Zirconia powder for laser sintering, and method for producing zirconia sintered body by laser sintering
A zirconia powder with controlled composition facilitates laser sintering without alumina, resulting in dense zirconia sintered bodies with improved density and uniformity.
Patent Information
- Application Number
- JP2023047212
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
Existing laser sintering methods for zirconia require the inclusion of alumina or compounds other than zirconium compounds, which hinders efficient sintering and results in less dense zirconia sintered bodies.
A zirconia powder with controlled composition, including oxygen-deficient and stabilizing element-containing zirconia, is used for laser sintering without alumina or other compounds, allowing for uniform sintering and the production of dense zirconia sintered bodies.
The zirconia powder enables the production of dense zirconia sintered bodies with high actual density and uniform sintering across the surface and deep layers, surpassing conventional methods in terms of density and structural integrity.
Smart Images

Figure 2024136186000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a zirconia powder for laser sintering and a method for producing a zirconia sintered body by laser sintering. [Background technology]
[0002] A method of sintering ceramics by irradiating them with a laser, known as laser sintering, is being investigated.
[0003] For example, Patent Document 1 discloses that a structure with high smoothness on the surface and sides can be obtained by sintering inorganic powder containing various absorbents on an alumina base material with a laser.
[0004] Furthermore, Patent Document 2 discloses laser sintering in which a mixed powder consisting of black yttria powder and aluminum oxide or aluminum nitride powder is molded and irradiated with a laser to form a sintered body. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2020-100141 A [Patent Document 2] International Publication No. 2021 / 172128 Summary of the Invention [Problem to be solved by the invention]
[0006] The laser sintering described in Patent Document 1 and Patent Document 2 is a sintering method in which an alumina eutectic and alumina are sintered by a laser, and both of these sintering methods require the inclusion of alumina and compounds other than aluminum compounds. In contrast, zirconia, which is also an inorganic oxide, is less susceptible to sintering than alumina. Thus, it has not been reported that a zirconia sintered body can be obtained by laser sintering without the inclusion of alumina and compounds other than zirconium compounds.
[0007] In view of these problems, the present disclosure has an object to provide at least one of a novel zirconia powder for laser sintering that enables sintering of zirconia by laser sintering without the inclusion of alumina or the use of compounds other than zirconium compounds, in particular a novel zirconia powder for laser sintering that can produce a dense zirconia sintered body by irradiating it with a laser, and a method for producing a sintered body by laser sintering using the same. [Means for solving the problem]
[0008] The present inventors have investigated the sintering of zirconia by laser sintering, and as a result, have found that by using zirconia with a controlled composition and controlling the color tone, laser sintering can proceed using only zirconia, without the inclusion of alumina or the inclusion of any compound other than the zirconium compound.
[0009] That is, the present invention is as described in the claims, and the gist of the present disclosure is as follows.
[0010] [1] A composite material comprising oxygen-deficient zirconia and a zirconia different from the oxygen-deficient zirconia, and further comprising L * a * b * Lightness L in color system * Zirconia powder for laser sintering, having a molecular weight of 94 or less. [2] The zirconia powder for laser sintering according to the above [1], wherein the content of the oxygen-deficient zirconia relative to the mass of the zirconia powder for laser sintering is 0.5 mass% or more and 10 mass% or less. [3] The zirconia powder for laser sintering according to the above [1] or [2], wherein one or more selected from the group consisting of the oxygen-deficient zirconia and the zirconia different from the oxygen-deficient zirconia is a stabilizing element-containing zirconia. [4] The zirconia powder for laser sintering according to the above [3], wherein the stabilizing element is one or more selected from the group consisting of calcium, magnesium and yttrium. [5] A method for producing a sintered body, comprising the step of irradiating a molded body containing the zirconia powder for laser sintering described in any one of [1] to [4] above with laser light to obtain a sintered body. Effect of the Invention
[0011] The present disclosure makes it possible to provide at least one of a novel zirconia powder for laser sintering that enables sintering of zirconia by laser sintering without the inclusion of alumina and without the essential use of compounds other than zirconium compounds, in particular a novel zirconia powder for laser sintering that can give a dense zirconia sintered body by irradiating it with a laser, and a method for producing a sintered body by laser sintering using the same. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a diagram showing a scanning electron microscope image of the surface of the surface layer portion near the laser irradiated surface of the zirconia sintered body of Example 1, which contains oxygen-deficient zirconia. [Diagram 2] FIG. 1 is a diagram showing a scanning electron microscope image of a cross section of a surface layer portion near a laser irradiated surface in a zirconia sintered body of Example 4 containing oxygen-deficient zirconia. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] In this specification, a numerical range indicated using "~" indicates a range that includes the numerical values before and after "~" as the minimum and maximum values, respectively.
[0014] A "powder" is an aggregate of powder particles (at least one of primary particles and secondary particles) and is a composition having flowability. A "zirconia powder" is a powder whose main component is zirconia, and is essentially a powder consisting of zirconia. In this specification, the individual particles that make up the aggregate "powder" are called "powder particles" to distinguish them from the aggregate "powder."
[0015] A "molded body" is a composition having a certain shape composed of powder particles aggregated by physical force, and in particular, a composition in a state in which no heat treatment has been performed after the shape has been imparted (e.g., after molding). For example, a "molded body" can be obtained by agglomerating the "powder" by physical force and imparting a certain shape. A "zirconia molded body" is a molded body whose main component is zirconia, and is essentially made of zirconia. The term "molded body" is also used interchangeably with "powder compact."
[0016] A "sintered body" is a composition having a certain shape composed of crystal grains, and is a composition in a state in which it has been heat-treated at a temperature equal to or higher than the sintering temperature. For example, a "sintered body" can be obtained by heat-treating the "molded body" at a temperature equal to or higher than the sintering temperature. A "zirconia sintered body" is a sintered body whose main component is zirconia, and is essentially a sintered body made of zirconia.
[0017] A "major component" refers to a component that becomes the main phase (matrix, base material, parent phase) in the composition of the composition, and preferably a component that accounts for a mass proportion of the composition of 60 mass% or more, 75 mass% or more, 85 mass% or more, 90 mass% or more, 95 mass% or more, 98 mass% or more, or 99 mass% or more, or less than 100 mass%.
[0018] "Consists essentially of component X" or "consists substantially of component X" means that the mass ratio of component X in the target object is 98% by mass or more, 99% by mass or more, or 99.5% by mass or more, and is 100% by mass or less, or less than 100% by mass. "Consists essentially of component X" or "consists substantially of component X" can also be rephrased as "consists essentially only of component X" or "consists substantially only of component X".
[0019] The term "stabilizing element" refers to an element that stabilizes the crystal phase of zirconia by dissolving in the zirconia.
[0020] "BET specific surface area" is the specific surface area [m2] measured by the BET multipoint method (5 points) using nitrogen as the adsorption gas in accordance with JIS R 1626:1996.2 / g], in particular the BET specific surface area measured under the following conditions:
[0021] Adsorption medium: N2 Adsorption temperature: -196℃ Pretreatment conditions: Degassing in air at 250℃ for 1 hour or more The BET specific surface area can be measured using a general specific surface area measuring device (for example, Tristar II 320, manufactured by Shimadzu Corporation).
[0022] "Color tone (L * , a * , b * )" and "Saturation (C * ) can be obtained using a spectrophotometer (e.g. Spectrophotometer SD 3000, manufactured by Nippon Denshoku Industries Co., Ltd.) equipped with an illumination and light receiving optical system conforming to the geometric condition c of JIS Z 8722:2009, and using values measured by the SCE method. Specific measurement conditions for color tone are as follows, using a white plate as the background (so-called white back measurement).
[0023] Light source: D65 light source Viewing angle: 10° Measurement method: SCE Lightness L * is an index of brightness and has a value between 0 and 100. * and b * is an index of color tone and has a value between -100 and 100. * is an index of vividness, and hue a * and b * From C * ={(a * ) 2 +(b * ) 2} 0.5 It is calculated by:
[0024] In this embodiment, the color tone of the powder is measured by sieving the powder through a sieve with an opening of 500 μm, uniaxially pressing the powder at 50 MPa to form a disk-shaped molded body with a diameter of 12 mm and a thickness of 1±0.5 mm, and measuring the color tone of the surface of the molded body. Note that the "diameter" is the diameter of the circumscribing circle of the disk shape.
[0025] "Measured density" is the density of the sample [cm 3 ] and the value [g / cm 3 The mass was determined by weighing the sample. The volume was determined by the Archimedes method according to JIS R 1634:1998. The Archimedes method used ion-exchanged water as the solvent, and the pretreatment was performed by boiling.
[0026] <Zirconia powder for laser sintering> Hereinafter, the zirconia powder for laser sintering of the present disclosure will be described with reference to an example of an embodiment. This embodiment includes oxygen-deficient zirconia and zirconia different from the oxygen-deficient zirconia, and further includes L * a * b * Lightness L in color system * A zirconia powder for laser sintering, having a refractive index of 94 or less.
[0027] The zirconia powder for laser sintering of the present embodiment is a zirconia powder that can be sintered by laser irradiation without the inclusion of alumina or the inclusion of any compound other than a zirconium compound, and has a particularly high lightness L * In this respect, the zirconia powder exhibits a color other than the color that zirconia (ZrO2) originally has. In other words, the zirconia powder for laser sintering of the present embodiment is a zirconia powder having a color tone that can absorb laser light.
[0028] As described above, the zirconia powder for laser sintering of this embodiment is a new zirconia powder for laser sintering that enables sintering of zirconia by laser sintering without the inclusion of alumina or the inclusion of any compound other than the zirconium compound, and in particular is a new zirconia powder for laser sintering that can obtain a dense zirconia sintered body by irradiating a laser. Since the sintering of zirconia by laser irradiation proceeds more uniformly regardless of the reduction in the sintering temperature due to the eutectic of alumina, etc., it is preferable that the zirconia powder for laser sintering of this embodiment does not contain alumina.
[0029] Moreover, the zirconia powder for laser sintering of this embodiment preferably does not contain any compounds other than zirconium compounds, and more preferably consists essentially of zirconia.
[0030] By laser sintering the zirconia powder for laser sintering of this embodiment, a sintered body having a thickness of, for example, 1.0±0.5 mm can be obtained, in which the surface layer and the deep layer in the thickness direction are sintered uniformly and densely. The measured density of the zirconia sintered body obtained by laser sintering the zirconia powder for laser sintering of this embodiment is higher than that of a conventional zirconia sintered body obtained by laser sintering, and is, for example, 4.00 g / cm 3 Above 5.00g / cm 3 , or even 5.40g / cm 3 This is because the relative density (true density) is 6.05 g / cm 3 This corresponds to 70% or more, more preferably 80% or more, and further 90% or more as the relative density. The relative density is 100% or less.
[0031] (Zirconia) The zirconia powder for laser sintering of the present embodiment contains oxygen-deficient zirconia and zirconia different from oxygen-deficient zirconia (hereinafter also referred to as "stoichiometric zirconia"). In this specification, oxygen-deficient zirconia and stoichiometric zirconia may be simply referred to as "zirconia" without distinction.
[0032] (stoichiometric zirconia) The stoichiometric zirconia may be zirconia having a composition of ZrO2. The stoichiometric zirconia is preferably zirconia containing a stabilizing element. The stabilizing element-containing zirconia is more preferably zirconia containing one or more selected from the group consisting of calcium (Ca), magnesium (Mg) and yttrium (Y), and is even more preferably zirconia containing yttrium. The stabilizing element only needs to have a function of stabilizing the crystal structure of the stoichiometric zirconia, and does not have to substantially contribute to increasing the laser absorption efficiency in the zirconia powder for laser sintering.
[0033] The zirconia powder for laser sintering of this embodiment includes stoichiometric zirconia in powder form.
[0034] The zirconia powder for laser sintering of the present embodiment may contain one type of stoichiometric zirconia alone, or may contain two or more types of stoichiometric zirconia in combination at any ratio.
[0035] (oxygen deficient zirconia) Oxygen-deficient zirconia is zirconia in which at least a portion of the zirconia is oxygen-deficient, and is represented by ZrO 2-x (where x>0). Oxygen-deficient zirconia has a darker color tone than stoichiometric zirconia due to oxygen deficiency. This not only promotes sintering, but also eliminates oxygen deficiency associated with laser sintering, thereby obtaining a sintered body substantially made of stoichiometric zirconia by laser sintering. The oxygen-deficient zirconia preferably contains a stabilizing element. The stabilizing element-containing zirconia is more preferably zirconia containing one or more stabilizing elements selected from the group consisting of calcium (Ca), magnesium (Mg) and yttrium (Y), and is even more preferably yttrium-containing oxygen-deficient zirconia. The stabilizing element only needs to have a function of stabilizing the crystal structure of oxygen-deficient zirconia, and does not have to substantially contribute to increasing the laser absorption efficiency in the zirconia powder for laser sintering.
[0036] The zirconia powder for laser sintering of the present embodiment contains oxygen-deficient zirconia in the form of a powder.
[0037] The zirconia powder for laser sintering of the present embodiment may contain one type of oxygen-deficient zirconia alone, or may contain two or more types of oxygen-deficient zirconia in combination at any ratio.
[0038] (Stoichiometric zirconia content) The content of stoichiometric zirconia in the zirconia powder for laser sintering of this embodiment is appropriately set according to the content of oxygen-deficient zirconia. The content of stoichiometric zirconia relative to the mass of the zirconia powder for laser sintering is preferably 60% by mass or more and 99.5% by mass or less, 90% by mass or more and 99.5% by mass or less, 70% by mass or more and 99% by mass or less, or 90% by mass or more and 98% by mass or less. This makes it possible to obtain a zirconia powder for laser sintering containing stoichiometric zirconia as the main component.
[0039] (Oxygen-deficient zirconia content) The content of oxygen-deficient zirconia in the zirconia powder for laser sintering of this embodiment is the lightness L * is an arbitrary amount as long as it shows a desired value. The content of oxygen-deficient zirconia relative to the mass of the zirconia powder for laser sintering is preferably 0.5% by mass or more and 40% by mass or less, 0.5% by mass or more and 10% by mass or less, 1% by mass or more and 30% by mass or less, or 2% by mass or more and 10% by mass or less. This makes it easier to proceed with sintering of the zirconia powder for sintering in laser sintering.
[0040] (stabilizing element content) The content of the stabilizing element contained in each of the zirconia powder for laser sintering, stoichiometric zirconia, and oxygen-deficient zirconia of this embodiment is arbitrary within a range that can exhibit the function of stabilizing the crystal structure of zirconia in a cubic or tetragonal crystal. For example, the content of the stabilizing element calculated as an oxide relative to the zirconia and the stabilizing element calculated as an oxide contained in each of the zirconia powder for laser sintering, stoichiometric zirconia, and oxygen-deficient zirconia of this embodiment can be 2 mol% or more or 2.5 mol% or more, and can be 10 mol% or less, 8 mol% or less, 7 mol% or less, or 4.5 mol% or less. The content of the stabilizing element in the zirconia powder for laser sintering, stoichiometric zirconia, and oxygen-deficient zirconia may be different from each other or may be the same.
[0041] When performing calculations based on the composition, such as calculating the content of stabilizing elements, hafnia, which is an inevitable impurity of zirconia, may be calculated by regarding it as zirconia.
[0042] (Other Ingredients) The zirconia powder for laser sintering of this embodiment may contain components other than stoichiometric zirconia, oxygen-deficient zirconia, and stabilizing elements, as long as the effects are not impaired. Examples of such components include at least one of a solvent and a binder. Examples of the solvent include at least one of water and an organic solvent, and further at least one of water and an alcohol. By including a solvent in the zirconia powder for laser sintering of this embodiment, it can be applied as a slurry. On the other hand, the binder improves the moldability and shape retention of the zirconia powder for laser sintering of this embodiment. Examples of the binder include polymer binders, and further one or more selected from the group consisting of polyvinyl butyral, polyvinyl acetate, polyvinyl alcohol, acrylic esters, and emulsions of acrylic esters.
[0043] For example, when the zirconia powder for laser sintering of this embodiment is a zirconia powder for laser sintering containing oxygen-deficient zirconia, stoichiometric zirconia, and a polymer binder, and the oxygen-deficient zirconia and the stoichiometric zirconia are each yttrium-stabilized zirconia, the mass of the zirconia powder for laser sintering can be calculated from Y2O3+ZrO2, and the content of the stabilizing element can be calculated from {Y2O3 / (Y2O3+ZrO2)}×100[mol%]. The content of the polymer binder can be calculated from {(W2-W1) / W2}×100[mass%] (wherein W1 is the mass of the zirconia powder for laser sintering after heat treatment in air at 150°C for 2 hours, and W2 is the mass of the zirconia powder for laser sintering before the heat treatment).
[0044] (color tone) The zirconia powder for laser sintering of this embodiment is L * a * b * Lightness L in color system * The L of the zirconia powder for laser sintering of this embodiment is 94 or less, and preferably 90 or less or 85 or less. * a * b * Lightness L in color system * By setting the upper limit of the above range, the laser absorption efficiency can be increased, and the sintering of zirconia proceeds quickly and sufficiently. * is 0 or more, and the lightness L * The L of the zirconia powder for laser sintering of this embodiment may be 0 or more, 50 or more, 70 or more, or 80 or more. * a * b * Lightness L in color system * When the lower limit is within the above range, sintering by laser sintering can proceed in a relatively short time.
[0045] The color tone of the zirconia powder for laser sintering of this embodiment is the above-mentioned brightness L * If it satisfies, then hue a * and b *are arbitrary, and can be, for example, −100 or more and 100 or less, further −10 or more and 10 or less, further −5 or more and 5 or less, and further −3 or more and 3 or less. The zirconia powder for laser sintering of this embodiment preferably exhibits an achromatic color, which is the inherent color tone of zirconia, or preferably white, and the chroma C * is preferably 3 or less, or 2 or less, and can be, for example, 0 or more, or 0.5 or more.
[0046] (Method of manufacturing zirconia powder for laser sintering) The zirconia powder for laser sintering of this embodiment may be produced by any method as long as it satisfies the above requirements. An example of such a method is a production method having a step of mixing stoichiometric zirconia powder and oxygen-deficient zirconia powder.
[0047] The stoichiometric zirconia powder used in the step of mixing the stoichiometric zirconia powder and the oxygen-deficient zirconia powder (hereinafter also referred to as the "mixing step") is a non-colored zirconia powder including zirconia having no oxygen deficiency, and has a lightness of, for example, L * The zirconia powder preferably has a molecular weight of more than 94 and not more than 100.
[0048] The oxygen-deficient zirconia powder subjected to the mixing step may be the same as the oxygen-deficient zirconia contained in the zirconia powder for laser sintering of this embodiment.
[0049] Furthermore, the stoichiometric zirconia powder and the oxygen-deficient zirconia powder are each preferably a stabilizing element-containing zirconia powder, more preferably a zirconia powder containing one or more elements selected from the group consisting of calcium (Ca), magnesium (Mg) and yttrium (Y), and even more preferably an yttrium-containing zirconia powder.
[0050] The content of the stabilizing element contained in the stoichiometric zirconia powder and the oxygen-deficient zirconia powder is arbitrary, but for example, the content of the stabilizing element calculated as an oxide relative to the zirconia and the stabilizing element calculated as an oxide contained in the zirconia powder can be 2 mol% or more or 2.5 mol% or more, and can be 10 mol% or less, 8 mol% or less, 7 mol% or less, or 4.5 mol% or less.
[0051] The mixing method in the mixing step may be such that the stoichiometric zirconia powder and the oxygen-deficient zirconia powder are mixed uniformly, and examples of such a mixing method include at least one of wet mixing and dry mixing, and further, pulverization mixing using a ball mill.
[0052] After mixing, the resulting mixture may be dried, if necessary.
[0053] (Method of manufacturing oxygen-deficient zirconia powder) The oxygen-deficient zirconia powder can be produced by any method, for example, by treating stoichiometric zirconia in a strong reducing atmosphere. Examples of such treatment include at least one of a treatment of irradiating stoichiometric zirconia with an electron beam (hereinafter also referred to as a "beam irradiation treatment") and a treatment of firing in a strong reducing atmosphere (hereinafter also referred to as a "reducing firing treatment").
[0054] It is preferable to produce oxygen-deficient zirconia by beam irradiation treatment, since it is easy to obtain zirconia powder for laser sintering having a color tone suitable for laser sintering. Note that the present embodiment also includes a method for producing a zirconia powder for laser sintering, which includes a step of irradiating zirconia with an electron beam to obtain oxygen-deficient zirconia, and a step of pulverizing the oxygen-deficient zirconia to obtain oxygen-deficient zirconia powder.
[0055] The conditions for the beam irradiation treatment are arbitrary. When oxygen-deficient zirconia is produced by irradiating stoichiometric zirconia with an electron beam, it is preferable to irradiate at least one of a stoichiometric zirconia powder, a molded body, and a sintered body with the electron beam, and it is more preferable to irradiate a sintered body with the electron beam.
[0056] The conditions for electron beam irradiation are as follows: Irradiation atmosphere: 10 -6 ~10 Pa, and even 10 -5 ~10 -3 Pa vacuum atmosphere, Irradiation power: 0.3kW / cm 2 More preferably, 1kW / cm 2 End Irradiation time: unit area (cm 2 ) for more than 1 second, or even more than 20 seconds.
[0057] The oxygen-deficient zirconia obtained by irradiating with the electron beam is appropriately pulverized and classified, and then subjected to a reduction firing treatment under the following conditions, for example. Treatment atmosphere: Hydrogen atmosphere or carbon monoxide atmosphere Treatment temperature: 1000℃ to 1400℃ The oxygen-deficient zirconia obtained by the reduction and firing treatment may be mixed with a solvent such as pure water to form a slurry, which may then be pulverized and dried to form a powder.
[0058] <Method of manufacturing zirconia sintered body> Hereinafter, the manufacturing method of the zirconia sintered body of the present disclosure will be described with reference to an example of the embodiment. The zirconia sintered body according to this embodiment can be manufactured by a manufacturing method having a step of irradiating a molded body containing the zirconia powder for laser sintering with a laser. That is, the manufacturing method of the zirconia sintered body according to this embodiment has a step of irradiating a laser beam to a molded body containing the zirconia powder for laser sintering of this embodiment to obtain a sintered body.
[0059] The above step (hereinafter also referred to as the "irradiation step") is a step of obtaining a sintered body by irradiating a molded body containing the zirconia powder for laser sintering of this embodiment with laser light.
[0060] (Molded body) The molded body to be subjected to the irradiation step is a molded body containing the zirconia powder for laser sintering of this embodiment, and is preferably a molded body consisting of only the zirconia powder for laser sintering of this embodiment.
[0061] The molded body can be obtained by a known molding method for ceramic powder. The molding method may be one or more molding methods selected from the group consisting of uniaxial pressing, CIP treatment, sheet molding, injection molding, and slip casting molding. For example, the zirconia powder for laser sintering of the present embodiment is filled into a mold, and uniaxially pressed at a molding pressure of 20 MPa to 80 MPa to obtain a molded body.
[0062] (conditions) In the irradiation step, the molded article is irradiated with a laser.
[0063] From the viewpoint of reactivity, it is preferable to use a laser having a wavelength of 500 nm or more and 11 μm or less as the light source of the laser. The laser used in the irradiation step may be one or more selected from the group consisting of a fiber laser, a Nd:YAG laser, a Nd:YVO laser, a Nd:YLF laser, a titanium sapphire laser, and a carbon dioxide gas laser.
[0064] The laser irradiation conditions may be appropriately selected depending on the sintered area (also referred to as the main area) of the molded body of the zirconia powder for laser sintering, the sintered depth of the molded body, and the like.
[0065] For smooth sintering, the laser output is set to 50W / cm 2 More than 2000W / cm 2 Below that, 100W / cm 2 More than 500W / cm 2 The irradiation time is preferably 1 second or more or 5 seconds or more and 60 minutes or less or 30 minutes or less.
[0066] The atmosphere for laser irradiation is not particularly limited as long as it is an oxygen atmosphere or a reducing atmosphere, and examples of the atmosphere include an air atmosphere, a nitrogen atmosphere, an argon atmosphere, and a helium atmosphere, and the air atmosphere is sufficient.
[0067] Prior to the laser irradiation, the molded body may be preheated. This allows the sintering by laser sintering to proceed more easily. The preheating temperature is 300°C or higher or 400°C or higher, and 1000°C or lower. The preheating method is not particularly limited, and may be one or more selected from the group consisting of an infrared lamp, a halogen lamp, resistance heating, high-frequency induction heating, and microwave heating.
[0068] The method of laser irradiation may be any method that allows the sintering of the molded body to proceed, but when sintering a large area of a molded body, examples include a method in which the molded body is fixed and the laser is irradiated while moving, and a method in which the laser light path is changed through a light diffusion lens and the molded body is irradiated while moving, and still other examples include a method in which the laser light path is fixed and the molded body is irradiated while moving.
[0069] <Zirconia sintered body> The zirconia sintered body produced by the method for producing a zirconia sintered body of the present embodiment is also included in the scope of the present disclosure. Since the zirconia sintered body of the present embodiment is produced by the method for producing a zirconia sintered body of the present embodiment, it can be a dense zirconia sintered body.
[0070] The zirconia sintered body of this embodiment is preferably a sintered body consisting of crystal grains formed by sintering the particles constituting the zirconia powder for laser sintering according to this embodiment.
[0071] According to the method for producing a zirconia sintered body of the present embodiment, for example, a sintered body having a thickness of 1.0±0.5 mm can be obtained, in which the surface layer and the deep layer in the thickness direction are sintered uniformly and densely. Therefore, the measured density of the zirconia sintered body is 4.00 g / cm, which is higher than that of a conventional zirconia sintered body obtained by laser sintering. 3 Above 5.00g / cm 3 , or even 5.40g / cm 3 This is because the relative density (true density) is 6.05 g / cm 3 Assuming that the density is 6.00 g / cm3, this corresponds to 70% or more, more preferably 80% or more, and even more preferably 90% or more. The higher the measured density, the better, but 3 Less than or equal to 5.65g / cm 3 The following can be given as examples.
[0072] The shape and size of the crystal grains of the zirconia sintered body of the present embodiment are not particularly limited, and examples thereof include a crystal grain diameter of 0.5 μm or more or 4 μm or more and 13 μm or less or 10 μm or less. The "crystal grain diameter" is a value measured by an intercept method.
[0073] The shape of the zirconia sintered body of the present embodiment is not particularly limited, and can be any shape depending on the purpose and use, such as a sphere, an oval sphere, a polyhedron, a line, a plate, or an irregular shape.
[0074] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention. EXAMPLES
[0075] The present disclosure will be described below using examples, but the present disclosure is not limited to these.
[0076] Synthesis Example 1 (Synthesis of oxygen-deficient zirconia) A 4 mol% yttria-containing zirconia powder (product name: TZ-4YS, manufactured by Tosoh Corporation) was molded and sintered to obtain a YSZ (yttria-stabilized zirconia) sintered body. -5 Under a vacuum of 10 Pa, an electron beam (3.0 kW / cm 2 ) was irradiated for 30 seconds per unit area. This resulted in a black oxygen-deficient zirconia sintered body. The resulting oxygen-deficient zirconia sintered body was pulverized in an alumina mortar to obtain oxygen-deficient zirconia powder (reduced YSZ powder).
[0077] Example 1 4.00 g of 3 mol% yttria-containing zirconia powder (stoichiometric zirconia) (product name: TZ-3YS, manufactured by Tosoh Corporation), 1.00 g of the oxygen-deficient zirconia powder obtained in Synthesis Example 1, and ethanol were mixed to form a slurry, and the resulting slurry was mixed for 24 hours in a ball mill equipped with zirconia balls having a diameter of 10 mm as a medium, and after removing the zirconia balls, the solvent was removed with an evaporator and dried to obtain the zirconia powder for laser sintering of this example. The composition of the zirconia powder for laser sintering of this example is shown in Table 1.
[0078] 0.2 g of the obtained powder was filled into a tablet molding machine and uniaxially pressed at a molding pressure of 10 MPa to form a disk-shaped molded body with a diameter of 10 mm and a thickness of 1 mm.
[0079] [Examples 2 to 8] The zirconia powders for laser sintering of Examples 2 to 8 were prepared in the same manner as in Example 1, except that the stoichiometric zirconia powder shown in Table 1 was used instead of the 3 mol% yttria-containing zirconia powder, and the content of the oxygen-deficient zirconia powder obtained in Synthesis Example 1 was set to the amount shown in Table 1.
[0080] Comparative Example 1 Zirconia powder of Comparative Example 1 was prepared in the same manner as in Example 1, except that no oxygen-deficient zirconia powder was used.
[0081] [Table 1]
[0082] [Evaluation of color tone] The color tones of the powders of the examples and comparative examples were measured by the following method. The powders sieved through a sieve with 500 μm openings were uniaxially pressed at 50 MPa to form disk-shaped molded bodies with a diameter of 12 mm and a thickness of 1±0.5 mm, and the color tones of the main surfaces of the molded bodies were measured under the following conditions. That is, measurements were performed using a color difference meter (Spectrophotometer SD 3000, manufactured by Nippon Denshoku Industries Co., Ltd.) with a white plate as the background (so-called white back measurement) under the following conditions. The results are shown in Table 2.
[0083] Light source: D65 light source Viewing angle: 10° Measurement method: SCE
[0084] [Table 2]
[0085] All the powders in the examples have a lightness of L * On the other hand, the powder of the comparative example had a lightness L * was over 94.
[0086] [Evaluation of sinterability] The powder compacts of the examples and comparative examples were placed and fixed on a SUS sample stage, and in an air atmosphere, the entire main surface (face with a diameter of 10 mm) of the compacts not in contact with the sample stage was irradiated with a fiber laser (wavelength: 1070 nm) while continuously sweeping. The conditions for laser irradiation were a spot diameter of 9 mm, a laser output of 200 W, and an irradiation time of 30 seconds. In this way, zirconia sintered bodies (laser sintered bodies) of the comparative examples and each example were obtained. The actual density of the obtained sintered bodies was measured by the following method. That is, the samples were weighed to determine the mass. In addition, the volume was obtained by the Archimedes method according to JIS R 1634:1998. The Archimedes method used ion-exchanged water as the solvent, and pretreatment was performed by boiling. The obtained volume [cm 3 ], the measured density [g / cm 3 In addition, for Examples 1 and 2 and Comparative Example 1, in which 3 mol % yttrium-containing zirconia powder was used as the stoichiometric zirconia, the true density was 6.05 g / cm 3 The relative density was calculated as the ratio of the actually measured density to the true density. The results are shown in Table 3.
[0087] [Table 3]
[0088] Lightness L * By laser sintering the zirconia powder for laser sintering of the following examples, the measured density of the powder consisting of zirconia alone is 4.00 g / cm 3 A zirconia sintered body (laser sintered body) with a lightness L * The powder of the comparative example having a zirconia sintering density of 99.23 was laser sintered, and the measured density of the obtained zirconia sintered body (laser sintered body) was 3.54 g / cm 3 It was confirmed that the sintered body consisting of stoichiometric zirconia alone did not undergo densification.
[0089] [Table 4]
[0090] The true density decreases with an increase in the stabilizing element. However, it was confirmed that, although Examples 3 to 8 are zirconia powders having a high content of stabilizing elements as stoichiometric zirconia, densification is more advanced than in Comparative Example 1, which contains 3 mol% yttrium-containing zirconia as stoichiometric zirconia.
[0091] [Evaluation of deep sintering] Fig. 1 is a scanning electron microscope (SEM) image (magnification: 2500 times) of the surface irradiated with the laser of the zirconia sintered body of Example 1, and Fig. 2 is an SEM image (magnification: 1000 times) of a cross section in a deep layer part close to the surface irradiated with the laser of the zirconia sintered body of Example 4. As shown in the SEM images of Fig. 1 and Fig. 2, the zirconia sintered body of the example had almost no voids in both the surface layer part and the deep layer part irradiated with the laser, and it was confirmed that the zirconia sintered body of the example was sufficiently sintered from the surface layer part to the deep layer part.
[0092] From the above results, it is considered that the zirconia containing oxygen deficiency and stoichiometric zirconia and L * a * b * Lightness L in color system * It was shown that the zirconia powders for laser sintering of the examples, which have a molecular weight of 94 or less, can obtain a zirconia sintered body by irradiating a laser without the inclusion of alumina and without the use of any compound other than the zirconium compound. Furthermore, it was shown that the zirconia sintered body obtained by laser sintering the zirconia powders for laser sintering of the examples has a dense crystal structure formed from the surface layer to the deep layer. [Industrial Applicability]
[0093] According to the present disclosure, it is possible to obtain a zirconia sintered body in which grains have been sufficiently grown in the depth direction from the surface. Therefore, it is possible to efficiently manufacture components known as uses of the zirconia sintered body, including, for example, structural materials, decorative materials, exterior components for electronic devices, high-temperature components (heat dissipation components, heat treatment containers, setters, furnace core tubes, temperature measuring protective tubes, etc.), insulating materials, light emitting tubes, etc.
Claims
1. A composite material comprising oxygen-deficient zirconia and a zirconia different from the oxygen-deficient zirconia, and further comprising L * a * b * Lightness L in color system * A zirconia powder for laser sintering, having a molecular weight of 94 or less.
2. The zirconia powder for laser sintering according to claim 1, wherein the content of the oxygen-deficient zirconia relative to the mass of the zirconia powder for laser sintering is 0.5 mass% or more and 10 mass% or less.
3. The zirconia powder for laser sintering according to claim 1 or 2, wherein one or more selected from the group consisting of the oxygen-deficient zirconia and the zirconia different from the oxygen-deficient zirconia is a stabilizing element-containing zirconia.
4. The zirconia powder for laser sintering according to claim 3 , wherein the stabilizing element is one or more selected from the group consisting of calcium, magnesium and yttrium.
5. A method for producing a sintered body, comprising the step of irradiating a molded body containing the zirconia powder for laser sintering according to claim 1 or 2 with laser light to obtain a sintered body.
Citation Information
Patent Citations
Inorganic material powder, and method for producing structure
JP2020100141A
Method for manufacturing sintered body
WO2021172128A1