Chromic composition

A titania nanoparticle and silver nanostructure composition for antimicrobial coatings changes color under high UV intensity and reverts to transparent, addressing visibility and design preservation issues in conventional chromic compounds.

JP2024136029APending Publication Date: 2024-10-04OSAKA GAS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023046981
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Conventional chromic compounds used for antimicrobial coatings are difficult to visually confirm after application and often impair the design due to low transparency and lack of color change under typical indoor UV conditions.

Method used

A composition comprising titania nanoparticles with acyloxy groups bonded to titanium atoms and silver nanostructures, which changes color under high-intensity UV irradiation and returns to transparent state, maintaining design integrity.

Benefits of technology

The composition provides transparent antimicrobial coatings that visibly confirm coating presence under high UV intensity and revert to transparent state, preserving design quality.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a transparent antimicrobial composition that allows for reversible checking of a coating film through irradiation with high-intensity UV rays and the like.SOLUTION: A composition includes titania nanoparticles and silver nano-structures.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a chromic composition. [Background technology]

[0002] Infectious diseases caused by microorganisms such as the new coronavirus and multidrug-resistant bacteria not only threaten human lives but also have a major impact on social activities, making countermeasures against them an urgent task.

[0003] In recent years, a method has been developed to suppress the increase in the number of microorganisms on the surface of an object by forming a long-lasting antimicrobial coating on the surface of the object. Antimicrobial coatings are being introduced not only to frequently touched surfaces such as doorknobs and touch panels, but also to interior items in homes and offices such as wallpaper, floors, and desks.

[0004] Thus, the materials used in antibacterial and antiviral processing (antibacterial and antiviral agents) include inorganic materials such as silver and copper, organic materials such as quaternary ammonium salts, and photocatalyst materials such as titanium oxide and tungsten oxide. It is important that these antibacterial and antiviral agents do not impair the design of the object being processed, and highly transparent antibacterial and antiviral agents have been developed.

[0005] Conventionally, however, these highly transparent antibacterial and antiviral agents have been difficult to visually check after processing, and once applied, it has been difficult to check whether the coating film remains.

[0006] Conventionally, chromic compounds have been known that are reversibly colored by combining a metal component with a photocatalyst such as titanium oxide and irradiating it with ultraviolet light, visible light, etc. Patent Document 1 describes a method in which silver ions are adsorbed onto a substrate coated with titanium oxide, and then ultraviolet light is irradiated to form silver fine particles on the titanium oxide, and the resulting silver fine particles are colored at a wavelength of 1 mW / cm. 2Patent Document 2 discloses a titanium oxide-based compound that is chromic when titanium oxide, sodium oxide, and metal compounds such as iron are mixed and baked, and the resulting mixture is colored brown with ultraviolet light of about 2 mW / cm. 2 This paper discloses a technology for coloring a material by irradiating it with ultraviolet light for one hour.

[0007] Conventionally, however, these chromic compounds use white powder of titanium oxide, which has problems in that it is low in transparency due to the sintering process, and that it becomes colored even when the intensity of ultraviolet light, visible light, etc. is weak, which impairs the design when used as a coating film in a general environment.

[0008] It is desirable for antibacterial and antiviral agents to be transparent and for the coating to be reversibly visible when exposed to high-intensity ultraviolet light (chromic materials, in which the color (optical properties) of a substance reversibly changes in response to external stimuli). [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Patent No. 4126691 [Patent Document 2] Patent No. 3213996 Summary of the Invention [Problem to be solved by the invention]

[0010] An object of the present invention is to provide an antibacterial composition which is transparent and enables the coating film to be reversibly confirmed by irradiation with high-intensity ultraviolet light or the like. [Means for solving the problem]

[0011] The present invention encompasses the following compositions comprising titania nanoparticles and silver nanostructures.

[0012] Section 1. A composition comprising titania nanoparticles and silver nanostructures, The titania nanoparticles have acyloxy groups bonded to at least some of the titanium atoms present on the surface, and when the titania nanoparticles are heated to 600°C using a thermogravimetric and differential thermal analyzer, the mass loss at 200°C or higher is 5% by mass or more; The silver nanostructure has an aspect ratio of 1 to 100.

[0013] Section 2. 2. The composition according to item 1, wherein the acyloxy group is a group represented by -OCOR (wherein R represents a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a hydroxyalkyl group having 1 to 2 carbon atoms).

[0014] Section 3. 3. The composition according to item 2, wherein the acyloxy group is derived from at least one organic acid selected from the group consisting of monocarboxylic acids having 1 to 4 carbon atoms and hydroxycarboxylic acids having 2 to 3 carbon atoms.

[0015] Section 4. 4. The composition according to item 3, wherein the organic acid is at least one organic acid selected from the group consisting of lactic acid and acetic acid.

[0016] Section 5. 5. The composition according to claim 4, wherein the organic acid is acetic acid.

[0017] Section 6. 2. The composition according to item 1, wherein the titania nanoparticles have a particle diameter of 1 nm to 50 nm.

[0018] Section 7. The specific surface area of ​​the titania nanoparticles is 150 m 2 / g~500m 2 3. The composition according to claim 1, wherein the weight of the composition is 1000 g / g.

[0019] Section 8. Item 2. The composition according to item 1, wherein the titania nanoparticles do not contain any crystal form other than anatase type.

[0020] Section 9. 2. The composition according to item 1, wherein the silver nanostructure is contained in an amount of 0.1% by mass to 25% by mass relative to the titania nanoparticles.

[0021] Section 10. 2. The composition according to item 1, wherein the silver nanostructure has a minor axis length of 1 nm to 100 nm.

[0022] Section 11. 11. A laminate comprising the composition according to any one of items 1 to 10.

[0023] Section 12. A coating film comprising the composition according to any one of items 1 to 10. Effect of the Invention

[0024] The present invention is transparent and does not discolor due to the ultraviolet light intensity of sunlight present in a typical indoor environment, and when irradiated with light intensity exceeding the ultraviolet light intensity, the coating film changes color, making it possible to confirm the color.

[0025] The present invention makes it possible to provide a composition whose color fades after a certain period of time and becomes transparent again, thereby preventing the design from being impaired. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] The present invention will be described in detail below.

[0027] The embodiments of the present invention are intended to provide a better understanding of the gist of the invention, and unless otherwise specified, do not limit the content of the invention.

[0028] In this specification, the terms "comprise" and "containing" are concepts which encompass all of "comprise," "consist essentially of," and "consist only of."

[0029] In this specification, when a numerical range is indicated as "A to B," it means "A or more and B or less."

[0030] In this specification, the designations parts, % etc. are generally used.

[0031] In this specification, unless otherwise specified, all parts by mass or % by mass (wt%) are used.

[0032] [1] A composition comprising titania nanoparticles and silver nanostructures The composition of the present invention comprising titania nanoparticles and silver nanostructures is The titania nanoparticles have acyloxy groups bonded to at least some of the titanium atoms present on the surface, and when the titania nanoparticles are heated to 600°C using a thermogravimetric and differential thermal analyzer, the mass loss at 200°C or higher is 5% by mass or more; The silver nanostructure has an aspect ratio of 1-100.

[0033] In the composition of the present invention, the acyloxy group is preferably a group represented by -OCOR (wherein R represents a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a hydroxyalkyl group having 1 to 2 carbon atoms).

[0034] In the composition of the present invention, the acyloxy group is preferably an acyloxy group derived from at least one organic acid selected from the group consisting of monocarboxylic acids having 1 to 4 carbon atoms and hydroxycarboxylic acids having 2 to 3 carbon atoms.

[0035] In the composition of the present invention, the organic acid is preferably at least one organic acid selected from the group consisting of lactic acid and acetic acid.

[0036] In the compositions of the present invention, the organic acid is preferably acetic acid.

[0037] In the composition of the present invention, the particle size of the titania nanoparticles is preferably from 1 nm to 50 nm.

[0038] In the composition of the present invention, the titania nanoparticles preferably have a specific surface area of ​​150 m 2 / g~500m2 / g.

[0039] In the compositions of the present invention, the titania nanoparticles are preferably free of crystalline forms other than anatase.

[0040] In the composition of the present invention, the silver nanostructure is preferably contained in a proportion of 0.1% by mass to 25% by mass relative to the titania nanoparticles.

[0041] In the composition of the present invention, the minor axis length of the silver nanostructure is preferably from 1 nm to 100 nm.

[0042] The present invention includes a laminate comprising the composition of the present invention.

[0043] The present invention includes a coating film comprising the composition of the present invention.

[0044] The composition of the present invention is transparent and does not discolor due to the ultraviolet light intensity of sunlight present in a typical indoor environment. When irradiated with light intensity exceeding the ultraviolet light intensity, the coating film changes color, which can be confirmed.

[0045] The composition of the present invention fades in color after a certain period of time and becomes transparent again, making it possible to provide a composition that does not impair the design properties.

[0046] [1-1] Silver-loaded titania nanoparticles and photocatalysts The silver-loaded titania nanoparticles are titania nanoparticles in which silver (silver nanostructure) is loaded on the surface of the titania nanoparticles.

[0047] The titania nanoparticles have acyloxy groups bonded to at least some of the titanium atoms present on the surface, and when the titania nanoparticles are heated to 600°C using a thermogravimetric and differential thermal analyzer, the mass loss at temperatures above 200°C is 5% by mass or more.

[0048] The titania nanoparticles preferably have silver supported on the surface thereof.

[0049] The average particle size and specific surface area of ​​the silver-loaded titania nanoparticles can be adjusted.

[0050] In the silver-loaded titania nanoparticles, the silver is in the form of a silver nanostructure, and it is possible to adjust the average particle size and specific surface area of ​​the silver nanostructure.

[0051] In the silver-loaded titania nanoparticles, the titania nanoparticles and silver are tightly adhered to each other, and the silver component is highly dispersible and does not easily aggregate. Therefore, without the use of additional additives such as dispersants or stabilizers, the silver component is stably dispersed, and the silver component has excellent heat resistance, resistance to discoloration when exposed to ultraviolet rays, coatability, and transparency.

[0052] The silver-loaded titania nanoparticles and photocatalyst have sufficient coatability and transparency without the need for additional dispersants and stabilizers, so their visible light catalytic activity and dark-place antibacterial and antiviral activity are not impaired by additives such as binders and dispersants.

[0053] The silver-supported titania nanoparticles and photocatalyst have high resistance to physical impacts such as abrasion, and therefore can maintain excellent visible light catalytic activity.

[0054] Silver-loaded titania nanoparticles are useful as photocatalysts (particularly visible light-responsive photocatalysts) and as coating materials for photocatalysts.

[0055] Silver-loaded titania nanoparticles can have antimicrobial activity in the light due to their photocatalytic activity.

[0056] Silver-loaded titania nanoparticles can have antimicrobial activity in the dark due to the presence of silver on the surface.

[0057] [1-2] Titania nanoparticles Water, inorganic acids, free organic acids, etc. generally evaporate at temperatures below 200°C.

[0058] In the titania nanoparticles constituting the metal-supported titania nanoparticles of the present invention, acyloxy groups are bonded to at least some of the titanium atoms present on the surface, and these groups are gradually eliminated in the range of 200° C. to 600° C. For example, in the case of acetoxy groups, they are gradually eliminated in the range of 200° C. to 600° C., reaching a peak at about 260° C.

[0059] The titania nanoparticles constituting the metal-supported titania nanoparticles of the present invention have acyloxy groups bonded to at least some of the titanium atoms present on the surface, which can suppress aggregation of the titania nanoparticles during drying or firing, making them less susceptible to cracking, peeling, etc., and they are particularly excellent in terms of coatability and transparency.

[0060] The titania nanoparticles constituting the metal-supported titania nanoparticles of the present invention can suppress cracking, peeling, and the like, and can easily support metals firmly, resulting in excellent visible light catalytic activity.

[0061] Titania nanoparticles generally have reduced visible light catalytic activity when they have acyloxy groups on their surfaces.

[0062] The titania nanoparticles constituting the metal-supported titania nanoparticles of the present invention can suppress aggregation of the titania nanoparticles during drying or firing, and therefore have a particularly excellent effect of suppressing cracks, peeling, and the like.

[0063] The titania nanoparticles constituting the metal-supported titania nanoparticles of the present invention can easily support metals firmly, and therefore can improve the visible light catalytic activity even though they have an acyloxy group.

[0064] Titania nanoparticles preferably have a large amount of acyloxy groups bonded to titanium atoms present on the surface. When acyloxy groups are present on at least some of the titanium atoms present on the surface, they are gradually released in the range of 200°C to 600°C, and therefore, when heated using a thermogravimetric and differential thermal analyzer (TG-DTA), there is a large mass loss at 200°C or higher.

[0065] When titania nanoparticles are heated using a thermogravimetric and differential thermal analyzer (TG-DTA), the mass loss at temperatures above 200°C is an indicator of the number of acetoxy groups bonded to titanium atoms on the surface.

[0066] When titania nanoparticles are heated up to 600° C. using a thermogravimetry-differential thermal analyzer (TG-DTA), the mass loss at 200° C. or higher is 5% by mass or more, preferably 7% by mass to 20% by mass.

[0067] The detailed conditions for the thermogravimetry-differential thermal analyzer (TG-DTA) were as follows: atmosphere: air, heating rate: 3° C. / min.

[0068] Titania nanoparticles have acyloxy groups bonded to at least some of the titanium atoms present on the surface. The acyloxy groups are preferably groups represented by -OCOR (wherein R represents a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a hydroxyalkyl group having 1 to 2 carbon atoms) and bonded to the titanium atoms. The acyloxy groups are preferably acyloxy groups derived from organic acids such as monocarboxylic acids having 1 to 4 carbon atoms and hydroxycarboxylic acids having 2 to 3 carbon atoms.

[0069] In -OCOR, the alkyl group of R is preferably a methyl group, an ethyl group, an n-propyl group, etc. In -OCOR, the monocarboxylic acid is preferably formic acid, acetic acid, propionic acid, butyric acid, etc.

[0070] In -OCOR, the hydroxyalkyl group of R is preferably a hydroxymethyl group, a 1-hydroxyethyl group, a 2-hydroxyethyl group, etc. In -OCOR, the hydroxycarboxylic acid is preferably glycolic acid, lactic acid, etc.

[0071] In -OCOR, from the viewpoints of volatility, toxicity, and decomposability, R is preferably a hydrogen atom, or a methyl group, a hydroxymethyl group, a 1-hydroxyethyl group, a 2-hydroxyethyl group, or the like.

[0072] In -OCOR, from the viewpoints of water solubility and odor, R is preferably a methyl group, a 1-hydroxyethyl group, a 2-hydroxyethyl group, or the like.

[0073] From the viewpoints of volatility, toxicity and decomposability, -OCOR is preferably a monocarboxylic acid such as formic acid or acetic acid.

[0074] From the viewpoints of volatility, toxicity and decomposability, -OCOR is preferably a hydroxycarboxylic acid such as glycolic acid or lactic acid.

[0075] From the viewpoints of water solubility and odor, particularly preferred -OCORs are acetic acid, glycolic acid, lactic acid, and the like.

[0076] The organic acid may be at least one compound selected from the group consisting of the above organic acids. These organic acids may be used alone or in combination (blend) of two or more depending on the purpose.

[0077] The average particle size of the titania nanoparticles is preferably 1 nm to 50 nm, more preferably 1 nm to 5 nm, and even more preferably 2 nm to 4 nm. By adjusting the average particle size of the titania nanoparticles to this range, the metals (silver and copper) can be supported on the titania nanoparticles appropriately and more firmly. The titania nanoparticles can form a film with higher visible light catalytic activity and higher transparency.

[0078] When the average particle size of titania nanoparticles is small, they generally shrink significantly when heated, and are therefore prone to cracking and peeling off from the substrate.

[0079] The metal-supported titania nanoparticles of the present invention are a material that has excellent coatability even when titania nanoparticles having a small average particle size are used.

[0080] The average particle size of the titania nanoparticles is measured by observation with a transmission electron microscope (TEM).

[0081] The specific surface area of ​​the titania nanoparticles is preferably 150 m 2 / g~500m 2 / g, more preferably 200m 2 / g~400m 2 / g. By adjusting the specific surface area of ​​the titania nanoparticles to this range, metals (silver and copper) can be supported on the titania nanoparticles appropriately and more firmly. Titania nanoparticles have high visible light catalytic activity.

[0082] The specific surface area of ​​the titania nanoparticles is measured by the BET method.

[0083] The titania nanoparticles can have the concentrations of N, Cl, and S elements each preferably in the range of 0 to 5,000 ppm, more preferably 0 to 1,000 ppm. By adjusting the concentrations of N, Cl, and S elements in the titania nanoparticles to within this range, corrosion of the substrate can be suppressed. The concentrations of N, Cl, and S elements in the titania nanoparticles mean that there is no impurity derived from the acidic titania precursor such as TiCl4 or TiOSO4, or there are only a very small amount of such impurities.

[0084] The concentrations of N, Cl, and S elements in the titania nanoparticles are measured by WDX (fluorescent X-ray).

[0085] The crystalline form of the titania nanoparticles is preferably anatase type, and the titania nanoparticles preferably do not contain any crystalline form other than anatase type. By adopting anatase type, the titania nanoparticles have improved visible light catalytic activity. The titania nanoparticles preferably do not contain any crystalline form other than anatase type, and are 100% anatase type.

[0086] [1-3] Silver nanostructures The form of the silver nanostructure is not particularly limited, and from the viewpoints of silver stability, antibacterial activity in light and dark places (particularly in dark places), and antiviral activity, it is preferable to use silver nanoparticles, silver nanorods, silver nanowires, etc.

[0087] When metal ions or metal nanoparticles are added to titanium oxide, generally, regardless of the specific surface area of ​​the titanium oxide or the metal ion concentration, the metal ions are reduced over time to produce metal nanoparticles, and the metal nanoparticles thermally agglomerate over time, often resulting in metal precipitation.

[0088] The titania nanoparticles constituting the metal-supported titania nanoparticles of the present invention have acyloxy groups bonded to at least some of the titanium atoms present on the surface, and the metal ions and metal nanoparticles are stabilized on the titania nanoparticles, thereby suppressing discoloration due to reduction over time, thermal aggregation, and aggregation upon exposure to ultraviolet light.

[0089] The average short axis length of the silver nanostructures is preferably 500 nm or less, more preferably 0.01 nm to 200 nm, even more preferably 0.1 nm to 100 nm, and particularly preferably 1 nm to 100 nm. By adjusting the average particle size of the supported silver nanostructures to fall within this range, a dispersion with high dispersion stability can be obtained, and a film with improved visible light catalytic activity and improved transparency can be formed.

[0090] The average minor axis length of the silver nanostructures is measured by observation using an electron microscope.

[0091] The amount of silver supported on the surface of titania nanoparticles is preferably less than 50% by mass, more preferably 0.01% to 40% by mass, and even more preferably 0.1% to 25% by mass, based on the titanium oxide in the titania nanoparticles, from the viewpoints of antimicrobial activity (antibacterial activity and antiviral activity), stability of the titania nanoparticles, etc. By adjusting the amount of silver supported on the surface of titania nanoparticles to fall within this range, the strength and transparency of the coating film containing the titania nanoparticles can be maintained.

[0092] The aspect ratio of the silver nanostructure (long axis length of silver nanostructure / short axis length of silver nanostructure) is preferably 500 or less, more preferably 1 to 200, even more preferably 1 to 100, and particularly preferably 1.1 to 100. By adjusting the aspect ratio of the silver nanostructure within this range, the titania nanoparticles can be made visible in the discoloration caused by irradiation with strong ultraviolet light, and can be made to re-transparent after the irradiation is stopped.

[0093] The average minor axis length and the average major axis length of the silver nanostructures are measured by observation using an electron microscope.

[0094] [2] Method for manufacturing silver nanostructure-supported titania nanoparticles and photocatalyst In the present invention, the method of supporting the silver nanostructure on the titania nanoparticles is preferably a photoprecipitation method in which the metal nanostructure and / or the silver complex are mixed with the titania nanoparticles and then the mixture is supported by light irradiation. The method of supporting the silver nanostructure on the titania nanoparticles is preferably a method in which the silver nanostructure synthesized by any method is brought into contact with the titania nanoparticles, mixed or allowed to stand, and supported.

[0095] In the present invention, any method can be adopted for supporting the silver nanostructure on the titania nanoparticles.

[0096] The metal-supported titania nanoparticles and the photocatalyst are preferably (A) a step of mixing a titanium-containing substance, an organic acid, and water to obtain a dispersion; (B) heating the dispersion obtained in step (A) at a temperature higher than 80° C. for at least 1 hour; Process (C): (C1) a step of chemically reducing the dispersion obtained by mixing the dispersion obtained in the step (B) with a silver nanostructure and / or a silver compound; (C2) A step of irradiating ultraviolet light onto the dispersion obtained by mixing the dispersion obtained in the step (B) with a silver nanostructure and / or a silver compound; (C3) mixing the dispersion obtained in the step (B) with a silver nanostructure; or (C4) A step of adding a silver nanostructure and / or a silver compound to the dispersion liquid obtained in the step (B) and allowing the dispersion liquid to stand. The method comprises the steps of:

[0097] In the step (C), steps (C1) and (C2) can improve the loading efficiency by applying energy from the outside.

[0098] In the step (C), the step (C3) can prevent the titania nanoparticle dispersion from becoming too viscous, and can obtain uniform particles.

[0099] In any of steps (C1), (C2), (C3), and (C4) of step (C), the controllability of the aspect ratio of the silver nanostructure can be further improved by cooling.

[0100] [2-1] Process (A) In step (A), a titanium-containing substance, an organic acid, and water are mixed to obtain a dispersion.

[0101] The titanium-containing substance used is preferably a substance that becomes titanium oxide when heated. The titanium-containing substance is preferably titanium oxide and / or a titanium oxide precursor, and more preferably titanium oxide; titanium hydroxide; titanium alkoxide; titanium halide such as titanium trichloride or titanium tetrachloride (particularly, one neutralized with a base); metallic titanium, etc.

[0102] From the viewpoints of dispersibility, coatability, and visible light catalysis of the resulting titania, the titanium-containing substance is preferably titanium alkoxide, titanium hydroxide, or titanium halide (particularly, one neutralized with a base). From the viewpoints of purity, dispersibility, coatability, transparency, and visible light catalysis, the titanium-containing substance is more preferably titanium alkoxide.

[0103] The titanium alkoxide is preferably titanium tetraisopropoxide, titanium tetra n-butoxide, titanium tetra n-propoxide, titanium tetraethoxide, etc. From the viewpoints of cost, water solubility of by-products, coatability, and visible light catalytic property, the titanium alkoxide is more preferably titanium tetraisopropoxide.

[0104] The titanium-containing substance may be at least one compound selected from the group consisting of the titanium-containing substances described above. These titanium-containing substances may be used alone or in combination (blend) of two or more types depending on the purpose.

[0105] Depending on the combination of titanium alkoxide and organic acid, the titania obtained may be used as a catalyst to liberate ester compounds that are difficult to dissolve in water. There is no problem with titania itself. For example, in the combination of titanium tetra n-butoxide and acetic acid, butyl acetate is generated and liberated at the stage of mixing and heating, but from the viewpoint of obtaining a uniform dispersion, it is preferable to adopt a combination of organic acid and titanium alkoxide that can obtain an organic acid alkoxide with excellent water solubility.

[0106] Titanium halides (titanium tetrachloride, titanium trichloride, etc.) are preferably neutralized with a base and the precipitate is washed from the viewpoints of impurities (halogens), corrosion of the reactor during mass production, crystallinity control, coating properties, transparency, and visible light catalysis. Titanium halides are preferably used without drying from the viewpoint of dispersibility of the obtained titania.

[0107] When a solid such as titanium oxide or metallic titanium is used as the titanium-containing substance, the average particle size is preferably 100 nm or less, more preferably 50 nm or less. There is no particular lower limit for the average particle size of the titanium-containing substance, and it is preferably about 1 nm.

[0108] When the particle size is large, it is preferable to use a planetary ball mill, a paint shaker or the like for dry or wet pulverization.

[0109] The average particle size of solids such as titanium oxide and titanium metal is measured by observation using a transmission electron microscope (TEM).

[0110] The concentration of the titanium-containing substance in the dispersion produced in step (A) is preferably 0.01 mol / L to 5 mol / L, and more preferably 0.05 mol / L to 3 mol / L, from the viewpoints of productivity, viscosity of the reaction liquid, coatability, transparency, and visible light catalytic properties.

[0111] The acid used in the reaction is an organic acid, and since it is preferably a volatile acid, it is preferably an acid represented by the chemical formula C n H 2n+1 Monocarboxylic acids represented by COOH (n=0 to 3) (monocarboxylic acids having 1 to 4 carbon atoms), hydroxycarboxylic acids having 2 to 3 carbon atoms, etc. are used.

[0112] The monocarboxylic acid is preferably formic acid (n=0) or acetic acid (n=1) from the viewpoints of volatility, toxicity and decomposability.

[0113] The hydroxycarboxylic acid is preferably glycolic acid, lactic acid, etc., and from the viewpoints of water solubility and odor, more preferably acetic acid, glycolic acid, lactic acid, etc.

[0114] The organic acid may be at least one compound selected from the group consisting of the above organic acids. These organic acids may be used alone or in combination (blend) of two or more depending on the purpose.

[0115] The amount of organic acid used is adjusted so that the number of moles of acyloxy groups is preferably 1.5 moles or more, particularly preferably 2 moles or more, per mole of titanium in the titanium-containing substance, from the viewpoints of dispersibility, coatability, transparency, and cost. The more organic acid is used, the more the stability over time, coatability, transparency, etc. can be improved. The upper limit of the amount of organic acid used is not particularly limited, and is preferably adjusted so that the number of moles of acyloxy groups is 10 moles or less per mole of titanium in the titanium-containing substance.

[0116] The concentration of the organic acid in the dispersion obtained in step (A) is preferably 0.02 mol / L to 10 mol / L, and more preferably 0.1 mol / L to 7 mol / L, from the viewpoints of dispersibility, coatability, transparency, visible light catalytic properties, and cost.

[0117] The reaction solvent is preferably an aqueous solvent such as water, the main component being preferably 50% by mass or more. The reaction solvent may contain an alcohol or an ester during the reaction.

[0118] When titanium tetraisopropoxide is used as a raw material, the reaction solvent reacts with an organic acid to produce isopropyl alcohol. Heating may produce an isopropyl ester of the organic acid. The alcohol or ester may be added to the dispersion obtained by step (A), or may be generated in the system. The alcohol or ester may be removed by heating in an open system at 100°C or less, or may be removed by reducing pressure, or may remain in the reaction liquid.

[0119] When alcohol is contained in the dispersion, the average particle size of the obtained titania nanoparticles and metal-supported titania nanoparticles tends to become small, and therefore alcohol may be intentionally added in order to control the average particle size.

[0120] In general, inorganic acids (especially strong inorganic acids) such as nitric acid, hydrochloric acid, and sulfuric acid are often used in the hydrothermal synthesis reaction of titania nanoparticles. Not only do the crystal forms of the resulting titania nanoparticles contain a mixture of anatase and brookite types, but it is preferable not to use them in principle from the viewpoints of the storage stability of the resulting dispersion, corrosion of the equipment, impurities, wastewater, etc.

[0121] Inorganic acids can be used supplementarily in the range of, for example, 0.01 mol / L or less, to enhance the dispersibility, transparency, uniformity, etc. of the raw material and to facilitate handling, without impairing the effect. The concentrations of N, Cl, and S elements in the dispersion obtained in step (A) are all 0.01 mol / L or less.

[0122] The pH of the dispersion obtained in step (A) is preferably 2 or more and less than 6, and more preferably 2.1 to 5, from the viewpoints of equipment corrosion, handling safety, dispersibility, and the like.

[0123] In step (A), the method of preparing the dispersion is not particularly limited, and the titanium-containing substance, the organic acid, and water (solvent) may be mixed simultaneously or sequentially. On a mass production scale, from the viewpoint of preventing aggregation and forming large lumps and facilitating continued stirring, it is preferable to mix the organic acid and water (solvent) and then add the titanium-containing substance while stirring. On a laboratory scale, it is preferable to mix the titanium-containing substance and the organic acid and then add water while stirring.

[0124] [2-2] Process (B) In step (B), the dispersion obtained in step (A) is heated at a temperature higher than 80° C. for 1 hour or more.

[0125] Step (B) is preferably carried out under normal pressure, or under pressure in a closed vessel. Step (B) is preferably carried out under normal pressure from the viewpoint of reducing the average particle size of the titania nanoparticles and the titania nanoparticles carrying metal nanoparticles. Step (B) is preferably carried out under conditions of 0.09 MPa to 0.11 MPa. When step (B) is carried out under pressure, the reaction is preferably carried out for a short time (about 5 minutes to 30 minutes) at 0.2 MPa or less (0.11 MPa to 0.2 MPa) from the viewpoint of easily forming a film having high visible light catalytic activity and high transparency.

[0126] In step (B), the mixture is preferably stirred during heating in order to sufficiently react the titanium-containing substance, the organic acid, and the water. The stirring method in step (B) is not particularly limited and follows a conventional method. The stirring time in step (B) is preferably 1 hour or more, more preferably 1.5 hours or more, in order to sufficiently react the titanium-containing substance, the organic acid, and the water. The upper limit of the stirring time in step (B) is not particularly limited and is preferably 240 hours.

[0127] The heating temperature in step (B) is preferably higher than 80° C., more preferably at least 82° C. If the heating temperature in step (B) is lower than 80° C., cracks are likely to occur, the coating properties are poor, and the coating falls off easily, making it difficult to form a coating film. The upper limit of the heating temperature in step (B) is not particularly limited, and is preferably 120° C. when the reaction is carried out at normal pressure.

[0128] The pH of the dispersion obtained in step (B) is preferably 2 or more and less than 6, and more preferably 2.1 to 5, from the viewpoints of equipment corrosion, handling safety, dispersibility, and the like.

[0129] [2-3] Process (C1) In step (C1), the dispersion obtained by mixing the dispersion obtained in step (B) with a silver nanostructure and / or a silver compound is subjected to a chemical reduction treatment.

[0130] When using a silver nanostructure as silver, the silver nanostructure may be a publicly known or commercially available product. When synthesizing a silver nanostructure, for example, it may be synthesized based on the method described in Silver Nanoparticles, Journal of the Adhesion Society of Japan, Vol. 44, No. 11, 2008, pp. 414-419.

[0131] The average minor axis diameter of the silver nanostructure is not particularly limited, and from the viewpoints of antibacterial and antiviral activity and dispersion stability of the nanoparticles, it is preferably 0.01 nm to 500 nm, and more preferably 0.1 nm to 100 nm.

[0132] When a silver salt is used as the silver compound, since the dispersion (sol) containing titania nanoparticles obtained in steps (A) and (B) is acidic, it is preferable to avoid the dispersion after step (C1) becoming basic. The silver salt is preferably a silver salt whose aqueous solution is acidic or neutral. The silver salt is preferably silver chloride (I), silver nitrate (I), organic acid silver (silver lactate (I), silver acetate (I), silver citrate (I), silver myristate (I), etc.), silver sulfide (I), silver oxide (I), silver phosphate (I), silver carbonate (I), silver bromide (I), silver iodide (I), etc. It is also possible to use the silver salt as a silver nanostructure precursor that becomes a silver nanostructure by reduction.

[0133] The silver nanostructure and silver salt may be at least one compound selected from the group consisting of the above-mentioned silver nanostructures and silver salts, and these silver nanostructures and silver salts may be used alone or in combination (blended) of two or more types depending on the purpose.

[0134] In step (C1), the amount of the silver nanostructure and / or silver compound used is, in terms of the mass of the silver element in the silver nanostructure and / or silver compound, preferably 50% by mass or less, more preferably 0.01% by mass to 40% by mass, and even more preferably 0.1% by mass to 25% by mass, relative to the titanium oxide in the titania nanoparticles contained in the dispersion liquid obtained in step (B), from the viewpoints of dispersibility, transparency, antimicrobial activity (antibacterial activity and antiviral activity), stability of the titania nanoparticles, etc. By adjusting the amount of the silver nanostructure and / or silver compound used within this range, it is easy to maintain the coatability and transparency, and the antibacterial activity, antiviral activity, and photocatalytic activity in the dark can be particularly improved.

[0135] In step (C1), the chemical reduction process is not particularly limited, and preferably, a method using a reducing agent such as sodium borohydride, a polyol reduction method, an ethanol reduction method, etc. When a reducing agent is used, the process is preferably carried out at a temperature of 0° C. or higher and lower than 20° C. (room temperature) from the viewpoints of dispersion stability, controllability of the aspect ratio, discoloration resistance when irradiated with low-intensity ultraviolet light, visibility when irradiated with high-intensity ultraviolet light, and re-transparency in an ultraviolet light-stopped environment.

[0136] Step (C1) may be carried out under an air atmosphere or an anaerobic atmosphere. The anaerobic atmosphere in step (C1) is preferably an inert gas atmosphere such as a nitrogen atmosphere or an argon atmosphere.

[0137] In the step (C1), in order to sufficiently react the dispersion obtained in the step (B) with the silver nanostructure and / or the silver compound during the chemical reduction treatment, the dispersion is preferably stirred. The stirring method is not particularly limited and may be performed according to a conventional method.

[0138] The pH of the resulting dispersion varies depending on the type of metal added and the amount of the metal added, but is preferably 1 to 5, and more preferably 2 to 4, from the viewpoint of coatability.

[0139] Thereafter, the silver nanostructure-supported titania nanoparticles can be recovered by precipitating and centrifuging the silver nanostructure-supported titania nanoparticles in a conventional manner, etc. A large amount of acyloxy groups are bonded to titanium atoms present on the surface, and titania nanoparticles with silver supported on the surface can be obtained.

[0140] [2-4] Process (C2) In the step (C2), the dispersion obtained by mixing the dispersion obtained in the step (B) with a silver nanostructure and / or a silver compound is irradiated with ultraviolet light.

[0141] When using a silver nanostructure as silver, the silver nanostructure may be a publicly known or commercially available product. When synthesizing a silver nanostructure, for example, it may be synthesized based on the method described in Silver Nanoparticles, Journal of the Adhesion Society of Japan, Vol. 44, No. 11, 2008, pp. 414-419.

[0142] The average particle size of the silver nanostructure is not particularly limited, and from the viewpoints of antibacterial and antiviral activity and dispersion stability of the nanoparticles, it is preferably 0.01 nm to 500 nm, and more preferably 0.1 nm to 100 nm.

[0143] When a silver salt is used as the silver compound, since the dispersion (sol) containing titania nanoparticles obtained in steps (A) and (B) is acidic, it is preferable to avoid the dispersion after step (C2) from becoming basic. The silver salt is preferably a silver salt whose aqueous solution is acidic or neutral. The silver salt is preferably silver chloride (I), silver nitrate (I), organic acid silver (silver lactate (I), silver acetate (I), silver citrate (I), silver myristate (I), etc.), silver sulfide (I), silver oxide (I), silver phosphate (I), silver carbonate (I), silver bromide (I), silver iodide (I), etc. It is also possible to use the silver salt as a silver nanostructure precursor that becomes a silver nanostructure by reduction.

[0144] The silver nanostructure and silver salt may be at least one compound selected from the group consisting of the above-mentioned silver nanostructures and silver salts, and these silver nanostructures and silver salts may be used alone or in combination (blended) of two or more types depending on the purpose.

[0145] In step (C2), the amount of the silver nanostructure and / or silver compound used is, in terms of the mass of the silver element in the silver nanostructure and / or silver compound, preferably 50% by mass or less, more preferably 0.01% by mass to 40% by mass, and even more preferably 0.1% by mass to 25% by mass, relative to the titanium oxide in the titania nanoparticles contained in the dispersion liquid obtained in step (B), from the viewpoints of dispersibility, transparency, antimicrobial activity (antibacterial activity and antiviral activity), stability of the titania nanoparticles, etc. By adjusting the amount of the silver nanostructure and / or silver compound used within this range, it is easy to maintain the coatability and transparency, and the antibacterial activity, antiviral activity, and photocatalytic activity in the dark can be particularly improved.

[0146] In step (C2), the ultraviolet light irradiation is preferably performed below room temperature (20° C.), more preferably below 15° C., from the viewpoints of ease of supporting silver on titania nanoparticles, visible light catalytic activity, reaction rate, productivity, controllability of aspect ratio, discoloration resistance when irradiated with low-intensity ultraviolet light, visibility when irradiated with high-intensity ultraviolet light, and re-transparency in an ultraviolet light-stopped environment, etc. The lower limit of the temperature for ultraviolet light irradiation is not particularly limited, and is preferably 0° C. when the reaction is performed at normal pressure.

[0147] In step (C2), during the ultraviolet light irradiation, the dispersion obtained in step (B) is preferably stirred in order to sufficiently react with the silver nanostructure and / or the silver compound. The stirring method is not particularly limited and may be performed according to a conventional method.

[0148] Step (C2) may be carried out under an air atmosphere or an anaerobic atmosphere. The anaerobic atmosphere in step (C2) is preferably an inert gas atmosphere such as a nitrogen atmosphere or an argon atmosphere.

[0149] The pH of the resulting dispersion varies depending on the type of metal added and the amount of the metal added, but is preferably 1 to 5, and more preferably 2 to 4, from the viewpoint of coatability.

[0150] Thereafter, the silver nanostructure-supported titania nanoparticles can be recovered by precipitating and centrifuging the silver nanostructure-supported titania nanoparticles in a conventional manner, etc. A large amount of acyloxy groups are bonded to titanium atoms present on the surface, and titania nanoparticles with silver supported on the surface can be obtained.

[0151] [2-5] Steps (C3) and (C4) Instead of step (C2), step (C3) can be adopted, which is a step of mixing the dispersion liquid obtained in step (B) with a silver nanostructure and / or a silver compound.

[0152] Instead of step (C2), step (C4) can be adopted in which a silver nanostructure and / or a silver compound is added to the dispersion liquid obtained in step (B) and allowed to stand.

[0153] The silver nanostructure and silver compound used are the same as those used in step (C1).

[0154] The amounts of the silver nanostructure and the silver compound used are the same as in step (C1).

[0155] In step (C3), the method of mixing the dispersion obtained in step (B) with the silver nanostructure and / or silver compound is not particularly limited and follows a conventional method. In step (C3), the silver nanostructure and / or silver compound is added to the dispersion obtained in step (B) and stirred. The stirring method is not particularly limited and follows a conventional method.

[0156] In step (C3), the ultraviolet light irradiation is preferably performed below room temperature (20° C.), more preferably below 15° C., from the viewpoints of ease of supporting silver on titania nanoparticles, visible light catalytic activity, reaction rate, productivity, controllability of aspect ratio, discoloration resistance when irradiated with low-intensity ultraviolet light, visibility when irradiated with high-intensity ultraviolet light, and re-transparency in an ultraviolet light-stopped environment, etc. The lower limit of the temperature for ultraviolet light irradiation is not particularly limited, and is preferably 0° C. when the reaction is performed at normal pressure.

[0157] Steps (C3) and (C4) may be carried out in an air atmosphere or an anaerobic atmosphere. The anaerobic atmosphere in steps (C3) and (C4) is preferably an inert gas atmosphere such as a nitrogen atmosphere or an argon atmosphere.

[0158] The pH of the resulting dispersion varies depending on the type of metal added and the amount of the metal added, but is preferably 1 to 5, and more preferably 2 to 4, from the viewpoint of coatability.

[0159] Thereafter, the silver nanostructure-supported titania nanoparticles can be recovered by precipitating and centrifuging the silver nanostructure-supported titania nanoparticles in a conventional manner, etc. A large amount of acyloxy groups are bonded to titanium atoms present on the surface, and titania nanoparticles with silver supported on the surface can be obtained.

[0160] [3] Titania nanoparticle dispersion supporting metal nanoparticles The metal-loaded titania nanoparticle dispersion of the present invention (particularly, photocatalyst dispersion, further, visible light responsive photocatalyst dispersion) uses a reaction liquid that has undergone step (A), step (B), step (C1), step (C2), step (C3), or step (C4), and, if necessary, a dispersion step such as ultrasonic dispersion is added to make the dispersion even more uniform.

[0161] In conventional visible light responsive photocatalyst dispersions, it was impossible to obtain a uniform dispersion unless a dispersing agent was used.

[0162] A dispersant may be added to the metal-supported titania nanoparticle dispersion of the present invention.

[0163] The dispersion of metal-supported titania nanoparticles of the present invention is a dispersion having far better dispersibility than ordinary visible light responsive photocatalysts, even without the addition of a dispersant.

[0164] The metal-supported titania nanoparticle dispersion of the present invention has good dispersibility, and therefore has excellent crack resistance of the coating. The metal-supported titania nanoparticle dispersion of the present invention does not require the addition of a dispersant, and therefore enables dense titania coating, and has excellent coatability and transparency, as well as excellent visible light catalytic activity.

[0165] In the metal-supported titania nanoparticle dispersion, the total amount of the metal-supported titania nanoparticle dispersion is taken as 100 mass%, and the content of water, which is the main solvent, is preferably 50 mass% or more, and more preferably 60 mass% or more, from the viewpoints of ease of coating, film properties of the coating, etc.

[0166] It is also possible to take out the metal-supported titania nanoparticles of the present invention from the reaction solution and change the solvent. Water may be removed from the reaction solution by centrifugation, a filtration membrane, etc., and replaced with an organic solvent. It is preferable not to dry the metal-supported titania nanoparticles from the viewpoint of dispersibility, transparency, etc.

[0167] The organic solvent used in the dispersion liquid is preferably alcohol, etc. The alcohol is preferably an aliphatic alcohol having 1 to 6 carbon atoms, such as methanol, ethanol, propanol, isopropanol, etc., a non-aliphatic alcohol, such as α-terpineol, etc., a glycol-based solvent, such as butyl carbitol (diethylene glycol monobutyl ether), hexylene glycol (2-methyl-2,4-pentanediol), ethylene glycol-2-ethylhexyl ether, ethylene glycol monomethyl ether, propylene glycol monomethyl ether, etc., or a diol, such as 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, etc.

[0168] The organic solvent used in the dispersion liquid is preferably an organic solvent that has affinity with titania and other solvents (water, alcohol, etc.) even if it does not have an OH group. The organic solvent is preferably diethylene glycol butyl methyl ether, tripropylene glycol dimethyl ether, triethylene glycol dimethyl ether, diethylene glycol dibutyl ether, triethylene glycol butyl methyl ether, tetraethylene glycol dimethyl ether, diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol diacetate, triethylene glycol diacetate, tetraethylene glycol diacetate, etc. From the viewpoint of boiling point, etc., it is more preferable to use diethylene glycol monobutyl ether acetate, tetraethylene glycol dimethyl ether, etc. as the organic solvent.

[0169] The viscosity of the metal-supported titania nanoparticle dispersion is preferably adjusted according to the application, and used as a paint. When the paint is applied by spin coating, dip coating, spraying, or the like, the viscosity is preferably adjusted to be low. When the paint is applied by brush coating, squeegee method, or the like, the viscosity is preferably adjusted to be higher. When the paint is applied by screen printing, the viscosity is preferably adjusted to be even higher to suppress flowability.

[0170] The resulting coating film allows for a dense coating.

[0171] The coated product having a coating film is not particularly limited, and examples thereof include building materials, building exteriors, building interiors, window frames, window glass, various lenses, structural members, building facilities such as housing, cooking utensils, textile products, furniture, displays, display protective films, plumbing members, vehicle lighting covers and window glass, mechanical equipment or exteriors of articles, dustproof covers and coatings, display devices, their covers, traffic signs, various display devices, display objects such as billboards, sound insulation walls for roads and railways, exteriors and coatings of bridges and guardrails, interiors and coatings of tunnels, insulators, solar cell covers, solar hot water heater heat collector covers, and other exterior parts of electronic and electrical devices used outside, particularly transparent members, exteriors of vinyl greenhouses, greenhouses, and the like. EXAMPLES

[0172] The present invention will be specifically described below with reference to examples.

[0173] The present invention is not limited to the following specific examples.

[0174] [Example 1] 25wt% silver nanostructure (aspect ratio 1.1) vs. TiO 2 142.1g (0.5mol) of titanium tetraisopropoxide was added with 30g (0.5mol) of acetic acid, stirred for 60 minutes, and then 538g of water was added. This dispersion had a titanium tetraisopropoxide concentration of 0.625mol / L, an acetic acid concentration of 0.625mol / L, and a pH of 2.2. A large amount of translucent precipitate was generated in this dispersion, but when the dispersion was stirred for 60 minutes and then heated at 70°C, all of the precipitate dissolved. In this dispersion, the concentration of inorganic acid, N, Cl, and S elements were all 0mol / L.

[0175] After that, the mixture was stirred at normal pressure (0.10 MPa) and 85°C for 3 hours, and a semi-transparent uniform titania dispersion was obtained without using an organic dispersant. When ultrasonic dispersion was applied to this dispersion, the viscosity was reduced and the transparency was increased. This dispersion had a water content of 67% by mass and a pH of 2.3.

[0176] The dispersion was dried to obtain titania nanoparticles. The BET specific surface area of ​​the titania nanoparticles was measured and found to be 250 m 2 / g. TEM observation revealed that the average particle size was about 3 nm. X-ray diffraction analysis of the crystallinity of the obtained titania nanoparticles revealed that they were 100% anatase type, with no other crystal forms present.

[0177] The dispersion was kept at 200°C using a moisture meter and dried until there was no mass loss. The TG-DTA of the titania nanoparticles was measured by heating the mixture to 600°C at a rate of 3°C / min in an air atmosphere. The mass loss above 200°C was 10% by mass. This mass loss above 200°C corresponds to the mass loss caused by the elimination of acetic acid, an organic acid. Since the liberated acetic acid almost evaporates below 200°C, the fact that the mass loss above 200°C is 10% by mass suggests that a large amount of acetyl groups, which are acyloxy groups, are bonded to titanium atoms in the form of -OCOCH3 on the surface of the titania nanoparticles.

[0178] In an air atmosphere, silver nitrate (I) was added to 15 g (5.2 mass%) of this dispersion so that silver became 25 mass% on a metal weight basis relative to the titania nanoparticles (titanium oxide) contained in the dispersion, and after thorough stirring, the mixture was irradiated with an ultraviolet lamp at 15°C for 2 hours to obtain a white-ish dispersion.

[0179] Even after leaving the solution for about a week, there was no change in the color of the solution, and it was confirmed that the silver component was present stably in the solution. At this time, the pH of the solution was 1.9. The form of the silver in the solution was silver nanoparticles (average particle size 20 nm, aspect ratio 1.1).

[0180] This dispersion was applied to a 0.7 mm thick glass sheet with a total solid content of 6 mg / cm 2 The coated substrate was dried at 80° C. and measured with a spectrophotometer (Konica Minolta CM-36sG), and the haze of the coating was 0.7. From this, it can be seen that Example 1 is excellent in transparency.

[0181] At this time, no cracks were observed in the coating film formed on the glass substrate, which shows that Example 1 has excellent crack resistance.

[0182] In addition, even when the surface of the obtained glass substrate sample was strongly rubbed with a finger, no slipping was observed. From this, it can be understood that the titania nanoparticles in Example 1 have a high degree of adhesion to the glass surface.

[0183] The obtained glass substrate was exposed to ultraviolet light at 1 mW / cm using an ultraviolet irradiator (Analytik Jena US UVP XX-15BLB). 2 When exposed to UV-A, no discoloration was observed. This shows that the material has high resistance to discoloration from low-intensity UV rays.

[0184] Next, the obtained glass substrate was exposed to 500 mW / cm 2 UV irradiation using an ultraviolet irradiation device (Ushio Electric Tabletop UVC-1212 UV irradiation device). 2 After 30 minutes of exposure to UV-C, ΔE*ab was 10.8, and discoloration was confirmed by the naked eye. After leaving it to stand in a room temperature environment without UV rays, ΔE*ab was 1.8, below the standard of 2 that is visible to the naked eye. This confirmed that when the silver content is 25wt% relative to titanium oxide, coloring occurs when exposed to high-intensity UV rays, and re-transparency occurs when left to stand in a room temperature environment.

[0185] When this dispersion was subjected to an antibacterial test against Escherichia coli (K-12) using a method based on JIS Z2801 (in the dark, at 35° C. for 1 hour), the antibacterial activity value was 2.0 or more.

[0186] [Example 2] 5wt% silver nanostructure (aspect ratio 1.1) vs. TiO 2 142.1g (0.5mol) of titanium tetraisopropoxide was added with 30g (0.5mol) of acetic acid, stirred for 60 minutes, and then 538g of water was added. This dispersion had a titanium tetraisopropoxide concentration of 0.625mol / L, an acetic acid concentration of 0.625mol / L, and a pH of 2.2. A large amount of translucent precipitate was generated in this dispersion, but when the dispersion was stirred for 60 minutes and then heated at 70°C, all of the precipitate dissolved. In this dispersion, the concentration of inorganic acid, N, Cl, and S elements were all 0mol / L.

[0187] After that, the mixture was stirred at normal pressure (0.10 MPa) and 85°C for 3 hours, and a semi-transparent uniform titania dispersion was obtained without using an organic dispersant. When ultrasonic dispersion was applied to this dispersion, the viscosity was reduced and the transparency was increased. This dispersion had a water content of 67% by mass and a pH of 2.3.

[0188] The dispersion was dried to obtain titania nanoparticles. The BET specific surface area of ​​the titania nanoparticles was measured to be 250 m 2 / g. TEM observation revealed that the average particle size was about 3 nm. X-ray diffraction analysis of the crystallinity of the obtained titania nanoparticles revealed that they were 100% anatase type, with no other crystal forms present.

[0189] The dispersion was kept at 200°C using a moisture meter and dried until there was no mass loss. The TG-DTA of the titania nanoparticles was measured by heating the mixture to 600°C at a rate of 3°C / min in an air atmosphere. The mass loss above 200°C was 10% by mass. This mass loss above 200°C corresponds to the mass loss caused by the elimination of acetic acid, an organic acid. Since the liberated acetic acid almost evaporates below 200°C, the fact that the mass loss above 200°C is 10% by mass suggests that a large amount of acetyl groups, which are acyloxy groups, are bonded to titanium atoms in the form of -OCOCH3 on the surface of the titania nanoparticles.

[0190] In an air atmosphere, silver nitrate (I) was added to 15 g (5.2 mass%) of this dispersion so that silver was 5 mass% on a metal weight basis relative to the titania nanoparticles (titanium oxide) contained in the dispersion, and after thorough stirring, the mixture was irradiated with an ultraviolet lamp at 15°C for 2 hours to obtain a white-ish dispersion.

[0191] Even after leaving the solution for about a week, there was no change in the color of the solution, and it was confirmed that the silver component was present stably in the solution. At this time, the pH of the solution was 2.1. The form of the silver in the solution was silver nanoparticles (average particle size 20 nm, aspect ratio 1.1).

[0192] This dispersion was applied to a 0.7 mm thick glass sheet with a total solid content of 6 mg / cm 2 The coated substrate was dried at 80° C. and measured with a spectrophotometer (Konica Minolta CM-36sG), and the haze of the coating was 0.3. From this, it can be seen that Example 2 is excellent in transparency.

[0193] At this time, no cracks were observed in the coating film formed on the glass substrate, which shows that Example 2 has excellent crack resistance.

[0194] In addition, even when the surface of the obtained glass substrate sample was strongly rubbed with a finger, no slipping was observed. From this, it can be understood that the adhesion between the titania nanoparticles and the glass surface in Example 2 is high.

[0195] The obtained glass substrate was exposed to ultraviolet light at 1 mW / cm using an ultraviolet irradiator (Analytik Jena US UVP XX-15BLB). 2 When exposed to UV-A, no discoloration was observed. This shows that the material has high resistance to discoloration caused by low-intensity UV rays.

[0196] Next, the obtained glass substrate was exposed to 500 mW / cm 2 UV irradiation using an ultraviolet irradiation device (Ushio Electric Tabletop UVC-1212 UV irradiation device). 2After 30 minutes of exposure to UV-C, ΔE*ab was 2.5, and discoloration was confirmed by the naked eye. After leaving it to stand in a room temperature environment without UV rays, ΔE*ab was 1.4, below the standard of 2 that is visible to the naked eye. This confirmed that when the silver content is 5wt% relative to titanium oxide, coloring occurs when exposed to high-intensity UV rays, and re-transparency occurs when left to stand in a room temperature environment.

[0197] When this dispersion was subjected to an antibacterial test against Escherichia coli (K-12) using a method based on JIS Z2801 (in the dark, at 35° C. for 1 hour), the antibacterial activity value was 2.0 or more.

[0198] [Example 3] 0.1wt% silver nanostructure (aspect ratio 1.1) vs. TiO 2 142.1g (0.5mol) of titanium tetraisopropoxide was added with 30g (0.5mol) of acetic acid, stirred for 60 minutes, and then 538g of water was added. This dispersion had a titanium tetraisopropoxide concentration of 0.625mol / L, an acetic acid concentration of 0.625mol / L, and a pH of 2.2. A large amount of translucent precipitate was generated in this dispersion, but when the dispersion was stirred for 60 minutes and then heated at 70°C, all of the precipitate dissolved. In this dispersion, the concentration of inorganic acid, N, Cl, and S elements were all 0mol / L.

[0199] After that, the mixture was stirred at normal pressure (0.10 MPa) and 85°C for 3 hours, and a semi-transparent uniform titania dispersion was obtained without using an organic dispersant. When ultrasonic dispersion was applied to this dispersion, the viscosity was reduced and the transparency was increased. This dispersion had a water content of 67% by mass and a pH of 2.3.

[0200] The dispersion was dried to obtain titania nanoparticles. The BET specific surface area of ​​the titania nanoparticles was measured and found to be 250 m 2 / g. TEM observation revealed that the average particle size was about 3 nm. X-ray diffraction analysis of the crystallinity of the obtained titania nanoparticles revealed that they were 100% anatase type, with no other crystal forms present.

[0201] The dispersion was kept at 200°C using a moisture meter and dried until there was no mass loss. The TG-DTA of the titania nanoparticles was measured by heating the mixture to 600°C at a rate of 3°C / min in an air atmosphere. The mass loss above 200°C was 10% by mass. This mass loss above 200°C corresponds to the mass loss caused by the elimination of acetic acid, an organic acid. Since the liberated acetic acid almost evaporates below 200°C, the fact that the mass loss above 200°C is 10% by mass suggests that a large amount of acetyl groups, which are acyloxy groups, are bonded to titanium atoms in the form of -OCOCH3 on the surface of the titania nanoparticles.

[0202] In an air atmosphere, silver nitrate (I) was added to 15 g (5.2 mass%) of this dispersion so that the silver content was 0.1 mass% on a metal weight basis relative to the titania nanoparticles (titanium oxide) contained in the dispersion. After thorough stirring, the mixture was irradiated with an ultraviolet lamp at 15°C for 2 hours to obtain a white-ish dispersion.

[0203] Even after leaving the solution for about a week, there was no change in the color of the solution, and it was confirmed that the silver component was present stably in the solution. At this time, the pH of the solution was 2.2. The form of the silver in the solution was silver nanoparticles (average particle diameter 20 nm, aspect ratio 1.1).

[0204] This dispersion was applied to a 0.7 mm thick glass sheet with a total solid content of 6 mg / cm 2 The coated substrate was dried at 80° C. and measured with a spectrophotometer (Konica Minolta CM-36sG), and the haze of the coating was 0.2. From this, it can be seen that Example 3 is excellent in transparency.

[0205] At this time, no cracks were observed in the coating film formed on the glass substrate, which shows that Example 3 has excellent crack resistance.

[0206] In addition, even when the surface of the obtained glass substrate sample was strongly rubbed with a finger, no slipping was observed. From this, it can be understood that the adhesion between the titania nanoparticles and the glass surface in Example 3 is high.

[0207] The obtained glass substrate was exposed to ultraviolet light at 1 mW / cm using an ultraviolet irradiator (Analytik Jena US UVP XX-15BLB). 2 When exposed to UV-A, no discoloration was observed. This shows that the material has high resistance to discoloration caused by low-intensity UV rays.

[0208] Next, the obtained glass substrate was exposed to 500 mW / cm 2 UV irradiation using an ultraviolet irradiation device (Ushio Electric Tabletop UVC-1212 UV irradiation device). 2 After 30 minutes of exposure to UV-C, ΔE*ab was 2.1, and discoloration was confirmed by the naked eye. After leaving it to stand in a room temperature environment without UV rays, ΔE*ab was 0.6, below the standard of 2 that is visible to the naked eye. This confirmed that when the silver content is 0.1wt% with respect to titanium oxide, coloring occurs when exposed to high-intensity UV rays, and re-transparency occurs when left to stand in a room temperature environment.

[0209] When this dispersion was subjected to an antibacterial test against Escherichia coli (K-12) using a method based on JIS Z2801 (in the dark, at 35° C. for 1 hour), the antibacterial activity value was 2.0 or more.

[0210] [Example 4] 5wt% silver nanowire (aspect ratio 100) vs. TiO 2 142.1g (0.5mol) of titanium tetraisopropoxide was added with 30g (0.5mol) of acetic acid, stirred for 60 minutes, and then 538g of water was added. This dispersion had a titanium tetraisopropoxide concentration of 0.625mol / L, an acetic acid concentration of 0.625mol / L, and a pH of 2.2. A large amount of translucent precipitate was generated in this dispersion, but when the dispersion was stirred for 60 minutes and then heated at 70°C, all of the precipitate dissolved. In this dispersion, the concentration of inorganic acid, N, Cl, and S elements were all 0mol / L.

[0211] After that, the mixture was stirred at normal pressure (0.10 MPa) and 85°C for 3 hours, and a semi-transparent uniform titania dispersion was obtained without using an organic dispersant. When ultrasonic dispersion was applied to this dispersion, the viscosity was reduced and the transparency was increased. This dispersion had a water content of 67% by mass and a pH of 2.3.

[0212] The dispersion was dried to obtain titania nanoparticles. The BET specific surface area of ​​the titania nanoparticles was measured to be 250 m 2 / g. TEM observation revealed that the average particle size was about 3 nm. X-ray diffraction analysis of the crystallinity of the obtained titania nanoparticles revealed that they were 100% anatase type, with no other crystal forms present.

[0213] The dispersion was kept at 200°C using a moisture meter and dried until there was no mass loss. The TG-DTA of the titania nanoparticles was measured by heating the mixture to 600°C at a rate of 3°C / min in an air atmosphere. The mass loss above 200°C was 10% by mass. This mass loss above 200°C corresponds to the mass loss caused by the elimination of acetic acid, an organic acid. Since the liberated acetic acid almost evaporates below 200°C, the fact that the mass loss above 200°C is 10% by mass suggests that a large amount of acetyl groups, which are acyloxy groups, are bonded to titanium atoms in the form of -OCOCH3 on the surface of the titania nanoparticles.

[0214] In an air atmosphere, silver nanorods with an aspect ratio of 100, synthesized with reference to a previous report, were added to 15 g (5.2 mass%) of this dispersion so that the silver content was 5 mass% on a metal weight basis relative to the titania nanoparticles (titanium oxide) contained in the dispersion. After thorough stirring, the mixture was irradiated with an ultraviolet lamp at 15°C for 2 hours to obtain a near-white dispersion.

[0215] Even after leaving the solution for about a week, there was no change in the color of the solution, and it was confirmed that the silver component was present stably in the solution. At this time, the pH of the solution was 2.3. The form of the silver in the solution was silver nanowires (average short axis length 50 nm, aspect ratio 100).

[0216] This dispersion was applied to a 0.7 mm thick glass sheet with a total solid content of 6 mg / cm 2 The coated substrate was dried at 80° C. and measured with a spectrophotometer (Konica Minolta CM-36sG), and the haze of the coating was 0.1. From this, it can be seen that Example 4 is excellent in transparency.

[0217] At this time, no cracks were observed in the coating film formed on the glass substrate, which shows that Example 4 has excellent crack resistance.

[0218] In addition, even when the surface of the obtained glass substrate sample was strongly rubbed with a finger, no slipping was observed. From this, it can be understood that the adhesion between the titania nanoparticles and the glass surface in Example 4 is high.

[0219] The obtained glass substrate was exposed to ultraviolet light at 1 mW / cm using an ultraviolet irradiator (Analytik Jena US UVP XX-15BLB). 2 When exposed to UV-A, no discoloration was observed. This shows that the material has high resistance to discoloration caused by low-intensity UV rays.

[0220] Next, the obtained glass substrate was exposed to 500 mW / cm 2 UV irradiation using an ultraviolet irradiation device (Ushio Electric Tabletop UVC-1212 UV irradiation device). 2 After 30 minutes of exposure to UV-C, ΔE*ab was 2.4, and discoloration was confirmed by the naked eye. After leaving it to stand in a room temperature environment away from UV rays, ΔE*ab was 0.6, below the standard of 2 that is visible to the naked eye. This confirmed that when silver nanowires with an aspect ratio of 100 are supported on titanium oxide, coloring occurs when exposed to high-intensity UV light, and re-transparency occurs when left to stand in a room temperature environment.

[0221] When this dispersion was subjected to an antibacterial test against Escherichia coli (K-12) using a method based on JIS Z2801 (in the dark, at 35° C. for 1 hour), the antibacterial activity value was 2.0 or more.

[0222] [Comparative Example 1] 5wt% silver nanowire (aspect ratio 1,000) vs. TiO 2 142.1g (0.5mol) of titanium tetraisopropoxide was added with 30g (0.5mol) of acetic acid, stirred for 60 minutes, and then 538g of water was added. This dispersion had a titanium tetraisopropoxide concentration of 0.625mol / L, an acetic acid concentration of 0.625mol / L, and a pH of 2.2. A large amount of translucent precipitate was generated in this dispersion, but when the dispersion was stirred for 60 minutes and then heated at 70°C, all of the precipitate dissolved. In this dispersion, the concentration of inorganic acid, N, Cl, and S elements were all 0mol / L.

[0223] After that, the mixture was stirred at normal pressure (0.10 MPa) and 85°C for 3 hours, and a semi-transparent uniform titania dispersion was obtained without using an organic dispersant. When ultrasonic dispersion was applied to this dispersion, the viscosity was reduced and the transparency was increased. This dispersion had a water content of 67% by mass and a pH of 2.3.

[0224] The dispersion was dried to obtain titania nanoparticles. The BET specific surface area of ​​the titania nanoparticles was measured to be 250 m 2 / g. TEM observation revealed that the average particle size was about 3 nm. X-ray diffraction analysis of the crystallinity of the obtained titania nanoparticles revealed that they were 100% anatase type, with no other crystal forms present.

[0225] The dispersion was kept at 200°C using a moisture meter and dried until there was no mass loss. The TG-DTA of the titania nanoparticles was measured by heating the mixture to 600°C at a rate of 3°C / min in an air atmosphere. The mass loss above 200°C was 10% by mass. This mass loss above 200°C corresponds to the mass loss caused by the elimination of acetic acid, an organic acid. Since the liberated acetic acid almost evaporates below 200°C, the fact that the mass loss above 200°C is 10% by mass suggests that a large amount of acetyl groups, which are acyloxy groups, are bonded to titanium atoms in the form of -OCOCH3 on the surface of the titania nanoparticles.

[0226] In an air atmosphere, silver nanorods with an aspect ratio of 1,000, synthesized with reference to a previous report, were added to 15 g (5.2 mass%) of this dispersion so that the silver content was 5 mass% on a metal weight basis relative to the titania nanoparticles (titanium oxide) contained in the dispersion. After thorough stirring, the mixture was irradiated with an ultraviolet lamp at 15°C for 2 hours to obtain a white-ish dispersion.

[0227] Even after leaving the solution for about a week, there was no change in the color of the solution, and it was confirmed that the silver component was present stably in the solution. At this time, the pH of the solution was 2.3. The form of the silver in the solution was silver nanowires (average short axis length 50 nm, aspect ratio 1,000).

[0228] This dispersion was applied to a 0.7 mm thick glass sheet with a total solid content of 6 mg / cm 2 The coated substrate was dried at 80° C. and measured with a spectrophotometer (Konica Minolta CM-36sG), and the haze of the coating was 0.2. From this, it can be seen that Comparative Example 3 is excellent in transparency.

[0229] At this time, no cracks were observed in the coating film formed on the glass substrate, which shows that Comparative Example 3 is excellent in crack resistance.

[0230] In addition, even when the surface of the obtained glass substrate sample was strongly rubbed with a finger, no slipping was observed. From this, it can be understood that the adhesion between the titania nanoparticles and the glass surface is high in Comparative Example 3.

[0231] The obtained glass substrate was exposed to ultraviolet light at 1 mW / cm using an ultraviolet irradiator (Analytik Jena US UVP XX-15BLB). 2 When exposed to UV-A, no discoloration was observed. This shows that the material has high resistance to discoloration from low-intensity UV rays.

[0232] Next, the obtained glass substrate was exposed to 500 mW / cm 2 UV irradiation using an ultraviolet irradiation device (Ushio Electric Tabletop UVC-1212 UV irradiation device). 2After 30 minutes of irradiation with UV-C, ΔE*ab was 0.0, and no discoloration was visible to the naked eye. This confirmed that when silver nanowires with an aspect ratio of 1,000 are supported on titanium oxide, no discoloration occurs due to high-intensity ultraviolet irradiation.

[0233] [Comparative Example 2] Conventional technology (titania nanoparticles with no acyl groups on the surface) Titania nanoparticles ST-01 (Ishihara Sangyo Kaisha, Ltd., specific surface area 300 m 2 To a dispersion liquid of 10 g of silver (10 g / g, average particle size calculated from the specific surface area: 5 nm, no acyl groups present on the surface), 30 g of acetic acid and 160 g of water were added, and silver nitrate (I) was added so that the silver content was 5 mass% on a metal weight basis. After thorough stirring, the mixture was irradiated with an ultraviolet lamp at 15°C for 2 hours to obtain a white-ish dispersion liquid.

[0234] After leaving the solution for about a week, a precipitate was observed. This indicated that the solution was unstable. At this time, the pH of the solution was 2.3.

[0235] Next, this suspension was applied (spin-coated) to a glass substrate having a thickness of 0.7 mm, the substrate was dried at 80° C., and the haze of the coating was measured with a spectrophotometer (Konica Minolta CM-36sG) to find that it was 92.5.

[0236] In addition, when the surface of the obtained glass substrate sample was lightly rubbed with a finger, the titania nanoparticles slid off. From this, it can be understood that the adhesion between the titania nanoparticles ST-01 and the glass surface in Comparative Example 4 is lower than that in Example 1.

[0237] [Industrial Applicability] The present invention makes it possible to provide a composition which is transparent, does not discolor due to the ultraviolet light intensity of sunlight present in a typical indoor environment, and when irradiated with light intensity exceeding the ultraviolet light intensity, the coating film changes color, which can be confirmed, and the color fades after a certain period of time and becomes transparent again, thereby not impairing the design properties.

Claims

1. A composition comprising titania nanoparticles and silver nanostructures, The titania nanoparticles have acyloxy groups bonded to at least some of the titanium atoms present on the surface, and when the titania nanoparticles are heated to 600°C using a thermogravimetric and differential thermal analyzer, the mass loss at 200°C or higher is 5% by mass or more; The silver nanostructures have an aspect ratio of 1-100.

2. 2. The composition according to claim 1, wherein the acyloxy group is a group represented by -OCOR (wherein R represents a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a hydroxyalkyl group having 1 to 2 carbon atoms).

3. 3. The composition according to claim 2, wherein the acyloxy group is derived from at least one organic acid selected from the group consisting of monocarboxylic acids having 1 to 4 carbon atoms and hydroxycarboxylic acids having 2 to 3 carbon atoms.

4. 4. The composition according to claim 3, wherein the organic acid is at least one organic acid selected from the group consisting of lactic acid and acetic acid.

5. 5. The composition of claim 4, wherein the organic acid is acetic acid.

6. 2. The composition according to claim 1, wherein the titania nanoparticles have a particle size of 1 nm to 50 nm.

7. The specific surface area of ​​the titania nanoparticles is 150 m 2 / g~500m 2 / g of the composition described in claim 1.

8. 2. The composition of claim 1, wherein the titania nanoparticles are free of any crystalline form other than anatase.

9. The composition according to claim 1, wherein the silver nanostructure is contained in an amount of 0.1% by mass to 25% by mass relative to the titania nanoparticles.

10. The composition of claim 1, wherein the short axis length of the silver nanostructure is 1 nm to 100 nm.

11. A laminate comprising the composition according to any one of claims 1 to 10.

12. A coating film comprising the composition according to any one of claims 1 to 10.

Citation Information

Patent Citations

  • Metal-carrying titania nanoparticle, and production method thereof

    JP2022155211A

  • Titanium oxide compound having photochromic properties and method for producing the same

    JP3213996B2

  • Multicolor photochromic material, method for manufacturing the same, and method for using the same

    JP4126691B2