Solid oxide fuel cell
The solid oxide fuel cell design addresses warpage and cracking issues by using a porous metal layer with mixed metal and ceramic layers to match thermal expansion coefficients, ensuring structural stability during temperature changes.
Patent Information
- Application Number
- JP2023046991
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
Existing solid oxide fuel cells face issues with warpage and cracking due to differences in thermal expansion coefficients between the metal support layer and electrolyte layer, particularly during rapid temperature changes.
A solid oxide fuel cell design incorporating a first porous metal layer with mixed metal and ceramic layers, where the thermal expansion coefficients are matched by controlling the mixing ratio of ceramic and metal materials, reducing warpage and suppressing cracking.
The design effectively reduces warpage and prevents cracking by providing a structure resistant to thermal shock, maintaining structural integrity during rapid temperature fluctuations.
Smart Images

Figure 2024136037000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a solid oxide fuel cell. [Background technology]
[0002] In order to develop a solid oxide fuel cell system that can be used in automobiles, etc., it is desirable to develop a cell that can withstand vibration and does not crack even when heated rapidly. Therefore, metal-supported solid oxide fuel cells that are supported by a metal support have been developed (for example, see Patent Documents 1 to 3). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2021-158026 A [Patent Document 2] JP 2013-79190 A Summary of the Invention [Problem to be solved by the invention]
[0004] In Patent Document 1, a ferritic metal support is used to match the thermal expansion coefficients of the metal support layer and the electrolyte layer. However, there is a limit to how much the thermal expansion coefficient of ferritic stainless steel can be adjusted even if the composition is adjusted, and the difference in thermal expansion coefficient with the ZrO2-based material of the electrolyte causes warping of the cell due to thermal stress.
[0005] In Patent Document 2, the mixture ratio of ZrO2-based material and NiO is adjusted to match the thermal expansion coefficient. However, the cells in Patent Documents 2 and 3 are not metal-supported cells, and therefore have the problem of cracking during rapid temperature increases and decreases.
[0006] The present invention has been made in consideration of the above problems, and has an object to provide a solid oxide fuel cell that can reduce the amount of warping and suppress cracking. [Means for solving the problem]
[0007] The solid oxide fuel cell of the present invention comprises a first porous metal layer mainly composed of metal, a first mixed layer provided on the first porous metal layer and having a structure in which a metallic material and a ceramic material are mixed, an anode provided on the first mixed layer and containing a ceramic material, and a second mixed layer provided below the first porous metal layer and having a structure in which a metallic material and a ceramic material are mixed.
[0008] In the solid oxide fuel cell, the first porous metal layer may be made of metal only.
[0009] In the solid oxide fuel cell, the first porous metal layer may be made of ferritic stainless steel.
[0010] In the solid oxide fuel cell, the thermal expansion coefficient of the ceramic material of the first mixed layer and the second mixed layer is 10.5×10 -6 / °C or less.
[0011] In the solid oxide fuel cell, the metal material of the mixed layer may be ferritic stainless steel.
[0012] In the first mixed layer and the second mixed layer of the solid oxide fuel cell, a volume ratio of the ceramic material may be 20 vol % or more and 80 vol % or less.
[0013] In the solid oxide fuel cell, the first porous metal layer may have a thickness greater than the thicknesses of the first mixed layer and the second mixed layer.
[0014] The solid oxide fuel cell may have a substantially rectangular shape in a plan view, and the amount of warping of the solid oxide fuel cell may be less than 1 / 10 of the length of one side of the substantially rectangular shape.
[0015] The solid oxide fuel cell may further comprise a second porous metal layer containing metal as a main component below the second mixed layer. Effect of the Invention
[0016] According to the present invention, it is possible to provide a solid oxide fuel cell capable of reducing the amount of warping and suppressing cracks. [Brief description of the drawings]
[0017] [Figure 1] 2 is a schematic cross-sectional view illustrating a stack structure of a fuel cell. FIG. [Diagram 2] FIG. 2 is an enlarged cross-sectional view illustrating details of the mixed layer, the porous metal layer, the mixed layer, and the anode. [Diagram 3] FIG. 2 is a diagram illustrating a flow of a method for manufacturing a fuel cell. [Figure 4] 6 is a schematic cross-sectional view illustrating a stack structure of a fuel cell according to a second embodiment. FIG. [Diagram 5] 11 is a schematic cross-sectional view illustrating a stack structure of a fuel cell according to a third embodiment. FIG. [Figure 6] 13 is a schematic cross-sectional view illustrating a stack structure of a fuel cell according to a fourth embodiment. FIG. [Figure 7] FIG. 13 is a diagram for explaining the amount of warpage. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, an embodiment will be described with reference to the drawings.
[0019] (First embodiment) Fig. 1 is a schematic cross-sectional view illustrating a stacked structure of a solid oxide fuel cell 100. As illustrated in Fig. 1, the fuel cell 100 has a structure in which, for example, a first porous metal layer 10a, a first mixed layer 20a, an anode 30, an electrolyte layer 40, an intermediate layer 50, and a cathode 60 are stacked in this order on a second mixed layer 20b. The fuel cell 100 has, for example, a substantially rectangular shape in a plan view. A fuel cell stack may be formed by stacking a plurality of fuel cells 100.
[0020] The electrolyte layer 40 is a dense layer mainly composed of a solid oxide having oxide ion conductivity and having gas impermeability. The electrolyte layer 40 is preferably mainly composed of ZrO2-based ceramics such as scandia-yttria stabilized zirconium oxide (ScYSZ) or YSZ (yttria stabilized zirconium oxide), or is preferably mainly composed of GDC (Gd-doped ceria) in which Gd (gadolinium) is doped into CeO2. When using ScYSZ, the oxide ion conductivity is highest when the concentration of Y2O3+Sc2O3 is between 6 mol% and 15 mol%, and it is desirable to use a material with this composition. In addition, the thickness of the electrolyte layer 40 is preferably 20 μm or less, and more preferably 10 μm or less. The thinner the electrolyte, the better, but in order to manufacture it so that gas does not leak from both sides, a thickness of 1 μm or more is desirable.
[0021] The cathode 60 is an electrode having electrode activity as a cathode, and has electronic conductivity and oxide ion conductivity. For example, the cathode 60 is mainly composed of a ceramic material having electronic conductivity and oxide ion conductivity. As the ceramic material, for example, a LaCoO3-based material, a LaMnO3-based material, a LaFeO3-based material, etc. can be used. For example, as the LaCoO3-based material, LSC (lanthanum strontium cobaltite) etc. can be used. LSC is LaCoO3 doped with Sr (strontium).
[0022] The intermediate layer 50 is mainly composed of a component that prevents a reaction between the electrolyte layer 40 and the cathode 60. The constituent material of the intermediate layer 50 is different from the constituent material of the electrolyte layer 40. The intermediate layer 50 has oxide ion conductivity, but does not have electrode activity as a cathode. For example, the intermediate layer 50 has a structure in which an additive is added to ceria (CeO2). The additive is not particularly limited. For example, the intermediate layer 50 may be made of GDC (e.g., Ce 0.8 Gd 0.2 O 2-x As an example, when the electrolyte layer 40 contains ScYSZ and the cathode 60 contains LSC, the intermediate layer 50 prevents the following reaction: Sr+ZrO2 → SrZrO3 La+ZrO3→La2Zr2O7
[0023] FIG. 2 is an enlarged cross-sectional view illustrating the details of the second mixed layer 20b, the first porous metal layer 10a, the first mixed layer 20a, and the anode 30. As illustrated in FIG. 2, the first porous metal layer 10a is a member that has gas permeability and can support the first mixed layer 20a, the second mixed layer 20b, the anode 30, the electrolyte layer 40, the intermediate layer 50, and the cathode 60. The first porous metal layer 10a is a metal porous body mainly composed of metal, such as ferritic stainless steel. By using ferritic stainless steel, the thermal expansion coefficient of the first porous metal layer 10a can be made close to the thermal expansion coefficient of the electrolyte layer 40. In addition, it is preferable that the first porous metal layer 10a is composed only of metal components. This is because the thermal shock resistance and mechanical shock resistance of the first porous metal layer 10a can be improved.
[0024] The anode 30 is an electrode having electrode activity as an anode, and has an electrode skeleton made of a ceramic material. The electrode skeleton does not contain metal components. In this configuration, the decrease in the porosity of the anode caused by the coarsening of the metal components during firing in a high-temperature reducing atmosphere is suppressed. In addition, alloying with the metal components of the first porous metal layer 10a is suppressed, and the decrease in catalytic function is suppressed.
[0025] The electrode skeleton of the anode 30 has electronic conductivity and oxide ion conductivity. The anode 30 contains an electronically conductive ceramic 31. As the electronically conductive ceramic 31, for example, a perovskite oxide having a composition formula of ABO3, in which the A site is at least one selected from the group consisting of Ca, Sr, Ba, and La, and the B site is at least one selected from the group consisting of Ti, Cr, Ni, Mg, and Co, can be used. The molar ratio of the A site to the B site may be B≧A. Specifically, as the electronically conductive ceramic 31, a LaCrO3-based material, a SrTiO3-based material, or the like can be used.
[0026] The electrode skeleton of the anode 30 contains oxide ion conductive ceramics 32. The oxide ion conductive ceramics 32 are ScYSZ or the like. For example, it is preferable to use ScYSZ having a composition range of 5 mol% to 16 mol% of scandia (Sc2O3) and 1 mol% to 3 mol% of yttria (Y2O3). It is more preferable to use ScYSZ in which the total amount of scandia and yttria added is 6 mol% to 15 mol%. This is because the oxide ion conductivity is highest in this composition range. The oxide ion conductive ceramics 32 are, for example, materials having an oxide ion transport number of 99% or more. GDC or the like may be used as the oxide ion conductive ceramics 32. In the example of FIG. 2, the same solid oxide as the solid oxide contained in the electrolyte layer 40 is used as the oxide ion conductive ceramics 32.
[0027] As shown in FIG. 2, in the anode 30, for example, an electron conductive ceramic 31 and an oxide ion conductive ceramic 32 form an electrode skeleton. This electrode skeleton forms a plurality of voids. An anode catalyst is supported on the surface of the electrode skeleton in the void portion. Therefore, in the electrode skeleton that is formed spatially continuously, a plurality of anode catalysts are arranged in a spatially dispersed manner. It is preferable to use a composite catalyst as the anode catalyst. For example, it is preferable that an oxide ion conductive ceramic 33 and a catalytic metal 34 are supported as the composite catalyst on the surface of the electrode skeleton. For example, Y-doped BaCe 1-x Zr x O3(BCZY, x=0~1), Y-doped SrCe 1-x Zr x O3 (SCZY, x=0-1), Sr-doped LaScO3 (LSS), GDC, etc. can be used. Ni, etc. can be used as the catalytic metal 34. The oxide ion conductive ceramics 33 may have the same composition as the oxide ion conductive ceramics 32, or may have a different composition. The metal functioning as the catalytic metal 34 may be in the form of a compound when power is not being generated. For example, Ni may be in the form of NiO (nickel oxide). These compounds are reduced by a reducing fuel gas supplied to the anode 30 during power generation, and take the form of a metal functioning as an anode catalyst.
[0028] The first mixed layer 20a and the second mixed layer 20b contain a metal material 21 and a ceramic material 22. In the first mixed layer 20a and the second mixed layer 20b, the metal material 21 and the ceramic material 22 are randomly mixed. Therefore, a structure in which a layer of the metal material 21 and a layer of the ceramic material 22 are laminated is not formed. The first mixed layer 20a and the second mixed layer 20b are porous and have a plurality of voids. The metal material 21 is not particularly limited as long as it is a metal. For example, it is preferable to use the same metal material as the first porous metal layer 10a as the metal material 21. For example, it is preferable to use ferritic stainless steel or the like as the metal material 21. In addition, it is preferable to use the same ceramic material as the ceramic material contained in the anode 30 as the ceramic material 22 as the ceramic material.
[0029] The first mixed layer 20a and the second mixed layer 20b need only have a configuration in which a metal material and a ceramic material are mixed, and do not necessarily have to include the same metal material and the same ceramic material.
[0030] The fuel cell 100 generates electricity by the following action. An oxidant gas containing oxygen, such as air, is supplied to the cathode 60. In the cathode 60, due to the effect of the electrode activity of the cathode 60, the oxygen that has reached the cathode 60 reacts with electrons supplied from an external electric circuit to become oxide ions. The oxide ions move to the anode 30 side by conducting through the intermediate layer 50 and the electrolyte layer 40. On the other hand, a fuel gas containing hydrogen, such as hydrogen gas or reformed gas, is supplied to the second mixed layer 20b. The fuel gas reaches the anode 30 through the second mixed layer 20b, the first porous metal layer 10a, and the first mixed layer 20a. Due to the effect of the electrode activity of the anode 30, the hydrogen that has reached the anode 30 releases electrons at the anode 30 and reacts with oxide ions that have been conducted through the electrolyte layer 40 from the cathode 60 side to become water (H2O). The released electrons are taken out to the outside by the external electric circuit. The electrons extracted to the outside perform electrical work and are then supplied to the cathode 60. Through the above-mentioned actions, electricity is generated.
[0031] The first mixed layer 20a and the second mixed layer 20b contain the metal material 21 and the ceramic material 22, and therefore have both the material properties of metal and ceramic. Therefore, the first porous metal layer 10a has high adhesion between the first mixed layer 20a and the second mixed layer 20b, and the second mixed layer 20b has high adhesion between the first porous metal layer 10a and the anode 30. For these reasons, interlayer peeling from the second mixed layer 20b to the anode 30 can be suppressed.
[0032] The fuel cell 100 includes the first porous metal layer 10a, which is mainly composed of metal, and is therefore resistant to thermal shock, mechanical shock, etc. Therefore, cracks caused by rapid temperature increases and decreases can be suppressed.
[0033] Due to the difference in materials, a difference in thermal expansion coefficient occurs between the electrolyte layer 40 and the first porous metal layer 10a. However, since the first mixed layer 20a and the second mixed layer 20b, which have both the material properties of metal and ceramic, are provided apart from each other, the effect of the difference in thermal expansion coefficient can be suppressed. As a result, warping of the fuel cell 100 is suppressed.
[0034] From the above, the fuel cell 100 according to this embodiment can reduce the amount of warping and suppress cracking.
[0035] The thermal expansion coefficients of the first mixture layer 20a and the second mixture layer 20b can be controlled by controlling the mixture ratio of the metal material 21 and the ceramic material 22 in the first mixture layer 20a and the second mixture layer 20b. From the viewpoint of bringing the thermal expansion coefficients of the first mixture layer 20a and the second mixture layer 20b closer to that of the first porous metal layer 10a, the thermal expansion coefficient of the ceramic material 22 is set to, for example, 10.5×10 -6 / °C or less. For example, ZrO2-based materials such as ScYSZ, GDC, La-doped SrTiO3-based materials, Ni-doped LaCrO3-based materials, mullite, aluminum nitride, etc. can be used as the ceramic material 22. Since the SrTiO3-based materials and LaCrO3-based materials have high electronic conductivity, the ohmic resistance in the first mixed layer 20a and the second mixed layer 20b can be reduced.
[0036] The volume ratio of the ceramic material 22 in the first mixed layer 20a and the second mixed layer 20b is preferably 20 vol% or more and 80 vol% or less. If the volume ratio exceeds 80 vol%, the adhesion between the first mixed layer 20a and the second mixed layer 20b and the first porous metal layer 10a may deteriorate, causing delamination between the layers, and if the ratio is less than 20 vol%, it may be difficult to adjust the thermal expansion coefficient, making it difficult to improve warpage.
[0037] In order to provide the first porous metal layer 10a with sufficient thermal shock resistance and mechanical shock resistance, it is preferable to set a lower limit for the thickness of the first porous metal layer 10a. In this embodiment, the thickness of the first porous metal layer 10a is preferably 50 μm or more, more preferably 150 μm or more, and even more preferably 200 μm or more.
[0038] On the other hand, from the viewpoint of cost and cell weight reduction, it is preferable to set an upper limit on the thickness of the first porous metal layer 10a. In this embodiment, the thickness of the first porous metal layer 10a is preferably 2 mm or less, more preferably 1 mm or less, and further preferably 0.8 mm or less.
[0039] From the viewpoint of not affecting the mechanical properties (flexibility, bending strength, etc.) of the entire cell, it is preferable that the first mixed layer 20a and the second mixed layer 20b are thin. Therefore, it is preferable that the thickness of each of the first mixed layer 20a and the second mixed layer 20b is smaller than the thickness of the first porous metal layer 10a. In addition, it is preferable that the total thickness of the first mixed layer 20a and the second mixed layer 20b is smaller than the thickness of the first porous metal layer 10a.
[0040] In addition, it is preferable to set an upper limit on the thickness of the first mixed layer 20a and the second mixed layer 20b. In this embodiment, the thickness of each of the first mixed layer 20a and the second mixed layer 20b is preferably 100 μm or less, more preferably 50 μm or less, and further preferably 30 μm or less.
[0041] On the other hand, from the viewpoint of maintaining adhesion and preventing delamination, it is preferable to set a lower limit for the thickness of the first mixed layer 20a and the second mixed layer 20b. In this embodiment, the thickness of each of the first mixed layer 20a and the second mixed layer 20b is preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 15 μm or more.
[0042] The following describes a method for producing the fuel cell 100. Figure 3 is a diagram illustrating an example of the flow of the method for producing the fuel cell 100.
[0043] (Process for producing porous metal layer material) As the material for the porous metal layer, a metal powder (for example, a particle size of 10 μm to 100 μm), a plasticizer (for example, adjusted to 1 wt% to 6 wt% to adjust the adhesion of the sheet), a solvent (toluene, 2-propanol (IPA), 1-butanol, terpineol, butyl acetate, ethanol, etc., 20 wt% to 30 wt% depending on the viscosity), a dissipating material (organic matter), and a binder (PVB, acrylic resin, ethyl cellulose, etc.) are mixed to form a slurry. The material for the porous metal layer is used as a material for forming the first porous metal layer 10a and the second porous metal layer 10b. The volume ratio of the organic component (dissipating material, binder solid content, plasticizer) to the metal powder is, for example, in the range of 1:1 to 20:1, and the amount of the organic component is adjusted depending on the porosity. It is preferable that the metal powder of the material for the porous metal layer does not contain Ni.
[0044] (Preparation process of materials for mixed layer) As the material for the mixed layer, ceramic material powder (for example, particle size 100 nm to 10 μm) which is the raw material of the ceramic material 22, metal material powder with a small particle size (for example, particle size 1 μm to 10 μm) which is the raw material of the metal material 21, solvent (toluene, 2-propanol (IPA), 1-butanol, terpineol, butyl acetate, ethanol, etc., 20 wt% to 30 wt% depending on the viscosity), plasticizer (for example, adjusted to 1 wt% to 6 wt% to adjust the adhesion of the sheet), vanishing material (organic matter), and binder (PVB, acrylic resin, ethyl cellulose, etc.) are mixed to form a slurry. The volume ratio of the organic component (vanishing material, binder solid content, plasticizer) to the ceramic material powder and metal material powder is, for example, in the range of 1:1 to 5:1, and the amount of the organic component is adjusted depending on the porosity. The pore size of the voids is controlled by adjusting the particle size of the vanishing material. The ceramic material powder may contain an electron conductive material powder and an oxide ion conductive material powder. In this case, the volume ratio of the electron conductive material powder to the oxide ion conductive material powder is preferably in the range of, for example, 1:9 to 9:1. Also, even if an electrolyte material such as ScYSZ or GDC is used instead of the electron conductive material, there is no peeling at the interface, and a cell can be fabricated. However, from the viewpoint of reducing the ohmic resistance, it is preferable to mix the electron conductive material with a metal powder.
[0045] (Anode material manufacturing process) As the anode material, a ceramic material powder constituting the electrode skeleton, a solvent (toluene, 2-propanol (IPA), 1-butanol, terpineol, butyl acetate, ethanol, etc., 20 wt% to 30 wt% depending on the viscosity), a plasticizer (for example, adjusted to 1 wt% to 6 wt% to adjust the adhesion of the sheet), a dissipating material (organic material), and a binder (PVB, acrylic resin, ethyl cellulose, etc.) are mixed to form a slurry. As the ceramic material powder constituting the electrode skeleton, an electron conductive material powder (for example, particle size 100 nm to 10 μm) which is the raw material of the electron conductive ceramic 31, an oxide ion conductive material powder (for example, particle size 100 nm to 10 μm) which is the raw material of the oxide ion conductive ceramic 32, etc. may be used. The volume ratio of the organic components (dissipating material, binder solids, plasticizer) to the electron conductive material powder is, for example, in the range of 1:1 to 5:1, and the amount of the organic components is adjusted depending on the porosity. The pore size of the voids is controlled by adjusting the particle size of the dissipating material. The volume ratio of the electron conductive material powder to the oxide ion conductive material powder is set in the range of 1:9 to 9:1, for example.
[0046] (Electrolyte layer material manufacturing process) As the material for the electrolyte layer, oxide ion conductive material powder (e.g., ScYSZ, YSZ, GDC, etc., with a particle size of D50%=10 nm to 1000 nm), solvent (toluene, 2-propanol (IPA), 1-butanol, terpineol, butyl acetate, ethanol, etc., 20 wt% to 30 wt% depending on the viscosity), plasticizer (e.g., adjusted to 1 wt% to 6 wt% to adjust the adhesion of the sheet), and binder (PVB, acrylic resin, ethyl cellulose, etc.) are mixed to form a slurry. The volume ratio of the organic components (binder solids, plasticizer) to the oxide ion conductive material powder is, for example, in the range of 6:4 to 3:4.
[0047] (Firing process) First, a porous metal green sheet is produced by coating a material for a porous metal layer on a PET (polyethylene terephthalate) film. A mixed layer green sheet is produced by coating a material for a mixed layer on another PET film. An anode green sheet is produced by coating an anode material on another PET film. An electrolyte layer green sheet is produced by coating an electrolyte layer material on another PET film. In this embodiment, the mixed layer green sheet, the porous metal green sheet, and the mixed layer green sheet are laminated in this order, and one anode green sheet and one electrolyte layer green sheet are laminated on top of them in this order, and then cut to a predetermined size. After that, the mixture is heated to 1000° C. for 20 minutes, and then cooled to 300° C. for 20 minutes. -20 The mixture is fired at a temperature range of about 1100°C to 1300°C in a reducing atmosphere of atm or less. As a result, a half cell including the second mixed layer 20b, the first porous metal layer 10a, the first mixed layer 20a, the electrode skeleton of the anode 30, and the electrolyte layer 40 can be obtained. The second mixed layer 20b, the first porous metal layer 10a, the first mixed layer 20a, the electrode skeleton of the anode 30, and the electrolyte layer 40 are sintered bodies. The reducing gas flowing in the furnace may be a gas in which H2 (hydrogen) is diluted with a non-flammable gas (Ar (argon), He (helium), N2 (nitrogen), etc.), or may be a gas containing 100% H2. For safety reasons, it is preferable to set an upper limit up to the explosion limit. For example, in the case of a mixed gas of H2 and Ar, the concentration of H2 is preferably 4 volume % or less.
[0048] (Anode impregnation process) Next, the raw materials of the oxide ion conductive ceramics 33 and the catalytic metal 34 are impregnated into the electrode skeleton of the anode 30. For example, nitrates or chlorides of Zr, Y, Sc, Ce, Gd, and Ni are dissolved in water or alcohols (ethanol, 2-propanol, methanol, etc.) so that Gd-doped ceria or Sc, Y-doped zirconia and Ni are produced when fired at a predetermined temperature in a reducing atmosphere, and the half cell is impregnated, dried, and the heat treatment is repeated as many times as necessary.
[0049] (Intermediate layer formation process) The intermediate layer 50 is formed by depositing the oxide ion conductive ceramics (GDC, SDC, etc.) contained in the intermediate layer 50 on the electrolyte layer 40 by, for example, PVD (physical vapor deposition) or PLD (pulsed laser ablation deposition).
[0050] (Cathode material manufacturing process) For the cathode material, conductive ceramic powder such as lanthanum strontium cobaltite (LSC: LaSrCoO3) is mixed with a solvent (toluene, 2-propanol (IPA), 1-butanol, terpineol, butyl acetate, ethanol, etc., at 20 wt% to 30 wt% depending on the viscosity), a plasticizer (for example, adjusted to 1 wt% to 6 wt% to adjust the adhesion of the sheet), and a binder (PVB, acrylic resin, ethyl cellulose, etc.) to form a slurry. The volume ratio of the organic components (binder solids, plasticizer) to the LSC powder is, for example, in the range of 6:4 to 1:4.
[0051] (Cathode formation process) The cathode material is printed on the intermediate layer by screen printing. It is then sintered at 1000°C in a neutral atmosphere such as nitrogen. Through these steps, an oxide-based fuel cell is completed.
[0052] Second embodiment Fig. 4 is a schematic cross-sectional view illustrating the stack structure of the fuel cell 100a according to the second embodiment. As illustrated in Fig. 4, the fuel cell 100a differs from the fuel cell 100 according to the first embodiment in that a second porous metal layer 10b is provided on the opposite side of the second mixed layer 20b to the first porous metal layer 10a.
[0053] The fuel cell 100a can be produced by laminating the porous metal green sheet and the mixed layer green sheet in the following order: porous metal green sheet, mixed layer green sheet, porous metal green sheet, mixed layer green sheet.
[0054] The configuration of the second porous metal layer 10b is not particularly limited as long as it is a porous body mainly composed of metal, but it is preferably composed of the same material as the first porous metal layer 10a. The thickness of the second porous metal layer 10b is not particularly limited, but it is preferably the same thickness as the first porous metal layer 10a.
[0055] In this embodiment, the fuel cell 100a has a first porous metal layer 10a and a second porous metal layer 10b mainly composed of metal, and thus has a structure resistant to thermal shock, mechanical shock, and the like. Therefore, it is possible to suppress cracking during rapid temperature rise and fall of the fuel cell 100a. In addition, since the first mixed layer 20a and the second mixed layer 20b are provided at a distance from each other, it is possible to suppress the influence of the difference in thermal expansion coefficient between the electrolyte layer 40 and the first porous metal layer 10a and the second porous metal layer 10b. This suppresses warping of the fuel cell 100a.
[0056] Third embodiment Fig. 5 is a schematic cross-sectional view illustrating the stack structure of a fuel cell 100b according to the third embodiment. As illustrated in Fig. 5, the fuel cell 100b differs from the fuel cell 100a according to the second embodiment in that a third mixed layer 20c is further provided. The third mixed layer 20c is provided on the surface of the second porous metal layer 10b opposite to the second mixed layer 20b.
[0057] The fuel cell 100b can be produced by stacking the porous metal green sheets and the mixed layer green sheets in the following order: mixed layer green sheet, porous metal green sheet, mixed layer green sheet, porous metal green sheet, mixed layer green sheet.
[0058] The configuration of the third mixed layer 20c is not particularly limited as long as it is a mixture of a metal material and a ceramic material, but is preferably made of at least one of the materials of the first mixed layer 20a and the second mixed layer 20b. The thickness of the third mixed layer 20c is not particularly limited, but is preferably the same as that of at least one of the first mixed layer 20a and the second mixed layer 20b.
[0059] In this embodiment, the fuel cell 100b has a first porous metal layer 10a and a second porous metal layer 10b mainly composed of metal, and thus has a structure resistant to thermal shock, mechanical shock, and the like. Therefore, cracking during rapid temperature rise and fall of the fuel cell 100b can be suppressed. In addition, the first mixed layer 20a, the second mixed layer 20b, and the third mixed layer 20c are provided at a distance from each other, so that the influence of the difference in thermal expansion coefficient between the electrolyte layer 40 and the first porous metal layer 10a and the second porous metal layer 10b can be suppressed. This suppresses warping of the fuel cell 100b.
[0060] (Fourth embodiment) Fig. 6 is a schematic cross-sectional view illustrating the stack structure of a fuel cell 100c according to the fourth embodiment. As illustrated in Fig. 6, the fuel cell 100c differs from the fuel cell 100 according to the third embodiment in that a third porous metal layer 10c is further provided. The third porous metal layer 10c is provided on the surface of the third mixed layer 20c opposite to the second porous metal layer 10b.
[0061] The fuel cell 100b can be produced by stacking the porous metal green sheets and the mixed layer green sheets in the following order: porous metal green sheets, mixed layer green sheets, porous metal green sheets, mixed layer green sheets, porous metal green sheets, mixed layer green sheets.
[0062] The configuration of the third porous metal layer 10c is not particularly limited as long as it is a porous body mainly composed of metal, but it is preferable that it is composed of at least one of the first porous metal layer 10a and the second porous metal layer 10b. The thickness of the third porous metal layer 10c is not particularly limited, but it is preferable that it is the same thickness as at least one of the first porous metal layer 10a and the second porous metal layer 10b.
[0063] In this embodiment, the fuel cell 100c has a first porous metal layer 10a, a second porous metal layer 10b, and a third porous metal layer 10c, which are mainly composed of metal, and thus has a structure that is resistant to thermal shock, mechanical shock, and the like. Therefore, cracking during rapid temperature rise and fall of the fuel cell 100c can be suppressed. In addition, since the first mixed layer 20a, the second mixed layer 20b, and the third mixed layer 20c are provided at a distance from each other, the influence of the difference in thermal expansion coefficient between the electrolyte layer 40 and the first porous metal layer 10a and the second porous metal layer 10b can be suppressed. This suppresses warping of the fuel cell 100c. EXAMPLES
[0064] A fuel cell was fabricated according to the above embodiment.
[0065] Example 1 In Example 1, a fuel cell according to the first embodiment was produced. Ferritic stainless steel powder was used as the porous metal layer material. ScYSZ was used as the ceramic material for the electrolyte layer material. La-doped SrTiO3-based material was used as the electron conductive ceramic for the anode material, and ScYSZ was used as the oxide ion conductive ceramic. GDC was used as the ceramic material for the intermediate layer material. LSC was used as the ceramic material for the cathode material. La-doped SrTiO3-based material was used as the ceramic material for the mixed layer material. SUS was used as the metal material for the mixed layer material. A porous metal layer green sheet, a mixed layer green sheet, an anode green sheet, and an electrolyte layer green sheet were laminated on a mixed layer green sheet, cut to a predetermined size, and then heated to a temperature of 100°C. -16The anode was impregnated with GDC and Ni in a reducing atmosphere at or below 850°C. The anode was then fired in an air atmosphere at a temperature of 850°C or lower. 0.8 Gd 0.2 O 2-x The intermediate layer was then coated with the cathode material by screen printing or the like and dried. The cathode material was then sintered by heat treatment in an air atmosphere at a temperature of 1000°C or less to form a cathode. The shape in plan view was a square of 100 mm square.
[0066] Example 2 In Example 2, a fuel cell according to the third embodiment was produced. When stacking the green sheets, the mixed layer green sheet, the porous metal layer green sheet, the mixed layer green sheet, the anode green sheet, and the electrolyte layer green sheet were stacked on the mixed layer green sheet. The other conditions were the same as those of Example 1.
[0067] Example 3 In Example 3, a fuel cell according to the fourth embodiment was produced. When stacking the green sheets, the porous metal layer green sheet, the mixed layer green sheet, the porous metal layer green sheet, the mixed layer green sheet, the anode green sheet, and the electrolyte layer green sheet were stacked on the porous metal layer green sheet, the mixed layer green sheet, the porous metal layer green sheet, and the mixed layer green sheet. The other conditions were the same as in Example 1.
[0068] Example 4 In Example 4, a fuel cell according to the second embodiment was produced. When stacking the green sheets, the porous metal layer green sheet, the mixed layer green sheet, the anode green sheet, and the electrolyte layer green sheet were stacked on the porous metal layer green sheet and the mixed layer green sheet. The other conditions were the same as those of Example 1.
[0069] Comparative Example 1 In Comparative Example 1, when laminating each green sheet, the anode green sheet and the electrolyte layer green sheet were laminated on the porous metal layer green sheet and the mixed layer green sheet. Therefore, there was one porous metal layer and one mixed layer. The other conditions were the same as in Example 1.
[0070] Comparative Example 2 In Comparative Example 2, when laminating each green sheet, the anode green sheet and the electrolyte layer green sheet were laminated on the mixed layer green sheet. Therefore, the mixed layer was one layer without providing a porous metal layer. The other conditions were the same as those of Example 1.
[0071] (Evaluation of the amount of warpage) For each of the fuel cells of Examples 1 to 4 and Comparative Examples 1 and 2, the amount of warping due to differences in the shrinkage behavior of each layer during the firing process was measured. As illustrated in FIG. 7, the distance between both sides of the fuel cell that contact the surface when placed on a flat surface is defined as distance B. Distance B corresponds to one side of the rectangular shape of the fuel cell when viewed from above. The vertical distance from the apex of the warping to the flat surface is defined as distance A. The thickness of the fuel cell is defined as L (mm). In this case, the amount of warping (mm) is defined as (AL). The warping rate is defined as = (AL) / B.
[0072] The results are shown in Table 1. As shown in Table 1, in Examples 1 to 4, the amount of warping was less than 10 mm, the warping rate was less than 1 / 10, and warping was suppressed. This is believed to be because two or more mixed layers were provided spaced apart from each other, thereby suppressing the effect of the difference in thermal expansion coefficient between the porous metal layer and the electrolyte layer. The initial power generation characteristics were also good. In contrast, in Comparative Example 1, the amount of warping was large at 10 mm. This is believed to be because the mixed layer was a single layer, and therefore the effect of the difference in thermal expansion coefficient between the porous metal layer and the electrolyte layer could not be suppressed.
[0073] (Rapid temperature rise and fall test) A rapid temperature increase / decrease test was conducted on each of the fuel cells of Examples 1 to 4 and Comparative Examples 1 and 2. In the rapid temperature increase, the temperature was increased from room temperature to 750°C in 15 minutes. Therefore, the temperature increase rate was set to 50°C / min. In the rapid temperature decrease, the temperature was decreased from 750°C to room temperature in 15 minutes. Therefore, the temperature decrease rate was set to 50°C / min. If no cracks occurred, it was judged as "Good", and if cracks occurred, it was judged as "Poor".
[0074] The results are shown in Table 1. As shown in Table 1, in Examples 1 to 4, no cracks occurred even when a rapid temperature increase / decrease test was performed. This is believed to be because the provision of a porous metal layer mainly composed of metal resulted in a configuration that was resistant to thermal shock. In contrast, in Comparative Example 2, cracks occurred when the rapid temperature increase / decrease test was performed. This is believed to be because the absence of a porous metal layer resulted in a configuration that was resistant to thermal shock. [Table 1]
[0075] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to such specific embodiments, and various modifications and variations are possible within the scope of the gist of the present invention described in the claims. [Explanation of symbols]
[0076] 10a 1st porous metal layer 10b Second porous metal layer 10c 3rd porous metal layer 20a 1st mixed layer 20b 2nd mixed layer 20c 3rd mixed layer 21 Metal materials 22 Ceramic Materials 30 Anode 31 Electronically Conductive Ceramics 32 Oxide-ion conductive ceramics 33 Oxide-ion conductive ceramics 34 Catalytic Metals 40 Electrolyte layer 50 Middle Class 60 Cathode 100 fuel cell
Claims
1. A first porous metal layer containing a metal as a main component; a first mixed layer provided on the first porous metal layer and having a structure in which a metal material and a ceramic material are mixed; an anode provided on the first mixed layer and including a ceramic material; a second mixed layer provided under the first porous metal layer and having a structure in which a metal material and a ceramic material are mixed,
2. 2. The solid oxide fuel cell according to claim 1, wherein the first porous metal layer is composed only of metal.
3. 2. The solid oxide fuel cell according to claim 1, wherein the first porous metal layer is made of ferritic stainless steel.
4. The thermal expansion coefficient of the ceramic material of the first mixture layer and the second mixture layer is 10.5×10 -6 2. The solid oxide fuel cell according to claim 1, wherein the temperature is 0.15 to 1.5° C. or less.
5. 2. The solid oxide fuel cell according to claim 1, wherein the metallic material of the mixed layer is ferritic stainless steel.
6. 2. The solid oxide fuel cell according to claim 1, wherein a volume ratio of said ceramic material in said first mixed layer and said second mixed layer is 20 vol % or more and 80 vol % or less.
7. 2. The solid oxide fuel cell according to claim 1, wherein the first porous metal layer has a thickness greater than each of the first mixed layer and the second mixed layer.
8. The solid oxide fuel cell has a generally rectangular shape in a plan view, 2. The solid oxide fuel cell according to claim 1, wherein the amount of warping of said solid oxide fuel cell is less than 1 / 10 of the length of one side of said substantially rectangular shape.
9. 2. The solid oxide fuel cell according to claim 1, further comprising a second porous metal layer mainly composed of metal, below the second mixed layer.
Citation Information
Patent Citations
Metal supported solid oxide fuel cell
US20110104584A1
Clad porous metal substrate for electrochemical cell
US20230051172A1
Method for producing nio-ceramic composite powder and nio-ceramic composite fuel electrode
JP2013079190A
Metal support for electrochemical element, electrochemical element, electrochemical module, electrochemical device, energy system, solid oxide fuel cell, and solid oxide electrolytic cell
JP2021158026A