Electrochemical capacitor
By employing a three-dimensional graphene structure and specific ionic liquid compositions, the energy density of electrochemical capacitors is enhanced through redox reactions, addressing the limitations of existing capacitors with low energy density.
Patent Information
- Application Number
- JP2023048465
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-07
AI Technical Summary
Existing electrochemical capacitors have low energy density and limited applications despite their capability for rapid charging and discharging.
The use of graphene sheets stacked in a three-dimensional manner via carbon nanotubes, combined with an ionic liquid electrolyte containing specific atomic ratios of elements like fluorine and boron, facilitates high voltage operation leading to increased energy density through redox reactions.
This configuration results in an electrochemical capacitor with significantly higher capacity and energy density, leveraging redox reactions and optimized graphene structure for enhanced ion adsorption and capacity development.
Smart Images

Figure 2024137092000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrochemical capacitor. [Background technology]
[0002] With the expanding demand for ICT applications such as personal computers and smartphones, in-vehicle applications, and power storage, there is a demand for electrochemical devices, such as capacitors, with higher capacities.
[0003] Graphene has a theoretical specific surface area of approximately 2600 m 2 / g and is conductive, making it a promising electrode material for capacitors.
[0004] Patent Document 1 proposes a graphene sheet film in which two or more graphene sheets are stacked in parallel via carbon nanotubes, and the graphene sheet stacks are electrically and mechanically connected to each other in a three-dimensional manner via the carbon nanotubes. A capacity of 290.6 F / g has been reported when this film is used as an electrode. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Re-tabled publication No. 2012 / 073998 Summary of the Invention [Problem to be solved by the invention]
[0006] The capacitor described in Patent Document 1 is capable of rapid charging and discharging and has a high output density compared to lithium ion batteries, but its energy density is still low and its applications are limited. In order to expand the applications of electrochemical capacitors, there is a demand for a further increase in energy density.
[0007] The higher the operating voltage of a capacitor, the higher the energy density that can be obtained, so combinations of electrolytes and electrode materials that can operate at high voltages are being explored. [Means for solving the problem]
[0008] In view of the above, one aspect of the present invention provides a method for producing an electrochemical cell comprising the steps of: providing a first electrode including a first active material; a second electrode including a second active material; and an electrolytic solution, the electrolytic solution including an ionic liquid; and determining whether or not a surface of the first electrode is quantitatively analyzed by X-ray photon spectroscopy (XPS) based on a relative sensitivity coefficient, the ratio of the number of atoms of element F derived from the ionic liquid to element C is R. F The present invention relates to an electrochemical capacitor in which the ratio of the capacitance to the capacitance of the capacitor is 10% or more. Effect of the Invention
[0009] According to the present disclosure, an electrochemical capacitor with high energy density can be realized. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a partially cutaway perspective view of an electrochemical capacitor according to an embodiment of the present disclosure. [Diagram 2] 1 is a graph showing the change in single-pole capacitance C1 with respect to the applied voltage V1 for the capacitors of Example 1 and Comparative Example 1. [Diagram 3] 1 shows F 1s spectra in XPS analysis of the negative electrode surfaces of the capacitors of Example 1 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, the term "electrochemical capacitor" includes capacitors having various electricity storage mechanisms, and means an electricity storage device that at least partially has an electricity storage mechanism, such as an electric double layer capacitor or a lithium ion capacitor. The electricity storage device or electrochemical capacitor includes a pair of capacitor electrodes and an electrolyte. The electrodes contain an active material.
[0012] An active material exhibits a capacity by, for example, doping and dedoping ions. The doping of an active material with ions is a concept including the adsorption of ions to the active material, the occlusion of ions by the active material, and chemical interaction between the active material and ions. The dedoping of an active material with ions is a concept including the desorption of ions from the active material, the release of ions from the active material, and the release of chemical interaction between the active material and ions. However, here, the doping of an active material with ions mainly refers to the adsorption of ions to the active material, and the dedoping of an active material with ions mainly refers to the desorption of ions from the active material. When ions are adsorbed to the active material, an electric double layer is formed, and a capacity is exhibited. That is, although the electrode for a capacitor mainly means a polarizable electrode, it may be an electrode that has the properties of a polarizable electrode and also contributes to the capacity through the Faraday reaction.
[0013] An electrochemical capacitor according to an embodiment of the present disclosure includes a first electrode including a first active material, a second electrode including a second active material, and an electrolyte. A separator is usually interposed between the first electrode and the second electrode. The electrolyte includes an ionic liquid. Hereinafter, the electrochemical capacitor according to the present disclosure may be simply referred to as a "capacitor."
[0014] In one embodiment of the electrochemical capacitor according to the present disclosure, the cations or anions constituting the ionic liquid are adsorbed to the first active material or the second active material, forming an electric double layer and exhibiting capacitance. In addition, when a high voltage equal to or higher than a threshold is applied, a reduction reaction of the cations constituting the ionic liquid or an oxidation reaction of the anions occurs, and the capacitance is also exhibited by the charge transfer between the active material and the cations or anions due to the oxidation-reduction reaction.
[0015] A voltage of 4.0 V or more can be applied between the first electrode and the second electrode. In this case, capacitance is generated by an oxidation-reduction reaction, and a capacitor with high capacity and high energy density can be realized.
[0016] Either the first electrode or the second electrode is a positive electrode of the capacitor, and the other is a negative electrode. In the following description, the first electrode is a negative electrode, and the second electrode is a positive electrode. That is, it is assumed that a lower potential is applied to the first electrode than to the second electrode. The first electrode and the second electrode may be the same electrode or different electrodes.
[0017] When the surface of the first electrode was quantitatively analyzed using X-ray photon spectroscopy (XPS) based on the relative sensitivity coefficient, the atomic ratio R of element F derived from the ionic liquid to element C was F is 10% or more. In this case, the capacitor can achieve high capacity and high energy density. The reason for this is believed to be as follows, based on the current knowledge of the inventors. However, the present invention is not limited to this.
[0018] The cations or anions contained in the ionic liquid can be reduced or oxidized by application of a high voltage, and reaction products of the reduction or oxidation reaction can be generated in the electrolyte solution. These reaction products can be adsorbed and deposited on the surface of the positive or negative electrode.
[0019] For example, at the negative electrode, the cations of the ionic liquid may be reduced to generate a reduction product. The reduction product may further react with the anions of the ionic liquid to generate a by-product. The reduction product may be adsorbed onto the negative electrode surface together with the anions, and / or an adsorption state may be formed in which the by-products with the anions are adsorbed onto the negative electrode surface. As a result, when the surface of the negative electrode is analyzed by a surface analysis method such as XPS, elements derived from the ionic liquid are observed. For example, when the cations or anions of the ionic liquid contain F (fluorine), F is measured by XPS analysis. When the cations or anions of the ionic liquid contain B (boron), B is measured by XPS analysis.
[0020] The atomic ratio R of F to C on the negative electrode surface calculated using the XPS method F When the ratio R is 10% or more, the capacity due to the redox reaction is significantly increased, and a capacitor with high capacity and high energy density can be realized. FThe ratio R may be 14% or more. F The ratio R may be 14% or more. F may be 30% or less, or may be 14% or more and 30% or less.
[0021] The adsorption state formed on the surface of the negative electrode may contain B. In that case, the atomic ratio R of B to C calculated by the XPS method is B may be 1% or more.
[0022] Specifically, for example, when 1-ethyl-3-methylimidazolium tetrafluoroborate (EMIBF4) shown in the following formula (1) is used as the ionic liquid, during charging at a voltage of 4.0 V or higher, the 1-ethyl-3-methylimidazolium cation (EMI + ) is reduced at the negative electrode, and EMI radicals can be generated by the reaction shown in formula (2) below.
[0023] Formula (1): [ka]
[0024] Formula (2): [ka]
[0025] On the other hand, during discharge, the reaction in the reverse order to that of formula (2) proceeds, and the EMI radical releases one electron to produce EMI + A reaction (oxidation reaction) that returns to the cation can proceed. Therefore, in addition to the capacitance that is generated by the adsorption of cations or anions, the capacitor also generates additional capacitance through the redox reaction, which is thought to result in a significantly high capacitance.
[0026] The radical that is the reaction product of formula (2) is the anion BF4 - The reaction products can reach the negative electrode surface and form adsorbates. - The ratio RF or ratio R B When the adsorbate contains F or B such that satisfies the above relational expression, high capacity and high energy density can be achieved.
[0027] X-ray photoelectron spectroscopy (XPS) is a method to analyze the composition and chemical bonding state of elements that compose a sample surface by irradiating the sample surface with X-rays and measuring the kinetic energy of photoelectrons emitted from the sample surface due to the ionization of atoms. The area of each peak in the XPS spectrum is proportional to the number of atoms of the corresponding element. However, since the ionization cross section for X-rays differs for each element and also depends on the settings of the instrument, it is not possible to determine the composition ratio between elements by comparing the areas of peaks corresponding to different elements. Therefore, measurements are performed on a sample with a known composition, and the relationship between the peak intensity and the number of atoms of each element is obtained in advance. The composition of the elements that compose the sample surface can be quantified with high accuracy by using the relative sensitivity factors (RSF).
[0028] An example of the conditions for XPS measurement is shown below. The C1s spectrum of graphite (248.5 eV) can be used to calibrate the binding energy. Measurement equipment: ULVAC-PHI ESCA5600 X-ray source used: Al-Kα ray, Mg-Kα ray Analysis area: 800μmΦ Quantitative conversion method: Quantitative value is calculated from the ratio of the peak area of each element multiplied by the relative sensitivity coefficient.
[0029] The first electrode and the second electrode may contain a fluorine-containing compound such as polyvinylidene fluoride (PVdF) or PTFE as a binder. In this case, in an XPS measurement of the electrode surface, in addition to the peak of the C element derived from the ionic liquid, a peak derived from the C-F bond derived from the binder contained in the electrode appears. The peak derived from the C-F bond derived from the binder appears at a position of binding energy different from that of the peak derived from the ionic liquid, so it is possible to determine whether or not the F present on the surface is derived from the ionic liquid based on the peak position. The ratio R F In calculating the ratio R, the number of F atoms originating from the binder is subtracted from the number of F atoms in the XPS spectrum to obtain the number of F atoms originating from the ionic liquid, and this is divided by the number of C atoms in the XPS spectrum to obtain the ratio R F Request.
[0030] Ratio R F (and the ratio R B ) depends on the types of anions and cations that make up the ionic liquid, the content (concentration) of the ionic liquid in the electrolyte, and also on the surface condition of the first electrode (first active material) on which the adsorbates accumulate. To obtain high capacity and high energy density, the ratio R F (and the ratio R B It is important to select an active material that satisfies the above relationship.
[0031] The first active material and / or the second active material may be a carbon material having a layered structure. That is, the carbon material includes a stacked structure of layers (commonly called graphene layers or graphene sheets) in which carbon atoms are bonded to form a hexagonal network in a plane. The carbon material may include graphene. The graphene may be reduced graphene oxide or graphene having a three-dimensional structure.
[0032] Graphene is a carbon material whose smallest unit is a graphene sheet with a thickness of one carbon atom, and is usually made up of multiple graphene sheets stacked together. A graphene sheet is an aggregate or molecule made of sp2 bonded carbon with a thickness of one carbon atom, and has a honeycomb lattice structure that spreads out in a sheet shape.
[0033] Of the first active material and the second active material, at least the first active material may contain a carbon material having a layered structure.
[0034] The carbon material having a layered structure can be used as either the positive electrode active material or the negative electrode active material. However, in one embodiment, an electrode containing the carbon material as a first active material is used as a first electrode and as a negative electrode, so that the ratio R F and the ratio R B becomes larger, and the capacity increases dramatically.
[0035] The carbon material preferably contains reduced graphene oxide, which can be obtained by reducing graphene oxide.
[0036] Graphene oxide (hereinafter, also referred to as "GO") has a structure in which oxygen-containing groups are bonded to graphene sheets. The oxygen-containing groups are considered to be bonded mainly to the edge surfaces of the graphene sheet laminate. The oxygen-containing groups are hydrophilic groups such as hydroxyl groups, carbonyl groups, carboxyl groups, and epoxy groups. Graphene oxide (GO) is generally dispersible in polar solvents such as water. Graphene oxide (GO) is generally insulating because it contains sp3 bonded carbon.
[0037] By reducing graphene oxide (GO), oxygen-containing groups are removed to obtain reduced graphene oxide (hereinafter also referred to as "rGO"). Reduced graphene oxide (rGO) is a graphene analogue that has electrical conductivity. Reduced graphene oxide may contain oxygen-containing groups that were not removed in the reduction process. Due to the presence of functional groups such as oxygen atoms in the graphene layer, the crystal structure of the carbon material deviates from the ideal graphene or graphite structure, and the carbon atoms in the graphene layer have a mixture of sp2 bonds and sp3 bonds. As a result, the graphene layers are easily spread apart by application of a high voltage, and cations and anions are easily inserted between the graphene layers, which makes it easier to expand the area where the electric double layer is formed. Therefore, by using reduced graphene oxide as an active material, the capacitance of a capacitor can be dramatically increased.
[0038] In addition, the presence of functional groups such as oxygen atoms can cause distortion in the planar structure of graphene, leading to disorder in the layer structure (or disorder in the interlayer distance), or the graphene layers can be bent or folded to form a three-dimensional structure. This increases the effective surface area available for adsorbing cations and anions, allowing for high capacity. In addition, adsorption is easily formed by reaction with ionic liquids, and R F and the ratio R B It is easy to control to a large value.
[0039] General graphene usually has a flat sheet shape. On the other hand, the graphene used in the capacitor of the present embodiment may be a graphene sheet laminate having various shapes, not a flat sheet shape, but having a disordered layer structure (or a disordered interlayer distance) (or having a three-dimensional structure). By using graphene having a three-dimensional structure (graphene sheet laminate) as an active material, the capacitance of the capacitor is dramatically increased.
[0040] The three-dimensional structure mainly means a microscopic three-dimensional structure (i.e., a microstructure) formed in a flake-shaped particle. By having a three-dimensional structure, the overlapping of graphene sheets is significantly suppressed compared to flat sheet-like graphene, and the large surface area of graphene can be effectively utilized. A plurality of protrusions or a plurality of depressions (i.e., folds) are formed on the main surface (mainly the 002 plane (basal plane)) of the graphene sheet laminate having a three-dimensional structure. By such a three-dimensional structure, the distance between the graphene sheets can be appropriately controlled, and the overlapping of the graphene sheets can be effectively reduced.
[0041] The three-dimensional structure may include a folded structure in which a graphene sheet having folds is folded. A laminate may be formed by folding one graphene sheet through the folded portion in a direction intersecting the plane of the sheet. The radius of curvature of the folded portion in the folded structure is, for example, in the range of 10 to 1000 nm. The interval between the folds is, for example, in the range of 10 to 100 nm.
[0042] The bent structure in the three-dimensional structure includes, for example, a crimped structure or a folded structure in the sheet portion between the bent portions. In this case, each graphene sheet laminate may have a microporous structure. This improves the diffusion of ions near the surface of the laminate. The presence of the crimped structure or the folded structure (i.e., the pleated portion) can be confirmed by an electron microscope (SEM, TEM, etc.) photograph of the graphene sheet laminate.
[0043] The crimped structure may be, for example, a structure having a plurality of randomly formed fold-like raised portions and recessed portions. The folded structure is a structure having a folded portion in which one graphene sheet laminate is partially folded a plurality of times, and is included in the category of the crimped structure. The height of the raised portion or the depth of the recessed portion formed in the folded portion may be greater than the thickness of the carbon portion of the graphene sheet laminate having that structure, and may be at least twice the thickness of the carbon portion.
[0044] Graphene having such a three-dimensional structure may have a peak in the pore diameter range of 2 nm to 4 nm in the logarithmic differential pore distribution, and may further have a distribution in which the volume increases quadratically with increasing pore diameter in the pore diameter range of 4 nm to 50 nm. The total pore volume of mesopores in the pore diameter range of 2 nm to 50 nm is, for example, 0.20 cm 3 The total mesopore volume can be 0.20 cm 3 / g~0.5cm 3 / g range, 0.25 cm 3 / g~0.4cm 3 / g range, or 0.25 cm 3 / g~0.35cm 3 / g. The total volume of pores with diameters of 4 nm to 50 nm may be, for example, 15 times or more the total volume of pores with diameters of 2 nm to 4 nm. The specific surface area and pore size distribution of graphene can be measured using a BELSORP 28SA device available from BEL Japan Co., Ltd. The Dollimore Heal method (DH method), which is calculated based on the capillary condensation theory (Kelvin's equation), is used as the analytical theory for mesopores.
[0045] Graphene having such a three-dimensional structure can provide a capacitor electrode having a maximum peak in the logarithmic differential pore volume distribution measured by a mercury porosimeter in the range of 0.3 μm or more and 6 μm or less. The three-dimensional structure significantly reduces overlapping of graphene sheets compared to flat sheet-like graphene, and the surface area of graphene can be effectively utilized for ion adsorption. The three-dimensional structure in which multiple protrusions or multiple depressions are formed on the basal surface appropriately controls the distance between graphene sheets, effectively reducing overlapping of graphene sheets. Therefore, the active sites of the active material can be increased without suppressing the movement (diffusion) of ions, and high capacity can be achieved.
[0046] The average number of layers in the graphene sheet stack is, for example, 10 or less, and may be 5 or less. It is preferable that the graphene sheet stack is as close to the minimum unit of a graphene sheet (i.e., a single-layer sheet) having a thickness of one carbon atom.
[0047] The average number of layers is estimated from the interplanar distance (d002) calculated from the diffraction peak assigned to the 002 plane (basal plane) of the X-ray diffraction profile (for example, Abstracts of the 2015 Autumn Meeting of the Physical Society of Japan, p. 1014). Alternatively, it may be an estimated value obtained from an electron microscope (SEM, etc.) photograph of graphene. For example, the number of layers of graphene sheets can be estimated from the scale of the SEM photograph of graphene and the interplanar distance of the 002 plane (basal plane) of the graphene sheet. For example, 20 arbitrary graphene sheet laminates are selected, the number of layers of each is estimated, the 5th largest value and the 5th smallest value are omitted, and the average value of the 10 middle values is taken as the average number of layers.
[0048] The interlayer distance between graphene sheets (i.e., the distance between basal planes) may vary randomly. A random variation in the interlayer distance means that the graphene sheet laminate has low crystallinity. The greater the disorder in the laminate's stacking structure, the more significant the variation in the interlayer distance becomes.
[0049] The X-ray diffraction profile of graphene usually has a diffraction peak assigned to the 002 plane. The greater the overlap between graphene sheets and the higher the crystallinity of graphene, the sharper the diffraction peak becomes.
[0050] On the other hand, when graphene has a three-dimensional structure, the diffraction peak becomes broad and can be separated into multiple peaks. A halo pattern attributed to an amorphous phase may be observed on the higher angle side of the diffraction peak.
[0051] The interplanar distance d002 of the 002 planes of graphene calculated from the X-ray diffraction profile is 0.330 nm or more and 0.360 nm or less. d002 is calculated by waveform separation of the diffraction peaks observed in the region around 2θ=26.38°, calculating d002 for each component, and calculating the average. The distance d002 of the 002 planes of graphene is preferably 0.340 nm (3.40 Å) or more, more preferably 0.360 nm (3.60 Å) or more, and even more preferably 0.370 nm (3.70 Å) or more.
[0052] The electrolyte solution contains an ionic liquid. As the ionic liquid, a salt compound that exists in a liquid state at room temperature (25°C) and normal pressure (atmospheric pressure) can be preferably used. Cations constituting the salt compound include imidazolium-based cations, pyrrolidinium-based cations, pyridinium-based cations, piperidinium-based cations, ammonium-based cations, and phosphonium-based cations. Examples of anions include halide ions (Cl - , Br - etc.), tetrafluoroborate ion (BF4 - ), hexafluorophosphate ion (PF6 - ), bis(fluorosulfonyl)imide ion ((FSO2)2N - ), bis(trifluoromethylsulfonyl)imide ion ((CF3SO2)2N - ) etc.
[0053] Among these cations, the use of cations having heteroaromatic rings can realize extremely high capacity. The reason for this is currently being elucidated, but possible reasons include that the delocalized π orbital derived from the aromatic ring easily bonds with the π orbital of graphene to form a specifically stable adsorption state, and that the radical compound generated by the reduction reaction can exist stably by adopting a resonance structure and easily forms a stable adsorption state with the π orbital of graphene.
[0054] The anion is tetrafluoroborate ion (BF4 -When the anion contains a hexafluorophosphate ion (PF6 - ) is also included in BF4 - Similarly, in the case where the anion contains BF4, the F1s spectrum of the negative electrode surface may have a peak in the binding energy range of 686 to 692 eV. By analyzing the B1s spectrum and the P1s spectrum, it is possible to determine whether the anion is BF4 - or PF6 - It is possible to determine whether the file contains either (or both).
[0055] The cation having a heteroaromatic ring may be an imidazolium cation. The imidazolium cation may be a cation in which some of the hydrogen atoms in the imidazole skeleton are substituted with an alkyl group or the like.
[0056] Examples of imidazolium cations include cations with heteroaromatic rings, such as 1-C 1-3 Alkyl-3-C 1-3 It may be an alkylimidazolium cation, more specifically, it may include a 1-ethyl-3-methylimidazolium cation. At least 80 mol % of the cation is 1-C 1-3 Alkyl-3-C 1-3 It may be an alkylimidazolium cation or a 1-ethyl-3-methylimidazolium cation.
[0057] In order to adjust the viscosity of the electrolyte and improve the output characteristics, a solvent may be mixed with the ionic liquid and used as the electrolyte. As the solvent, any solvent (non-aqueous solvent) that is conventionally used as an electrolyte for a capacitor can be used as long as it is uniformly mixed with the ionic liquid.
[0058] The non-aqueous solvent is preferably a high boiling point solvent, for example, lactones such as γ-butyrolactone, carbonates such as propylene carbonate, polyhydric alcohols such as ethylene glycol and propylene glycol, cyclic sulfones such as sulfolane, amides such as N-methylacetamide, N,N-dimethylformamide, and N-methyl-2-pyrrolidone, esters such as methyl acetate, ethers such as 1,4-dioxane, ketones such as methyl ethyl ketone, and formaldehyde can be used.
[0059] When the electrolytic solution contains a solvent other than the ionic liquid, the proportion of the ionic liquid in the entire electrolytic solution may be 75 mass % or more, or 80 mass % or more, or may even be 90 mass % or more.
[0060] The graphene having the above structure is used as an active material to manufacture a first electrode and / or a second electrode as an electrode for a capacitor. The electrode for a capacitor may contain a binder. The binder plays a role of assisting the bonding of graphene to graphene and the bonding of graphene to a current collector when forming the graphene having the above three-dimensional structure into an electrode layer.
[0061] Hereinafter, an example of a method for producing graphene according to an embodiment of the present disclosure and a method for producing a capacitor electrode using the graphene produced thereby will be described.
[0062] <Graphene manufacturing method> (i) Dispersion preparation process First, an aqueous dispersion containing graphene oxide is prepared. The aqueous dispersion may contain a dispersant such as carboxymethyl cellulose (CMC) in addition to graphene oxide and water. Graphene oxide can be produced by exfoliating graphite in a single layer or multiple layers, for example, via oxidation of graphite.
[0063] The oxidation of graphite can be carried out, for example, using an oxidizing agent in water. Examples of the oxidizing agent that can be used include sulfuric acid, potassium permanganate, chromic acid, sodium dichromate, sodium nitrate, peroxide, persulfate, and organic peracid. A water-soluble solvent may be added to the water. Examples of the water-soluble solvent include alcohols, ketones such as acetone, and ethers such as dioxane and tetrahydrofuran. An aqueous dispersion of graphene oxide is produced by the oxidation reaction in water.
[0064] The oxygen content of the graphene oxide may be, for example, 10 to 60 mass %, may be 20 to 50 mass %, or may be 30 to 50 mass %.
[0065] (ii) Reduction step Next, reduced graphene oxide is produced by reducing the graphene oxide in an aqueous dispersion containing the graphene oxide (first reduction step). A preferred reduction method is, for example, hydrothermal treatment. For example, the aqueous dispersion may be sealed in an autoclave and subjected to hydrothermal treatment to produce a gel-like product. The temperature of the hydrothermal treatment may be, for example, 150°C or higher, preferably 170°C or higher and 200°C or lower.
[0066] Although it is possible to obtain reduced graphene oxide having a three-dimensional structure by hydrothermal treatment alone, the gel product may be contacted with a reducing agent to further promote the reduction (second reduction step). Examples of the reducing agent include metal hydrides, borohydrides, boranes, hydrazines or hydrazides, ascorbic acids, thioglycolic acids, cysteines, sulfurous acids, thiosulfates, and dithionous acids. For example, the gel product may be immersed in an aqueous solution containing a water-soluble reducing agent such as sodium ascorbate. The temperature of the aqueous solution may be, for example, 20 to 110°C, 40 to 100°C, or 50 to 100°C. The amount of the reducing agent used may be appropriately adjusted depending on the type of reducing agent, the oxygen content of the first carbon raw material (graphene oxide), the amount of the gel product, and the like.
[0067] The gel product may then be freeze-dried. Freeze-drying can provide a dry gel (xerogel) in which the three-dimensional structure of graphene is highly maintained. Freeze-drying may be performed, for example, at -50°C to 0°C, preferably -50°C to -20°C, under reduced pressure of 100 Pa or less, and further 1 Pa or less.
[0068] Next, the dried gel is thermally reduced in a non-oxidizing atmosphere to eliminate the remaining functional groups (third reduction step).
[0069] The non-oxidizing atmosphere may be a reduced pressure atmosphere (for example, 0.1 MPa or less (preferably 10 Pa or less)), a reducing atmosphere (for example, a hydrogen atmosphere of 0.01 MPa or less), an inert gas atmosphere (for example, an atmosphere with N2, Ar, Ne, He, or the like flowing therethrough), or the like.
[0070] The heating temperature in the non-oxidizing atmosphere is 700°C or more, and may be 800°C or more, 900°C or more, 1000°C or more, or 1200°C or more. However, there is a limit to the reduction of the oxygen content of reduced graphene oxide, and in consideration of the production cost, the heating temperature in the non-oxidizing atmosphere may be 1800°C or less, 1400°C or less, or 1200°C or less. When the temperature range is specified, these upper and lower limits may be combined arbitrarily. The temperature range may be, for example, 1000°C to 1800°C.
[0071] The heating time in the non-oxidizing atmosphere is appropriately selected depending on the heating conditions and the amount of carbon to be treated, but may be, for example, about 0.1 to 5 hours.
[0072] The oxygen content of the dried gel after thermal reduction is less than 5% by mass, may be 4% by mass or less, may be 3% by mass or less, preferably less than 2.6% by mass, may be 2% by mass or less, or may be 1.5% by mass or less. When the oxygen content is reduced to less than 5% by mass, the amount of reactants generated by the oxidation-reduction reaction between the oxygen-containing group and the electrolyte solution components is reduced. Such reactants block the pores of the electrode, reducing the diffusibility of the ions and reducing the number of ion adsorption sites. Therefore, the less the reactants, the higher the capacity can be achieved without reducing the diffusibility of the ions and reducing the number of ion adsorption sites.
[0073] The dried gel after thermal reduction is pulverized to obtain reduced graphene oxide powder (rGO powder). By the above method, graphene having a three-dimensional structure (reduced graphene oxide) is produced. Using the produced graphene, a capacitor electrode can be produced, for example, by the following method.
[0074] <Method for manufacturing capacitor electrodes> (iii) Electrode process For example, rGO powder is dispersed in a dispersion medium such as water together with a binder to prepare a slurry. The obtained slurry is applied to a conductive substrate (current collector), and the coating is dried to form an electrode layer supported on the current collector, thereby obtaining a capacitor electrode. The electrode layer may then be rolled.
[0075] Examples of binders that can be used include fluororesins such as polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), and vinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP); and water-soluble resins such as carboxymethyl cellulose (CMC), polyethylene oxide (PEO), polyethylene glycol (PEG), polyacrylonitrile (PAN), polymethyl methacrylate (PMMA), polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), polyacrylic acid (PAA), and polyvinyl acetate.
[0076] The electrode layer may contain other active materials such as activated carbon in addition to the graphene. The electrode layer may also contain carbon particles such as carbon fibers such as carbon nanotubes (CNTs), carbon black, and graphite. However, from the viewpoint of achieving both high capacity and high reliability, it is preferable that graphene constitutes 50 mass % or more of the electrode layer, and more preferably 65 mass % or more.
[0077] The current collector may be a metal foil, a metal porous body, or the like. The current collector may be made of aluminum, copper, nickel, iron, stainless steel, platinum, or the like. An alloy containing these metals as a main component may also be used. The metal foil may be a plain foil, or may be a foil that has been roughened by etching or the like, or a foil that has been subjected to plasma treatment. The metal porous body may have, for example, a three-dimensional mesh structure.
[0078] The mass per unit area of the metal porous body is, for example, 500 g / m 2 Less than 150g / m 2 The porosity of the metal porous body may be, for example, 80 volume % to 98 volume %, and may be 90 volume % to 98 volume %.
[0079] The average pore size of the pores in the metal porous body may be, for example, 50 μm or more and 1000 μm or less, or may be 400 μm or more and 900 μm or less, or 450 μm or more and 850 μm or less.
[0080] <Capacitor> Next, an example of an electrochemical capacitor having the above-mentioned capacitor electrodes as a first electrode and a second electrode will be described. FIG 1 is a partially cutaway perspective view of a capacitor 10.
[0081] The illustrated capacitor 10 includes a wound type capacitor element 1. The capacitor element 1 is formed by winding a first electrode 2 and a second electrode 3, each of which is in the form of a sheet, with a separator 4 interposed therebetween. The first electrode 2 and the second electrode 3 each have a first current collector and a second current collector made of metal, and a first electrode layer and a second electrode layer carried on the surface thereof, respectively, and exhibit capacitance by adsorbing and desorbing ions. For example, aluminum foil is used for the first and second current collectors. The surface of the current collector may be roughened by a method such as etching. Lead wires 5a and 5b are connected to the first electrode 2 and the second electrode 3, respectively, as lead members. The capacitor element 1 is housed in a cylindrical exterior case 6 together with an electrolyte (not shown). The material of the exterior case 6 may be, for example, a metal such as aluminum, stainless steel, copper, iron, or brass. The opening of the exterior case 6 is sealed by a sealing member 7. The lead wires 5a and 5b are led out to the outside so as to pass through the sealing member 7. The sealing member 7 is made of, for example, a rubber material such as butyl rubber.
[0082] The electrode layer includes an active material as an essential component, and may include a binder, a conductive assistant, and the like as optional components. The active material includes, for example, graphene having the characteristics already described. The electrode layer is obtained, for example, by applying a slurry obtained by kneading the active material, a binder (for example, carboxymethyl cellulose (CMC)), and the like together with water in a kneader to the surface of a current collector, drying the coating, and rolling it.
[0083] The separator preferably contains cellulose or a derivative thereof. Cellulose is stable against both acids and alkalis, and is stable even in an environment where a high voltage is applied. In addition, it has a large tensile strength, and has sufficient strength even when the first electrode and the second electrode are wound to form a wound electrode group. The separator may be in the form of, for example, a microporous membrane, a woven fabric, or a nonwoven fabric. The thickness of the separator is, for example, 8 to 50 μm, preferably 12 to 35 μm, and more preferably 14 to 35 μm or 16 to 35 μm.
[0084] In the above embodiment, a wound type capacitor has been described, but the scope of application of the present invention is not limited to the above, and the present invention may also be applied to capacitors of other structures, such as laminated type or coin type capacitors.
[0085] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples.
[0086] <Example 1> (1) Preparation of electrodes for capacitors Graphite was oxidized in water using potassium permanganate as an oxidizing agent to obtain graphene oxide. An aqueous dispersion containing 1% by mass of graphene oxide was subjected to hydrothermal treatment at 180° C. for 6 hours to obtain a gel-like product (first reduction step).
[0087] Subsequently, the gel product was immersed in an aqueous solution of sodium ascorbate (sodium ascorbate concentration: 1.0 mol / L) as a reducing agent, heated to 100° C., and held for 2 hours to sufficiently reduce the carbon (second reduction step).
[0088] The gel product was then freeze-dried at -20°C under reduced pressure of 100 Pa to obtain a xerogel. The xerogel was then heat-treated at 1200°C for 2 hours under nitrogen flow (third reduction step). The xerogel after the heat treatment was pulverized to obtain a reduced graphene oxide powder.
[0089] A slurry was prepared by dispersing 100 parts by mass of reduced graphene oxide powder and 10 parts by mass of CMC as a binder in an appropriate amount of water. The obtained slurry was applied to a current collector made of Al foil with a thickness of 30 μm, and the coating was vacuum dried at 110° C. and rolled to form an electrode layer, thereby obtaining an electrode for a capacitor.
[0090] (2) Making the capacitor A pair of capacitor electrodes was prepared and punched out into a square shape of 20 mm x 20 mm. A lead wire was connected to each of the capacitor electrodes, and the capacitor electrodes were stacked with a cellulose nonwoven separator sandwiched between them so that the coated surfaces of the electrode layers faced each other, to obtain a laminated capacitor element. The capacitor element was housed in an exterior case made of Al laminate together with an electrolyte, and sealed with a sealing member to complete the capacitor A1 of Example 1. Thereafter, an aging treatment was performed at 60°C for 6 hours while applying 2.5 V.
[0091] The electrolyte for the capacitor A1 was 1-ethyl-3-methylimidazolium tetrafluoroborate (EMIBF4), which is an ionic liquid.
[0092] <Comparative Example 1> Physically exfoliated graphene was prepared by physically exfoliating graphite. Instead of the reduced graphene oxide of Example 1, this physically exfoliated graphene was used as an active material to produce a capacitor electrode, and a capacitor element was obtained by using this capacitor electrode. Capacitor B1 of Comparative Example 1 was fabricated in the same manner as in Example 1 except for this.
[0093] The capacitors A1 and B1 were each evaluated as follows.
[0094] <Evaluation> The capacitance of each of the capacitors A1 and B1 was evaluated by the following method.
[0095] The manufactured capacitor was charged at a constant current of 0.1 to 1 A / g relative to the weight of the cell active material (the total weight of the positive electrode active material and the negative electrode active material) up to a set voltage V1 (=2.8 V). Then, constant voltage charging was performed at the set voltage V1 for 8 minutes.
[0096] After the constant voltage charge, the cells were discharged at a constant current of 0.1 to 1 A / g relative to the weight of the active material of the cell to 0 V. The capacity was calculated from the slope of the voltage change during discharge from 2.1 V to 0.1 V. The capacity was calculated using the following formula, where I (A) is the constant current value during discharge and t (sec) is the discharge time until the voltage drops from 2.1 V to 0.1 V. Capacity(F)=It / (2.1-0.1)
[0097] From the calculated capacity, the single electrode capacity was calculated assuming that the positive and negative electrode capacities (mass of positive and negative electrode active materials) were the same, and the single electrode capacity C1 (F / g) per gram of positive and negative electrode active material mass when voltage V1 was applied was determined.
[0098] The single-electrode capacity C1 (F / g) per gram of the positive and negative electrode active material mass was similarly determined while changing the set voltage V1 from 2.8 V to 5.0 V, and the dependency of the single-electrode capacity C1 on the voltage V1 was evaluated. The results are shown in the graph of FIG.
[0099] Furthermore, after completing the above charging at V1 = 4.4 V, the negative electrode was removed from the capacitor. The removed negative electrode was washed with dimethyl carbonate and then dried. XPS quantitative analysis was performed on the surface of the dried negative electrode, and the ratio R F and R B The results are shown in Table 1.
[0100] [Table 1]
[0101] 2, in capacitor A1, the monopole capacitance C1 increases rapidly as the applied voltage V1 to the capacitor is increased to 4.0 V or higher. On the other hand, in capacitor B1, the monopole capacitance C1 is smaller than that of capacitor A1, and even if the applied voltage V1 to the capacitor is increased to 4.0 V or higher, the increase in the monopole capacitance C1 is small.
[0102] From Table 1, in capacitor A1, the ratio R of F to C on the negative electrode surface is Fis large at 10% or more, and the ratio of B to C is R B The ratio R F and the ratio R B In capacitor B1, only minute amounts of B and F are present on the negative electrode surface, and it can be seen that no increase in capacitance due to oxidation-reduction reactions occurs.
[0103] Figure 3 shows the F1s spectrum in the XPS analysis of the negative electrode surface of capacitors A1 and B1. Capacitors A1 and B1 both show peaks in the F1s spectrum, but the peak of capacitor B1 is smaller than that of capacitor A1 and the peak position is different. This is because the peak appearing in the F1s spectrum of capacitor B1 is due to BF4 - In contrast, in the case of capacitor A1, the peaks appearing in the F 1s spectrum are due to EMI + The reaction product of the reduction of the cation is further converted to BF4 - This is thought to be due to the by-product of the reaction with and the different bonding state of F. [Industrial Applicability]
[0104] According to the present invention, an electrochemical capacitor with high energy density can be obtained. [Explanation of symbols]
[0105] 1: capacitor element, 2: first electrode, 3: second electrode, 4: separator, 5a: first lead wire, 5b: second lead wire, 6: exterior case, 7: sealing member, 10: capacitor
Claims
1. a first electrode including a first active material; a second electrode comprising a second active material; an electrolyte; The electrolyte solution contains an ionic liquid, When the surface of the first electrode is quantitatively analyzed based on a relative sensitivity coefficient using X-ray photon spectroscopy (XPS), the atomic ratio R of element F derived from the ionic liquid to element C is F is 10% or more.
2. The ratio R F The electrochemical capacitor according to claim 1 , wherein the capacitance is 14% or more.
3. When the surface of the first electrode is quantitatively analyzed based on a relative sensitivity coefficient using X-ray photon spectroscopy (XPS), the atomic ratio R of element B to element C is B The electrochemical capacitor of claim 1 , wherein the capacitance is 1% or more.
4. 4. The electrochemical capacitor according to claim 1, wherein a lower potential is applied to the first electrode than to the second electrode.
5. The electrochemical capacitor according to claim 4 , wherein a voltage of 4.0 V or more is applied between the first electrode and the second electrode.
6. The electrochemical capacitor according to claim 1 , wherein the first active material comprises reduced graphene oxide.
7. The electrochemical capacitor according to any one of claims 1 to 3, wherein the ionic liquid contains a cation having a heteroaromatic ring.
8. The electrochemical capacitor of claim 7 , wherein the cation comprises a 1-ethyl-3-methylimidazolium cation.
9. The electrochemical capacitor according to any one of claims 1 to 3, wherein the ionic liquid contains a tetrafluoroborate anion.