Manufacturing method for semiconductor substrate, semiconductor substrate, and semiconductor device

By forming an amorphous layer in SiC substrates through ion implantation and peeling, followed by bonding and etching, the method addresses the high cost and processing challenges of SiC substrates, producing cost-effective and high-quality semiconductor substrates and devices.

JP2024137131AActive Publication Date: 2024-10-07SHIN ETSU HANDOTAI CO LTD
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2023048530
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-07
Estimated Expiration
2043-03-24

AI Technical Summary

Technical Problem

The high cost of SiC substrates for semiconductor devices is a significant challenge, and existing peeling techniques for SiC substrates often result in rough surfaces that hinder reuse and increase manufacturing costs due to difficult bonding and polishing requirements.

Method used

A method involving ion implantation of silicon, carbon, and oxygen into SiC substrates to form an amorphous layer, followed by bonding with a support substrate, peeling at the amorphous layer, and subsequent plasma etching and epitaxial growth to create a high-quality, cost-effective SiC substrate.

Benefits of technology

This method enables the reuse of SiC substrates at a lower cost by simplifying bonding and polishing processes, resulting in high-quality semiconductor substrates and devices with reduced manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137131000001_ABST
    Figure 2024137131000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method for a semiconductor substrate, by which a semiconductor substrate with high quality can be manufactured at lower cost using a 4H-SiC separation technique.SOLUTION: A manufacturing method for a semiconductor substrate 5 includes: an ion injection step of performing ion injection of at least one of silicon, carbon, and oxygen for a 4H-SiC substrate 1, thereby forming an amorphous layer 2 in the 4H-SiC substrate; a bonding step of forming a thin film on at least one of the 4H-SiC substrate 1 and a supporting substrate 3, thereby performing bonding through the thin film; a separating step of separating the 4H-SiC substrate 1 at the amorphous layer 2 into a bonding substrate 12, in which a surface layer of the 4H-SiC substrate 1 is transferred to the supporting substrate 3, and a separation substrate 11, in which the surface layer is separated from the 4H-SiC substrate 1; an etching step of plasma-etching at least one separation surface of the bonding substrate 12 and the separation substrate 11; and an epitaxial step of performing epitaxial growth on at least one of the bonding substrate 12 and the separation substrate 11.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a semiconductor substrate, a semiconductor substrate, and a semiconductor device. [Background technology]

[0002] SiC has a wide band gap of 2.2 to 3.3 eV, which gives it high dielectric breakdown strength. It also has high thermal conductivity, making it a promising material for use as a semiconductor material in various semiconductor devices such as power devices and high-frequency devices.

[0003] However, Non-Patent Document 1 reports that in devices using SiC, the manufacturing process of the SiC substrate and the subsequent epitaxial process account for half of the cost, and therefore reducing the cost of the substrate is extremely important.

[0004] As a cost reduction measure, H + A method has been proposed in which ion implantation is performed to separate the substrate. + There are several prior art reports on implantation of ions into SiC.

[0005] Patent Document 1 describes a method for producing a substrate for semiconductor electronic devices, in which two SiC single crystal wafers are prepared, an oxide layer is formed on each, hydrogen ions are implanted into one of the substrates, the two are bonded together at room temperature via the oxide layer, and then the SiC single crystal wafer is divided into two at the hydrogen ion implanted portion by heat treatment at 500° C. or higher. In this method, an oxide film exists at the bonded portion, and when a vertical device is formed, this oxide film functions as an insulating layer, greatly limiting the function as a power device substrate.

[0006] In addition, Patent Document 2 states that + A method has been disclosed in which the implanted single crystal and polycrystalline SiC substrates are bonded together, and then the single crystal and polycrystalline are peeled off separately. However, there are problems with the increased cost of peeling off twice and the difficulty of peeling off each step in the designated process.

[0007] In Patent Document 3, attention is paid to impurity concentration and defect density, and a high resistance substrate with a low defect density is developed using H + A method of transferring using implantation is described. This method reduces defects present in the original substrate, but there is no mention of the substrate after peeling.

[0008] Furthermore, Patent Document 4 states that + The document describes the technology that causes substrate peeling, and mentions the diffusion barrier (oxygen diffusion barrier) function, but makes no mention of the substrate after peeling.

[0009] Furthermore, Patent Document 5 also describes a wide variety of substrates. + The method of fabricating the device using the above-mentioned peeling technique is described, and a method of epitaxially growing InGaN after polishing and dry etching the surface is described, but there is no description on how to handle the peeled substrate.

[0010] Furthermore, Patent Document 6 describes a method in which a device is fabricated on a silicon carbide substrate, a protective film is formed, ion implantation is performed, and the substrate is bonded to a support substrate, followed by high-temperature annealing, and the substrate is reused after separation. However, there is no description of how to handle the substrate after separation.

[0011] In addition, Patent Document 7 states that + The paper describes a method in which ions are implanted into single crystal SiC, polycrystalline SiC is formed on the opposite surface, annealed, and then the SiC is epitaxially grown after the ion-implanted surface is peeled off and the peeled surface is polished. + In the substrate technology using the above, no specific method for reusing the peeled substrate is mentioned.

[0012] Furthermore, H + Patent Document 8 describes a method for forming a support substrate for ion implantation and subsequent peeling. + Polycrystalline SiC is grown on the substrate after implantation at 1000 to 1600 °C. Patent document 9 describes H +Growth by DLI-CVD (Direct Liquid Injection-CVD) on the substrate after injection. Patent document 10 describes H + Methods such as sintering onto the substrate after implantation and liquid deposition are disclosed.

[0013] This method is adopted because, as described in Patent Document 8, it is difficult to join SiC to itself, and problems have been pointed out regarding the presence of metals when joining via W or Mo.

[0014] However, in this way + After implantation, deposition on a supporting substrate at high temperature results in H + Peeling of the implanted layer can occur during deposition, and H + The substrate itself having the implanted layer is exposed to high temperatures, which not only changes the crystallinity but also forms a polycrystalline layer on the side surface, preventing reuse. [Prior art documents] [Patent documents]

[0015] [Patent Document 1] Japanese Patent Application Publication No. 11-003842 [Patent Document 2] JP 2016-018890 A [Patent Document 3] JP 2014-022711 A [Patent Document 4] JP 2007-329470 A [Patent Document 5] Special Publication No. 2013-513963 [Patent Document 6] JP 2022-140396 A [Patent Document 7] International Publication No. 2022 / 158085 [Patent Document 8] Special table 2022-542224 publication [Patent Document 9] Special table 2023-502571 publication [Patent Document 10] Special publication 2023-502572 [Non-patent literature]

[0016] [Non-Patent Document 1] Iwamuro, "Progress in High Performance and High Reliability of SiC MOSFETs," Proceedings of the Wide Bandgap Semiconductor Society Special Open Symposium, Wide Bandgap Semiconductor Society, 2022 [Non-Patent Document 2] H. Biard, W. Schwarzenbach, S. Odoul, I. Radu, A. Potier, M. Ferrato, E. Guajioty, “Tailored polycrystalline substrate for SmartSiCTM substrates enabling high performance power devices”, ICSCRM2022, 2022 [Non-Patent Document 3] Suga, "Room-temperature bonding by surface activation and its mechanism," Applied Physics, The Japan Society of Applied Physics, 89(9), 2020. p498 Summary of the Invention [Problem to be solved by the invention]

[0017] Thus, 4H-SiC is expected to be used in high-voltage devices, but the high cost of the substrate is a problem, and the challenge is how to reduce the cost of the bulk substrate. + A technology has been proposed to perform ion implantation and peel off the substrate, but in this case, the cost can be reduced by reusing the substrate after peeling (otherwise the cost would remain high). For this reason, it is very important to reuse the substrate after peeling (to make a high-quality substrate), and H + This is the core technology that will enable the widespread adoption of substrate peeling technology that uses ions, etc.

[0018] On the other hand, H +After ion implantation and the substrate is peeled off, the peeled surface of the peeled substrate is rough and must be flattened before it can be re-bonded, and bonding of SiC to itself is difficult. In addition, it may be preferable to flatten the peeled surface of the SiC transferred to the support substrate by peeling before performing epitaxial growth on the peeled surface.

[0019] However, because SiC is a hard material that is difficult to process, the cost of flattening the peeled surface by polishing such as CMP is high, which ultimately increases the manufacturing cost of the substrate. + In the method of growing a support substrate after implantation, peeling off during the growth of the support substrate and unintended growth of polycrystalline SiC on the original substrate hinder reuse.

[0020] H + In the case of injection, as mentioned earlier, + After implantation, deposition of the support substrate at high temperature results in H + Peeling of the implanted layer can occur during deposition, and H + The substrate itself having the implanted layer is exposed to high temperatures, which not only changes the crystallinity but also forms a polycrystalline layer on the side surface, preventing reuse.

[0021] The present invention has been made to solve the above problems, and has an object to provide a semiconductor substrate manufacturing method that uses 4H—SiC peeling technology to produce cheaper, higher quality semiconductor substrates. Another object of the present invention is to provide a semiconductor substrate and a semiconductor device which are less expensive and of higher quality. [Means for solving the problem]

[0022] The present invention relates to a manufacturing method for SiC wafers made to achieve the above-mentioned object, and more specifically to a substrate peeling technology that utilizes ion implantation of silicon, carbon, and oxygen, bonding to a support substrate, and reuse of the substrate after peeling, thereby providing a cheaper, higher quality SiC substrate. Specifically, the present invention has been made to achieve the above-mentioned object, and provides a method for manufacturing a semiconductor substrate, comprising: an ion implantation step of implanting at least one of ions of silicon, carbon and oxygen into a surface of a 4H-SiC substrate to form an amorphous layer in the 4H-SiC substrate by amorphizing silicon and carbon; a bonding step of forming a thin film on at least one of the surface of the 4H-SiC substrate subjected to the ion implantation step and a bonding surface of another support substrate, and bonding the substrates via the thin film to obtain a bonded substrate; a delamination step of peeling the 4H-SiC substrate using the amorphous layer of the bonded substrate to separate the 4H-SiC substrate into a bonded substrate in which the surface layer of the 4H-SiC substrate is transferred as a 4H-SiC layer onto the support substrate, and a delamination substrate, which is the substrate after the surface layer has been delaminated from the 4H-SiC substrate; an etching step of plasma-etching the delamination surface of at least one of the bonded substrate or the delamination substrate after the delamination step; and an epitaxial step of performing epitaxial growth on at least one of the bonded substrate or the delamination substrate.

[0023] According to this method of manufacturing a semiconductor substrate, at least one of silicon, carbon, and oxygen ions are implanted into the surface of a 4H-SiC substrate to break the bonds between silicon and carbon, forming an amorphous layer. After bonding to a support substrate, the 4H-SiC substrate is peeled off from the amorphous layer, and the 4H-SiC layer is transferred to the bonded substrate.

[0024] In this way, in the ion implantation process using at least one of silicon, carbon, and oxygen ions, it is possible to inject damage to a specified depth by adjusting the acceleration energy during implantation. Specifically, the damage is the breaking of the bonds between silicon and carbon caused by the ion implantation of these ions. The broken silicon and carbon exist in an amorphous state.

[0025] The amorphous layer formed in this way can be peeled off by inserting a thin metal object from the side and applying an impact. Furthermore, the amorphous layer becomes black due to the influence of carbon, making it easier to absorb light, so it can be further excited by irradiating it with light and peeled off. Alternatively, it can be peeled off by combining light irradiation and impact.

[0026] In particular, when silicon or carbon is ion-implanted, such a peeling layer will not peel even if it is exposed to high heat, and the peeling process can be carried out at any time during the manufacturing process. Also, when oxygen is ion-implanted, the injected oxygen can be bonded to the carbon in the amorphous layer by heat treatment, and then gasified, which allows peeling.

[0027] In this way, in the present invention, at least one of silicon, carbon, and oxygen ions is implanted and then bonding is performed. In this case, by using a polycrystalline body or a sintered body as the support substrate, as well as a single crystal, it is possible to significantly reduce costs.

[0028] It has also been reported that using a polycrystalline material is more effective in reducing the substrate resistance (Non-Patent Document 2), and in addition to cost, it is extremely effective in improving quality when considered as a vertical device.

[0029] Then, a thin film of silicon or the like is sputtered onto the bonding surfaces of the substrate implanted with silicon or the like ions and the support substrate, and bonding is performed via this thin film, making it possible to bond SiC substrates together, which are difficult to bond.

[0030] In particular, by preparing an inexpensive support substrate such as a polycrystalline substrate, forming a thin film of silicon or the like on the bonding surface, and bonding via the silicon or the like film, it becomes possible to bond SiC, which was previously difficult to bond when the support substrate was SiC.

[0031] Furthermore, in the present invention, the peeled surface of at least one of the peeled substrate and the bonded substrate is etched with plasma to remove the damaged layer and flatten it, after which it is reused or epitaxially grown. In this way, SiC, which is a difficult material to process, can be flattened at a lower cost than polishing such as CMP, and a high-quality substrate can be obtained.

[0032] Although SiC is normally difficult to etch with plasma, it can be etched due to the weakening of the surface caused by ion implantation. If a single high-quality SiC substrate can be prepared by performing epitaxial growth using the CVD method in this way, it becomes possible to inexpensively produce high-quality SiC substrates by repeating the ion implantation, bonding, peeling, etching, and epitaxial processes to transfer the surface layer of the 4H-SiC substrate to a support substrate and then repeating the epitaxial growth using the CVD method.

[0033] At this time, in the peeling step, the amorphous layer is irradiated with light, impacted, or subjected to a combination of these processes, thereby enabling the 4H-SiC substrate to be peeled off.

[0034] In this manner, by irradiating the amorphous layer with light and allowing the layer to absorb the light, the energy required for peeling can be directly imparted to the amorphous layer.

[0035] Furthermore, when the bonded substrate is peeled off by applying an impact to the amorphous layer, the peeling can be achieved simply by inserting, for example, a thin metal blade into the amorphous layer, which has the advantage that the equipment required for peeling can be simplified.

[0036] Furthermore, by combining light irradiation and impact for peeling, the time required for peeling can be shortened compared to when either method is used alone.

[0037] In this case, oxygen ions are implanted in the ion implantation process, and in the peeling process, the amorphous layer is irradiated with light, impacted, or heat-treated to cause the injected oxygen to react with carbon in the amorphous layer to generate gas, or a combination of these processes is performed, thereby peeling off the 4H—SiC substrate.

[0038] By irradiating the amorphous layer with light in this way, the energy required for peeling can be directly applied to the amorphous layer. Also, when peeling off the bonded substrate by applying an impact to the amorphous layer, peeling can be achieved by simply inserting a thin metal blade into the amorphous layer.

[0039] Furthermore, when oxygen ions are injected in the ion implantation process, the injected oxygen reacts with the carbon in the amorphous layer to generate gas, which can then be used for peeling using gas pressure. Therefore, peeling can be achieved by heating in addition to light irradiation and impact, broadening the options for peeling methods. Furthermore, by performing the peeling in combination, the time required for peeling can be shortened compared to performing each of them individually.

[0040] At this time, in the bonding step, a silicon thin film can be formed as the thin film and bonding can be performed via this.

[0041] Thin silicon films are sometimes used as a base for epitaxial growth of 4H-SiC, so they are easy to bond to 4H-SiC, and are also easy to bond to polycrystalline or sintered SiC. Therefore, bonding is made easier by preparing a support substrate such as polycrystalline SiC, which is cheaper than single-crystal SiC, forming a thin layer of silicon on the bonding surface, and bonding via silicon.

[0042] At this time, in the bonding step, the silicon thin film can be formed by a sputtering method using silicon as a target.

[0043] In this way, forming a silicon thin film by sputtering, in which silicon is used as a target and an inert gas such as Ar is ionized and irradiated to form a film, is advantageous in terms of adhesion, etc. It is known that the roughness of the bonding surface in this case is preferably 1 nm or less (Non-Patent Document 3). In addition, the sputtering method does not require high-temperature processing of the substrate on which the film is to be formed, and does not damage the SiC surface at the bonding surface.

[0044] In this case, a mixed gas of fluorocarbon gas and oxygen can be used as a source gas in the etching step.

[0045] Since the mixed gas of fluorocarbon gas and oxygen is a gas used for etching silicon and the like, using it as the source gas has the advantage that there is no need to prepare a gas specifically for etching SiC.

[0046] In this case, after the peeling step and before the etching step, an annealing step can be performed in which the peeled surface of the bonded substrate or the peeled substrate to be subjected to the etching step is annealed at a temperature of 1000° C. or higher in a hydrogen atmosphere.

[0047] By performing hydrogen annealing and then etching in this way, the uneven shape of the peeled surface that has become rough due to peeling is reformed by hydrogen annealing before etching and is flattened to a certain extent, which makes it easier to improve the flatness of the peeled surface in the etching process.

[0048] In this case, in the etching step, the peeled surface of the bonded substrate may be plasma etched, and further, after the etching step, the epitaxial step may be performed on the etched peeled surface of the bonded substrate.

[0049] In this manner, by growing an epitaxial layer on the etched, exfoliated surface of the bonded substrate, devices can be formed on the epitaxial layer, resulting in higher quality devices.

[0050] The present invention also provides a semiconductor substrate comprising a support substrate and a 4H—SiC layer bonded to a surface of the support substrate, the support substrate being made of SiC, the 4H—SiC layer being bonded to the support substrate via a thin silicon film, and the surface being etched.

[0051] In such a semiconductor substrate, the surface of the 4H—SiC layer of the semiconductor substrate is etched, so the surface is flat and an epitaxial layer can be formed without costly planarization processes such as CMP, resulting in a cheaper, higher quality product.

[0052] Furthermore, when the 4H-SiC layer is bonded to a SiC support substrate via a silicon thin film, the silicon thin film is sometimes used as a base when epitaxially growing 4H-SiC, so the bond between the 4H-SiC and the support substrate is strong, and the bond can be strong even when the support substrate is a polycrystalline or sintered SiC body. Therefore, the bond between the support substrate and the 4H-SiC layer is strong.

[0053] The present invention further provides a semiconductor device comprising the semiconductor substrate described above. Such a semiconductor device includes the above-described less expensive and higher quality semiconductor substrate, and therefore is less expensive, has high quality and is highly reliable. Effect of the Invention

[0054] As described above, according to the semiconductor substrate manufacturing method of the present invention, a cheaper and higher quality semiconductor substrate can be manufactured using 4H-SiC peeling technology, and the manufacturing cost of the substrate can be reduced. Also, according to the semiconductor substrate manufacturing method of the present invention, it is possible to effectively utilize the 4H-SiC substrate after peeling off the surface layer, and the manufacturing cost of the semiconductor substrate can be reduced. Furthermore, the semiconductor substrate of the present invention can be produced at a lower cost and with higher quality, and the semiconductor device of the present invention can be produced at a lower cost and with higher quality. [Brief description of the drawings]

[0055] [Figure 1] 1 shows a schematic diagram of a semiconductor substrate of the present invention; [Diagram 2] 1 shows a flow diagram of a method for manufacturing a semiconductor substrate according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0056] The present invention will be described in detail below, but the present invention is not limited thereto.

[0057] As described above, there has been a demand for a semiconductor substrate manufacturing method that can produce cheaper, higher quality semiconductor substrates using 4H—SiC delamination technology and that can reduce the substrate manufacturing costs, cheaper, higher quality semiconductor substrates, and cheaper, higher quality semiconductor devices.

[0058] As a result of intensive research into the above-mentioned problems, the present inventors have discovered a method for manufacturing a 4H-SiC substrate, comprising the steps of: an ion implantation step of implanting at least one of ions of silicon, carbon and oxygen into a surface of a 4H-SiC substrate to form an amorphous layer in the 4H-SiC substrate by amorphizing silicon and carbon; a bonding step of forming a thin film on at least one of the surface of the 4H-SiC substrate subjected to the ion implantation step and a bonding surface of another support substrate, and bonding the substrate via the thin film to obtain a bonded substrate; and a bonding step of peeling off the 4H-SiC substrate at the amorphous layer of the bonded substrate to obtain a bonded substrate. The inventors have found that a cheaper, higher quality semiconductor substrate can be manufactured using 4H-SiC peeling technology by a method for manufacturing a semiconductor substrate, the method comprising: a peeling step of separating a 4H-SiC substrate into a bonded substrate in which the surface layer of the 4H-SiC substrate has been transferred onto the supporting substrate as a 4H-SiC layer; and a peeled substrate, which is the substrate remaining after the surface layer has been peeled off from the 4H-SiC substrate; an etching step of plasma etching the peeled surface of at least one of the bonded substrate or the peeled substrate after the peeling step; and an epitaxial step of performing epitaxial growth on at least one of the bonded substrate or the peeled substrate, thereby completing the present invention.

[0059] Furthermore, as a result of extensive investigation into the above-mentioned problems, the inventors have found that a cheaper, higher quality semiconductor substrate can be provided by a semiconductor substrate comprising a support substrate and a 4H—SiC layer bonded to a surface of the support substrate, wherein the support substrate is made of SiC, the 4H—SiC layer is bonded to the support substrate via a thin silicon film, and has an etched surface, and have completed the present invention.

[0060] Furthermore, as a result of extensive research into the above-mentioned problems, the inventors discovered that a semiconductor device comprising the semiconductor substrate described above can provide a cheaper, higher quality semiconductor device, and thus completed the present invention.

[0061] Preferred embodiments of the present invention will now be described with reference to the drawings. First, the configuration of the semiconductor substrate 5 will be described with reference to FIG. As shown in FIG. 1, a semiconductor substrate 5 according to an embodiment of the present invention comprises a support substrate 3 and a 4H—SiC layer 1a bonded to the surface of the support substrate 3, with the 4H—SiC layer 1a bonded to the support substrate 3 via a thin film 7.

[0062] Support substrate 3 is a substrate that supports 4H—SiC layer 1a via thin film 7, and the material and dimensions can be appropriately selected so long as it has sufficient strength to support 4H—SiC layer 1a and does not cause unintended reactions with thin film 7. Specifically, bulk 4H—SiC using the same material as 4H—SiC layer 1a can be exemplified, but in consideration of cost, a sintered SiC substrate or a polycrystalline SiC substrate, which is less expensive than bulk 4H—SiC, may also be used.

[0063] The 4H—SiC layer 1a is a single crystal layer of 4H—SiC, and is bonded to the surface of a supporting substrate 3. For this bonding, a thin film 7 is formed on the bonding surfaces of the 4H—SiC layer 1a and the supporting substrate 3, and bonding via this thin film 7 enables a strong bond to be formed.

[0064] The thin film 7 is made of a material, such as a silicon thin film, that can be bonded to the 4H—SiC layer 1a and the support substrate 3. In the following description, unless otherwise specified, the present invention will be described taking the case where a silicon thin film is used as the thin film 7 as an example.

[0065] Moreover, 4H—SiC layer 1a has surface 25 that has been etched. Since 4H—SiC layer 1a has surface 25 that has been etched, surface 25 becomes flat, and an epitaxial layer can be formed without performing expensive flattening treatment such as CMP, resulting in a cheaper and higher quality semiconductor substrate 5.

[0066] The 4H-SiC layer 1a may be a bulk 4H-SiC single crystal layer, or may be an epitaxial layer of 4H-SiC.

[0067] The thickness of the 4H-SiC layer 1a should be at least such that it can maintain its shape as a layer, can form a device, and is not lost during etching, polishing, etc. On the other hand, the maximum thickness is, for example, such that there is as little waste as possible when forming a device. The thickness can be, for example, 0.01 μm to 400 μm.

[0068] Next, the configuration of the semiconductor device 6 will be described with reference to FIG. The semiconductor device 6 shown in FIG. A specific example of the semiconductor device 6 is one in which a desired semiconductor device is formed on the semiconductor substrate 5, particularly the 4H-SiC layer 1a. Of course, the semiconductor device 6 can be made into chips by dicing.

[0069] By including the semiconductor device 6 in the semiconductor substrate 5 which is less expensive and has higher quality, the semiconductor device 6 also becomes less expensive, has higher quality, and is more reliable.

[0070] Next, an outline of a method for manufacturing the semiconductor substrate 5 of the present invention will be described with reference to FIG. 2(a), a 4H—SiC substrate 1 is prepared. Here, single-crystal bulk 4H—SiC is exemplified as the 4H—SiC substrate 1, but a 4H—SiC epitaxial substrate may also be used.

[0071] In this embodiment, the surface layer of the 4H—SiC substrate 1 is transferred to the support substrate 3, but the peeled substrate 11 finally produced after the transfer may be reused as the 4H—SiC substrate 1. It is preferable that the 4H—SiC substrate 1 is epitaxially grown by CVD.

[0072] Next, at least one of silicon, carbon, and oxygen ions is implanted into the 4H-SiC substrate 1 to break the bonds between silicon and carbon near the surface of the 4H-SiC substrate 1, forming an amorphous layer 2 in which silicon and carbon are both amorphous, as shown in Figure 2(b) (ion implantation process).

[0073] By adjusting the acceleration energy of the ion implantation, it is possible to form an amorphous layer 2 in which the silicon and carbon are amorphous and exist at a predetermined depth. When oxygen ions are implanted, an amorphous layer 2 and a layer in which oxygen exists are formed.

[0074] The ion species to be implanted needs to be at least one of silicon, carbon, and oxygen, and multiple types of ions may be implanted. In addition, the type of ion to be implanted (silicon, carbon, or oxygen) may be appropriately selected in consideration of the advantages of each.

[0075] For example, when ion implanting silicon or carbon, these elements are elements that make up SiC, so it is advantageous that they do not become impurities when implanted. On the other hand, when ion implanting oxygen, it is advantageous in that there are more options for the delamination method, since the 4H-SiC substrate 1 can be delaminate by heating in a post-process.

[0076] The acceleration energy during ion implantation varies depending on the depth position where the amorphous layer 2 is formed. Specifically, the deeper the position in the depth direction, the greater the acceleration energy; for example, it is about 200 keV.

[0077] The amount of ions to be implanted may be sufficient to form the amorphous layer 2. For example, 1.0×10 17 atoms / cm 2 That's about it.

[0078] 2(c), a substrate separate from the 4H—SiC substrate 1 is prepared as support substrate 3. Support substrate 3 may be single crystal 4H—SiC having the same structure as 4H—SiC substrate 1, but considering the cost, it is preferable to use sintered SiC or polycrystalline SiC produced by sintering, for example.

[0079] Next, as shown in FIG. 2(d), a thin film 7 such as a silicon thin film is formed on the surface 14 of the 4H—SiC substrate 1 that has been subjected to the silicon ion implantation process and on the bonding surface 8 of the support substrate 3, and then these are bonded to obtain the bonded substrate 10 shown in FIG. 2(e) (bonding process).

[0080] It is preferable to form a silicon thin film as the thin film 7 and perform bonding via this. Since a silicon thin film is sometimes used as a base for epitaxial growth of 4H-SiC, it is easy to bond to 4H-SiC, and it is also easy to bond to polycrystalline or sintered SiC. Therefore, by preparing a support substrate 3 such as polycrystalline SiC, which is cheaper than single crystal SiC, forming a thin layer of silicon on the bonding surface 8, and bonding via silicon, it becomes possible to bond even SiC, which is difficult to bond.

[0081] As a specific method for depositing the thin film 7, a sputtering method in which a silicon target is used and Ar ions are irradiated onto the target to deposit the film is effective because it does not require high temperature heating of the substrate and does not damage the SiC surface at the bonding surface.

[0082] Moreover, as a method for bonding the 4H—SiC substrate 1 and the support substrate 3 via the thin film 7, for example, room temperature bonding can be mentioned.

[0083] Next, as shown in FIG. 2(f), the 4H—SiC substrate 1 is peeled off at the amorphous layer 2 of the bonded substrate 10, thereby separating the 4H—SiC substrate 1 into a bonded substrate 12 in which the surface layer of the 4H—SiC substrate 1 is transferred onto the supporting substrate 3 as a 4H—SiC layer 1a, and a peeled substrate 11, which is the substrate remaining after the surface layer has been peeled off from the 4H—SiC substrate 1 (peeling process).

[0084] Specifically, in the peeling step, the amorphous layer 2 is irradiated with light, subjected to an impact, or subjected to a combination of these processes, thereby enabling the 4H—SiC substrate 1 to be peeled off.

[0085] When light irradiation is performed, light is irradiated onto bonded substrate 10 and the light is absorbed by amorphous layer 2 of silicon and carbon formed in the ion implantation process. This serves as a starting point for peeling off 4H-SiC substrate 1, separating bonded substrate 10 into bonded substrate 12 in which the surface layer of 4H-SiC substrate 1 is transferred onto supporting substrate 3 as 4H-SiC layer 1a, and peeled substrate 11, which is the substrate remaining after the surface layer has been peeled off from 4H-SiC substrate 1.

[0086] In this manner, the amorphous layer 2 is irradiated with light and absorbs the light, so that the energy required for peeling can be directly imparted to the amorphous layer 2.

[0087] The light source of the irradiated light is not particularly limited as long as it can impart to the amorphous layer 2 sufficient energy to peel off the 4H—SiC substrate 1 starting from the amorphous layer 2, and an example of the light source is a YAG laser. When a YAG laser is used as the light source, the wavelength of the irradiated light can be a fundamental wavelength (1064 nm).

[0088] In the peeling step, when an impact is applied to the amorphous layer 2, it is possible to peel the amorphous layer 2 by simply inserting, for example, a thin metal blade into the amorphous layer 2 without irradiating it with light. The method of peeling the amorphous layer 2 by applying an impact in this manner is advantageous in that the equipment required for peeling can be simplified.

[0089] Furthermore, it is also possible to combine light irradiation and impact to peel off. Specifically, in addition to light irradiation, it is also possible to insert a thin metal blade or the like into the carbon amorphous layer 2 to apply impact to peel off. In this case, the time required for peeling can be shortened compared to when light irradiation or impact is applied alone.

[0090] If oxygen ions are implanted in the ion implantation process, the 4H—SiC substrate 1 can be peeled off in the peeling process by irradiating the amorphous layer 2 with light, applying an impact, or performing a heat treatment to cause the injected oxygen to react with the carbon in the amorphous layer to generate gas, or by performing a combination of these processes.

[0091] Since the separated surface 23 of the bonded substrate 12 obtained by peeling in this manner has a rough surface, it may be preferable to flatten the surface if an epitaxial layer is to be formed in a later process. The separated substrate 11 can be reused by repeatedly performing the ion implantation process, bonding process, and peeling process to transfer the surface layer to a plurality of supporting substrates 3, but since the separated surface 21 has a rough surface, it is necessary to flatten the surface in order to bond it to the supporting substrate 3. The procedure for flattening the separated surfaces 23 and 21 will be described below.

[0092] First, as shown in FIG. 2(h), at least one of the peeled surface 23 of the bonded substrate 12 and the peeled surface 21 of the peeled substrate 11 after the peeling step is plasma etched (etching step).

[0093] 2 shows an example in which both the peeled surface 23 of the bonded substrate 12 and the peeled surface 21 of the release substrate 11 are etched, but at least one of them may be etched. For example, when an epitaxial layer can be formed without planarizing the peeled surface 23 of the bonded substrate 12, or when the 4H—SiC layer 1a is an epitaxial layer and no further epitaxial layer needs to be formed, only the peeled surface 21 of the release substrate 11 may be etched.

[0094] By plasma etching at least one of the separated surface 23 of the bonded substrate 12 and the separated surface 21 of the separated substrate 11, the surface of SiC, which is a difficult-to-process material, can be flattened at a lower cost than by CMP or the like.

[0095] A mixed gas of fluorocarbon gas and oxygen can be used as the source gas for etching. Specific examples of fluorocarbon gas include CHF3 and CF4. Since a mixed gas of fluorocarbon gas and oxygen is used for etching silicon and the like, using it as the source gas has the advantage that it is not necessary to prepare a gas specifically for etching SiC.

[0096] The plasma form during the etching process may be optimized depending on the device, and may be, but is not limited to, RF plasma. Generally, SiC is not etched with a mixture of fluorocarbon gas and oxygen gas, but the peeled surfaces 23 and 21 are weakened by the ion implantation process, and the surface layer is a damaged layer, so this layer including the peeled surfaces 23 and 21 can be removed by etching to make the surface flat. The weakening can be achieved not only by the damage caused by ion implantation, but also by plasma processing using H2 gas.

[0097] After the peeling step and before the etching step, as shown in FIG. 2(g), the peeled surface 23 of the bonded substrate 12 or the peeled surface 21 of the peeled substrate 11 to be subjected to the etching step may be annealed at a temperature of 1000° C. or higher in a hydrogen atmosphere (annealing step).

[0098] By carrying out the etching step after carrying out the hydrogen annealing in the annealing step in this way, the uneven shape of the peeled surface 23 or the peeled surface 21 that has become rough due to peeling is reformed by the hydrogen annealing before etching, and is flattened to some extent. Therefore, it becomes easier to improve the flatness of the peeled surface 23 or the peeled surface 21 in the etching step.

[0099] After the peeling process, the peeled substrate 11 can be reused as the 4H—SiC substrate 1 by repeating the ion implantation process, bonding process, and peeling process again, until it becomes thick enough that it cannot be peeled any further, and can be reused as a substrate for transferring 4H—SiC to the support substrate 3.

[0100] Here, when the release surface 21 of the release substrate 11 is etched in an etching process, the release surface 21 is planarized by etching, so that the support substrate 3 can be bonded to the release surface 21 without performing costly planarization processing such as CMP.

[0101] Next, epitaxial growth is performed on at least one of the bonded substrate 12 and the separated substrate 11 (epitaxial step). Specifically, the epitaxial layer 4 may be grown by CVD or the like.

[0102] FIG. 2( i ) illustrates an example in which an epitaxial layer 4 of 4H—SiC is grown on a 4H—SiC layer 1 a of a bonded substrate 12 . Here, when the peeled surface 23 of the 4H—SiC layer 1 a is etched in the etching process, the peeled surface 23 is planarized by etching, so that the epitaxial layer 4 can be formed on the peeled surface 23 without performing a costly planarization process such as CMP, and the bonded substrate 12 can be made into a cheaper, higher quality semiconductor substrate 5.

[0103] In addition, when the 4H—SiC layer 1a is an epitaxial layer, and the thickness of the transferred 4H—SiC layer 1a is sufficient for forming a device in a subsequent process, it is not necessarily necessary to perform the epitaxial process shown in FIG. 2(i).

[0104] On the other hand, if the 4H—SiC layer 1a is not an epitaxial layer, or if the 4H—SiC layer 1a is an epitaxial layer but has an insufficient thickness for forming a device when transferred in the peeling step, it is preferable to perform an epitaxial step on the bonded substrate 12. In this case, it is preferable to smooth the peeled surface 23 by an etching step before performing the epitaxial step on the bonded substrate 12.

[0105] Specifically, it is preferable to plasma etch the exfoliated surface 23 of the bonded substrate 12 in an etching step as shown in FIG. 2(h), and then to grow an epitaxial layer 4 on the etched exfoliated surface 23 of the bonded substrate 12 in an epitaxial step as shown in FIG. 2(i).

[0106] In this way, by growing the epitaxial layer 4 on the etched release surface 23 of the bonded substrate 12, devices can be formed on the epitaxial layer 4, resulting in higher quality devices. EXAMPLES

[0107] The present invention will be described in detail below with reference to examples, but these are not intended to limit the scope of the present invention. It is not. We attempted to reuse the exfoliated substrate 11 as the 4H-SiC substrate 1 by performing the ion implantation process of silicon, carbon, and oxygen, the bonding process (silicon thin film formation and bonding), the peeling process, and the etching process on the 4H-SiC substrate 1, and then performing the ion implantation process and the bonding process again.

[0108] Example 1 First, a 4H-SiC single crystal substrate with a diameter of 200 mm, a thickness of 355 μm, n-type, resistivity of 10 Ω·cm, and an offset of 4° from the (0001) plane was prepared as the 4H-SiC substrate 1. In the ion implantation process, silicon ions were implanted into the substrate at a rate of 1×10 with an acceleration energy of 200 keV using an ion implanter. 17 atoms / cm 2 Injected.

[0109] Next, the following steps were performed as the bonding process. First, a polycrystalline SiC substrate of the same diameter as the 4H-SiC substrate 1 was prepared as the support substrate 3, and a silicon thin film was formed as the thin film 7 on both the 4H-SiC substrate 1 and the support substrate 3 by sputtering using silicon as a target and irradiating Ar ions. The thickness of the silicon thin film at this time was set to 20 nm. After this, the 4H-SiC substrate 1 and the support substrate 3 were bonded at room temperature via the silicon thin film to obtain a bonded substrate 10.

[0110] Following the bonding step, a YAG laser (wavelength 1064 nm) was used to irradiate and excite the amorphous layer 2 as a peeling step, and the bonded substrate 10 was separated into a bonded substrate 12 and a peeled substrate 11.

[0111] On this bonded substrate 12, a hot wall type CVD apparatus was used as an epitaxial process, and H2 was used as a carrier gas, and SiH4 and C3H8 were used as raw material gases to perform epitaxial growth of 4H—SiC, thereby obtaining a semiconductor substrate 5. The temperature at this time was 1600° C., and the pressure inside the furnace was 7 kPa.

[0112] In this way, an RF plasma etching process was performed on the peeled surface 21 of the peeled substrate 11 that was obtained when the semiconductor substrate 5 was obtained, under the following conditions: the source gases were CHF3 and O2 at 100 sccm and 10 sccm, respectively, the pressure was 100 Torr (13,332.2 Pa), and the RF power was 500 W.

[0113] When the exfoliated substrate 11 after the etching process was subjected to the silicon ion implantation process and bonding process again in the same manner as above, the support substrate 3 could be bonded to the exfoliated surface 21 of the exfoliated substrate 11, and the bonded substrate 10 could be obtained in the same manner.

[0114] Example 2 First, a 4H-SiC single crystal substrate with a diameter of 200 mm, a thickness of 355 μm, n-type, resistivity of 10 Ω·cm, and an offset of 4° from the (0001) plane was prepared as the 4H-SiC substrate 1. In the ion implantation process, carbon ions were implanted into the substrate at a dose of 1.0×10 with an acceleration energy of 200 keV using an ion implanter. 17 atoms / cm 2 Injected.

[0115] Next, the following steps were performed as the bonding process. First, a polycrystalline SiC substrate of the same diameter as the 4H-SiC substrate 1 was prepared as the support substrate 3, and silicon was used as a target and irradiated with Ar ions to form silicon as a thin film 7 on both the 4H-SiC substrate 1 and the support substrate 3 by sputtering. The silicon thin film at this time was 20 nm. After this, the 4H-SiC substrate 1 and the support substrate 3 were bonded at room temperature via the silicon thin film to obtain a bonded substrate 10.

[0116] Following the bonding step, a YAG laser (wavelength 1064 nm) was used to irradiate and excite the amorphous layer 2 as a peeling step, and the bonded substrate 10 was separated into a bonded substrate 12 and a peeled substrate 11.

[0117] On this bonded substrate 12, a hot wall type CVD apparatus was used as an epitaxial process, and H2 was used as a carrier gas, and SiH4 and C3H8 were used as raw material gases to perform epitaxial growth of 4H—SiC, thereby obtaining a semiconductor substrate 5. The temperature at this time was 1600° C., and the pressure inside the furnace was 7 kPa.

[0118] In this way, an RF plasma etching process was performed on the peeled surface 21 of the peeled substrate 11 that was obtained when the semiconductor substrate 5 was obtained, under the following conditions: the source gases were CHF3 and O2 at 100 sccm and 10 sccm, respectively, the pressure was 100 Torr (13,332.2 Pa), and the RF power was 500 W.

[0119] When the peeled substrate 11 after the etching process was subjected to the carbon ion implantation process and bonding process again in the above-mentioned reuse flow, the support substrate 3 could be bonded to the peeled surface 21 of the peeled substrate 11, and a bonded substrate 10 could be obtained in the same manner.

[0120] Example 3 First, a 4H-SiC single crystal substrate with a diameter of 200 mm, a thickness of 355 μm, n-type, resistivity of 10 Ω·cm, and an offset of 4° from the (0001) plane was prepared as the 4H-SiC substrate 1. In the ion implantation process, oxygen ions were implanted into the substrate at a rate of 1.0×10 with an acceleration energy of 200 keV using an ion implanter. 17 atoms / cm 2 Injected.

[0121] Next, the following steps were performed as the bonding process. First, a polycrystalline SiC substrate of the same diameter as the 4H-SiC substrate 1 was prepared as the support substrate 3, and silicon was used as a target and irradiated with Ar ions to form silicon as a thin film 7 on both the 4H-SiC substrate 1 and the support substrate 3 by sputtering. The thickness of the silicon thin film at this time was set to 20 nm. After this, as the bonding process, the 4H-SiC substrate 1 and the support substrate 3 were bonded at room temperature to obtain a bonded substrate 10.

[0122] Following the bonding step, a YAG laser (wavelength 1064 nm) was used to irradiate and excite the amorphous layer 2 as a peeling step, and the bonded substrate 10 was separated into a bonded substrate 12 and a peeled substrate 11.

[0123] On this bonded substrate 12, a hot wall type CVD apparatus was used as an epitaxial process, and H2 was used as a carrier gas, and SiH4 and C3H8 were used as raw material gases to perform epitaxial growth of 4H—SiC, thereby obtaining a semiconductor substrate 5. The temperature at this time was 1600° C., and the pressure inside the furnace was 7 kPa.

[0124] In this way, an RF plasma etching process was performed on the peeled surface 21 of the peeled substrate 11 that was obtained when the semiconductor substrate 5 was obtained, under the following conditions: the source gases were CHF3 and O2 at 100 sccm and 10 sccm, respectively, the pressure was 100 Torr (13,332.2 Pa), and the RF power was 500 W.

[0125] When the exfoliated substrate 11 after the etching process was subjected to the oxygen ion implantation process and bonding process again in the same manner as above, the support substrate 3 could be bonded to the exfoliated surface 21 of the exfoliated substrate 11, and the bonded substrate 10 could be obtained in the same manner.

[0126] As described above, according to the embodiment of the present invention, amorphous layer 2 is formed on 4H—SiC substrate 1 by ion implantation, and then supporting substrate 3 is bonded thereto via thin film 7, and 4H—SiC substrate 1 is peeled off at amorphous layer 2, thereby obtaining bonded substrate 12 in which the surface layer of 4H—SiC substrate 1 is transferred onto supporting substrate 3 as 4H—SiC layer 1a. In addition, peeled substrate 11 can be reused as 4H—SiC substrate 1.

[0127] The present specification includes the following aspects. [1]: an ion implantation step of implanting at least one of silicon, carbon, and oxygen ions into a surface of a 4H-SiC substrate to form an amorphous layer of silicon and carbon in the 4H-SiC substrate; a bonding step of forming a thin film on at least one of the surface of the 4H—SiC substrate subjected to the ion implantation step and a bonding surface of another support substrate, and bonding the substrate via the thin film to obtain a bonded substrate; a peeling step of peeling the 4H—SiC substrate at the amorphous layer of the bonded substrate to separate the 4H—SiC substrate into a bonded substrate in which a surface layer of the 4H—SiC substrate is transferred onto the supporting substrate as a 4H—SiC layer, and a peeled substrate which is a substrate obtained after the surface layer is peeled off from the 4H—SiC substrate; an etching step of plasma etching at least one of the release surfaces of the bonded substrate and the release substrate after the peeling step; A method for manufacturing a semiconductor substrate, comprising the step of performing epitaxial growth on at least one of the bonded substrate and the separated substrate. [2]: The method for producing a semiconductor substrate according to [1] above, wherein in the peeling step, the amorphous layer is irradiated with light, impacted, or subjected to a combination of these processes to peel off the 4H—SiC substrate. [3]: In the ion implantation step, oxygen ions are implanted; The method for manufacturing a semiconductor substrate according to [1] or [2] above, wherein in the peeling step, the amorphous layer is irradiated with light, impacted, or heat-treated to cause a reaction between injected oxygen and carbon in the amorphous layer to generate gas, or a combination of these processes is used to peel off the 4H—SiC substrate. [4]: The method for producing a semiconductor substrate according to any one of [1] to [3] above, wherein in the bonding step, a silicon thin film is formed as the thin film and bonding is performed via the silicon thin film. [5]: The method for producing a semiconductor substrate according to [4] above, wherein in the bonding step, the silicon thin film is formed by a sputtering method using silicon as a target. [6]: The method for producing a semiconductor substrate according to any one of [1] to [5] above, wherein a mixed gas of a carbon fluoride gas and oxygen is used as a source gas in the etching step. [7]: The method for producing a semiconductor substrate according to any one of [1] to [6] above, characterized in that after the peeling step and before the etching step, an annealing step is performed in which the peeled surface of the bonded substrate or the peeled substrate to be subjected to the etching step is annealed at a temperature of 1000° C. or higher in a hydrogen atmosphere. [8]: The method for producing a semiconductor substrate according to any one of [1] to [7] above, characterized in that in the etching step, the peeled surface of the bonded substrate is plasma etched, and further, after the etching step, the epitaxial step is performed on the etched peeled surface of the bonded substrate. [9]: A semiconductor laser device comprising: a support substrate; and a 4H—SiC layer bonded to a surface of the support substrate; the support substrate is SiC; A semiconductor substrate, wherein the 4H-SiC layer is bonded to the support substrate via a thin silicon film, and the surface of the semiconductor substrate is etched.

[10] : A semiconductor device comprising the semiconductor substrate described in [9] above.

[0128] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. [Explanation of symbols]

[0129] 1...4H-SiC substrate, 1a...4H-SiC layer, 2...amorphous layer, 3...support substrate, 4...epitaxial layer, 5...semiconductor substrate, 6...semiconductor device, 7...thin film, 8...bonding surface, 10...bonded substrate, 11...peeled substrate, 12...bonded substrate, 14...surface, 21...peeled surface, 23...peeled surface, 25...surface.

Claims

1. an ion implantation step of implanting at least one of ions of silicon, carbon, and oxygen into a surface of a 4H-SiC substrate to form an amorphous layer in the 4H-SiC substrate in which silicon and carbon are amorphized; a bonding step of forming a thin film on at least one of the surface of the 4H—SiC substrate subjected to the ion implantation step and a bonding surface of another support substrate, and bonding the substrate via the thin film to obtain a bonded substrate; a peeling step of peeling the 4H—SiC substrate at the amorphous layer of the bonded substrate to separate the 4H—SiC substrate into a bonded substrate in which a surface layer of the 4H—SiC substrate is transferred onto the support substrate as a 4H—SiC layer, and a peeled substrate which is a substrate obtained after the surface layer is peeled off from the 4H—SiC substrate; an etching step of plasma etching at least one of the release surfaces of the bonded substrate and the release substrate after the peeling step; A method for manufacturing a semiconductor substrate, comprising the step of performing epitaxial growth on at least one of the bonded substrate and the separated substrate.

2. 2. The method for producing a semiconductor substrate according to claim 1, wherein in the peeling step, the 4H-SiC substrate is peeled off by irradiating the amorphous layer with light, applying an impact, or performing a combination of these processes.

3. In the ion implantation step, oxygen ions are implanted, 2. The method for producing a semiconductor substrate according to claim 1, wherein in the peeling step, the 4H-SiC substrate is peeled off by irradiating the amorphous layer with light, applying an impact, or performing a heat treatment on the amorphous layer, reacting implanted oxygen with carbon in the amorphous layer to generate a gas, or performing a combination of these treatments.

4. 2. The method for manufacturing a semiconductor substrate according to claim 1, wherein in the bonding step, a silicon thin film is formed as the thin film and bonding is performed via the silicon thin film.

5. 5. The method for manufacturing a semiconductor substrate according to claim 4, wherein in the bonding step, the silicon thin film is formed by a sputtering method using silicon as a target.

6. 2. The method for manufacturing a semiconductor substrate according to claim 1, wherein a mixed gas of a fluorocarbon gas and oxygen is used as a source gas in said etching step.

7. 2. The method for manufacturing a semiconductor substrate according to claim 1, further comprising the step of: performing an annealing step after the peeling step and before the etching step, in which the peeled surface of the bonded substrate or the peeled substrate to be subjected to the etching step is annealed at a temperature of 1000° C. or higher in a hydrogen atmosphere.

8. The method for manufacturing a semiconductor substrate according to any one of claims 1 to 7, characterized in that, in the etching step, the peeled surface of the bonded substrate is plasma etched, and further, after the etching step, the epitaxial step is performed on the etched peeled surface of the bonded substrate.

9. A support substrate and a 4H—SiC layer bonded to a surface of the support substrate, the support substrate is SiC; The 4H-SiC layer is bonded to the support substrate via a thin silicon film, and the surface of the semiconductor substrate is etched.

10. A semiconductor device comprising the semiconductor substrate according to claim 9.

Citation Information

Patent Citations

  • Semiconductor substrate structure and power semiconductor device

    JP2019210162A

  • Semiconductor substrate, composite semiconductor substrate, and semiconductor joint substrate

    JP2021006501A

  • Method for processing semiconductor substrate and method for manufacturing semiconductor device in which said processing method is used

    WO2015156381A1

  • Semiconductor substrate and semiconductor substrate production method

    WO2016006663A1

  • Semiconductor substrate and method for producing same

    WO2022158078A1