins and modified polyolefins may be derived from fossil fuels, may be derived from biomass raw materials, or may be mixtures thereof.
[0041] The reinforcing fibers 210 may be bundled and then opened. In this case, the number of single fibers per bundle of carbon fibers is preferably 100 or more and 100,000 or less, and more preferably 1,000 or more and 50,000 or less.
[0042] The content of the reinforcing fibers 210 relative to the total mass of each fiber reinforced resin is preferably 20 mass% or more and 80 mass% or less, more preferably 30 mass% or more and 75 mass% or less, even more preferably 30 mass% or more and 65 mass% or less, and particularly preferably 35 mass% or more and 60 mass% or less.
[0043] The content of reinforcing fibers 210 relative to the total volume of each fiber reinforced resin is preferably 10 volume % or more and 70 volume % or less, more preferably 15 volume % or more and 60 volume % or less, and even more preferably 20 volume % or more and 60 volume % or less.
[0044] The material of the matrix resin 220 is not particularly limited, and the matrix resin 220 may be a thermoplastic resin or a thermosetting resin. The matrix resin 220 may be a crystalline resin or a non-crystalline resin. These thermoplastic resins and thermosetting resins may be derived from fossil fuels, may be derived from biomass raw materials, or may be a mixture of these.
[0045] Examples of the thermoplastic resin include polyolefin resins such as polyethylene, polypropylene, polybutene, and poly4-methyl-1-pentene, polyamide resins, polyester resins, polystyrene resins, thermoplastic polyimide resins, polyamideimide resins, polycarbonate resins, polyphenylene ether resins, polyphenylene sulfide resins, polyacetal resins, acrylic resins, polyetherimide resins, polysulfone resins, polyether ketone resins, polyether ether ketone resins, polyarylate resins, polyether nitrile resins, vinyl chloride resins, ABS resins, and fluororesins.
[0046] Examples of the thermosetting resin include epoxy resin, phenol resin, melamine resin, urea resin, diallyl phthalate resin, silicone resin, urethane resin, furan resin, ketone resin, xylene resin, thermosetting polyimide resin, unsaturated polyester resin, and diallyl terephthalate resin.
[0047] Among these, thermoplastic resins are preferred from the viewpoint of further improving the moldability of the reinforcing material 120. Among the thermoplastic resins, polyamide resins and polyolefin resins are preferred, and polyolefin resins are more preferred from the viewpoint of enabling molding at lower temperatures and further improving production efficiency.
[0048] The matrix resin 220 may be a resin composition containing an additive. Examples of the additive include known fillers (inorganic fillers, organic fillers), pigments, dyes, weathering stabilizers, heat stabilizers, antistatic agents, antislip agents, antioxidants, antifungal agents, antibacterial agents, flame retardants, and softeners. For example, when the reinforcing material 120 is formed by fusing the UD sheet by irradiating a laser, the matrix resin 220 is preferably a resin composition containing a dye that absorbs the laser of the irradiated wavelength. The dye may be any dye that absorbs light of any wavelength between 300 nm and 3000 nm, and is preferably carbon black.
[0049] Furthermore, the matrix resin 220 may contain other components such as resins other than those mentioned above, or short fibers having a length shorter than that of the reinforcing fibers mentioned above.
[0050] The content of matrix resin 220 relative to the total mass of each fiber reinforced resin is preferably 20 mass% or more and 80 mass% or less, more preferably 25 mass% or more and 70 mass% or less, even more preferably 35 mass% or more and 70 mass% or less, and particularly preferably 40 mass% or more and 65 mass% or less.
[0051] [Method of designing a structure, manufacturing method of reinforcement material, manufacturing method of a structure] FIG. 7 is a flow chart showing a method for designing the above-mentioned structure.
[0052] First, it is determined how to arrange the reinforcing material with respect to the stress member, and it is determined at what position the reinforcing material is to be fastened (step S710). Specifically, it is determined where to arrange the reinforcing material to obtain the desired strength improvement effect for the stress member, whose shape is determined according to the application. At this time, it is also determined the orientation direction of the reinforcing fibers in each layer contained in the reinforcing material according to the strength improvement effect. At this time, it is also determined the fastening method, etc.
[0053] Next, when the structure is subjected to an external force EF, the stress generated in the stress member is analyzed (step S720). The analysis can be performed using known software. At this time, among the stresses generated in the stress member, the stress with the largest amount of energy is defined as the first stress F1, and the stress generated at the position of the fastening member and smaller than the first stress F1 is defined as the second stress F2. Then, the directions of the first stress F1 and the second stress F2 are specified. Note that, when the structure is subjected to an external force EF from different directions depending on the application, the first stress F1 and the second stress F2 may be determined based on the external force from the direction in which the largest stress is generated in the stress member.
[0054] Next, the angle difference between the orientation direction of the reinforcing fibers in each layer included in the reinforcing material and the second stress F2 is calculated. Then, it is determined whether the reinforcing material includes a stress absorbing layer in which the reinforcing fibers are oriented in a direction of ±60°±15° with respect to the direction of the second stress F2 (step S730). As shown in FIG. 6, when the direction of the second stress F2 differs for each position of the multiple fastening members, if there is at least one position of the fastening member where there is a stress absorbing layer in which the reinforcing fibers are oriented in a direction of ±60°±15° with respect to the direction of the second stress F2, it is determined that the reinforcing material includes the above-mentioned stress absorbing layer.
[0055] When it is determined in the previous step that the reinforcing material includes a stress absorbing layer in which reinforcing fibers are oriented in a direction of ±60°±15° relative to the direction of the second stress, the layer configuration of the reinforcing material is determined so that the reinforcing material includes a fastening reinforcement layer in which reinforcing fibers are oriented in a direction of ±0°±10° relative to the direction of the second stress (step S740). When it is determined that the reinforcing material does not include a stress absorbing layer in which reinforcing fibers are oriented in a direction of ±60°±15° relative to the direction of the second stress, the reinforcing material may include the fastening reinforcement layer or may not include the fastening reinforcement layer.
[0056] In this way, the structure can be designed so that the reinforcement material includes a fastening reinforcement layer depending on the relationship between the direction of the second stress F2 at the position of the fastening member and the orientation direction of the reinforcing fibers.
[0057] Once the structure is designed, the reinforcing material to be included in the structure is manufactured. Specifically, multiple UD sheets are laminated so that the orientation direction of the reinforcing fibers corresponds to the layer structure of the reinforcing material in the designed structure. When the UD sheets contain a thermoplastic resin as the matrix resin, the laminated UD sheets can be heated and pressurized to fuse them together. When the UD sheets contain a thermosetting resin as the matrix resin, the laminated UD sheets can be cured by heat or the like to fuse them together.
[0058] The reinforcing material thus manufactured is fastened to a stress member at a position according to the design of the structure, thereby making it possible to manufacture the above-mentioned structure.
[0059] It should be noted that the above description is merely an illustrative embodiment of the present invention, and it goes without saying that the present invention is not limited to the above embodiment.
[0060] For example, in the structure illustrated in FIG. 1, the reinforcing material is fastened to the flange portion of the columnar member having a hat-shaped cross section, but it may also be fastened to the side portion or the like.
[0061] Furthermore, the shape of the stress member is not particularly limited, and may be a columnar shape other than a hat-shaped cross section, or may be another shape.
[0062] The above-described structures can be used for A-, B-, C- and D-pillars in automobiles, flooring materials in automobiles and residential buildings, vibration-damping braces in building materials, battery enclosures, and the like. EXAMPLES
[0063] [Experiment 1] In experiment 1, the relationship between the orientation angle of the reinforcing fibers in each layer constituting the reinforcing material and the fastening strength depending on the number of fastening members was investigated.
[0064] 1-1. Creating a laminate A UD sheet (manufactured by Mitsui Chemicals, Inc., TAFNEX (registered trademark), fiber volume fraction (VF): 50%, thickness difference: 0.16 mm) was prepared by impregnating carbon fibers aligned in one direction with polypropylene. This UD sheet was cut into a size of 215 mm length x 215 mm width to obtain a single-layer UD sheet. At this time, multiple types of single-layer UD sheets with different fiber orientation directions relative to the vertical direction were produced.
[0065] Twelve of the above single-layer UD sheets were laminated on a polyester release film (bottom film) with the carbon fiber orientation direction in each layer being the direction shown in Table 1, and a polyester release film (top film) was placed on top of them. The carbon fiber orientation direction shown in Table 1 is the direction when the vertical direction is set to 0°.
[0066] The materials were layered in the following order: a stainless steel plate 240 mm long, 240 mm wide, and 2 mm thick; an aluminum alloy film 240 mm long, 240 mm wide, and 0.1 mm thick; a stainless steel frame 240 mm long, 240 mm wide, and 1.5 mm thick, with an inner dimension of 220 mm long and 220 mm wide; and a polyester film 240 mm long, 240 mm wide, and 0.1 mm thick. The laminate of the UD sheets was placed inside the frame, and a polyester release film, an aluminum alloy film, and a stainless steel plate, all of which were the same size as the above, were layered on top of each other. This was placed in a hydraulic press (Mini Test Press, manufactured by Toyo Seiki Seisakusho Co., Ltd.), and the temperature during pressing was set to 180°C, and a pressure of 1 MPa was applied and held for 2 minutes, and then a pressure of 5 MPa was applied and held for 3 minutes, after which the pressure was released. Immediately thereafter, the molded structure was placed in a hydraulic press (Toyo Seiki Co., Ltd., Mini Test Press) in which cooling water at 15°C was circulated, and after holding for 3 minutes while applying a pressure of 5 MPa, the pressure was released. The molded body was then removed from the hydraulic press, and the stainless steel plate, polyester film, aluminum alloy film, and stainless steel frame were removed to obtain Reinforcements 1-1 to 1-5.
[0067] [Table 1]
[0068] 1-2. Fabrication of the structure Test pieces measuring 100 mm in the vertical direction and 25 mm in the horizontal direction were taken from each reinforcement material using water jet cutting to prepare the test specimens.
[0069] The test piece and an aluminum plate (JIS H4000:2014 5052-O) with a length of 100 mm, width of 25 mm and thickness of 2.0 mm were placed on the joining die attached to the C-frame of a self-piercing rivet joining device (Emhart SPR, manufactured by Pop Rivet & Fastener Co., Ltd.) as shown in Figure 8.
[0070] Then, a self-piercing rivet element (SPR550S1C0-4Y1, manufactured by Pop Rivet & Fastener Co., Ltd.) was pressed into the test piece side with a tool attached to the self-piercing riveting device to produce a self-piercing riveted joint, and a structure in which the test piece was fastened to the aluminum plate was obtained. At this time, the amount of press-in of the self-piercing rivet was controlled so that the difference in the depth direction between the flat part of the self-piercing rivet element and the surface of the laminate was within the range of -0.3mm to 0.3mm.
[0071] After that, a portion of the structure measuring 50 mm in length and 25 mm in width from both ends of the self-piercing rivet joint was blasted with #320 emery paper and degreased with acetone. Tabs measuring 50 mm in length and 25 mm in width and made of the same material as each of the constituent materials were prepared, blasted with #320 emery paper, and degreased with acetone. The ends of the test specimen and aluminum plate opposite the fastening portion were blasted and degreased, and a primer (made by Toa Gosei Co., Ltd.) was applied to this portion and allowed to dry thoroughly. After that, a cyanoacrylate adhesive (made by Toa Co., Ltd.) was applied, and a tab made of the same material was placed on each portion to bond the structure and the tab.
[0072] The position where the self-piercing rivet was formed was changed as shown in Figures 9A to 9D to obtain the respective structures. Note that in the configurations of Figures 9B and 9D, the width in the longitudinal direction of the contact portion between the test piece and the aluminum plate was doubled, and in the configurations of Figures 9C and 9D, the width in the lateral direction of the test piece and the aluminum plate was doubled.
[0073] 1-3.Evaluation The above structure was subjected to a tensile test to measure the relationship between the load and displacement of the joint. A precision universal testing machine (AG-X 100kN, manufactured by Shimadzu Corporation) was used for the tensile test. Tabs were fixed to the crosshead of the precision universal testing machine and the grip for the tensile test attached to the test machine base, and a forced displacement in the tensile direction was imposed on the crosshead. The grip distance when the above structure was fixed to the grip was 75 mm for the structures of Figures 9A and 9C, and 100 mm for the structures of Figures 9B and 9D. The displacement speed was 10 mm per minute, and the test temperature was 23°C. The load at which the fastening portion was destroyed was taken as the maximum endurance load. The results obtained are shown in Figure 10. In Figure 10, the horizontal axis shows the type of reinforcing material, and the vertical axis shows the maximum endurance load.
[0074] As shown in FIG. 10, the fastening strength (maximum durability strength) against stress at the fastening portion (stress occurred in the 0° direction in this test) tended to improve when the number of fastening members was increased. However, when there was a layer in which the reinforcing fibers were oriented in a direction that was ±60°±15° relative to the stress at the fastening portion, the fastening strength did not improve even when the number of fastening members was increased.
[0075] [Experiment 2] In experiment 2, it was investigated whether the maximum durability strength would be improved when a layer in which reinforcing fibers were oriented in a direction that was ±0°±10° relative to the stress at the fastening site was added to Reinforcement 1-5.
[0076] Reinforcement material 2-1 was prepared in the same manner as Reinforcement material 1-5, except that, in relation to the layer structure of Reinforcement material 1-5, one layer with a carbon fiber orientation direction of 0° was added to the outside of each of the first and twelfth layers.
[0077] Reinforcement material 2-2 was prepared in the same manner as Reinforcement material 1-5, except that, with respect to the layer structure of Reinforcement material 1-5, one layer with a carbon fiber orientation direction of 0° was added between the 6th and 7th layers.
[0078] For Reinforcement 2-1 and Reinforcement 2-2, structures were fabricated in the same manner as in Experiment 1, and the maximum endurance load was measured. The results are shown in Figure 11. In Figure 11, the horizontal axis shows the position of the fastening member (self-piercing rivet joint) (see Figure 9), and the vertical axis shows the maximum endurance load.
[0079] As shown in FIG. 10, in the reinforcement material 1-5, when there was a fastening reinforcement layer in which reinforcing fibers were oriented in a direction of ±0°±10° relative to the stress at the fastening portion, the fastening strength was improved. [Industrial Applicability]
[0080] The present invention can increase the fastening strength of a reinforcing material laminated with a UD sheet. [Explanation of symbols]
[0081] 100, 400, 500, 600 structures 110, 410, 510, 610 Pillar members 112 Top part 114 Side part 116 Flange part 120, 420, 520, 620 Reinforcement 122, 128, 422, 428, 522, 528, 622, 628 layers (stress absorbing layers) 124, 126, 424, 426, 524, 526, 624, 626 layers (fastening reinforcement layer) 130, 430, 530, 630 Fastening members 210 Reinforced Fiber 220 Matrix Resin
Claims
1. A stress member that generates stress when subjected to an external force; a reinforcing member fastened to the stress member by a fastening member; The reinforcing material is a laminate formed by fusing a fiber-reinforced resin containing a plurality of reinforcing fibers oriented in one direction and a matrix resin, The laminate has a stress absorbing layer in which the reinforcing fibers are oriented at an angle of ±60°±15° with respect to the direction of stress generated at the position of the fastening member of the stress member when an external force is applied, and a fastening reinforcement layer in which the reinforcing fibers are oriented at an angle of 0°±15°. structure.
2. When an external force is applied to the stress member, a first stress having a maximum energy amount is generated, and a second stress having a smaller energy amount than the first stress is generated at a position of the fastening member, The laminate has a stress absorbing layer in which the reinforcing fibers are oriented at an angle of ±60°±15° with respect to the direction of the second stress, and a fastening reinforcement layer in which the reinforcing fibers are oriented at an angle of 0°±15°. The structure of claim 1.
3. When the stress member receives an external force, the second stress is generated at the position of the fastening member in a direction different from that of the first stress. The structure of claim 2.
4. The fastening layer is disposed as the outermost layer of the reinforcement material. The structure of claim 1.
5. The stress absorbing layer is a layer in which the reinforcing fibers are oriented at +60°±15° and a layer in which the reinforcing fibers are oriented at -60°±15°, which are continuously arranged in the stacking direction. The structure of claim 1.
6. It is a columnar structure, The fastening member is disposed on the side surface of the columnar member. The structure of claim 1.
7. A structure having a hat-shaped cross section having a top surface portion, a side surface portion, and a flange portion, The fastening member is disposed on the side surface portion or the flange portion, The structure of claim 1.
8. It is a columnar structure, The fastening member is disposed at an end portion of the column in the longitudinal direction. The structure of claim 1.
9. A pillar of a car. The structure according to any one of claims 1 to 8.
10. A step of analyzing a direction of stress generated at a position of a fastening member of a structure having a stress member that generates stress by receiving an external force and a reinforcing material fastened to the stress member by a fastening member, the reinforcing material being a laminate formed by fusing a fiber-reinforced resin containing a plurality of reinforcing fibers oriented in one direction and a matrix resin; A step of determining whether the laminate includes a stress absorbing layer in which the reinforcing fibers are oriented at an angle of ±60°±15° with respect to the direction of stress generated at the position of the fastening member of the stress member when an external force is applied; When it is determined that the stress absorption layer is included, a step of determining that the laminate is provided with a fastening reinforcement layer in which the reinforcing fibers are oriented at 0°±15° with respect to the direction of the stress generated at the position of the fastening member; A method for designing a structure comprising the steps of:
Citation Information
Patent Citations
Fastening structure for carbon fiber-reinforced resin
JP2016114139A
Fiber-reinforced resin sheet, fiber-reinforced composite and molded product
JP2022103810A