Substrate processing method and substrate processing apparatus
A two-step etching process for substrates addresses the challenges of fence-like residues and shoulder chipping by forming a step in the first region, ensuring reliable suppression and precise comb-teeth formation without complex condition adjustments.
Patent Information
- Application Number
- JP2023048727
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2043-03-24
AI Technical Summary
Existing substrate etching methods face challenges in reliably suppressing the formation of fence-like residues and shoulder chipping during the reduction of torsion bar thickness, requiring precise adjustment of etching conditions to balance protective film and etching effects.
A two-step etching process is employed, where the first region is etched to form a step by reducing its width in subsequent stages, ensuring that fence-like residues and shoulder chipping are minimized by etching the step portion where the width becomes smaller.
This approach effectively suppresses fence-like residues and shoulder chipping without the need for precise etching condition adjustments, simplifying the process and ensuring high precision in forming comb-teeth structures.
Smart Images

Figure 2024137269000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a substrate processing method and a substrate processing apparatus, and more particularly to a substrate processing method and a substrate processing apparatus for etching a substrate. [Background technology]
[0002] 2. Description of the Related Art Conventionally, a substrate processing method for etching a substrate is known (see, for example, Patent Document 1).
[0003] The above-mentioned Patent Document 1 discloses a configuration in which, in order to form an elongated torsion bar in a substrate containing silicon, the periphery of the portion corresponding to the torsion bar is etched, and then the portion corresponding to the torsion bar is etched to reduce the thickness of the torsion bar, thereby forming the torsion bar. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 5223381 Summary of the Invention [Problem to be solved by the invention]
[0005] However, as in the above Patent Document 1, there are cases where the torsion bar having an elongated shape is etched to reduce the thickness in a state where the periphery of the torsion bar is etched. At this time, if the action of protecting the substrate by the protective film during etching is stronger than the action of scraping the substrate by etching, the substrate near the protective film is unlikely to be etched, and it is considered that a fence-shaped residue is formed at the end of the torsion bar near the protective film. On the other hand, if the action of scraping the substrate by etching is stronger than the action of protecting the substrate by the protective film during etching, it is considered that the end of the torsion bar is scraped by etching and shoulder chipping occurs. In addition, by adjusting the conditions of the etching process to adjust the balance between the action of protecting the substrate by the protective film and the action of scraping the substrate by etching, it is possible to suppress the formation of fence-shaped residues and the occurrence of shoulder chipping, but it is necessary to adjust the conditions of the etching process with high precision. For this reason, it is very difficult to adjust the etching conditions in order to adjust the balance between the action of protecting the substrate by the protective film and the action of scraping the substrate by etching. As a result, there is a problem that it is difficult to reliably suppress the formation of fence-shaped residues and the occurrence of shoulder chipping when etching a part of a substrate whose periphery is etched to reduce the thickness.
[0006] The present invention has been made to solve the above-mentioned problems, and one object of the present invention is to provide a substrate processing method and substrate processing apparatus that can reliably suppress the formation of fence-shaped residues and the occurrence of shoulder chips when etching a portion of a substrate whose periphery is etched to reduce its thickness. [Means for solving the problem]
[0007] In order to achieve the above object, a substrate processing method according to a first aspect of the present invention includes a first etching step of etching the peripheries of a first region and a second region of a substrate containing silicon, and a second etching step of etching the first region such that a height of the first region is smaller than a height of the second region of the first and second regions in a state in which the peripheries have been etched by the first etching step, wherein the first etching step includes a first step of etching the periphery of the first region so that the width of the first region has a first width, and a second step of etching the periphery of the first region so that after the first step, the width of the first region has a second width smaller than the first width, forming a step in the first region.
[0008] In the substrate processing method according to the first aspect of the present invention, as described above, the first etching step includes a first step of etching the periphery of the first region so that the width of the first region has a first width, and a second step of etching the periphery of the first region so that the width of the first region has a second width smaller than the first width after the first step, forming a step in the first region. Thereby, in the first etching step, the width of the upper part of the first region can be increased so that the step can be formed. As a result, in the second etching step, even if a fence-shaped residue is formed in the upper part of the first region when the first region is etched, if the first region is etched to the step part where the width is reduced, the fence-shaped residue cannot be supported in the first region, and the fence-shaped residue is removed. This makes it possible to reliably suppress the formation of the fence-shaped residue. In addition, even if a shoulder chip occurs in the upper part of the first region, if the width is reduced by etching to the step part where the width is reduced, the occurrence of a shoulder chip at the end can be suppressed by the amount of the reduced width. As a result, it is possible to reliably suppress the formation of the fence-shaped residue and the occurrence of the shoulder chip when a part of the substrate whose periphery is etched is etched to reduce the thickness. Furthermore, since there is no need to precisely adjust the etching conditions in the second etching step in order to adjust the balance between the effect of protecting the substrate by the protective film and the effect of removing the substrate by etching, the work of setting the etching conditions can be prevented from becoming complicated.
[0009] In the substrate processing method according to the first aspect, preferably, the second etching step etches the first region so that the height of the first region is smaller than the height of the second region by a predetermined length, and the first etching step etches the periphery of the first region by a depth corresponding to the predetermined length in the first step. With this configuration, a step in which the width of the first region changes in accordance with the height position in which the height of the first region is reduced in the second etching step can be formed in the first etching step.
[0010] In the substrate processing method according to the first aspect, the first etching step preferably involves dry etching by the Bosch process, in which the periphery of the first region is etched so that the size of the concaves of the uneven scallops is reduced in the first step, and the periphery of the first region is etched so that the size of the concaves of the scallops is larger in the second step than in the first step, thereby forming a step in the first region. With this configuration, the width of the first region can be changed by adjusting the size of the scallops in the first and second steps, thereby easily forming a step.
[0011] In this case, preferably, in the first etching step, at least one of the etching time, pressure, gas flow rate, and coil applied power is made larger in the second step than in the first step, and the periphery of the first region is etched so that the size of the scallops is larger than in the first step. With this configuration, in the first etching step, at least one of the etching time, pressure, gas flow rate, and coil applied power is adjusted in the first and second steps to change the width of the first region, thereby making it easier to form a step.
[0012] In the substrate processing method according to the first aspect, the first region and the second region are preferably each processed into a comb-like shape in a plan view, and the teeth of the comb are processed so as to be alternately arranged. With this configuration, when the teeth of the comb are processed to have different heights, the formation of fence-like residues and shoulder chipping can be reliably suppressed, and the substrate can be accurately processed into comb-like shapes having different heights.
[0013] In order to achieve the above object, a substrate processing apparatus according to a second aspect of the present invention includes a processing chamber in which a substrate containing silicon is placed, a gas supply unit that supplies a gas for processing the substrate to the processing chamber, a plasma generating unit that converts the gas in the processing chamber into plasma, and a control unit that controls the gas supply unit and the plasma generating unit to control an etching process on the substrate, wherein the control unit controls the etching process to perform a first etching step of etching peripheries of a first region and a second region of the substrate placed in the processing chamber, and a second etching step of etching the first region such that a height of the first region is smaller than a height of the second region among the first region and the second region in a state in which the peripheries have been etched by the first etching step, and the first etching step includes a first step of etching the periphery of the first region so that the width of the first region has a first width, and a second step of etching the periphery of the first region so that after the first step, the width of the first region has a second width smaller than the first width, forming a step in the first region.
[0014] In the substrate processing apparatus according to the second aspect of the present invention, as described above, the first etching step includes a first step of etching the periphery of the first region so that the width of the first region has a first width, and a second step of etching the periphery of the first region so that the width of the first region has a second width smaller than the first width, forming a step in the first region. This makes it possible to increase the width of the upper part of the first region so as to form a step in the first etching step. As a result, even if a fence-shaped residue is formed in the upper part of the first region when the first region is etched in the second etching step, the first region cannot support the residue when the first region is etched up to the step part where the width is reduced, and the fence-shaped residue is removed. This makes it possible to reliably suppress the formation of the fence-shaped residue. Furthermore, even if a shoulder chip occurs in the upper part of the first region, the width is reduced when the first region is etched up to the step part where the width is reduced, so that the occurrence of a shoulder chip at the end can be suppressed. As a result, it is possible to provide a substrate processing apparatus capable of reliably suppressing the formation of a fence-shaped residue and the occurrence of a shoulder chip when a portion of a substrate whose periphery is etched is etched to reduce the thickness. Furthermore, since there is no need to precisely adjust the etching process conditions in order to adjust the balance between the effect of protecting the substrate by the protective film and the effect of removing the substrate by etching, a substrate processing apparatus can be provided that can prevent the work of setting the etching process conditions in the second etching process from becoming complicated. Effect of the Invention
[0015] According to the present invention, as described above, when a portion of a substrate whose periphery has been etched is etched to reduce its thickness, the formation of fence-shaped residue and the occurrence of shoulder chipping can be reliably suppressed. [Brief description of the drawings]
[0016] [Figure 1] 1 is a schematic diagram showing a schematic configuration of a substrate processing apparatus; [Diagram 2] FIG. 2 is a schematic plan view showing a processed comb-shaped substrate. [Diagram 3] 1A to 1C are schematic diagrams for explaining an overview of a substrate processing method. [Figure 4] 1A and 1B are schematic diagrams for explaining steps formed in etching a substrate. [Diagram 5] 1 is a table showing an example of processing conditions for forming a step in an etching process of a substrate. [Figure 6] 1A to 1C are schematic diagrams for explaining a state when a thickness of a portion of a substrate is reduced in an etching process. [Figure 7] FIG. 13 is a schematic diagram showing fence-shaped residues in a substrate etching process according to a comparative example. [Figure 8] FIG. 1 is a schematic diagram for explaining the formation of a fence-like residue. [Figure 9] FIG. 13 is a schematic diagram showing a shoulder chip in a substrate etching process according to a comparative example. [Figure 10] 1A to 1C are schematic views for explaining a first example of a substrate processing method. [Figure 11] FIG. 1 is a flow chart illustrating a first example of a substrate processing method. [Figure 12] 11A to 11C are schematic views for explaining a second example of the substrate processing method. [Figure 13] FIG. 11 is a flow chart illustrating a second example of the substrate processing method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.
[0018] A substrate processing apparatus 100 for performing a substrate processing method according to the present embodiment will be described with reference to FIG.
[0019] (Substrate processing equipment) As shown in FIG. 1, the substrate processing apparatus 100 is a plasma processing apparatus that forms plasma in a processing chamber 10 and performs dry etching on a substrate 200. The substrate 200 is a silicon wafer made of silicon. For example, as shown in FIG. 2, the substrate processing apparatus 100 processes the substrate 200 to have a comb-shaped comb-tooth electrode unit 201 (comb-tooth portion 201a, connecting portion 201b) and a comb-tooth electrode unit 202 (comb-tooth portion 202a, connecting portion 202b). Specifically, the comb-tooth portion 201a is formed in a first region 210 of the substrate 200, and the comb-tooth portion 202a is formed in a second region 220 of the substrate 200. The first region 210 and the second region 220 are each processed to have a comb-tooth shape in a plan view, and are processed so that the teeth of the comb are alternately arranged. Moreover, the comb tooth portion 201a in the first region 210 is formed to have a smaller height than the comb tooth portion 202a in the second region 220. Furthermore, the comb tooth portion 201a and the comb tooth portion 202a are in a state of being vertically floating with respect to the substrate 200. The substrate 200 on which the comb tooth electrode units 201 and 202 are formed is used in MEMS devices such as, for example, an acceleration sensor, a gyro sensor (angular velocity sensor), and a vibrating mirror.
[0020] The substrate processing apparatus 100 includes a processing chamber 10, a substrate mounting unit 20, a gas supply unit 30, a plasma generating unit 40, an exhaust unit 50, a high-frequency power supply 60, and a control unit 70. The processing chamber 10 is an example of a "processing chamber" in the claims. The gas supply unit 30 is an example of a "gas supply unit" in the claims. The plasma generating unit 40 is an example of a "plasma generating unit" in the claims.
[0021] The processing chamber 10 has a closed space and accommodates a substrate placement part 20 within the closed space. The processing chamber 10 is composed of an upper chamber 11 and a lower chamber 12 having internal spaces that communicate with each other. A substrate 200 containing silicon is placed in the processing chamber 10.
[0022] The substrate placement part 20 has a placement surface 20a on which the substrate 200 is placed. The substrate placement part 20 has a disk shape and includes a base 21, an electrostatic chuck 22 installed on the base 21, and a ring member 23 surrounding the periphery of the electrostatic chuck 22. The substrate placement part 20 is provided so as to be freely raised and lowered in the processing chamber 10 by a lifting cylinder 25. The electrostatic chuck 22 is connected to an electrostatic adsorption power source (not shown) that applies a voltage for electrostatic adsorption. When a voltage is applied to the electrostatic chuck 22, the substrate 200 is attracted to the placement surface 20a, which is the upper surface of the electrostatic chuck 22, by electrostatic induction. The substrate placement part 20 is provided with an internal pipe (not shown), and a chiller device (not shown) is attached to introduce a predetermined coolant into the internal pipe and circulate the coolant while controlling the temperature of the coolant (for example, at 10° C.). This cools the substrate placement part 20 during the execution of the plasma processing. During the plasma processing, a cooling gas (an inert gas such as He gas) is supplied to the rear surface of the substrate 200 from a predetermined cooling gas supply pipe (not shown), thereby cooling the substrate 200.
[0023] The gas supply device 30 supplies gases for processing the substrate 200 to the processing chamber 10. Specifically, the gas supply device 30 supplies an etching gas and a protective film forming gas into the processing chamber 10. The gas supply device 30 includes an SF6 gas supply unit 31 that supplies SF6 gas as an etching gas, and a C4F8 gas supply unit 32 that supplies C4F8 gas as a protective film forming gas. Each gas supply unit is connected to the inside of the processing chamber 10 from the top surface of the upper chamber 11 by a branched supply pipe 33 for gas supply. SF6 gas and C4F8 gas are supplied into the processing chamber 10 through the supply pipe 33.
[0024] The plasma generating device 40 converts the gas in the processing chamber 10 into plasma. Specifically, the plasma generating device 40 is a device that generates inductively coupled plasma (ICP) from the gas supplied into the processing chamber 10. The plasma generating device 40 includes a spiral coil 41 provided on the outer periphery of the upper chamber 11, and a high-frequency power supply 42 that supplies high-frequency power to the coil 41. The gas supplied into the upper chamber 11 is converted into plasma by supplying high-frequency power to the coil 41 by the high-frequency power supply 42.
[0025] The exhaust device 50 reduces the pressure in the processing chamber 10. The exhaust device 50 includes a vacuum pump 51 that exhausts gas from the processing chamber 10, and an exhaust pipe 52 that connects the vacuum pump 51 to the processing chamber 10. The vacuum pump 51 exhausts gas from the processing chamber 10 via the exhaust pipe 52, and sets the inside of the processing chamber 10 to a predetermined pressure state close to a vacuum.
[0026] The high frequency power supply 60 supplies high frequency power for a bias potential to the substrate mounting portion 20. The high frequency power supply 60 supplies high frequency power to the base 21 of the substrate mounting portion 20, thereby applying a bias potential between the substrate mounting portion 20 (base 21) and plasma.
[0027] The control unit 70 controls each part of the substrate processing apparatus 100. Specifically, the control unit 70 controls the gas supply unit 30 and the plasma generating unit 40 to control the etching process for the substrate 200.
[0028] (Outline of substrate processing method) Next, an outline of the substrate processing method of this embodiment will be described. As shown in Figures 3(A) to 3(D), the substrate processing method of this embodiment includes a first etching step of etching the peripheries of a first region 210 and a second region 220 of a substrate 200 containing silicon, and a second etching step of etching the first region 210 such that the height of the first region 210 is smaller than the height of the second region 220 among the first region 210 and the second region 220 in a state in which the peripheries are etched by the first etching step.
[0029] The periphery of the first region 210 and the second region 220 (portions etched in the first etching step) is a peripheral portion that does not include the connecting portion 201b connected to the first region 210 (comb tooth portion 201a) and the connecting portion 202b connected to the second region 220 (comb tooth portion 202a) in the example shown in Fig. 2. In other words, the periphery of the first region 210 and the second region 220 (portions etched in the first etching step) includes a portion (I) adjacent to the first region 210 (comb tooth portion 201a) and the second region 220 (comb tooth portion 202a) in the direction in which the first region 210 (comb tooth portion 201a) and the second region 220 (comb tooth portion 202a) face each other (Y direction). The periphery of the first region 210 and the second region 220 (the portion to be etched in the first etching step) includes a portion (II) adjacent to the tip surface (the end opposite the connecting portion 201b in the X direction) of the first region 210 (the comb tooth portion 201a) and a portion (III) adjacent to the tip surface (the end opposite the connecting portion 202b in the X direction) of the second region 220 (the comb tooth portion 202a). The first region 210 and the second region 220 are three-dimensional regions. That is, the first region 210 and the second region 220 are regions including dimensions in the depth direction (Z direction) in addition to the X direction and the Y direction (plane).
[0030] In the substrate processing method of this embodiment, the first etching process includes a first process of etching the periphery of the first region 210 so that the width of the first region 210 has a first width W1, as shown in Figures 3(B) and (C), and after the first process, a second process of etching the periphery of the first region 210 so that the width of the first region 210 has a second width W2 that is smaller than the first width W1, forming a step 230 on the side wall of the first region 210.
[0031] Specifically, as shown in FIG. 3(D), the second etching step etches the first region 210 so that the height of the first region 210 is smaller than the height of the second region 220 by a predetermined length L1. Also, as shown in FIG. 3(B), the first etching step etches the periphery of the first region 210 so that the width of the first region 210 has a first width W1 by a depth L2 corresponding to the predetermined length L1 in the first step. The length L1 etched in the second etching step (the amount by which the height of the first region 210 is shortened) is preferably, for example, about 1 to 1.1 times the depth L2 etched in the first step of the first etching step. That is, the length L1 is about 1 to 1.3 times the depth L2. Preferably, the length L1 is about 1 to 1.2 times the depth L1. More preferably, the length L1 is about 1 to 1.1 times the depth L2. Furthermore, for L1 and L2, average values on the surface of the substrate 200 may be used, or values on a portion of the substrate 200 where the amount of etching is large, or values on a portion of the substrate 200 where the amount of etching is small may be used.
[0032] In the first etching step, as shown in Fig. 4, the periphery of the first region 210 is etched by dry etching using the Bosch process so that the size D1 of the concave portion of the uneven scallop is reduced in the first step. In the second step, the periphery of the first region 210 is etched so that the size D2 of the concave portion of the scallop is larger than in the first step, thereby forming a step 230 on the side wall of the first region 210. Note that the size of the scallop in the first region 210 in Fig. 4 is exaggerated for the sake of explanation.
[0033] In the dry etching by the Bosch process, a process of forming a protective film, an anisotropic etching process, and an isotropic etching process are repeated multiple times. In the process of forming a protective film, C4F8 gas is supplied and plasma is generated by discharge to form a protective film on the substrate 200. In the anisotropic etching process, SF6 gas is supplied and plasma is generated by discharge. Then, ions in the plasma are collided with the substrate 200 to remove the protective film on the bottom surface. In the isotropic etching process, SF6 gas is supplied and plasma is generated by discharge. Then, radicals in the plasma react with silicon of the substrate 200 to isotropically etch the silicon in the portion where the protective film has been removed. Scallops are formed for each cycle of the process of forming a protective film, the anisotropic etching process, and the isotropic etching process. The number of cycles is set according to the depth to be etched.
[0034] In the first etching step, at least one of the etching time, pressure, gas flow rate, and coil power (coil applied power) is made larger in the second step than in the first step, and the periphery of the first region 210 is etched so that the size of the scallops is larger than in the first step. For example, as shown in FIG. 5, in the second step, the time of etching (Etch2) is made longer than in the first step, and the pressure of etching (Etch2) is made higher than in the first step. Here, in the etching process, in etching (Etch1), anisotropic etching is used to mainly remove the protective film on the bottom surface. In addition, in etching (Etch2), isotropic etching is used to progress etching to the side in addition to downward. In other words, by making the time of etching (Etch2) longer, etching to the side progresses more, and the size of the scallops becomes larger. Note that the gas flow rate in etching (Etch2) in the second step may be made larger than the gas flow rate in etching (Etch2) in the first step. Furthermore, the coil power (Coil RF) in the second etching step (Etch2) may be set to be greater than the coil power in the first etching step (Etch2).
[0035] 6, in the second etching step, when the height of the first region 210 in a state in which the step 230 has been formed in the first etching step is reduced, even if a fence-shaped residue is formed on the upper part of the first region 210, if the portion of the step 230 where the width is reduced is etched, the fence-shaped residue cannot be supported in the first region 210. This removes the fence-shaped residue.
[0036] On the other hand, when the height of a part of the substrate is reduced, if there is no step 230, and the protective film protects the substrate when etching in the Bosch process, as in the comparative example shown in FIG. 7, the substrate near the protective film is less likely to be etched, and a fence-like residue is formed at the end near the protective film in the region where the substrate height is reduced. Specifically, in FIG. 8(B), a protective film is formed on the substrate before processing shown in FIG. 8(A). Then, in FIG. 8(C), the protective film on the bottom surface is removed by anisotropic etching. Here, if the protective film is strong, the etching of the substrate (Si) near the protective film progresses more slowly. That is, in FIG. 8(D), the etching progresses more slowly at the end b near the protective film than at the center a. Specifically, during isotropic etching after the protective film removal (anisotropic etching), the center a reacts with radicals over the entire surface, whereas the end b near the protective film is less likely to etch the substrate (Si) because the protective film is attached thereto. For this reason, as shown in FIG. 8(E), a fence-like residue is formed on the end portion of the processed substrate close to the protective film.
[0037] Furthermore, as in the comparative example shown in FIG. 9, when the effect of etching the substrate during etching in the Bosch process is stronger than the effect of protecting the substrate by the protective film, the edge of the region where the height of the substrate is reduced by etching is scraped off, causing a shoulder chip.
[0038] (Substrate processing method (first example)) Next, a detailed description will be given of the substrate processing method of the present embodiment. As shown in Figures 10 and 11, the substrate processing method according to the first example of the present embodiment includes the following steps S1 to S9.
[0039] In step S1 of FIG. 11, as shown in FIG. 10(A), an oxide film (SiO2) 204 is formed on the surface (on silicon (Si) 203) of the substrate 200. The oxide film 204 is formed, for example, by a CVD method. In addition, in the substrate 200, a layer of silicon 203 is formed on a support substrate 208 via an insulating layer 207. That is, the silicon 203 is a silicon-on-insulator (SOI). In addition, the support substrate 208 may be attached after processing the silicon 203. In addition, the material of the support substrate 208 is not particularly limited. For example, the support substrate 208 may be formed of silicon or glass. In addition, a cavity (hollow) may be formed in the support substrate 208 or the insulating layer 207. That is, the silicon 203 may be a Cavity-SOI. In step S2, as shown in FIG. 10(B), a resist 205 is patterned in a position corresponding to the second region 220 of the substrate 200.
[0040] 10(C), the oxide film 204 is etched using the resist 205 as a mask to remove the oxide film 204 except for the resist 205 portion (the position corresponding to the second region 220). In step S4, the resist 205 is peeled off to remove the resist 205 from the position corresponding to the second region 220, as shown in FIG. 10(D).
[0041] In step S5, as shown in FIG. 10(E), a resist 206 is patterned in positions corresponding to the first region 210 and the second region 220 of the substrate 200.
[0042] In steps S6 and S7, as a first etching step, the silicon 203 is etched using the resist 206 as a mask, as shown in FIG. 10(F), to etch the periphery of the first region 210 and the second region 220.
[0043] Specifically, in step S6, as the first step of the first etching process, the scallops are controlled to be small, and silicon 203 is etched to a predetermined depth L2. That is, in the first step of the first etching process in step S6, the periphery of first region 210 is etched to a depth L2 corresponding to the predetermined length L1, so that first region 210 has a first width W1.
[0044] Then, in step S7, as the second step of the first etching step, etching of silicon 203 is performed while controlling so that the scallops become large.
[0045] In step S8, as shown in FIG. 10(G), the resist 206 is peeled off to remove the resist 206 from the positions corresponding to the first region 210 and the second region 220.
[0046] In step S9, as a second etching step, as shown in Fig. 10(H), the silicon 203 is etched using the oxide film 204 as a mask, thereby reducing the height of the first region 210.
[0047] That is, in the second etching step of step S9, the first region 210 is etched so that the height of the first region 210 is smaller than the height of the second region 220 by a predetermined length L1.
[0048] Thereafter, the insulating layer 207 (layer below the silicon 203) which will be the sacrificial layer is removed. The insulating layer 207 is, for example, an oxide film or a nitride film. As a result, the first region 210 and the second region 220 are formed in a comb-tooth shape. In addition, the oxide film 204 remaining as the etching mask is removed. Note that the oxide film 204 may be removed simultaneously with the insulating layer 207 (sacrificial layer).
[0049] (Substrate processing method (second example)) As shown in FIGS. 12 and 13, the substrate processing method according to the second example of the present embodiment includes the following steps S11 to S19.
[0050] In step S11 of FIG. 13, as shown in FIG. 12(A), an oxide film (SiO2) 204 is formed on the surface (on silicon (Si) 203) of the substrate 200. The oxide film 204 is formed, for example, by a CVD method. In addition, in the substrate 200, a layer of silicon 203 is formed on a support substrate 208 via an insulating layer 207. That is, the silicon 203 is a silicon-on-insulator (SOI). In addition, the support substrate 208 may be attached after processing the silicon 203. In addition, the material of the support substrate 208 is not particularly limited. For example, the support substrate 208 may be formed of silicon or glass. In addition, a cavity (hollow) may be formed in the support substrate 208 or the insulating layer 207. That is, the silicon 203 may be a cavity-SOI. In step S12, as shown in FIG. 12(B), a resist 205 is patterned in a position corresponding to the second region 220 of the substrate 200.
[0051] 12(C), the oxide film 204 is etched using the resist 205 as a mask to reduce the height of the oxide film 204 other than the resist 205 portion (the position corresponding to the second region 220). In step S14, the resist 206 is patterned at the positions corresponding to the first region 210 and the second region 220 of the substrate 200 as shown in FIG. 12(D).
[0052] In step S15, as shown in FIG. 12(E), the oxide film 204 is etched using the resist 206 as a mask to remove the oxide film 204 except for the resist 206 portions (positions corresponding to the first region 210 and the second region 220).
[0053] 12(F), silicon 203 is etched using oxide film 204 as a mask to etch the periphery of first region 210 and second region 220. Note that resist 206 may be peeled off and removed before etching silicon 203, or resist 206 may be left and used as a mask together with oxide film 204.
[0054] Specifically, in step S16, as the first step of the first etching process, the silicon 203 is etched to a predetermined depth L2 while controlling so that the scallops become small.
[0055] Then, in step S17, as the second step of the first etching step, etching of silicon 203 is performed while controlling so that the scallops become large.
[0056] In step S18, as shown in FIG. 12(G), the oxide film 204 is etched to remove the oxide film 204 from the first region 210.
[0057] In step S19, as a second etching step, as shown in Fig. 12(H), the silicon 203 is etched using the oxide film 204 as a mask, thereby reducing the height of the first region 210.
[0058] That is, in the second etching step of step S19, the first region 210 is etched so that the height of the first region 210 is smaller than the height of the second region 220 by a predetermined length L1.
[0059] Thereafter, the insulating layer 207 (layer below the silicon 203) which will be the sacrificial layer is removed. The insulating layer 207 is, for example, an oxide film or a nitride film. As a result, the first region 210 and the second region 220 are formed in a comb-tooth shape. In addition, the oxide film 204 remaining as the etching mask is removed. Note that the oxide film 204 may be removed simultaneously with the insulating layer 207 (sacrificial layer).
[0060] (Effects of this embodiment) In this embodiment, the following effects can be obtained.
[0061] In the substrate processing method of the present embodiment, as described above, the first etching step includes a first step of etching the periphery of the first region 210 so that the width of the first region 210 has a first width W1, and a second step of etching the periphery of the first region 210 so that the width of the first region 210 has a second width W2 smaller than the first width W1 after the first step, forming a step 230 in the first region 210. This makes it possible to increase the width of the upper part of the first region 210 so that the step 230 can be formed in the first etching step. As a result, even if a fence-shaped residue is formed in the upper part of the first region 210 when the first region 210 is etched in the second etching step, if the first region 210 is etched up to the step 230 where the width is reduced, the fence-shaped residue cannot be supported in the first region 210, and the fence-shaped residue is removed. This makes it possible to reliably suppress the formation of the fence-shaped residue. Furthermore, even if a chipped shoulder occurs at the top of the first region 210, when the etching reaches the portion of the step 230 where the width is reduced, the chipped shoulder at the end can be suppressed by the reduced width. As a result, when a portion of the substrate 200 whose periphery is etched is etched to reduce the thickness, the formation of fence-shaped residue and the chipped shoulder can be reliably suppressed. Furthermore, since there is no need to precisely adjust the etching conditions in order to adjust the balance between the function of protecting the substrate 200 by the protective film and the function of removing the substrate 200 by etching, the operation of setting the etching conditions can be prevented from becoming complicated.
[0062] In this embodiment, as described above, the second etching step etches the first region 210 so that the height of the first region 210 is smaller than the height of the second region 220 by a predetermined length L1, and the first etching step etches the periphery of the first region 210 by a depth L2 corresponding to the predetermined length L1 in the first step. This makes it possible to form in the first etching step a step 230 in which the width of the first region 210 changes in accordance with the height position where the height of the first region 210 is reduced in the second etching step.
[0063] In this embodiment, as described above, the first etching step is performed by dry etching using the Bosch process, in which the periphery of the first region 210 is etched so that the size D1 of the recesses of the uneven scallops is reduced in the first step, and the periphery of the first region 210 is etched so that the size D2 of the recesses of the scallops is larger than in the first step in the second step, thereby forming the step 230 in the first region 210. As a result, by adjusting the size of the scallops in the first and second steps, the width of the first region 210 can be changed and the step 230 can be easily formed.
[0064] In this embodiment, as described above, in the first etching step, at least one of the etching time, pressure, gas flow rate, and coil applied power is increased in the second step compared to the first step, and the periphery of the first region 210 is etched so that the size of the scallops is larger than in the first step. As a result, in the first etching step, at least one of the etching time, pressure, gas flow rate, and coil applied power is adjusted between the first and second steps to change the width of the first region 210 and more easily form the step 230.
[0065] In this embodiment, as described above, the first region 210 and the second region 220 are each processed into a comb-like shape in a plan view, and the teeth of the comb are processed so as to be arranged alternately with each other. This makes it possible to reliably suppress the formation of fence-like residues and shoulder chipping when processing the teeth of the comb to have different heights, and to accurately process the substrate 200 into comb-like shapes with different heights.
[0066] (Modification) The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The scope of the present invention is indicated by the claims, not by the description of the embodiments above, and further includes all modifications (variations) within the meaning and scope of the claims.
[0067] For example, in the above embodiment, an example was shown in which the substrate processing method was performed using the substrate processing apparatus 100 shown in Fig. 1, but the present invention is not limited thereto. The configuration of the substrate processing apparatus for performing the substrate processing method of the present invention is not particularly limited, and may be different from the configuration of the apparatus shown in Fig. 1.
[0068] In the above embodiment, the first etching step is configured to perform isotropic etching for a longer time and under a larger pressure in the second step than in the first step, but the present invention is not limited to this. In the present invention, other conditions in the second step of the first etching step may be set differently from those in the first step.
[0069] In the above embodiment, the substrate 200 to be processed is a Si substrate containing Si, but the present invention is not limited to this. In the present invention, the substrate 200 to be processed may be a SiGe substrate containing SiGe, or a SiC substrate containing SiC.
[0070] [Aspects] It will be appreciated by those skilled in the art that the exemplary embodiments described above are examples of the following aspects.
[0071] (Item 1) A first etching step of etching peripheries of a first region and a second region of a substrate including silicon; a second etching step of etching the first region such that a height of the first region is smaller than a height of the second region in the first and second regions whose peripheries have been etched by the first etching step; A substrate processing method, wherein the first etching step includes a first step of etching the periphery of the first region so that the width of the first region has a first width, and a second step of etching the periphery of the first region after the first step so that the width of the first region has a second width smaller than the first width, thereby forming a step in the first region.
[0072] (Item 2) the second etching step etches the first region such that a height of the first region is smaller than a height of the second region by a predetermined length; 2. The substrate processing method according to claim 1, wherein in the first etching step, a periphery of the first region is etched to a depth corresponding to the predetermined length.
[0073] (Item 3) 3. The substrate processing method according to item 1 or 2, wherein the first etching step etches the periphery of the first region by dry etching using a Bosch process so that in the first step, the size of the concaves of the uneven scallops is reduced, and in the second step, the periphery of the first region is etched so that the size of the concaves of the scallops is larger than in the first step, thereby forming a step in the first region.
[0074] (Item 4) 4. The substrate processing method according to item 3, wherein in the first etching step, at least one of an etching time, a pressure, a gas flow rate, and a coil applied power is made larger than in the first step, and the periphery of the first region is etched so that the size of the scallop is larger than in the first step.
[0075] (Item 5) 5. The substrate processing method according to any one of items 1 to 4, wherein the first region and the second region are each processed into a comb-like shape in a plan view, and the teeth of the comb are processed so as to be arranged alternately with each other.
[0076] (Item 6) a process chamber in which a silicon-containing substrate is disposed; a gas supply unit that supplies a gas for processing a substrate to the processing chamber; a plasma generating unit for generating plasma from a gas in the processing chamber; a control unit that controls the gas supply unit and the plasma generation unit to control an etching process for a substrate, the control unit controls an etching process to perform a first etching process for etching peripheries of a first region and a second region of the substrate placed in the processing chamber, and a second etching process for etching the first region such that a height of the first region is smaller than a height of the second region in the first and second regions in a state in which the peripheries are etched by the first etching process; the first etching step includes a first step of etching the periphery of the first region so that the width of the first region has a first width, and after the first step, a second step of etching the periphery of the first region so that the width of the first region has a second width smaller than the first width, forming a step in the first region. [Explanation of symbols]
[0077] 10: processing chamber (processing room), 30: gas supply device (gas supply section), 40: plasma generation device (plasma generation section), 70: control section, 100: substrate processing apparatus, 200: substrate, 210: first region, 220: second region, 230: step
Claims
1. a first etching step of etching peripheries of a first region and a second region of a substrate including silicon; a second etching step of etching the first region such that a height of the first region is smaller than a height of the second region in the first region and the second region in a state in which the periphery of the first region is etched by the first etching step; A substrate processing method, wherein the first etching process includes a first process of etching the periphery of the first region so that the width of the first region has a first width, and after the first process, a second process of etching the periphery of the first region so that the width of the first region has a second width smaller than the first width, thereby forming a step in the first region.
2. the second etching step etches the first region such that a height of the first region is smaller than a height of the second region by a predetermined length; 2. The substrate processing method according to claim 1, wherein in the first etching step, the periphery of the first region is etched to a depth corresponding to the predetermined length.
3. 2. The substrate processing method according to claim 1, wherein the first etching step is performed by dry etching using a Bosch process, the periphery of the first region being etched so that a size of a concave portion of an uneven scallop is reduced in the first step, and the periphery of the first region being etched so that a size of a concave portion of the scallop is larger in the second step than in the first step, thereby forming a step in the first region.
4. 4. The substrate processing method according to claim 3, wherein in the first etching step, the periphery of the first region is etched so that the size of the scallops is larger than that in the first step by increasing at least one of an etching time, a pressure, a gas flow rate, and a coil applied power in the second step compared to the first step.
5. 2 . The substrate processing method according to claim 1 , wherein the first region and the second region are each processed into a comb-like shape in a plan view, and are processed so that teeth of the comb are arranged alternately with each other.
6. a process chamber in which a silicon-containing substrate is disposed; a gas supply unit that supplies a gas for processing a substrate to the processing chamber; a plasma generating unit for generating plasma from a gas in the processing chamber; a control unit that controls the gas supply unit and the plasma generation unit to control an etching process for a substrate, the control unit controls an etching process to perform a first etching process for etching peripheries of a first region and a second region of the substrate placed in the processing chamber, and a second etching process for etching the first region such that a height of the first region is smaller than a height of the second region in the first and second regions in a state in which the peripheries are etched by the first etching process; The first etching process includes a first process of etching the periphery of the first region so that the width of the first region has a first width, and after the first process, a second process of etching the periphery of the first region so that the width of the first region has a second width smaller than the first width, forming a step in the first region.
Citation Information
Patent Citations
Micro movable element, wafer and wafer manufacturing method
JP2008246604A
Wafer processing method and substrate manufacturing method
JP2021100022A
Fine stereoscopic structure formation method, fine stereoscopic structure, plasma etching apparatus, and gas supply system
JP2022144645A
Method of detecting transparent objects
JP1977023381A