Abrasive composition for magnetic disk substrate
The abrasive composition for magnetic disk substrates, using colloidal silica, a water-soluble polymer, and a quaternary ammonium salt, addresses halation and debris issues, improving polishing efficiency and substrate quality.
Patent Information
- Application Number
- JP2023046917
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
Existing abrasive compositions for magnetic disk substrates fail to effectively reduce halation, residual abrasive grains, and polishing debris while maintaining polishing rate, which affects magnetic recording density and substrate surface quality.
An abrasive composition comprising colloidal silica, a water-soluble polymer compound with specific monomers, a quaternary ammonium salt type organic compound, and controlled pH, which reduces halation and debris while maintaining polishing efficiency.
The composition achieves reduced halation, minimal residual abrasive grains, and improved cleaning properties, enhancing magnetic recording density and substrate surface quality.
Smart Images

Figure 2024135978000001 
Figure 2024135978000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an abrasive composition for magnetic disk substrates. More specifically, the present invention relates to an abrasive composition for magnetic disk substrates used for polishing electronic parts such as semiconductors and magnetic recording media such as hard disks, and in particular to an abrasive composition for magnetic disk substrates used for polishing the surfaces of substrates for magnetic recording media such as glass magnetic disk substrates and aluminum magnetic disk substrates.
[0002] Further, the present invention relates to an abrasive composition for magnetic disk substrates, which is preferably used for finish polishing of aluminum magnetic disk substrates for magnetic recording media, which have an aluminum alloy substrate surface on which an electroless nickel-phosphorus plating film is formed. [Background technology]
[0003] Conventionally, abrasive compositions for magnetic disk substrates are used to polish the surface of electroless nickel-phosphorus plating film of aluminum magnetic disk substrates, and in particular, various polishing properties are required for the abrasive compositions for magnetic disk substrates in order to improve magnetic recording density.For example, scratches remaining on the surface after polishing may cause writing and reading errors when used as a magnetic disk substrate, and further, there is a risk of the head colliding with the "burrs" generated around the scratched parts.Therefore, there is a demand for reducing scratches on the surface after polishing.
[0004] Therefore, colloidal silica is often used as an abrasive component for mechanical polishing of an abrasive composition for magnetic disk substrates in the finish polishing of aluminum magnetic disk substrates. In this case, in industrial polishing, a mixture of an abrasive component for mechanical polishing of an abrasive composition for magnetic disk substrates and a chemical component for chemical polishing is generally used immediately before the polishing step.
[0005] It is known that when colloidal silica and a drug component are mixed as abrasive grain components, colloidal silica tends to aggregate.In order to prevent such problems, attempts have been made to prevent the aggregation of colloidal silica and reduce scratches when used as an abrasive composition for magnetic disk substrates by removing coarse particles, agglomerated particles, etc. contained in the abrasive composition for magnetic disk substrates before mixing, adjusting the shape of colloidal silica particles, or adjusting the corrosiveness of the abrasive itself, including the abrasive composition for magnetic disk substrates.For example, attempts have been proposed to adjust the corrosiveness of the abrasive (Patent Document 1), adjust the shape of particles (Patent Document 2), adjust the content of agglomerated particles (Patent Document 3), etc. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2009-120850 A [Patent Document 2] JP 2009-172709 A [Patent Document 3] JP 2010-170650 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, in order to improve the magnetic recording density, there remain problems to be solved, such as reducing the above-mentioned scratches and waviness on the substrate surface, as well as reducing halation that is believed to be caused by surface defects that are even finer than the scratches, and preventing the adhesion of remaining abrasive grains and polishing debris to the substrate surface.
[0008] In view of the above circumstances, an object of the present invention is to provide an abrasive composition for magnetic disk substrates which maintains the removal rate while reducing halation and has excellent cleaning properties, such that no residual abrasive grains or polishing debris remain on the substrate surface after polishing. [Means for solving the problem]
[0009] In order to solve the above problems, the inventors have conducted extensive research and have found that by using the following abrasive composition for magnetic disk substrates, it is possible to reduce halation and adhesions on the substrate surface while maintaining the removal rate, thereby arriving at the present invention.
[0010] [1] An abrasive composition used for finish polishing of electrolessly nickel-phosphorus plated aluminum magnetic disk substrates, comprising colloidal silica, a water-soluble polymeric compound, a quaternary ammonium salt type organic compound, and water, wherein the water-soluble polymeric compound contains a copolymer having at least a monomer having a carboxylic acid group and a monomer having a sulfonic acid group as essential monomers, and the quaternary ammonium salt type organic compound contains a copolymer in which the four hydrocarbon groups bonded to nitrogen atoms are saturated aliphatic hydrocarbon groups having 1 to 20 carbon atoms and / or unsaturated aliphatic hydrocarbon groups having 2 to 20 carbon atoms.
[0011] [2] The abrasive composition for magnetic disk substrates according to [1], wherein the quaternary ammonium salt type organic compound has four hydrocarbon groups bonded to nitrogen atoms which are saturated aliphatic hydrocarbon groups having 1 to 10 carbon atoms and / or unsaturated aliphatic hydrocarbon groups having 2 to 20 carbon atoms.
[0012] [3] The abrasive composition for magnetic disk substrates according to [2], wherein the quaternary ammonium salt type organic compound is at least one selected from the group consisting of vinyltrimethylammonium chloride, allyltrimethylammonium chloride, divinyldimethylammonium chloride, diallyldimethylammonium chloride, diallyldimethylammonium fluoride, diallyldimethylammonium bromide, diallyldimethylammonium iodide, diallyldiethylammonium chloride, tetraallylammonium chloride, diethyldimethylammonium chloride, triethylmethylammonium chloride, tetraethylammonium chloride, dibutyldimethylammonium chloride, tetrabutylammonium chloride, dioctyldimethylammonium chloride, didecyldimethylammonium chloride, octyltrimethylammonium chloride, and decyltrimethylammonium chloride.
[0013] [4] The abrasive composition for magnetic disk substrates according to [1] above, wherein the quaternary ammonium salt type organic compound is a mixture containing at least one of: a first quaternary ammonium salt type organic compound in which the four hydrocarbon groups bonded to the nitrogen atom are saturated aliphatic hydrocarbon groups having 1 to 20 carbon atoms; and a second quaternary ammonium salt type organic compound in which at least one of the four hydrocarbon groups bonded to the nitrogen atom is an unsaturated aliphatic hydrocarbon group having 2 to 20 carbon atoms, and the remaining hydrocarbon groups are saturated aliphatic hydrocarbon groups having 1 to 20 carbon atoms.
[0014] [5] The abrasive composition for magnetic disk substrates according to any one of [1] to [4], wherein the water-soluble polymer compound further contains a copolymer having at least a monomer having a carboxylic acid group and a monomer having an amide group as essential monomers.
[0015] [6] The abrasive composition for magnetic disk substrates according to any one of the above [1] to [5], further comprising an acid and / or a salt thereof and having a pH value (25° C.) in the range of 0.1 to 4.0.
[0016] [7] The abrasive composition for magnetic disk substrates according to any one of the above [1] to [6], further comprising an oxidizing agent. Effect of the Invention
[0017] The polishing compound of the present invention contains colloidal silica, a water-soluble polymeric compound, a quaternary ammonium salt type organic compound, and water, and the water-soluble polymeric compound is a copolymer having, as essential monomers, a monomer having a carboxylic acid group and a monomer having a sulfonic acid group. When used in polishing a magnetic disk substrate, the polishing compound exerts the effect of reducing halation and reducing adhesion of residual abrasive grains and polishing debris to the substrate surface while maintaining the polishing rate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The following describes the embodiments of the present invention. However, the present invention is not limited to the following embodiments. It should be understood that modifications and improvements made to the following embodiments based on the ordinary knowledge of those skilled in the art without departing from the spirit of the present invention are also within the scope of the present invention.
[0019] 1. Abrasive composition An abrasive composition for magnetic disk substrates (hereinafter simply referred to as "abrasive composition") which is one embodiment of the present invention contains colloidal silica, a water-soluble polymeric compound, a quaternary ammonium salt type organic compound, and water, and optionally contains an acid and / or its salt, an oxidizing agent, and other additives.
[0020] 1.1 Colloidal Silica The colloidal silica used in the polishing compound composition of the present embodiment preferably has an average particle size (D50) of 1 to 100 nm. More preferably, it is 2 to 80 nm, and even more preferably, it is 3 to 40 nm. Colloidal silica can be obtained by the water glass method in which an alkali metal silicate such as sodium silicate or potassium silicate is used as a raw material and the raw material is subjected to a condensation reaction in an aqueous solution to grow particles, the alkoxysilane method in which an alkoxysilane such as tetraethoxysilane is used as a raw material and the raw material is subjected to a condensation reaction by hydrolysis with an acid or alkali in water containing a water-soluble organic solvent such as alcohol to grow particles, or a method in which metal silicon is reacted with water in the presence of an alkali catalyst to form silica particles while generating hydrogen.
[0021] Colloidal silica is known to have shapes such as spherical, chain-like, confetti-shaped, and irregular shapes, and the primary particles are monodispersed in water to form a colloid. As the colloidal silica to be used, spherical or nearly spherical colloidal silica is particularly preferred. The use of spherical or nearly spherical colloidal silica has the advantage of reducing scratches.
[0022] The concentration of colloidal silica in the polishing compound is preferably within the range of 1 to 50 mass %, more preferably 2 to 40 mass %.
[0023] 1.2 Water-soluble polymer compounds The water-soluble polymer compound used in the polishing compound of this embodiment is a copolymer having a carboxylic acid group-containing monomer and a sulfonic acid group-containing monomer as essential monomers. It is also a preferred embodiment to use a copolymer having a carboxylic acid group-containing monomer and an amide group-containing monomer as essential monomers in combination.
[0024] 1.2.1 Copolymers containing a monomer having a carboxylic acid group and a monomer having a sulfonic acid group as essential monomers Examples of monomers having a carboxylic acid group include acrylic acid, methacrylic acid, maleic acid, itaconic acid, and salts thereof, while examples of monomers having a sulfonic acid group include isoprene sulfonic acid, 2-acrylamido-2-methylpropane sulfonic acid, 2-methacrylamido-2-methylpropane sulfonic acid, styrene sulfonic acid, vinyl sulfonic acid, allyl sulfonic acid, and salts thereof.
[0025] Specific examples of copolymers having a monomer having a carboxylic acid group and a monomer having a sulfonic acid group as essential monomers include acrylic acid / isoprene sulfonic acid copolymer, methacrylic acid / isoprene sulfonic acid copolymer, acrylic acid / 2-acrylamide-2-methylpropane sulfonic acid copolymer, methacrylic acid / 2-acrylamide-2-methylpropane sulfonic acid copolymer, acrylic acid / 2-methacrylamide-2-methylpropane sulfonic acid copolymer, methacrylic acid / 2-methacrylamide-2-methylpropane sulfonic acid copolymer, and the like.
[0026] In the copolymer having the above-mentioned monomer having a carboxylic acid group and monomer having a sulfonic acid group as essential monomers, the ratio of the constituent units derived from the monomer having a carboxylic acid group to the constituent units derived from the monomer having a sulfonic acid group is preferably in the range of 95:5 to 5:95 in molar ratio, more preferably 90:10 to 10:90, and even more preferably 80:20 to 20:80 in molar ratio.
[0027] The weight-average molecular weight of the copolymer containing the above-mentioned monomer having a carboxylic acid group and monomer having a sulfonic acid group as essential monomers is preferably in the range of 1,000 to 1,000,000, and more preferably in the range of 3,000 to 500,000. The weight-average molecular weight of the copolymer is measured by gel permeation chromatography (GPC) in terms of polyacrylic acid.
[0028] The concentration of the copolymer having the above-mentioned monomer having a carboxylic acid group and monomer having a sulfonic acid group as essential monomers in the polishing compound is preferably 0.0001 to 2.0 mass%, more preferably 0.001 to 1.0 mass%, and even more preferably 0.005 to 0.5 mass%, calculated as solid content.
[0029] 1.2.2 Copolymers containing a carboxylic acid group-containing monomer and an amide group-containing monomer as essential monomers In the polishing compound composition of this embodiment, a copolymer having a carboxylic acid group-containing monomer and an amide group-containing monomer as essential monomers, which is preferably used for the purpose of improving the polishing rate, will be described below.
[0030] The monomer having a carboxylic acid group may be contained in part as a salt of a carboxylic acid, such as a sodium salt, a potassium salt, a magnesium salt, an ammonium salt, an amine salt, or an alkyl ammonium salt.
[0031] To incorporate a monomer having a carboxylic acid group as a carboxylic acid, the monomer may be polymerized as a monomer having a carboxylic acid group, or a monomer having a carboxylic acid salt group may be polymerized and then converted to a carboxylic acid by cation exchange. To incorporate a monomer having a carboxylic acid group as a carboxylic acid salt, the monomer may be polymerized as a monomer having a carboxylate group, or a monomer having a carboxylic acid group may be polymerized and then neutralized with a base to form a carboxylic acid salt.
[0032] In order to evaluate the ratio of the monomer having a carboxylic acid group and the monomer having a carboxylic acid salt group, the pH value of the copolymer aqueous solution can be used. When the pH value of the copolymer aqueous solution is low, it can be evaluated that the content ratio of the monomer having a carboxylic acid group is high. On the other hand, when the pH value of the copolymer aqueous solution is high, it can be evaluated that the content ratio of the monomer having a carboxylic acid salt group is high. In the present invention, for example, a copolymer having a pH value in the range of 1 to 13 in a copolymer aqueous solution with a concentration of 10% by mass can be used.
[0033] Specific examples of monomers having an amide group include acrylamide, methacrylamide, N-alkylacrylamide, and N-alkylmethacrylamide.
[0034] Specific preferred examples of N-alkylacrylamides and N-alkylmethacrylamides include N-methylacrylamide, N-ethylacrylamide, Nn-propylacrylamide, N-iso-propylacrylamide, Nn-butylacrylamide, N-iso-butylacrylamide, N-sec-butylacrylamide, N-tert-butylacrylamide, N-methylmethacrylamide, N-ethylmethacrylamide, Nn-propylmethacrylamide, N-iso-propylmethacrylamide, Nn-butylmethacrylamide, N-iso-butylmethacrylamide, N-sec-butylmethacrylamide, N-tert-butylmethacrylamide, etc. Among these, Nn-butylacrylamide, N-iso-butylacrylamide, N-tert-butylacrylamide, Nn-butylmethacrylamide, N-iso-butylmethacrylamide, N-sec-butylmethacrylamide, N-tert-butylmethacrylamide, etc. are particularly preferred.
[0035] It is preferable to combine and polymerize these monomer components to form a copolymer. As the combination of the copolymer, a combination of acrylic acid and / or a salt thereof with N-alkylacrylamide, a combination of acrylic acid and / or a salt thereof with N-alkylmethacrylamide, a combination of methacrylic acid and / or a salt thereof with N-alkylacrylamide, and a combination of methacrylic acid and / or a salt thereof with N-alkylmethacrylamide are preferably used. Among them, N-alkylacrylamides or N-alkylmethacrylamides in which the alkyl group is at least one selected from the group consisting of n-butyl group, iso-butyl group, sec-butyl group, and tert-butyl group are particularly preferably used.
[0036] In the copolymer having the above-mentioned monomer having a carboxylic acid group and monomer having an amide group as essential monomers, the ratio of the structural units derived from the monomer having a carboxylic acid group to the structural units derived from the monomer having an amide group is preferably in the range of 95:5 to 5:95 in molar ratio, and more preferably 90:10 to 10:90 in molar ratio.
[0037] The weight-average molecular weight of the copolymer containing the above-mentioned monomer having a carboxylic acid group and monomer having an amide group as essential monomers is preferably in the range of 1,000 to 1,000,000, and more preferably in the range of 3,000 to 500,000. The weight-average molecular weight of the copolymer is measured by gel permeation chromatography (GPC) in terms of polyacrylic acid.
[0038] The concentration of the copolymer having the above-mentioned monomer having a carboxylic acid group and monomer having an amide group as essential monomers in the polishing compound is preferably 0.0001 to 2.0 mass%, more preferably 0.001 to 1.0 mass%, and even more preferably 0.005 to 0.5 mass%, calculated as solid content.
[0039] 1.2.3 Method for producing water-soluble polymer compounds The method for producing the water-soluble polymer compound is not particularly limited, but for example, an aqueous solution polymerization method is preferred. According to the aqueous solution polymerization method, the water-soluble polymer compound can be obtained as a homogeneous solution.
[0040] The polymerization solvent for the aqueous solution polymerization is preferably an aqueous solvent, and particularly preferably water. In order to improve the solubility of the monomer components in the solvent, an organic solvent may be added within a range that does not adversely affect the polymerization of each monomer. Examples of the organic solvent include alcohols such as isopropyl alcohol and ketones such as acetone. These can be used alone or in combination of two or more.
[0041] A method for producing a water-soluble polymer compound using the above aqueous solvent will be described below. In the polymerization reaction, a known polymerization initiator can be used, and a radical polymerization initiator is particularly preferably used.
[0042] Examples of the radical polymerization initiator include persulfates such as sodium persulfate, potassium persulfate, and ammonium persulfate, hydroperoxides such as t-butyl hydroperoxide, water-soluble peroxides such as hydrogen peroxide, ketone peroxides such as methyl ethyl ketone peroxide and cyclohexanone peroxide, oil-soluble peroxides such as dialkyl peroxides such as di-t-butyl peroxide and t-butylcumyl peroxide, and azo compounds such as azobisisobutyronitrile and 2,2-azobis(2-methylpropionamidine)dihydrochloride. These peroxide-based radical polymerization initiators may be used alone or in combination of two or more.
[0043] The amount of the radical polymerization initiator is not particularly limited, but is preferably 0.1 to 15 mass%, particularly 0.5 to 10 mass%, based on the total mass of all monomers in the water-soluble polymer compound. By making this ratio 0.1 mass% or more, the copolymerization rate can be improved, and by making it 15 mass% or less, the stability of the water-soluble polymer compound can be improved.
[0044] In some cases, the water-soluble polymer compound may be produced using a water-soluble redox polymerization initiator, which may be a combination of an oxidizing agent (such as the above-mentioned peroxides) and a reducing agent such as sodium bisulfite, ammonium bisulfite, ammonium sulfite, or sodium hydrosulfite, or iron alum, potassium alum, or the like.
[0045] In the production of a water-soluble polymer compound, a chain transfer agent may be appropriately added to the polymerization system in order to adjust the molecular weight. Examples of the chain transfer agent include sodium phosphite, sodium hypophosphite, potassium hypophosphite, sodium sulfite, sodium hydrogen sulfite, mercaptoacetic acid, mercaptopropionic acid, thioglycolic acid, 2-propanethiol, 2-mercaptoethanol, and thiophenol.
[0046] The polymerization temperature when producing the water-soluble polymer compound is not particularly limited, but the polymerization temperature is preferably 60 to 100° C. By setting the polymerization temperature at 60° C. or higher, the polymerization reaction proceeds smoothly and the productivity is excellent, and by setting the polymerization temperature at 100° C. or lower, coloring can be suppressed.
[0047] The polymerization reaction can be carried out under increased or reduced pressure, but is preferably carried out under normal pressure since it requires costs to prepare equipment for the reaction under increased or reduced pressure. The polymerization time is preferably 2 to 20 hours, more preferably 3 to 10 hours.
[0048] After the polymerization reaction, neutralization is carried out as necessary with a basic compound, such as alkali metal hydroxides (e.g., sodium hydroxide, potassium hydroxide, etc.), alkaline earth metal hydroxides (e.g., calcium hydroxide, magnesium hydroxide, etc.), aqueous ammonia, and organic amines (e.g., monoethanolamine, diethanolamine, triethanolamine, etc.).
[0049] The pH value (25° C.) after neutralization is preferably 2 to 9, and more preferably 3 to 8, in the case of an aqueous solution having a water-soluble polymer compound concentration of 10% by mass.
[0050] 1.3 Quaternary ammonium salt organic compounds The quaternary ammonium salt type organic compound contained in the polishing compound composition of this embodiment is a quaternary ammonium salt type organic compound in which the hydrocarbon group bonded to the nitrogen atom is composed of a saturated aliphatic hydrocarbon group having 1 to 20 carbon atoms and / or an unsaturated aliphatic hydrocarbon group having 2 to 20 carbon atoms.
[0051] Specific examples include vinyl trimethyl ammonium chloride, allyl trimethyl ammonium chloride, divinyl dimethyl ammonium chloride, diallyl dimethyl ammonium chloride, diallyl dimethyl ammonium fluoride, diallyl dimethyl ammonium bromide, diallyl dimethyl ammonium iodide, diallyl diethyl ammonium chloride, tetraallyl ammonium chloride, diethyl dimethyl ammonium chloride, triethyl methyl ammonium chloride, tetraethyl ammonium chloride, dibutyl dimethyl ammonium chloride, tetrabutyl ammonium chloride, dioctyl dimethyl ammonium chloride, didecyl dimethyl ammonium chloride, octyl trimethyl ammonium chloride, decyl trimethyl ammonium chloride, and dodecyl trimethyl ammonium chloride.
[0052] From the viewpoint of suppressing the slimy feeling of the polishing composition and suppressing a decrease in the polishing rate, a quaternary ammonium salt type organic compound in which the four hydrocarbon groups bonded to the nitrogen atom are saturated aliphatic hydrocarbon groups having 1 to 10 carbon atoms and / or unsaturated aliphatic hydrocarbon groups having 2 to 20 carbon atoms is preferably used as the quaternary ammonium salt type organic compound.
[0053] These quaternary ammonium salt type organic compounds can be used alone or in combination of two or more kinds of quaternary ammonium salt type organic compounds. In particular, it is preferable to use a mixture containing at least one of a first quaternary ammonium salt type organic compound in which the hydrocarbon group bonded to the nitrogen atom is composed of four saturated aliphatic hydrocarbon groups having 1 to 20 carbon atoms, and a second quaternary ammonium salt type organic compound in which at least one of the hydrocarbon groups bonded to the nitrogen atom is an unsaturated aliphatic hydrocarbon group having 2 to 20 carbon atoms, and the remaining hydrocarbon groups are saturated aliphatic hydrocarbon groups having 1 to 20 carbon atoms. More specifically, for example, a mixture containing diallyldimethylammonium chloride and dodecyltrimethylammonium chloride can be used.
[0054] The concentration of the quaternary ammonium salt type organic compound in the polishing composition is usually 0.00001 to 1.0 mass %, preferably 0.00005 to 0.5 mass %, more preferably 0.0001 to 0.3 mass %, and even more preferably 0.0001 to 0.1 mass %.
[0055] 1.4 Acids and / or their salts The polishing compound composition of the present embodiment may contain an acid and / or a salt thereof for the purpose of controlling the pH value (25° C.).Specific examples of the acid include inorganic acids and / or salts thereof such as nitric acid, sulfuric acid, hydrochloric acid, phosphoric acid, phosphonic acid, phosphinic acid, pyrophosphoric acid, and tripolyphosphoric acid, organic phosphonic acids and / or salts thereof such as 2-aminoethylphosphonic acid, 1-hydroxyethylidene-1,1-diphosphonic acid, aminotri(methylenephosphonic acid), ethylenediaminetetra(methylenephosphonic acid), diethylenetriamine(methylenephosphonic acid), ethane-1,1-diphosphonic acid, and methanehydroxyphosphonic acid, aminocarboxylic acids and / or salts thereof such as glutamic acid and aspartic acid, and carboxylic acids and / or salts thereof such as citric acid, tartaric acid, oxalic acid, nitroacetic acid, and maleic acid.
[0056] It is also a preferred embodiment to use two or more of the above compounds in combination. Specific examples include a combination of sulfuric acid and / or a salt thereof with an organic phosphonic acid and / or a salt thereof, and a combination of phosphoric acid and / or a salt thereof with an organic phosphonic acid and / or a salt thereof.
[0057] The content of the acid and / or its salt in the polishing compound is appropriately determined depending on the pH value (25° C.) of the polishing compound.
[0058] 1.5 Oxidizing agents The polishing composition of the present invention may contain an oxidizing agent to improve the removal rate. Examples of the oxidizing agent include peroxides, permanganic acid or a salt thereof, chromic acid or a salt thereof, and periodic acid or a salt thereof.
[0059] Specific examples include hydrogen peroxide, sodium peroxide, barium peroxide, potassium permanganate, orthoperiodic acid, and sodium metaperiodate. Among these, hydrogen peroxide is preferred. The oxidizing agent is usually used in an amount of 0.1 to 10.0% by mass in the polishing compound. When the oxidizing agent is contained in an amount of 0.1% by mass or more, the polishing rate is improved. When the oxidizing agent is contained in an amount of 10.0% by mass or more, no improvement in the polishing rate is observed, which is economically disadvantageous.
[0060] The polishing composition of the present invention may contain, in addition to the above components, a buffering agent, an antifungal agent, an antibacterial agent, and the like.
[0061] 1.6 Water The water used in the present invention is preferably water from which impurities have been removed, such as distilled water or ion-exchanged water. Since water has a function of controlling the fluidity of the polishing compound, its content can be appropriately determined according to the target polishing characteristics such as the polishing rate. For example, the content of water is preferably 50 to 95% by mass. If the content of water is less than 50% by mass of the polishing compound, the viscosity of the polishing compound may increase and the fluidity may be impaired. On the other hand, if the content of water exceeds 95% by mass, the concentration of abrasive grains may decrease and a sufficient polishing rate may not be obtained.
[0062] 2. Physical properties The pH value (25°C) of the polishing compound is preferably 0.1 to 4.0, more preferably 0.5 to 3.0. When the pH value (25°C) of the polishing compound is 0.1 or more, deterioration of surface smoothness can be suppressed. When the pH value (25°C) of the polishing compound is 4.0 or less, decrease in removal rate can be suppressed.
[0063] In polishing electroless nickel-phosphorus plated aluminum magnetic disk substrates, for which the abrasive composition of the present invention is preferably used, the electroless nickel-phosphorus plating film tends to dissolve under conditions of a pH value (25°C) of 4.0 or less, so that an abrasive composition having a pH value (25°C) of 4.0 or less is preferably used from the viewpoint of improving the polishing rate. 3. Method for polishing magnetic disk substrate The polishing agent composition of the present invention is suitable for use in polishing magnetic disk substrates such as electroless nickel-phosphorus plated aluminum magnetic disk substrates and glass magnetic disk substrates. It is particularly suitable for use in polishing electroless nickel-phosphorus plated aluminum magnetic disk substrates. It is further suitable for use in finish polishing of electroless nickel-phosphorus plated aluminum magnetic disk substrates.
[0064] A polishing method to which the abrasive composition of the present embodiment can be applied includes, for example, a method in which a polishing pad is attached to the platen of a polishing machine, the abrasive composition is supplied to the surface to be polished of an object to be polished (e.g., an aluminum magnetic disk substrate) or to the polishing pad, and the surface to be polished is rubbed with the polishing pad.
[0065] For example, when polishing the front and back surfaces of an aluminum magnetic disk substrate simultaneously, the aluminum magnetic disk substrate is sandwiched between polishing pads attached to an upper and lower surface plate, an abrasive composition is supplied between the polishing surface and the polishing pad, and the two polishing pads are rotated simultaneously to polish the front and back surfaces of the aluminum magnetic disk substrate.
[0066] Various types of polishing pads can be used, and the surface shape of the polishing pad may be either with or without grooves. EXAMPLES
[0067] The present invention will be described in detail below based on examples. However, the present invention is not limited to these examples, and it goes without saying that the present invention can be embodied in various forms as long as it falls within the technical scope of the present invention.
[0068] (1) Method for preparing abrasive composition The polishing compound compositions used in Examples 1 to 13 and Comparative Examples 1 to 4 were prepared so that the colloidal silica, acid, oxidizing agent, quaternary ammonium salt type organic compound, and water-soluble polymer compound were of the types and contained in the polishing compound compositions as shown in Table 1.
[0069] In Table 1, "AA" represents acrylic acid, "TBAA" represents N-tert-butylacrylamide, and "ATBS" represents 2-acrylamido-2-methylpropanesulfonic acid. As shown in Table 1, the polymers of Synthesis Nos. 1 and 2 were used as water-soluble polymer compounds.
[0070] [Table 1]
[0071] Preparation of Example 1 A polishing compound composition was prepared by adding colloidal silica, sulfuric acid, hydrogen peroxide, the polymer of Synthesis No. 1 as a water-soluble polymeric compound, and diallyldimethylammonium chloride as a quaternary ammonium salt type organic compound to pure water with stirring so as to obtain the contents shown in Table 1.
[0072] Preparation of Example 2 A polishing compound was prepared in the same manner as in Example 1, except that the amount of diallyldimethylammonium chloride added was changed to the amount shown in Table 1.
[0073] Preparation of Example 3 A polishing compound was prepared in the same manner as in Example 1, except that the amount of diallyldimethylammonium chloride added was changed to the amount shown in Table 1.
[0074] Preparation of Example 4 A polishing compound was prepared in the same manner as in Example 1, except that the amount of diallyldimethylammonium chloride added was changed to the amount shown in Table 1.
[0075] Preparation of Example 5 A polishing compound was prepared in the same manner as in Example 1, except that tetrabutylammonium chloride was used instead of diallyldimethylammonium chloride.
[0076] Preparation of Example 6 A polishing compound composition was prepared in the same manner as in Example 1, except that n-octyltrimethylammonium chloride was used instead of diallyldimethylammonium chloride.
[0077] Preparation of Example 7 A polishing compound was prepared in the same manner as in Example 1, except that decyltrimethylammonium chloride was used instead of diallyldimethylammonium chloride.
[0078] Preparation of Example 8 A polishing compound composition was prepared in the same manner as in Example 1, except that dodecyltrimethylammonium chloride was used instead of diallyldimethylammonium chloride in Example 1. After preparation, the polishing compound composition of Example 8 had a slimy feel.
[0079] Preparation of Example 9 A polishing composition was prepared in the same manner as in Example 1, except that in addition to diallyldimethylammonium chloride as the quaternary ammonium salt type organic compound, dodecyltrimethylammonium chloride was added to the composition in an amount shown in Table 1. Note that, since the amount of dodecyltrimethylammonium chloride added was small, the prepared polishing composition of Example 9 did not have a slimy feel.
[0080] Preparation of Example 10 A polishing composition was prepared in the same manner as in Example 9, except that the amount of dodecyltrimethylammonium chloride added was set to the amount shown in Table 1. The prepared polishing composition of Example 10 had no slimy feeling because the amount of dodecyltrimethylammonium chloride added was small.
[0081] Preparation of Example 11 A polishing composition was prepared in the same manner as in Example 9, except that the amount of dodecyltrimethylammonium chloride added was set to the amount shown in Table 1. The polishing composition of Example 11 after preparation had a slight slimy feel.
[0082] Preparation of Example 12 A polishing agent composition was prepared in the same manner as in Example 1, except that in addition to the polymer of Synthesis No. 1, the polymer of Synthesis No. 2 was added as the water-soluble polymer compound in an amount shown in Table 1.
[0083] Preparation of Example 13 A polishing composition was prepared in the same manner as in Example 9, except that in Example 9, the polymer of Synthesis No. 2 was added as the water-soluble polymer compound in addition to the polymer of Synthesis No. 1 so as to have the content shown in Table 1. The polishing composition of Example 12 after preparation did not have a slimy feel.
[0084] (Preparation of Comparative Example 1) A polishing compound of Comparative Example 1 was prepared in the same manner as in Example 1, except that the water-soluble polymer compound and the quaternary ammonium salt type organic compound were not added.
[0085] (Preparation of Comparative Example 2) A polishing compound of Comparative Example 2 was prepared in the same manner as in Example 1, except that the quaternary ammonium salt type organic compound was not added.
[0086] (Preparation of Comparative Example 3) A polishing compound of Comparative Example 3 was prepared in the same manner as in Example 12, except that the quaternary ammonium salt type organic compound was not added.
[0087] (Preparation of Comparative Example 4) A polishing composition of Comparative Example 4 was prepared in the same manner as in Example 8, except that the water-soluble polymer compound was not added. After preparation, the polishing composition of Comparative Example 4 had a slimy feel.
[0088] A polishing test was carried out using the polishing compound compositions of Examples 1 to 13 and Comparative Examples 1 to 4 prepared as described above. The results are shown in Table 2 below.
[0089] [Table 2]
[0090] The copolymers of Synthesis Nos. 1 and 2 shown in Table 1 were used as the water-soluble polymeric compounds contained in the polishing compound composition. The weight-average molecular weight of the water-soluble polymeric compounds was measured by gel permeation chromatography (GPC) in terms of polyacrylic acid. The GPC measurement conditions are shown below.
[0091] (2) GPC measurement conditions Column: G4000PWXL (manufactured by Tosoh Corporation) + G2500PWXL (manufactured by Tosoh Corporation) Eluent: 0.2M phosphate buffer / acetonitrile = 9 / 1 (volume ratio) Flow rate: 1.0ml / min Temperature: 40℃ Detection: 210nm (UV) Sample: concentration 5mg / ml (injection volume 100μl) Polymer for calibration curve: Polyacrylic acid Molecular weight (peak top molecular weight: Mp) 115,000, 28,000, 4100, 1250 (manufactured by Sowa Chemical Co., Ltd., American Polymer Standards Corp.)
[0092] (3) Method for measuring particle size and average particle size of colloidal silica The particle diameter (Heywood diameter) of the colloidal silica was measured as the Heywood diameter (diameter equivalent to a circle with a projected area) by photographing a field of view at a magnification of 100,000 times using a transmission electron microscope (TEM) (JEM2000FX (200 kV) manufactured by JEOL Ltd.) and analyzing the photograph using analysis software (Mac-View Ver. 4.0 manufactured by Mountec Co., Ltd.).
[0093] The average particle size of colloidal silica is the average particle size (D50) calculated by analyzing the particle sizes of approximately 2,000 colloidal silica particles using the method described above, and calculating the particle size at which the cumulative particle size distribution (accumulated volume basis) from the small particle size side is 50% using the above analysis software (Mountec Co., Ltd., Mac-View Ver. 4.0).
[0094] (4) Polishing conditions The polishing target was an electroless nickel-phosphorus plated aluminum magnetic disk substrate having an outer diameter of 97 mm that had been roughly polished. Polishing machine: Speedfam Co., Ltd., 9B double-sided polishing machine Polishing pad: P2 pad manufactured by FILWEL Co., Ltd. Rotation speed of surface plate: Upper surface plate -6.7min -1 Lower surface plate 20.0min -1 Abrasive composition supply rate: 100ml / min Polishing time: 340 seconds Processing pressure: 14kPa
[0095] (5) Evaluation of the polished disk surface (5-1) Polishing speed ratio The removal rate was calculated based on the following formula by measuring the mass of the aluminum magnetic disk substrate lost after polishing. Polishing rate (mg / min) = mass loss of aluminum magnetic disk substrate (mg) / polishing time (min) Furthermore, the polishing rate ratio is a relative value when the polishing rate calculated using the above formula when the substrate was polished in Comparative Example 1 is taken as 1 (reference).
[0096] (5-2) Method for evaluating halation on substrate surface after polishing Halation was measured using a full-surface substrate defect inspection machine (NS2000H, manufactured by Hitachi High-Tech Fine Technology Systems Corporation).
[0097] The conditions for measuring halation are as follows: PMT / APD Power Control Voltage Hi-Light 1 OFF Hi-Light 2 875V Scan Pitch 3μm Inner / Outer Radius 15.500-48.000mm Positive Level 73mV H2 White Spot Level 250mV
[0098] Under the above inspection conditions, halation is detected as a minute defect on the substrate surface and can be quantitatively evaluated as a halation count. The halation count thus obtained was ranked according to the following criteria. The ranking results are shown in Table 2 above. ◎: Count number 0~499 〇: Count number 500~549 △: Count number 550~599 ×: Count number 600 or more
[0099] (5-3) Method for evaluating the cleaning properties of abrasives In each Example and Comparative Example, the surface of the polished aluminum magnetic disk substrate was rinsed with ion-exchanged water, then scrubbed with ion-exchanged water, and after scrubbing, rinsed with ion-exchanged water and then spin-dried. The obtained aluminum magnetic disk substrate was used as a substrate for cleaning evaluation. The above operations were carried out in a clean room.
[0100] The substrate for cleaning evaluation obtained above was inspected using an inspection device (Vision Scitex MicroMAX VMX-4100) capable of highlighting and inspecting minute residual particles on the substrate surface, and the front and back surfaces of the aluminum disk were observed under the following measurement conditions in 6 fields of view on the front surface and 6 fields of view on the back surface (total of 12 fields of view), and the number of residual particles observed in one field (9 mm x 7 mm) was counted. The number of residual particles observed by the above method was then calculated and ranked from the total number of residual particles in the 12 fields of view in accordance with the "Cleaning Evaluation Criteria" below. The ranking results are shown in Table 2.
[0101] (5-4) Measurement conditions of the inspection device (MicroMAX VMX-4100) Tilt: -5° Iris: 10 Zoom:10
[0102] Cleanability evaluation standard (average number of residual particles per field of view) ◎: Number of residual particles: 0 to 1.0 〇: Residual particle count 1.1 to 2.0 △: Number of remaining particles: 2.1 to 5.0 ×: Number of remaining particles > 5.1
[0103] (6) Discussion In Examples 1 to 8, by using a polishing composition containing both a water-soluble polymer compound and a quaternary ammonium salt type organic compound, it was found that the cleaning ability was significantly improved and the polishing rate was also improved compared to Comparative Example 1, which used a polishing composition containing neither.
[0104] In contrast, Comparative Example 2, which contained only a water-soluble polymer compound, showed a slight improvement in cleaning performance compared to Comparative Example 1, but the improvement was insufficient. It was found that Example 1, which contained a water-soluble polymer compound and a quaternary ammonium salt-type organic compound, showed an even improved cleaning performance compared to Comparative Example 2.
[0105] Furthermore, in Comparative Example 4, which contains only a quaternary ammonium salt type organic compound, the cleaning ability is improved compared to Comparative Example 1, but the halation is deteriorated and the polishing rate is also decreased. On the other hand, in Examples 1 to 8, which contain a quaternary ammonium salt type organic compound and a water-soluble polymer compound, the halation is good and the polishing rate is improved.
[0106] Examples 2 to 4 are examples in which the content of the quaternary ammonium salt type organic compound in Example 1 is changed. Examples 5 to 8 are examples in which the type of the quaternary ammonium salt type organic compound in Example 1 is changed.
[0107] Comparing Comparative Example 4, which uses dodecyltrimethylammonium chloride as the quaternary ammonium salt type organic compound, with Example 8, Example 8 has improved cleaning performance, improved halation, and improved polishing speed compared to Comparative Example 4. This is due to the synergistic effect of the combined use of a water-soluble polymer compound and a quaternary ammonium salt type organic compound.
[0108] Example 9 is an example in which the total amount of quaternary ammonium salt type organic compound added is the same as that of Example 2, but two types of quaternary ammonium salt type organic compounds are used in combination, and the cleaning performance is improved compared to Example 2.
[0109] Example 10 is an example in which the total amount of quaternary ammonium salt type organic compound added is the same as that of Example 3, but two types of quaternary ammonium salt type organic compounds are used in combination, and the cleaning performance is improved compared to Example 3.
[0110] Example 11 is an example in which the total amount of quaternary ammonium salt type organic compound added is the same as that of Example 4, but two types of quaternary ammonium salt type organic compounds are used in combination, and the cleaning performance is improved compared to Example 4.
[0111] Example 12 is an example in which the water-soluble polymer compound of Synthesis No. 2 is further added in addition to the water-soluble polymer compound of Synthesis No. 1 in Example 1, and the polishing rate is improved compared to Example 1. At the same time, Example 12 is an example in which a quaternary ammonium salt type organic compound is added in Comparative Example 3, and the cleaning performance is improved.
[0112] Example 13 is an example in which the water-soluble polymer compound of Synthesis No. 2 was further added in addition to the water-soluble polymer compound of Synthesis No. 1 in Example 9, and the polishing rate was improved compared to Example 9.
[0113] From the above, it is clear that the polishing agent composition containing the water-soluble polymer compound of the present invention and the quaternary ammonium salt type organic compound has a better balance of polishing speed, halation, and cleaning ability than Comparative Example 1 which contains neither, and Comparative Examples 2 to 4 which contain either one of them. [Industrial Applicability]
[0114] The polishing agent composition of the present invention can be used for polishing electronic parts such as semiconductors and magnetic recording media such as hard disks. In particular, it can be used for surface polishing of substrates for magnetic recording media such as glass magnetic disks and aluminum magnetic disks. Furthermore, it can be suitably used for finish polishing of aluminum substrates for magnetic recording media having an electroless nickel-phosphorus plating film formed on the surface of an aluminum alloy substrate.
Claims
1. An abrasive composition for magnetic disk substrates used for finish polishing of electroless nickel-phosphorus plated aluminum magnetic disk substrates, comprising: Colloidal silica, A water-soluble polymer compound, A quaternary ammonium salt type organic compound; Water and Contains The water-soluble polymer compound is The copolymer contains at least a monomer having a carboxylic acid group and a monomer having a sulfonic acid group as essential monomers, The quaternary ammonium salt type organic compound is An abrasive composition for magnetic disk substrates, wherein four hydrocarbon groups bonded to a nitrogen atom are saturated aliphatic hydrocarbon groups having 1 to 20 carbon atoms and / or unsaturated aliphatic hydrocarbon groups having 2 to 20 carbon atoms.
2. The quaternary ammonium salt type organic compound is 2. The abrasive composition for magnetic disk substrates according to claim 1, wherein the four hydrocarbon groups bonded to the nitrogen atom are saturated aliphatic hydrocarbon groups having 1 to 10 carbon atoms and / or unsaturated aliphatic hydrocarbon groups having 2 to 20 carbon atoms.
3. The quaternary ammonium salt type organic compound is 3. The abrasive composition for magnetic disk substrates according to claim 2, which is at least one selected from the group consisting of vinyltrimethylammonium chloride, allyltrimethylammonium chloride, divinyldimethylammonium chloride, diallyldimethylammonium chloride, diallyldimethylammonium fluoride, diallyldimethylammonium bromide, diallyldimethylammonium iodide, diallyldiethylammonium chloride, tetraallylammonium chloride, diethyldimethylammonium chloride, triethylmethylammonium chloride, tetraethylammonium chloride, dibutyldimethylammonium chloride, tetrabutylammonium chloride, dioctyldimethylammonium chloride, didecyldimethylammonium chloride, octyltrimethylammonium chloride, and decyltrimethylammonium chloride.
4. The quaternary ammonium salt type organic compound is a first quaternary ammonium salt type organic compound, in which four hydrocarbon groups bonded to a nitrogen atom are saturated aliphatic hydrocarbon groups having 1 to 20 carbon atoms; a second quaternary ammonium salt type organic compound in which at least one of the four hydrocarbon groups bonded to the nitrogen atom is an unsaturated aliphatic hydrocarbon group having 2 to 20 carbon atoms, and the remaining hydrocarbon groups are saturated aliphatic hydrocarbon groups having 1 to 20 carbon atoms; 2. The abrasive composition for magnetic disk substrates according to claim 1, which is a mixture containing at least one of the following:
5. 2. The abrasive composition for magnetic disk substrates according to claim 1, wherein the water-soluble polymer compound further contains a copolymer having at least a monomer having a carboxylic acid group and a monomer having an amide group as essential monomers.
6. Further comprising an acid and / or a salt thereof, 2. The abrasive composition for magnetic disk substrates according to claim 1, which has a pH value (25° C.) in the range of 0.1 to 4.
0.
7. 2. The abrasive composition for magnetic disk substrates according to claim 1, further comprising an oxidizing agent.
Citation Information
Patent Citations
Grinding liquid composition
JP2003041239A
Polishing agent composition for magnetic disk substrate
JP2019016417A
Polishing liquid composition
JP2009120850A
Polishing liquid composition for magnetic disk substrate
JP2009172709A
Polishing liquid composition for magnetic disk substrate
JP2010170650A