Manufacturing method of r-t-b system permanent magnet

The use of a lubricant with specific polar and hydrocarbon groups during the pulverization process addresses the challenge of achieving high crystal orientation and low residual carbon in R-T-B permanent magnets, resulting in improved magnetic properties.

JP2024137076APending Publication Date: 2024-10-07TDK CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023048444
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

Existing methods for manufacturing R-T-B permanent magnets struggle to achieve both high crystal orientation and low residual carbon content, leading to a decrease in residual magnetic flux density.

Method used

A manufacturing method involving the use of a lubricant containing a specific compound represented by general formula (1), which includes polar functional groups and hydrocarbon groups, is applied during the pulverization process to enhance crystal orientation and reduce residual carbon.

Benefits of technology

The method results in R-T-B permanent magnets with improved crystal orientation and reduced residual carbon content, enhancing residual magnetic flux density and coercive force.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137076000007
    Figure 2024137076000007
  • Figure 2024137076000008
    Figure 2024137076000008
  • Figure 2024137076000009
    Figure 2024137076000009
Patent Text Reader

Abstract

To provide a manufacturing method of an R-T-B system permanent magnet, capable of obtaining the R-T-B system permanent magnet of which a crystal orientation level is high, and a remaining carbon amount is low.SOLUTION: A manufacturing method of an R-T-B system permanent magnet, containing a rare earth element R, and transition metal elements T and B, contains: a preparation step of preparing a raw material alloy for the R-T-B system permanent magnet; a smash step of obtaining an alloy powder by smashing the raw material alloy; a molding step obtaining a molding body by molding the alloy powder; and a sintering step of sintering the molding body. In the smash step, a lubricant is added to at least one of the raw material alloy and the alloy powder, and the lubricant contains a chemical compound represented by the following formula (1) (however, excluding isobutyl amid). In formula (1), R1 is a functional group with a polarity, R2 is a hydrogen atom, or a hydrocarbon group including a benzene ring, an alkyl group, an alkenyl group, or an alkynyl group, R3 and R4 independently represents the hydrocarbon group having the benzene ring, the alkyl group, and the alkenyl group, or the alkynyl group.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for producing an RTB based permanent magnet. [Background technology]

[0002] RTB permanent magnets, which contain rare earth elements R, transition metal elements T, and boron B, are widely used as magnets with excellent magnetic properties, and demand for them is increasing along with the miniaturization and high performance of motors for automobiles and industrial machines. In the production of RTB permanent magnets, raw alloys are pulverized to obtain alloy powder. The alloy powder is then pressed in a magnetic field to form a shape, and heat treated to produce a permanent magnet.

[0003] In the grinding process, a sufficient amount of lubricant is added. This is expected to improve grindability. The addition of a lubricant also reduces the kinetic friction between particles when the alloy powder is molded. As a result, the resulting permanent magnet is expected to have improved crystal orientation and a higher residual magnetic flux density (Br). On the other hand, the addition of a lubricant increases the amount of residual carbon, which tends to reduce the coercive force (Hcj) of the permanent magnet.

[0004] Patent Document 1 discloses a method for producing an RTB sintered magnet in which a lubricant containing two or more types of fatty acid amides whose total carbon number (n+1) is 16 or less, with the fatty acid amides whose total carbon number (n+1) is 16 or less accounting for 80 wt% or more, is used to reduce the amount of additive, thereby reducing the amount of residual carbon in the sintered body. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2007-197826 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, the remanence of the magnetic flux density of the sintered magnets obtained by the manufacturing method described in Patent Document 1 decreases significantly as the amount of residual carbon decreases. In other words, the manufacturing method described in Patent Document 1 was unable to achieve both a high degree of crystal orientation and a low amount of residual carbon.

[0007] The present disclosure provides a method for producing an RTB permanent magnet that can produce an RTB permanent magnet with a high degree of crystal orientation and a low amount of residual carbon. [Means for solving the problem]

[0008] [1] A method for producing an RTB type permanent magnet containing a rare earth element R, a transition metal element T and B, comprising the steps of: a preparation step of preparing a raw material alloy for an RTB permanent magnet; a crushing step of crushing the raw alloy to obtain an alloy powder; a molding step of molding the alloy powder to obtain a compact; a sintering step of sintering the compact; Equipped with In the pulverization step, a lubricant is added to at least one of the raw alloy and the alloy powder; The lubricant comprises a compound represented by the following general formula (1) (excluding isobutyramide): [ka] [In formula (1), R 1 represents a polar functional group, and R 2 represents a hydrogen atom, a hydrocarbon group having a benzene ring, an alkyl group, an alkenyl group, or an alkynyl group; R 3 and R 4 each independently represents a hydrocarbon group having a benzene ring, an alkyl group, an alkenyl group, or an alkynyl group. [2] R in the above general formula (1) 1 is an amide group, a carboxyl group, a hydroxyl group, an amino group or an acetyl group. [3] The method for producing an RTB permanent magnet according to [1] or [2], wherein the compound represented by the general formula (1) has 5 or more carbon atoms. [4] R in the above general formula (1) 2 The method for producing an RTB permanent magnet according to any one of [1] to [3], wherein is a hydrocarbon group having a benzene ring, an alkyl group, an alkenyl group, or an alkynyl group. [5] The method for producing an RTB permanent magnet according to any one of [1] to [4], wherein the amount of the lubricant added in the crushing step is 0.1 mass % or more based on the total amount of the raw material alloy. [6] The method for producing an RTB permanent magnet according to any one of [1] to [5], wherein the compound represented by general formula (1) is at least one selected from the group consisting of pivalamide, isobutyric acid, 2-ethylbutanamide, 2,2-diethylbutanamide, pivalic acid, 2-ethyl-1-butanol, 2,2-diethyl-1-butanol, 2-ethyl-1-butanamine, 2,2-diethyl-1-butanamine, 3-methyl-2-butanone, 3,3-dimethyl-2-butanone, 2,2-dimethyl-4-pentenamide, and 2-hexyl-4-pentynoic acid. [7] The pulverization step includes a first pulverization step of pulverizing the raw alloy, and a second pulverization step of further pulverizing the alloy powder obtained by the first pulverization step; The method for producing an RTB permanent magnet according to any one of [1] to [6], wherein in the second pulverization step, the lubricant is added to the alloy powder. Effect of the Invention

[0009] According to the present disclosure, there is provided a method for producing an RTB permanent magnet that can produce an RTB permanent magnet with a high degree of crystal orientation and a low amount of residual carbon. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic perspective view of an apparatus for measuring the dynamic friction coefficient of alloy powder. [Diagram 2]2(a), (b), and (c) in FIG. 2 are schematic diagrams showing the procedure for measuring the dynamic friction coefficient using the measuring device shown in FIG. 1, and are cross-sectional views of the measuring device and alloy powder. [Diagram 3] FIG. 3 shows the time profiles of shear force and lower normal stress of the alloy powder measured by the measuring device shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] A preferred embodiment of the present disclosure will be described in detail below. However, the present disclosure is not limited to the following embodiment. In the following, all "permanent magnets" refer to "RTB permanent magnets."

[0012] (Manufacturing method of permanent magnets) The method for producing a permanent magnet according to this embodiment includes a preparation step of preparing a raw alloy for an RTB permanent magnet, a crushing step of crushing the raw alloy to obtain an alloy powder, a molding step of molding the alloy powder to obtain a compact, and a sintering step of sintering the compact. In the crushing step, a lubricant is added to at least one of the raw alloy and the alloy powder. The method for producing a permanent magnet may further include an orientation step of applying a magnetic field to the alloy powder to orient the alloy powder. Each step will be described in detail below.

[0013] [Preparation process] A raw material alloy for a permanent magnet is produced from a metal (metal raw material) containing each element constituting a permanent magnet. The raw material alloy may be produced by a strip casting method, a book mold method, or a centrifugal casting method. The raw material metal may be, for example, a rare earth element (metal element), pure iron, ferroboron, or an alloy containing these. These raw material metals are weighed so as to approximately match the composition of the desired permanent magnet. One type of raw material alloy may be used. Multiple types of raw material alloys may be used. The raw material alloy before the pulverization process may be a number of particles. For example, the raw material alloy may be flaky particles. The raw material alloy may be an ingot.

[0014] The raw material alloy for the permanent magnet contains a rare earth element R, a transition metal element T, and boron B. The rare earth element R may be at least one selected from the group consisting of Sc, Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu. The permanent magnet may contain only Fe as the transition metal element T. The permanent magnet may contain both Fe and Co as the transition metal element T. The chemical composition of the raw material alloy may be adjusted according to the chemical composition of the main phase and grain boundary phase of the permanent magnet to be finally obtained. In other words, the raw material alloy may be prepared by weighing and mixing each starting material containing the above elements according to the composition of the target permanent magnet. The permanent magnet may be, for example, a neodymium magnet. The main phase of the permanent magnet may be, for example, Nd 2 Fe 14 The grain boundary phase may be, for example, a phase (R-rich phase) having a higher content of rare earth element R than the main phase. The grain boundary phase may include a transition metal-rich phase, a B-rich phase, an oxide phase, or a carbide phase.

[0015] [Crushing process] In the pulverization step, the lubricant is added to at least one of the raw alloy and the alloy powder. Addition of the lubricant means that the lubricant is physically combined with the raw alloy or the alloy powder. The composition of the raw alloy itself does not need to be changed by the addition of the lubricant. In other words, the composition of the raw alloy itself does not need to be changed in the pulverization step.

[0016] The pulverization step may include a first pulverization step for pulverizing the raw alloy, and a second pulverization step for further pulverizing the alloy powder obtained by the first pulverization step. The first pulverization step may be referred to as a coarse pulverization step. The second pulverization step may be referred to as a fine pulverization step. By carrying out the first pulverization step and the second pulverization step, it is easy to obtain an alloy powder having a small average particle size. However, the pulverization step does not have to be divided into the first pulverization step and the second pulverization step. In other words, the alloy powder may be produced from the raw alloy by only one pulverization step. In the following, a pulverization step including the first pulverization step and the second pulverization step will be described. The raw alloy pulverized in the first pulverization step is referred to as alloy powder. The lubricant may be added to at least one of the raw alloy and the alloy powder. The lubricant may be added multiple times. Each of the following steps may be carried out in a non-oxidizing atmosphere in which the oxygen concentration is 50 ppm or less.

[0017] The lubricant contains a compound represented by the following general formula (1) (excluding isobutylamide). The compound represented by the following general formula (1) (hereinafter also referred to as "compound (1)") reduces the dynamic friction coefficient between the alloy powders. Compound (1) will be described in detail below.

[0018] [ka] [In formula (1), R 1 represents a polar functional group, and R 2 represents a hydrogen atom, a hydrocarbon group having a benzene ring, an alkyl group, an alkenyl group, or an alkynyl group; R 3 and R 4 each independently represents a hydrocarbon group having a benzene ring, an alkyl group, an alkenyl group, or an alkynyl group.

[0019] R 1 For example, an amide group (-CONR 11 2 group), carboxyl group (-COOH group), hydroxyl group (-OH group), amino group (-NR 11 2group), acetyl group (-COR 11 group), phosphate group (-R 11 OPO(OH)(OR 11 ) groups). R in amide group, amino group, acetyl group, and phosphate group 11 may be a hydrogen atom or a hydrocarbon group. The hydrocarbon group may be a linear or branched alkyl group. The number of carbon atoms in the hydrocarbon group and the alkyl group may be 1 to 12, 1 to 8, or 1 to 2. A plurality of R 11 may be the same or different.

[0020] R 1 is preferably an amide group, a carboxyl group, a hydroxyl group, an amino group or an acetyl group, and more preferably an amide group, since this further improves the degree of crystal orientation of the permanent magnet while further reducing the amount of residual carbon.

[0021] R 2 R is preferably a hydrocarbon group having a benzene ring, an alkyl group, an alkenyl group, or an alkynyl group, since it further improves the crystal orientation of the permanent magnet while further reducing the amount of residual carbon. 2 is R 1When is an amide group, it is preferable that the amide group is a hydrocarbon group having a benzene ring, an alkyl group, an alkenyl group, or an alkynyl group, since it further improves the degree of crystal orientation of the permanent magnet while further reducing the amount of residual carbon. Examples of the hydrocarbon group having a benzene ring include an aryl group and an aralkyl group. The number of carbon atoms of the hydrocarbon group having a benzene ring may be 6 to 20. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, and an octyl group. The number of carbon atoms of the alkyl group may be, for example, 1 to 20. Examples of the alkenyl group include an ethenyl group, a propenyl group, a butenyl group, a pentenyl group, a hexenyl group, and an octenyl group. The number of carbon atoms of the alkenyl group may be 2 to 20. Examples of the alkynyl group include an ethynyl group, a propynyl group, a butynyl group, a pentynyl group, a hexynyl group, and an octynyl group. The number of carbon atoms of the alkynyl group may be 2 to 20. The alkyl, alkenyl and alkynyl groups may be straight or branched chain.

[0022] R 3 and R 4 The hydrocarbon group, alkyl group, alkenyl group and alkynyl group having a benzene ring are each represented by R 2 Examples of the aryl group include the hydrocarbon group having a benzene ring, the alkyl group, the alkenyl group and the alkynyl group.

[0023] Specific examples of compound (1) include pivalamide, isobutyric acid, 2-ethylbutanamide, 2,2-diethylbutanamide, pivalic acid, 2-ethyl-1-butanol, 2,2-diethyl-1-butanol, 2-ethyl-1-butanamine, 2,2-diethyl-1-butanamine, 3-methyl-2-butanone, 3,3-dimethyl-2-butanone, 2,2-dimethyl-4-pentenamide, 2-hexyl-4-pentynoic acid, 2-methylbutanamide, valpromide, 2,2-dipropylpentanamide, α-methylcyclohexaneacetamide, 2-ethylbutanoic acid, 2,2-ethylbutanoic acid, 3-ethyl-2-pentanone, 2-hydrogen isopropyl phosphate, and diisopropyl hydrogen phosphate. Compound (1) may be used alone or in combination of two or more.

[0024] The number of carbon atoms in compound (1) is preferably 5 or more, since this further improves the degree of crystal orientation of the permanent magnet while further reducing the amount of residual carbon. From the same viewpoint, the number of carbon atoms in compound (1) is preferably 20 or less, and more preferably 15 or less.

[0025] The content of compound (1) in the lubricant may be 60 mass % or more, 70 mass % or more, 80 mass % or more, 90 mass % or more, or 100 mass % based on the total amount of the lubricant.

[0026] The amount of lubricant added in the grinding step is preferably 0.1% by mass or more and 1.0% by mass or less, and more preferably 0.1% by mass or more and 0.3% by mass or less, based on the total amount of the raw alloy, in order to further improve the crystal orientation of the permanent magnet while further reducing the amount of residual carbon. The absolute value of the mass of the raw alloy may be expressed as m (kg), the total absolute value of the mass of the lubricant may be expressed as a (kg), and the total amount of the lubricant added relative to the total amount of the raw alloy may be expressed as 100a / m (mass%).

[0027] The means for pulverizing the raw alloy in the first pulverization step may be at least one means selected from the group consisting of hydrogen absorption pulverization, a disk mill, a jaw crusher, a Braun mill, and a stamp mill. In the first pulverization step, the raw alloy may be pulverized by a plurality of kinds of pulverization means. The average particle size of the alloy powder obtained in the first pulverization step may be, for example, 10 μm or more and 1000 μm or less. The alloy powder obtained in the first pulverization step may be called a coarse powder.

[0028] In the first pulverization step, the raw alloy is preferably pulverized by hydrogen absorption pulverization. In the hydrogen absorption pulverization, hydrogen is absorbed into the raw alloy. After the hydrogen is absorbed, the raw alloy is heated to release hydrogen from the raw alloy. The raw alloy is pulverized by the release of hydrogen from the raw alloy. The hydrogen absorption pulverization makes it easy to reduce the average particle size of the raw alloy to a target value at a high pulverization speed. In order to release hydrogen from the raw alloy, the raw alloy in which hydrogen has been absorbed may be heated at 200°C or higher or 350°C or higher. The heating time may be 30 minutes or more or 60 minutes or more. In order to release hydrogen from the raw alloy, the raw alloy in which hydrogen has been absorbed may be heated in a vacuum or in a flow of argon (Ar) gas.

[0029] When a raw alloy to which a lubricant has been added is pulverized by hydrogen absorption pulverization, the lubricant is likely to be reduced due to hydrodecomposition of the lubricant. Due to the reduction in the lubricant in the first pulverization step, the pulverization speeds in the first pulverization step and the second pulverization step are likely to decrease. Therefore, when a raw alloy to which a lubricant has been added is pulverized by hydrogen absorption pulverization in the first pulverization step, it is preferable to add a lubricant to the alloy powder in the second pulverization step in order to prevent hydrodecomposition of the lubricant in the first pulverization step.

[0030] The means for pulverizing the alloy powder in the second pulverization step may be at least one means selected from the group consisting of a jet mill (airflow pulverizer), a ball mill, a bead mill, a vibration mill, and a wet attritor. In the second pulverization step, the alloy powder may be pulverized by a plurality of kinds of pulverization means. The average particle size of the alloy powder pulverized in the second pulverization step may be, for example, 0.5 μm or more and 4 μm or less. The alloy powder pulverized in the second pulverization step may be called a fine powder.

[0031] In the second pulverization step, the alloy powder is preferably pulverized by a jet mill. In the jet mill, high-pressure inert gas is sprayed from a nozzle at high speed, and the alloy powder is accelerated by the inert gas. The alloy powder is further pulverized by collisions between the accelerated alloy powder particles and between the alloy powder and the inner wall of the container. The average particle size of the alloy powder is easily reduced to a target value by the jet mill at a high pulverization speed. The inert gas may be, for example, Ar.

[0032] In the second pulverization step, the alloy powder to which the lubricant has been added may be pulverized. For example, in the second pulverization step, the alloy powder and the lubricant may be mixed by a cone mixer (Nauta mixer), a V-type mixer, or a stirring blade mixer, and the mixture may be pulverized by a jet mill.

[0033] The alloy powder may have a dynamic friction coefficient of 0.43 or less. The method for measuring the dynamic friction coefficient will be described later.

[0034] [Molding process and orientation process] In the compacting step, a mold is used to produce a compact from the alloy powder. The compacting step and the orientation step may be performed simultaneously. When the compacting step and the orientation step are performed simultaneously, the alloy powder is pressed by the mold while a magnetic field is applied to the alloy powder in the mold. As a result, a compact containing the alloy powder oriented along the magnetic field is obtained. The alloy powder contains compound (1), which reduces friction between the alloy particles constituting the alloy powder. As a result, the density of the compact is increased, the alloy powder is easily oriented along the magnetic field, and the residual magnetic flux density of the permanent magnet is increased.

[0035] The pressure exerted by the die on the alloy powder may be 30 MPa to 300 MPa. The strength of the magnetic field applied to the alloy powder in the die may be 796 kA / m to 1990 kA / m. The magnetic field may be a static magnetic field or a pulsed magnetic field. The mixture of the alloy powder and the lubricant may be compacted.

[0036] After the molding step, an orientation step may be performed. In the molding step performed before the orientation step, a mold is used to form a compact from the alloy powder. The mold may be made of at least one material selected from the group consisting of resin, metal, and ceramic. In the molding step performed before the orientation step, the pressure applied by the mold to the alloy powder may be 0.049 MPa or more and 20 MPa or less. In the orientation step performed after the molding step, a magnetic field is applied to the compact held in the mold. That is, by applying a magnetic field to the compact in the mold, the alloy powder constituting the compact is oriented along the magnetic field. The magnetic field may be a static magnetic field or a pulse magnetic field. The strength of the magnetic field applied to the compact in the mold may be, for example, 796 kA / m or more and 5173 kA / m or less. In the orientation step, the compact in the mold may also be pressurized. In the orientation step, the pressure applied by the mold to the compact may be 0.049 MPa or more and 20 MPa or less.

[0037] After the compacting and orienting steps, the compact may be demagnetized.

[0038] [Sintering process] In the sintering step, the compact is sintered in a sintering furnace to obtain a sintered body. The atmosphere in the sintering furnace may be a vacuum or an inert gas. The inert gas may be, for example, Ar. The conditions of the sintering step may be appropriately set according to the composition of the target permanent magnet, the crushing method of the raw alloy, the average particle size of the alloy powder, and the like. The sintering temperature may be, for example, 900°C or higher and 1200°C or lower. The sintering time may be 1 hour or higher and 20 hours or lower. Some of the compound (1) contained in the compact is volatilized at high temperatures, and the rest is reduced by hydrogen in the compact and leaves the compact. As a result, the amount of residual carbon in the obtained sintered body is reduced.

[0039] In the aging treatment step, the sintered body may be further heated. The magnetic properties of the sintered body are improved by the aging treatment step. The atmosphere in the aging treatment step may be a vacuum or an inert gas. The inert gas may be, for example, Ar. In the aging treatment step, the sintered body may be heated at about 600°C for 1 to 3 hours. A multi-stage aging treatment step may be performed. For example, in the first aging treatment, the sintered body may be heated at 700 to 900°C for 1 to 3 hours, and in the second aging treatment following the first aging treatment, the sintered body may be heated at 500 to 700°C for 1 to 3 hours. The aging treatment step may be performed consecutively to the sintering step.

[0040] The sintered body may be quenched by a cooling step following the aging treatment step. The sintered body may be quenched in an inert gas. The inert gas may be, for example, Ar. The cooling rate of the sintered body may be, for example, 5° C. / min or more and 100° C. / min or less.

[0041] In the processing step, the size and shape of the sintered body may be adjusted by cutting, polishing, etc. The sintered body obtained by the above method may not contain a heavy rare earth element. The sintered body may already contain a heavy rare earth element. Regardless of the presence or absence of a heavy rare earth element in the sintered body, the following diffusion step may be carried out. However, the diffusion step is not essential.

[0042] When manufacturing a permanent magnet containing a heavy rare earth element, a diffusion step may be carried out. The heavy rare earth element may be, for example, at least one of Tb and Dy. In the diffusion step, the heavy rare earth element or a compound thereof may be attached to the surface of the sintered body, and then the sintered body may be heated. For example, the heavy rare earth element may be attached to the surface of the sintered body. The sintered body may be heated in steam containing the heavy rare earth element. In the diffusion step, the heavy rare earth element diffuses from the surface of the sintered body to the inside, and the heavy rare earth element further diffuses to the surfaces of the main phase particles via the grain boundaries.

[0043] A paint containing a heavy rare earth element may be applied to the surface of the sintered body. The composition of the paint is not limited as long as the paint contains a heavy rare earth element. The paint may be, for example, a simple substance of a heavy rare earth element, an alloy containing a heavy rare earth element, or a compound containing a heavy rare earth element. The compound containing a heavy rare earth element may be a hydride, a fluoride, or an oxide. The solvent (dispersion medium) contained in the paint may be a solvent other than water. For example, the solvent may be an organic solvent such as an alcohol, an aldehyde, or a ketone. The concentration of the heavy rare earth element in the paint is not limited.

[0044] The diffusion treatment temperature in the diffusion step may be 800°C or higher and 950°C or lower. The diffusion treatment time may be 1 hour or higher and 50 hours or lower. By setting the diffusion treatment temperature and diffusion treatment time within the above ranges, it is easy to control the concentration distribution of the heavy rare earth element, and the manufacturing cost of the permanent magnet is reduced. The diffusion step may also serve as the above-mentioned aging treatment step.

[0045] After the diffusion step, the permanent magnet may be further subjected to a heat treatment. The heat treatment temperature after the diffusion step may be 450°C or higher and 600°C or lower. The heat treatment time may be 1 hour or higher and 10 hours or lower. The heat treatment after the diffusion step tends to improve the magnetic properties (especially the coercive force) of the final permanent magnet.

[0046] After the diffusion step, the size and shape of the sintered body may be adjusted by cutting, polishing, or the like.

[0047] A passive layer may be formed on the surface of the sintered body by oxidation or chemical treatment of the surface of the sintered body. The surface of the sintered body may be covered with a resin film. The formation of the passive layer or resin film further improves the corrosion resistance of the permanent magnet.

[0048] A permanent magnet is manufactured by the above method. The shape of the permanent magnet is not limited. For example, the shape of the permanent magnet may be a rectangular parallelepiped, a cube, a rectangle (plate), a polygonal prism, an arc segment, a sector, an annular sector, a sphere, a disk, a cylinder, a tube, a ring, or a capsule. The cross-sectional shape of the permanent magnet may be, for example, a polygon, an arc (circular chord), a bow, an arch, a C-shape, or a circle. The permanent magnet may be applied to a motor, a generator, an actuator, or the like. For example, the permanent magnet is used in various fields such as hybrid cars, electric cars, hard disk drives, magnetic resonance imaging devices (MRI), smartphones, digital cameras, flat-screen TVs, scanners, air conditioners, heat pumps, refrigerators, vacuum cleaners, washing and drying machines, elevators, and wind power generators.

[0049] [Mechanism of action] According to the method for producing an RTB permanent magnet according to this embodiment, the lubricant added in the pulverization step contains compound (1), so that a permanent magnet with a high degree of crystal orientation and a low amount of residual carbon can be obtained. The inventors of the present invention speculate that the reason for this effect is as follows. That is, compound (1) contains R 1 The polar functional group present in R enhances the adsorption force to the alloy powder. 3 and R 4 The alkyl group or the like having as a functional group enhances the repulsive force between the compounds (1) due to its bulkiness. Therefore, the compound (1) adsorbed to the alloy powder promotes the repulsion between the alloy powders, thereby reducing the coefficient of kinetic friction. This increases the fluidity of the alloy powder when it is compacted. As a result, the degree of crystal orientation of the obtained permanent magnet is improved. In addition, the residual magnetic flux density of the obtained permanent magnet is improved.

[0050] In addition, compound (1) is R 3 and R 4 The alkyl group or the like having as R enhances the repulsive force between the compound (1) and the adsorbed alloy powder due to its bulkiness. 2 ~R 4Compared with compounds in which two of the carbon atoms are hydrogen atoms, these are more likely to volatilize during the sintering process. As a result, the amount of residual carbon in the resulting permanent magnet is low. In addition, the coercive force of the resulting permanent magnet is improved.

[0051] (Method of measuring the dynamic friction coefficient) A method for measuring the kinetic friction coefficient of the alloy powder will be described in detail below. FIG. 1 shows a measuring device 10 for measuring the kinetic friction coefficient. The measuring device 10 includes a cell 8, a substrate 12, a lower pressure gauge 5, a punch 6, a vertical servo cylinder 4 (servomotor), and a horizontal servo cylinder 14. The cell 8 is a cylinder, and is placed on the surface of the substrate 12 so that the end face of the cell 8 is in contact with the surface of the substrate 12. The cell 8 is not fixed to the surface of the substrate 12, and is separable from the substrate 12. A recess communicating with the space inside the cell 8 is formed on the surface of the substrate 12. At least a part of the punch 6 is a cylinder, and is fitted inside the cell 8. The punch 6 is placed between the cell 8 and the vertical servo cylinder 4, and the end face of the punch 6 is pressed by the tip of the vertical servo cylinder 4, so that the punch 6 is inserted inside the cell 8. The vertical servo cylinder 4 freely controls the position and moving speed of the punch 6 in the vertical direction (perpendicular direction). The vertical direction can be rephrased as a direction perpendicular to the surface of the substrate 12 on which the cell 8 is placed. The horizontal servo cylinder 14 pushes the side surface of the substrate 12 to move the substrate 12 in the horizontal direction. The horizontal servo cylinder 14 freely controls the horizontal position and moving speed of the substrate 12. The horizontal direction can be rephrased as the direction parallel to the surface of the substrate 12 on which the cells 8 are installed. The lower pressure gauge 5 is installed under the substrate 12.

[0052] As shown in (a) of Fig. 2, the alloy powder 3 is placed inside the cell 8 and in the recess of the substrate 12. A small gap is provided between the cell 8 and the substrate 12 so that the alloy powder 3 does not leak out of the cell 8. Next, as shown in (b) of Fig. 2, a punch 6 is inserted into the cell 8, and the end face of the punch 6 compresses the alloy powder 3. The lower normal stress F that the alloy powder 3 in the cell 8 exerts on the bottom surface is LN is measured by the lower pressure gauge 5.

[0053] Lower normal stress F LN When the pressure reaches the set value Fa, the positions of the punch 6 and the cells 8 are fixed while the alloy powder 3 in the cells 8 is pressed by the punch 6, and the volume of the alloy powder 3 (the volume of the area surrounded by the punch 6, the cells 8, and the recesses of the substrate 12) is maintained constant. At this time, the individual metal particles constituting the alloy powder 3 move and rotate to rearrange themselves so that the stress applied to the entire alloy powder 3 is minimized.

[0054] As shown in (c) of FIG. 2, the side of the substrate 12 is pushed by the tip of the horizontal servo cylinder 14, thereby moving the substrate 12 in the horizontal direction at a constant shear rate. As a result, a shear force f acts on the alloy powder 3 in the cell 8. The shear force f is equal to the force f that the horizontal servo cylinder 14 exerts on the side of the substrate 12. Therefore, the shear force f is measured by a load cell installed at the tip of the horizontal servo cylinder 14. The shear force f and the lower normal stress F LN The change over time of each is shown in Figure 3. The vertical axis on the right side of Figure 3 is the shear force f (unit: N). The vertical axis on the left side of Figure 3 is the lower normal stress F LN (Unit: N) The horizontal axis of FIG. 3 is time T (unit: seconds).

[0055] As the alloy powder 3 is sheared, the metal particles located near the shear plane move and rotate to rearrange. When the rearrangement of the metal particles progresses sufficiently and the shear plane reaches a steady state, the shear force f reaches a maximum value fc. On the other hand, the lower normal stress F LN decreases as the rearrangement of the metal particles on the shear plane progresses. When the shear force f reaches its maximum value fc, the lower normal stress F LN leads to Fd. That is, Fd is the lower normal stress F when the shear force f is at its maximum value fc. LN It is defined as:

[0056] The above shear force f(fc) and the lower normal stress F LN Based on the measurement method of (Fd), the dynamic friction coefficient μ of the alloy powder 3 is defined by the following formula 1A. μ = fc / Fd (1A) EXAMPLES

[0057] The present disclosure will be described in more detail below with reference to examples, but the present disclosure is not limited to these examples.

[0058] Example 1 The flake-shaped raw alloy was produced by strip casting. The raw alloy consisted of Nd, Co, Cu, Zr, Al, B and Fe. The contents of each element in the raw alloy were as follows: Nd content: 29% by mass Co content: 0.5 mass% Cu content: 0.1% by mass Zr content: 0.2 mass% Al content: 0.2 mass% B content: 0.97% by mass Fe content: balance

[0059] In the first pulverization step, hydrogen was absorbed into the raw alloy at room temperature for one hour. After hydrogen absorption, the raw alloy was heated at 500°C for one hour to dehydrogenate the raw alloy. The raw alloy was pulverized by the above hydrogen absorption pulverization to obtain alloy powder. The average particle size of the alloy powder obtained by the first pulverization step was 500 μm.

[0060] In the second milling step following the first milling step, a lubricant was added to the alloy powder. The lubricants in Example 1 are shown in Table 1 below. The carbon number of the lubricant and the R 1 The name and structure of R 2 , R 3 and R 4 The number of hydrocarbon groups among these is shown in Table 1. The amount of lubricant added based on the total amount of the alloy powder is shown in Table 1 below.

[0061] In the second milling step, the lubricant and the alloy powder were mixed at room temperature for 10 minutes. The lubricant and the alloy powder were mixed in a V-type mixer. The alloy powder mixed with the lubricant was further milled in a jet mill. The alloy powder was milled in the jet mill until the average particle size of the alloy powder was 3 μm. The air flow of the jet mill was N 2 The oxygen concentration in the airstream was below 50 ppm.

[0062] The above first and second pulverization steps produced the alloy powder for permanent magnets of Example 1. The dynamic friction coefficient of the alloy powder of Example 1 was measured by the method described below.

[0063] [Measurement of dynamic friction coefficient] The dynamic friction coefficient μ of the alloy powder of Example 1 was measured by the above-mentioned method. The measurement device used was a powder bed shear force measuring device NS-S500 manufactured by Nano Seeds Co., Ltd. The outline of the measurement device is as shown in Figures 1, 2 and 3. The inner diameter φ of the cylindrical cell 8 used in the measurement was 15 mm. In the measurement, a gap of 0.3 mm was provided between the end face of the cell 8 and the surface of the substrate 12. In the measurement, 10 g of the alloy powder 3 was filled into the inside of the cell 8 and the recess of the substrate 12. The pressing speed of the punch 6 was maintained at 0.2 mm / sec. The relaxation time of the stress between the particles was 200 seconds. The shear speed in the measurement of the dynamic friction coefficient μ was maintained at 10 μm / sec. As a result, the lower normal stress F LN The set value Fa is changed to 40N and 60N, and the maximum value of the shear force f (when the set value is 40N: fc1, when the set value is 60N: fc2) and the lower normal stress F when the shear force f is the maximum value are calculated. LN (When the set value was 40N: Fd1, when the set value was 60N: Fd2) were measured. With the lower normal stress on the horizontal axis and the shear force on the vertical axis, (Fd1, fc1) and (Fd2, fc2) were plotted, and a linear approximation curve was drawn using the least squares method, and the slope of the curve was taken as the dynamic friction coefficient μ.

[0064] The alloy powder was stirred by a V-type mixer. After stirring, the alloy powder was pressed with a die while a magnetic field was applied to the alloy powder in the die, to produce a compact. In other words, the compacting and orientation processes were carried out simultaneously. The pressure that the die exerted on the alloy powder was 1.4t / cm. 2 The strength of the magnetic field applied to the alloy powder in the die was 1193 kA / m.

[0065] In the sintering process, the compact was heated in Ar gas to obtain a sintered body. In the sintering process, the compact was heated at 1030°C for 4 hours. Following the sintering process, the sintered body was quenched.

[0066] After quenching, the sintered body was subjected to a first aging treatment and a second aging treatment following the first aging treatment. In both the first aging treatment and the second aging treatment, the sintered body was heated in Ar gas. In the first aging treatment, the sintered body was heated at 900°C for 1 hour. In the second aging treatment, the sintered body was heated at 530°C for 1 hour.

[0067] By the above method, the permanent magnet of Example 1 was produced.

[0068] [Measurements of coercivity, residual magnetic flux density, residual magnetic polarization and saturation magnetic polarization] The coercive force (Hcj) and residual magnetic flux density (Br) of the permanent magnet of Example 1 were measured at room temperature (23° C.) using a BH tracer.

[0069] [Method for measuring crystal orientation] The degree of crystal orientation of the permanent magnet of Example 1 was measured by the Lotgering method. Specifically, first, the magnetic pole surface of the permanent magnet was mirror-polished. Then, the mirror-polished surface was subjected to X-ray diffraction measurement. The intensity of the diffraction peak obtained by the measurement was substituted into the following formula 1 to calculate the degree of orientation (unit: %). I(00l) in the following formula 1 is the diffraction intensity of the reflected X-ray on the (00l) surface of the permanent magnet. I(hkl) in the following formula 1 is the diffraction intensity of the reflected X-ray on the (hkl) surface of the permanent magnet. In order to calculate the degree of crystal orientation that corresponds to the actual situation, it is preferable to perform vector correction on the diffraction peak, so in this example, the degree of crystal orientation was calculated after performing vector correction. The results are shown in Table 1.

number

[0070] [Measurement of residual carbon] The residual carbon amount of the permanent magnet of Example 1 was measured by infrared absorption method. The results are shown in Table 1.

[0071] (Examples 2 to 16, Comparative Examples 1 to 6) In the first pulverization step of each Example and Comparative Example, the lubricant shown in Table 1 below was added to the alloy powder. The amount of lubricant added for each Example and Comparative Example is shown in Table 1 below. Except for these details, the alloy powder and permanent magnet of each Example and Comparative Example were produced in the same manner as in Example 1. The dynamic friction coefficient of the alloy powder of each Example and Comparative Example was measured in the same manner as in Example 1. The coercive force, residual magnetic flux density and residual carbon content of the permanent magnet of each Example and Comparative Example were measured in the same manner as in Example 1. The crystal orientation of the permanent magnet of each Example and Comparative Example was calculated in the same manner as in Example 1. The results are shown in Table 1.

[0072] [Table 1] [Explanation of symbols]

[0073] 3...Alloy powder.

Claims

1. A method for producing an R-T-B system permanent magnet containing a rare earth element R, transition metal elements T and B, comprising the steps of: A preparation step of preparing a raw material alloy for an R-T-B based permanent magnet; a crushing step of crushing the raw alloy to obtain an alloy powder; a molding step of molding the alloy powder to obtain a compact; a sintering step of sintering the compact; Equipped with In the pulverization step, a lubricant is added to at least one of the raw alloy and the alloy powder; The lubricant contains a compound represented by the following general formula (1) (excluding isobutylamide): [Case 1] [In formula (1), R 1 represents a polar functional group, R 2 represents a hydrogen atom, a hydrocarbon group having a benzene ring, an alkyl group, an alkenyl group, or an alkynyl group; R 3 and R 4 each independently represents a hydrocarbon group having a benzene ring, an alkyl group, an alkenyl group, or an alkynyl group.

2. R in the general formula (1) 1 The method for producing an R-T-B system permanent magnet according to claim 1, wherein is an amide group, a carboxyl group, a hydroxyl group, an amino group or an acetyl group.

3. 3. The method for producing an R-T-B system permanent magnet according to claim 1, wherein the compound represented by the general formula (1) has 5 or more carbon atoms.

4. R in the general formula (1) 2 The method for producing an R-T-B system permanent magnet according to claim 1 or 2, wherein is a hydrocarbon group having a benzene ring, an alkyl group, an alkenyl group, or an alkynyl group.

5. 3. The method for producing an R-T-B system permanent magnet according to claim 1, wherein the amount of the lubricant added in the pulverizing step is 0.1 mass % or more based on the total amount of the raw material alloy.

6. 3. The method for producing an R-T-B system permanent magnet according to claim 1 or 2, wherein the compound represented by general formula (1) is at least one selected from the group consisting of pivalamide, isobutyric acid, 2-ethylbutanamide, 2,2-diethylbutanamide, pivalic acid, 2-ethyl-1-butanol, 2,2-diethyl-1-butanol, 2-ethyl-1-butanamine, 2,2-diethyl-1-butanamine, 3-methyl-2-butanone, 3,3-dimethyl-2-butanone, 2,2-dimethyl-4-pentenamide, and 2-hexyl-4-pentynoic acid.

7. the pulverization step includes a first pulverization step of pulverizing the raw alloy, and a second pulverization step of further pulverizing the alloy powder obtained by the first pulverization step, 3. The method for producing an RTB system permanent magnet according to claim 1, wherein the lubricant is added to the alloy powder in the second pulverization step.

Citation Information

Patent Citations

  • Manufacture of rare earth element-iron-boron sintered permanent magnet and molding material

    JP1996316017A

  • Method of manufacturing rare earth sintered magnet and method of pulverizing raw alloy powder for sintered magnet

    JP2006041501A

  • Method of manufacturing rare earth magnet

    JP2019176012A

  • Method for production of alloy powder for rare earth permanent magnet, and method for production of rare earth permanent magnet

    JP2020167208A

  • Lubricant for compacting, composition for compacting and method for producing r-t-b based sintered magnet

    JP2007197826A