Watch decorative member and method of manufacturing the same
The decorative member for watches, featuring a dielectric multilayer film, light-shielding layer, and printed layers, addresses the need for improved design by ensuring visibility of decorative patterns under varying lighting conditions.
Patent Information
- Application Number
- JP2023046662
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-03-23
AI Technical Summary
There is a demand for decorative members for watches to further improve their design.
A decorative member for a watch comprising a light-transmitting member with a dielectric multilayer film having openings representing a predetermined pattern, a light-shielding layer, a first printed layer formed of transparent paint, and a second printed layer, where the first printed layer can be luminous and the second printed layer is high-light-shielding.
The decorative member achieves an excellent design with the first printed layer enhancing visibility in dark places and the second printed layer ensuring clear visibility of the decorative pattern, regardless of lighting conditions.
Smart Images

Figure 2024135793000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a decorative member for a watch and a method for producing the same. [Background technology]
[0002] In decorative components for watches, various structures have been proposed to enhance the design. For example, Patent Document 1 describes a rotating bezel body for a watch in which a colored film is formed on the lower part of a transparent cover glass and a luminous paint is applied. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 5-1247 Summary of the Invention [Problem to be solved by the invention]
[0004] There is a demand for improved design in decorative members for watches.
[0005] The present invention has been made to solve the above-mentioned problems, and has an object to provide a decorative member for a watch having excellent design properties and a manufacturing method thereof. [Means for solving the problem]
[0006] The watch decorative member of an embodiment of the present invention is characterized by having a translucent member, a dielectric multilayer film covering one side of the translucent member and having openings representing a predetermined pattern formed therein, a light-shielding layer covering the dielectric multilayer film, a first printed layer formed from translucent paint and covering the openings in the dielectric multilayer film, and a second printed layer covering the first printed layer.
[0007] Moreover, it is preferable that the first printed layer further covers the light-shielding layer.
[0008] Moreover, the paint that forms the first printed layer is preferably a luminous paint.
[0009] In addition, it is preferable that the dielectric multilayer film is formed by stacking a plurality of thin films, and the plurality of thin films includes a first thin film having a first refractive index and a second thin film having a second refractive index different from the first refractive index.
[0010] In addition, the second printed layer preferably has a light-shielding property.
[0011] A manufacturing method for a watch decorative member in an embodiment of the present invention is characterized by including the steps of forming a dielectric multilayer film on one side of a translucent member, forming a metal layer covering the dielectric multilayer film, forming openings of a predetermined pattern in the dielectric multilayer film and the metal layer, forming a first printed layer using a translucent paint that covers the openings in the dielectric multilayer film and the metal layer, and forming a second printed layer that covers the first printed layer. Effect of the Invention
[0012] The decorative member for watches according to the present invention has excellent design. The manufacturing method for a decorative member for watches according to the present invention makes it possible to manufacture a decorative member for watches having excellent design. [Brief description of the drawings]
[0013] [Figure 1] FIG. [Diagram 2] FIG. [Diagram 3] FIG. 2 is a schematic cross-sectional view of a bezel 7. [Figure 4] 4 is a flow diagram showing an example of the flow of a manufacturing method of the bezel 7. FIG. [Diagram 5] 1A is a schematic cross-sectional view of the bezel 7 immediately after the light-shielding layer forming step, and FIG. 1B is a schematic cross-sectional view of the bezel 7 immediately after the opening forming step. [Figure 6] 10 is a flow diagram showing another example of the flow of the manufacturing method of the bezel 7. FIG. [Figure 7](A) is a schematic cross-sectional view of the bezel 7 immediately after the mask formation process, (B) is a schematic cross-sectional view of the bezel 7 immediately after the light-shielding layer formation process, and (C) is a schematic cross-sectional view of the bezel 7 immediately after the mask removal process. [Figure 8] FIG. 13 is a diagram showing the reflection characteristics of a bezel according to an embodiment. [Figure 9] 11 is an image of a bezel according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, various embodiments of the present invention will be described with reference to the drawings. It should be noted that the technical scope of the present invention is not limited to these embodiments, but covers the inventions described in the claims and their equivalents.
[0015] 1 is a plan view of a timepiece 1 according to an embodiment of the present invention. The timepiece 1 is a wristwatch, and includes an exterior case 2, a dial 3, hands 4, a face cover 5, a crystal 6, and a bezel 7. The bezel 7 is an example of a decorative member for a timepiece.
[0016] The exterior case 2 is a substantially cylindrical member that houses each component of the watch 1. The exterior case 2 is made of metal such as titanium or stainless steel, ceramic, or resin. Mounting sections 21 for attaching a band (not shown) are formed on the side of the exterior case 2, on the 6 o'clock side and the 12 o'clock side of the watch 1. In addition, a crown 22 is disposed on the side of the exterior case 2, on the 3 o'clock side of the watch 1, which is inserted through the exterior case 2 and connected to the movement (not shown) of the watch 1.
[0017] The dial 3 is a disc-shaped member housed in the exterior case 2. Hour characters 31 are formed on the dial 3. The hour characters 31 may be formed by printing on the dial 3, may be formed by processing the dial 3, or may be formed by arranging a member having the shape of the hour characters 31 on the dial 3. In the example shown in Fig. 1, twelve hour characters 31 are formed on the dial 3 at 30 degree intervals.
[0018] The hands 4 include an hour hand 41, a minute hand 42, and a second hand 43 arranged above the dial 3. The hour hand 41, the minute hand 42, and the second hand 43 rotate according to the rotational force transmitted from the movement, and indicate the time by pointing to the hour digits 31.
[0019] The faceplate 5 is an annular member that is disposed on the upper surface of the dial 3 so as to cover the outer periphery of the dial 3. In the example shown in Fig. 1, the faceplate 5 has 60 minute gradations 51 formed at 6 degree intervals.
[0020] The crystal 6 is a translucent, disk-shaped member that is disposed above the dial 3 and the faceplate 5. The crystal 6 is made of, for example, sapphire glass, mineral glass, acrylic glass, or the like.
[0021] The bezel 7 is an annular member that is arranged on the upper surface of the exterior case 2 so as to surround the crystal 6. A predetermined decorative pattern P is displayed on the bezel 7. In the example shown in FIG. 1, characters indicating a city name are displayed as the decorative pattern P. However, the decorative pattern P is not limited to this example and may be any characters, symbols, figures, etc.
[0022] Fig. 2 is a plan view of the bezel 7, and Fig. 3 is a schematic cross-sectional view of the bezel 7 taken along line III-III in Fig. 2. The bezel 7 has a light-transmitting member 71, a dielectric multilayer film 72, a light-shielding layer 73, a first printed layer 74, and a second printed layer 75. The light-transmitting member 71, the dielectric multilayer film 72, the light-shielding layer 73, the first printed layer 74, and the second printed layer 75 are arranged in this order from the front of the timepiece 1 (from the top in Fig. 3).
[0023] The light-transmitting member 71 is an annular member having light-transmitting properties. The light-transmitting member 71 is formed of, for example, sapphire glass. Preferably, the light-transmitting member 71 is formed of sapphire glass. The thickness of the light-transmitting member 71 is preferably 1.2 mm or more.
[0024] The dielectric multilayer film 72 is formed by laminating a plurality of thin films made of a dielectric material so as to cover one surface of the light-transmitting member 71. Some of the thin films have a refractive index different from the other thin films. That is, the plurality of thin films include a first thin film having a first refractive index and a second thin film having a second refractive index different from the first refractive index. The dielectric material forming the thin films is, for example, high refractive index materials such as TiO2, Nb2O5, Ta2O5, and ZrO2, intermediate refractive index materials such as Al2O3, and low refractive index materials such as SiO2 and MgF2. The dielectric multilayer film 72 has different reflection characteristics depending on the angle of incidence of light due to the refractive index and film thickness of the material, and is therefore visually recognized in different colors depending on the line of sight.
[0025] The light-shielding layer 73 is formed so as to cover the dielectric multilayer film 72. The light-shielding layer 73 is formed of a material having high light-shielding properties. The light-shielding layer 73 is formed of a silver-white metal such as Cr, Ag, Ti, Zr, Al, Pt, Pd, Rh, or an alloy thereof. The light-shielding layer 73 may be formed of a colored metal such as Au, Cu, or an Au-Cu alloy. The light-shielding layer 73 may be formed of a metal nitride such as TiAlN, TiN, or CrN. The light-shielding layer 73 may be formed of a non-metal such as DLC (Diamond Like Carbon). The thickness of the light-shielding layer 73 is preferably 10 nm or more. This allows the light-shielding layer 73 to have high light-shielding properties, and the color of the dielectric multilayer film 72 to be clearly visible.
[0026] Openings 721 and 731 representing the decorative pattern P are formed in the dielectric multilayer film 72 and the light-shielding layer 73, respectively. That is, an opening 721 is formed in a region of the dielectric multilayer film 72 corresponding to the decorative pattern P, and an opening 731 is formed in a region of the light-shielding layer 73 corresponding to the decorative pattern P. In this way, the dielectric multilayer film 72 and the light-shielding layer 73 represent the decorative pattern P.
[0027] The first printed layer 74 is formed of a light-transmitting paint. The first printed layer 74 is filled into the openings 721 of the dielectric multilayer film 72 and the openings 731 of the light-shielding layer 73, thereby covering the openings 721 of the dielectric multilayer film 72 and the openings 731 of the light-shielding layer 73. The first printed layer 74 also covers the light-shielding layer 73. The thickness of the first printed layer 74 (the distance between the light-shielding layer 73 and the second printed layer 75) is preferably 2 μm or more and 30 μm or less.
[0028] The paint forming the first printed layer 74 is preferably a luminous paint in which aluminate-based, sulfide-based, or other phosphorescent pigments are dispersed in a translucent resin. This allows the area of the decorative pattern P to emit light in a dark place, making the decorative pattern P easily visible and providing the bezel 7 with excellent design.
[0029] The second printed layer 75 is formed of paint and is disposed so as to cover the first printed layer 74. The paint forming the second printed layer 75 is a paint having high light blocking properties. The paint forming the second printed layer 75 is preferably a white paint. Since the first printed layer 74 is formed of a light-transmitting paint, forming the second printed layer 75 of a white paint makes the decorative pattern P visible in white. In general, the dielectric multilayer film 72 strongly reflects light of a specific color, so that the decorative pattern P is visible in white, and therefore the color of the dielectric multilayer film 72 and the color of the decorative pattern P are clearly distinguished, and the decorative pattern P is easily visible.
[0030] FIG. 4 is a flow diagram showing an example of the flow of a manufacturing method for the bezel 7.
[0031] First, in a light-transmitting member preparation step (step S11), the light-transmitting member 71 is prepared.
[0032] Next, in a dielectric multilayer film forming process (step S12), a dielectric multilayer film 72 is formed to cover one surface of the translucent member 71. The dielectric multilayer film 72 is formed by sequentially stacking a plurality of thin films on one surface of the translucent member 71. Each thin film is formed by stacking a dielectric material on one surface of the translucent member 71 by vacuum deposition. Each thin film may be formed by sputtering, arc ion plating, CVD (Chemical Vapor Deposition), or the like. The thickness of the thin film may vary depending on the position on the surface of the translucent member 71. For example, by using a shielding mask that prevents deposition when stacking a part of the thin film, the thickness of the thin film can be made to vary depending on the position. When the thickness of the thin film is changed by the shielding mask in this way, gradation colors with various hues can be formed.
[0033] Next, in a light-shielding layer formation step (step S13), a light-shielding layer 73 is formed to cover the dielectric multilayer film 72. The light-shielding layer 73 is formed by laminating a material such as a metal, a metal nitride, or DLC by vapor deposition on the dielectric multilayer film 72. The light-shielding layer 73 may be formed by sputtering, arc ion plating, CVD, or the like.
[0034] Fig. 5(A) is a schematic cross-sectional view of the bezel 7 immediately after the light-shielding layer forming step. As shown in Fig. 5(A), immediately after the light-shielding layer forming step, the dielectric multilayer film 72 and the light-shielding layer 73 are uniformly laminated on one surface of the light-transmitting member 71. That is, the openings 721 and 731 are not formed in the dielectric multilayer film 72 and the light-shielding layer 73.
[0035] Returning to FIG. 4, next, in the opening formation step (step S14), openings 721 and 731 representing decorative pattern P are formed in dielectric multilayer film 72 and light-shielding layer 73. Openings 721 and 731 are formed by removing areas of dielectric multilayer film 72 and light-shielding layer 73 corresponding to decorative pattern P by etching. Etching is performed by laser irradiation or a solution.
[0036] Fig. 5(B) is a schematic cross-sectional view of the bezel 7 immediately after the opening forming step. As shown in Fig. 5(B), immediately after the opening forming step, an opening 721 is formed in the region of the dielectric multilayer film 72 corresponding to the decorative pattern P, and an opening 731 is formed in the region of the light-shielding layer 73 corresponding to the decorative pattern P.
[0037] 4, next, in a first printed layer formation step (step S15), a first printed layer 74 is formed to cover the openings 721 and 731 of the dielectric multilayer film 72 and the light-shielding layer 73. The first printed layer 74 is formed by applying a light-transmitting paint to the light-shielding layer 73 by pad printing. The first printed layer 74 may also be formed by screen printing, painting, or the like.
[0038] Next, in a second printed layer forming step (step S16), a second printed layer 75 is formed to cover the first printed layer 74. The second printed layer 75 is formed by applying paint to the first printed layer 74 by pad printing. The second printed layer 75 may also be formed by screen printing, painting, or the like. In this manner, the bezel 7 is manufactured.
[0039] As described above, the bezel 7 includes the light-transmitting member 71, the dielectric multilayer film 72 covering one surface of the light-transmitting member 71 and having the opening 721 representing the decorative pattern P formed therein, the light-shielding layer 73 covering the dielectric multilayer film 72, the first printed layer 74 formed of light-transmitting paint and covering the opening of the dielectric multilayer film 72, and the second printed layer 75 covering the first printed layer 74. This provides the bezel 7 with excellent design.
[0040] That is, the dielectric multilayer film 72 has different reflection characteristics depending on the angle of incidence of light, and is therefore visible in different shades depending on the line of sight. Also, the dielectric multilayer film 72 has an opening 721 representing the decorative pattern P, and the first printed layer 74 covering the opening 721 is formed of a light-transmitting paint, so that the area corresponding to the decorative pattern P is visible in a shade corresponding to the second printed layer 75. The decorative pattern P is visible in a constant shade, and the area other than the decorative pattern P is visible in a different shade depending on the line of sight, so that the bezel 7 has excellent design.
[0041] In addition, in the bezel 7, the paint forming the first printed layer 74 is preferably a luminous paint. By forming the first printed layer 74 from a luminous paint, the area of the decorative pattern P emits light in a dark place, making the decorative pattern P easily visible, and the bezel 7 has a different design from when it is in a bright place.
[0042] In addition, in the bezel 7, the paint forming the second printed layer 75 is preferably a white paint. Generally, a dielectric multilayer film strongly reflects light of a specific color and is visually recognized as a color, so by forming the second printed layer 75 with a white paint, the decorative pattern P can be easily recognized. In addition, when the first printed layer 74 is formed of a luminous paint, by forming the second printed layer 75 with a white paint, the light emitted from the first printed layer is strongly reflected by the second printed layer 75, and the decorative pattern P can be more easily recognized.
[0043] In the above description, the first printed layer 74 covers the openings 721 and 731 of the dielectric multilayer film 72 and the light-shielding layer 73, and also covers the light-shielding layer 73, but is not limited to this example. The first printed layer 74 may cover only the openings 721 and 731 of the dielectric multilayer film 72 and the light-shielding layer 73, and may not cover the light-shielding layer 73. In other words, the first printed layer 74 may be formed only inside the opening 721 of the dielectric multilayer film 72 and the opening 731 of the light-shielding layer 73. Even in this manner, the bezel 7 has excellent design.
[0044] In the above description, the openings 721 and 731 are formed in the regions of the dielectric multilayer film 72 and the light-shielding layer 73 corresponding to the decorative pattern P, respectively, so that the dielectric multilayer film 72 and the light-shielding layer 73 represent the decorative pattern P, but this is not limited to an example. For example, the dielectric multilayer film 72 and the light-shielding layer 73 may be formed only in the region corresponding to the decorative pattern P, so that the dielectric multilayer film 72 and the light-shielding layer 73 represent the decorative pattern P. Even in this case, the bezel 7 has excellent design.
[0045] In the above description, the bezel 7 is manufactured by the manufacturing method shown in the flow diagram of FIG. 4, but the manufacturing method is not limited to this example.
[0046] FIG. 6 is a flow diagram showing another example of the flow of the manufacturing method of the bezel 7.
[0047] First, in a light-transmitting member preparation step (step S21), the light-transmitting member 71 is prepared in the same manner as in step S11.
[0048] Next, in a mask formation step (step S22), a mask M is formed in an area corresponding to the decorative pattern P on one surface of the light-transmitting member 71. The mask M is formed by applying a resin to one surface of the light-transmitting member 71 by pad printing. The mask M may also be formed by screen printing, painting, or the like.
[0049] Fig. 7(A) is a schematic cross-sectional view of the bezel 7 immediately after the mask forming step. As shown in Fig. 5(A), immediately after the mask forming step, a mask M is formed in an area corresponding to the decorative pattern P on one surface of the light-transmitting member 71.
[0050] 6, in the dielectric multilayer film formation step (step S23), the dielectric multilayer film 72 is formed in the same manner as in step S12. At this time, since a mask M is formed in the region corresponding to the decorative pattern P, the dielectric multilayer film 72 is formed on the mask M rather than on the surface of the light-transmitting member 71.
[0051] Next, in a light-shielding layer forming step (step S24), the light-shielding layer 73 is formed in the same manner as in step S13. At this time, since the mask M is formed in the region corresponding to the decorative pattern P, the light-shielding layer 73 is formed so as to cover the dielectric multilayer film 72 on the mask M.
[0052] 7(B) is a schematic cross-sectional view of the bezel 7 immediately after the light-shielding layer forming step. Since a mask M is formed in the area of the light-transmitting member 71 corresponding to the decorative pattern P, the dielectric multilayer film 72 and the light-shielding layer 73 are formed in the area excluding the area corresponding to the decorative pattern P on one surface of the light-transmitting member 71 and on the mask M.
[0053] Returning to FIG. 6, in the mask removal process (step S25), the mask M formed on one surface of the light-transmitting member 71 is removed together with the dielectric multilayer film 72 and the light-shielding layer 73 formed on the mask M. As a result, openings 721 and 731 representing the decorative pattern P are formed in the dielectric multilayer film 72 and the light-shielding layer 73. The mask M is removed by immersing the light-transmitting member 71 in an organic solvent such as acetone or ethanol. Ultrasonic waves may be irradiated to the light-transmitting member 71 immersed in the organic solvent. This allows the mask M to be removed more efficiently.
[0054] 7(C) is a schematic cross-sectional view of the bezel 7 immediately after the mask removal step. By removing the mask M formed in the region corresponding to the decorative pattern P of the light-transmitting member 71, openings 721 and 731 are formed in the regions of the dielectric multilayer film 72 and the light-shielding layer 73 corresponding to the decorative pattern P, i.e., the region where the mask M was formed.
[0055] Returning to FIG. 6, next, in a first printed layer forming step (step S26), a first printed layer 74 is formed in the same manner as in step S15.
[0056] Next, in a second printed layer forming step (step S27), the second printed layer 75 is formed in the same manner as in step S16. In this manner, the bezel 7 is manufactured.
[0057] The bezel 7 manufactured in this manner has an excellent design, similar to the bezel 7 manufactured by the manufacturing method shown in the flow diagram of FIG.
[0058] In the above description, the decorative member for a timepiece is a bezel 7, but is not limited to such an example. The decorative member for a timepiece may be a dial 3 or a face cover 5. When the decorative member for a timepiece is a dial 3, the dial 3 has a configuration shown in the cross-sectional view of FIG. 3, and is manufactured by the manufacturing method shown in the flow chart of FIG. 4 or FIG. 6. In this case, the decorative pattern P is, for example, hour characters 31. When the decorative member for a timepiece is a face cover 5, the face cover 5 has a configuration shown in the cross-sectional view of FIG. 3, and is manufactured by the manufacturing method shown in the flow chart of FIG. 4 or FIG. 6. In this case, the decorative pattern P is, for example, a minute scale 51. The decorative member for a timepiece may also be a pointer 4 that represents a predetermined decorative pattern. EXAMPLES
[0059] A bezel according to the embodiment was manufactured by the manufacturing method shown in the flow diagram of FIG.
[0060] First, in step S11, a transparent member made of a ring-shaped sapphire glass having a thickness of 1.2 mm was prepared.
[0061] Next, in step S12, the light-transmitting member was placed in a vacuum deposition apparatus. A dielectric multilayer film was formed on one surface of the light-transmitting member by alternately stacking five thin films made of TiO2 and five thin films made of SiO2, i.e., a total of ten thin films. In order to visually recognize the dielectric multilayer film as blue, the thin films were formed to have thicknesses of 42 nm, 52 nm, 52 nm, 21 nm, 100 nm, 53 nm, 39 nm, 38 nm, 76 nm, and 136 nm, respectively, from the light-transmitting member side.
[0062] Next, in step S13, a light-shielding layer was formed by evaporating Cr on one surface of the light-transmitting member. The light-shielding layer was formed to have a thickness of 50 nm.
[0063] Next, in step S14, the light-transmitting member was removed from the vacuum deposition apparatus. After that, openings 721 and 731 representing the decorative pattern P were formed in the dielectric multilayer film 72 and the light-shielding layer 73 by etching using laser irradiation.
[0064] Next, in step S15, the light-transmitting member was washed. After that, a luminous paint was applied to the light-shielding layer by pad printing to form a first printed layer. The first printed layer was formed to have a thickness of 5 μm.
[0065] Next, in step S16, a white paint was applied to the first printed layer by pad printing to form a second printed layer. The second printed layer was formed to have a thickness of 10 μm. In this manner, the bezel according to the embodiment was manufactured.
[0066] Fig. 8 is a diagram showing the reflection characteristics of the bezel according to the embodiment measured immediately after step S13. In the graph of Fig. 8, the horizontal axis is wavelength, and the vertical axis is reflectance expressed as a percentage. In addition, the solid line in the graph of Fig. 8 shows the reflection characteristics for light with an incident angle of 0 degrees, and the dashed line shows the reflection characteristics for light with an incident angle of 30 degrees. The incident angle is an angle with respect to the normal direction of the light-transmitting member.
[0067] As shown in Fig. 8, the peak wavelength of the reflectance characteristic for light with an incident angle of 0 degrees and the peak wavelength of the reflectance characteristic for light with an incident angle of 30 degrees were both less than 450 nm and slightly different from each other. Therefore, the bezel according to the example was perceived as a blue color with a slightly different hue depending on the location.
[0068] FIG. 9 is an image of the bezel according to the embodiment. As shown in FIG. 9, the bezel according to the embodiment had different colors depending on the location. Although the hue is not shown in FIG. 9, the bezel according to the embodiment was visually recognized as having a color that changed from blue-purple to blue-green from the upper right to the lower left. In addition, the character string that is the decorative pattern P was visually recognized as white, and therefore easily distinguishable from the blue dielectric multilayer film. In this way, it was confirmed that the bezel according to the embodiment has excellent design and allows the decorative pattern to be easily visually recognized.
[0069] It should be understood by those skilled in the art that various changes, substitutions, and modifications can be made to the present invention without departing from the scope of the present invention. For example, the above-described embodiments and modifications may be appropriately combined within the scope of the present invention. [Explanation of symbols]
[0070] 7 Bezel 71 Translucent material 72 Dielectric multilayer film 721 Aperture 73 Light blocking layer 731 Aperture 74 1st printing layer 75 2nd printing layer P decorative pattern
Claims
1. A light-transmitting member; a dielectric multilayer film covering one surface of the light-transmitting member and having openings representing a predetermined pattern; a light-shielding layer covering the dielectric multilayer film; a first printed layer formed of a light-transmitting paint and covering the opening of the dielectric multilayer film; A second printed layer covering the first printed layer; A decorative member for a watch, comprising:
2. The first printed layer further covers the light-shielding layer. The decorative member for a watch according to claim 1.
3. The paint forming the first printing layer is a luminous paint. The decorative member for a watch according to claim 1.
4. The dielectric multilayer film is formed by stacking a plurality of thin films, the plurality of thin films include a first thin film having a first refractive index and a second thin film having a second refractive index different from the first refractive index; The decorative member for a watch according to claim 1.
5. The second printed layer has a light-shielding property. The decorative member for a watch according to claim 1.
6. forming a dielectric multilayer film on one surface of the light-transmitting member; forming a light-shielding layer covering the dielectric multilayer film; forming openings in a predetermined pattern in the dielectric multilayer film and the light-shielding layer; forming a first printed layer by using a light-transmitting paint to cover the opening of the dielectric multilayer film and the light-shielding layer; forming a second printed layer covering the first printed layer; A method for manufacturing a decorative member for a watch, comprising the steps of:
Citation Information
Patent Citations
Dial plate for timepiece, method of manufacturing dial plate for timepiece, and timepiece
JP2009210358A
Decorative member
JP2010228307A
Component for watch and watch
JP2018124268A
Method for depositing coating on substrate
JP2023092467A
Luminous paint and colored luminous part
JP1993001247A