Method for transporting laminate, method for manufacturing bonded body using the same, and method for manufacturing ceramic circuit board

By tilting the transport container to align metal plates and ceramic substrates, the method addresses displacement issues, enhancing the yield and precision of ceramic circuit boards.

JP2024136337AActive Publication Date: 2024-10-04NITERRA MATERIALS CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023047426
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-04
Estimated Expiration
2043-03-24

AI Technical Summary

Technical Problem

During the transportation of laminates for ceramic circuit boards, metal plates tend to displace, leading to misalignment and reduced positioning accuracy, which affects the quality of the final bonded body.

Method used

A method involving the storage of laminates in a transport container followed by tilting the container to align the metal plates and ceramic substrates, using a U-shaped container with setters to prevent displacement, and mechanized transport to maintain precise positioning.

Benefits of technology

The method effectively suppresses metal plate displacement, ensuring high yield and precise alignment, reducing variations in circuit shapes during the etching process and improving the quality of ceramic circuit boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136337000001_ABST
    Figure 2024136337000001_ABST
Patent Text Reader

Abstract

To provide a method for transporting a laminate that suppresses positional deviation of a metal plate during a transport process.SOLUTION: A method according to an embodiment that transports a laminate in which a brazing material layer and a metal plate are laminated on at least one surface of a ceramic substrate includes the steps of storing the laminate in a transport container, tilting the transport container, and transporting the transport container. In addition, the step of transporting the transport container is preferably performed in a tilted state. In addition, in the step of tilting the transport container, the angle at which the transport container is tilted is preferably within a range of 5° to 30°.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The embodiments described below generally relate to a method for transporting a laminate, a method for manufacturing a bonded body using the same, and a method for manufacturing a ceramic circuit board. [Background technology]

[0002] In recent years, semiconductor elements have become more and more sophisticated. As the performance of semiconductor elements has improved, the amount of heat generated by the semiconductor elements has increased. Ceramic circuit boards are used as circuit boards for mounting semiconductor elements. Ceramic circuit boards with good TCT (thermal cycle test) characteristics have been developed. For example, in Japanese Patent No. 6789955 (Patent Document 1), the size of the protruding portion of the bonding layer is controlled to improve the TCT characteristics. Ceramic circuit boards are made by heating and bonding a laminate in which a brazing material layer and a metal plate are arranged on a ceramic substrate. To obtain a laminate in which a brazing material layer and a metal plate are arranged on a ceramic substrate, it is necessary to arrange them while aligning them. For example, Japanese Patent No. 6314567 (Patent Document 2) discloses a method in which a ceramic substrate is fixed with guide pins, and a brazing material layer and a metal plate are arranged. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 6789955 [Patent Document 2] Patent No. 6314567 Summary of the Invention [Problem to be solved by the invention]

[0004] The method of Patent Document 2 allows for accurate alignment. However, in order to heat-bond the laminate, it is necessary to transport it to a heat-bonding device. During the transport process after the laminate is produced, there is a problem that the metal plate may become misaligned. The embodiment is intended to provide a method for transporting a laminate that suppresses positional deviation of a metal plate during the transport process. [Means for solving the problem]

[0005] The method for transporting a laminate in accordance with the embodiment is a method for transporting a laminate in which a brazing material layer and a metal plate are laminated on at least one surface of a ceramic substrate, and is characterized by including a step of storing the laminate in a transport container, a step of tilting the transport container, and a step of transporting the transport container. [Brief description of the drawings]

[0006] [Figure 1] FIG. 2 is a diagram showing an example of a laminate according to an embodiment. [Diagram 2] FIG. 4 is a diagram showing an example of a transport process of a laminate according to an embodiment. [Diagram 3] FIG. 11 is a diagram showing another example of a transport process of a laminate according to an embodiment. [Figure 4] FIG. 2 is a diagram showing an example of a bonded body according to an embodiment. [Diagram 5] FIG. 1 is a diagram showing an example of a ceramic circuit board according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] The method for transporting a laminate according to the embodiment is a method for transporting a laminate in which a brazing material layer and a metal plate are laminated on at least one surface of a ceramic substrate, storing the laminate in a transport container; tilting the transport container; Transporting the transport container; The present invention is characterized in that it has the following features. An example of the laminate is shown in Figure 1. Also, an example of a method for conveying the laminate is shown in Figures 2 and 3. In the figure, reference numeral 1 denotes a laminate, reference numeral 2 denotes a ceramic substrate, reference numeral 3 denotes a metal plate, reference numeral 4 denotes a brazing material layer, reference numeral 5 denotes a transport container, reference numeral 6 denotes a setter, and reference numeral 7 denotes a transport device. The laminate 1 has a brazing material layer 4 and a metal plate 3 laminated on a ceramic substrate 2. FIG. 1 shows the brazing material layer 4 and the metal plate 3 laminated on both sides of the ceramic substrate 2. The laminate 1 is not limited to this structure. For example, the brazing material layer 4 and the metal plate 3 may be laminated on only one side of the ceramic substrate 2. Alternatively, the laminate 1 may have a multi-layer structure in which the three-layer structure of ceramic substrate 2 / brazing material layer 4 / metal plate 3 is repeated.

[0008] First, the laminate 1 is prepared. Next, a step of storing the laminate in a transport container is performed. The transport container 5 in FIG. 2 is exemplified as one having a U-shaped cross section. The transport container 5 has at least a bottom surface portion on which the laminate 1 is placed and a side surface portion for aligning the laminate 1. The top surface portion of the transport container 5 can be used as a place for fixing with the transport device 7. Fixing with the transport device may be performed using a robot such as suction. The transport device 7 may be fixed using the side surface portion or bottom surface portion of the transport container 5. The side surface portion may be provided on each side of the transport container 5. The laminate 1 may be used as a pre-stacked one, or may be stacked inside the transport container 5. A plurality of laminates 1 may be stored in the transport container 5. The plurality of laminates may be arranged side by side or stacked. FIG. 2 illustrates a stacked arrangement of a plurality of laminates 1. When a plurality of laminates 1 are stored in the storage container 5, it is preferable to arrange a setter 6 between the laminates 1. The setter 6 is not deformed at the temperature of the heat bonding process. Examples of such a setter include a boron nitride plate or a carbon plate. The number of setters 6 is arbitrary. The setter 6 may be arranged between each of the laminates 1. A setter 6 may be arranged for each of the plurality of laminates 1. It is preferable to arrange the setter 6 between each of the laminates 1. By arranging the setter 6 between the laminates 1, it is possible to prevent the metal plates from burning together during the heat bonding process.

[0009] Next, a step of tilting the transport container is performed. By tilting the transport container 5, the stack 1 gathers on the side of the transport container 5. That is, the side of the transport container 5 serves to align the stack 1. In addition, in the step of tilting the transport container, the angle at which the transport container is tilted is preferably within a range of 5° to 30°. The angle θ at which the transport container is tilted is counted as 0° when the stack 1 is placed horizontally. If the angle θ at which the transport container is tilted is less than 5°, the tilt is small, so there is a possibility that the alignment of the stack 1 will vary. If the angle θ exceeds 30°, there is a possibility that no further effect will be obtained. In addition, when aligning the stack 1, there is a possibility that the surface of the metal plate 3 will be rubbed and scratched. For this reason, the angle θ at which the transport container is tilted is preferably within a range of 5° to 30°, and more preferably 7° to 20°. The angle θ is the angle at which the transport container is tilted in one or both of the X-axis direction and the Y-axis direction. For convenience, the X direction is the longitudinal direction of the laminate 1 , and the Y axis direction is the short side direction of the laminate 1 .

[0010] FIG. 4 shows an example of the laminate 1 after alignment. In the figure, reference numeral 2 denotes a ceramic substrate, and reference numeral 3 denotes a metal plate. The figure shows a state in which the metal plate 3 has been aligned by a process of tilting the transport container. FIG. 4(a) shows one side of the ceramic substrate 2 aligned with one side of the metal plate 3. FIG. 4(b) shows two sides of the ceramic substrate 2 aligned with two sides of the metal plate 3. For example, when the angle θ is applied in either the X-axis direction or the Y-axis direction, the result is likely to be as shown in FIG. 4(a). When the angle θ is applied in both the X-axis direction or the Y-axis direction, the result is likely to be as shown in FIG. 4(b). It is preferable that the creepage distance of at least one side of the ceramic substrate and the metal plate is within the range of 0 mm to 0.5 mm by the step of tilting the transfer container. As described above, the creepage distance can be reduced by aligning one or two sides of the ceramic substrate 2 and the metal plate 3. In addition, taking into account the accuracy of alignment, it is preferable that the creepage distance is 0 mm. The creepage distance is calculated by rounding off to one decimal place. It is also preferable that the creepage distance exceeds 0.5 mm for at least one side of the ceramic substrate 2 and the metal plate 3. The creepage distance is 0 mm or more and 0.5 mm or less at the position where one or two sides of the ceramic substrate 2 and the metal plate 3 are aligned. It is preferable that the creepage distance exceeds 0.5 mm for the sides that are not aligned.

[0011] For example, even if the creepage distance is set to 0.5 mm or less beforehand when placing the metal plate 3 on the ceramic substrate 2 and the brazing material layer 4, the metal plate 3 may shift during transportation. For this reason, it is effective to perform alignment by tilting the transportation container. In order to prevent the metal plate 3 from shifting during transportation, it is effective to transport the transportation container 5 while tilted. In addition, the creepage distance can be controlled by tilting the transport container 5. Therefore, even if the position of the metal plate 3 is misaligned when the laminate 1 is produced, the position can be adjusted during the transport process. In other words, even if the positioning accuracy of the metal plate 3 is poor when the laminate 1 is produced, the creepage distance can be controlled during the transport process. Also, by tilting the transport container 5, the creepage distance of the metal plate 3 can be set within the range of 0 mm to 0.5 mm. As the metal plate 3 moves, the brazing material layer 4 also moves. As described below, the active metal brazing material is made into a paste and applied to become the brazing material layer 4. Since the paste is viscous, it moves with the metal plate 3 when it moves. Also, the brazing material layer may be applied widely in advance, assuming the range in which the metal plate will move. In addition, it is preferable that the process of transporting the transport container 5 is mechanized. By mechanizing the process, a robot is used. By automating the process using a robot, it is possible to easily control the angle θ. After the conveying step, a step of heat-bonding the conveyed laminate is performed. A bonded body can be obtained by performing the heat-bonding step. Furthermore, by performing the heat-bonding step, the brazing material layer 4 becomes a bonding layer 10. In the obtained bonded body, at least one side of the ceramic substrate and the metal plate has a creepage distance in the range of 0 mm to 0.5 mm.

[0012] The bonded body according to the embodiment can be used for a ceramic circuit board. FIG. 5 shows an example of a ceramic circuit board. In the figure, reference numeral 2 denotes a ceramic substrate, reference numeral 8 denotes a circuit board, reference numeral 9 denotes a heat sink, reference numeral 10 denotes a bonding layer, and reference numeral 11 denotes a ceramic circuit board. FIG. 5 shows a case where the front metal plate is a circuit board 8 and the rear metal plate is a heat sink 9. The ceramic circuit board according to the embodiment is not limited to such a structure, and both sides may be circuit boards 8. FIG. 5 shows an example where two circuit boards 8 are used, but the number of circuit boards 8 can be increased as necessary. Furthermore, by imparting a circuit shape to the metal plate 3, it becomes a circuit plate 8. The process for imparting the circuit shape is preferably an etching process. The etching process is a method of removing the metal plate using a chemical solution. In the etching process, resist is applied to the areas that are to be left as the circuit shape. The resist application process is mechanized. The position for application is detected according to the circuit shape. The edge of the ceramic substrate 2 or metal plate 3 is used for position detection. The position of the edge of the ceramic substrate 2 or metal plate 3 is detected by a detector. The detector may be a CCD camera or the like. The position can be detected based on a point on at least one side of the ceramic substrate and the metal plate where the creepage distance is in the range of 0 mm to 0.5 mm. The position can also be detected using a point where the creepage distance exceeds 0.5 mm.

[0013] To make the creepage distance 0 mm, it is possible to make the length and width of the ceramic substrate 2 and the metal plate 3 the same. If the length and width are the same, misalignment may occur during transportation. Furthermore, the degree of misalignment is likely to vary from one plate to another, reducing the accuracy of position detection. If the accuracy of position detection decreases, the position of the resist coating will shift. Misalignment of the resist coating position will lead to misalignment of the circuit shape. By tilting the transport container, it is possible to create a location where the creepage distance is in the range of 0 mm to 0.5 mm. This allows the positions of the ceramic substrate 2 and the metal plate 3 to be constant. In addition, by transporting the transport container while tilting it, it is possible to prevent the metal plate from shifting during transport. From this point of view, it is preferable to have a location where the creepage distance is 0 mm. In addition, the presence of a portion where the creepage distance is within the range of 0 mm to 0.5 mm and a portion where the creepage distance exceeds 0.5 mm can improve the position detection accuracy. For example, when a CCD camera is used, position detection is performed by the difference in contrast. The presence of a portion where the creepage distance exceeds 0.5 mm makes it easier to detect the end of the ceramic substrate. In other words, the displacement of the metal plate is prevented at a portion where the creepage distance is less than 0.5 mm, and the position detection accuracy of the end of the ceramic substrate can be improved at a portion where the creepage distance exceeds 0.5 mm. This can prevent the displacement of the applied position of the resist. In other words, it is suitable for a ceramic circuit substrate that is applied with resist and then subjected to an etching process. Moreover, an etching process may be used to give an inclined shape to the side surfaces of the circuit board 8 and the heat sink 9. Furthermore, a bonding layer protruding portion may be provided by protruding the bonding layer from the end portions of the circuit board 8 and the heat sink 9.

[0014] In addition, various types of ceramic substrates can be used as the ceramic substrate 2. Examples of ceramic substrates include silicon nitride substrates, aluminum nitride substrates, alumina substrates, zirconia substrates, and alumina substrates. The alumina substrate is a ceramic sintered body made by mixing alumina and zirconia. In addition, the thickness of the ceramic substrate 2 is preferably within a range of 0.2 mm to 3 mm. The silicon nitride substrate preferably has a three-point bending strength of 600 MPa or more. Also, the thermal conductivity is preferably 80 W / m·K or more. By increasing the strength of the silicon nitride substrate, the substrate thickness can be reduced. For this reason, the silicon nitride substrate preferably has a three-point bending strength of 600 MPa or more, and more preferably 700 MPa or more. The silicon nitride substrate can be reduced in thickness to 2 mm or less, and even 0.40 mm or less. Furthermore, the three-point bending strength of the aluminum nitride substrate is approximately 300 to 450 MPa. On the other hand, the thermal conductivity of the aluminum nitride substrate is 160 W / m·K or more. Since the aluminum nitride substrate has low strength, the substrate thickness is preferably 0.60 mm or more. Aluminum oxide substrates have a three-point bending strength of about 300 to 450 MPa, but are inexpensive, while alumina substrates have a high three-point bending strength of about 550 MPa, but have a thermal conductivity of about 30 to 50 W / m K. A silicon nitride substrate is preferable as the ceramic substrate 2. A silicon nitride substrate has high strength, and therefore will not be damaged by the impact when the transfer container 5 is tilted. Examples of the metal plate 3 include a copper plate (including copper alloys) and an aluminum plate (including aluminum alloys). Examples of the copper plate include an oxygen-free copper plate. As specified in JIS-H-3100, oxygen-free copper has a copper purity of 99.96 wt% or more.

[0015] The brazing material is preferably an active metal brazing material. The active metal brazing material used to bond copper plates contains titanium (Ti). Ti is an active metal. Ti reacts with the ceramic substrate to improve the bonding strength. The Ti used in the active metal brazing material can be titanium or titanium hydride (TiH2). The active metal brazing material preferably contains one or more elements selected from Ag (silver), Cu (copper), Sn (tin), In (indium), and C (carbon). The active metal brazing material preferably contains Ti, one or more elements selected from Cu or Ag, and one or more elements selected from Sn, In, or C. The components of the active metal brazing material include 1% by mass or more and 15% by mass or less of Ti (titanium) or TiH2 (titanium hydride). In addition, the components include 15% by mass or more and 85% by mass or less of Cu (copper), and 0% by mass or more and 70% by mass or less of Ag (silver). In addition, the components include 1% by mass or more and 50% by mass or less of one or two elements selected from Sn (tin) and In (indium). In addition, the components include 0.1% by mass or more and 2% by mass or less of C (carbon). In addition, the active metal brazing material used when joining aluminum plates is preferably an Al-based brazing material containing one or both of silicon (Si) and magnesium (Mg). Si or Mg is the active metal. As a component of the active metal brazing material, the Si content is preferably within the range of 0.01% by mass to 20% by mass. Furthermore, the Mg content is preferably within the range of 0.01% by mass to 20% by mass. The heating and bonding method using an active metal brazing material is called the active metal bonding method. An active metal brazing material is mixed with a binder or a solvent to prepare an active metal brazing material paste. By making it into a paste, the brazing material layer 4 can also move in accordance with the movement of the metal plate 3 when the transport container 5 is tilted. In addition, if the movement range of the metal plate 3 is large, the brazing material paste may be applied widely in advance. An active metal brazing paste is applied to the ceramic substrate 2, and the metal plate 3 is placed thereon. This process produces the laminate 1. In the heat bonding process, the bonding temperature is preferably within a range of 600° C. or more and 980° C. or less. The method for transporting a laminate according to the embodiment can suppress misalignment between the ceramic substrate 2 and the metal plate 3 during transport. This can improve the yield of the bonded body. In addition, it can suppress variations in the circuit shape during the etching process.

[0016] (Example) (Examples 1 to 4, Comparative Example 1) A Ti-containing active brazing material was applied to both sides of a silicon nitride substrate (200 mm long x 160 mm wide x 0.32 mm thick), and a copper plate (195 mm long x 150 mm wide x 0.8 mm thick) was placed on top to create a laminate. A U-shaped cross section was prepared as a transport container. In other words, the transport container has a bottom, side, and top surface. The laminates and the setters were alternately stacked in the transport container. The number of stacks is the number of laminates. For example, in the case of a laminate / setter / laminate / setter stack, the number of stacks is two. The transportation process was carried out as shown in Table 1. The transportation process was mechanized.

[0017] [Table 1]

[0018] As can be seen from the table, in Examples 1 to 4, there were locations where the creepage distance was 0 mm or more and 0.5 mm or less. In Example 1, the plate was tilted only in the X-axis direction, so there was only one side where the creepage distance was 0 mm or more and 0.5 mm or less. In Examples 2 to 4, the plate was tilted in both the X-axis and Y-axis directions, so there were two sides where the creepage distance was 0 mm or more and 0.5 mm or less. In Comparative Example 1, the plate was not transported while tilted, so there were no locations where the creepage distance was 0 mm or more and 0.5 mm or less. In Comparative Example 1, there was also variation in the creepage distance. This is because the metal plate was misaligned during transportation.

[0019] Next, the laminate was formed by heat bonding, and then a resist coating step and an etching step were performed to produce a ceramic circuit board. In the resist application process, the position was detected using a CCD camera and the resist was applied. The position detection using the CCD camera was performed based on the point where the creepage distance exceeded 0.5 mm. Products that were within 0 mm or more and 0.3 mm or less of the intended resist application position were deemed to be good products. Products in which even one location was observed where the resist was misaligned by 0.4 mm or more were deemed to be defective products. Products with a good product rate of 99% or more and 100% or less were rated as ◎, products with a good product rate of 95% or more and less than 99% were rated as ◯, and products with a good product rate of less than 95% were rated as ×. The results are shown in Table 2.

[0020] [Table 2]

[0021] In the working example, the deviation of the resist coating position was reduced. Therefore, the deviation of the circuit shape after the etching process was also suppressed. In contrast, in the comparative example 1, the deviation of the resist coating position was large, and the circuit shape after etching was uneven. The method for manufacturing a ceramic circuit board according to the embodiment can produce a circuit board with reduced variation in shape with a high yield.

[0022] Although some embodiments of the present invention have been illustrated above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, modifications, etc. can be made without departing from the gist of the invention. Modifications of these embodiments are included in the scope and gist of the invention, and are included in the scope of the invention and its equivalents described in the claims. In addition, the above-mentioned embodiments can be implemented in combination with each other. [Explanation of symbols]

[0023] 1...Laminate 2...Ceramic substrate 3...Metal plate 4…Brazing layer 5...Transportation container 6. Setter 7...Transportation device 8...Circuit board 9...Heat sink 10...Joining layer 11...Ceramic circuit board

Claims

1. A method for conveying a laminate in which a brazing material layer and a metal plate are laminated on at least one surface of a ceramic substrate, comprising the steps of: storing the laminate in a transport container; tilting the transport container; Transporting the transport container; A method for transporting a laminate, comprising:

2. 2. The method for transporting a laminate according to claim 1, wherein the step of transporting the transport container is performed in a tilted state.

3. 3. The method for transporting a laminate according to claim 1, wherein the step of storing the laminate in a transport container stores a plurality of laminates in the transport container via a setter.

4. 3. The method for transporting a laminate according to claim 1, wherein in the step of tilting the transport container, the angle at which the transport container is tilted is within a range of 5 degrees to 30 degrees.

5. 3. The method for transporting a laminate according to claim 1, wherein the step of tilting the transport container causes a creepage distance of at least one side of the ceramic substrate and the metal plate to fall within a range of 0 mm to 0.5 mm.

6. 5. The method for transporting a laminate according to claim 4, wherein the creepage distance of at least one side of the ceramic substrate and the metal plate is within a range of 0 mm to 0.5 mm by the step of tilting the transport container.

7. 3. The method for transporting a laminate according to claim 1, wherein the step of tilting the transport container causes a creepage distance of 0 mm for at least one side of the ceramic substrate and the metal plate.

8. 5. The method for transporting a laminate according to claim 4, wherein the step of tilting the transport container causes a creepage distance of 0 mm on at least one side of the ceramic substrate and the metal plate.

9. 3. The method for transporting a laminate according to claim 1, wherein the ceramic substrate is a silicon nitride substrate, the metal plate is a copper plate, and the brazing material layer is an active metal brazing material.

10. 7. The method for transporting a laminate according to claim 6, wherein the ceramic substrate is a silicon nitride substrate, the metal plate is a copper plate, and the brazing material layer is an active metal brazing material.

11. 3. A method for producing a bonded body, comprising a step of heat-bonding a laminate transported by the laminate transport method according to claim 1 or 2.

12. A method for producing a bonded body, comprising a step of heat-bonding a laminate transported by the laminate transport method according to claim 10.

13. 12. A method for producing a ceramic circuit board, comprising the steps of: applying a resist to the metal plate of the bonded body obtained by the method for producing a bonded body according to claim 11; and etching the metal plate.

14. 13. A method for producing a ceramic circuit board, comprising the steps of: applying a resist to the metal plate of the bonded body obtained by the method for producing a bonded body according to claim 12; and etching the metal plate.

Citation Information

Patent Citations

  • Ceramic bonded body and manufacture

    JP1985077178A

  • Apparatus for producing laminate for honeycomb core

    JP1999207841A

  • Moving device and moving method for article

    JP2000038218A

  • Manufacturing method of ceramic substrate and use of ceramic substrate

    JP2006068988A

  • Manufacturing method and manufacturing apparatus of power module

    JP2014022535A