Steel material

A steel material with controlled Mo and Mn segregation at grain boundaries, combined with a specific chemical composition and microstructure, addresses the challenge of hydrogen embrittlement in sour environments, achieving high strength and resistance to cracking.

JP2024137052APending Publication Date: 2024-10-04NIPPON STEEL CORPORATION

Patent Information

Application Number
JP2023048406
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing steel materials used in sour environments, such as oil wells and high-pressure hydrogen accumulators, face challenges in achieving high strength and sufficient hydrogen embrittlement resistance, as current techniques do not adequately address the issue of hydrogen-induced cracking and embrittlement.

Method used

A steel material with a specific chemical composition and microstructure is developed, including elements like Mo and Mn segregation control, to enhance hydrogen embrittlement resistance by ensuring a high ratio of martensite and bainite, refined austenite grains, and a balanced Mo and Mn segregation at grain boundaries, defined by the equation [Mo]_SEG - [Mn]_SEG > 8.00.

Benefits of technology

The steel material exhibits high strength and excellent hydrogen embrittlement resistance, maintaining a yield strength of 758 to 965 MPa with a relative fracture stress ratio of 0.80 or more, effectively preventing hydrogen-induced cracking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137052000001_ABST
    Figure 2024137052000001_ABST
Patent Text Reader

Abstract

To provide a steel material having high strength and excellent in hydrogen brittleness resistance.SOLUTION: A disclosed steel material contains, by mass percentage, C: 0.15-0.50%, Si: 0.05-0.50%, Mn: 0.01-1.00%, P: not exceeding 0.0300%, S: not exceeding 0.0100%, Cr: 0.20-1.20%, Mo: 0.40-1.50%, Ti: 0.0010-0.0300%, V: 0.01-0.50%, Nb: 0.0050-0.1000%, Al: 0.0050-0.1000%, B: 0.0001-0.0050%, N: not exceeding 0.0100%, and O: not exceeding 0.0050%, the remainder consists of Fe and impurities, with a total area fraction of martensite and bainite exceeding 90%, a crystal grain size of the former austenite grains is 15.0 μm or less, and a segregation amount of Mo at grain boundaries [Mo]SEG and Mn segregation amount [Mn]SEG satisfy the following equation: [Mo]SEG-[Mn]SEG>8.00.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This disclosure relates to steel products, and more particularly, to steel products for use in sour environments. [Background technology]

[0002] Some oil wells and gas wells (hereinafter, oil wells and gas wells are collectively referred to as "oil wells") have environments that contain a large amount of corrosive substances. Examples of corrosive substances include corrosive gases such as hydrogen sulfide. In this specification, an environment that contains hydrogen sulfide is referred to as a "sour environment." The temperature of a sour environment is from room temperature to about 200°C, depending on the depth of the well.

[0003] Examples of steel materials used in such sour environments include oil well steel pipes, which are used as oil well tubular goods, and line pipe steel pipes, which are used as line pipes, etc. High strength is required for steel materials used in such sour environments.

[0004] Furthermore, when steel materials are used in sour environments, contact with corrosive substances causes an electrochemical reaction, generating hydrogen on the steel surface. This hydrogen makes the steel susceptible to hydrogen embrittlement cracking, typically sulfide stress corrosion cracking (SSC). Therefore, steel materials used in sour environments are required to have high strength as well as excellent hydrogen embrittlement resistance.

[0005] Techniques for improving hydrogen embrittlement resistance in steel materials used in sour environments are disclosed in JP 2011-246798 A (Patent Document 1) and JP 2015-38247 A (Patent Document 2).

[0006] In Patent Document 1, a certain amount of solute Mo is secured in an oil well steel pipe made of low alloy steel, prior austenite grains are refined, and M2C type precipitates are dispersed. This improves SSC resistance. Patent Document 1 also forms Mo segregation regions at prior austenite grain boundaries to further improve hydrogen embrittlement resistance.

[0007] In Patent Document 2, in an oil well steel pipe made of low alloy steel, the Mo segregation region is suppressed as much as possible, thereby improving hydrogen embrittlement resistance.

[0008] More recently, progress has been made in the development of fuel cell vehicles that run on hydrogen as fuel, and in the practical application of hydrogen stations that supply hydrogen to fuel cell vehicles. High-pressure hydrogen gas is stored in high-pressure hydrogen storage tanks installed at hydrogen stations. Development of automobiles equipped with high-pressure hydrogen storage tanks as fuel cell vehicles is also underway. The steel materials used in such high-pressure hydrogen storage tanks are required to have high strength as well as excellent hydrogen embrittlement resistance.

[0009] A technology for improving hydrogen embrittlement resistance in steel materials for use in high-pressure hydrogen storage tanks is proposed in JP 2009-74122 A (Patent Document 3). In Patent Document 3, in a steel material made of low alloy steel, the V content and Mo content are increased more than conventionally, thereby improving the morphology of carbides at the prior austenite grain boundaries and improving hydrogen embrittlement resistance. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2011-246798 A [Patent Document 2] JP 2015-38247 A [Patent Document 3] JP 2009-74122 A Summary of the Invention [Problem to be solved by the invention]

[0011] However, high strength and sufficient hydrogen embrittlement resistance may be obtained by other means than those described in the above Patent Documents 1 to 3.

[0012] An object of the present disclosure is to provide a steel material having high strength and excellent resistance to hydrogen embrittlement. [Means for solving the problem]

[0013] The steel material of the present disclosure has the following configuration.

[0014] A steel material, Chemical composition, in mass%, C: 0.15-0.50%, Si: 0.05 to 0.50%, Mn: 0.01 to 1.00%, P:0.0300% or less, S: 0.0100% or less, Cr: 0.20~1.20%, Mo: 0.40-1.50%, Ti: 0.0010 to 0.0300%, V: 0.01 to 0.50%, Nb: 0.0050~0.1000%, Al: 0.0050~0.1000%, B: 0.0001~0.0050%, N: 0.0100% or less, O: 0.0050% or less, W: 0 to 2.00%, Co: 0-0.20%, Cu: 0-0.50%, Ni: 0 to 0.50%, Sn: 0-0.50%, Mg: 0 to 0.0100%, Ca: 0 to 0.0100%, Rare earth elements: 0 to 0.0100%, and the balance being Fe and impurities, The total area ratio of martensite and bainite is 90% or more, The yield strength is less than 758 to 965 MPa, The grain size of the prior austenite grains is 15.0 μm or less, One end point of a 10 nm line segment SL that is centered on the grain boundary of a prior austenite grain and perpendicular to the grain boundary is defined as E1 and the other end point is defined as E2. At each measurement point arranged at a pitch of 0.2 nm from the end point E1 to the end point E2 of the line segment SL, the Mo content (mass%) and the Mn content (mass%) at each measurement point on the line segment SL are determined by elemental analysis using energy dispersive X-ray spectroscopy; In the line segment SL, The measurement point on the line segment SL where the Mo content is maximum is defined as the Mo peak measurement point, The region having a width of 2.0 nm and centered on the Mo peak measurement point is defined as the Mo segregation region. A region between the end point E1 and the Mo segregation region is defined as a first Mo intragranular region, A region between the end point E2 and the Mo segregation region is defined as a second Mo intragranular region, The arithmetic average value of the Mo content at all the measurement points in the first Mo grain region is defined as [Mo] BM1 (% by mass), The arithmetic average value of the Mo content at all the measurement points in the second Mo intragranular region is defined as [Mo] BM2 (% by mass), In the line segment SL, The measurement point on the line segment SL where the Mn content is maximum is defined as the Mn peak measurement point, A region having a width of 2.0 nm and centered on the Mn peak measurement point is defined as a Mn segregation region. A region between the end point E1 and the Mn segregation region is defined as a first Mn intragranular region, A region between the end point E2 and the Mn segregation region is defined as a second Mn intragranular region, The arithmetic average value of the Mn content at all the measurement points in the first Mn grain region is defined as [Mn] BM1 (% by mass), The arithmetic average value of the Mn content at all the measurement points in the second Mn grain region is defined as [Mn] BM2 (mass%), The amount of Mo segregation defined by formula (1) [Mo] SEG and the amount of Mn segregation defined by equation (2) [Mn] SEG and satisfy the formula (3). Steel material. [Mo] SEG= {(total Mo content at all the measurement points on the line segment SL × 0.2) - [Mo] BM1 × (distance between the end point E1 and the Mo peak measurement point)−[Mo] BM2 × (the distance between the end point E2 and the Mo peak measurement point)} / 0.8 + ([Mo] BM1 +[Mo] BM2 ) / twenty one) [Mn] SEG = {(total Mn content at all the measurement points on the line segment SL × 0.2) - [Mn] BM1 × (distance between the end point E1 and the Mn peak measurement point)−[Mn] BM2 × (the distance between the end point E2 and the Mn peak measurement point)} / 0.8 + ([Mn] BM1 +[Mn] BM2 ) / twenty two) [Mo] SEG -[Mn] SEG >8.00 (3) Effect of the Invention

[0015] The steel material according to the present disclosure has high strength and excellent resistance to hydrogen embrittlement. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a diagram showing the relationship between Fn1 (=[Mo]SEG-[Mn]SEG) and the relative fracture stress ratio, which is an index of hydrogen embrittlement resistance. [Diagram 2] FIG. 2 is a schematic diagram of the observation surface of a polished test piece in the method for measuring the amount of Mo segregation [Mo]SEG and the amount of Mn segregation [Mn]SEG. [Diagram 3] FIG. 3 is a schematic diagram of a measurement area in the observation plane shown in FIG. 2, in which the grain boundaries of prior austenite grains are identified. [Figure 4] FIG. 4 is a schematic diagram showing how a thin film sample is taken from the measurement region shown in FIG. [Diagram 5] FIG. 5 is a perspective view of the thin film sample of FIG. [Figure 6]FIG. 6 is a schematic diagram for explaining the relationship between the electron beam and the crystal grain boundaries in a thin film sample during TEM observation and elemental analysis by the EDS method. [Figure 7] FIG. 7 is a schematic diagram showing the relationship between the irradiation direction of the electron beam EB in the EDS method, the crystal grain boundary GB on the surface 10 of the thin film sample TP, and the element concentration profile. [Figure 8] FIG. 8 shows an example of the Mo content on a line segment SL that is centered on a grain boundary and perpendicular to the grain boundary. [Figure 9] FIG. 9 is a schematic diagram for explaining the formula (1). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The present inventors first investigated a steel material having high strength and excellent hydrogen embrittlement resistance from the viewpoint of chemical composition. As a result, the composition was found to be, in mass%, C: 0.15-0.50%, Si: 0.05-0.50%, Mn: 0.01-1.00%, P: 0.0300% or less, S: 0.0100% or less, Cr: 0.20-1.20%, Mo: 0.40-1.50%, Ti: 0.0010-0.0300%, V: 0.01-0.50%, Nb: 0.0050-0.1000%, Al: 0.0050-0.1000%, B: 0.0001-0.0001. It was believed that a chemical composition consisting of the following elements may be possible: Cu: 0-0.0050%, N: 0.0100% or less, O: 0.0050% or less, W: 0-2.00%, Co: 0-0.20%, Cu: 0-0.50%, Ni: 0-0.50%, Sn: 0-0.50%, Mg: 0-0.0100%, Ca: 0-0.0100%, rare earth elements: 0-0.0100%, and the remainder being Fe and impurities.

[0018] The present inventors further investigated the microstructure of the steel material and found that, if the steel material has the above-mentioned chemical composition and the total area ratio of martensite and bainite is 90% or more, a high strength of 758 to less than 965 MPa (110 ksi class to 125 ksi class) can be obtained.

[0019] Therefore, the inventors further studied means for improving the hydrogen embrittlement resistance of steel material having the above-mentioned chemical composition and a total area ratio of martensite and bainite of 90% or more. Here, the inventors verified the mechanism of hydrogen embrittlement. As a result, the inventors considered that the hydrogen embrittlement resistance of the steel material can be improved by refining the prior austenite grains to increase the grain boundary area and strengthening the grain boundaries. As a result of the verification, the inventors considered that a sufficient grain boundary area can be secured if the grain size of the prior austenite grains is 15.0 μm or less.

[0020] Therefore, the present inventors further investigated ways to strengthen the grain boundaries. First, the inventors focused on the amount of Mo segregation in the steel material. Then, they found that the grain boundaries can be strengthened by increasing the amount of Mo segregation at the grain boundaries.

[0021] However, there are cases where sufficient hydrogen embrittlement resistance cannot be obtained simply by increasing the amount of Mo segregation at the grain boundaries. Therefore, the present inventors further investigated the strengthening mechanism of the grain boundaries. As a result, the following findings were obtained.

[0022] Among the elements in the above chemical composition, if the amount of Mo segregated at the grain boundary is high, the grain boundary will be strengthened. In other words, Mo is an element that strengthens the grain boundary. On the other hand, if the amount of Mn segregated at the grain boundary is high, the grain boundary will be embrittled. In other words, Mn is an element that embrittles the grain boundary.

[0023] Therefore, even if the amount of Mo segregation at the grain boundaries is large, if the amount of Mn segregation at the grain boundaries is also large, the grain boundary strengthening effect due to the amount of Mo segregation is offset by the grain boundary embrittlement effect due to the amount of Mn segregation.

[0024] Considering the above, the inventors of the present invention thought that if the amount of Mo segregation at the grain boundaries is large relative to the amount of Mn segregation at the grain boundaries, the grain boundaries will be strengthened, and as a result, sufficient hydrogen embrittlement resistance will be obtained. Based on this technical idea, the inventors of the present invention have SEG (mass%) and the amount of Mn segregation at grain boundaries [Mn]SEG As a result, the amount of Mo segregation at the grain boundaries [Mo] defined by the formula (1) below was SEG and the amount of Mn segregation at the grain boundary defined by the equation (2) described below [Mn] SEG However, the present inventors have found that sufficient hydrogen embrittlement resistance can be obtained if formula (3) is satisfied. [Mo] SEG -[Mn] SEG >8.00 (3)

[0025] Let Fn1 be defined as follows: Fn1=[Mo] SEG -[Mn] SEG Fig. 1 is a diagram showing the relationship between Fn1 and the relative rupture stress ratio, which is an index of hydrogen embrittlement resistance. The higher the relative rupture stress ratio, the better the hydrogen embrittlement resistance. Fig. 1 was created based on the results of the examples described later.

[0026] 1, in a steel material having the above-mentioned chemical composition and a yield strength of 758 to less than 965 MPa, if Fn1 exceeds 8.00, the relative fracture stress ratio is 0.80 or more, and excellent hydrogen embrittlement resistance is obtained. On the other hand, if Fn1 is 8.00 or less, the relative fracture stress ratio is less than 0.80, and hydrogen embrittlement resistance is significantly reduced.

[0027] Therefore, the amount of Mo segregation at the grain boundaries [Mo] SEG and the amount of Mn segregation at grain boundaries [Mn] SEG If and satisfy formula (3), sufficient hydrogen embrittlement resistance can be obtained.

[0028] The steel material according to this embodiment, which has been completed based on the above findings, has the following configuration.

[0029] [1] A steel material, Chemical composition, in mass%, C: 0.15-0.50%, Si: 0.05 to 0.50%, Mn: 0.01 to 1.00%, P:0.0300% or less, S: 0.0100% or less, Cr: 0.20~1.20%, Mo: 0.40-1.50%, Ti: 0.0010 to 0.0300%, V: 0.01 to 0.50%, Nb: 0.0050~0.1000%, Al: 0.0050~0.1000%, B: 0.0001~0.0050%, N: 0.0100% or less, O: 0.0050% or less, W: 0 to 2.00%, Co: 0-0.20%, Cu: 0-0.50%, Ni: 0 to 0.50%, Sn: 0-0.50%, Mg: 0 to 0.0100%, Ca: 0 to 0.0100%, Rare earth elements: 0 to 0.0100%, and the balance being Fe and impurities, The total area ratio of martensite and bainite is 90% or more, The yield strength is less than 758 to 965 MPa, The grain size of the prior austenite grains is 15.0 μm or less, One end point of a 10 nm line segment SL that is centered on the grain boundary of a prior austenite grain and perpendicular to the grain boundary is defined as E1 and the other end point is defined as E2. At each measurement point arranged at a pitch of 0.2 nm from the end point E1 to the end point E2 of the line segment SL, the Mo content (mass%) and the Mn content (mass%) at each measurement point on the line segment SL are determined by elemental analysis using energy dispersive X-ray spectroscopy; In the line segment SL, The measurement point on the line segment SL where the Mo content is maximum is defined as the Mo peak measurement point, The region having a width of 2.0 nm and centered on the Mo peak measurement point is defined as the Mo segregation region. A region between the end point E1 and the Mo segregation region is defined as a first Mo intragranular region, A region between the end point E2 and the Mo segregation region is defined as a second Mo intragranular region, The arithmetic average value of the Mo content at all the measurement points in the first Mo grain region is defined as [Mo] BM1 (% by mass), The arithmetic average value of the Mo content at all the measurement points in the second Mo intragranular region is defined as [Mo] BM2 (% by mass), In the line segment SL, The measurement point on the line segment SL where the Mn content is maximum is defined as the Mn peak measurement point, A region having a width of 2.0 nm and centered on the Mn peak measurement point is defined as a Mn segregation region. A region between the end point E1 and the Mn segregation region is defined as a first Mn intragranular region, A region between the end point E2 and the Mn segregation region is defined as a second Mn intragranular region, The arithmetic average value of the Mn content at all the measurement points in the first Mn grain region is defined as [Mn] BM1 (% by mass), The arithmetic average value of the Mn content at all the measurement points in the second Mn grain region is defined as [Mn] BM2 (mass%), The amount of Mo segregation defined by formula (1) [Mo] SEG and the amount of Mn segregation defined by equation (2) [Mn] SEG and satisfy the formula (3). Steel material. [Mo] SEG = {(total Mo content at all the measurement points on the line segment SL × 0.2) - [Mo] BM1 × (distance between the end point E1 and the Mo peak measurement point)−[Mo] BM2 × (the distance between the end point E2 and the Mo peak measurement point)} / 0.8 + ([Mo] BM1 +[Mo] BM2 ) / twenty one) [Mn] SEG = {(total Mn content at all the measurement points on the line segment SL × 0.2) - [Mn] BM1 × (distance between the end point E1 and the Mn peak measurement point)−[Mn]BM2 × (the distance between the end point E2 and the Mn peak measurement point)} / 0.8 + ([Mn] BM1 +[Mn] BM2 ) / twenty two) [Mo] SEG -[Mn] SEG >8.00 (3)

[0030] [2] The steel material according to [1], The chemical composition is W: 0.01 to 2.00%, Co: 0.01 to 0.20%, Cu: 0.01 to 0.50%, Ni: 0.01 to 0.50%, Sn: 0.01 to 0.50%, Mg: 0.0001 to 0.0100%, Ca: 0.0001 to 0.0100%, and Rare earth elements: 0.0001~0.0100%, Contains one or more elements selected from the group consisting of Steel material.

[0031] [3] The steel material according to [1] or [2], The steel material is any one of a steel pipe for oil wells, a steel pipe for line pipes, and a steel pipe for high-pressure hydrogen storage tanks. Steel material.

[0032] [4] The steel material according to [1] or [2], The steel material is any one of a seamless steel pipe for oil wells, a seamless steel pipe for line pipes, and a seamless steel pipe for high-pressure hydrogen storage tanks. Steel material.

[0033] In this specification, "oil well steel pipe" means steel pipe used as oil well tubular goods. Oil well tubular goods is a general term for casing, tubing, and drill pipe used for drilling oil wells or gas wells, extracting crude oil or natural gas, etc. "Oil well seamless steel pipe" means that the oil well steel pipe is a seamless pipe.

[0034] In this specification, "steel pipe for line pipe" means a steel pipe for line pipe use constituting a pipeline for transporting produced fluid (crude oil or natural gas) extracted from an oil well or gas well. Examples of pipelines include flow lines for transporting produced fluid from oil wells or gas wells, gathering lines for collecting the produced fluid transported in the flow lines and transporting it to a primary treatment facility, trunk lines for transporting the produced fluid that has been subjected to primary treatment such as dehydration to the vicinity of the market, and distribution lines for transporting it to consumers. "Seamless steel pipe for line pipe" means that the steel pipe for line pipe is a seamless steel pipe.

[0035] In this specification, "steel pipe for high-pressure hydrogen pressure storage vessel" refers to a steel pipe standardized by ISO11439, ANSI / NGV, the High Pressure Gas Safety Act, Container Safety Regulation Exemplary Standards, etc., and used as a high-pressure hydrogen pressure storage vessel in which high-pressure hydrogen gas is stored. High-pressure hydrogen pressure storage vessels are installed, for example, at hydrogen stations or mounted on fuel cell vehicles. "Seamless steel pipe for high-pressure hydrogen pressure storage vessel" means that the steel pipe for high-pressure hydrogen pressure storage vessel is a seamless steel pipe.

[0036] The steel material of this embodiment will be described in detail below. "%" for elements means mass % unless otherwise specified.

[0037] [Features of the steel material of this embodiment] The steel material of this embodiment satisfies the following characteristics 1 to 5. (Feature 1) Chemical composition, by mass%, is C: 0.15-0.50%, Si: 0.05-0.50%, Mn: 0.01-1.00%, P: 0.0300% or less, S: 0.0100% or less, Cr: 0.20-1.20%, Mo: 0.40-1.50%, Ti: 0.0010-0.0300%, V: 0.01-0.50%, Nb: 0.0050-0.1000%, Al: 0.0050- 0.1000%, B: 0.0001-0.0050%, N: 0.0100% or less, O: 0.0050% or less, W: 0-2.00%, Co: 0-0.20%, Cu: 0-0.50%, Ni: 0-0.50%, Sn: 0-0.50%, Mg: 0-0.0100%, Ca: 0-0.0100%, rare earth elements: 0-0.0100%, and the balance is Fe and impurities. (Feature 2) The total area ratio of martensite and bainite is 90% or more. (Feature 3) The yield strength is less than 758 to 965 MPa. (Feature 4) The grain size of the prior austenite is 15.0 μm or less. (Feature 5) One end point of a 10 nm line segment SL that is centered on the grain boundary of a prior austenite grain and perpendicular to the grain boundary is defined as E1 and the other end point as E2. At each measurement point arranged at a pitch of 0.2 nm from end point E1 to end point E2 on the line segment SL, the Mo content (mass%) and the Mn content (mass%) at each measurement point on the line segment SL are determined by elemental analysis using energy dispersive X-ray spectroscopy; On the line segment SL, The measurement point on the line segment SL where the Mo content is maximum is defined as the Mo peak measurement point. The 2.0 nm wide region centered on the Mo peak measurement point was defined as the Mo segregation region. The region between the end point E1 and the Mo segregation region is defined as the first Mo intragranular region, The region between the end point E2 and the Mo segregation region is defined as the second Mo intragranular region, The arithmetic mean value of the Mo content at all measurement points in the first Mo grain region is defined as [Mo] BM1 (% by mass), The arithmetic mean value of the Mo content at all measurement points in the second Mo grain region was defined as [Mo] BM2 (% by mass), On the line segment SL, The measurement point on the line segment SL where the Mn content is maximum is defined as the Mn peak measurement point. The 2.0 nm wide region centered on the Mn peak measurement point was defined as the Mn segregation region. The region between the end point E1 and the Mn segregation region is defined as a first Mn intragranular region, The region between the end point E2 and the Mn segregation region is defined as the second Mn intragranular region, The arithmetic mean value of the Mn content at all measurement points in the first Mn grain intragranular region is defined as [Mn] BM1 (% by mass), The arithmetic mean value of the Mn content at all measurement points in the second Mn grain region is defined as [Mn] BM2 (mass%), The amount of Mo segregation defined by formula (1) [Mo] SEG and the amount of Mn segregation defined by equation (2) [Mn] SEG and satisfy the formula (3). [Mo] SEG = {(Sum of Mo content at all measurement points on line segment SL × 0.2) - [Mo] BM1 × (distance between end point E1 and Mo peak measurement point) - [Mo] BM2 × (distance between end point E2 and Mo peak measurement point)} / 0.8 + ([Mo] BM1 +[Mo] BM2 ) / twenty one) [Mn] SEG = {(total Mn content at all measurement points on line segment SL × 0.2) - [Mn] BM1 × (distance between end point E1 and Mn peak measurement point) - [Mn] BM2 × (distance between end point E2 and Mn peak measurement point)} / 0.8 + ([Mn] BM1 +[Mn] BM2 ) / twenty two) [Mo] SEG -[Mn] SEG >8.00 (3) Features 1 to 5 will be explained below.

[0038] [(Feature 1) Chemical composition] The chemical composition of the steel material of this embodiment contains the following elements.

[0039] C: 0.15-0.50% Carbon (C) improves hardenability and increases the strength of the steel material. C also forms carbides or carbonitrides, which increases the strength of the steel material. If the C content is less than 0.15%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the C content exceeds 0.50%, even if the contents of other elements are within the ranges of this embodiment, the amount of carbides in the steel material will be excessively large, and in this case, the hydrogen embrittlement resistance of the steel material will decrease. Therefore, the C content is 0.15 to 0.50%. The lower limit of the C content is preferably 0.17%, more preferably 0.19%, more preferably 0.21%, more preferably 0.23%, and even more preferably 0.25%. The upper limit of the C content is preferably 0.45%, more preferably 0.40%, further preferably 0.35%, and further preferably 0.32%.

[0040] Silicon: 0.05 to 0.50% Silicon (Si) deoxidizes steel and reduces inclusions in the steel material. As a result, the hydrogen embrittlement resistance of the steel material is improved. If the Si content is less than 0.05%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Si content exceeds 0.50%, the hydrogen embrittlement resistance of the steel material decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the Si content is 0.05 to 0.50%. The lower limit of the Si content is preferably 0.07%, more preferably 0.09%, further preferably 0.11%, and further preferably 0.13%. The upper limit of the Si content is preferably 0.45%, more preferably 0.43%, further preferably 0.41%, and further preferably 0.38%.

[0041] Mn: 0.01 to 1.00% Manganese (Mn) deoxidizes steel. Mn also improves hardenability and strength of steel. If the Mn content is less than 0.01%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Mn content is too high, even if the contents of other elements are within the ranges of this embodiment, coarse sulfide-based inclusions are formed, and the hydrogen embrittlement resistance of the steel material decreases. Therefore, the Mn content is 0.01 to 1.00%. The lower limit of the Mn content is preferably 0.05%, more preferably 0.10%, even more preferably 0.15%, and still more preferably 0.20%. The upper limit of the Mn content is preferably 0.95%, more preferably 0.90%, more preferably 0.80%, more preferably 0.70%, more preferably 0.60%, more preferably 0.50%, more preferably 0.45%, and more preferably 0.30%.

[0042] P:0.0300% or less Phosphorus (P) is an unavoidable impurity, meaning that the lower limit of the P content is greater than 0%. If the P content exceeds 0.0300%, P will segregate to grain boundaries even if the contents of other elements are within the ranges of this embodiment, and therefore the hydrogen embrittlement resistance of the steel material will decrease. Therefore, the P content is 0.0300% or less. It is preferable that the P content is as low as possible. However, an extreme reduction in the P content significantly increases the production cost. Therefore, in consideration of industrial production, the lower limit of the P content is preferably 0.0001%, more preferably 0.0005%, and even more preferably 0.0010%. The upper limit of the P content is preferably 0.0250%, more preferably 0.0230%, more preferably 0.0210%, more preferably 0.0200%, more preferably 0.0190%, and more preferably 0.0180%.

[0043] S: 0.0100% or less Sulfur (S) is an unavoidable impurity. In other words, the lower limit of the S content is greater than 0%. If the S content exceeds 0.0100%, S will segregate to grain boundaries even if the contents of other elements are within the ranges of this embodiment, and therefore the hydrogen embrittlement resistance of the steel material will decrease. Therefore, the S content is 0.0100% or less. The S content is preferably as low as possible. However, an extreme reduction in the S content significantly increases the production cost. Therefore, in consideration of industrial production, the lower limit of the S content is preferably 0.0001%, more preferably 0.0002%, and even more preferably 0.0005%. The upper limit of the S content is preferably 0.0090%, more preferably 0.0080%, more preferably 0.0070%, more preferably 0.0060%, more preferably 0.0050%, more preferably 0.0040%, more preferably 0.0030%, and more preferably 0.0020%.

[0044] Cr: 0.20~1.20% Chromium (Cr) enhances the hardenability of steel. Cr also enhances the temper softening resistance of steel, making high-temperature tempering possible. As a result, hydrogen embrittlement resistance of steel is improved. If the Cr content is less than 0.20%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Cr content exceeds 1.20%, the hydrogen embrittlement resistance of the steel material decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the Cr content is 0.20 to 1.20%. The lower limit of the Cr content is preferably 0.25%, more preferably 0.30%, and further preferably 0.35%. The upper limit of the Cr content is preferably 1.10%, more preferably 1.05%, further preferably 1.00%, and further preferably 0.95%.

[0045] Mo: 0.40-1.50% Molybdenum (Mo) improves the hardenability of steel. Mo also improves the temper softening resistance of steel, making high-temperature tempering possible. As a result, hydrogen embrittlement resistance of steel is improved. If the Mo content is less than 0.40%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Mo content exceeds 1.50%, the above effects become saturated even if the contents of other elements are within the ranges of this embodiment. Therefore, the Mo content is 0.40 to 1.50%. The lower limit of the Mo content is preferably 0.45%, more preferably 0.50%, and further preferably 0.55%. The upper limit of the Mo content is preferably 1.48%, more preferably 1.46%, more preferably 1.40%, more preferably 1.35%, more preferably 1.30%, more preferably 1.25%, more preferably 1.20%, and more preferably 1.15%.

[0046] Ti: 0.0010~0.0300% Titanium (Ti) forms fine precipitates such as Ti nitrides and refines crystal grains. As a result, hydrogen embrittlement resistance of the steel material is improved. If the Ti content is less than 0.0010%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Ti content exceeds 0.0300%, even if the contents of other elements are within the range of this embodiment, coarse Ti nitrides are generated. The coarse Ti nitrides become the starting points of cracks. As a result, the hydrogen embrittlement resistance of the steel material is reduced. Therefore, the Ti content is 0.0010 to 0.0300%. The lower limit of the Ti content is preferably 0.0015%, more preferably 0.0020%, more preferably 0.0025%, more preferably 0.0030%, and more preferably 0.0040%. The upper limit of the Ti content is preferably 0.0250%, more preferably 0.0200%, more preferably 0.0150%, more preferably 0.0120%, and more preferably 0.0100%.

[0047] V: 0.01 to 0.50% Vanadium (V) forms carbides and refines the crystal grains of steel due to the pinning effect of the carbides. This improves the hydrogen embrittlement resistance of the steel. Furthermore, V forms fine carbides during tempering to improve the temper softening resistance of the steel, thereby improving the strength of the steel. If the V content is less than 0.01%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the V content exceeds 0.50%, even if the contents of other elements are within the ranges of this embodiment, carbonitrides and the like are formed in excess, which reduces the hydrogen embrittlement resistance of the steel material. Therefore, the V content is 0.01 to 0.50%. The lower limit of the V content is preferably 0.02%, more preferably 0.05%, further preferably 0.07%, and further preferably 0.10%. The upper limit of the V content is preferably 0.45%, more preferably 0.40%, more preferably 0.35%, more preferably 0.30%, more preferably 0.25%, and more preferably 0.20%.

[0048] Nb: 0.0050~0.1000% Niobium (Nb) forms carbides, nitrides, or carbonitrides (hereinafter referred to as "carbonitrides, etc."), and the pinning effect of the carbonitrides, etc., refines the crystal grains of the steel material. This improves the hydrogen embrittlement resistance of the steel material. Nb also forms fine carbides during tempering, which improves the temper softening resistance of the steel material. This improves the strength of the steel material. If the Nb content is less than 0.0050%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Nb content exceeds 0.1000%, even if the contents of other elements are within the ranges of this embodiment, excessive amounts of carbonitrides and the like are formed, and therefore the hydrogen embrittlement resistance of the steel material decreases. Therefore, the Nb content is 0.0050 to 0.1000%. The lower limit of the Nb content is preferably 0.0100%, more preferably 0.0150%, and further preferably 0.0200%. The upper limit of the Nb content is preferably 0.0800%, more preferably 0.0750%, more preferably 0.0700%, more preferably 0.0650%, and more preferably 0.0600%.

[0049] Al: 0.0050~0.1000% Aluminum (Al) deoxidizes steel. Furthermore, Al bonds with N to form Al nitrides. Al nitrides suppress grain coarsening through a pinning effect. As a result, the hydrogen embrittlement resistance of the steel material is improved. If the Al content is less than 0.0050%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Al content exceeds 0.1000%, even if the contents of other elements are within the ranges of this embodiment, coarse oxides are generated, and the hydrogen embrittlement resistance of the steel material decreases. Therefore, the Al content is 0.0050 to 0.1000%. The lower limit of the Al content is preferably 0.0080%, more preferably 0.0100%, and further preferably 0.0120%. The upper limit of the Al content is preferably 0.0800%, more preferably 0.0600%, more preferably 0.0400%, more preferably 0.0300%, and even more preferably 0.0200%. The "Al" content in this specification means the content of "acid-soluble Al", that is, "sol. Al".

[0050] B: 0.0001 to 0.0050% Boron (B) improves the hardenability of steel material and increases its strength. B also suppresses the grain boundary segregation of P and increases the hydrogen embrittlement resistance of steel material. If the B content is less than 0.0001%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the B content exceeds 0.0050%, even if the contents of other elements are within the ranges of this embodiment, coarse B nitrides are generated. The coarse B nitrides become the starting points of cracks. Therefore, the hydrogen embrittlement resistance of the steel material is reduced. Therefore, the B content is 0.0001 to 0.0050%. The lower limit of the B content is preferably 0.0003%, more preferably 0.0005%, and further preferably 0.0007%. The upper limit of the B content is preferably 0.0040%, more preferably 0.0035%, more preferably 0.0030%, more preferably 0.0028%, and even more preferably 0.0026%.

[0051] N: 0.0100% or less Nitrogen (N) is unavoidably contained. In other words, the lower limit of the N content is more than 0%. N combines with Ti to form nitrides, which have a pinning effect and refine the grains of the steel. As a result, the strength of the steel is increased. However, if the N content is too high, even if the contents of other elements are within the ranges of this embodiment, coarse nitrides are formed, and the hydrogen embrittlement resistance of the steel material decreases. Therefore, the N content is 0.0100% or less. The lower limit of the N content is preferably 0.0001%, more preferably 0.0005%, and further preferably 0.0010%. The upper limit of the N content is preferably 0.0080%, more preferably 0.0070%, and further preferably 0.0060%.

[0052] O: 0.0050% or less Oxygen (O) is an unavoidable impurity. That is, the lower limit of the O content is more than 0%. If the O content exceeds 0.0050%, even if the contents of other elements are within the ranges of this embodiment, coarse oxides are formed, and the hydrogen embrittlement resistance of the steel material decreases. Therefore, the O content is 0.0050% or less. The O content is preferably as low as possible. However, an extreme reduction in the O content increases the production cost. Therefore, in consideration of industrial production, the lower limit of the O content is preferably 0.0001%, more preferably 0.0005%, and even more preferably 0.0010%. The upper limit of the O content is preferably 0.0045%, more preferably 0.0040%, and further preferably 0.0035%.

[0053] The balance of the chemical composition of the steel material according to the present embodiment is composed of Fe and impurities. Here, the impurities in the chemical composition refer to substances that are mixed in from raw materials such as ore and scrap, or from the manufacturing environment, during industrial production of the steel material, and are not intentionally contained, but are allowed within a range that does not adversely affect the steel material according to the present embodiment.

[0054] [Optional Elements] The chemical composition of the steel material of this embodiment is further Instead of part of Fe, W: 0 to 2.00%, Co: 0 to 0.20% Cu: 0-0.50%, Ni: 0 to 0.50%, Sn: 0-0.50%, Mg: 0 to 0.0100%, Ca: 0 to 0.0100%, and Rare earth elements (REM): 0~0.0100%, It may contain one or more elements selected from the group consisting of:

[0055] [Group 1: W, Co, Cu, Ni and Sn] The chemical composition of the steel material according to the present embodiment may further contain, instead of a part of Fe, one or more elements selected from the group consisting of W, Co, Cu, Ni, and Sn. All of these elements are optional elements and may not be contained. When contained, W, Co, Cu, Ni, and Sn all increase the hydrogen embrittlement resistance of the steel material.

[0056] W:0~2.00% Tungsten (W) is an optional element and may not be contained, i.e., the W content may be 0%. When W is contained, it forms a corrosion film on the surface of the steel in a sour environment. This suppresses the penetration of hydrogen into the steel. Therefore, the hydrogen embrittlement resistance of the steel is improved. Even if even a small amount of W is contained, the above effect can be obtained to a certain extent. However, if the W content is too high, even if the contents of other elements are within the ranges of this embodiment, coarse carbides are formed, and therefore the hydrogen embrittlement resistance of the steel material decreases. Therefore, the W content is 0 to 2.00%. The lower limit of the W content is preferably 0.01%, more preferably 0.05%, further preferably 0.10%, and further preferably 0.15%. The upper limit of the W content is preferably 1.50%, more preferably 1.20%, more preferably 1.00%, more preferably 0.90%, and more preferably 0.80%.

[0057] Co: 0 to 0.20% Cobalt (Co) is an optional element and may not be contained, that is, the Co content may be 0%. When contained, Co increases the hydrogen embrittlement resistance of the steel material. Furthermore, Co dissolves in the steel material to increase the hardenability and strength of the steel material. Even if even a small amount of Co is contained, the above effects can be obtained to a certain extent. However, when the Co content exceeds 0.20%, the effect becomes saturated. Therefore, the Co content is 0 to 0.20%. The lower limit of the Co content is preferably 0.01%, more preferably 0.02%, and further preferably 0.03%. The upper limit of the Co content is preferably 0.18%, more preferably 0.15%, further preferably 0.12%, and further preferably 0.10%.

[0058] Cu: 0-0.50% Copper (Cu) is an optional element and may not be contained, that is, the Cu content may be 0%. When contained, Cu enhances the hydrogen embrittlement resistance of the steel material. Furthermore, Cu dissolves in the steel material to enhance the hardenability and strength of the steel material. Even if even a small amount of Cu is contained, the above effects can be obtained to a certain extent. However, if the Cu content exceeds 0.50%, Cu precipitates in the steel material even if the contents of other elements are within the ranges of this embodiment, and in this case, the hydrogen embrittlement resistance of the steel material decreases. Therefore, the Cu content is 0 to 0.50%. The lower limit of the Cu content is preferably 0.01%, more preferably 0.02%, more preferably 0.03%, more preferably 0.05%, and even more preferably 0.07%. The upper limit of the Cu content is preferably 0.48%, more preferably 0.46%, and further preferably 0.44%.

[0059] Ni: 0 to 0.50% Nickel (Ni) is an optional element and may not be contained, that is, the Ni content may be 0%. When contained, Ni enhances the hydrogen embrittlement resistance of the steel. Ni also dissolves in the steel to enhance the hardenability and strength of the steel. Even if even a small amount of Ni is contained, the above effects can be obtained to a certain extent. However, if the Ni content exceeds 0.50%, even if the contents of other elements are within the ranges of this embodiment, localized corrosion progresses and the hydrogen embrittlement resistance of the steel material decreases. Therefore, the Ni content is 0 to 0.50%. The lower limit of the Ni content is preferably 0.01%, more preferably 0.02%, further preferably 0.03%, and further preferably 0.05%. The upper limit of the Ni content is preferably 0.49%, more preferably 0.48%, and further preferably 0.47%.

[0060] Sn: 0 to 0.50% Tin (Sn) is an optional element and may not be contained, that is, the Sn content may be 0%. When contained, Sn enhances the hydrogen embrittlement resistance of the steel material. Even if even a small amount of Sn is contained, the above effect can be obtained to a certain extent. However, if the Sn content exceeds 0.50%, the hot workability of the steel material decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the Sn content is 0 to 0.50%. The lower limit of the Sn content is preferably 0.01%, more preferably 0.02%, further preferably 0.03%, and further preferably 0.05%. The upper limit of the Sn content is preferably 0.49%, more preferably 0.48%, and further preferably 0.47%.

[0061] [Group 2: Mg, Ca and rare earth elements (REM)] The chemical composition of the steel material according to the present embodiment may further contain, instead of a portion of Fe, one or more elements selected from the group consisting of Mg, Ca, and rare earth elements (REM). All of these elements are optional elements and may not be contained. When contained, Mg, Ca, and rare earth elements (REM) increase the hydrogen embrittlement resistance of the steel material.

[0062] Magnesium: 0 to 0.0100% Magnesium (Mg) is an optional element and may not be contained, that is, the Mg content may be 0%. When contained, Mg refines Mn sulfides in the steel material and improves the hydrogen embrittlement resistance of the steel material. Even if even a small amount of Mg is contained, the above effect can be obtained to a certain extent. However, if the Mg content exceeds 0.0100%, even if the contents of other elements are within the ranges of this embodiment, the oxides in the steel material become coarse, and therefore the hydrogen embrittlement resistance of the steel material decreases. Therefore, the Mg content is 0 to 0.0100%. The lower limit of the Mg content is preferably 0.0001%, more preferably 0.0003%, more preferably 0.0006%, and even more preferably 0.0010%. The upper limit of the Mg content is preferably 0.0090%, more preferably 0.0080%, more preferably 0.0070%, more preferably 0.0060%, and more preferably 0.0050%.

[0063] Ca: 0 to 0.0100% Calcium (Ca) is an optional element and may not be contained, that is, the Ca content may be 0%. When contained, Ca refines Mn sulfides in the steel material and improves the hydrogen embrittlement resistance of the steel material. Even if even a small amount of Ca is contained, the above effect can be obtained to a certain extent. However, if the Ca content exceeds 0.0100%, even if the contents of other elements are within the ranges of this embodiment, the oxides in the steel material become coarse, and therefore the hydrogen embrittlement resistance of the steel material decreases. Therefore, the Ca content is 0 to 0.0100%. The lower limit of the Ca content is preferably 0.0001%, more preferably 0.0003%, further preferably 0.0005%, and further preferably 0.0007%. The upper limit of the Ca content is preferably 0.0080%, more preferably 0.0060%, further preferably 0.0050%, and further preferably 0.0040%.

[0064] Rare earth elements (REM): 0~0.0100% Rare earth elements (REM) are optional elements and may not be included, i.e., the REM content may be 0%. When contained, REM refines Mn sulfides in the steel material and improves the hydrogen embrittlement resistance of the steel material. Even if even a small amount of REM is contained, the above effect can be obtained to a certain extent. However, if the REM content exceeds 0.0100%, even if the contents of other elements are within the ranges of this embodiment, the oxides in the steel material become coarse, and therefore the hydrogen embrittlement resistance of the steel material decreases. Therefore, the REM content is 0 to 0.0100%. The lower limit of the REM content is preferably 0.0001%, more preferably 0.0003%, still more preferably 0.0005%, and still more preferably 0.0010%. The upper limit of the REM content is preferably 0.0080%, more preferably 0.0060%, still more preferably 0.0050%, and still more preferably 0.0040%.

[0065] In this specification, REM refers to one or more elements selected from the group consisting of scandium (Sc) with atomic number 21, yttrium (Y) with atomic number 39, and the lanthanides lanthanum (La) with atomic number 57 to lutetium (Lu) with atomic number 71. In addition, in this specification, the REM content refers to the total content of these elements.

[0066] [(Feature 2) Total area ratio of martensite and bainite] In the microstructure of the steel material according to this embodiment, the total area ratio of martensite and bainite is 90% or more. The remainder of the microstructure is, for example, ferrite and / or pearlite. When the yield strength of a steel material satisfying characteristic 1 satisfies characteristic 3 and further satisfies characteristic 4, the microstructure of the steel material has a total area ratio of martensite and bainite of 90% or more. In other words, the microstructure of the steel material according to this embodiment is mainly composed of martensite. Note that martensite as used herein also includes tempered martensite. Furthermore, bainite also includes tempered bainite.

[0067] [Method for measuring the total area ratio of martensite and bainite] The total area ratio of martensite and bainite in the microstructure of the steel material of this embodiment can be determined by the following method. A test piece having an observation surface is taken from the steel material. When the steel material is a steel plate, a test piece is taken from the center of the plate width, which includes the plate thickness t / 4 part as the observation target region, and has an observation surface parallel to the rolling direction. Here, the plate thickness t / 4 part means a depth position of t / 4 from the surface of the steel plate, where t is the thickness of the steel plate. When the steel material is a steel pipe, a test piece is taken that includes the center of the wall thickness, which is the observation target area, and has an observation surface parallel to the axial direction of the pipe. When the steel material is a round bar (a steel bar with a circular cross section), a test piece is taken that includes the R / 2 portion, which is the observation target area, and has an observation surface parallel to the rolling direction. Here, the R / 2 portion refers to the center position of the radius in a cross section perpendicular to the axial direction of the round bar. The size of the test piece is not particularly limited. The size of the test piece is, for example, 10 mm in the length in the rolling direction × 5 mm in the width direction × 10 mm in the thickness direction. When the steel material is a steel plate, the thickness direction corresponds to the plate thickness direction, and the width direction corresponds to the plate width direction. When the steel material is a steel pipe, the rolling direction corresponds to the pipe axis direction, the thickness direction corresponds to the wall thickness direction, and the width direction corresponds to the direction perpendicular to the pipe axis direction and the wall thickness direction (circumferential direction). When the steel material is a round steel, the rolling direction corresponds to the axial direction, the thickness direction corresponds to the radial direction, and the width direction corresponds to the direction perpendicular to the rolling direction and the radial direction (circumferential direction). The surface including the rolling direction and the thickness direction (the surface of 10 mm × 10 mm in the case of the above-mentioned test piece size) is the observation surface.

[0068] After the observation surface of the test piece is polished to a mirror finish, it is immersed in a nital etching solution for about 10 seconds to reveal the structure by etching. Any 10 fields of view within the observation area of ​​the etched observation surface are observed as secondary electron images using a scanning electron microscope (SEM). If the steel material is a steel plate, the observation area is the plate thickness t / 4 part. If the steel material is a steel pipe, the observation area is the wall thickness center part. If the steel material is a round bar, the observation area is the R / 2 part. The area of ​​each of the 10 fields of view within the observation area is, for example, 400 μm 2 (Magnification: 5000x).

[0069] In each field, martensite and bainite are identified. In each field, martensite and bainite can be distinguished from other structures (ferrite, pearlite, etc.) based on their morphology. Specifically, a structure having a lamellar structure can be identified as pearlite. A woven phase including laths and lenses can be identified as martensite and bainite. A structure without a substructure within the grains can be identified as ferrite.

[0070] The total area ratio of the specified martensite and bainite is calculated. The method for calculating the total area ratio is not particularly limited, and any known method may be used. For example, the total area ratio of martensite and bainite can be calculated by image analysis. In this embodiment, the arithmetic average value of the total area ratio of martensite and bainite calculated in all visual fields (10 visual fields) is defined as the total area ratio (%) of martensite and bainite.

[0071] [Feature 3: Yield strength] The steel material according to this embodiment has a yield strength of 758 to less than 965 MPa. In this specification, the yield strength means a 0.2% proof stress obtained in a tensile test. The steel material according to this embodiment satisfies Features 1, 2, 4, and 5, and therefore has excellent hydrogen embrittlement resistance even if the yield strength is 758 to less than 965 MPa (i.e., 758 MPa or more and less than 965 MPa).

[0072] [Method of measuring yield strength] The yield strength of the steel material according to this embodiment can be determined by the following method. A tensile test is carried out according to a method in accordance with JIS Z2241: 2011. A round bar test piece is prepared from the steel material according to this embodiment. If the steel material is a steel plate, a round bar test piece is prepared from the center of the plate width and the center of the plate thickness. If the steel material is a steel pipe, a round bar test piece is prepared from the center of the wall thickness. If the steel material is a steel bar with a circular cross section, a round bar test piece is prepared from the R / 2 position. The size of the round bar test piece is, for example, a parallel part diameter of 6.0 mm and a parallel part length of 40 mm. The axial direction of the round bar test piece is parallel to the rolling direction of the steel material.

[0073] A tensile test is carried out using a round bar test piece at room temperature (25°C) in air, and the obtained 0.2% proof stress is defined as the yield strength (MPa).

[0074] [(Feature 4) Regarding the grain size of prior austenite grains] In the steel material according to the present embodiment, the grain size of the prior austenite grains is 15.0 μm or less. In this specification, the grain size of the prior austenite grains means the grain size of the prior austenite grains determined in accordance with the measurement method of the average intercept method specified in JIS G0551:2020.

[0075] Hydrogen embrittlement is likely to occur when hydrogen accumulates at grain boundaries. In steel satisfying Features 1 to 3, if the crystal grains are fine, the area of ​​the crystal grain boundaries increases. In this case, the amount of hydrogen accumulated per unit area of ​​the crystal grain boundaries decreases. This improves the hydrogen embrittlement resistance of the steel. If the prior γ grain size of the steel is 15.0 μm or less, it is possible to achieve both high strength and excellent hydrogen embrittlement resistance, provided that Features 1 to 3 and 5 are satisfied.

[0076] The upper limit of the grain size of the prior austenite grains in the steel material according to the present embodiment is preferably 14.5 μm, more preferably 14.0 μm, even more preferably 13.5 μm, and still more preferably 13.0 μm. The lower limit of the grain size of the prior austenite grains of the steel material according to the present embodiment is not particularly limited. The lower limit of the grain size of the prior austenite grains of the steel material according to the present embodiment is, for example, 3.0 μm, for example, 3.5 μm, for example, 4.0 μm.

[0077] [Method for measuring the grain size of prior austenite grains] The grain size of the prior austenite grains of the steel material of this embodiment can be determined by the following method: The grain size of the prior austenite grains is determined in accordance with the measurement method of the mean intercept method specified in JIS G0551:2020.

[0078] First, a test piece having an observation surface is taken from a steel material. When the steel material is a steel plate, a test piece is taken from the center of the plate width, including the plate thickness t / 4 part, which is the observation target area, and has an observation surface parallel to the rolling direction. When the steel material is a steel pipe, a test piece is taken from the center of the wall thickness, which is the observation target area, and has an observation surface parallel to the pipe axis direction. When the steel material is a round steel (a steel bar with a circular cross section), a test piece is taken from the R / 2 part, which is the observation target area, and has an observation surface parallel to the rolling direction. The size of the test piece is not particularly limited. The size of the test piece is, for example, 10 mm in the length in the rolling direction × 5 mm in the width direction × 10 mm in the thickness direction. The surface including the rolling direction and the thickness direction (10 mm × 10 mm surface when the test piece size is as described above) is the observation surface.

[0079] The observation surface of the test piece is mirror-polished. After mirror-polishing, the observation surface is immersed in a picral etching solution for about 10 seconds to expose the prior γ grain boundaries by etching. Ten arbitrary fields of view of the observation target area of ​​the etched observation surface are observed as secondary electron images using a scanning electron microscope (SEM) to generate photographic images. The observation magnification is, for example, 500 μm × 500 μm (magnification 200 times).

[0080] Using the generated photographic images, the grain size number is evaluated in accordance with the measurement method of the average intercept method specified in JIS G0551:2020. The grain size of the prior austenite grains in each field of view is calculated from the evaluated grain size number. The arithmetic average value of the grain size of the prior austenite grains calculated in 10 fields of view is defined as the grain size of the prior austenite grains (prior γ grain size) (μm).

[0081] [(Feature 5) Mo segregation amount [Mo] SEG and Mn segregation amount [Mn] SEG About As mentioned above, when Mo segregates to the grain boundaries, the grain boundaries are strengthened by Mo. On the other hand, when Mn segregates to the grain boundaries, the grain boundaries are embrittled by Mn. Therefore, when improving the hydrogen embrittlement resistance of steel, it is effective to increase the amount of Mo segregation at the grain boundaries while reducing the amount of Mn segregation at the grain boundaries as much as possible.

[0082] In the steel material of this embodiment, the difference between the amount of Mo segregation and the amount of Mn segregation at the grain boundaries of prior austenite grains is increased by increasing the amount of Mo segregation that strengthens the grain boundaries and reducing the amount of Mn segregation that embrittles the grain boundaries as much as possible, thereby strengthening the grain boundaries of prior austenite grains and improving hydrogen embrittlement resistance in sour environments.

[0083] Specifically, in the steel material of this embodiment, the amount of Mo segregation [Mo] defined by the formula (1) SEG and the amount of Mn segregation defined by equation (2) [Mn] SEG and satisfy the formula (3). [Mo] SEG = {(Sum of Mo content at all measurement points on line segment SL × 0.2) - [Mo] BM1 × (distance between end point E1 and Mo peak measurement point) - [Mo] BM2 × (distance between end point E2 and Mo peak measurement point)} / 0.8 + ([Mo] BM1 +[Mo] BM2 ) / twenty one) [Mn] SEG = {(total Mn content at all measurement points on line segment SL × 0.2) - [Mn] BM1 × (distance between end point E1 and Mn peak measurement point) - [Mn] BM2 × (distance between end point E2 and Mn peak measurement point)} / 0.8 + ([Mn] BM1 +[Mn] BM2 ) / twenty two) [Mo] SEG -[Mn] SEG >8.00 (3) The following is the amount of Mo segregation [Mo] SEG , Mn segregation amount [Mn] SEG We will now explain how to determine and the formulas (1) to (3).

[0084] [Mo segregation amount [Mo] SEG , Mn segregation amount [Mn] SEG How to calculate The amount of Mo segregation in the steel material of this embodiment [Mo] SEG , and Mn segregation amount [Mn] SEG can be calculated in the following way:

[0085] First, a test piece is taken from the steel material. When the steel material is a steel plate, a test piece is taken from the center of the plate width, including the specific position of the plate thickness t / 4 part, and having an observation surface including the rolling direction and the plate thickness direction. When the steel material is a steel pipe, a test piece is taken from the specific position of the wall thickness center, including the specific position of the pipe axis direction and the wall thickness direction. When the steel material is a round steel (a steel bar with a circular cross section), a test piece is taken from the specific position of the R / 2 part, including the specific position of the rolling direction and the radial direction. The size of the test piece is not particularly limited. The size of the test piece is, for example, 10 mm in the rolling direction length x 5 mm in the width direction x 8 mm in the thickness direction. As described above, the surface including the rolling direction and the thickness direction (10 mm x 8 mm surface when the test piece size is as described above) is the observation surface.

[0086] The observation surface is mechanically polished. It is then chemically polished with a colloidal silica suspension. Figure 2 is a schematic diagram of the observation surface of the test piece after polishing. In Figure 2, the T direction is the thickness direction, and the L direction is the rolling direction. If the steel material is a steel plate, the T direction is the plate thickness direction, and the L direction is the rolling direction. If the steel material is a steel pipe, the T direction is the wall thickness direction, and the L direction is the pipe axial direction. If the steel material is a round bar, the T direction is the radial direction, and the L direction is the rolling direction.

[0087] Referring to FIG. 2, the observation area 100 on the observation surface of the polished test piece is observed with a 200x optical microscope to obtain an optical microscope image. The observation area 100 includes a specific position. When the steel material is a steel plate, the observation area 100 is the center of the plate width and includes the plate thickness t / 4 part. When the steel material is a steel pipe, the observation area 100 includes the center of the wall thickness. When the steel material is a round bar, the observation area includes the 2 / R part. In the observation area 100, an arbitrary rectangular measurement area 10 of 100 μm×100 μm is selected. At this time, the measurement area 10 is selected so as to include the specific position. Marks 20 are applied to multiple corners of the measurement area so that the position of the selected measurement area 10 can be specified. The marks 20 may be, for example, impressions made by a micro Vickers hardness tester.

[0088] EBSD (Electron Back Scattering Diffraction) analysis is performed on the selected measurement area 10 to obtain crystal orientation information of the martensite phase. The step size in the EBSD analysis is set to 0.1 μm. Based on the obtained crystal orientation information and the Kurdjumov-Sachs relationship, the grain boundaries of the prior austenite grains are identified.

[0089] Fig. 3 is a schematic diagram of a measurement region 10 in which grain boundaries of prior austenite grains are identified. With reference to Fig. 3, a grain boundary GB in which the crystal orientation difference between adjacent prior austenite grains is 18° or more is selected from the grain boundaries identified in the measurement region 10. Then, a thin film sample TP perpendicular to the selected grain boundary GB is prepared.

[0090] Specifically, as shown in Fig. 4, a plate-shaped thin film sample TP is collected from the measurement region 10 by focused ion beam (FIB) processing. The upper surface of the thin film sample TP corresponds to a part of the measurement region 10. The upper surface of the thin film sample TP is rectangular, and the plate-shaped thin film sample TP is collected so that the long side of the upper surface is perpendicular to the selected grain boundary GB. As an FIB processing device, for example, a product name SMI3050SE manufactured by Hitachi High-Tech Science Corporation is used.

[0091] The collected thin film sample TP is shown in Figure 5. In the thin film sample TP, surface 10 corresponds to a part of the measurement region 10. Surface 30 is a surface perpendicular to surface 10. The grain boundary GB selected on surface 10 (measurement region 10) is naturally observed also on surface 30. The film thickness T10 of the thin film sample TP is 100 nm.

[0092] The collected thin film sample TP is used to perform TEM observation using a transmission electron microscope (TEM). A transmission electron microscope equipped with an EDS device is used for TEM observation. For example, a transmission electron microscope with a spherical aberration corrector manufactured by JEOL Ltd. (product name: NEOARM) and an EDS analyzer (product name: JED-2300T) manufactured by JEOL Ltd. are used for TEM observation.

[0093] As shown in FIG. 6, in the TEM observation, the thin film sample TP is first positioned so that the electron beam EB is incident on the surface 30 of the thin film sample TP. Then, the thin film sample TP is tilted so that the prior austenite grain boundary GB on the surface 10 is parallel to the incident direction of the electron beam EB. After that, a line segment SL with a total length of 10 nm is identified, which is centered on the prior austenite grain boundary GB on the surface 30 and perpendicular to the prior austenite grain boundary GB as viewed from the incident direction of the electron beam EB. Here, one end point of the line segment SL is defined as end point E1, and the other end point as viewed from the incident direction of the electron beam EB is defined as end point E2. The distance between end points E1 and E2 is 10 nm.

[0094] Next, elemental analysis is performed by energy dispersive X-ray spectroscopy (EDS) at each measurement point arranged at a pitch of 0.2 nm from end point E1 to end point E2 of the line segment SL. The Mo content (mass%) and Mn content (mass%) at each measurement point on the line segment SL are determined.

[0095] 7 is a schematic diagram showing the relationship between the irradiation direction of the electron beam EB during elemental analysis by the EDS method (during TEM observation), the grain boundary GB on the surface 10 of the thin film sample TP, and the element concentration profile. As shown in FIG. 7(A), when the electron beam EB is not parallel to the grain boundary GB on the surface 10 of the thin film sample TP, the peak of the element concentration profile PR on the line segment SL obtained by elemental analysis by the EDS method becomes broad. On the other hand, as shown in FIG. 7(B), when the electron beam EB is parallel to the grain boundary GB on the surface 10 of the thin film sample TP, the peak of the element concentration profile PR on the line segment SL becomes sharp. Therefore, when elemental analysis by the EDS method is performed, the thin film sample TP is tilted so that the electron beam EB is parallel to the grain boundary GB on the surface 10 of the thin film sample TP.

[0096] After determining the Mo content (mass%) and Mn content (mass%) at each measurement point on the line segment SL by elemental analysis using the EDS method, the amount of Mo segregation [Mo] was measured by the following method. SEG and Mn segregation amount [Mn] SEG Request.

[0097] [Mo segregation amount [Mo] SEG How to calculate Fig. 8 shows an example of the Mo content on the line segment SL. With reference to Fig. 8, the following definitions are given. The measurement point on line segment SL where the Mo content is maximum is defined as Mo peak measurement point P. The 2.0 nm wide region centered on the Mo peak measurement point P is defined as the Mo segregation region GB0. The region between the end point E1 of the line segment SL and the Mo segregation region GB0 is defined as the first Mo intragranular region BM1. The region between the end point E2 of the line segment SL and the Mo segregation region GB0 is defined as the second Mo intragranular region BM2. The arithmetic mean value of the Mo content at all measurement points in the first Mo grain intragranular region BM1 is defined as [Mo] BM1 (% by mass). The arithmetic mean value of the Mo content at all measurement points in the second Mo grain region BM2 is defined as [Mo] BM2 (% by mass).

[0098] Referring to FIG. 8, [Mo] in the first Mo grain region BM1 BM1 (mass%) and [Mo] in the second Mo grain region BM2 BM2 (mass%) is regarded as the Mo content in the grains of adjacent prior austenite grains across the prior austenite grain boundary GB. [Mo] BM1 (mass) and [Mo] BM2 In some cases, the average Mo content ([Mo] ) in the prior austenite grains in the first Mo intragranular region BM1 and the second Mo intragranular region BM2 is approximately the same, and in other cases, the average Mo content ([Mo] ) in the prior austenite grains in the first Mo intragranular region BM1 and the second Mo intragranular region BM2 is approximately the same, as in FIG. BM1 , [Mo] BM2 ) is required.

[0099] Mo content at each measurement point on line segment SL, [Mo] BM1 , [Mo] BM2 Using the above, the amount of Mo segregation at the line segment SL [Mo] SEG is defined as in equation (1). [Mo] SEG = {(Sum of Mo content at all measurement points on line segment SL × 0.2) - [Mo] BM1 × (distance between end point E1 and Mo peak measurement point) - [Mo] BM2 × (distance between end point E2 and Mo peak measurement point)} / 0.8 + ([Mo] BM1 +[Mo] BM2 ) / twenty one)

[0100] Here, equation (1) is divided as follows: A = (sum of Mo content at all measurement points on line segment SL × 0.2) B=[Mo] BM1 × (distance between end point E1 and Mo peak measurement point) C=[Mo] BM2 × (distance between end point E2 and Mo peak measurement point) D=([Mo] BM1 +[Mo] BM2 ) / 2

[0101] A corresponds to the total area of ​​the Mo content distribution in Fig. 8, that is, the total amount of Mo content on the line segment SL. Note that "0.2" in A means 0.2 nm, which is the pitch of the measurement points. B corresponds to the total amount of Mo content in the region BM10 between the end point E1 and the peak measurement point P of the line segment SL. The average Mo content in the region BM10 is expressed as [Mo] BM1 Region BM10 corresponds to the ideal intragranular region of a prior austenite grain when the Mo peak measurement point is assumed to be an ideal grain boundary. C corresponds to the total amount of Mo content in the region BM20 between the end point E2 and the peak measurement point P of the line segment SL. The average Mo content in the region BM20 is expressed as [Mo] BM2 The region BM20 corresponds to the ideal intragranular region of a prior austenite grain when the Mo peak measurement point is assumed to be an ideal grain boundary. Therefore, in formula (1), (ABC) is a value obtained by subtracting the total amount of Mo content in ideal intragranular regions BM10 and BM20 adjacent to each other across the ideal grain boundary GB from the total amount of Mo content on the line segment SL, as shown in FIG. 9, and corresponds to the difference ΔMo of Mo content in the Mo segregation region GB0 in FIG. 9.

[0102] As described above, ideally, the grain boundary GB perpendicular to the line segment SL does not exist as a wide range (line) on the line segment SL like the Mo segregation region GB0, but exists in a very narrow range centered on the Mo peak measurement point P. Therefore, in this specification, a 0.8 nm wide region on the line segment SL centered on the peak measurement point P is assumed to be the grain boundary GB region.

[0103] As described above, it is assumed that the ideal grain boundary GB is located in a 0.8 nm wide region centered on the Mo peak measurement point P on the line segment SL, and that ideal intragranular regions BM10 and BM20 exist in other regions as described above. In this case, it is assumed that the ideal distribution of Mo content on the line segment SL is such that the Mo content is maximum at the ideal grain boundary GB, and that the Mo content is constant at the average Mo content in the ideal intragranular regions BM10 and BM20. The above-mentioned D corresponds to the average Mo content in the ideal intragranular regions. Under the above assumptions, the Mo content (mass%) at the grain boundary GB is regarded as the value obtained by dividing ΔMo (=ABC) by 0.8 and adding the average value D of the Mo content in the ideal intragranular regions BM10 and BM20, i.e., formula (1).

[0104] The amount of Mo segregation [Mo] defined by the formula (1) obtained by the above method SEG is an index of the Mo content at the grain boundary GB.

[0105] [Mn segregation amount [Mn] SEG How to calculate Mn segregation amount [Mn] SEG The above [Mo segregation amount [Mo] SEG [Mn] is calculated in the same manner as in [Calculation of Mn]. Specifically, on the line segment SL, the measurement point where the Mn content is maximum on the line segment SL is defined as the Mn peak measurement point P. A 2.0 nm wide region centered on the Mn peak measurement point P is defined as the Mn segregation region GB0. On the line segment SL, the region between the end point E1 and the Mn segregation region GB0 is defined as the first Mn grain intragranular region BM1. The region between the end point E2 and the Mn segregation region GB0 is defined as the second Mn grain intragranular region BM2. The arithmetic average value of the Mn content at all measurement points in the first Mn grain intragranular region BM1 is defined as [Mn] BM1 The arithmetic mean value of the Mn content at all measurement points in the second Mn grain region BM2 is defined as [Mn] BM2 (% by mass). Based on the above definitions, the amount of Mn segregation [Mn] SEG Define. [Mn] SEG= {(total Mn content at all measurement points on line segment SL × 0.2) - [Mn] BM1 × (distance between end point E1 and Mn peak measurement point) - [Mn] BM2 × (distance between end point E2 and Mn peak measurement point)} / 0.8 + ([Mn] BM1 +[Mn] BM2 ) / twenty two)

[0106] [Regarding formula (3)] In the steel material of this embodiment, the amount of Mo segregation [Mo] obtained by the above method SEG and Mn segregation amount [Mn] SEG satisfies equation (3). [Mo] SEG -[Mn] SEG >8.00 (3)

[0107] Fn1=[Mo] SEG -[Mn] SEG If Fn1 exceeds 8.00, excellent hydrogen embrittlement resistance can be obtained in a sour environment, provided that Features 1 to 4 are satisfied.

[0108] The preferred lower limit of Fn1 is 8.10, more preferably 8.20, more preferably 8.30, more preferably 8.50, more preferably 9.00, more preferably 9.50, more preferably 10.00, more preferably 10.50, and more preferably 11.00. The upper limit of Fn1 is not particularly limited. However, taking into consideration the chemical composition of Feature 1, the upper limit of Fn1 is, for example, 16.00, for example, 15.50, for example, 15.00.

[0109] [Steel shape] The shape of the steel material of the present embodiment is not particularly limited, and may be a steel pipe, a steel plate, or a round steel bar (steel bar).

[0110] Preferably, the steel material of this embodiment is any one of steel pipes for oil wells, steel pipes for line pipes, and steel pipes for high-pressure hydrogen storage tanks. Steel pipes for oil wells refer to steel pipes for use as oil well tubular goods. Oil well tubular goods are, for example, casings, tubing, drill pipes, etc. used for drilling oil wells or gas wells, extracting crude oil or natural gas, etc. Steel pipes for line pipes refer to steel pipes for use as line pipes constituting pipelines for transporting production fluids (crude oil or natural gas) extracted from oil wells or gas wells. Examples of pipelines include flow lines that transport production fluids from oil wells or gas wells, gathering lines that collect the production fluids transported by the flow lines and transport them to primary treatment facilities, trunk lines that transport production fluids that have been subjected to primary treatment such as dehydration to the vicinity of the market, and distribution lines that transport them to consumers. Steel pipes for high-pressure hydrogen pressure storage tanks are standardized by ISO11439, ANSI / NGV, the High Pressure Gas Safety Act, and the Illustrated Standards for Container Safety Regulations, and refer to steel pipes for use as high-pressure hydrogen pressure storage tanks in which high-pressure hydrogen gas is stored. High-pressure hydrogen pressure storage tanks are installed, for example, in hydrogen stations and on fuel cell vehicles.

[0111] More preferably, the steel material of this embodiment is any one of a seamless steel pipe for oil wells, a seamless steel pipe for line pipes, and a seamless steel pipe for high-pressure hydrogen pressure tanks. Seamless steel pipe for oil wells means that the steel pipe for oil wells is a seamless steel pipe. Seamless steel pipe for line pipes means that the steel pipe for line pipes is a seamless steel pipe. Seamless steel pipe for high-pressure hydrogen pressure tanks means that the steel pipe for high-pressure hydrogen pressure tanks is a seamless steel pipe.

[0112] [Manufacturing method] An example of a method for manufacturing the steel material of this embodiment will be described. Note that the manufacturing method described below is just one example, and the manufacturing method of the steel material of this embodiment is not limited to this. In other words, as long as the steel material of this embodiment having the above-mentioned configuration can be manufactured, the manufacturing method is not limited to the manufacturing method described below. However, the manufacturing method described below is a suitable manufacturing method for manufacturing the steel material of this embodiment.

[0113] An example of a method for manufacturing a steel material according to this embodiment includes the following steps. (Process 1) Material preparation process (Process 2) Hot processing process (Step 3) Quenching and tempering In this manufacturing method, the quenching and tempering step 3 satisfies the following conditions. (Condition 1) In the cooling during the tempering process, the average cooling rate CR1 at 640 to 500° C. is set to 30 to 100° C. / min. Each step will be described below.

[0114] [(Process 1) Material preparation process] In the material preparation process, first, molten steel having the above-mentioned chemical composition that satisfies Feature 1 is produced by a known refining method. The produced molten steel is used to produce a slab by continuous casting. Here, the slab is a slab, a bloom, or a billet. Instead of the slab, the molten steel may be used to produce an ingot by ingot casting. If necessary, the slab, bloom, or ingot may be hot-rolled to produce a billet. The material (slab, bloom, or billet) is produced by the above-mentioned production process.

[0115] [(Process 2) Hot processing process] In the hot working process, the prepared material is hot worked. When the final product is a steel pipe, first, the raw material is heated in a heating furnace. The heating temperature is not particularly limited, but is, for example, 1100 to 1300°C. The raw material extracted from the heating furnace is subjected to hot working to manufacture a mother pipe (seamless steel pipe). For example, the Mannesmann process is performed as the hot working to manufacture a mother pipe. In this case, the billet is pierced and rolled using a piercing machine. The billet after piercing and rolling is subjected to elongation rolling using a mandrel mill. Furthermore, as necessary, the billet after elongation rolling is subjected to sizing rolling using a reducer or a sizing mill. Through the above steps, a mother pipe is manufactured.

[0116] A blank pipe may be produced from the billet by a hot working method other than the Mannesmann process. For example, in the case of a short, thick-walled steel material such as a coupling, a blank pipe may be produced by forging such as the Erhardt process, or by hot extrusion.

[0117] When the final product is a steel plate, for example, the raw material (slab) is hot-rolled using one or more rolling mills each including a pair of rolls to produce the steel plate. The heating temperature before hot rolling is not particularly limited, but is, for example, 1100 to 1300°C.

[0118] When the final product is a steel bar, for example, blooming using a blooming mill and / or hot rolling using a continuous rolling mill are performed on the raw material (bloom). That is, blooming may be performed on the raw material to produce a steel bar, or blooming may not be performed on the raw material but hot rolling using a continuous rolling mill to produce a steel bar, or blooming using a blooming mill and hot rolling using a continuous rolling mill to produce a steel bar. The continuous rolling mill has a plurality of rolling stands arranged in a row, and each stand includes a pair of rolling rolls. When blooming is performed, the heating temperature before blooming is not particularly limited, but is, for example, 1100 to 1300°C. When hot rolling is performed using a continuous rolling mill, the heating temperature before hot rolling is not particularly limited, but is, for example, 1100 to 1300°C.

[0119] [(Step 3) Quenching and tempering process] In the quenching and tempering process, the steel material after the hot working process is subjected to the quenching and tempering processes.

[0120] [Quenching process] In the quenching process, the steel material produced in the hot working process is quenched. Quenching is performed by a well-known method. Specifically, the hot worked steel material is loaded into a heat treatment furnace and held at the quenching temperature. The quenching temperature is A C3 The temperature is equal to or higher than the transformation point, for example, 900 to 1000° C. After the steel material is held at the quenching temperature, it is rapidly cooled (quenched).

[0121] The holding time at the quenching temperature is not particularly limited, but is, for example, 10 to 60 minutes. The quenching method is, for example, water cooling. The quenching method is not particularly limited. When the steel material is a steel pipe, the mother pipe may be quenched by immersing it in a water tank or an oil tank, or the steel pipe may be quenched by pouring cooling water onto the outer surface and / or inner surface of the steel pipe or spraying cooling water from a nozzle.

[0122] After the hot working, the steel material may be quenched (direct quenching) immediately after the hot working without being cooled to room temperature, or the steel material may be loaded into a reheating furnace before the temperature of the hot working steel material drops and held at the quenching temperature, after which quenching is performed.

[0123] [Tempering process] In the tempering process, the steel material after the quenching process is tempered to adjust the yield strength of the steel material to 758 to less than 965 MPa.

[0124] The tempering temperature is, for example, 650 to 1000°C. C1 The tempering temperature is the transformation point. The holding time at the tempering temperature is not particularly limited, but is, for example, 10 to 180 minutes. By appropriately adjusting the tempering temperature depending on the chemical composition, the yield strength of the steel material having the above-mentioned chemical composition that satisfies the characteristic 1 can be adjusted.

[0125] The tempering temperature described above means the furnace temperature (° C.) in the heat treatment furnace, and the holding time at the tempering temperature means the furnace time (the time from charging into the heat treatment furnace to being extracted).

[0126] [Regarding condition 1] In the tempering process, after the above-mentioned holding time has elapsed at the above-mentioned tempering temperature, the steel material is cooled. This cooling satisfies the following conditions. (Condition 1) The average cooling rate CR1 at 640 to 500°C is set to 30 to 100°C / min. The temperature range of 640 to 500°C is where the diffusion of Mn is promoted. If the average cooling rate CR1 is less than 30°C / min, the diffusion of Mn is promoted, and as a result, Mn accumulates at the grain boundaries. Therefore, the amount of Mn segregation [Mn] SEGTherefore, Fn1 is 8.00 or less. On the other hand, if the average cooling rate CR1 exceeds 100°C / min, the amount of Mo segregation [Mo] SEG Therefore, Fn1 is 8.00 or less. If the average cooling rate CR1 is 30 to 100°C / min, the amount of Mo segregation [Mo] SEG and Mn segregation amount [Mn] SEG is in the appropriate range, and Fn1 exceeds 8.00.

[0127] The average cooling rate CR1 is determined by the following method: Measure the time it takes for the steel temperature to drop from 640°C to 500°C. Based on the obtained time, calculate the average cooling rate CR1.

[0128] The quenching step and the tempering step may be performed once each, or may be performed multiple times. For example, after the quenching step and the tempering step are performed, the quenching step and the tempering step may be performed again. When the quenching step and the tempering step are performed multiple times, the tempering step performed last may be performed so as to satisfy condition 1.

[0129] By carrying out the above manufacturing process, a steel material satisfying Features 1 to 5 can be manufactured. EXAMPLES

[0130] The effect of the steel material of this embodiment will be described more specifically with reference to examples. The conditions in the following examples are one example of conditions adopted to confirm the feasibility and effect of the steel material of this embodiment. Therefore, the steel material of this embodiment is not limited to this one example of conditions.

[0131] Steel materials (steel plates) having the chemical compositions shown in Tables 1-1 and 1-2 were manufactured.

[0132] [Table 1-1]

[0133] [Table 1-2]

[0134] In Table 1-2, "-" indicates that the content of the corresponding element is below the impurity level.

[0135] The steel materials of each test number were manufactured by the following method. Ingots having the chemical compositions shown in Tables 1-1 and 1-2 were manufactured by a casting method. The ingots were subjected to hot forging to manufacture blocks having a thickness of 50 mm.

[0136] The block material was subjected to a hot working process. Specifically, the block material was heated to 1250°C. The heated block material was then hot rolled to produce a steel material (steel plate) having a thickness of 15 mm. The produced steel material was allowed to cool to room temperature.

[0137] The steel material was cooled to room temperature and then subjected to quenching and tempering processes. Specifically, the steel material was quenched at the quenching temperature (°C) and for the holding time (minutes) at the quenching temperature shown in Table 2. After the holding time had elapsed, the steel material was quenched by water cooling. The steel material after quenching was tempered. The tempering temperature (°C), holding time (min) at the tempering temperature, and average cooling rate CR1 in the temperature range of 640 to 500°C during cooling are as shown in Table 2. In the "Tempering process" column in Table 2, the notation "30-100" in "CR1 (°C / min)" means that the average cooling rate CR1 was within the range of 30 to 100°C / min.

[0138] [Table 2]

[0139] Through the above manufacturing process, steel materials (steel plates) with each test number were manufactured.

[0140] [Evaluation test] The manufactured steel materials were subjected to the following evaluation tests. (Test 1) Total area ratio measurement test of martensite and bainite (Test 2) Yield strength measurement test (Test 3) Measurement of grain size of prior austenite grains (Test 4) Mo segregation amount [Mo] SEG , Mn segregation amount [Mn] SEG Measurement Test (Test 5) Hydrogen embrittlement resistance evaluation test Each evaluation test will be described below.

[0141] [(Test 1) Measurement of total area ratio of martensite and bainite] A test piece was taken from the center of the plate width of the steel material of each test number, including the plate thickness t / 4 part, which was the observation target area, and the surface including the rolling direction and the plate thickness direction was taken as the observation surface. The size of the test piece was 10 mm in the rolling direction, 5 mm in the plate width direction, and 10 mm in the plate thickness direction. The observation surface was 10 mm in the rolling direction × 10 mm in the plate thickness direction. The martensite area ratio (%) was determined by carrying out a method conforming to the above-mentioned [Method for measuring the total area ratio of martensite and bainite] on the taken test piece. The field area was 400 μm 2 The total area ratio (%) of martensite and bainite obtained is shown in the "M+B total area ratio (%)" column in Table 2.

[0142] [(Test 2) Yield strength measurement test] A round bar test piece was taken from the center of the plate thickness of the steel material of each test number. The parallel part of the round bar test piece had a diameter of 6.0 mm and a length of 40 mm. The axial direction of the round bar test piece was the same as the rolling direction of the steel material. The yield strength (MPa) was determined using the round bar test piece in accordance with the above-mentioned [Method of measuring yield strength]. The obtained yield strength is shown in the "Yield strength (MPa)" column in Table 2.

[0143] [(Test 3) Measurement of grain size of prior austenite grains] A test piece was taken from the center of the sheet width of the steel material of each test number, including the sheet thickness t / 4 part, which is the observation target area, and the surface including the rolling direction and the sheet thickness direction as the observation surface. The size of the test piece was 10 mm in the rolling direction, 5 mm in the sheet width direction, and 10 mm in the sheet thickness direction. The observation surface was 10 mm in the rolling direction × 10 mm in the sheet thickness direction. The prior γ grain size (μm) of the taken test piece was obtained according to the above-mentioned [Method of measuring the crystal grain size of prior austenite grains]. At this time, the field area was 500 μm × 500 μm (magnification 200 times). The obtained prior γ grain size is shown in the "Prior γ grain size (μm)" column in Table 2.

[0144] [(Test 4) Mo segregation amount [Mo] SEG , Mn segregation amount [Mn] SEG Measurement Test] A test piece was taken from the center of the sheet width of the steel material of each test number, including the sheet thickness t / 4 part, which was the observation target area, and the surface including the rolling direction and the sheet thickness direction was the observation surface. The size of the test piece was 10 mm in the rolling direction, 5 mm in the sheet width direction, and 8 mm in the sheet thickness direction. The observation surface was 10 mm in the rolling direction × 8 mm in the sheet thickness direction. Using the obtained test piece, the above-mentioned [Mo segregation amount [Mo] SEG , Mn segregation amount [Mn] SEG According to the method for determining the amount of Mo segregation [Mo] SEG (mass%) and Mn segregation amount [Mn] SEG The amount of Mo segregation (mass%) was calculated. SEG and Mn segregation amount [Mn] SEG Based on this, Fn1 was calculated. The amount of Mo segregation obtained [Mo] SEG , Mn segregation amount [Mn] SEG , and Fn1 are shown in Table 2.

[0145] [(Test 5) Hydrogen embrittlement resistance evaluation test] The hydrogen embrittlement resistance of the steel material having each test number was evaluated by the following method.

[0146] First, two round bar test pieces with an annular notch were cut from the center of the plate width and the plate thickness t / 4 part of the steel material of each test number. The outer diameter of the parallel part of each test piece was 4.0 mm, the length of the parallel part was 25 mm, and an annular notch was formed at the longitudinal center position of the parallel part. The notch shape had a notch depth of 0.3 mm, a notch angle of 60°, and a curvature radius of the notch bottom of 0.125 mm.

[0147] Assuming use in a sour environment, hydrogen was charged to one of the two annular notched round bar specimens by the cathodic hydrogen charging method. Specifically, a room temperature cathodic hydrogen charging solution was prepared. The cathodic hydrogen charging solution was an aqueous solution containing 5 mass% sodium chloride solution at room temperature, 30 g / L NHSCN, and an acetate buffer solution, and the pH before the test was adjusted to pH 3.5 using the acetate buffer solution.

[0148] The annular notched round bar test specimens were immersed in the cathodic hydrogen charging solution and charged with hydrogen at a potential of -1.5V for 24 hours. In other words, a sour environment was simulated by charging with hydrogen. A zinc plating film was formed on the surface of the hydrogen-charged annular notched round bar test specimen under the same conditions for each test number, to prevent hydrogen from leaking out of the annular notched round bar test specimen. Hydrogen was not charged to the other annular notched round bar test specimen.

[0149] A round bar specimen with a ring notch on which a zinc plating film was formed was subjected to a strain rate test of 4.2×10 at room temperature in air using a slow strain rate tester (SSRT). -6 The tensile test was carried out at a strain rate of 1 / sec to determine the breaking stress BS1 (MPa). The obtained breaking stress is shown in the "Hydrogen charge breaking stress (MPa)" column in Table 2.

[0150] In addition, a circular notched round bar specimen with each test number that was not charged with hydrogen was subjected to a strain rate test of 4.2×10 at room temperature in air using a slow strain rate test machine (SSRT). -6The tensile test was carried out at a strain rate of 1 / sec to determine the breaking stress BS0 (MPa). The breaking stress obtained is shown in the "Breaking stress without hydrogen charging (MPa)" column in Table 2.

[0151] Using the determined breaking stresses BS0 and BS1, the relative breaking stress ratio (%) was calculated according to the following formula. Relative breaking stress ratio = BS1 / BS0 When the relative rupture stress ratio was 0.80 or more, it was determined that the hydrogen embrittlement resistance was excellent. The obtained relative rupture stress ratios are shown in the "Relative rupture stress ratio" column in Table 2.

[0152] [Evaluation Results] With reference to Tables 1-1, 1-2, and 2, in test numbers 1 to 58, the steel materials satisfied features 1 to 5. Therefore, even though the yield strength was high at 758 to 965 MPa, the relative fracture stress ratio was high at 0.80 or more, and excellent hydrogen embrittlement resistance was obtained.

[0153] On the other hand, in test numbers 59 and 60, the average cooling rate CR1 from 640 to 500°C was less than 30°C / min. Therefore, Fn1 was 8.00 or less. As a result, the relative fracture stress ratio was less than 0.80, and sufficient hydrogen embrittlement resistance was not obtained.

[0154] In test numbers 61 and 62, the average cooling rate CR1 at 640 to 500°C exceeded 100°C / min. Therefore, Fn1 was 8.00 or less. As a result, the relative fracture stress ratio was less than 0.80, and sufficient hydrogen embrittlement resistance was not obtained.

[0155] In test number 63, the C content was too high, so the relative fracture stress ratio was less than 0.80, and sufficient hydrogen embrittlement resistance was not obtained.

[0156] In test number 64, the C content was too low, so the yield strength was less than 758 MPa.

[0157] In test number 65, the Si content was too high, so the relative fracture stress ratio was less than 0.80, and sufficient hydrogen embrittlement resistance was not obtained.

[0158] In test number 66, the Si content was too low, so the relative fracture stress ratio was less than 0.80, and sufficient hydrogen embrittlement resistance was not obtained.

[0159] In test number 67, the Mn content was too high, so the relative fracture stress ratio was less than 0.80, and sufficient hydrogen embrittlement resistance was not obtained.

[0160] In test number 68, the S content was too high, so the relative fracture stress ratio was less than 0.80, and sufficient hydrogen embrittlement resistance was not obtained.

[0161] In test number 69, the Cr content was too high, so the relative fracture stress ratio was less than 0.80, and sufficient hydrogen embrittlement resistance was not obtained.

[0162] In test number 70, the Cr content was too low, so the relative fracture stress ratio was less than 0.80, and sufficient hydrogen embrittlement resistance was not obtained.

[0163] In test number 71, the Mo content was too low, so the relative fracture stress ratio was less than 0.80, and sufficient hydrogen embrittlement resistance was not obtained.

[0164] The embodiments of the present disclosure have been described above. However, the above-described embodiments are merely examples for implementing the present disclosure. Therefore, the present disclosure is not limited to the above-described embodiments, and can be implemented by appropriately modifying the above-described embodiments without departing from the spirit of the present disclosure.

Claims

1. A steel material, The chemical composition, in mass%, is C: 0.15-0.50%, Si: 0.05-0.50%, Mn: 0.01-1.00%, P: 0.0300% or less, S: 0.0100% or less, Cr: 0.20-1.20%, Mo: 0.40-1.50%, Ti: 0.0010-0.0300%, V: 0.01-0.50%, Nb: 0.0050 to 0.1000%, Al: 0.0050-0.1000%, B: 0.0001 to 0.0050%, N: 0.0100% or less, O: 0.0050% or less, W: 0-2.00%, Co: 0 to 0.20%, Cu: 0 to 0.50%, Ni: 0 to 0.50%, Sn: 0 to 0.50%, Mg: 0 to 0.0100%, Ca: 0-0.0100%, Rare earth elements: 0 to 0.0100%, and The balance is Fe and impurities, The total area ratio of martensite and bainite is 90% or more, The yield strength is less than 758 to 965 MPa; The grain size of the prior austenite grains is 15.0 μm or less, One end point of a 10 nm line segment SL that is centered on the grain boundary of a prior austenite grain and perpendicular to the grain boundary is defined as E1 and the other end point is defined as E2. At each measurement point arranged at a pitch of 0.2 nm from the end point E1 to the end point E2 of the line segment SL, the Mo content (mass%) and the Mn content (mass%) at each measurement point on the line segment SL are determined by elemental analysis using energy dispersive X-ray spectroscopy; In the line segment SL, The measurement point on the line segment SL where the Mo content is maximum is defined as the Mo peak measurement point, A region having a width of 2.0 nm and centered on the Mo peak measurement point is defined as a Mo segregation region, A region between the end point E1 and the Mo segregation region is defined as a first Mo intragranular region, A region between the end point E2 and the Mo segregation region is defined as a second Mo intragranular region, The arithmetic average value of the Mo content at all the measurement points in the first Mo grain region is defined as [Mo] BM1 (mass%), The arithmetic average value of the Mo content at all the measurement points in the second Mo grain region is defined as [Mo] BM2 (mass%), In the line segment SL, The measurement point on the line segment SL where the Mn content is maximum is defined as the Mn peak measurement point, A region having a width of 2.0 nm and centered on the Mn peak measurement point is defined as a Mn segregation region, A region between the end point E1 and the Mn segregation region is defined as a first Mn intragranular region, A region between the end point E2 and the Mn segregation region is defined as a second Mn intragranular region, The arithmetic average value of the Mn content at all the measurement points in the first Mn grain region is defined as [Mn] BM1 (mass%), The arithmetic average value of the Mn content at all the measurement points in the second Mn intragranular region is defined as [Mn] BM2 (mass%), The amount of Mo segregation [Mo] defined by the formula (1) SEG and the amount of Mn segregation [Mn] defined by the formula (2). SEG and satisfy the formula (3). Steel material. [Mo] SEG = {(the sum of the Mo contents at all the measurement points on the line segment SL × 0.2) - [Mo] BM1 × (distance between the end point E1 and the Mo peak measurement point) - [Mo] BM2 × (the distance between the end point E2 and the Mo peak measurement point)) / 0.8 + ([Mo] BM1 + [Mo] BM2 ) / 2 (1) [Mn] SEG = {(total Mn content at all the measurement points on the line segment SL × 0.2) - [Mn] BM1 × (distance between the end point E1 and the Mn peak measurement point)−[Mn] BM2 × (the distance between the end point E2 and the Mn peak measurement point)) / 0.8 + ([Mn] BM1 + [Mn] BM2 ) / 2 (2) [Mo] SEG -[Mn] SEG >8.00 (3)

2. The steel material according to claim 1, The chemical composition is W: 0.01-2.00%, Co: 0.01-0.20%, Cu: 0.01 to 0.50%, Ni: 0.01 to 0.50%, Sn: 0.01-0.50%, Mg: 0.0001 to 0.0100%, Ca: 0.0001 to 0.0100%, and Rare earth elements: 0.0001 to 0.0100%, Contains one or more elements selected from the group consisting of Steel material.

3. The steel material according to claim 1 or 2, The steel material is any one of a steel pipe for oil wells, a steel pipe for line pipes, and a steel pipe for high-pressure hydrogen storage tanks. Steel material.

4. The steel material according to claim 1 or 2, The steel material is any one of a seamless steel pipe for oil wells, a seamless steel pipe for line pipes, and a seamless steel pipe for high-pressure hydrogen storage tanks. Steel material.

Citation Information

Patent Citations

  • Low alloy steel for high pressure hydrogen gas environment, and vessel for high pressure hydrogen

    JP2009074122A

  • High-strength seamless steel tube for oil well with excellent resistance to sulfide stress cracking, and method for producing the same

    JP2011246798A

  • High-strength seamless steel pipe with excellent resistance to sulfide stress cracking for oil well and method for producing the same

    JP2015038247A

Cited By

  • steel

    JP7908623B1

  • Steel material

    WO2026094452A1