Separation membrane, and manufacturing method thereof
A crosslinked polyimide membrane addresses the issues of swelling and deterioration in conventional separation membranes, ensuring long-term performance stability and efficiency in separating water from mixed liquids.
Patent Information
- Application Number
- JP2023047133
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional separation membranes made of zeolite or PVA swell with high water content, reducing performance, while polyimide membranes deteriorate over time due to cracks and peeling, leading to decreased separation efficiency.
A separation membrane with a crosslinked polyimide functional layer that suppresses swelling and deterioration by using ionic or covalent bonds, enhancing durability and maintaining separation performance over time.
The crosslinked polyimide membrane effectively prevents swelling and peeling, maintaining high separation performance even after prolonged use, ensuring consistent efficiency in separating water from mixed liquids containing volatile organic compounds.
Smart Images

Figure 2024136141000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a separation membrane and a method for producing the same. [Background technology]
[0002] Pervaporation and vapor permeation have been developed as methods for separating water from a mixture containing volatile organic compounds and water. These methods are particularly suitable for separating water from azeotropic mixtures such as a mixture containing ethanol and water. Pervaporation is also advantageous in that it does not require vaporization of the mixture before treatment.
[0003] Materials for the separation membrane used in the pervaporation method include zeolite, polyvinyl alcohol (PVA), polyimide, etc. For example, Patent Document 1 discloses an example of a separation membrane containing polyimide. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2014-184424 A Summary of the Invention [Problem to be solved by the invention]
[0005] Zeolite and PVA are highly hydrophilic, so when the mixed liquid contains a high content of water, separation membranes made of zeolite or PVA may swell with water, causing a decrease in the separation performance of the separation membrane. On the other hand, polyimide is a material that can suppress swelling with water compared to zeolite and PVA. However, separation membranes containing conventional polyimide tend to show a significant decrease in separation performance after long-term use.
[0006] Therefore, an object of the present invention is to provide a separation membrane suitable for suppressing deterioration in separation performance when used for a long period of time. [Means for solving the problem]
[0007] As a result of intensive research, the present inventors have newly discovered that when a conventional separation membrane is used to separate water from a mixed liquid containing water for a long period of time, stripe-shaped cracks are generated on the surface of the separation functional layer of the separation membrane, and peeling occurs between the layers constituting the separation membrane, causing the separation membrane to deteriorate, and thus the separation performance of the separation membrane tends to decrease. Based on this knowledge, the present inventors have furthered their research and discovered that the above deterioration can be suppressed by using a crosslinked polyimide having a crosslinked structure as the material for the separation membrane, and have completed the present invention.
[0008] The present invention relates to A separation membrane for separating water from a mixed liquid containing a volatile organic compound and water, The separation membrane includes a separation functional layer including a crosslinked polyimide.
[0009] Further, the present invention relates to The method for producing the separation membrane, The manufacturing method includes: Applying a coating liquid containing polyimide onto a substrate to form a coating film; drying the coating film to form the crosslinked polyimide from the polyimide, thereby obtaining the separation functional layer; The present invention provides a method for producing a separation membrane, comprising the steps of: Effect of the Invention
[0010] According to the present invention, a separation membrane suitable for suppressing deterioration of separation performance when used for a long period of time can be provided. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a separation membrane according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view that illustrates a separation functional layer used for evaluating the gel fraction and the like. [Diagram 3] 1 is a schematic cross-sectional view of a membrane separation device equipped with a separation membrane of the present invention. [Figure 4] FIG. 11 is a perspective view that illustrates a modified example of a membrane separation device provided with a separation membrane of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The separation membrane according to the first aspect of the present invention is A separation membrane for separating water from a mixed liquid containing a volatile organic compound and water, The separation membrane includes a separation functional layer including a crosslinked polyimide.
[0013] In a second aspect of the present invention, for example, in the separation membrane according to the first aspect, the separation functional layer has a gel fraction of 80% or more.
[0014] In a third aspect of the present invention, for example, in the separation membrane according to the first or second aspect, the crosslinked polyimide is a polyimide crosslinked via an ionic bond or a covalent bond.
[0015] In a fourth aspect of the present invention, for example, in the separation membrane according to the third aspect, the polyimide has at least one functional group F selected from the group consisting of a carboxyl group, a hydroxyl group, a thiol group, and a sulfonic acid group.
[0016] In a fifth aspect of the present invention, for example, in the separation membrane according to the fourth aspect, the polyimide has a carboxyl group as the functional group F.
[0017] In a sixth aspect of the present invention, for example, in the separation membrane according to the fourth or fifth aspect, the crosslinked polyimide is formed by exchange of a dissociable proton contained in the functional group F with a metal ion.
[0018] In a seventh aspect of the present invention, for example, in the separation membrane according to the fourth or fifth aspect, the crosslinked polyimide is formed by reacting the functional group F with a crosslinking agent.
[0019] In an eighth aspect of the present invention, for example, in the separation membrane according to the seventh aspect, the crosslinking agent includes at least one selected from the group consisting of an epoxy-based crosslinking agent and an isocyanate-based crosslinking agent.
[0020] In a ninth aspect of the present invention, for example, in the separation membrane according to any one of the fourth to eighth aspects, the polyimide contains a structural unit X1 represented by the following formula (1). [ka] In the formula (1), A 1 is a tetravalent linking group, B 1 is a divalent linking group. 1 and B. 1 At least one selected from the group consisting of contains the functional group F.
[0021] In a tenth aspect of the present invention, for example, in the separation membrane according to the ninth aspect, the structural unit X1 is a structural unit X2 represented by the following formula (2). [ka] In the formula (2), A 2 and B. 1 are each independently a divalent linking group, R 1 ~R 6 are each independently a hydrogen atom or any substituent. 2 , B 1 and R 1 ~R 6 At least one selected from the group consisting of contains the functional group F.
[0022] In an eleventh aspect of the present invention, for example, in a separation membrane according to any one of the first to tenth aspects, the surface area A1 (cm 2 ) of the separation functional layer before carrying out the following test is 2 ) to the surface area A2 (cm 2 ) of the separation functional layer after the test 2) minus the area A1, is 10% or less. Test: The separation functional layer is immersed in a test liquid consisting of ethanol and water for one day, where the content of ethanol in the test liquid is 50 wt %, and the temperature of the test liquid is 60°C.
[0023] In a twelfth aspect of the present invention, for example, in a separation membrane according to any one of the first to eleventh aspects, the ratio R2 of the weight W2 (g) of the separation functional layer after conducting the test below minus the weight W1 (g) of the separation functional layer before the test is conducted is 10% or less. Test: The separation functional layer is immersed in a test liquid consisting of ethanol and water for one day, where the content of ethanol in the test liquid is 50 wt %, and the temperature of the test liquid is 60°C.
[0024] In a thirteenth aspect of the present invention, for example, the separation membrane according to any one of the first to twelfth aspects further comprises a porous support supporting the separation functional layer.
[0025] A method for producing a separation membrane according to a fourteenth aspect of the present invention includes the steps of: A method for producing a separation membrane according to any one of the first to thirteenth aspects, The manufacturing method includes: Applying a coating liquid containing polyimide onto a substrate to form a coating film; drying the coating film to form the crosslinked polyimide from the polyimide, thereby obtaining the separation functional layer; Includes.
[0026] The present invention will now be described in detail, but the following description is not intended to limit the present invention to a specific embodiment.
[0027] <Embodiments of separation membrane> As shown in Fig. 1, the separation membrane 10 of this embodiment includes a separation functional layer 1 containing a crosslinked polyimide. The separation membrane 10 is typically a membrane that allows water to preferentially permeate from a mixed liquid L containing a volatile organic compound C and water. Therefore, the separation membrane 10 can be used for separating water from the mixed liquid L described above.
[0028] The separation membrane 10 further includes, for example, an intermediate layer 2 and a porous support 3. The porous support 3 supports the separation functional layer 1. The intermediate layer 2 is disposed between the separation functional layer 1 and the porous support 3, and is in direct contact with both the separation functional layer 1 and the porous support 3.
[0029] (separation functional layer) The separation functional layer 1 is, for example, a layer that allows water to preferentially permeate from the above-mentioned mixed liquid L, and is typically a dense layer (non-porous layer) in which no pores can be detected when observed at a magnification of 5000 times using a scanning electron microscope (SEM).
[0030] As described above, the separation functional layer 1 includes a crosslinked polyimide. The crosslinked polyimide is, for example, polyimide P crosslinked via ionic or covalent bonds. In this specification, "polyimide P crosslinks via ionic bonds" means, for example, that polyimide P (more specifically, a plurality of polyimide P molecules) is coordinated to a metal ion to form an ionic bond, thereby forming a crosslinked structure. "polyimide P crosslinks via covalent bonds" means, for example, that polyimide P (more specifically, a plurality of polyimide P molecules) reacts with a crosslinking agent to form a covalent bond, thereby forming a crosslinked structure.
[0031] The polyimide P has at least one functional group F selected from the group consisting of, for example, a carboxyl group, a hydroxyl group, a thiol group, and a sulfonic acid group. The functional group F can function as a crosslinking point when synthesizing a crosslinked polyimide. From the viewpoint of ease of synthesis of the crosslinked polyimide and stability of the crosslinked polyimide, it is preferable that the polyimide P has a carboxyl group as the functional group F.
[0032] The polyimide P includes, for example, a structural unit X1 represented by the following formula (1). [ka]
[0033] In formula (1), A 1 is a tetravalent linking group, B 1 is a divalent linking group. 1 and B. 1 At least one selected from the group consisting of contains the functional group F described above.
[0034] The structural unit X1 is preferably a structural unit X2 represented by the following formula (2). [ka]
[0035] In formula (2), A 2 and B. 1 are each independently a divalent linking group, R 1 ~R 6 are each independently a hydrogen atom or any substituent. 2 , B 1 and R 1 ~R 6 At least one selected from the group consisting of contains the functional group F described above.
[0036] [A 2 A preferred form of In a preferred embodiment, in formula (2), A 2 For example, the main chain does not contain an arylene group and the solubility parameter according to the Fedors method is 5.0 (cal / cm 3 ) 1 / 2 As used herein, the "backbone" is a 2 The term "arylene group" refers to a divalent aromatic group having an aromatic ring composed of carbon atoms.2 It is preferable that A does not contain a heteroarylene group in the main chain. The term "heteroarylene group" refers to a divalent aromatic group having a heteroaromatic ring containing a heteroatom such as an oxygen atom, a nitrogen atom, or a sulfur atom. In particular, A 2 It is preferable that the formula (I) does not contain an aromatic ring or a heteroaromatic ring, and it is more preferable that the formula (I) does not contain a ring structure.
[0037] In this specification, the "solubility parameter by the Fedors method" may be referred to as the SP value. The "solubility parameter by the Fedors method" can be calculated from the following formula. In the following formula, δi is the SP value of the atom or atomic group of the i component. Δei is the evaporation energy of the atom or atomic group of the i component. Δvi is the molar volume of the atom or atomic group of the i component. δi[(cal / cm 3 ) 1 / 2 ]=(Δei / Δvi) 1 / 2
[0038] Details of the "Solubility Parameter by the Fedors Method" are disclosed, for example, in "Polymer Engineering and Science" by Robert F. Fedors, 1974, Vol. 14, No. 2, pp. 147-154.
[0039] In this form, A 2 The SP value is 5.0(cal / cm 3 ) 1 / 2 Greater than. A 2 In this case, such a high SP value tends to facilitate the penetration of water into the separation functional layer 1. 2 The SP value is preferably 8.5 (cal / cm 3 ) 1 / 2 More preferably, it is 11.0 (cal / cm 3 ) 1 / 2 More preferably, it is 12.0 (cal / cm 3 ) 1 / 2 That's all. 2 The upper limit of the SP value is not particularly limited, but is, for example, 30.0 (cal / cm 3 ) 1 / 214.0 (cal / cm 3 ) 1 / 2 It may be. A 2 A preferred example of the SP value is 12.68 (cal / cm 3 ) 1 / 2 etc.
[0040] A 2 For example, A contains at least one selected from the group consisting of an oxygen atom, a nitrogen atom, a sulfur atom, and a silicon atom. 2 A preferably contains at least one selected from the group consisting of an oxygen atom and a nitrogen atom, and particularly preferably contains an oxygen atom. 2 may contain, for example, the above-mentioned functional group F, or another functional group G such as an ether group, a carbonyl group, an amide group, a thioether group, or a sulfonyl group. Specific examples of the carbonyl group include an ester group and a ketone group. 2 It is preferable that the functional group G contains at least one selected from the group consisting of an ether group and an ester group, and it is more preferable that the functional group G contains an ester group.
[0041] A 2 may contain other groups, such as a hydrocarbon group, in addition to the functional group F or G. The number of carbon atoms in the hydrocarbon group is not particularly limited, but is, for example, 1 to 15, preferably 1 to 5, and more preferably 1 to 3. A 2 It is preferable that the divalent hydrocarbon group, particularly an alkylene group, is contained. Examples of the divalent hydrocarbon group include a methylene group, an ethylene group, a propane-1,3-diyl group, a propane-2,2-diyl group, a butane-1,4-diyl group, a pentane-1,5-diyl group, and a 2,2-dimethylpropane-1,3-diyl group, and an ethylene group is preferable. At least one hydrogen atom contained in these hydrocarbon groups may be substituted with a halogen atom.
[0042] A 2 is, for example, the general formula -OR 7 -O- or the general formula -COO-R 8A linking group represented by the general formula -OOC-, in particular -COO-R 8 Preferably, R is a linking group represented by -OOC-. 7 and R 8 is a divalent hydrocarbon group having 1 to 15 carbon atoms. Examples of the divalent hydrocarbon group include those mentioned above.
[0043] A 2 The SP value is 5.0 (cal / cm 3 ) 1 / 2 As long as the linking group is larger than the functional group F, it does not have to include the functional group G. 2 Examples of the alkylene group include an alkylene group. The number of carbon atoms in the alkylene group is not particularly limited, and may be, for example, 1 to 15, or 1 to 5. The alkylene group may be branched, but is preferably linear. The alkylene group may have some of its hydrogen atoms substituted with halogen atoms, but is preferably in an unsubstituted state, that is, a linear or branched alkylene group itself.
[0044] In formula (2), A 2 Among the bond chains connecting two phthalimide structures linked by A, the number of atoms constituting the bond chain with the smallest number of atoms is, for example, 2 or more, preferably 4 or more, and more preferably 6 to 11. In this specification, the bond chain with the smallest number of atoms may be referred to as the "shortest bond chain." Suppose A 2 is a propane-1,3-diyl group, A 2 The number of atoms constituting the shortest bond between two phthalimide structures connected by A is 3. 2 is a propane-2,2-diyl group, A 2 The number of atoms constituting the shortest bond between the two phthalimide structures linked by is 1.
[0045] A 2A may be one of the linking groups 1 to 16 shown in Table 1 below. Table 1 also shows the chemical structure, SP value, and number of atoms constituting the shortest bond chain for each of the linking groups 1 to 16. 2 is preferably a linking group 12. 2 is the linking group 12, the polyimide P is easily dissolved in a polar organic solvent such as N-methyl-2-pyrrolidone (NMP), and the desired manufacturing method for the separation functional layer 1 is easily applicable.
[0046] [Table 1]
[0047] [A 2 Another preferred form of In another preferred embodiment, in formula (2), A 2 is a linking group containing an arylene group in the main chain. The aromatic ring contained in the arylene group may be polycyclic, but is preferably monocyclic. The number of carbon atoms in the aromatic ring is not particularly limited, but is, for example, 6 to 14. Examples of the aromatic ring include a benzene ring, a naphthalene ring, an anthracene ring, and a phenanthrene ring.
[0048] A 2 In the above, the aromatic ring contained in the arylene group may or may not have a substituent. Examples of the substituent include the above functional group F, a halogen atom, an alkoxy group having 1 to 30 carbon atoms, and a hydrocarbon group having 1 to 30 carbon atoms. The alkoxy group and the hydrocarbon group may be either linear or branched. The number of carbon atoms in the alkoxy group and the hydrocarbon group is preferably 1 to 20, more preferably 1 to 10, and particularly preferably 1 to 5. Examples of the alkoxy group include a methoxy group, an ethoxy group, and a propoxy group. Examples of the hydrocarbon group include a methyl group, an ethyl group, and a propyl group. At least one hydrogen atom contained in the alkoxy group and the hydrocarbon group may be substituted with a halogen atom. When the aromatic ring has a plurality of substituents, the plurality of substituents may be the same as or different from each other.
[0049] A 2 In the above, the arylene group is preferably a phenylene group which may have a substituent or a naphthalenediyl group which may have a substituent, and more preferably a phenylene group which may have a substituent. When the arylene group is a phenylene group which may have a substituent, it is preferably represented by the following formula (3). Formula (3) shows a p-phenylene structure. A polyimide having a p-phenylene structure is not three-dimensionally bulky compared to polyimides having an o-phenylene structure or an m-phenylene structure, and is suitable for improving the separation performance of the separation membrane 10. [ka]
[0050] In formula (3), R 9 ~R 12 are each independently a hydrogen atom or an arbitrary substituent. Examples of the arbitrary substituent include the above-mentioned functional group F, a halogen atom, an alkoxy group having 1 to 30 carbon atoms, and a hydrocarbon group having 1 to 30 carbon atoms. Examples of the alkoxy group and the hydrocarbon group include those described above.
[0051] A 2 In addition to the arylene group, A may contain at least one atom selected from the group consisting of an oxygen atom, a nitrogen atom, a sulfur atom, and a silicon atom. 2 A preferably contains at least one selected from the group consisting of an oxygen atom and a nitrogen atom, and particularly preferably contains an oxygen atom. 2 may contain, for example, the above-mentioned functional group F, or other functional groups G, such as ether groups, carbonyl groups, amide groups, thioether groups, and sulfonyl groups. 2 It is preferable that the functional group G contains at least one selected from the group consisting of an ether group and an ester group, and it is more preferable that the functional group G contains an ether group.
[0052] A 2 is, for example, the general formula -OR13 -O- or the general formula -COO-R 14 -OOC-, in particular, a linking group represented by the general formula -OR 13 Preferably, R is a linking group represented by -O-. 13 and R 14 is a divalent hydrocarbon group containing an arylene group in the main chain. The number of carbon atoms in this hydrocarbon group is, for example, 6 to 15. Examples of the hydrocarbon group include a 1,4-phenylene group, a 2,5-di-tert-butyl-1,4-phenylene group, a 1-methyl-1,1-ethanediylbis(1,4-phenylene) group, and a biphenyl-4,4'-diyl group.
[0053] In formula (2), A 2 The SP value of the linking group represented by the formula is, for example, 5.0 (cal / cm 3 ) 1 / 2 Greater than. A 2 In this case, such a high SP value tends to facilitate the penetration of water into the separation functional layer 1. 2 The SP value is preferably 8.5 (cal / cm 3 ) 1 / 2 More preferably, it is 11.0 (cal / cm 3 ) 1 / 2 That's all. 2 The upper limit of the SP value is not particularly limited, but is, for example, 30.0 (cal / cm 3 ) 1 / 2 14.0 (cal / cm 3 ) 1 / 2 It may be. A 2 A preferred example of the SP value is 11.02 (cal / cm 3 ) 1 / 2 etc.
[0054] In formula (2), A 2 Among the bonding chains connecting two phthalimide structures linked by, the number of atoms constituting the bonding chain with the smallest number of atoms is, for example, 6 or more, and preferably 10 or more. The upper limit of this number of atoms is not particularly limited and is, for example, 15.
[0055] A2 A may be one of the linking groups 17 to 26 shown in Table 2 below. Table 2 also shows the chemical structure, SP value, and number of atoms constituting the shortest bond chain for each of the linking groups 17 to 26. 2 is preferably a linking group 19. 2 is the linking group 19, the polyimide P is easily dissolved in a polar organic solvent such as N-methyl-2-pyrrolidone (NMP), and the desired manufacturing method for the separation functional layer 1 is easily applicable.
[0056] [Table 2]
[0057] [R 1 ~R 6 ] In formula (2), R 1 ~R 6 are each independently a hydrogen atom or an arbitrary substituent. Examples of the arbitrary substituent include the above-mentioned functional group F, a halogen atom, an alkoxy group having 1 to 30 carbon atoms, and a hydrocarbon group having 1 to 30 carbon atoms. 1 ~R 6 At least one of these may be the functional group F, and R 2 and R 5 Each of A may be the above-mentioned functional group F (particularly a carboxyl group). As the alkoxy group and the hydrocarbon group, A 2 The above-mentioned items can be mentioned.
[0058] In addition, R 2 and R 3 , and R 5 and R 6 may be bonded to each other to form a ring structure. The ring structure is, for example, a benzene ring.
[0059] [B 1 A preferred form of In a preferred embodiment, B 1 is expressed, for example, by the following formula (4). -Ar 1 -B 2-Ar 2 - (4)
[0060] In formula (4), B 2 is a divalent linking group. This linking group has, for example, an SP value of 8.56 (cal / cm 3 ) 1 / 2 Greater than. 2 In this case, such a high SP value tends to facilitate the penetration of water into the separation functional layer 1. 2 The SP value is preferably 9.0 (cal / cm 3 ) 1 / 2 More preferably, it is 11.0 (cal / cm 3 ) 1 / 2 More preferably, it is 12.0 (cal / cm 3 ) 1 / 2 More preferably, it is 14.0 (cal / cm 3 ) 1 / 2 That's all. B 2 The upper limit of the SP value is not particularly limited, but is, for example, 30.0 (cal / cm 3 ) 1 / 2 It may be. B 2 A preferred example of the SP value is 14.51 (cal / cm 3 ) 1 / 2 etc.
[0061] B 2 For example, B contains at least one selected from the group consisting of an oxygen atom, a nitrogen atom, a sulfur atom, and a silicon atom. 2 B preferably contains at least one selected from the group consisting of an oxygen atom and a nitrogen atom, and particularly preferably contains an oxygen atom. 2 contains, for example, the functional group F described above and other functional groups G such as ether groups, carbonyl groups, amide groups, thioether groups, sulfonyl groups, etc. 2 It is preferable that the functional group G contains at least one selected from the group consisting of an ether group and a carbonyl group, and it is more preferable that the functional group G contains an ether group.
[0062] B 2may contain other groups, such as hydrocarbon groups, in addition to the functional groups F and G. 2 In the above, the hydrocarbon group may contain an arylene group. 2 The above-mentioned items can be mentioned. 2 A 2 It may be the same as or different from.
[0063] In formula (4), B 2 Ar linked by 1 and Ar 2 Among the bonding chains connecting the bonding chains, the number of atoms constituting the bonding chain with the smallest number of atoms (shortest bonding chain) is, for example, 1 or more. The upper limit of the number of atoms constituting the shortest bonding chain is not particularly limited, but may be 12 or 5. The number of atoms constituting the shortest bonding chain is preferably 1.
[0064] B 2 may be one of the linking groups 1 to 16 shown in Table 1 above, or may be one of the linking groups 17 to 26 shown in Table 2. 2 is preferably one of the linking groups 5 to 26, more preferably the linking group 13, the linking group 18 or the linking group 22, and particularly preferably the linking group 13.
[0065] In formula (4), Ar 1 and Ar 2 is a divalent aromatic group. The divalent aromatic group has an aromatic ring composed of carbon atoms or a heteroaromatic ring containing a heteroatom, and preferably has an aromatic ring composed of carbon atoms. The nitrogen atom contained in the phthalimide structure of formula (2) is 1 Aromatic rings (or heteroaromatic rings) contained in, or Ar 2 In the formula (4), B is preferably directly bonded to an aromatic ring (or a heteroaromatic ring). 2 Ar 1 Aromatic rings (or heteroaromatic rings) contained in, and Ar 2 may be directly bonded to each of the aromatic rings (or heteroaromatic rings) contained in
[0066] Ar 1 and Ar 2 In the above, the aromatic ring (or heteroaromatic ring) may be polycyclic, but is preferably monocyclic. The number of carbon atoms in the aromatic ring (or heteroaromatic ring) is not particularly limited, and may be, for example, 4 to 14 or 6 to 10. Examples of the aromatic ring and heteroaromatic ring include a benzene ring, a naphthalene ring, an anthracene ring, a phenanthrene ring, a furan ring, a pyrrole ring, a pyridine ring, and a thiophene ring.
[0067] Ar 1 and Ar 2 In the above, the aromatic ring (or heteroaromatic ring) may or may not have a substituent. Examples of the substituent include the above-mentioned functional group F, a halogen atom, an alkoxy group having 1 to 30 carbon atoms, and a hydrocarbon group having 1 to 30 carbon atoms. Examples of the alkoxy group and the hydrocarbon group include A 2 When the aromatic ring (or heteroaromatic ring) has a plurality of substituents, the plurality of substituents may be the same or different.
[0068] Ar 1 and Ar 2 is preferably a phenylene group which may have a substituent, or a naphthalenediyl group which may have a substituent. 1 and Ar 2 When is an optionally substituted phenylene group, it is preferably represented by the above formula (3).
[0069] Ar 1 and Ar 2 In the above, the naphthalenediyl group which may have a substituent has, for example, a naphthalene-2,6-diyl structure, a naphthalene-1,4-diyl structure, a naphthalene-1,5-diyl structure or a naphthalene-1,8-diyl structure. A specific example of the naphthalenediyl group which may have a substituent is a naphthalene-2,6-diyl group.
[0070] Ar1 and Ar 2 and may be the same or different. 1 is a naphthalene-2,6-diyl group, and Ar 2 may be a p-phenylene group.
[0071] [B 1 Another preferred form of In another preferred embodiment, B 1 is expressed, for example, by the following formula (5). -Ar 3 - (5)
[0072] In formula (5), Ar 3 is a divalent aromatic group. The divalent aromatic group has an aromatic ring composed of carbon atoms or a heteroaromatic ring containing a heteroatom, and preferably has an aromatic ring composed of carbon atoms. The nitrogen atom contained in the phthalimide structure of formula (2) is 3 It is preferable that the aromatic ring (or heteroaromatic ring) is directly bonded to the aromatic ring (or heteroaromatic ring) contained in the above.
[0073] Ar 3 In the above, the aromatic ring (or heteroaromatic ring) may be polycyclic, but is preferably monocyclic. The number of carbon atoms in the aromatic ring (or heteroaromatic ring) is not particularly limited, and may be, for example, 4 to 14 or 6 to 10. Examples of the aromatic ring and heteroaromatic ring include Ar 1 and Ar 2 The above-mentioned items can be mentioned.
[0074] Ar 3 In the above, the aromatic ring (or heteroaromatic ring) may or may not have a substituent. Examples of the substituent include the above-mentioned functional group F, a halogen atom, an alkoxy group having 1 to 30 carbon atoms, and a hydrocarbon group having 1 to 30 carbon atoms. Examples of the alkoxy group and the hydrocarbon group include A 2 When the aromatic ring (or heteroaromatic ring) has a plurality of substituents, the plurality of substituents may be the same or different.
[0075] Ar 3 Examples of Ar include an optionally substituted phenylene group, an optionally substituted naphthalenediyl group, and an optionally substituted biphenylene group. 3 When is an optionally substituted phenylene group, it is preferably represented by the following formula (6). [ka]
[0076] In formula (6), R 23 ~R 26 are each independently a hydrogen atom or an arbitrary substituent. Examples of the arbitrary substituent include the above-mentioned functional group F, a halogen atom, an alkoxy group having 1 to 30 carbon atoms, and a hydrocarbon group having 1 to 30 carbon atoms. In particular, R 23 ~R 26 At least one of the functional groups F is preferably the functional group F. 25 is preferably the above-mentioned functional group F (particularly a carboxyl group). As the alkoxy group and the hydrocarbon group, A 2 Examples of the linking group represented by formula (6) include those mentioned above. A specific example of the linking group represented by formula (6) is a 5-carboxy-1,3-phenylene group. This linking group is derived from diaminobenzoic acid (3,5-diaminobenzoic acid). Polyimide P containing a structural unit derived from diaminobenzoic acid is suitable for increasing the flux of water that permeates the separation membrane 10.
[0077] The structural unit X2 preferably includes at least one selected from the group consisting of a structural unit X3 represented by the following formula (7) and a structural unit X4 represented by the following formula (8), and particularly preferably includes the structural unit X4. [ka]
[0078] In equation (7), A 2 , B 2 and R 1 ~R6 is the same as described above for equations (2) and (4). 15 ~R 22 are each independently a hydrogen atom or an arbitrary substituent. Examples of the arbitrary substituent include the above-mentioned functional group F, a halogen atom, an alkoxy group having 1 to 30 carbon atoms, and a hydrocarbon group having 1 to 30 carbon atoms. 15 ~R 22 is preferably a hydrogen atom.
[0079] In equation (8), A 2 , R 1 ~R 6 and R 23 ~R 26 is the same as described above for equations (2) and (6).
[0080] The polyimide P contains, for example, the structural unit X1 (particularly, the structural units X2 to X4) as a main component. In this specification, the term "main component" refers to the structural unit contained in the polyimide P in the largest amount on a molar basis. The content of the structural unit X1 (particularly, the structural units X2 to X4) in the polyimide P is, for example, 50 mol% or more, and may be 60 mol% or more, 70 mol% or more, 80 mol% or more, 90 mol% or more, or even 100 mol%. However, the content of the structural unit X1 in the polyimide P may be less than 50 mol% in some cases. The polyimide P may contain one type of the structural unit X1 (particularly, the structural units X2 to X4) alone, or may contain two or more types. As an example, the polyimide P may contain A 2 A is a structural unit X2 that does not have an arylene group in the main chain, 2 The polyimide P may contain both a structural unit X1 containing an arylene group in its main chain and a structural unit X2 containing an arylene group in its main chain. The polyimide P may contain a structural unit not containing the functional group F, together with a structural unit containing the functional group F. The structural unit not containing the functional group F may have the same structure as the structural unit X1 (particularly the structural units X2 to X4) described above, except that it does not contain the functional group F.
[0081] As an example, polyimide P can be obtained by reacting tetracarboxylic dianhydride C1 represented by the following formula (9) with diamine D1 represented by the following formula (10). 1 is the same as equation (1). In equation (10), B 1 is the same as equation (1). [ka]
[0082] The tetracarboxylic dianhydride C1 is preferably a tetracarboxylic dianhydride C2 represented by the following formula (11). 2 and R 1 ~R 6 is the same as equation (2). [ka]
[0083] The tetracarboxylic dianhydride C1 may be a tetracarboxylic dianhydride other than the above-mentioned tetracarboxylic dianhydride C2 (for example, pyromellitic dianhydride).
[0084] Diamine D1 is preferably diamine D2 represented by the following formula (12) or diamine D3 represented by the following formula (13). 2 , Ar 1 and Ar 2 is the same as formula (4). In formula (13), Ar 3 is the same as equation (5). H2N-Ar 1 -B 2 -Ar 2 -NH2(12) H2N-Ar 3 -NH2(13)
[0085] The diamine D1 may be a diamine other than the above diamines D2 and D3.
[0086] The weight average molecular weight (Mw) of the polyimide P is not particularly limited, and is, for example, 5×10 4 More than 7×10 4 More preferably, it is 10×10 4 More preferably, it is 15×10 4 That is all. The larger the weight average molecular weight of polyimide P, the higher the durability of separation membrane 10 tends to be. The upper limit of the weight average molecular weight of polyimide P is not particularly limited, and is, for example, 1×10 6 The weight average molecular weight of polyimide P can be calculated, for example, by measuring the molecular weight distribution of polyimide P using a gel permeation chromatograph (GPC) equipped with a refractive index detector (RID) and using a calibration curve based on standard polystyrene from the obtained chromatogram (chart).
[0087] In a preferred embodiment, the crosslinked polyimide is formed, for example, by exchanging a dissociable proton contained in a functional group F in the polyimide P with a metal ion (more specifically, a metal cation). This crosslinked polyimide is suitable for increasing the flux of water passing through the separation membrane 10. When the dissociable proton is exchanged with a metal ion, the polyimide P is coordinated to the metal ion via the functional group F, forming an ionic bond. A crosslinked structure is formed by coordinating a plurality of polyimide P molecules to the metal ion via the functional group F.
[0088] The metal constituting the metal ion is not particularly limited, and examples thereof include Li, Na, K, Be, Mg, Ca, Ba, Sc, Y, Ti, Zr, V, Cr, Mo, Mn, Fe, Co, Ni, Cu, Ag, Zn, B, Al, Ga, In, Pb, etc., and are preferably Mg, Fe, Al, and Ga, and particularly preferably Al. The metal constituting the metal ion may be Na, Ca, etc.
[0089] The valence of the metal ion is, for example, 1 or more, preferably 2 or more, and more preferably 3 or more.
[0090] In another preferred embodiment, the crosslinked polyimide is formed, for example, by reacting a functional group F in the polyimide P with a crosslinking agent. This crosslinked polyimide tends to further suppress the deterioration of the separation performance when the separation membrane 10 is used for a long period of time. Furthermore, the structure and performance of the crosslinked polyimide tend to be easily adjusted depending on the type of crosslinking agent.
[0091] As an example, the functional group F reacts with the functional group H contained in the crosslinking agent to form a covalent bond between the functional group F and the crosslinking agent. In a plurality of polyimide P molecules, the functional group F reacts with the functional group H of the crosslinking agent to form a crosslinked structure. In this case, the crosslinked polyimide usually has a crosslinked structure in which a plurality of polyimide P molecules are indirectly bonded to each other via the crosslinking agent. However, the crosslinking agent may be a condensing agent that forms a crosslinked structure by promoting a condensation reaction between the functional groups F in the plurality of polyimide P molecules. In this specification, such a condensing agent is also classified as a crosslinking agent that reacts with the functional group F. When a condensing agent is used, the crosslinked polyimide usually has a crosslinked structure in which a plurality of polyimide P molecules are directly bonded to each other.
[0092] Examples of the crosslinking agent containing a functional group H include an epoxy-based crosslinking agent, an isocyanate-based crosslinking agent, an amine-based crosslinking agent, etc. The crosslinking agent preferably contains at least one selected from the group consisting of an epoxy-based crosslinking agent and an isocyanate-based crosslinking agent, and more preferably contains an epoxy-based crosslinking agent.
[0093] The epoxy crosslinking agent is a compound (epoxy compound) containing an epoxy group as a functional group H. The number of epoxy groups contained in the epoxy compound is typically 2 or more, and may be 3 to 5. The epoxy compounds may be used alone or in combination of two or more.
[0094] Specific examples of epoxy compounds include N,N,N',N'-tetraglycidyl-m-xylylenediamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, 1,6-hexanediol diglycidyl ether, polyethylene glycol diglycidyl ether, and polyglycerol polyglycidyl ether.
[0095] Commercially available epoxy crosslinking agents include "TETRAD-C" and "TETRAD-X" manufactured by Mitsubishi Gas Chemical Company, Inc., "Epiclon CR-5L" manufactured by DIC Corporation, "Denacol EX-512" manufactured by Nagase ChemteX Corporation, and "TEPIC-G" manufactured by Nissan Chemical Industries, Ltd.
[0096] The isocyanate-based crosslinking agent is a compound (isocyanate compound) containing an isocyanate group as a functional group H. The number of isocyanate groups contained in the isocyanate compound is typically 2 or more, and may be 3 to 5. The isocyanate compounds may be used alone or in combination of two or more.
[0097] Examples of the isocyanate compound include an aliphatic isocyanate compound, an alicyclic isocyanate compound, and an aromatic isocyanate compound.
[0098] Examples of the aliphatic isocyanate compound include 1,2-ethylene diisocyanate; tetramethylene diisocyanates such as 1,2-tetramethylene diisocyanate, 1,3-tetramethylene diisocyanate, and 1,4-tetramethylene diisocyanate; hexamethylene diisocyanates such as 1,2-hexamethylene diisocyanate, 1,3-hexamethylene diisocyanate, 1,4-hexamethylene diisocyanate, 1,5-hexamethylene diisocyanate, 1,6-hexamethylene diisocyanate, and 2,5-hexamethylene diisocyanate; 2-methyl-1,5-pentane diisocyanate, 3-methyl-1,5-pentane diisocyanate, and lysine diisocyanate.
[0099] Examples of the alicyclic isocyanate compound include isophorone diisocyanate; cyclohexyl diisocyanates such as 1,2-cyclohexyl diisocyanate, 1,3-cyclohexyl diisocyanate, and 1,4-cyclohexyl diisocyanate; cyclopentyl diisocyanates such as 1,2-cyclopentyl diisocyanate and 1,3-cyclopentyl diisocyanate; hydrogenated xylylene diisocyanate, hydrogenated tolylene diisocyanate, hydrogenated diphenylmethane diisocyanate, hydrogenated tetramethylxylene diisocyanate, and 4,4'-dicyclohexylmethane diisocyanate.
[0100] Examples of aromatic isocyanate compounds include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, 4,4'-diphenylether diisocyanate, 2-nitrodiphenyl-4,4'-diisocyanate, 2,2'-diphenylpropane-4,4'-diisocyanate, 3, Examples of the diisocyanate include 3'-dimethyldiphenylmethane-4,4'-diisocyanate, 4,4'-diphenylpropane diisocyanate, m-phenylene diisocyanate, p-phenylene diisocyanate, naphthylene-1,4-diisocyanate, naphthylene-1,5-diisocyanate, 3,3'-dimethoxydiphenyl-4,4'-diisocyanate, xylylene-1,4-diisocyanate, and xylylene-1,3-diisocyanate.
[0101] Examples of the isocyanate-based crosslinking agent include polymers (dimers, trimers, pentamers, etc.) of the above-mentioned isocyanate compounds, adducts obtained by adding them to polyhydric alcohols such as trimethylolpropane, urea-modified products, biuret-modified products, allophanate-modified products, isocyanurate-modified products, carbodiimide-modified products, and urethane prepolymers obtained by adding them to polyether polyols, polyester polyols, acrylic polyols, polybutadiene polyols, polyisoprene polyols, and the like.
[0102] Commercially available isocyanate crosslinking agents include, for example, Duranate TPA-100 manufactured by Asahi Kasei Chemicals Corporation, and Coronate L, Coronate HL, Coronate HK, Coronate HX, and Coronate 2096 manufactured by Tosoh Corporation.
[0103] The amine-based crosslinking agent is a compound (amine compound) containing an amino group as a functional group H. The number of amino groups contained in the amine compound is typically 2 or more, and may be 3 or more. The amine compound may be used alone or in combination of two or more.
[0104] Specific examples of the amine compound include aziridine and polyethyleneimine.
[0105] Examples of cross-linking agents that function as condensing agents include acidic compounds such as Eaton's reagent (a mixture of P2O5 and methanesulfonic acid) and polyphosphoric acid.
[0106] The content of crosslinked polyimide in the separation functional layer 1 is, for example, 50 wt% or more, and may be 60 wt% or more, 70 wt% or more, 80 wt% or more, 90 wt% or more, or even 95 wt% or more. The separation functional layer 1 may be substantially composed of crosslinked polyimide only. However, the separation functional layer 1 may contain uncrosslinked polyimide P in addition to the crosslinked polyimide.
[0107] The separation functional layer 1 may contain a filler in addition to the crosslinked polyimide. The filler is, for example, hydrophilic and porous. Such a filler is suitable for increasing the flux of water passing through the separation membrane 10 without significantly reducing the separation performance of the separation membrane 10. The filler contains, for example, at least one selected from the group consisting of zeolite and metal-organic framework (MOF). From the viewpoint of durability against water, the filler preferably contains a metal-organic framework, but may not contain one. Examples of zeolites include molecular sieves 3A, 4A, 5A and 13X.
[0108] The metal organic framework is also called a porous coordination polymer (PCP). The metal organic framework contains, for example, metal ions and organic ligands. Examples of the metal ions include Co ions, Ni ions, Zn ions, Mg ions, Zr ions, and Cu ions. The organic ligand does not need to have a polar group, but preferably has a polar group. Examples of the polar group include an aldehyde group, an amino group, an amide group, a hydroxyl group, a carboxyl group, and a nitro group. The organic ligand contains, for example, an aromatic ring. Examples of the aromatic ring contained in the organic ligand include a benzene ring and an imidazole ring. Examples of the organic ligand include 2-hydroxymethylimidazole, 2-formylimidazole, terephthalic acid, 2-hydroxyterephthalic acid, 2,5-dihydroxyterephthalic acid, and 2-aminoterephthalic acid.
[0109] Examples of the metal organic framework include ZIF-90, ZIF-91, UiO-66, UiO-66-NH2, UiO-66-OH, UiO-66-NO2, UiO-66-COOH, HKUST-1, and MOF-74 (M=Co, Ni, Zn, Mg, etc.). From the viewpoint of increasing the flux of water permeating the separation membrane 10, the metal organic framework preferably contains at least one selected from the group consisting of ZIF-90, UiO-66-NH2, UiO-66-OH, UiO-66-NO2, UiO-66-COOH, and MOF-74(Ni), and more preferably contains UiO-66-COOH.
[0110] A filler capable of adsorbing water is suitable. In particular, a filler that is more likely to adsorb water than ethanol is suitable. The ratio R3 of the amount of water adsorbed Q2 to the filler under water vapor at 25°C and 3.2 kPa to the amount of ethanol adsorbed Q1 to the filler under an ethanol atmosphere at 25°C and 7.4 kPa is, for example, 2.0 or more, preferably 3.0 or more. The upper limit of the ratio R3 is not particularly limited, and is, for example, 5.0. The ratio R3 may be used as an index of the hydrophilicity of the filler. In this specification, the "adsorption amount" means the value obtained by converting the volume of gas adsorbed by 1 g of the filler into the standard state (298 K, 1 atm).
[0111] The amount of ethanol adsorption Q1 to the filler can be specified by the following method. First, the filler is pretreated by heating it under a reduced pressure atmosphere. The pretreatment may be performed under a vacuum atmosphere. The temperature of the pretreatment is, for example, 100° C. or higher. The time of the pretreatment is not particularly limited, and is, for example, 1 hour or more. Next, the filler is set in a known vapor adsorption amount measuring device such as BELSORP-maxII manufactured by Microtrack Bell. Next, gaseous ethanol is introduced into the measuring device at a measuring temperature of 25° C. The introduced gaseous ethanol is adsorbed by the filler. The gaseous ethanol is introduced until the pressure of the ethanol in the measuring device reaches 7.4 kPa. 7.4 kPa corresponds to the equilibrium vapor pressure (saturated vapor pressure) of ethanol at 25° C. After it is confirmed that the adsorption of ethanol by the filler has reached an equilibrium state, the amount of ethanol adsorption by the filler is specified. It can be determined that the adsorption of ethanol by the filler has reached an equilibrium state by the change in the pressure of ethanol in the measuring device. For example, when the change in the pressure of ethanol in the measuring device is 40 Pa or less in 500 seconds, it can be determined that the adsorption of ethanol by the filler has reached an equilibrium state. The amount of adsorption of ethanol determined by the above method can be regarded as the amount of adsorption Q1.
[0112] The amount of water adsorbed by the filler, Q2, can be determined by the following method. First, the filler is subjected to the above-mentioned pretreatment. The filler is set in the vapor adsorption measurement device. Next, water vapor is introduced into the measurement device at a measurement temperature of 25°C. The introduction of water vapor is continued until the pressure of the water vapor in the measurement device reaches 3.2 kPa. 3.2 kPa corresponds to the equilibrium vapor pressure of water at 25°C. After it is confirmed that the adsorption of water by the filler has reached an equilibrium state, the amount of water adsorbed by the filler is determined. The determined amount of water adsorbed can be regarded as the adsorption amount Q2.
[0113] The amount of ethanol adsorbed on the filler, Q1, is, for example, 200 cm 3 / g or less. The lower limit of the adsorption amount Q1 is not particularly limited, and is 90 cm 3 / g, 100 cm 3 The amount of water adsorbed by the filler, Q2, may be, for example, 300 cm 3 / g or more, and in some cases 350 cm 3 / g or more, and 3 / g or more, and 3 / g or more, and 3 The upper limit of the adsorption amount Q2 is not particularly limited, and may be, for example, 800 cm 3 / g.
[0114] The filler may have a ratio R4 of the BET (Brunauer-Emmett-Teller) specific surface area S2 by water vapor adsorption to the BET specific surface area S1 by nitrogen gas adsorption of 0.005 or more. The ratio R4 may be used as an index of the hydrophilicity of the filler. In the filler, the ratio R4 is, for example, 0.01 or more, preferably 0.1 or more, more preferably 0.2 or more, and even more preferably 0.3 or more. The ratio R4 may be 25 or less, 10 or less, 1.0 or less, or 0.6 or less.
[0115] The filler has a BET specific surface area S1 determined by nitrogen gas adsorption of, for example, 1500 m 2 / g or less, preferably 1000m 2 / g or less, and in some cases 900m 2 / g or less. The specific surface area S1 is 30 m 2 / g or more, 2 The filler may have a BET specific surface area S2 determined by water vapor adsorption of, for example, 10 m 2 / g or more, preferably 100m 2 / g or more, more preferably 150m 2 / g or more, and in some cases 200m 2 / g or more. The specific surface area S2 is 1000 m 2 / g or less, and 2 / g or less, and2 / g or less.
[0116] The shape of the filler is not particularly limited, and is, for example, particulate. In this specification, "particulate" includes spherical, ellipsoidal, scaly, fibrous, and the like. The average particle size of the filler is not particularly limited, and is, for example, 5 nm to 10,000 nm. The average particle size of the filler can be specified, for example, by the following method. First, the cross section of the separation functional layer 1 is observed with a transmission electron microscope. In the obtained electron microscope image, the area of a specific filler is calculated by image processing. The diameter of a circle having the same area as the calculated area is regarded as the particle size (particle diameter) of the specific filler. The particle sizes of an arbitrary number of fillers (at least 50) are calculated, and the average of the calculated values is regarded as the average particle size of the filler.
[0117] The filler content in the separation functional layer 1 may be, for example, 1 wt% or more, 5 wt% or more, 10 wt% or more, 15 wt% or more, 20 wt% or more. The filler content in the separation functional layer 1 may be 30 wt% or less.
[0118] The thickness of the separation functional layer 1 is not particularly limited, and may be, for example, 200 μm or less, 100 μm or less, 50 μm or less, 10 μm or less, 4 μm or less, 2 μm or less, or even 1.5 μm or less. The thickness of the separation functional layer 1 may be 0.05 μm or more, or 0.1 μm or more.
[0119] The gel fraction of the separation functional layer 1 is not particularly limited, and may be, for example, 60% or more, 70% or more, 80% or more, 85% or more, or even 90% or more. The higher the gel fraction of the separation functional layer 1, the more likely it is that the separation membrane 10 will be prevented from deteriorating in separation performance when used for a long period of time. The upper limit of the gel fraction of the separation functional layer 1 is, for example, 99% or less.
[0120] The gel fraction of the separation functional layer 1 can be evaluated, for example, by the following method. First, the intermediate layer 2 and the porous support 3 are removed from the separation membrane 10 to prepare a free-standing membrane (single layer membrane) of the separation functional layer 1 (FIG. 2). However, the method for preparing the free-standing membrane of the separation functional layer 1 is not limited to the above method. For example, the free-standing membrane of the separation functional layer 1 may be prepared by preparing a layer having the same composition and thickness as the separation functional layer 1 of the separation membrane 10 on a substrate (e.g., a release liner made of PET), and removing the substrate. The free-standing membrane of the separation functional layer 1 is dried as necessary to make it in a dry state. The "dry state" means that the content of liquid such as water in the separation functional layer 1 is 0.5 wt% or less.
[0121] Next, the free-standing membrane of the separation functional layer 1 is cut into a size of 2 cm length x 2 cm width to prepare a test piece, and the weight A (g) of the test piece is measured. The test piece is immersed in N-methyl-2-pyrrolidone (NMP) in a sample bottle and left at room temperature (25°C) for one day. Next, the test piece is removed from the sample bottle and dried at 130°C for one hour, and the weight B (g) of the test piece after drying is measured. Based on the weights A and B, the gel fraction (%) of the separation functional layer 1 can be calculated using the following formula. Gel fraction (%) = 100 × B / A
[0122] In this embodiment, the surface area A1 (cm 2 ) of the separation functional layer 1 before the following test (immersion test) was performed. 2 ) relative to the surface area A2 (cm 2 ) minus the area A1, the ratio R1 is, for example, 10% or less. Immersion test: The separation functional layer 1 is immersed in a test liquid consisting of ethanol and water for one day. Here, the content of ethanol in the test liquid is 50 wt %, and the temperature of the test liquid is 60°C.
[0123] The ratio R1 is preferably 8.0% or less, and may be 5.0% or less, 4.0% or less, 3.0% or less, 2.0% or less, or even 1.5% or less. The lower the ratio R1, the more likely it is that the separation performance of the separation membrane 10 will be suppressed from decreasing when the separation membrane 10 is used for a long period of time. The lower limit of the ratio R1 is, for example, 0% or more.
[0124] Specifically, the ratio R1 can be determined by the following method. First, a free-standing film (single layer film) of the separation functional layer 1 is prepared by the method described above for evaluating the gel fraction (FIG. 2). The free-standing film of the separation functional layer 1 is dried as necessary to bring it into a dry state.
[0125] Next, the free-standing membrane of the separation functional layer 1 was cut into a size of 2 cm in length × 2 cm in width to prepare a test piece, and the area A1 (cm 2 ) is determined. The test piece is immersed in the above test liquid in the sample bottle and left at 60°C for one day. The test piece is then removed from the sample bottle, and the test liquid adhering to the surface is quickly wiped off. A Kimtowel, for example, can be used to wipe off the test liquid. The area A2 (cm2) of the surface 1a of the obtained test piece is then determined. 2 Based on the areas A1 and A2, the ratio R1 (%) can be calculated using the following formula: Ratio R1(%)=100×(A2-A1) / A1
[0126] In this embodiment, the ratio R2 of the weight W2 (g) of the separation functional layer 1 after the above-mentioned immersion test is performed minus the weight W1 to the weight W1 (g) of the separation functional layer 1 before the test is performed is, for example, 10% or less.
[0127] The ratio R2 is preferably 9.0% or less, and may be 8.0% or less, 7.0% or less, 6.0% or less, 5.0% or less, or even 4.0% or less. The lower the ratio R2, the more likely it is that the separation performance of the separation membrane 10 will be suppressed from decreasing when the separation membrane 10 is used for a long period of time. The lower limit of the ratio R2 is, for example, 1.0% or more.
[0128] In detail, the ratio R2 can be determined by the following method. First, a free-standing film (single layer film) of the separation functional layer 1 is prepared by the method described above for evaluating the gel fraction (FIG. 2). The free-standing film of the separation functional layer 1 is dried as necessary to bring it into a dry state.
[0129] Next, the free-standing membrane of the separation functional layer 1 is cut into a size of 2 cm length x 2 cm width to prepare a test piece, and its weight W1 (g) is determined. This test piece is immersed in the above test liquid in the sample bottle and left at 60°C for one day. Next, the test piece is removed from the sample bottle, and the test liquid adhering to the surface is quickly wiped off. For example, a Kimtowel can be used to wipe off the test liquid. The weight W2 (g) of the obtained test piece is determined. Based on the weights W1 and W2, the ratio R2 (%) can be calculated using the following formula. Ratio R2(%)=100×(W2-W1) / W1
[0130] (Middle class) The intermediate layer 2 may, for example, contain a resin and further contain nanoparticles dispersed in the resin (matrix). The nanoparticles may be separated from one another in the matrix or may be partially aggregated. However, the intermediate layer 2 may not contain nanoparticles and may be substantially composed of a resin.
[0131] The material of the matrix is not particularly limited, and examples thereof include silicone resins such as polydimethylsiloxane, fluororesins such as polytetrafluoroethylene, epoxy resins such as polyethylene oxide, polyimide resins, polysulfone resins, polyacetylene resins such as polytrimethylsilylpropyne and polydiphenylacetylene, polyolefin resins such as polymethylpentene, polyurethane resins, etc. The matrix preferably contains a polyurethane resin.
[0132] The nanoparticles may contain an inorganic material or an organic material. Examples of the inorganic material contained in the nanoparticles include silica, titania, and alumina. The nanoparticles preferably contain silica.
[0133] The thickness of the intermediate layer 2 is not particularly limited and is, for example, less than 50 μm, preferably 40 μm or less, and more preferably 30 μm or less. The lower limit of the thickness of the intermediate layer 2 is not particularly limited and is, for example, 1 μm.
[0134] (porous support) The porous support 3 is a member that supports the separation function layer 1 via the intermediate layer 2. Examples of the porous support 3 include nonwoven fabric, porous polytetrafluoroethylene, aromatic polyamide fiber, porous metal, sintered metal, porous ceramic, porous polyester, porous nylon, activated carbon fiber, latex, silicone, silicone rubber, permeable (porous) polymers including at least one selected from the group consisting of polyvinyl fluoride, polyvinylidene fluoride, polyurethane, polypropylene, polyethylene, polycarbonate, polysulfone, polyether ether ketone, polyacrylonitrile, polyimide, and polyphenylene oxide, metal foams having open or closed cells, polymer foams having open or closed cells, silica, porous glass, and mesh screens. The porous support 3 may be a combination of two or more of these. As an example, the porous support 3 may be a laminate of a nonwoven fabric and a porous layer (for example, a polyvinylidene fluoride porous layer).
[0135] The porous support 3 has an average pore size of, for example, 0.01 to 0.4 μm. The thickness of the porous support 3 is not particularly limited and is, for example, 10 μm or more, preferably 20 μm or more, and more preferably 50 μm or more. The thickness of the porous support 3 is, for example, 300 μm or less, preferably 200 μm or less, and more preferably 75 μm or less.
[0136] (Separation membrane shape) In this embodiment, the separation membrane 10 is typically a flat membrane. However, the separation membrane 10 may have a shape other than a flat membrane, for example, a hollow fiber membrane. As an example, the separation membrane 10 as a hollow fiber membrane may include a separation function layer 1 and a porous support 3, but may not include an intermediate layer 2.
[0137] (Membrane manufacturing method) A manufacturing method of the separation membrane 10 includes, for example, applying a coating liquid containing the above-mentioned polyimide P onto a substrate to form a coating film, and drying the coating film to form a cross-linked polyimide from the polyimide P to obtain a separation functional layer 1.
[0138] The polyimide P can be prepared, for example, by the following method. First, a diamine group including the above diamine D1 is dissolved in a solvent to obtain a solution. The solvent may be, for example, a polar organic solvent such as N-methyl-2-pyrrolidone.
[0139] Next, the tetracarboxylic dianhydride group including the above tetracarboxylic dianhydride C1 is gradually added to the obtained solution. As a result, the tetracarboxylic dianhydride C1 reacts with the monomer group including the diamine D1 to form a polyamic acid. The addition of the tetracarboxylic dianhydride group is performed, for example, under stirring conditions.
[0140] Next, polyamic acid is imidized to obtain polyimide P. Examples of the imidization method include chemical imidization and thermal imidization. The chemical imidization method is a method in which polyamic acid is imidized, for example, under room temperature conditions, using a dehydration condensation agent. Examples of the dehydration condensation agent include acetic anhydride, pyridine, and triethylamine. The thermal imidization method is a method in which polyamic acid is imidized by heat treatment. The temperature of the heat treatment is, for example, 180° C. or higher.
[0141] The content of polyimide P in the coating liquid can be appropriately adjusted depending on the solubility of polyimide P, and is, for example, 1 wt % to 30 wt %.
[0142] The coating liquid further contains, for example, a solvent. The solvent is typically a good solvent capable of dissolving polyimide P, such as N-methyl-2-pyrrolidone (NMP). The content of the solvent in the coating liquid is, for example, 30 wt % to 95 wt %.
[0143] In a preferred embodiment, the coating liquid further contains a compound M having a metal. In this embodiment, the compound M can function as a source of metal ions. Examples of the metal contained in the compound M include those described above for the crosslinked polyimide. In the compound M, the metal exists, for example, as a cation. Examples of the compound M include a metal complex having a metal and a ligand coordinated to the metal, and an inorganic salt containing a metal. It is preferable that the compound M contains a metal complex.
[0144] In the metal complex, the ligand is preferably volatile. As an example, the boiling point of the ligand may be 20°C to 260°C under atmospheric pressure (101.325 kPa). A volatile ligand is likely to volatilize during drying of the coating film described below, and is unlikely to remain in the separation functional layer 1. The ligand does not necessarily have to be volatile. In this case, the ligand can be easily removed from the separation functional layer 1 by performing a washing operation after the formation of the separation functional layer 1.
[0145] In the metal complex, the ligand is typically an organic ligand having a functional group for coordinating with the metal. The number of carbon atoms in the organic ligand is not particularly limited, and is, for example, 1 to 10. Examples of the functional group contained in the organic ligand include a carbonyl group such as a ketone group. The number of functional groups contained in the organic ligand is, for example, 1 or more, and may be 2 or more. Specific examples of the organic ligand include acetylacetonate (acac). Specific examples of the metal complex include Al(acac)3, Fe(acac)2, Ga(acac)3, and Mg(acac)2.
[0146] Inorganic salts include chlorides, nitrates, sulfates, etc., and more specifically, LiCl, NaCl, KCl, AgNO3, MgCl2, CaCl2, BaCl2, NiCl2, ZnCl2, CuCl2, Pb(NO3)2, Al(NO3)3, Fe2(SO4)3, Ga(NO3)3, Fe(NO3)2, Mg(NO3)2, etc.
[0147] In the coating solution, the ratio of the weight of compound M to the weight of polyimide P can be appropriately adjusted depending on the composition of polyimide P, and may be, for example, 1 to 20 wt %, or may be 1 to 10 wt %. In the coating solution, the ratio of the substance amount of compound M to the substance amount of functional group F contained in polyimide P is not particularly limited, and is, for example, 2.0 or more.
[0148] The coating liquid may further contain a ligand when it contains a metal complex as compound M. In the coating liquid, the ratio of the weight of the ligand to the weight of the polyimide P can be appropriately adjusted depending on the contents of the polyimide P and the metal complex, and may be, for example, 1 to 20 wt%, or 1 to 10 wt%.
[0149] In another preferred embodiment, the coating liquid further contains a crosslinking agent. Examples of the crosslinking agent include those mentioned above. In the coating liquid, the ratio of the weight of the crosslinking agent to the weight of the polyimide P can be appropriately adjusted depending on the composition of the polyimide P, and may be, for example, 1 to 20 wt%, or 1 to 10 wt%. In the coating liquid, the ratio of the substance amount of the crosslinking agent to the substance amount of the functional group F contained in the polyimide P is not particularly limited, and is, for example, 2.0 or more.
[0150] The substrate to which the coating liquid containing polyimide P is applied is, for example, a laminate of a porous support 3 and an intermediate layer 2. This laminate can be produced, for example, by the following method. First, a coating liquid containing the material of the intermediate layer 2 is prepared. Next, the coating liquid containing the material of the intermediate layer 2 is applied onto the porous support 3, and dried to form the intermediate layer 2. The method of applying the coating liquid is not particularly limited, and for example, a spin coating method, a dip coating method, etc. can be used. The coating liquid may be applied using a wire bar or the like. The drying of the coating liquid can be performed, for example, under heating conditions. The heating temperature of the coating liquid is, for example, 50°C or higher. The heating time of the coating liquid is, for example, 1 minute or more, and may be 5 minutes or more. Furthermore, the surface of the intermediate layer 2 may be subjected to an easy-adhesion treatment as necessary. Examples of the easy-adhesion treatment include surface treatments such as application of an undercoat agent, corona discharge treatment, and plasma treatment.
[0151] The method for applying the coating liquid containing polyimide P to the substrate is not particularly limited, and can utilize the methods described above for the intermediate layer 2. The thickness of the coating film obtained by applying the coating liquid to the substrate can be appropriately adjusted according to the intended thickness of the separation functional layer 1, and is, for example, 1 μm to 100 μm.
[0152] In this embodiment, as described above, the coating film is dried and a crosslinked polyimide is formed from the polyimide P to obtain the separation functional layer 1. When a laminate of a porous support 3 and an intermediate layer 2 is used as the substrate, the separation functional layer 1 is formed to obtain a separation membrane 10.
[0153] The drying conditions of the coating film are not particularly limited, and for example, the drying temperature is 50°C to 200°C, and the drying time is 1 minute to 10 hours. The coating film can be dried, for example, by using a heater. As an example, the coating film may be dried by passing through a heating unit equipped with a heater. The coating film may be dried by passing through a plurality of heating units. The set temperatures of the plurality of heating units may be the same or different from each other.
[0154] When the coating liquid contains a compound M having a metal, for example, when the coating film is dried, a dissociable proton contained in the functional group F of the polyimide P is exchanged with the metal (metal ion) of the compound M. In particular, when the compound M is a metal complex and the ligand contained in the metal complex is volatile, the exchange between the dissociable proton of the functional group F and the metal of the compound M tends to be promoted by the volatilization of the ligand during drying. A crosslinked structure is formed by the exchange between the dissociable proton of the functional group F and the metal of the compound M, and a crosslinked polyimide is obtained.
[0155] In the case where the coating liquid contains a crosslinking agent, for example, when the coating film is dried, the functional group F of the polyimide P reacts with the crosslinking agent, thereby forming a crosslinked structure and obtaining a crosslinked polyimide.
[0156] The crosslinked polyimide may be formed after drying the coating film to form a dry film. For example, a coating liquid containing the above polyimide P and a solvent is applied onto a substrate, and dried to form a dry film. The dry film may be immersed in a solution containing compound M or a crosslinking agent, and further heated as necessary to form a crosslinked polyimide. In this case, an example of the solution containing compound M is an aqueous solution containing the above inorganic salt. The concentration of the inorganic salt in the aqueous solution is not particularly limited, and is, for example, 0.01 to 1 mol / L. The conditions for immersing the dry film in the solution are not particularly limited, and may be, for example, at room temperature for 1 to 48 hours. The film after immersing in the above solution may be further washed with water or dried. The drying process may be performed at a temperature of 150° C. or less for 1 to 24 hours.
[0157] The manufacturing method of this embodiment may further include subjecting the obtained separation functional layer 1 to a heat treatment (annealing treatment). This step tends to improve the separation performance of the separation functional layer 1 and also suppress deterioration over time of the separation performance of the separation functional layer 1. This step also makes it possible to obtain a separation functional layer 1 that contains almost no residual solvent by sufficiently volatilizing the solvent.
[0158] The temperature of the heat treatment may be, for example, higher than 200° C., 230° C. or higher, or even 250° C. or higher. The upper limit of the temperature of the heat treatment is not particularly limited, and may be, for example, 350° C. or lower, or may be 300° C. or lower. The time of the heat treatment is, for example, 1 minute or more, may be 10 minutes or more, or may be 30 minutes or more. The upper limit of the time of the heat treatment is not particularly limited, and may be, for example, 24 hours or less.
[0159] The manufacturing method of this embodiment is not limited to the above. Instead of the coating liquid containing polyimide P, a coating liquid containing polyamic acid, which is a precursor of polyimide P, may be used. This coating liquid may be applied onto a substrate, polyamic acid may be imidized to form polyimide P, and then crosslinked polyimide may be formed from polyimide P to produce the separation functional layer 1.
[0160] Furthermore, the separation membrane 10 may be produced by the following method. First, a separation functional layer 1 formed on a substrate such as a release liner is prepared by the above-mentioned method. Next, a coating liquid containing a material for the intermediate layer 2 is applied onto the separation functional layer 1 and dried to form the intermediate layer 2. The laminate of the intermediate layer 2 and the separation functional layer 1 is transferred to a porous support 3. In this way, the separation membrane 10 is obtained.
[0161] (Separation membrane characteristics) As described above, the separation membrane 10 allows water to preferentially permeate from the mixed liquid L containing the volatile organic compound C and water. As an example, the separation coefficient α1 of water with respect to ethanol of the separation membrane 10 in the initial state is, for example, 10 or more, and may be 15 or more, or even 20 or more. The upper limit of the separation coefficient α1 is not particularly limited and is, for example, 100.
[0162] The separation coefficient α1 can be measured by the following method. First, a mixed liquid consisting of ethanol and water is brought into contact with one side of the separation membrane 10 (for example, the main surface 11 of the separation membrane 10 on the separation functional layer side), and the space adjacent to the other side of the separation membrane 10 (for example, the main surface 12 of the separation membrane 10 on the porous support side) is depressurized. As a result, a permeated fluid that has permeated the separation membrane 10 is obtained. The volume ratio of water and the volume ratio of ethanol in the permeated fluid are measured. In the above operation, the content of ethanol in the mixed liquid is 50 wt %. The mixed liquid brought into contact with the separation membrane 10 has a temperature of 60° C. The space adjacent to the other side of the separation membrane 10 is depressurized so that the pressure in the space is 100 kPa lower than the atmospheric pressure in the measurement environment. The separation coefficient α1 can be calculated from the following formula. In the following formula, X A and X B are the volume fractions of water and ethanol in the mixed liquid, respectively. Y A and Y B are the volume fraction of water and the volume fraction of ethanol, respectively, in the permeate fluid that has permeated the separation membrane 10. Separation factor α1=(Y A / Y B ) / (X A / X B )
[0163] Under the above measurement conditions for the separation factor α1, the flux T1 of water permeating the separation membrane 10 is, for example, 0.05 (kg / m 2 / hr) or more, and 0.10 (kg / m 2 / hr) or more, and even 0.15 (kg / m 2 The upper limit of the flux T1 of water permeating through the separation membrane 10 is not particularly limited, and may be, for example, 1.0 (kg / m 2 / hr).
[0164] As described above, in the separation membrane 10 of this embodiment, the separation functional layer 1 contains crosslinked polyimide. This separation functional layer 1 is less likely to swell when it comes into contact with a mixed liquid containing water, and dimensional changes tend to be suppressed. Therefore, even if the separation membrane 10 is used for a long period of time, it is possible to suppress the occurrence of stripe-like cracks on the surface of the separation functional layer 1 and the occurrence of peeling between the layers constituting the separation membrane 10 (for example, between the nonwoven fabric and the porous layer in the porous support 3), and the separation membrane 10 is less likely to deteriorate. In this way, the separation membrane 10 is suitable for suppressing the deterioration of separation performance when used for a long period of time.
[0165] The deterioration of the separation performance of the separation membrane 10 due to long-term use can be evaluated, for example, by the following durability test. First, the operation of measuring the above-mentioned separation factor α1 (separation operation) is performed for 3 hours. Next, the separation membrane 10 is left overnight at room temperature without contacting the mixed liquid. After that, the above-mentioned separation operation is performed for another 3 hours. For the separation membrane 10 after the above durability test, the separation factor α2 of water relative to ethanol is measured by the same method as the separation factor α1. The deterioration of the separation performance can be evaluated based on the ratio α2 / α1 of the separation factor α2 to the separation factor α1 (retention rate of the separation factor).
[0166] In the separation membrane 10, the ratio α2 / α1 is, for example, 0.5 or more, and may be 0.6 or more, 0.7 or more, 0.8 or more, 0.9 or more, or even 1.0 or more. The upper limit of the ratio α2 / α1 is, for example, 1.2 or less.
[0167] The separation factor α2 after the durability test is, for example, 10 or more, and may be 15 or more, or even 20 or more. The upper limit of the separation factor α2 is not particularly limited, and is, for example, 100.
[0168] Under the above measurement conditions for the separation factor α2, the flux T2 of water permeating the separation membrane 10 after the durability test is, for example, 0.05 (kg / m 2 / hr) or more, and 0.10 (kg / m 2 / hr) or more, and even 0.15 (kg / m 2The upper limit of the flux T2 of water permeating through the separation membrane 10 is not particularly limited, and may be, for example, 1.0 (kg / m 2 / hr) The ratio T2 / T1 of the flux T2 to the flux T1 is not particularly limited and is, for example, 0.7 to 1.3.
[0169] (Applications of separation membranes) The separation membrane 10 of this embodiment is suitable for use in separating water from a mixed liquid L containing a volatile organic compound C and water. The organic compound C is not particularly limited as long as it is volatile. In this specification, the term "volatile organic compound" refers to an organic compound having a boiling point of 20°C to 260°C under atmospheric pressure (101.325 kPa).
[0170] The number of carbon atoms in the organic compound C is not particularly limited, and may be, for example, 10 or less, 8 or less, 6 or less, or even 4 or less. The lower limit of the number of carbon atoms in the organic compound C may be 1 or 2. The organic compound C has a functional group containing an oxygen atom, such as a hydroxyl group, a carbonyl group, an ether group, or an ester group. In the organic compound C, the number of functional groups containing an oxygen atom is typically one.
[0171] Examples of the organic compound C include alcohols, ketones, esters, and the like, and are typically alcohols. The alcohol may be an alkyl alcohol composed only of an alkyl group and a hydroxyl group, or an aryl alcohol containing an aryl group and a hydroxyl group. The alkyl alcohol may be linear, branched, or cyclic. Examples of the alkyl alcohol include methanol, ethanol, n-propanol, isopropanol, n-butanol, 2-butanol, isobutanol, t-butanol, and n-pentanol, and preferably ethanol. Examples of the aryl alcohol include phenol, and the like.
[0172] The ketone may be a dialkyl ketone consisting of only alkyl and carbonyl groups, such as methyl ethyl ketone (MEK) and acetone.
[0173] The ester may be a fatty acid alkyl ester composed only of alkyl and ester groups, such as ethyl acetate.
[0174] The organic compound C is not limited to the above-mentioned compounds, and may be an aromatic hydrocarbon such as benzene, toluene, or xylene.
[0175] The mixed liquid L may contain one type of organic compound C, or may contain two or more types of organic compounds C. The content of the organic compound C in the mixed liquid L is, for example, 10 wt% or more, and may be 20 wt% or more. The separation membrane 10 is particularly suitable for separating water from a mixed liquid L having a medium content of the organic compound C (20 wt% to 80 wt%, particularly 30 wt% to 70 wt%). However, the content of the organic compound C in the mixed liquid L may be 80 wt% or more. The mixed liquid L may be substantially composed of the organic compound C and water.
[0176] <Embodiment of Membrane Separation Apparatus> As shown in Fig. 3, the membrane separation device 100 of this embodiment includes a separation membrane 10 and a tank 20. The tank 20 includes a first chamber 21 and a second chamber 22. The first chamber 21 functions as a supply space to which a supply fluid (specifically, the above-mentioned mixed liquid L) is supplied. The second chamber 22 functions as a permeation space to which a permeated fluid L1 is supplied. The permeated fluid L1 is obtained by the permeation of the mixed liquid L through the separation membrane 10.
[0177] The separation membrane 10 is disposed inside the tank 20. Inside the tank 20, the separation membrane 10 separates a first chamber 21 and a second chamber 22. The separation membrane 10 extends from one of a pair of wall surfaces of the tank 20 to the other.
[0178] The first chamber 21 has an inlet 21a and an outlet 21b. The second chamber 22 has an outlet 22a. The inlet 21a is an opening for supplying the mixed liquid L to the supply space (first chamber 21). The outlet 22a is an opening for discharging the permeated fluid L1 from the permeated space (second chamber 22). The outlet 21b is an opening for discharging the mixed liquid L (non-permeated fluid L2) that has not permeated the separation membrane 10 from the supply space (first chamber 21). Each of the inlet 21a, the outlet 21b, and the outlet 22a is formed, for example, on a wall surface of the tank 20.
[0179] The membrane separation apparatus 100 is suitable for a flow-through (continuous) membrane separation method, but may also be used for a batch-type membrane separation method.
[0180] (Membrane separation device operation method) The membrane separation device 100 is operated, for example, as follows. First, the mixed liquid L is supplied to the first chamber 21 of the membrane separation device 100 through the inlet 21a. This allows the mixed liquid L to come into contact with one surface of the separation membrane 10 (for example, the main surface 11).
[0181] The temperature of the mixed liquid L may be higher than the boiling point of the organic compound C, but is preferably lower than the boiling point of the organic compound C. The temperature of the mixed liquid L is, for example, 25° C. or higher, preferably 40° C. or higher, and more preferably 60° C. or higher. The temperature of the mixed liquid L may be 75° C. or lower.
[0182] Next, with the mixed liquid L in contact with one surface of the separation membrane 10, the space adjacent to the other surface (e.g., the main surface 12) of the separation membrane 10 is depressurized. In detail, the pressure inside the second chamber 22 is reduced through the outlet 22a. The membrane separation device 100 may further include a pump (not shown) for reducing the pressure inside the second chamber 22. The pressure inside the second chamber 22 is reduced so that the pressure inside the second chamber 22 is, for example, 10 kPa or more, preferably 50 kPa or more, and more preferably 100 kPa or more lower than the atmospheric pressure in the measurement environment.
[0183] By reducing the pressure inside the second chamber 22, a permeated fluid L1 having a high water content can be obtained on the other side of the separation membrane 10. In other words, the permeated fluid L1 is supplied to the second chamber 22. The permeated fluid L1 contains, for example, water as a main component. However, the permeated fluid L1 may contain a small amount of an organic compound C in addition to water. The permeated fluid L1 may be a gas or a liquid. The permeated fluid L1 is discharged to the outside of the membrane separation device 100 through the outlet 22a.
[0184] On the other hand, the content of the organic compound C in the mixed liquid L gradually increases from the inlet 21a to the outlet 21b of the first chamber 21. The mixed liquid L (non-permeated fluid L2) treated in the first chamber 21 is discharged to the outside of the membrane separation device 100 through the outlet 21b. The non-permeated fluid L2 is typically a liquid.
[0185] The membrane separation apparatus 100 of the present embodiment is preferably used for pervaporation. However, the membrane separation apparatus 100 may be used for other membrane separation methods, such as vapor permeation. That is, in the above-mentioned membrane separation method, a mixed gas containing a gaseous organic compound C and gaseous water may be used instead of the mixed liquid L.
[0186] <Modification of Membrane Separation Device> The membrane separation device 100 may be a spiral-type membrane element, a hollow fiber membrane element, a disk-tube-type membrane element in which a plurality of separation membranes are stacked, a plate-and-frame-type membrane element, or the like. Fig. 4 shows a spiral-type membrane element. The membrane separation device 110 in Fig. 4 includes a central tube 41 and a stack 42. The stack 42 includes the separation membrane 10.
[0187] The central tube 41 has a cylindrical shape. A plurality of holes or slits are formed on the surface of the central tube 41 for allowing the permeation fluid L1 to flow into the inside of the central tube 41. Examples of materials for the central tube 41 include resins such as acrylonitrile-butadiene-styrene copolymer resin (ABS resin), polyphenylene ether resin (PPE resin), and polysulfone resin (PSF resin); and metals such as stainless steel and titanium. The inner diameter of the central tube 41 is, for example, in the range of 20 to 100 mm.
[0188] The laminate 42 further includes a feed-side flow path material 43 and a permeate-side flow path material 44 in addition to the separation membrane 10. The laminate 42 is wound around a central tube 41. The membrane separation device 110 may further include an exterior material (not shown).
[0189] The feed-side passage material 43 and the permeate-side passage material 44 may be, for example, a resin net made of polyethylene, polypropylene, polyethylene terephthalate (PET), polyphenylene sulfide (PPS), or ethylene-chlorotrifluoroethylene copolymer (ECTFE).
[0190] The membrane separation device 110 can be operated, for example, in the following manner. First, the mixed liquid L is supplied to one end of the wound laminate 42, and the space inside the central tube 41 is depressurized. As a result, the permeated fluid L1 that has permeated the separation membrane 10 of the laminate 42 moves into the inside of the central tube 41. The permeated fluid L1 is discharged to the outside through the central tube 41. The mixed liquid L (non-permeated fluid L2) that has been treated in the membrane separation device 110 is discharged to the outside from the other end of the wound laminate 42. EXAMPLES
[0191] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto.
[0192] [Synthesis of Polyimide P] First, polyimide P was synthesized using an automatic polymerization apparatus (Mettler Toledo, EasyMax402). A Dimroth, stirring rod, internal thermometer, nitrogen inlet tube and flat stopper were attached to the separable flask (capacity 2000 mL) attached to the apparatus. A cooling liquid set to 10°C was circulated in the Dimroth chiller. N2 gas was circulated in the flask at a flow rate of 400 mL / min. The stirring speed was set to 150 rpm. Next, 250 g of 1-methyl-2-pyrrolidone as a solvent, 23 g of 4,4'-diaminodiphenyl ether and 2 g of 3,5-diaminobenzoic acid as diamines were added to the flask. The diamine was dissolved in the solvent by stirring these at room temperature. To the resulting solution, 20 g of 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride as a tetracarboxylic dianhydride and 37 g of bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylate)ethylene (Rikacid TMEG-100, manufactured by New Japan Chemical Co., Ltd.) were further added. Next, the mixture was stirred at a stirring speed of 150 rpm for 40 minutes, 100 rpm for 10 minutes, 50 rpm for 3 hours, and 10 rpm for 18 hours. The internal temperature of the flask was cooled to 25°C and allowed to stand overnight.
[0193] Next, 6 g of triethylamine and 37 g of acetic anhydride were added, the jacket temperature was raised to 60°C, and the mixture was stirred at a stirring speed of 150 rpm for 6 hours. After leaving the reaction solution to stand overnight, 1,250 g of 1,3-dioxolane was added to dilute the reaction solution. Next, the precipitated solid was filtered using a PET filter paper (Seiren Co., Ltd., #1000) cut to the size of the Buchner funnel, and the operation of washing with 2600 ml of ion-exchanged water was performed three times. After washing, the filtered solid was dried in a hot air circulation dryer at 60°C for 15 hours, and further dried in a vacuum dryer at 100°C for 8 hours. As a result, polyimide P was obtained with a yield of 70 g.
[0194] [Laminate of porous support and intermediate layer] First, a silicone resin (POLON MF-56 manufactured by Shin-Etsu Chemical Co., Ltd.) and a polyurethane resin (Takelac W-6010 manufactured by Mitsui Chemicals, Inc.) were mixed so that the solid content ratio was 90:10, and further diluted with ion-exchanged water so that the solid content concentration was 10 wt%. Next, the obtained coating liquid was applied to a porous support using a bar coater. As the porous support, an ultrafiltration membrane (RS-50 manufactured by Nitto Denko Corporation) was used. The coating liquid was applied under the condition that the coating thickness was 10 μm. Next, the obtained coating film was dried at 110° C. for 5 minutes. As a result, a laminate of a porous support and an intermediate layer was obtained. The thickness of the intermediate layer was 1 μm.
[0195] Example 1 The polyimide P was added to a 10L pail, and N-methyl-2-pyrrolidone (NMP) as a solvent and acetylacetone as a ligand were added to obtain a mixed solution. The mixed solution was stirred for 1 hour at a rotation speed of 700 to 1400 rpm using a propeller-type stirring blade. Next, NMP and Al(acac)3 as compound M (metal complex) were added to another screw tube, and an ultrasonic treatment was performed using an ultrasonic cleaner to obtain an Al(acac)3 solution. The Al(acac)3 solution and the mixed solution were further mixed, and the mixture was stirred for 1 hour at a rotation speed of 700 to 1400 rpm using a propeller-type stirring blade to prepare a coating solution.
[0196] In the coating solution, the ratio of the weight of polyimide P to the total weight of polyimide P and NMP was 8 wt%, and the ratio of the weight of NMP to the total weight was 92 wt%. In the coating solution, the ratio of the weight of Al(acac)3 to the weight of polyimide P and the weight of acetylacetone to the weight of polyimide P were both 6 wt%.
[0197] Next, the obtained coating liquid was applied onto a laminate (substrate) of the porous support and the intermediate layer to prepare a coating film. The coating liquid was applied using a slot die.
[0198] Next, the coating film was transported at a speed of 1 m / min and dried by passing through three heating parts. In detail, the coating film passed through the first heating part, the second heating part, and the third heating part in this order. The set temperature of the first heating part was 100°C, the set temperature of the second heating part was 130°C, and the set temperature of the third heating part was 130°C. The time (drying time) for the coating film to pass through the first to third heating parts was 6 minutes. By drying the coating film, the dissociative protons of the functional group F (carboxyl group) contained in the polyimide P were exchanged with Al of the metal complex, and a crosslinked polyimide was formed from the polyimide P. As a result, a separation functional layer was formed, and the separation membrane of Example 1 was obtained.
[0199] Example 2 The polyimide P was added to a 10 L pail, and N-methyl-2-pyrrolidone (NMP) as a solvent and an epoxy-based crosslinking agent (TETRAD-C (1,3-bis(N,N-diglycidylaminomethyl)cyclohexane) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as a crosslinking agent were added to obtain a mixed solution. The mixed solution was stirred for 1 hour at a rotation speed of 700 to 1400 rpm using a propeller-type stirring blade to prepare a coating solution.
[0200] In the coating solution, the ratio of the weight of polyimide P to the total weight of polyimide P and NMP was 8 wt%, and the ratio of the weight of NMP to the total weight was 92 wt%. In the coating solution, the ratio of the weight of the crosslinking agent to the weight of polyimide P was 6 wt%.
[0201] Except for using the above coating solution, the separation membrane of Example 2 was obtained by the same method as in Example 1. Note that in Example 2, when the coating membrane was dried, the functional group F (carboxyl group) contained in the polyimide P reacted with the crosslinking agent to form a crosslinked polyimide from the polyimide P.
[0202] Comparative Example 1 The polyimide P was added to a 10 L pail can, and N-methyl-2-pyrrolidone (NMP) was added as a solvent to obtain a mixed solution. The mixed solution was stirred for 1 hour at a rotation speed of 700 to 1400 rpm using a propeller-type stirring blade to prepare a coating solution. A separation membrane of Comparative Example 1 was obtained by the same method as in Example 1, except that this coating solution was used. Note that in Comparative Example 1, no crosslinked polyimide was formed from the polyimide P.
[0203] [Gel fraction] First, a layer having the same composition and thickness as the separation functional layer of the separation membrane of Examples 1 and 2 was prepared on a release liner. A polyethylene terephthalate (PET) film (Mitsubishi Chemical Corporation, MRE38) was used as the release liner. Next, the release liner was removed to prepare a free-standing membrane of the separation functional layer. The gel fraction of this free-standing membrane was measured by the method described above.
[0204] [Ratios R1 and R2] Using the method described above, a layer having the same composition and thickness as the separation functional layer of the separation membranes of the Examples and Comparative Examples was prepared on the release liner. Next, the release liner was removed to prepare a free-standing membrane of the separation functional layer. An immersion test was performed on this free-standing membrane using the method described above. The surface area A1 (cm2) of the separation functional layer before the immersion test was 2 ) and the surface area A2 (cm2) of the separation functional layer after the immersion test 2 ) The ratio R1 was calculated based on the weight W1 (g) of the separation functional layer before the immersion test and the weight W2 (g) of the separation functional layer after the immersion test.
[0205] [Separation characteristics] For the separation membranes of the examples and comparative examples, the separation factor α1 of water relative to ethanol in the initial state and the water flux T1 were measured by the above-mentioned method. Furthermore, the above-mentioned durability test was performed on the separation membrane, and the separation factor α2 of water relative to ethanol and the water flux T2 after the durability test were measured. From these results, the ratio α2 / α1 of the separation factor α2 to the separation factor α1 (retention rate of the separation factor) was calculated.
[0206] [Table 3]
[0207] As can be seen from Table 3, the separation membranes of the examples containing crosslinked polyimide had a higher ratio α2 / α1 (retention rate of separation factor) than the comparative examples. From this result, it can be estimated that the separation membranes of the examples are prevented from decreasing in separation performance even when used for a long period of time. The separation membranes of the examples had an initial separation factor α1 of 20 or more and a water flux T1 of 0.1 (kg / m 2 / hr), all of which were sufficient for practical use.
[0208] In the examples, the ratio R1 for the separation functional layer was low, and the dimensional change before and after the immersion test was suppressed. Similarly, in the examples, the ratio R2 for the separation functional layer was low, and the weight change before and after the immersion test was suppressed. Thus, in the examples, the separation functional layer tended not to swell when contacted with a mixed liquid containing water. Due to this, it is presumed that the ratio α2 / α1 was high in the separation membrane of the examples. [Industrial Applicability]
[0209] The separation membrane of this embodiment is suitable for separating water from a mixed liquid containing a volatile organic compound and water. [Explanation of symbols]
[0210] 1 Separation functional layer 2. Middle Tier 3 Porous support 10 Separation membrane 100,110 Membrane separation device
Claims
1. A separation membrane for separating water from a mixed liquid containing a volatile organic compound and water, The separation membrane comprises a separation functional layer containing a crosslinked polyimide.
2. The separation membrane according to claim 1 , wherein the separation functional layer has a gel fraction of 80% or more.
3. The separation membrane according to claim 1 , wherein the crosslinked polyimide is a polyimide crosslinked via an ionic bond or a covalent bond.
4. The separation membrane according to claim 3 , wherein the polyimide has at least one functional group F selected from the group consisting of a carboxyl group, a hydroxyl group, a thiol group, and a sulfonic acid group.
5. The separation membrane according to claim 4 , wherein the polyimide has a carboxyl group as the functional group F.
6. The separation membrane according to claim 4 , wherein the crosslinked polyimide is formed by exchanging a dissociable proton contained in the functional group F with a metal ion.
7. The separation membrane according to claim 4 , wherein the crosslinked polyimide is formed by reacting the functional group F with a crosslinking agent.
8. The separation membrane according to claim 7 , wherein the crosslinking agent comprises at least one selected from the group consisting of an epoxy-based crosslinking agent and an isocyanate-based crosslinking agent.
9. The separation membrane according to claim 4 , wherein the polyimide contains a structural unit X1 represented by the following formula (1): 【Chemistry 1】 In the formula (1), A 1 is a tetravalent linking group, B 1 is a divalent linking group. 1 and B 1 At least one selected from the group consisting of the functional group F is included.
10. The separation membrane according to claim 9 , wherein the structural unit X1 is a structural unit X2 represented by the following formula (2): 【Chemistry 2】 In the formula (2), A 2 and B 1 are each independently a divalent linking group, R 1 ~R 6 are each independently a hydrogen atom or an arbitrary substituent. 2 , B 1 and R 1 ~R 6 At least one selected from the group consisting of the functional group F is included.
11. The surface area A1 (cm ) of the separation functional layer before the following test was performed 2 ) to the surface area A2 (cm ) of the separation functional layer after the test 2 2. The separation membrane according to claim 1, wherein a ratio R1 obtained by subtracting the area A1 from the area A1 is 10% or less. Test: The separation functional layer is immersed in a test liquid consisting of ethanol and water for one day, where the content of ethanol in the test liquid is 50 wt %, and the temperature of the test liquid is 60° C.
12. The separation membrane described in claim 1, wherein the ratio R2 of the weight W2 (g) of the separation functional layer after performing the test minus the weight W1 (g) of the separation functional layer before performing the test is 10% or less. Test: The separation functional layer is immersed in a test liquid consisting of ethanol and water for one day, where the content of ethanol in the test liquid is 50 wt %, and the temperature of the test liquid is 60° C.
13. The separation membrane according to claim 1 , further comprising a porous support supporting the separation functional layer.
14. A method for producing a separation membrane according to any one of claims 1 to 13, The manufacturing method includes: Applying a coating liquid containing polyimide onto a substrate to form a coating film; drying the coating film to form the crosslinked polyimide from the polyimide, thereby obtaining the separation functional layer; A method for producing a separation membrane comprising the steps of:
Citation Information
Patent Citations
Asymmetric hollow fiber gas separation membrane and gas separation method
JP2014184424A