R-t-b based permanent magnet
The R-T-B permanent magnet composition with controlled heavy rare earth element distribution and specific additives enhances magnetic properties and corrosion resistance, addressing the challenges of existing magnets with low Co content.
Patent Information
- Application Number
- JP2023047177
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
Existing R-T-B permanent magnets with low Co content face challenges in maintaining excellent magnetic properties and corrosion resistance, particularly at room and high temperatures, while minimizing the use of heavy rare earth elements.
The R-T-B permanent magnet composition includes specific ranges of rare earth elements, transition metals, and other additives like Si, Zr, Ga, and B, with a controlled concentration gradient of heavy rare earth elements, forming core-shell particles and a concentration distribution that enhances magnetic properties and corrosion resistance.
The solution results in improved residual magnetic flux density, coercive force, squareness ratio, and corrosion resistance, with optimized magnetic properties at room and high temperatures, and reduced reliance on heavy rare earth elements.
Smart Images

Figure 2024136167000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to RTB based permanent magnets. [Background technology]
[0002] Patent Document 1 discloses an RTB permanent magnet that has a low Co content and is excellent in magnetic properties and corrosion resistance. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-161812 A Summary of the Invention [Problem to be solved by the invention]
[0004] An object of one aspect of the present disclosure is to provide an RTB permanent magnet that has excellent corrosion resistance and magnetic properties (particularly coercive force at room temperature and at high temperatures) even with a small content of heavy rare earth elements. [Means for solving the problem]
[0005] In order to achieve the above object, the RTB permanent magnet of the present disclosure contains at least rare earth elements, Fe, Co, Si, Zr, Ga, and B, Contains heavy rare earth elements as rare earth elements, The content of rare earth elements is 28.50% by mass to 31.50% by mass, The content of heavy rare earth elements is 0.30 mass% or less (excluding 0 mass%), The Co content is 0.20 mass% to 1.00 mass%. The Si content is 0.35 mass% to 1.20 mass%. The Zr content is 0.21 mass% to 0.85 mass%. The Ga content is 0.04 mass% to 0.40 mass%; The B content is 0.90 mass% to 1.02 mass%; The content of C is 0 mass% to 0.11 mass%.
[0006] The value obtained by dividing the content of Ga by the content of Si on a mass basis may be 0.04 to 0.70.
[0007] It may further contain O, and the content of O may be 0.11 mass% or less (excluding 0 mass%).
[0008] It may further contain Al, and the content of Al may be 0.03 mass% to 0.45 mass%.
[0009] It may have a concentration distribution of heavy rare earth elements that decreases from the magnet surface toward the inside.
Brief Description of the Drawings
[0010] [Figure 1] It is a schematic diagram of the R-T-B type permanent magnet according to this embodiment.
Embodiments for Carrying Out the Invention
[0011] Hereinafter, the present disclosure will be described based on the embodiments shown in the drawings.
[0012] <R-T-B type permanent magnet> The R-T-B type permanent magnet according to this embodiment has main phase particles composed of crystal particles having an R2T 14 B-type crystal structure. Further, it has grain boundaries formed by two or more adjacent main phase particles.
[0013] R-T-B type permanent magnet and R2T 14 In the R2T
[0014] R-T-B type permanent magnet and R2T 14The rare earth element contained as R in the B-type crystal structure may be Sc, Y, or a lanthanoid, or may be Y and a lanthanoid. The transition metal element contained as T does not include a rare earth element. The transition metal element contained as T may be an iron group element. A part of the boron contained as B may be substituted with carbon.
[0015] There are no particular limitations on the shape of the RTB permanent magnet according to this embodiment.
[0016] The RTB permanent magnet according to this embodiment contains a number of specific elements in specific ranges of content, which allows for improved remanence Br, coercivity HcJ, squareness ratio Hk / HcJ, and corrosion resistance. Note that Br and Hk / HcJ are both measured at room temperature.
[0017] Furthermore, the RTB permanent magnet according to this embodiment may have a concentration distribution in which the concentration of the heavy rare earth element decreases from the outside to the inside of the RTB permanent magnet 1. There are no particular limitations on the type of heavy rare earth element. For example, it may be Dy or Tb, or it may be Tb.
[0018] Specifically, as shown in FIG. 1, the rectangular parallelepiped RTB permanent magnet 1 according to this embodiment has a surface portion and a center portion, and the content of the heavy rare earth element in the surface portion may be 2% or more higher, 5% or more higher, or 10% or more higher by mass than the content of the heavy rare earth element in the center portion. The surface portion refers to the surface of the RTB permanent magnet 1. For example, POINTS C and C' (the centers of gravity of the surfaces facing each other in FIG. 1) in FIG. 1 are the surface portion. The center portion refers to the center of the RTB permanent magnet 1. For example, it refers to a portion that is half the thickness of the RTB permanent magnet 1. For example, POINT M (the midpoint between POINT C and POINT C') in FIG. 1 is the center portion. POINTS C and C' in FIG. 1 may be the center of gravity of the surface with the largest area among the surfaces of the RTB permanent magnet 1, and the center of gravity of the surface facing the surface.
[0019] Rare earth elements are generally classified into light rare earth elements and heavy rare earth elements. In the RTB permanent magnet according to this embodiment, the light rare earth elements are Sc, Y, La, Ce, Pr, Nd, Sm, and Eu, and the heavy rare earth elements are Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu.
[0020] There are no particular limitations on the method for forming the concentration distribution of the heavy rare earth element in the RTB permanent magnet according to this embodiment. For example, the concentration distribution of the heavy rare earth element can be formed in the RTB permanent magnet by grain boundary diffusion of the heavy rare earth element, which will be described later.
[0021] Furthermore, the main phase particles of the RTB permanent magnet according to this embodiment may be core-shell particles consisting of a core and a shell covering the core. At least the shell may contain a heavy rare earth element, Dy or Tb, or Tb may be present.
[0022] By having a heavy rare earth element present in the shell, the magnetic properties of the RTB permanent magnet can be efficiently improved.
[0023] In this embodiment, the shell is defined as a portion where the ratio of heavy rare earth elements to light rare earth elements (heavy rare earth elements / light rare earth elements (molar ratio)) is at least twice the ratio at the center of the main phase particle. Note that the ratio at the center of the main phase particle may be, for example, the ratio at a portion of the main phase particle whose depth from the particle surface is at least 30% of the particle diameter.
[0024] There is no particular limit to the thickness of the shell, but it may be 500 nm or less on average. There is no particular limit to the particle size of the main phase particles, but it may be 1.0 μm or more and 6.5 μm or less on average. When calculating the above average, a cross section of the RTB permanent magnet may be observed using an SEM. An observation range may be set large enough to accommodate 50 or more core-shell particles. The shell thicknesses of all core-shell particles within the observation range may be measured and averaged. The particle sizes of all main phase particles within the observation range may be measured and averaged. The observation range may be, for example, 100 μm x 100 μm.
[0025] There is no particular limitation on the method for making the main phase particles into the above-mentioned core-shell particles. For example, there is a method using grain boundary diffusion, which will be described later. The heavy rare earth element diffuses into the grain boundaries and replaces the rare earth element on the surface of the main phase particle, forming a shell with a high ratio of the heavy rare earth element, thereby forming the above-mentioned core-shell particle.
[0026] The RTB permanent magnet according to this embodiment may contain at least one selected from Nd and Pr as a light rare earth element, and may contain at least one selected from Dy and Tb as a heavy rare earth element. Also, the RTB permanent magnet according to this embodiment preferably contains at least Nd and Tb.
[0027] The RTB permanent magnet according to this embodiment may have a total content of rare earth elements other than Nd, Pr, Dy and Tb of 0.3 mass% or less, with the mass of the entire RTB permanent magnet being 100 mass%, or the total content of rare earth elements other than Nd, Pr and Tb may be 0.3 mass% or less.
[0028] The total content of rare earth elements (TRE) in the RTB permanent magnet according to this embodiment is 28.50% by mass or more and 31.50% by mass or less, with the mass of the entire RTB permanent magnet being 100% by mass. It may be 29.50% by mass or more and 30.80% by mass or less. If the TRE is too small, HcJ at room temperature (23±1°C), HcJ at high temperatures (100°C or more and 200°C or less) and Hk / HcJ decrease. If the TRE is too large, Br and corrosion resistance decrease.
[0029] There are no particular limitations on the total content of Nd and Pr in the RTB permanent magnet according to this embodiment, but it may be 28.25% by mass or more and 31.25% by mass or less, or 29.25% by mass or more and 30.55% by mass or less, with the mass of the entire RTB permanent magnet being 100% by mass.
[0030] When the RTB permanent magnet contains one or more selected from Nd and Pr, the Pr content may be 0.0 mass % or more and 10.0 mass % or less, or 0.0 mass % or more and 7.6 mass % or less.
[0031] The value obtained by dividing the Pr content by the total content of Nd and Pr on a mass basis may be 0 or more and 0.35 or less.
[0032] The RTB permanent magnet according to this embodiment does not necessarily have to intentionally contain Pr. If Pr is not intentionally contained, HcJ at high temperatures tends to be high. If Pr is not intentionally contained, it may contain less than 0.2 mass% Pr as an impurity, or may contain 0.1 mass% or less.
[0033] Furthermore, the RTB permanent magnet of this embodiment has a heavy rare earth element content (HRE) of 0.30 mass% or less (excluding 0 mass%) in total, with the mass of the entire RTB permanent magnet being 100 mass%. If the heavy rare earth element content is too high, the raw material cost increases. Furthermore, Br is likely to decrease. The heavy rare earth element content may be 0.10 mass% or more and 0.30 mass% or less, or may be 0.15 mass% or more and 0.25 mass% or less.
[0034] The Co content is 0.20% by mass or more and 1.00% by mass or less, with the total mass of the RTB permanent magnet being 100% by mass. It may be 0.50% by mass or more and 0.80% by mass or less. If the Co content is too high, the raw material cost increases. If the Co content is too low, the corrosion resistance decreases.
[0035] The Fe content is the substantial remainder of the RTB permanent magnet. The Fe content is the substantial remainder of the RTB permanent magnet means that in the RTB permanent magnet, the remainder excluding the rare earth elements and Co described above, and the below-described B, Si, Al, Zr, Ga, Cu, C, and O, is essentially Fe alone. For example, the total content of elements other than the rare earth elements, Fe, Co, B, Si, Al, Zr, Ga, Cu, C, and O may be 1.0 mass% or less, assuming that the mass of the entire RTB permanent magnet is 100 mass%.
[0036] The B content in the RTB permanent magnet according to this embodiment is 0.90% by mass or more and 1.02% by mass or less, with the mass of the entire RTB permanent magnet being 100% by mass. It may be 0.94% by mass or more and 0.98% by mass or less. If the B content is too low, the HcJ at high temperatures tends to decrease. If the B content is too high, the HcJ at room temperature and at high temperatures tends to decrease.
[0037] The RTB permanent magnet according to this embodiment further contains Si. The Si content is 0.35% by mass or more and 1.20% by mass or less, with the mass of the entire RTB permanent magnet being 100% by mass. It may be 0.55% by mass or more and 0.95% by mass or less. If the Si content is too low, the effect of improving HcJ due to the grain boundary diffusion of heavy rare earth elements described below decreases, and HcJ at room temperature and HcJ at high temperatures tend to decrease. Furthermore, Hk / HcJ also tends to decrease. If the Si content is too high, Br, HcJ at room temperature and HcJ at high temperatures tend to decrease. Moreover, if the Si content is too high or too low, the effect of improving HcJ due to the grain boundary diffusion of heavy rare earth elements described below tends to decrease.
[0038] The RTB permanent magnet according to this embodiment may further contain Al. The Al content may be 0% by mass or more and 0.45% by mass or less, 0.03% by mass or more and 0.45% by mass or less, or 0.05% by mass or more and 0.25% by mass or more, with the mass of the entire RTB permanent magnet being 100% by mass. When Al is 0.45% by mass or less, it is particularly easy to improve Br.
[0039] The RTB permanent magnet according to this embodiment further contains Zr. The Zr content is 0.21% by mass or more and 0.85% by mass or less, with the mass of the entire RTB permanent magnet being 100% by mass. It may be 0.33% by mass or more and 0.71% by mass or less. If the Zr content is too low, HcJ at room temperature, HcJ at high temperatures, and Hk / HcJ tend to decrease. If the Zr content is too high, Br tends to decrease.
[0040] The RTB permanent magnet according to this embodiment further contains Ga. The Ga content is 0.04% by mass or more and 0.40% by mass or less, with the mass of the entire RTB permanent magnet being 100% by mass. It may be 0.10% by mass or more and 0.37% by mass or less. If the Ga content is too low, the HcJ at room temperature and the HcJ at high temperatures tend to decrease. If the Ga content is too high, the Br tends to decrease.
[0041] The RTB permanent magnet according to this embodiment may further contain Cu. The Cu content may be from 0.03% to 0.50% by mass, from 0.04% to 0.45% by mass, or from 0.05% to 0.40% by mass, with the total mass of the RTB permanent magnet being 100% by mass.
[0042] The RTB permanent magnet according to this embodiment further contains C. The C content is 0.05% by mass or more and 0.11% by mass or less, with the mass of the entire RTB permanent magnet being 100% by mass. It may be 0.05% by mass or more and 0.10% by mass or less. If the C content is too low, Br is likely to decrease. If the C content is too high, HcJ at room temperature and HcJ at high temperatures are likely to decrease.
[0043] The RTB permanent magnet according to this embodiment may further contain O. The O content may be 0.35% by mass or less, or 0.11% by mass or less (not including 0% by mass), with the mass of the entire RTB permanent magnet being 100% by mass. In order to manufacture an RTB permanent magnet with low O content, it is necessary to reduce the oxygen concentration in the atmosphere during manufacture, so if there is little O, the manufacturing costs of the RTB permanent magnet are likely to increase. If there is too much O, Br, HcJ at room temperature, and HcJ at high temperatures are likely to decrease.
[0044] In the RTB permanent magnet according to this embodiment, the value obtained by dividing the Ga content by the Si content on a mass basis (hereinafter sometimes simply referred to as Ga / Si) may be 0.04 to 0.70, or 0.05 to 0.64. By keeping Ga / Si within the above range, it becomes easier to obtain an RTB permanent magnet that is all excellent in Br, HcJ at room temperature, HcJ at high temperatures, Hk / HcJ, and corrosion resistance.
[0045] The RTB permanent magnet according to this embodiment may contain other elements other than the above-mentioned rare earth elements, Fe, Co, Si, Al, Zr, Ga, Cu, B, C, and O. There are no particular restrictions on the content of the other elements, as long as they do not significantly affect the magnetic properties and corrosion resistance of the RTB permanent magnet. For example, the content of each of the other elements may be 0.1% by mass or less, and the total content may be 1.0% by mass or less, assuming that the mass of the entire RTB permanent magnet is 100% by mass.
[0046] The various components contained in the RTB permanent magnet according to this embodiment can be measured by a method generally known in the art. The amounts of various elements are measured, for example, by X-ray fluorescence analysis and inductively coupled plasma emission spectrometry (ICP analysis). The O content is measured, for example, by inert gas fusion-non-dispersive infrared absorption spectrometry. The C content is measured, for example, by combustion in an oxygen stream-infrared absorption spectrometry.
[0047] There are no particular limitations on the shape of the RTB permanent magnet according to this embodiment, and examples include a rectangular parallelepiped shape.
[0048] Below, a method for producing an RTB based sintered magnet will be described in detail as one example of a method for producing an RTB based permanent magnet according to this embodiment, but the method for producing an RTB based permanent magnet is not limited to this, and other known methods may be used.
[0049] [Raw powder preparation process] The raw material powder can be prepared by a known method. In this embodiment, a one-alloy method using a single alloy will be described, but a so-called two-alloy method in which two or more alloys with different compositions are mixed to prepare the raw material powder may also be used.
[0050] First, a raw material alloy for the RTB permanent magnet is prepared (alloy preparation step). In the alloy preparation step, raw material metals corresponding to the composition of the RTB permanent magnet according to this embodiment are melted by a known method, and then cast to produce a raw material alloy having the desired composition.
[0051] As the raw material metal, for example, a simple substance of a rare earth element, a simple substance of a metal element such as Fe or Co, an alloy consisting of a plurality of kinds of metals (e.g., an Fe-Co alloy), or a compound consisting of a plurality of kinds of elements (e.g., ferroboron, ferrosilicon) can be appropriately used. There is no particular limitation on the casting method for casting the raw material alloy from the raw material metal. A strip casting method may be used to obtain an RTB permanent magnet with high magnetic properties. The obtained raw material alloy may be subjected to a homogenization treatment by a known method as necessary.
[0052] After the raw alloy is prepared, it is pulverized (pulverization step). The atmosphere in each step from the pulverization step to the sintering step can have a low oxygen concentration in order to obtain high magnetic properties. For example, the oxygen concentration in the atmosphere in each step can be set to 200 ppm or less. By controlling the oxygen concentration in the atmosphere in each step, the O content in the RTB permanent magnet can be controlled.
[0053] The following describes the case where the pulverization process is carried out in two stages: a coarse pulverization process in which the particles are pulverized to a particle size of several hundred μm to several mm, and a fine pulverization process in which the particles are pulverized to a particle size of approximately several μm. However, the process may be carried out in a single stage, namely, the fine pulverization process alone.
[0054] In the coarse pulverization step, the material is coarsely pulverized until the particle size is about several hundred μm to several mm. This produces a coarsely pulverized powder. There is no particular limitation on the method of coarse pulverization, and it can be performed by a known method such as a method of hydrogen absorption pulverization or a method using a coarse pulverizer.
[0055] Next, the obtained coarsely pulverized powder is pulverized until the average particle size is about several μm (fine pulverization step). This produces finely pulverized powder (raw powder). The average particle size of the finely pulverized powder may be 1 μm or more and 10 μm or less, 2 μm or more and 6 μm or less, or 2 μm or more and 4 μm or less.
[0056] There is no particular limitation on the method of pulverization, and it can be carried out, for example, by a method using various pulverizers.
[0057] When the coarsely pulverized powder is pulverized, various grinding aids such as lauric acid amide and oleic acid amide can be added to obtain a finely pulverized powder in which the crystal grains tend to be oriented in a specific direction when pressed and molded in a magnetic field. In addition, the C content in the RTB permanent magnet can be controlled by changing the amount of grinding aid added.
[0058] [Molding process] In the molding process, the finely pulverized powder is molded into a desired shape. There are no particular limitations on the molding method. In this embodiment, the finely pulverized powder is filled into a mold and pressurized in a magnetic field. The resulting molded body has crystal grains oriented in a specific direction, resulting in an RTB permanent magnet with a higher Br.
[0059] The pressure during molding can be 20 MPa or more and 300 MPa or less. The magnetic field applied can be 950 kA / m or more, or 950 kA / m or more and 1600 kA / m or less. The magnetic field applied is not limited to a static magnetic field, and can also be a pulsed magnetic field. A static magnetic field and a pulsed magnetic field can also be used in combination.
[0060] As a molding method, in addition to the dry molding in which the finely pulverized powder is molded as is as described above, wet molding in which a slurry in which the finely pulverized powder is dispersed in a solvent such as oil can also be applied.
[0061] There is no particular restriction on the shape of the compact obtained by compacting the finely pulverized powder. The density of the compact at this stage is 4.0 Mg / m 3 ~4.3Mg / m 3 It can be said that:
[0062] [Sintering process] The sintering process is a process in which the compact is sintered in a vacuum or in an inert gas atmosphere to obtain a sintered body. The sintering conditions need to be adjusted depending on various conditions such as the composition, the crushing method, the particle size and particle size distribution, etc. For example, the compact is sintered by, for example, heating in a vacuum or in an inert gas atmosphere at 1000°C to 1200°C for 1 hour to 20 hours. By sintering under the above sintering conditions, a high-density sintered body can be obtained. In this embodiment, the density is at least 7.45 Mg / m 3 The density of the sintered body is 7.50Mg / m 3 It may be more than that.
[0063] [Aging treatment process] The aging treatment step is a step of subjecting the sintered body to a heat treatment (aging treatment) at a temperature lower than the sintering temperature. There is no particular restriction on whether or not the aging treatment is performed, and there is no particular restriction on the number of times the aging treatment is performed, and the aging treatment is performed appropriately depending on the desired magnetic properties. In addition, the grain boundary diffusion step described later may also serve as the aging treatment step. Hereinafter, an embodiment in which the aging treatment is performed twice will be described.
[0064] The first aging step is called the first aging step, the second aging step is called the second aging step, the aging temperature of the first aging step is called T1, and the aging temperature of the second aging step is called T2.
[0065] There is no particular limitation on T1 and the aging time in the first aging step. T1 can be 700° C. or more and 950° C. or less. The aging time can be 1 hour or more and 10 hours or less.
[0066] There is no particular limitation on T2 and the aging time in the second aging step. T2 can be 450° C. or more and 700° C. or less. The aging time can be 1 hour or more and 10 hours or less.
[0067] Such an aging treatment can improve the magnetic properties, particularly the HcJ, of the finally obtained RTB permanent magnet.
[0068] [Processing process (before grain boundary diffusion)] If necessary, a process may be included in which the sintered body according to the present embodiment is processed into a desired shape. Examples of the processing method include shaping such as cutting and grinding, and chamfering such as barrel polishing.
[0069] [Grain boundary diffusion process] The grain boundary diffusion step can be carried out by attaching a diffusion material to the surface of the sintered body and heating the sintered body to which the diffusion material is attached. Then, an RTB permanent magnet is obtained. In this embodiment, there is no particular limitation on the type of diffusion material. The diffusion material may contain a heavy rare earth element (e.g., Tb), or may contain a heavy rare earth element and Cu.
[0070] In the grain boundary diffusion process, as the temperature rises, the grain boundary phase, which has a high concentration of rare earth elements present in the grain boundaries of the magnet base material (sintered body), becomes a liquid phase, and the diffusion material dissolves into the liquid phase, causing the components of the diffusion material to diffuse from the surface of the magnet base material into its interior.
[0071] The magnet base material according to this embodiment has the characteristic that the Si content is within a predetermined range, etc. The diffusion material according to this embodiment has the above-mentioned characteristics.
[0072] Therefore, in this embodiment, the liquid phase generated during heating contains Si within a predetermined range. Compared to a magnet base material that does not contain Si, the reaction rate between the components of the diffusion material and the liquid phase is slower in a magnet base material containing Si. In addition, since the volume diffusion of the heavy rare earth element into the main phase particles is suppressed, the heavy rare earth element is more likely to diffuse to the center of the magnet base material. Therefore, good characteristics can be obtained with a relatively small diffusion amount of the heavy rare earth element. Furthermore, the diffusion of the heavy rare earth element makes it easier to improve HcJ at room temperature.
[0073] The diffusing material may be a slurry containing a solvent in addition to the above-mentioned heavy rare earth element hydride, etc. The solvent contained in the slurry may be a solvent other than water. For example, it may be an organic solvent such as alcohol, aldehyde, ketone, etc. Furthermore, the diffusing material may contain a binder. There is no particular limit to the type of binder. For example, a resin such as an acrylic resin may be contained as a binder. By containing a binder, the diffusing material is more likely to adhere to the surface of the sintered body.
[0074] The diffusion material may be a paste containing a solvent and a binder in addition to the above-mentioned heavy rare earth element hydride, etc. The paste has flowability and high viscosity. The viscosity of the paste is higher than that of the slurry.
[0075] Before the diffusion treatment described below, the sintered body to which the slurry or paste has been applied may be dried to remove the solvent and binder.
[0076] The holding temperature during drying may be 200°C or higher and 800°C or lower, and the holding time may be 10 minutes or higher and 10 hours or lower. The drying atmosphere is in an inert gas. By drying the sintered body to which the slurry or paste is attached, the generation of carbides of the heavy rare earth element formed on the surface of the magnet base material can be suppressed, and the amount of the heavy rare earth element used can be further reduced.
[0077] The diffusion treatment in the grain boundary diffusion step according to this embodiment may be performed consecutively from the drying. Alternatively, the diffusion treatment may be performed by cooling to room temperature once after the drying and then heating again. The holding temperature during the diffusion treatment may be 700°C or higher and 1000°C or lower. In the grain boundary diffusion step, the temperature of the magnet base material may be gradually increased from a temperature lower than the diffusion treatment temperature to the diffusion treatment temperature.
[0078] The time during which the temperature of the substrate is maintained at the diffusion treatment temperature (diffusion treatment time) may be, for example, 1 hour or more and 50 hours or less. The atmosphere around the substrate in the diffusion treatment step may be a non-oxidizing atmosphere. The non-oxidizing atmosphere may be, for example, a rare gas such as argon. The pressure of the atmosphere around the magnet substrate in the diffusion step may be 1 kPa or less. By creating such a reduced pressure atmosphere, the dehydrogenation reaction of the hydride is promoted, and the dissolution of the diffusion material into the liquid phase is easily promoted.
[0079] Furthermore, after the diffusion treatment, a further heat treatment may be performed. In this case, the heat treatment temperature may be 450°C or higher and 600°C or lower. The heat treatment time may be 1 hour or higher and 10 hours or lower. By performing such a heat treatment, it is possible to improve the magnetic properties of the finally obtained RTB permanent magnet, particularly the HcJ at room temperature and the HcJ at high temperatures.
[0080] [Processing process (after grain boundary diffusion)] After the grain boundary diffusion step, polishing may be performed to remove any remaining diffusion material on the surface of the RTB permanent magnet. The RTB permanent magnet may also be subjected to other processing. For example, surface processing such as shaping, such as cutting and grinding, and chamfering, such as barrel polishing, may be performed.
[0081] In this embodiment, processing steps are performed before and after the grain boundary diffusion, but these steps do not necessarily have to be performed. The grain boundary diffusion step may also serve as the aging step. There is no particular limitation on the heating temperature when the grain boundary diffusion step also serves as the aging step. It is particularly preferable to carry out the aging step at a temperature that is both preferred in the grain boundary diffusion step and also preferred in the aging step.
[0082] In particular, the RTB permanent magnet after grain boundary diffusion tends to have a concentration distribution in which the concentration of the heavy rare earth element decreases from the outside to the inside of the RTB permanent magnet. Furthermore, the main phase particles contained in the RTB permanent magnet after grain boundary diffusion tends to have the above-mentioned core-shell structure.
[0083] The RTB permanent magnet according to this embodiment thus obtained has the desired properties. Specifically, it has high Br, HcJ at room temperature, HcJ and Hk / HcJ at high temperatures, and excellent corrosion resistance. Furthermore, the diffusion of heavy rare earth elements has a significant effect on improving HcJ at room temperature.
[0084] The RTB permanent magnet according to this embodiment obtained by the above method becomes a magnetic RTB permanent magnet by magnetization.
[0085] The RTB permanent magnet according to this embodiment is suitable for use in motors, generators, and the like.
[0086] It should be noted that the present disclosure is not limited to the above-described embodiments, and various modifications can be made within the scope of the present disclosure.
[0087] The manufacturing method of the RTB permanent magnet is not limited to the above method and may be changed as appropriate. For example, the manufacturing method of the RTB permanent magnet described above is a manufacturing method by sintering, but the RTB permanent magnet according to this embodiment may be manufactured by hot working. The method of manufacturing an RTB permanent magnet by hot working includes the following steps. (a) A melting and quenching process in which raw metal is melted and the resulting bath is quenched to obtain a thin strip. (b) A grinding process in which the ribbon is pulverized to obtain a flake-shaped raw powder. (c) Cold forming process in which the crushed raw powder is cold-formed (d) A preheating step of preheating the cold-formed body (e) A hot forming process in which the preheated cold-formed body is hot-formed. (f) A hot plastic working process in which the hot-formed body is plastically deformed into a desired shape. (g) Aging treatment process for aging RTB permanent magnets The steps after the aging treatment are the same as those in the case of production by sintering. EXAMPLES
[0088] The present disclosure will be described below based on more detailed examples, but the present disclosure is not limited to these examples.
[0089] (Production of RTB permanent magnets) Raw material alloys were prepared by a strip casting method so that the composition of the final RTB permanent magnet would be the composition of each sample shown in Tables 1 to 3. The Pr content was between 0% and 12% by mass. N, H, Ca, La, Ce, Cr, and other elements not listed in Tables 1 to 3 may be detected. Ca, La, and Ce are mixed in from the rare earth raw material. Also, Cr may be mixed in from the electrolytic iron. The Fe content in Tables 1 to 3 is listed as bal. to indicate that the Fe content is essentially the remainder when the entire RTB permanent magnet including these other elements is taken as 100% by mass.
[0090] Next, hydrogen gas was flowed into the raw alloy at room temperature for 1 hour to absorb hydrogen, and then the atmosphere was switched to Ar gas, and dehydrogenation treatment was carried out at 500° C. for 1 hour, and the raw alloy was hydrogen-absorbed and crushed.
[0091] Next, 0.1% by mass of oleic acid amide was added as a grinding aid to the raw alloy powder, and the mixture was mixed using a Nauta mixer.
[0092] Next, the mixture was finely pulverized in a nitrogen gas flow using a collision plate type jet mill to obtain a fine powder (raw powder) having an average particle size of about 3.0 μm. The average particle size was the average particle size D50 measured by a laser diffraction type particle size distribution analyzer.
[0093] The obtained fine powder was molded in a magnetic field to produce a compact. The magnetic field applied was a static magnetic field of 1200 kA / m. The pressure during molding was 120 MPa. The magnetic field application direction and the pressure direction were perpendicular to each other.
[0094] Next, the green body was sintered to obtain a sintered body. The optimum sintering conditions differ depending on the composition, etc., but the temperature was kept within the range of 1030°C to 1070°C for 4 hours. The sintering atmosphere was a vacuum. The sintered density was 7.51 Mg / m 3 ~7.55Mg / m 3 Thereafter, a first aging treatment was performed in an Ar atmosphere at atmospheric pressure at a first aging temperature T1 of 800°C for 1 hour, and then a second aging treatment was performed at a second aging temperature T2 of 560°C for 2 hours. As a result, sintered bodies of the samples shown in Tables 1 to 3 were obtained.
[0095] The sintered body before grain boundary diffusion, which will be described later, was vertically processed to 11 mm long x 11 mm wide x 4.2 mm thick (the easy axis of magnetization is 4.2 mm), and HcJ was evaluated at room temperature using a BH tracer. Note that before measuring HcJ, the RTB permanent magnet was magnetized using a pulsed magnetic field of 4000 kA / m. In addition, because the thickness of the sintered body was thin, three sintered bodies were stacked together to evaluate HcJ.
[0096] (Preparation of diffusion material paste) Next, a diffusion material paste to be used for grain boundary diffusion was prepared.
[0097] First, hydrogen gas was flowed at room temperature to metal Tb with a purity of 99.9% to absorb hydrogen. Then, the atmosphere was switched to Ar gas, and dehydrogenation was performed at 500°C for 1 hour, and metal Tb was hydrogen-absorbed and crushed. Next, zinc stearate was added as a grinding aid at 0.05 mass% relative to 100 mass% metal Tb, and mixed using a Nauta mixer. After that, fine grinding was performed using a jet mill in an atmosphere containing 3000 ppm oxygen, and finely ground powder of Tb hydride with an average particle size of about 10.0 μm was obtained.
[0098] A diffusion material paste was prepared by kneading 60 parts by mass of finely pulverized powder of Tb hydride, 10 parts by mass of metallic Cu powder, 25 parts by mass of alcohol, and 5 parts by mass of acrylic resin. Note that the alcohol is a solvent, and the acrylic resin is a binder.
[0099] (Application of diffusion paste and heat treatment) The above sintered body was processed to a size of 11 mm long x 11 mm wide x 4.2 mm thick (thickness in the direction of easy magnetization 4.2 mm). Then, the body was immersed in a mixed solution of nitric acid and ethanol (100% by mass ethanol and 3% by mass nitric acid) for 3 minutes, and then immersed in ethanol for 1 minute, for an etching treatment. The etching treatment of immersing in the mixed solution for 3 minutes and then immersing in ethanol for 1 minute was performed twice.
[0100] Next, the above-mentioned diffusion material paste was applied to the entire surface of the sintered body after the etching treatment. The amount of the diffusion material paste applied was set so that the Tb content in the final RTB permanent magnet would be the value shown in Tables 1 to 3.
[0101] Next, the sintered body was dried. Specifically, the sintered body coated with the diffusion material paste was left in an oven at 400°C in an Ar gas atmosphere for 3 hours to remove the solvent and binder in the diffusion material paste. Then, the sintered body was heated at 900°C for 30 hours while flowing Ar at atmospheric pressure (1 atm). After that, the sintered body was heated at 560°C for 4 hours while flowing Ar at atmospheric pressure. From the above, the RTB permanent magnets of the samples shown in Tables 1 to 3 were obtained.
[0102] The surface of the RTB permanent magnet was scraped off by 0.1 mm on each side, and then the composition, magnetic properties, and corrosion resistance were evaluated.
[0103] The RTB permanent magnet was processed vertically to a size of 11 mm long x 11 mm wide x 4.2 mm thick (the easy axis direction of magnetization is 4.2 mm), and the magnetic properties were evaluated at room temperature using a BH tracer. The RTB permanent magnet was magnetized using a pulse magnetic field of 4000 kA / m before measuring the magnetic properties. Since the RTB permanent magnet was thin, three magnets were stacked to evaluate the magnetic properties. In this embodiment, Hk / HcJ was calculated by Hk / HcJ x 100 (%), with Hk (kA / m) being the magnetic field when the magnetization was 90% of Br in the second quadrant of the magnetization J-magnetic field H curve (JH demagnetization curve). The high-temperature HcJ, which is the HcJ when heated to 150°C, was also measured.
[0104] In this embodiment, a Br of 1400mT or more for the RTB permanent magnet was rated as good, with 1410mT or more being even better. A HcJ of 1850kA / m or more at room temperature for the RTB permanent magnet was rated as good, with 1900kA / m or more being even better. A high-temperature HcJ of 700kA / m or more for the RTB permanent magnet was rated as good, with 715kA / m or more being even better. A Hk / HcJ of 93.0% or more for the RTB permanent magnet was rated as good, with 95.0% or more being even better.
[0105] A corrosion resistance test was conducted on the RTB permanent magnet. The corrosion resistance test was carried out using a PCT test (Pressure Cooker Test) under saturated vapor pressure. Specifically, the RTB permanent magnet was placed in an environment of 2 atmospheres and 100% RH for 1000 hours, and the change in mass was measured before and after the test. The absolute value of the mass change per surface area of the RTB permanent magnet was 0.3 mg / cm 2 The corrosion resistance is considered to be good when the corrosion rate is less than 0.1 mg / cm 2 The corrosion resistance was deemed to be better when the following conditions were met: If the RTB permanent magnet itself crumbled into pieces, this was noted in the corrosion resistance column as "collapsed."
[0106] Furthermore, for each sample, the HcJ at room temperature after grain boundary diffusion was subtracted from the HcJ at room temperature before grain boundary diffusion to calculate ΔHcJ. The results are shown in Tables 1 to 3. A ΔHcJ of 750 kA / m or more was considered good, and a ΔHcJ of 850 kA / m or more was considered even better.
[0107] A comprehensive evaluation was performed on each sample in Tables 1 to 3. Samples in which Br, HcJ, ΔHcJ, high-temperature HcJ, Hk / HcJ and corrosion resistance were all better were rated A. Samples in which Br, HcJ, ΔHcJ, high-temperature HcJ, Hk / HcJ or corrosion resistance were not good were rated C. Samples in which none of the above were good were rated B. The results are shown in Tables 1 to 3.
[0108] [Table 1]
[0109] [Table 2]
[0110] [Table 3]
[0111] As can be seen from Tables 1 to 3, in each of the examples in which all compositions were within a specific range, good magnetic properties and corrosion resistance were obtained.
[0112] As can be seen from Table 1, sample No. 1, which had too much TRE, had reduced Br and corrosion resistance. Sample No. 7, which had too little TRE, had reduced HcJ at room temperature, HcJ and Hk / HcJ at high temperatures. Samples Nos. 8 and 9, which had too much Si, had reduced Br, HcJ at room temperature, HcJ and ΔHcJ at high temperatures. Sample No. 14, which had too little Si, had reduced HcJ, ΔHcJ, HcJ and Hk / HcJ at room temperature and high temperatures. Sample No. 22, which had too little Co, had reduced corrosion resistance.
[0113] As can be seen from Table 2, sample No. 23, which contained too much Zr, had a decreased Br. Sample No. 28, which contained too little Zr, had decreased HcJ at room temperature, and HcJ and Hk / HcJ at high temperatures. Sample No. 29, which contained too much Ga, had a decreased Br. Sample No. 34, which contained too little Ga, had decreased HcJ at room temperature and at high temperatures. Sample No. 35, which contained too much B, had decreased HcJ at room temperature and at high temperatures. Sample No. 39, which contained too little B, had decreased HcJ at high temperatures.
[0114] From Table 3, sample No. 44, which had too much HRE, had a decreased Br. Sample No. 48, which had too much C, had decreased HcJ at room temperature and at high temperatures. Sample No. 52, which had too little C, had a decreased Br.
[0115] For all the RTB permanent magnets of the examples and comparative examples, the Tb concentration distribution was analyzed using an electron probe microanalyzer (EPMA), and it was confirmed that the Tb concentration distribution decreased from the outside to the inside. [Explanation of symbols]
[0116] 1...RTB permanent magnet
Claims
1. Contains at least rare earth elements, Fe, Co, Si, Zr, Ga and B; Contains heavy rare earth elements as rare earth elements, The content of rare earth elements is 28.50% by mass to 31.50% by mass, The content of heavy rare earth elements is 0.30% by mass or less (excluding 0% by mass), The Co content is 0.20 mass% to 1.00 mass%; The Si content is 0.35% by mass to 1.20% by mass, The Zr content is 0.21 mass% to 0.85 mass%; The Ga content is 0.04% by mass to 0.40% by mass, The B content is 0.90 mass% to 1.02 mass%; An RTB system permanent magnet having a C content of 0 mass % to 0.11 mass %.
2. 2. The RTB system permanent magnet according to claim 1, wherein the value obtained by dividing the Ga content by the Si content on a mass basis is 0.04 to 0.
70.
3. 3. The R-T-B system permanent magnet according to claim 1, further comprising O, the O content being 0.11 mass % or less (excluding 0 mass %).
4. 3. The RTB system permanent magnet according to claim 1, further comprising Al, the Al content being 0.03 mass % to 0.45 mass %.
5. 3. The R-T-B system permanent magnet according to claim 1, wherein the concentration of the heavy rare earth element is distributed in a manner that decreases from the surface of the magnet toward the inside.
Citation Information
Patent Citations
Manufacturing method of r-t-b-based sintered magnet
JP2022052818A
Manufacturing method of r-t-b system sintered magnet and r-t-b system sintered magnet
JP2022151483A
R-t-b sintered magnet
WO2022065242A1
Magnetic material for high frequency use, and method for producing same
WO2022202760A1
R-t-b based permanent magnet
JP2020161812A