Coating material for wood having fireproof performance holding effect
A solvent-based coating composition with methylphenyl-based silicone alkoxy oligomer and scaly silica powder addresses the issue of crystallization and efflorescence in flame-retardant treated wood, providing durable and weather-resistant organic-inorganic composite films.
Patent Information
- Application Number
- JP2023047699
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-03-24
AI Technical Summary
Existing organic-inorganic composite paints and inorganic paints react with flame-retardant treated wood, causing crystallization and efflorescence, and their long-term weather resistance is uncertain.
A solvent-based coating composition comprising a methylphenyl-based silicone alkoxy oligomer, a hydrolyzable silicone compound with an epoxy group, and scaly silica powder reacted with an isocyanate compound, forming a flexible and durable organic-inorganic composite coating film.
Prevents leaching of flame-retardant chemicals, reduces efflorescence, and maintains excellent weather resistance and durability on flame-retardant treated wood.
Smart Images

Figure 2024136549000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a wood coating material which is less likely to cause efflorescence even on fire-retardant treated wood, and which is capable of forming an organic-inorganic composite coating film which has excellent durability in outdoor environments while retaining fire retardant performance. [Background technology]
[0002] The active use of wood in buildings has been promoted, for example, by enacting the Law for Promoting Wood Use in Public Buildings and Buildings Contributing to the Realization of a Carbon-Free Society. When wood is used as exterior wood, the surface of the wood is generally coated with paint to improve its durability. For such exterior wood, some kind of fire prevention measure is required for parts that are at risk of fire spreading, and flame retardant treatment is required. The chemicals used in the flame retardant treatment of wood are often water-soluble. Therefore, when flame retardant-treated wood is used outdoors, the chemicals are leached out early by wind and rain, which causes a problem of shortening the duration of the flame retardant effect. In addition, the leached chemicals precipitate on the surface of the wood, causing a poor appearance called efflorescence.
[0003] As a method for preventing the leaching of the chemicals used in such flame retardant treatment, coating the surface of the wood with a paint is considered. Coatings for wood can be broadly divided into "impregnation type" that soaks into the wood, "semi-film type (thin film)" that soaks into the wood while forming a film on the surface, and "film type (thick film)" that forms a thick film on the surface. However, the "film type" is not very popular because it makes the wood grain invisible and loses the wood texture. Furthermore, exterior wood paints are required to deal with aging such as discoloration and cracking due to exposure to ultraviolet rays, wind and rain, etc., and also to be able to follow dimensional changes, since wood expands and contracts as it absorbs and releases moisture depending on the surrounding humidity, causing changes in dimensions.
[0004] In the case of organic paints such as acrylic resins and urethane resins, which are impregnating paints, it is easy to control flexibility and there is little risk of cracking, but they have the disadvantage of poor weather resistance. In the case of semi-film-forming or thick-film wood protection paints, silicone paints, fluororesin paints, or inorganic paints whose main components are inorganic substances such as ceramics and silicon are desirable from the standpoint of weather resistance, but these paints are usually too hard to follow the movement of the wood and have the disadvantage of being prone to cracking.
[0005] In order to solve the problem of poor weather resistance of such organic wood paints, many semi-film-forming or film-forming organic / inorganic composite paints or inorganic paints have been developed. For example, Patent Document 1 (JP 2021-102673 A) discloses an invention of an aqueous exterior wood paint that uses a scaly silica powder and a smectite powder reacted with polycarbodiimide as inorganic particles in an organic / inorganic composite paint containing an aqueous paint composition mainly composed of a reactive aqueous polysiloxane-acrylic composite resin and a curing agent for the aqueous paint composition mainly composed of a hydrolyzable silicone compound.
[0006] Furthermore, Patent Document 2 (JP 2006-159554 A) discloses an invention relating to a coating composition comprising a silicone emulsion composition in which components consisting of an organopolysiloxane containing at least two hydroxyl groups bonded to silicon atoms in one molecule, a reaction product of an amino group-containing organoalkoxysilane and an acid anhydride, an epoxy group-containing organoalkoxysilane and / or a partial hydrolyzate thereof, colloidal silica and / or polysilsesquioxane, and a curing catalyst are emulsified and dispersed in water in the presence of a surfactant.
[0007] Furthermore, Patent Document 3 (JP 2017-052853 A) discloses an invention for a two-component wood paint that contains a base agent containing a polyester polyol and a curing agent containing a polyisocyanate, and further contains a first additive containing a surfactant having two or more isocyanate groups, and a second additive containing an inorganic compound having a silanol group at its terminal. It also discloses the use of a flake-shaped silicon compound such as muscovite as the second additive (see
[0033] ).
[0008] Furthermore, Patent Document 4 (Japanese Patent No. 6,985,638) discloses an invention for a wood paint that comprises a paint composition whose main component is a methylphenyl-based silicone alkoxy oligomer that is a composite of a tertiary amino group-containing acrylic resin and nanosilica, and a curing agent that contains a hydrolyzable silicone compound with an epoxy group, and that has a high effect of preventing the leaching of wood preservatives such as preservatives even with a single coating film, and that can form an organic-inorganic composite coating film that is excellent in weather resistance and durability. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2021-102673 A [Patent Document 2] JP 2006-159554 A [Patent Document 3] JP 2017-052853 A [Patent Document 4] Patent No. 6985638 Summary of the Invention [Problem to be solved by the invention]
[0010] The organic-inorganic composite paints or inorganic paints disclosed in the above Patent Documents 1 to 4 have excellent properties as exterior wood paints, not only in terms of elasticity but also in terms of weather resistance and durability. On the other hand, when applied to wood that has been treated for flame retardancy, many water-based paints react with the flame retardant chemicals to cause crystallization, etc., and there is a problem that the paint cannot be applied normally. The organic-inorganic composite paints or inorganic paints disclosed in Patent Documents 1 and 2 are also water-based paints, so when applied to wood that has been treated for flame retardancy, they crystallize, making it impossible to apply the paint normally.
[0011] In addition, the two-component wood paint disclosed in Patent Document 3 is solvent-based and can be applied normally to wood that has been treated to be flame retardant, and furthermore, it has been shown that no efflorescence occurred after a 7-day weathering test (see paragraph
[0049] ), but its long-term weather resistance is unclear. Incidentally, the wood paint disclosed in Patent Document 4 is able to provide a good effect of preventing the leaching of wood preservatives on wood that has been treated with preservatives, but its effect of preventing the leaching of flame retardant treatment chemicals on flame retardant-treated wood is not necessarily excellent, and further improvements are required.
[0012] The present invention has been made to solve the problems of the prior art as described above, and has an object to provide a wood protective coating which is highly effective in preventing the leaching of flame retardant treatment agents contained in wood, is less likely to cause efflorescence, and is capable of forming an organic-inorganic composite coating film which has excellent weather resistance and durability. [Means for solving the problem]
[0013] The wood protective coating material of the present invention, which has a flame retardant treatment agent sealing effect, is characterized by being a mixture of a coating composition mainly composed of a solvent-based acrylic resin and a methylphenyl-based silicone alkoxy oligomer, and a scaly silica powder obtained by reacting an isocyanate compound with a curing agent containing a hydrolyzable silicone compound having an epoxy group.
[0014] According to the wood protective paint of the present invention, when a coating film is formed on fire-retardant treated wood, it is not gelled by the fire-retardant treatment chemicals, and a film is formed on the surface of the wood, so that it is possible to prevent the fire-retardant treatment chemicals from leaching out from the fire-retardant treated wood and to prevent efflorescence that appears as a white product on the surface of the wood. In addition, the coating film has a high flexibility and can well follow the expansion and contraction of the wood, so a coating film with good weather resistance and durability is obtained.
[0015] The wood protective coating material of the present invention having the effect of sealing flame retardant treatment agents can be a "three-component" coating material in which the "coating composition", the "hardening agent", and the "scaly silica powder reacted with an isocyanate compound" are mixed together at the time of use to form the wood protective coating material, or it can be a "two-component" coating material in which the hardening agent and the scaly silica powder reacted with an isocyanate compound are mixed in advance, and at the time of use, the "coating composition" and the "mixture of the hardening agent and the scaly silica powder reacted with an isocyanate compound" are mixed together to form the wood protective coating material.
[0016] In general, the curing mechanism between acrylic resin and hydrolyzable silicone compound containing epoxy groups is thought to be the formation of a cured coating film made of a polysiloxane-acrylic composite resin, as shown in the following reaction formula (1). TIFF2024136549000002.tif32140
[0017] As shown in the chemical formula below, silicone alkoxy oligomers are relatively low molecular weight silicone resins whose molecular terminals are alkoxysilyl groups (≡Si-OR), and which simultaneously contain an organic substituent (R) and a hydrolyzable alkoxy group (-OR) within the molecule. TIFF2024136549000003.tif13153
[0018] As shown in the following reaction formula (2), this silicone alkoxy oligomer can be moisture-cured at room temperature due to the alkoxysilyl group. TIFF2024136549000004.tif16140
[0019] The methylphenyl-based silicone alkoxy oligomer in the wood protective coating material of the present invention has both methyl and phenyl groups and has good compatibility with organic resins such as solvent-based acrylic resins. Moreover, the copolymer obtained by crosslinking reaction with solvent-based acrylic resins becomes a coating resin with excellent weather resistance, heat resistance and chemical resistance.
[0020] In the wood protective coating of the present invention, the solvent-based acrylic resin acts as a soft segment, and the methylphenyl-based silicone alkoxy oligomer acts as a hard segment, forming a thermoplastic resin component. Note that thermoplastic resins are basically composed of two segments: a hard segment and a soft segment, the soft segment being a rubber component that provides elasticity and plays a role in providing flexibility, and the hard segment flows at high temperatures but plays a role in providing a restraining property that prevents deformation at room temperature.
[0021] In addition, the methyl-based silicone alkoxy oligomers having methyl groups as organic substituents form cured coating films with high hardness and excellent scratch resistance, but tend to be easily cracked when bent or impacted, and have poor deformation followability. In contrast, the methylphenyl-based silicone alkoxy oligomers containing phenyl groups have the characteristic that the hardness can be adjusted and that they have good compatibility with organic resins such as solvent-based acrylic resins. Therefore, for preparing the wood protective coating of the present invention, methylphenyl-based silicone alkoxy oligomers containing phenyl groups are used. In addition, the alkoxy group in the methylphenyl-based silicone alkoxy oligomers is a methoxy group, and those with an alkoxy content in the range of 10 to 50% are commercially available. Among these, methylphenyl-based silicone alkoxy oligomers with an alkoxy content of 30 to 35% have particularly good mixing stability with solvent-based acrylic resins, and are excellent in water resistance and weather resistance.
[0022] The content of the methylphenyl-based silicone alkoxy oligomer in the wood protective coating of the present invention is preferably 10 to 60 parts by mass per 100 parts by mass of the solvent-based acrylic resin. If the content of the methylphenyl-based silicone alkoxy oligomer is less than 10 parts by mass per 100 parts by mass of the solvent-based acrylic resin, the effect of improving water resistance and weather resistance will be small, and if it exceeds 60 parts by mass, the crack prevention effect will decrease.
[0023] In addition, many kinds of acrylic resins are commercially available, both water-based and solvent-based, and the solvent-based acrylic resin in the wood protective coating of the present invention can be appropriately selected from commercially available ones.In addition, as the methylphenyl silicone alkoxy oligomer, commercially available KR-401N, KR-510, KR-213, KR-9218, etc. of Shin-Etsu Chemical Co., Ltd., and TSR165, XR31-B2230, XR31-B6667, etc. (all trade names) of Momentive Performance Materials Japan, LLC can be used.
[0024] In addition, in the wood protective coating material of the present invention, the amount of hydrolyzable silicone compound having an epoxy group added as a curing agent is preferably 0.5 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the coating composition mainly composed of a solvent-based acrylic resin and a methylphenyl-based silicone alkoxy oligomer.
[0025] The scaly silica powder reacted with an isocyanate compound can be prepared, for example, by adding an appropriate amount of polyisocyanate compound and scaly silica powder to methyl ethyl ketone, stirring and mixing, leaving to stand for several minutes to several tens of minutes, filtering and drying. The critical limits of the amounts of the isocyanate compound and scaly silica powder added are not clear, but it is preferable to set the mass ratio to 1:0.1-0.5. If the amount of the isocyanate compound added is less than 0.1 times the amount of the scaly silica powder added, the effect of reacting the isocyanate compound is not well manifested, and if it is more than 0.5 times, the unreacted isocyanate compound is wasted, which is uneconomical.
[0026] This isocyanate compound reacts with the functional groups (hydroxyl groups) contained in the polysiloxane-acrylic composite resin to form urethane bonds, so that the scaly silica powder that has been reacted with the isocyanate compound is firmly bonded to the polysiloxane-acrylic composite resin to form a composite, allowing it to exist stably in the coating film.
[0027] The isocyanate compound to be reacted with the scaly silica powder is not particularly limited, and any isocyanate compound known as a curing agent for two-liquid reactive paints can be used. Examples of the isocyanate compound include aromatic diisocyanates such as tolylene diisocyanate (TDI), 4,4'-diphenylmethane diisocyanate (MDI), xylylene diisocyanate (XDI), and meta-xylylene diisocyanate (MXDI); aliphatic diisocyanates such as hexamethylene diisocyanate (HDI), tetramethylene diisocyanate, 2-methyl-pentane-1,5-diisocyanate, 3-methyl-pentane-1,5-diisocyanate, lysine diisocyanate, and trioxyethylene diisocyanate; and alicyclic diisocyanates such as isophorone diisocyanate (IPDI), cyclohexyl diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, norbornane diisocyanate, hydrogenated tolylene diisocyanate, hydrogenated xylylene diisocyanate, and hydrogenated tetramethylxylylene diisocyanate. These may be used alone or in combination of two or more. Among these, aliphatic diisocyanates are preferred, and HDI is more preferred, in that they have a relatively low viscosity.
[0028] In addition, scaly silica has excellent water resistance and heat resistance, and has self-filming properties, but has low swelling properties. Therefore, when only scaly silica powder is contained in the coating film, a strong coating film with low elasticity is obtained, but it is not suitable as a coating material for exterior wood because it has poor followability to the expansion and contraction of wood. However, when scaly silica powder reacted with an isocyanate compound is contained, a coating film with good elasticity and good followability to the expansion and contraction of wood is obtained. In addition, since the scaly silica powder is an inorganic material, it is possible to obtain good durability. The particle size of the scaly silica powder may be appropriately selected from those commercially available for coating, and for example, commercially available Sun Lovely (registered trademark, AGCSI Tech Co., Ltd.) can be used.
[0029] In addition, the function of the scaly silica powder reacted with an isocyanate compound in the wood protective coating of the present invention is presumably not to form a coating film, but to act as a reinforcing material that penetrates into the voids inside the wood and strengthens the anchor function between the wood and the coating film.
[0030] Therefore, according to the wood protective coating of the present invention, the scaly silica powder reacted with an isocyanate compound is firmly compounded in the coating film, so that an organic-inorganic composite coating film with good durability is obtained, which can well follow the dimensional changes caused by the expansion and contraction of the wood even if the coating film expands and contracts. Moreover, since the scaly silica powder is an inorganic material, good durability can be obtained.
[0031] In addition, the amount of the scaly silica powder used in the wood protective coating of the present invention is preferably 0.5 parts by mass or more and 5 parts by mass or less per 100 parts by mass of the coating composition mainly composed of a solvent-based acrylic resin and a methylphenyl-based alkoxy silicone oligomer. If the content of the scaly silica powder is less than 0.5 parts by mass per 100 parts by mass of the coating composition, a good crack prevention and reinforcement effect for wood cannot be obtained, and if it exceeds 5 parts by mass, the appearance of the coating film is impaired. More preferably, the content of the scaly silica powder in the coating composition mainly composed of a solvent-based acrylic resin and a methylphenyl-based alkoxy silicone oligomer is 0.5 parts by mass or more and 4 parts by mass or less per 100 parts by mass of the coating composition. The average particle size of the scaly silica powder used in the wood protective coating of the present invention is preferably 0.5 μm or more and 3.0 μm or less, although the critical limit is not necessarily clear.
[0032] Furthermore, in the wood protective coating of the present invention, ultraviolet absorbers, light stabilizers, preservatives, pigments, etc. commonly used in exterior wood coatings may be appropriately added. As the ultraviolet absorber, at least one of organic ultraviolet absorbers and inorganic ultraviolet absorbers can be used. As the organic ultraviolet absorber, triazine ultraviolet absorber Tinuvin 400 (trade name, manufactured by BASF), benzotriazole ultraviolet absorbers Adeka STAB LA31, Adeka STAB LA32, Adeka STAB LA36 (all trade names, manufactured by ADEKA Corporation), HOSTAVIN 3315 DISP, HOSTAVIN 3326 DISP (all trade names, manufactured by Clariant Chemicals Co., Ltd.), etc. can be used. Furthermore, as the inorganic ultraviolet absorber, titanium oxide, zinc oxide, cerium oxide, etc. can be used. In the wood protective coating of the present invention having a fire retardant performance retention effect, it is preferable to use an organic ultraviolet absorber and an inorganic ultraviolet absorber in combination.
[0033] In addition, hindered amine light stabilizers (HALS) are commonly used as light stabilizers, and are additives that suppress photodegradation of polymers, and are particularly excellent in preventing surface degradation. Examples of light stabilizers that can be used include BASF's Tinuvin (trade name), Adeka STAB LA72, Adeka STAB LA82 (all trade names, manufactured by ADEKA CORPORATION), HOSTAVIN3051-2DISP, and HOSTAVIN3070DISP (all trade names, manufactured by Clariant Chemicals Co., Ltd.).
[0034] The preservative may be appropriately selected from among those well known as wood preservatives, and examples of the preservative that may be used include quaternary ammonium compounds, copper-quaternary ammonium compounds, and copper-azole compounds.
[0035] In addition, the wood protective coating of the present invention contains silanol groups in the coating film structure, and the coating film surface is hydrophilized due to the silanol groups. In the case of a general building exterior coating, the presence of the silanol groups allows the self-cleaning function by rainwater to be expressed, forming a coating film with excellent stain resistance, but when used as a wood protective coating, moisture is easily penetrated into the inside of the wood, which leads to the proliferation of decay fungi and promotes wood deterioration. Therefore, in the wood protective coating of the present invention, a water-repellent additive may be added to the coating composition mainly composed of a solvent-based acrylic resin and a methylphenyl-based silicone alkoxy oligomer. This provides water repellency to the surface of the coating film, and even when used for wood, moisture is less likely to penetrate into the inside of the wood, thereby suppressing wood deterioration.
[0036] Examples of the water-repellent additive that can be used include Modivar F3636 (trade name, manufactured by NOF Corporation), a fluorine / acrylic copolymer, Modivar FS720 (manufactured by NOF Corporation), a silicon / acrylic copolymer, and Megafac F-552 (trade name, manufactured by DIC Corporation), a fluororesin. In addition, general silicone oil can also be used. Effect of the Invention
[0037] As described above, according to the wood protective coating material of the present invention, a scaly silica powder obtained by reacting an isocyanate compound is added to a coating composition whose main components are a solvent-based acrylic resin and a methylphenyl-based silicone alkoxy oligomer, and therefore a coating composition is obtained which, even when used on fire-retardant treated wood, can form an organic-inorganic composite coating film which has good durability, such as weather resistance, stain resistance and water resistance, and which has the effect of sealing in the fire-retardant treatment agent. [Brief description of the drawings]
[0038] [Figure 1] 1 shows surface photographs of test specimens immediately after application of each of Experimental Example 1, Comparative Example 1, and Comparative Example 2. [Diagram 2] 1 shows surface photographs of test pieces of Experimental Examples 1 to 7 and Comparative Example 2 after repeated wet and dry tests. [Diagram 3] 1 shows surface photographs of test pieces of Experimental Examples 1 to 7 and Comparative Example 2 after a weather resistance test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0039] The wood protective coating having the effect of sealing flame retardant treatment agents according to the present invention will be described in detail below using various experimental examples and comparative examples. However, the various experimental examples shown below are examples for embodying the technical idea of the present invention, and are not intended to limit the present invention to those shown in these experimental examples. The present invention can be equally applied to other embodiments included in the scope of the claims.
[0040] [Scaly silica powder reacted with isocyanate compound] First, the preparation process of scaly silica powder reacted with isocyanate compound required for wood protective coating material having flame retardant treatment agent sealing effect of the present invention will be described. First, commercially available scaly silica powder (Sun Lovely (registered trademark, AGCSI Tech Co., Ltd.) was dispersed in methyl ethyl ketone, and polyisocyanate compound was added in a mass ratio of 1 / 10 of the scaly silica powder, stirred well for 5 minutes, filtered and dried to obtain scaly silica powder reacted with isocyanate compound used in various experimental examples.
[0041] [About the flame-retardant wood test specimen] A wide variety of water-soluble flame retardants are commercially available, and are not particularly limited, and may be, for example, inorganic phosphorus-based flame retardants or boron-based flame retardants. As a test specimen for confirming the flame-retardant treatment agent sealing effect of the wood protective coating of the present invention, any wood may be impregnated with a commercially available water-soluble flame retardant, but in the following, various tests were performed using commercially available flame-retardant treated wood as is.
[0042] [Experimental Example 1] The paint composition mainly composed of a solvent-based acrylic resin and a methylphenyl-based silicone alkoxy oligomer in the wood protective paint of Experimental Example 1 was prepared from a solvent-based acrylic resin (ACRYDIC A-814 (trade name), DIC Corporation) and a methylphenyl-based silicone oligomer (KR-401N (trade name), Shin-Etsu Chemical Co., Ltd.). The curing agent used was a hydrolyzable silicone compound (OFS6040 (trade name), Dow Toray) dissolved in a high-boiling aromatic solvent.
[0043] Furthermore, various additives were used, including scaly silica powder reacted with the isocyanate compound prepared as described above, water-repellent additives (Modivar F3636, Modivar F720, etc. (trade names, manufactured by NOF Corporation)), inorganic UV absorbers (titanium oxide), organic UV absorbers (Tinuvin 400 (trade name, manufactured by BASF)), light stabilizers (Tinuvin (trade name), manufactured by BASF), preservatives (didecyldimethylammonium chloride), mineral spirits, xylene, and naphthalene solvents, and furthermore, red ocher and iron oxide yellow were used as pigments to make the paint a pinny color.
[0044] The wood protective coating material in Experimental Example 1 was prepared by mixing all the components except for the curing agent containing a hydrolyzable silicone compound and the scaly silica powder reacted with an isocyanate compound in the coating composition mainly composed of the above-mentioned solvent-based acrylic resin and methylphenyl-based silicone alkoxy oligomer as liquid A, and mixing the curing agent containing a hydrolyzable silicone compound and the scaly silica powder reacted with an isocyanate compound as liquid B, and mixing them in a ratio of liquid A: liquid B = 1: 1 (mass ratio) immediately before use. The wood protective coating material in Experimental Example 1 is a "film-forming (semi-film-forming) type", the content of the methylphenyl-based silicone alkoxy oligomer relative to 100 parts by mass of the solvent-based acrylic resin is 10 parts by mass, and the amount of the curing agent added relative to 100 parts by mass of the coating composition (solvent-based acrylic resin + methylphenyl-based silicone alkoxy oligomer) corresponds to 5 parts by mass. The entire composition of the wood protective coating material in Experimental Example 1 is summarized in Table 1 below along with the compositions of the coating materials in Comparative Examples 1 and 2 for each component.
[0045] [Comparative Examples 1 and 2] As the wood protective coating of Comparative Example 1, a commercially available water-based highly durable wood protective coating T-WOOD COAT (trade name, Taisei Corporation) in light brown color was used as is, and as the wood protective coating of Comparative Example 2, a commercially available oil-based wood protective coating in light brown color was used as is. The wood protective coating of Comparative Example 1 was a "film-forming (semi-film-forming) type", and the wood protective coating of Comparative Example 2 was an "impregnation type". The entire composition of the wood protective coatings of Comparative Examples 1 and 2 is summarized in Table 1 for each component with that of Experimental Example 1. The content ratio of the methylphenyl-based silicone alkoxy oligomer in the wood protective coating of Experimental Example 1 to the solvent-based acrylic resin corresponds to 25.0%. Furthermore, the content of the hydrolyzable silicone compound having an epoxy group, which is a curing agent, to 100 parts by mass of a resin composition mainly composed of a solvent-based acrylic resin and a methylphenyl-based silicone alkoxy oligomer corresponds to 2.0 parts by mass.
[0046] [Table 1]
[0047] [Painting test (Experimental Example 1, Comparative Examples 1 and 2)] Using each of the wood protective paints of Experimental Example 1, Comparative Examples 1 and 2, commercially available flame-retardant treated cedar wood (knot-free) measuring 70 x 150 x 10 mm was prepared, and immediately applied to a predetermined thickness by spraying or brushing under predetermined conditions, and the surface condition of the test specimen immediately after painting was observed. The obtained surface conditions of the test specimens of Experimental Example 1, Comparative Example 1 and Comparative Example 2 are shown in Figure 1. Note that Figure 1 is a surface photograph of each of the test specimens of Experimental Example 1, Comparative Example 1 and Comparative Example 2 immediately after painting.
[0048] From the results shown in Figure 1, no abnormality was observed in the coating film of the specimens of Experimental Example 1 and Comparative Example 2, but crystallization was observed in the coating film of the specimen of Comparative Example 1, and it was found that a normal coating film could not be obtained. This indicates that the wood protective coatings of Experimental Example 1 and Comparative Example 2 are both solvent-based (oil-based), while the wood protective coating of Comparative Example 1 is water-based, and therefore reacts with the water-soluble flame retardant treatment agent contained in the wood. Therefore, the following wet-dry cycle test and weather resistance test were conducted without the wood protective coating of Comparative Example 1.
[0049] [Experimental Example 2] The wood protective coating of Experimental Example 2 has the same composition as the wood protective coating of Experimental Example 1, except that simple flaky silica is used instead of the flaky silica powder reacted with an isocyanate compound used in the wood protective coating of Experimental Example 1, and the amount of high-boiling aromatic solvent is increased accordingly.
[0050] The content ratio of the methylphenyl-based silicone alkoxy oligomer in the wood protective coating of Experimental Example 2 relative to 100 parts by mass of the solvent-based acrylic resin, and the content ratio of the hydrolyzable silicone compound having an epoxy group as a curing agent relative to 100 parts by mass of a coating composition mainly composed of the solvent-based acrylic resin and the methylphenyl-based silicone alkoxy oligomer correspond to 25.0 parts by mass and 2.0 parts by mass, respectively, the same as in Experimental Example 1. Note that the wood protective coating of Experimental Example 2 does not contain scaly silica powder reacted with an isocyanate compound.
[0051] [Experimental Example 3] The wood protective coating of Experimental Example 3 has the same composition as that of Experimental Example 1, except that the scaly silica powder used in the wood protective coating of Experimental Example 1 is excluded (but polyisocyanate is included) and the content of mineral spirits is increased accordingly. The content ratio of the methylphenyl silicone alkoxy oligomer in the wood protective coating of Experimental Example 3 to 100 parts by mass of the solvent-based acrylic resin, and the content ratio of the hydrolyzable silicone compound having an epoxy group as a hardener to 100 parts by mass of the coating composition mainly composed of the solvent-based acrylic resin and the methylphenyl silicone alkoxy oligomer also correspond to 25.0 parts by mass and 2.0 parts by mass, respectively, which are the same as those in Experimental Example 1. Note that the wood protective coating of Experimental Example 3 does not contain the scaly silica powder reacted with the isocyanate compound.
[0052] [Experimental Example 4] The wood protective coating of Experimental Example 4 has the same composition as the wood protective coating of Experimental Example 1, except that the content of the methylphenyl-based silicone alkoxy oligomer used in the wood protective coating of Experimental Example 1 is reduced to 2.0 mass%, the content of the scaly silica component in the scaly silica powder reacted with an isocyanate compound is reduced from 5.0 parts by mass to 0.1 parts by mass, the content of the polyisocyanate component is reduced from 3.5 parts by mass to 0.01 parts by mass, the content of the hydrolyzable silicone compound having an epoxy group, which serves as a curing agent, is also reduced from 0.5 parts by mass to 0.1 parts by mass, and the contents of the mineral spirits and high-boiling aromatic solvents are correspondingly increased.
[0053] The content ratio of the methylphenyl silicone alkoxy oligomer in the wood protective coating of Experimental Example 4 to 100 parts by mass of the solvent-based acrylic resin corresponds to 10.0 parts by mass. The content ratio of the hydrolyzable silicone compound having an epoxy group as the hardener to 100 parts by mass of the solvent-based acrylic resin and the methylphenyl silicone alkoxy oligomer corresponds to 0.45 parts by mass. The content of the hydrolyzable silicone compound having an epoxy group as the hardener to 100 parts by mass of the resin composition mainly composed of the solvent-based acrylic resin and the methylphenyl silicone alkoxy oligomer corresponds to 0.5 parts by mass.
[0054] [Experimental Example 5] The wood protective coating of Experimental Example 5 has the same composition as the wood protective coating of Experimental Example 1, except that the content of the methylphenyl-based silicone alkoxy oligomer used in the wood protective coating of Experimental Example 1 is increased to 12.0 mass%, the content of the scaly silica component in the scaly silica powder reacted with an isocyanate compound is increased from 5.0 parts by mass to 6.4 parts by mass, the content of the polyisocyanate component is increased from 3.5 parts by mass to 6.4 parts by mass, the content of the hydrolyzable silicone compound having an epoxy group, which serves as a curing agent, is also increased from 0.5 parts by mass to 6.4 parts by mass, and the contents of the mineral spirits and high-boiling aromatic solvents are correspondingly reduced.
[0055] The content ratio of the methylphenyl silicone alkoxy oligomer in the wood protective coating material of Experimental Example 5 to 100 parts by mass of the solvent-based acrylic resin corresponds to 60 parts by mass. The content ratio of the hydrolyzable silicone compound having an epoxy group, which is the curing agent, to 100 parts by mass of the solvent-based acrylic resin and the methylphenyl silicone alkoxy oligomer corresponds to 20 parts by mass. Furthermore, the content ratio of the scaly silica powder reacted with an isocyanate compound to 100 parts by mass of the solvent-based acrylic resin and the methylphenyl silicone alkoxy oligomer corresponds to 40 parts by mass.
[0056] [Experimental Example 6] The wood protective coating of Experimental Example 6 has the same composition as the wood protective coating of Experimental Example 1, except that the content of the flaky silica powder reacted with an isocyanate compound in the wood protective coating of Experimental Example 1 is increased from 4.0 parts by mass to 15.0 parts by mass, and the contents of the mineral spirits and high-boiling aromatic solvents are increased accordingly.
[0057] The content ratio of the methylphenyl-based silicone alkoxy oligomer in the wood protective coating material of Experimental Example 6 relative to 100 parts by mass of the solvent-based acrylic resin, and the content ratio of the hydrolyzable silicone compound having an epoxy group as a curing agent relative to 100 parts by mass of a coating composition mainly composed of the solvent-based acrylic resin and the methylphenyl-based silicone alkoxy oligomer also correspond to 25.0 parts by mass and 2.0 parts by mass, respectively, the same as in Experimental Example 1. The content ratio of the scaly silica powder reacted with an isocyanate compound relative to 100 parts by mass of the solvent-based acrylic resin and the methylphenyl-based silicone alkoxy oligomer corresponds to 74 parts by mass.
[0058] [Experimental Example 7] The wood protective coating of Experimental Example 7 has the same composition as the wood protective coating of Experimental Example 1, except that the amount of isocyanate compound in the wood protective coating of Experimental Example 1 was increased from 3.5 parts by mass to 7.0 parts by mass, and the amount of high-boiling aromatic solvent was reduced by the same amount.
[0059] The content ratio of the methylphenyl silicone alkoxy oligomer in the wood protective coating of Experimental Example 7 relative to 100 parts by mass of the solvent-based acrylic resin, and the solvent-based hydrolyzable silicone compound having an epoxy group as a hardener The content ratios relative to 100 parts by mass of a coating composition mainly composed of an acrylic resin and a methylphenyl-based silicone alkoxy oligomer also correspond to 25.0 parts by mass and 2.0 parts by mass, respectively, the same as in Experimental Example 1. The content ratio of the scaly silica powder reacted with an isocyanate compound relative to 100 parts by mass of the solvent-based acrylic resin and the methylphenyl-based silicone alkoxy oligomer corresponds to 48 parts by mass.
[0060] The compositions of the wood protective coatings of Experimental Examples 2 to 7 thus prepared are shown together with the composition of the wood protective coating of Experimental Example 1 for each component in Table 2 below. [Table 2]
[0061] [Painting test (Experimental Examples 2-7)] Using the wood protective paints of Experimental Examples 2-7 thus prepared, commercially available flame-retardant treated cedar wood (knot-free) of 70 x 100 x 10 mm and 70 x 150 x 10 mm were prepared, and immediately applied to a predetermined thickness by brush coating under predetermined conditions, and the surface condition immediately after coating was observed. As a result, just after coating, no abnormalities were found in the coating film, as in Experimental Example 1 and Comparative Example 2, and it was confirmed that a normal coating film was formed.
[0062] [Wet and dry cycle test (Experimental Examples 1 to 7, Comparative Example 2)] Next, a wet and dry cycle test was conducted on the test specimens on which the wood protective coatings of Experimental Examples 1 to 7 and Comparative Example 2 were formed, to confirm the extent to which efflorescence occurred. The wet and dry cycle test consisted of leaving the specimens under conditions of 40°C and 90% RH for 24 hours, followed by sending them to dry at 60°C for 24 hours, and this cycle was repeated up to 5 times to determine the extent of efflorescence generation and the paint's evaluation. The surface condition of the test specimens on which the wood protective coatings of Experimental Examples 1 to 7 and Comparative Example 2 were formed after the wet and dry cycle test is shown in FIG. 2. FIG. 2 is a surface photograph of each of the test specimens of Experimental Examples 1 to 7 and Comparative Example 2 after the wet and dry cycle test.
[0063] The degree of efflorescence was evaluated as follows based on the surface condition after the wet-dry cycle test shown in FIG. 2. First, a transparent sheet divided into squares was used to count the number of squares in the area where efflorescence was observed on the surface of the test specimen, and the ratio of the number of squares to the total number of squares on the surface of the test specimen was measured and evaluated. The size of the squares was 5 mm squares. Regarding the distinction between efflorescence and non-efflorescence, if there was white (including light white) on the surface of the coating film, it was considered to be an efflorescence area, and discoloration inside the coating film was not evaluated. In addition, efflorescence transferred from the side to the edge of the coating film surface was also not evaluated. In this evaluation, if the number of squares in the efflorescence area was less than 5% of the total, it was judged as "◯", if it was 5% or more but less than 30%, it was judged as "△", and if it was 30% or more, it was judged as "X". The efflorescence generation ratio and the judgment results are shown in Table 3 below, along with the content of methylphenyl-based silicone alkoxy oligomer relative to 100 parts by mass of solvent-based acrylic resin and the amount of curing agent added to the coating composition.
[0064] [Table 3]
[0065] The results shown in Table 3 reveal the following: The wood protective paint of Experimental Example 2 contains simple flaky silica instead of the flaky silica powder reacted with an isocyanate compound in the wood protective paint of Experimental Example 1, and the wood protective paint of Experimental Example 3 does not contain flaky silica powder itself, but the rate of efflorescence formation is very high at 86% to 78%. In contrast, when the wood protective paint of Experimental Example 1, which uses flaky silica powder reacted with an isocyanate compound, is used, the rate of efflorescence formation is very low at 1%. This is because the scaly silica powder reacted with the isocyanate compound used in the wood protective paint of Experimental Example 1 has its isocyanate groups firmly fixed by reaction with the solvent-based acrylic resin and methylphenyl-based silicone alkoxy oligomer in the paint composition, and combined with the fact that the wood protective paint of Experimental Example 1 forms a strong, glassy coating film, the coating film is unlikely to be scratched or damaged even when subjected to repeated wet and dry tests, and it is believed that this prevents the leaching of the flame retardant treatment agent from the flame retardant-treated wood and prevents the formation of efflorescence.
[0066] In addition, the wood protective coating material of Experimental Example 4 contains less scaly silica powder reacted with an isocyanate compound and less hydrolyzable silicone compound having an epoxy group as a curing agent than the wood protective coating material of Experimental Example 1, but the efflorescence generation rate is 1%, which is the same as that of Experimental Example 1. Therefore, taking into consideration the results of Experimental Examples 1 to 4, if the wood protective coating material contains a coating composition mainly composed of a solvent-based acrylic resin and a methylphenyl-based silicone alkoxy oligomer, a curing agent containing a hydrolyzable silicone compound having an epoxy group, and a scaly silica powder reacted with an isocyanate compound, when a coating film is formed on wood that has been flame-retardant treated, it shows that a good efflorescence suppression effect is achieved even if it is repeatedly dried and wet. From the results of Experimental Example 4, the lower limit of the content of the methylphenyl-based silicone alkoxy oligomer is thought to be 10 parts by mass relative to 100 parts by mass of the solvent-based acrylic resin. Furthermore, based on the results of Experimental Example 4, the lower limit of the content of the curing agent containing a hydrolyzable silicone compound having an epoxy group in a coating composition mainly composed of a solvent-based acrylic resin and a methylphenyl-based silicone alkoxy oligomer is believed to be 0.5 parts by mass.
[0067] Furthermore, the wood protective coating of Experimental Example 5 is the wood protective coating of Experimental Example 1, except that the content of methylphenyl-based silicone alkoxy oligomer relative to the solvent-based acrylic resin has been increased, and the content of a curing agent containing a hydrolyzable silicone compound having an epoxy group and a scaly silica powder reacted with an isocyanate compound has been increased; however, the rate of efflorescence formation was 1%, which is the same as in Experimental Example 1.
[0068] In addition, the wood protective coating of Experimental Example 6 is the wood protective coating of Experimental Example 1, in which the proportion of scaly silica powder in the scaly silica powder reacted with an isocyanate compound is increased, and the amount of the isocyanate compound itself is the same, and the wood protective coating of Experimental Example 7 is the wood protective coating of Experimental Example 1, in which the proportion of isocyanate in the scaly silica powder reacted with an isocyanate compound is increased, and the amount of the scaly silica powder is the same, but the efflorescence generation rate is very high at 86% to 78%. Therefore, taking into consideration the results of Experimental Examples 1 and 5 to 7 comprehensively, the upper limit of the content of the methylphenyl-based silicone alkoxy oligomer is thought to be 60 parts by mass relative to 100 parts by mass of the solvent-based acrylic resin, based on the results of Experimental Example 5. In addition, the upper limit of the content of the curing agent containing a hydrolyzable silicone compound having an epoxy group in the coating composition mainly composed of a solvent-based acrylic resin and a methylphenyl-based silicone alkoxy oligomer is thought to be 20.0 parts by mass, based on the results of Experimental Example 5.
[0069] [Weather Resistance Test] Next, a weather resistance test was conducted on other test specimens on which the wood protective coatings of Experimental Examples 1 to 7 and Comparative Example 2 were formed, to confirm the extent to which efflorescence occurred. The weather resistance test was conducted by performing accelerated deterioration by ultraviolet light and water for 500 hours in accordance with the cycle A method of JIS K5600-7-7 using an accelerated weather resistance tester (xenon lamp method), and the degree of efflorescence generation and the evaluation as a paint were obtained in the same manner as in the above-mentioned dry-wet repeated test. The surface state of the test specimens on which the wood protective coatings of Experimental Examples 1 to 7 and Comparative Example 2 were formed after the weather resistance test is shown in FIG. 3. Note that FIG. 3 is a surface photograph of each of the test specimens of Experimental Examples 1 to 7 and Comparative Example 2 after the weather resistance test.
[0070] The rate of efflorescence formation and the evaluation results are shown in Table 4 below, together with the content of methylphenyl-based silicone alkoxy oligomer per 100 parts by mass of solvent-based acrylic resin and the amount of curing agent added to the coating composition.
[0071] [Table 4]
[0072] From the results shown in Table 4, depending on the weather resistance test, almost no efflorescence was observed in Experimental Examples 1 to 6, and a little more efflorescence was observed in Experimental Example 7. However, even in Experimental Example 7, the efflorescence generation rate was almost the same as in Comparative Example 2, and it was confirmed that efflorescence is unlikely to occur in fire-retardant treated wood in the weather resistance test. Therefore, according to the wood protective coating of the present invention, since the coating film is unlikely to be scratched or damaged even by repeated drying and wetting, even if the fire-retardant treated wood is used outdoors, the agent is not prematurely leached out by wind and rain, the fire-retardant effect is sustained for a long period of time, and furthermore, the elution of the fire-retardant treatment agent from the fire-retardant treated wood is suppressed, and the formation of efflorescence is reduced.
Claims
1. A wood protective paint having a flame retardant treatment agent sealing effect, A coating composition mainly composed of a solvent-based acrylic resin and a methylphenyl-based silicone alkoxy oligomer; a curing agent including a hydrolyzable silicone compound having an epoxy group; a scaly silica powder reacted with an isocyanate compound; A protective coating for wood, comprising a coating prepared from a mixture of:
2. 2. The wood protective coating according to claim 1, wherein the content of the methylphenyl-based silicone alkoxy oligomer is from 10 to 60 parts by mass per 100 parts by mass of the solvent-based acrylic resin.
3. 3. The wood protective coating according to claim 1, wherein the amount of the hardener added is 0.5 parts by mass or more and 20 parts by mass or less based on 100 parts by mass of the coating composition.
Citation Information
Patent Citations
Flexibility-imparting normal temperature curable inorganic coating agent for protection of chemical floor
JP2010163584A
Two liquid type wood coating material, and flame retardant treatment method for wood using the two liquid type wood coating material
JP2017052853A
Coating for wood
JP2022166929A
A coating composition system, the preparation method, and the use thereof
US20190330494A1
Modified wood treated with silicone emulsion composition
JP2006159554A