Inorganic-tin emulsion composition and method for producing the same
The inorganic tin emulsion composition addresses storage stability and curability issues by stabilizing inorganic tin in aqueous systems, achieving stable emulsion particles for improved film properties and reduced environmental toxicity.
Patent Information
- Application Number
- JP2023046586
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-03-23
AI Technical Summary
Existing silicone emulsion compositions face issues with storage stability, curability, and environmental toxicity due to the use of organic tin compounds, and inorganic tin compounds are difficult to stabilize in aqueous systems.
An inorganic tin emulsion composition comprising inorganic tin compound, hydrocarbon oil, surfactant, and water, with a production method that includes emulsification and high-pressure particle size reduction to achieve stable emulsion particles of 500 nm or less.
The inorganic tin emulsion composition exhibits excellent storage stability and curability, reducing environmental impact while maintaining film properties like hardness and tensile strength.
Smart Images

Figure 2024135743000001 
Figure 2024135743000002 
Figure 2024135743000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an inorganic tin emulsion composition and a method for producing the same. [Background technology]
[0002] Silicone emulsions which form a rubber film when dried have conventionally been available in a variety of compositions and have been used as fiber treatment agents, rubber coating agents, building material coating agents, paper and plastic film coating agents, and the like, or as additives thereto, for the purpose of imparting slipperiness, water repellency and release properties.
[0003] As a method for forming a rubber film, there is a method in which a silicone elastomer film is formed by addition reaction between an alkenylsilyl group and a hydrosilyl group at the same time as drying. As the composition, for example, an emulsion composition consisting of a diorganopolysiloxane with a vinyl group blocked at the molecular chain end, an organohydrogenpolysiloxane and a platinum catalyst, a diorganopolysiloxane containing a vinyl group at the molecular chain end or on the side chain, a polysiloxane having a hydrogen atom bonded to a silicon atom, colloidal silica and a platinum catalyst have been proposed. However, in these compositions, if the siloxane containing a hydrosilyl group and the platinum catalyst are allowed to coexist, the reaction progresses over time or hydrogen gas is generated, so that the silicone emulsion and the platinum catalyst must be mixed before use, which is inconvenient. In addition, there is a drawback that the coating does not cure sufficiently if the substrate to be coated contains a compound that inhibits the addition reaction, such as a compound containing amine, tin, phosphorus, or sulfur.
[0004] As a method for forming a silicone rubber film other than the addition reaction, there is a method in which a condensation reaction of silicone is caused to proceed during drying.A silicone emulsion composition (Patent Document 1) is known which is composed of an anionically stabilized hydroxylated diorganopolysiloxane, colloidal silica, and an organic tin compound or an organic amine compound, and has a pH of 9 to 11.5. In compositions that cure through a condensation reaction, the use of an organotin compound with high catalytic activity is necessary to obtain a sufficiently cured rubber film in a short period of time. However, in recent years, the use of organotin compounds has come to be avoided due to their toxicity.
[0005] As a method for forming a silicone rubber film without using an organotin compound, Patent Document 2 proposes a composition obtained by emulsifying a mixture of a hydroxy-containing organopolysiloxane and an aminoxy-containing siloxane and / or silane. Although this composition does not require a condensation catalyst to form a cured film, there is a problem in that an amino compound is by-produced during the condensation reaction.
[0006] Patent Document 3 proposes a silicone emulsion composition consisting of an organopolysiloxane having a hydroxyl group and / or an alkoxy group bonded to a silicon atom at the molecular chain end and an alkyl group containing an amino group, a trialkoxysilane or a tetraalkoxysilane, and a metal compound. This composition can obtain a sufficiently hardened rubber film in a short time by condensation reaction without using a tin compound, but the organopolysiloxane, which is the raw material of this composition, is gradually polymerized over time and the molecular weight increases, so it cannot be stored for a long time, and the emulsion of organopolysiloxane in this composition cannot be produced by emulsion polymerization, so it cannot be made into an emulsion of organopolysiloxane with a high degree of polymerization.
[0007] Also proposed is a silicone emulsion composition comprising a hydroxyl group-containing organopolysiloxane, colloidal silica, an amide group- and carboxyl group-containing silane, and an epoxy group-containing silane (Patent Document 4).Patent Document 5 proposes the use of a bismuth compound.
[0008] If an organotin compound is not used, there is a problem that curing is poor and the strength of the rubber film is reduced. As a method of not using an organotin compound, the use of an inorganic tin compound can be considered. Inorganic tin compounds can be an effective alternative to organic tin as a curing catalyst in solvent-based systems, but their use in aqueous systems is difficult due to the tendency of inorganic tin to be hydrolyzed and deactivated. The prior art does not describe the use of inorganic tin compounds in aqueous systems. In order to use inorganic tin compounds as curing catalysts in aqueous compositions, it is important to obtain emulsion compositions containing inorganic tin compounds as the main component and having excellent stability. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Japanese Patent Publication No. 56-16553 [Patent Document 2] Japanese Patent Application Publication No. 6-73291 [Patent Document 3] JP 2005-306994 A [Patent Document 4] JP 2008-231276 A [Patent Document 5] JP 2014-224164 A Summary of the Invention [Problem to be solved by the invention]
[0010] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide an inorganic tin emulsion having good storage stability and a method for producing the same. [Means for solving the problem]
[0011] The present invention has been made to achieve the above object, (A) Inorganic tin compound: 100 parts by mass (B) Hydrocarbon oil: 5 to 100 parts by mass (C) Surfactant: 5 to 50 parts by mass (D) Water: 50~2,000 parts by mass The present invention provides an inorganic tin emulsion composition comprising:
[0012] This configuration makes it possible to obtain an inorganic tin emulsion composition that has excellent storage stability and can be used as a water-based curing catalyst.
[0013] In this case, the component (B) may be an aliphatic hydrocarbon oil having 10 to 50 carbon atoms.
[0014] This makes it possible to obtain an inorganic tin emulsion composition having superior storage stability.
[0015] The component (A) may be at least one of tin bis(2-ethylhexanoate) and tin bisneodecanoate.
[0016] These materials are easy to obtain and easy to handle, and can be preferably used in the present invention.
[0017] The inorganic tin emulsion composition may have an average particle size of 500 nm or less.
[0018] This results in a more preferable emulsion composition with excellent stability.
[0019] The emulsion composition may be free of organotin compounds.
[0020] This allows for lower environmental and toxicological impacts.
[0021] The emulsion composition may be a film-forming silicone emulsion composition.
[0022] This makes it possible to obtain a film having improved film properties such as hardness and tensile strength.
[0023] The emulsion composition may also be used as a coating agent.
[0024] This makes it possible to obtain an excellent coating agent.
[0025] In the present invention, (A) Inorganic tin compound: 100 parts by mass (B) Hydrocarbon oil: 5 to 100 parts by mass (C) Surfactant: 5 to 50 parts by mass (D) Water: 50~2,000 parts by mass The present invention provides a method for producing an inorganic tin emulsion composition, the method comprising the step of forming emulsion particles by emulsifying a mixture containing the above-mentioned components using an emulsifier.
[0026] According to this production method, an inorganic tin emulsion composition having excellent storage stability can be produced.
[0027] The manufacturing method of the present invention may further include a step of reducing the particle size of the emulsion particles using an emulsifier that uses high pressure to reduce the particle size.
[0028] By reducing the particle size of the emulsion particles, it is possible to produce an inorganic tin emulsion composition having superior storage stability.
[0029] In the step of reducing the particle size of the emulsion particles by using an emulsifier that reduces the particle size of the emulsion particles by using high pressure, the average particle size of the emulsion particles can be reduced to 500 nm or less.
[0030] This makes it possible to produce an inorganic tin emulsion composition having even better storage stability. Effect of the Invention
[0031] As described above, the inorganic tin emulsion composition of the present invention has high storage stability and is therefore useful as a curing catalyst for aqueous systems. In addition, since it does not contain an organotin compound, it has low toxicity and environmental impact. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0032] As described above, there has been a demand for the development of an inorganic tin emulsion composition having excellent storage stability.
[0033] As a result of extensive investigations into the above-mentioned problems, the present inventors have found that an inorganic tin emulsion composition containing the following components (A) to (D) has excellent storage stability and can be used as an aqueous curing catalyst, and have completed the present invention.
[0034] That is, the present invention provides: (A) Inorganic tin compound: 100 parts by mass (B) Hydrocarbon oil: 5 to 100 parts by mass (C) Surfactant: 5 to 50 parts by mass (D) Water: 50~2,000 parts by mass The inorganic tin emulsion composition is characterized by comprising: The manufacturing method of the present invention further comprises the steps of: (A) Inorganic tin compound: 100 parts by mass (B) Hydrocarbon oil: 5 to 100 parts by mass (C) Surfactant: 5 to 50 parts by mass (D) Water: 50~2,000 parts by mass A method for producing an inorganic tin emulsion composition, comprising the step of forming emulsion particles by emulsifying a mixture containing the inorganic tin emulsion composition using an emulsifier.
[0035] The present invention will be described in detail below, but the present invention is not limited thereto.
[0036] Component (A) Component (A) of the present invention is an inorganic tin compound. Note that the inorganic tin compound in the present invention is a tin compound that does not have a tin-carbon bond. The component (A) is not particularly limited as long as it is an inorganic tin compound, but tin carboxylates are preferred. Among them, tin bis(2-ethylhexanoate) and tin bisneodecanoate are particularly preferred from the viewpoints of availability and ease of handling. The component (A) may be used alone or in combination of two or more.
[0037] (B) Component The component (B) of the present invention is a hydrocarbon oil. In the present invention, by blending an appropriate amount of the component (B), an inorganic tin compound that is inherently unstable in an aqueous system can be made into an emulsion with good storage stability. As long as it is a hydrocarbon oil, there is no restriction as to whether it is linear or branched, and examples include α-olefin oligomer, isoparaffin, isododecane, isohexadecane, squalane, synthetic squalane, vegetable squalane, ceresin, paraffin, paraffin wax, polyethylene wax, polyethylene-polypropylene wax, (ethylene / propylene / styrene) copolymer, (butylene / propylene / styrene) copolymer, liquid paraffin, pristane, polyisobutylene, hydrogenated polyisobutene, microcrystalline wax, and petrolatum. The component (B) is preferably an aliphatic hydrocarbon oil having 10 to 50 carbon atoms, and more preferably an aliphatic hydrocarbon oil having 10 to 40 carbon atoms. Examples of the aliphatic hydrocarbon oil having 10 to 50 carbon atoms include isoparaffin, isododecane, isohexadecane, and liquid paraffin. Liquid paraffin is particularly preferred. The component (B) may be used alone or in combination of two or more types.
[0038] The blend amount of the component (B) is 5 to 100 parts by mass, preferably 8 to 70 parts by mass, more preferably 10 to 50 parts by mass, and particularly preferably 20 to 40 parts by mass, per 100 parts by mass of the component (A). If the amount of component (B) is less than the lower limit, the storage stability of the emulsion will deteriorate, whereas if it exceeds the upper limit, the amount of hydrocarbon oil in the composition will be too high, decreasing the catalytic activity.
[0039] (C) Component The component (C) of the present invention is a surfactant, and is an emulsifier for emulsifying and dispersing the components (A) and (B) in water to form an emulsion composition. The surfactant of the component (C) is not particularly limited, and is a nonionic surfactant, an anionic surfactant, a cationic surfactant, or an amphoteric surfactant. These can be used alone or in appropriate combination of two or more.
[0040] Examples of the nonionic surfactant used herein include polyoxyethylene alkyl ethers, polyoxyethylene polyoxypropylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyethylene glycol fatty acid esters, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene sorbitol fatty acid esters, glycerin fatty acid esters, polyoxyethylene glycerin fatty acid esters, polyglycerin fatty acid esters, propylene glycol fatty acid esters, polyoxyethylene castor oil, polyoxyethylene hydrogenated castor oil, polyoxyethylene hydrogenated castor oil fatty acid esters, polyoxyethylene alkylamines, polyoxyethylene fatty acid amides, polyoxyethylene modified organopolysiloxanes, and polyoxyethylene polyoxypropylene modified organopolysiloxanes.
[0041] Examples of the anionic surfactant include alkyl sulfate salts such as sodium lauryl sulfate, polyoxyethylene alkyl ether sulfate salts, polyoxyethylene alkyl phenyl ether sulfate salts, alkyl benzene sulfonates, polyoxyethylene alkyl phenyl ether sulfonates, alkyl diphenyl ether disulfonates, alkanesulfonates, N-acyltaurate salts, dialkyl sulfosuccinates, monoalkyl sulfosuccinates, polyoxyethylene alkyl ether sulfosuccinates, fatty acid salts, polyoxyethylene alkyl ether carboxylates, N-acyl amino acid salts, monoalkyl phosphate salts, dialkyl phosphate salts, polyoxyethylene alkyl ether phosphate salts, and the like.
[0042] Examples of the cationic surfactant include alkyltrimethylammonium salts, dialkyldimethylammonium salts, polyoxyethylenealkyldimethylammonium salts, dipolyoxyethylenealkylmethylammonium salts, tripolyoxyethylenealkylammonium salts, alkylbenzyldimethylammonium salts, alkylpyridinium salts, monoalkylamine salts, and monoalkylamidoamine salts.
[0043] Examples of the amphoteric surfactant include alkyl dimethylamine oxide, alkyl dimethyl carboxybetaine, alkyl amidopropyl dimethyl carboxybetaine, alkyl hydroxysulfobetaine, and alkyl carboxymethyl hydroxyethyl imidazolinium betaine.
[0044] As the surfactant, a nonionic surfactant is preferred because a small amount of the surfactant can emulsify the oil phase components and form fine particles.
[0045] From the viewpoint of emulsion stability, the nonionic surfactant (when multiple surfactants are used, the HLB value of the entire mixture) preferably has an HLB value in the range of 9.0 to 18.0, more preferably 10.0 to 17.0, and even more preferably 11.0 to 16.0. The HLB value is a value calculated by the Griffin method. The HLB value is calculated by the following formula. N = N1 × W1 + N2 × W2 N: HLB value when using two surfactants with different HLB values N1, N2: HLB of each surfactant W1, W2: weight fraction of each surfactant (W1+W2=1)
[0046] The amount of component (C) used is 5 to 50 parts by mass, preferably 7 to 30 parts by mass, and particularly preferably 10 to 25 parts by mass, per 100 parts by mass of component (A). If the amount of component (C) used is less than 5 parts by mass per 100 parts by mass of component (A), the stability of the emulsion decreases, whereas if it exceeds 50 parts by mass, the catalytic activity decreases.
[0047] (D) Component The emulsion composition of the present invention contains water as component (D). As component (D), any water such as ion-exchanged water or purified water can be used. The amount of water is 50 to 2,000 parts by mass, more preferably 100 to 1,000 parts by mass, per 100 parts by mass of component (A). If the amount of water is less than 50 parts by mass per 100 parts by mass of component (A), emulsification becomes difficult, and if the amount of water exceeds 2,000 parts by mass, the concentration of inorganic tin in component (A) becomes low, and a large amount of the emulsion composition needs to be added to use it as a catalyst, making it difficult to use it as a catalyst.
[0048] The production method of the present invention will now be described. The mixture containing the components (A), (B), (C) and (D) is emulsified using an emulsifier to prepare an inorganic tin emulsion composition. For the emulsification here, an emulsifier such as a homodisper, homomixer, colloid mill, line mixer, universal mixer, ultramixer, planetary mixer, combimix, high-pressure homogenizer, etc. may be used. In addition, after preparing an emulsion composition by emulsifying a mixture containing the components (A), (B), (C) and (D) using a homodisper, homomixer, etc., the emulsion particles may be further reduced in size using an emulsifier that reduces the emulsion particles in size using high pressure such as a high-pressure homogenizer. The emulsifier used may be one type or two or more types in combination. More preferably, the production method uses an emulsifier that reduces the emulsion particles in size using high pressure such as a high-pressure homogenizer. A particularly preferred production method is to use an emulsifier that uses high pressure, such as a high-pressure homogenizer, to reduce the emulsion particles to a small particle size, so that the average particle size is 500 nm or less.
[0049] The average particle size of the emulsion particles in the emulsion composition of the present invention is preferably 800 nm or less, more preferably 500 nm or less, and particularly preferably 400 nm or less. The lower limit is not particularly limited, but is about 50 nm or more. If the average particle size exceeds 800 nm, the stability of the emulsion decreases, which is not preferable. The average particle size of the emulsion particles is the particle size at 50% of the volume accumulated value by the laser diffraction / scattering method.
[0050] From the viewpoints of environment and toxicity, it is preferable that the emulsion composition of the present invention does not contain an organotin compound.
[0051] The emulsion composition of the present invention may contain inorganic powders, pigments, dyes, thickeners, preservatives, antibacterial agents, deodorants, rust inhibitors, antioxidants, antifoaming agents, antistatic agents, ultraviolet absorbers, antifreeze agents, water-soluble resins, organic resin emulsions, and the like.
[0052] The emulsion composition of the present invention can be used as an alternative catalyst to the conventionally used organotin compounds. For example, it can be used as a catalyst for urethane reaction, esterification reaction, transesterification reaction, silicone condensation reaction, etc. The emulsion composition of the present invention has good storage stability, so it is particularly suitable as a catalyst for water-based compositions, and can be used as a curing catalyst for silicone emulsions, for example.
[0053] The emulsion composition of the present invention is useful as a curing catalyst for silicone emulsions. By using the emulsion composition of the present invention as a curing catalyst for film-forming silicone emulsions, it is possible to improve film properties such as film hardness and tensile strength. The film-forming silicone emulsion in the present invention refers to the silicone emulsion that can form a film after drying.For example, the emulsion that contains the organopolysiloxane with crosslinked structure can form a film after drying, and is a film-forming silicone emulsion.The presence or absence of film-forming property can be evaluated by, for example, weighing each silicone emulsion composition so that non-volatile content is 8.0g on a 15cm×10cm PP (polypropylene) tray, drying at 25°C for 48 hours, and then drying at 105°C for 1 hour, and then checking whether film is formed.
[0054] An example of a silicone having a crosslinked structure is an organopolysiloxane having a viscosity of 300,000 mPa·s or more at 25° C., as shown in the following formula: [ka] (In the formula, R 1 are each independently a hydrogen atom or a substituted or unsubstituted monovalent organic group having 1 to 20 carbon atoms; R 2 are each independently the above R 1 a, b, c, and d are values that satisfy the viscosity of the organopolysiloxane at 25°C of 300,000 mPa·s or more, a≧2, c≧0, d≧0, c+d≧1, and b can typically be a value of 200 or more, preferably 500 or more. However, when the value of c+d is large, the number of crosslinking units increases, so even if b is 200 or less, the viscosity may be 300,000 mPa·s or more.
[0055] In the present invention, the viscosity was measured at 25°C using a BM or BH type rotational viscometer. For those that can be measured in liquid form, the viscosity is measured as is, but for those that are too high to be measured, the viscosity of a 15% or 10% toluene solution may be measured. For those that are too high to be measured in liquid form, the viscosity is always 300,000 mPa s or higher.
[0056] Compositions utilizing the composition of the present invention as a catalyst are widely applicable, for example, as damage protection agents, water repellents, and release agents for paper, plastic sheets, and rubber articles; damage protection agents, water repellents, waterproofing agents, texture improving agents, and filling agents for cloth; water repellents, waterproofing agents, and release agents for concrete, mortar, and wood; binders for inorganic or organic substances, fiber treatment agents, paints, release agents, coating agents, and the like. EXAMPLES
[0057] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. "%" representing concentration and content indicates "% by mass".
[0058] (A) Inorganic tin compounds (A-1) Neostan U-28 (product name): manufactured by Nitto Kasei Co., Ltd., tin bis(2-ethylhexanoate) (A-2) Neostan U-50 (product name): manufactured by Nitto Kasei Co., Ltd., tin bisneodecanoate
[0059] (B) Liquid paraffin (B-1) KAYDOL (trade name): manufactured by Sonneborn, liquid paraffin, average carbon number 35
[0060] (C) Surfactant (C-1) Emulgen 1108 (product name): manufactured by Kao Chemical Co., Ltd., polyoxyethylene alkyl lauryl ether, HLB value = 13.5 (C-2) Emulgen 104P (product name): manufactured by Kao Chemical Co., Ltd., polyoxyethylene lauryl ether, HLB value = 9.6 (C-3) Emulgen 123P (product name): manufactured by Kao Chemical Co., Ltd., polyoxyethylene lauryl ether, HLB value = 16.9 (E) Organotin compounds (E-1) Neostan U-810 (product name): manufactured by Nitto Kasei Co., Ltd., dioctyltin dilaurate
[0061] [Average emulsion particle size] The particle size is measured using a laser diffraction / scattering particle size distribution analyzer LA-960 (manufactured by Horiba, Ltd.) at a volume cumulative value of 50%.
[0062] [Example 1] (A-1) Neostan U-28: 100 parts by mass (B-1)KAYDOL: 18.0 parts by mass (C-1) Emulgen 1108: 9.6 parts by weight (D) Water: 191.9 parts by mass The mixture was mixed and emulsified using a homomixer to obtain an emulsion composition. The mixture was then passed through a high-pressure homogenizer set at a pressure of 60 MPa to reduce the particle size of the emulsified particles of the emulsion, thereby obtaining an inorganic tin emulsion composition (I-1). The average particle size of the obtained (I-1) was 330 nm.
[0063] [Example 2] (A-1) Neostan U-28: 100 parts by mass (B-1)KAYDOL: 28.5 parts by mass (C-1) Emulgen 1108: 20.2 parts by mass (D) Water: 105.4 parts by mass The mixture was mixed and emulsified using a homomixer to obtain an emulsion composition. The mixture was then passed through a high-pressure homogenizer at a pressure setting of 60 MPa to reduce the particle size of the emulsified particles of the emulsion, thereby obtaining an inorganic tin emulsion composition (I-2). The average particle size of the obtained (I-2) was 310 nm.
[0064] [Example 3] (A-1) Neostan U-28: 100 parts by mass (B-1)KAYDOL: 19.1 parts by mass (C-2) Emulgen 104P: 11.9 parts by mass (C-3) Emulgen 123P: 2.4 parts by weight (D) Water: 105.9 parts by mass The mixture was mixed and emulsified using a homomixer to obtain an emulsion composition. The mixture was then passed through a high-pressure homogenizer set at a pressure of 60 MPa to reduce the particle size of the emulsified particles of the emulsion, thereby obtaining an inorganic tin emulsion composition (I-3). The average particle size of the obtained (I-3) was 350 nm.
[0065] [Example 4] (A-1) Neostan U-28: 100 parts by mass (B-1)KAYDOL: 19.1 parts by mass (C-1) Emulgen 1108: 13.5 parts by mass (D) Water: 105.4 parts by mass The above ingredients were mixed and emulsified using a homomixer to obtain an emulsion composition (I-4). The average particle size of the resulting (I-4) was 440 nm.
[0066] [Example 5] (A-1) Neostan U-28: 100 parts by mass (B-1)KAYDOL: 22.0 parts by mass (C-2) Emulgen 104P: 12.9 parts by mass (C-3) Emulgen 123P: 1.8 parts by mass (D) Water: 104.6 parts by mass The mixture was mixed and emulsified using a homomixer to obtain an emulsion composition. The mixture was then passed through a high-pressure homogenizer set at a pressure of 60 MPa to reduce the particle size of the emulsified particles of the emulsion, thereby obtaining an inorganic tin emulsion composition (I-5). The average particle size of the obtained (I-5) was 280 nm.
[0067] [Example 6] (A-2) Neostan U-50: 100 parts by mass (B-1)KAYDOL: 19.1 parts by mass (C-2) Emulgen 104P: 11.4 parts by mass (C-3) Emulgen 123P: 1.7 parts by weight (D) Water: 105.9 parts by mass The mixture was mixed and emulsified using a homomixer to obtain an emulsion composition. The mixture was then passed through a high-pressure homogenizer at a pressure setting of 60 MPa to reduce the particle size of the emulsified particles of the emulsion, thereby obtaining an inorganic tin emulsion composition (I-6). The average particle size of the obtained (I-6) was 490 nm.
[0068] [Example 7] (A-2) Neostan U-50: 100 parts by mass (B-1)KAYDOL: 25.5 parts by mass (C-1) Emulgen 1108: 13.5 parts by mass (D) Water: 107.0 parts by mass The mixture was mixed and emulsified using a homomixer to obtain an emulsion composition. The mixture was then passed through a high-pressure homogenizer set at a pressure of 60 MPa to reduce the particle size of the emulsion particles, thereby obtaining an inorganic tin emulsion composition (I-7). The average particle size of the obtained (I-7) was 390 nm.
[0069] [Example 8] (A-2) Neostan U-50: 100 parts by mass (B-1)KAYDOL: 19.5 parts by mass (C-2) Emulgen 104P: 11.4 parts by mass (C-3) Emulgen 123P: 1.7 parts by weight (D) Water: 105.9 parts by mass The above ingredients were mixed and emulsified using a homomixer to obtain an emulsion composition (I-8). The average particle size of the resulting (I-8) was 520 nm.
[0070] [Example 9] (A-1) Neostan U-28: 100 parts by mass (B-1)KAYDOL: 9.0 parts by mass (C-1) Emulgen 1108: 12.5 parts by mass (D) Water: 110.5 parts by mass The mixture was mixed and emulsified using a homomixer to obtain an emulsion composition. The mixture was then passed through a high-pressure homogenizer set at a pressure of 60 MPa to reduce the particle size of the emulsion particles, thereby obtaining an inorganic tin emulsion composition (I-9). The average particle size of the resulting (I-9) was 450 nm.
[0071] [Example 10] (A-1) Neostan U-28: 100 parts by mass (B-1)KAYDOL: 20.0 parts by mass (C-1) Emulgen 1108: 8.5 parts by weight (D) Water: 110.0 parts by mass The mixture was mixed and emulsified using a homomixer to obtain an emulsion composition. The mixture was then passed through a high-pressure homogenizer set at a pressure of 60 MPa to reduce the particle size of the emulsified particles of the emulsion, thereby obtaining an inorganic tin emulsion composition (I-10). The average particle size of the obtained (I-10) was 500 nm.
[0072] [Comparative Example 1] (A-1) Neostan U-28: 100 parts by mass (C-1) Emulgen 1108: 15.0 parts by mass (D) Water: 105.0 parts by mass The mixture was mixed and emulsified using a homomixer to obtain an emulsion composition. The mixture was then passed through a high-pressure homogenizer at a pressure setting of 60 MPa to reduce the particle size of the emulsified particles of the emulsion, thereby obtaining an inorganic tin emulsion composition (II-1). The average particle size of the obtained (II-1) was 1120 nm.
[0073] [Comparative Example 2] (A-1) Neostan U-28: 100 parts by mass (B-1)KAYDOL: 3.5 parts by mass (C-1) Emulgen 1108: 15.0 parts by mass (D) Water: 105.0 parts by mass The mixture was mixed and emulsified using a homomixer to obtain an emulsion composition. The mixture was then passed through a high-pressure homogenizer at a pressure setting of 60 MPa to reduce the particle size of the emulsified particles of the emulsion, thereby obtaining an inorganic tin emulsion composition (II-2). The average particle size of the obtained (II-2) was 850 nm.
[0074] [Comparative Example 3] (A-1) Neostan U-28: 100 parts by mass (B-1)KAYDOL: 15.0 parts by mass (C-1) Emulgen 1108: 4.5 parts by weight (D) Water: 105.0 parts by mass The mixture was mixed and emulsified using a homomixer to obtain an emulsion composition. The mixture was then passed through a high-pressure homogenizer set at a pressure of 60 MPa to reduce the particle size of the emulsion particles, thereby obtaining an inorganic tin emulsion composition (II-3). The average particle size of the resulting (II-3) was 1200 nm.
[0075] [Comparative Example 4] Organotin Compound (E-1) Neostan U-810: 100 parts by mass (B-1)KAYDOL: 18.0 parts by mass (C-1) Emulgen 1108: 9.6 parts by weight (D) Water: 191.9 parts by mass The mixture was mixed and emulsified using a homomixer to obtain an emulsion composition. The mixture was then passed through a high-pressure homogenizer at a pressure setting of 60 MPa to reduce the particle size of the emulsion particles, thereby obtaining an organotin emulsion composition (II-4). The average particle size of the resulting (II-4) was 320 nm.
[0076] [Average emulsion particle size] The particle size is measured using a laser diffraction / scattering particle size distribution analyzer LA-960 (manufactured by Horiba, Ltd.) at a volume cumulative value of 50%.
[0077] [Storage stability (25℃)] Each emulsion composition obtained in the Examples and Comparative Examples was stored at 25° C. for 3 months in a stationary state. After storage, the emulsion compositions were visually inspected, and those in which layer separation was observed within 1 month were marked with an X, those in which no separation was observed within 1 month but within 2 months were marked with a △, those in which no separation was observed within 2 months but within 3 months were marked with an ○, and those in which no separation was observed even after 3 months were marked with an ◎.
[0078] [Storage stability (40℃)] Each emulsion composition obtained in the Examples and Comparative Examples was stored at 40° C. for 2 weeks in a stationary state. After storage, the emulsion compositions were visually inspected, and those in which layer separation was observed within 1 week were marked with an X, those in which no separation was observed within 1 week but within 2 weeks were marked with a △, and those in which no separation was observed even after 2 weeks were marked with an ◯.
[0079] [Table 1]
[0080] [Table 2]
[0081] [Table 3]
[0082] As shown in Tables 1 to 3, in each of the Examples of the present invention, the average particle size and the storage stability at 25° C. and 40° C. were all good. On the other hand, in Comparative Examples 1 to 3, the average particle size was large and the storage stability at 25° C. and 40° C. were poor. Furthermore, each of the Examples of the present invention shows that the average particle size and the storage stability at 25° C. and 40° C. are not poor, similar to Comparative Example 4, which used an organotin compound.
[0083] [Film properties] According to Production Example 1 of Patent Document 5, an organopolysiloxane emulsion was prepared as follows. 498g of octamethylcyclotetrasiloxane, 2g of triethoxyphenylsilane, 50g of 10% aqueous sodium lauryl sulfate solution, and 50g of 10% aqueous dodecylbenzenesulfonic acid solution were charged and emulsified uniformly using a homomixer, then 400g of water was gradually added to dilute the mixture, and the mixture was passed through a high-pressure homogenizer at a pressure of 30MPa to obtain a uniform white emulsion. This emulsion was transferred to a glass flask equipped with a stirrer, thermometer, and reflux condenser, and polymerized at 50°C for 24 hours, then aged at 110°C for 24 hours, and then neutralized with 12g of 10% aqueous sodium carbonate solution. The above procedure gave the average composition formula: [ka] An emulsion (III) containing an organopolysiloxane represented by the following formula was prepared. 30 g of the obtained emulsion (III) was added to 200 g of IPA with stirring to break down the emulsion and extract the organopolysiloxane. This organopolysiloxane was dried at 105°C for 3 hours and then its viscosity was measured with a rotational viscometer at 25°C. However, since it was impossible to measure in its current state, the viscosity was measured in a 15% toluene solution, which was found to be 1350 mPa s. Using the emulsion (III), the film properties were measured as follows.
[0084] (III): 100 parts by mass (IV) Colloidal silica (Snowtex C, manufactured by Nissan Chemical Industries, Ltd.): 30 parts by mass Emulsion of tin compound obtained in each Example and Comparative Example: 3 parts by mass The mixture was mixed, 20 g was poured into a polypropylene resin disposable tray (150 mm x 105 mm x 19 mm), and left for 48 hours in an atmosphere of 25°C and 60% relative humidity, and then heated at 105°C for 1 hour to produce a cured film of approximately 1 mm in thickness. The hardness, tensile strength, and elongation of this film were measured in accordance with JIS K 6249. The results are shown in the table below. Comparative Example 5 is a comparative example that does not contain any of the emulsion compositions (I) or (II) obtained in the above-mentioned Examples and Comparative Examples.
[0085] [Table 4]
[0086] [Table 5]
[0087] [Table 6]
[0088] As is clear from the above results, the inorganic tin emulsion composition of the present invention has better storage stability than Comparative Examples 1 to 3, has curability equivalent to that of the organotin catalyst of Comparative Example 4, and has superior curability to the inorganic tin emulsion composition of Comparative Example 5 and one not containing any organotin emulsion composition.
[0089] The present specification includes the following aspects. [1]: (A) inorganic tin compound: 100 parts by mass, (B) hydrocarbon oil: 5 to 100 parts by mass An inorganic tin emulsion composition comprising: (C) a surfactant: 5 to 50 parts by mass; and (D) water: 50 to 2,000 parts by mass. [2]: The emulsion composition according to [1] above, wherein the component (B) is an aliphatic hydrocarbon oil having 10 to 50 carbon atoms. [3]: The emulsion composition of the above [1] or [2], wherein the component (A) is at least one of tin bis(2-ethylhexanoate) and tin bisneodecanoate. [4]: The emulsion composition according to any one of the above [1] to [3], wherein the average particle size of the emulsified particles of the inorganic tin emulsion composition is 500 nm or less. [5]: The emulsion composition according to any one of the above [1] to [4], which does not contain an organotin compound. [6]: A film-forming silicone emulsion composition comprising any one of the compositions [1] to [5] above. [7]: A coating agent comprising any one of the compositions [1] to [6] above. [8]: A method for producing an inorganic tin emulsion composition, comprising the step of forming emulsion particles by emulsifying a mixture containing (A) 100 parts by mass of an inorganic tin compound, (B) 5 to 100 parts by mass of a hydrocarbon oil, (C) 5 to 50 parts by mass of a surfactant, and (D) 50 to 2,000 parts by mass of water using an emulsifier. [9]: A method for producing the inorganic tin emulsion composition according to the above [8], further comprising a step of reducing the particle size of the emulsion particles using an emulsifier that reduces the particle size of the emulsion particles using high pressure.
[10] : The method according to the above [9], wherein in the step of reducing the size of emulsion particles using an emulsifier that reduces the size of emulsion particles by using high pressure, the average size of the emulsion particles is reduced to 500 nm or less. [Industrial Applicability]
[0090] The inorganic tin emulsion composition of the present invention has good storage stability and excellent curing properties, and is suitable as a curing catalyst for water-based compositions.
[0091] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention.
Claims
1. (A) Inorganic tin compound: 100 parts by mass (B) Hydrocarbon oil: 5 to 100 parts by mass (C) Surfactant: 5 to 50 parts by mass (D) Water: 50 to 2,000 parts by mass An inorganic tin emulsion composition comprising:
2. The emulsion composition according to claim 1, wherein the component (B) is an aliphatic hydrocarbon oil having 10 to 50 carbon atoms.
3. 2. The emulsion composition according to claim 1, wherein the component (A) is at least one of tin bis(2-ethylhexanoate) and tin bisneodecanoate.
4. 2. The emulsion composition according to claim 1, wherein the average particle size of the emulsified particles of the inorganic tin emulsion composition is 500 nm or less.
5. 2. The emulsion composition according to claim 1, which is free of organotin compounds.
6. A film-forming silicone emulsion composition comprising the composition of claim 1.
7. A coating agent comprising the composition according to any one of claims 1 to 6.
8. (A) Inorganic tin compound: 100 parts by mass (B) Hydrocarbon oil: 5 to 100 parts by mass (C) Surfactant: 5 to 50 parts by mass (D) Water: 50 to 2,000 parts by mass A method for producing an inorganic tin emulsion composition, comprising the step of forming emulsion particles by emulsifying a mixture containing the above-mentioned components using an emulsifier.
9. 9. The method for producing an inorganic tin emulsion composition according to claim 8, further comprising a step of reducing the particle size of the emulsion particles by an emulsifier that reduces the particle size of the emulsion particles by using high pressure.
10. 10. The method according to claim 9, wherein the step of reducing the emulsion particle size by an emulsifier using high pressure reduces the average particle size of the emulsion particles to 500 nm or less.
Citation Information
Patent Citations
Silicone rubber powder and producing method for it
JP2009057499A
Curable resin composition
JP2014189577A
Curable silicone emulsion composition
JP2014224164A
Large, stable aqueous silicone rubber suspension and method for producing superior aesthetic matte coating using the same
JP2019534903A
Aqueous silicone dispersion, coating film and cosmetic
WO2018135369A1