Boron nitride ceramic sheet sintered compact and production method thereof
A boron nitride ceramic sheet is produced with a sintering aid and precise filament layer formation to address disintegration, discoloration, and warpage issues, ensuring high durability and stability for severe handling.
Patent Information
- Application Number
- JP2023048735
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-07
AI Technical Summary
Conventional ceramic setters made of boron nitride are prone to disintegration, discoloration, and loss of brightness during firing, and suffer from warpage and poor durability, making them unsuitable for severe handling conditions such as dropping and multi-tier stacking.
A boron nitride ceramic sheet sintered body is manufactured by impregnating a sintering aid into a raw material paste containing boron nitride powder, forming a molded body with intersecting filament layers, and firing it using a boron nitride-containing jig to create a stable, uniformly colored, and bright ceramic sheet.
The resulting boron nitride ceramic sheet exhibits high durability, maintains brightness, and minimizes warpage, allowing it to withstand severe handling conditions without disintegration, enhancing the stability of fired objects.
Smart Images

Figure 2024137274000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a boron nitride ceramic sheet sintered body and a method for producing the same, and more specifically to a boron nitride ceramic sheet sintered body that does not collapse after firing, has sufficient brightness with little discoloration, and can withstand severe handling such as being dropped, and a method for producing the same. [Background technology]
[0002] When firing ceramic substrates, the object to be fired is generally placed on a setter, also called a shelf or base plate, and fired. In order to shorten the degreasing and firing time of the object to be fired and increase the number of pieces produced per unit time, it is necessary to heat and cool the firing process rapidly. However, when conventional ceramic setters are heated and / or cooled rapidly, defects such as cracks tend to occur. Furthermore, repeated use also tends to cause defects such as cracks. In addition, when a metal setter is used, there are problems that it cannot be used in an oxidizing atmosphere, and problems that it becomes significantly deformed when used repeatedly in high temperature ranges of 1200°C or higher have been pointed out.
[0003] A technique for preventing cracks and the like from occurring in a setter when a sintered object is rapidly heated and cooled is disclosed, for example, in Patent Document 1 (JP Patent Publication No. 2018-193274). Specifically, Patent Document 1 discloses a ceramic lattice having a plurality of first linear stripes made of ceramics and a plurality of second linear stripes made of ceramics intersecting the first linear stripes, in which only the apex of the convex curved portion of the first linear stripes and the apex of the downwardly convex circular or elliptical second linear stripes are in contact (so-called point contact) in a vertical cross-sectional view of the intersection. Also reported is a ceramic lattice having a plurality of first ceramic filament portions and a plurality of second ceramic filament portions intersecting the first ceramic filament portions, in which the first filament portions and the second filament portions are in contact with each other not as points but as surfaces at their respective contact locations.
[0004] Among the materials constituting ceramics, nitrides generally have desirable properties for use in firing processes, such as high thermal conductivity, low dielectric constant, low thermal expansion coefficient, etc. Therefore, nitrides such as boron nitride are expected to be materials that have the potential to be suitably used as ceramic setters for firing ceramic substrates and the like. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2018-193274 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, in the prior art, a ceramic lattice firing setter formed using boron nitride has not been specifically disclosed. The inventors have attempted to manufacture a ceramic lattice as a firing setter using boron nitride powder, but have found that it may have problems such as easily collapsing when the fired product is removed from the firing furnace. In addition, when a ceramic lattice is manufactured using boron nitride powder, discoloration may become significant or the brightness may decrease, so it has been found that there are problems in manufacturing a sintered body with a uniform color tone.
[0007] On the other hand, ceramic firing setters are often placed in conditions where they are subjected to strict handling, including dropping, and are often stored and transported on conveying devices such as conveyors and carts, or stacked in multiple layers. For example, when a firing setter is transported from a storage facility to another location over a step using a cart, if the physical durability of the firing setter is low, it may be damaged or collapsed due to a fall or the vibration of the cart. In addition, if the firing setter is significantly warped, not only will the stability be impaired when firing the object to be fired, but the setter may also be damaged or collapsed due to the vibration of the cart.
[0008] Here, for ceramic setters for firing, discoloration and loss of brightness after firing during the manufacture of the setter are correlated with a decrease in the physical strength and durability of the setter, so setters for firing that have discoloration and non-uniform color tone or loss of brightness after firing are likely to be damaged or disintegrated by being dropped or by the vibration of a dolly, etc. Therefore, it is desirable to obtain a ceramic setter for firing that has a uniform color tone with little discoloration after firing and sufficient brightness.
[0009] In addition, when a firing setter having a flat (plate) shape is significantly warped after firing, it is possible to reduce the warp and flatten it by grinding. However, when a firing setter for a ceramic lattice is significantly warped after firing, even if an attempt is made to flatten it by grinding, if the line width of the filament is narrow, there is a risk that the filament will be damaged due to stress, so such post-flattening is impossible. Therefore, when obtaining a ceramic firing setter, particularly a firing setter for a ceramic lattice, a boron nitride lattice with small warpage is desired immediately after the production (firing) of the ceramic lattice.
[0010] In view of these disadvantages of the conventional techniques, the first problem that the present invention aims to solve is to provide a boron nitride ceramic sheet sintered body that does not collapse after firing, has a uniform color tone with little discoloration after firing, and has sufficient brightness, and a method for producing the same. Furthermore, a second problem to be solved by the present invention is to provide a boron nitride ceramic sheet sintered body that does not collapse after firing, has a uniform color tone with little discoloration after firing, has sufficient brightness, and preferably has little warping after firing, and a manufacturing method thereof. [Means for solving the problem]
[0011] As a result of extensive research, the inventors unexpectedly discovered that by adding a sintering aid to a raw material paste containing boron nitride raw material powder to create a molded body for sintering, and then sintering the body using a sintering jig made of boron nitride, it is possible to produce a boron nitride ceramic sheet sintered body that does not collapse after sintering, has a uniform color tone with little discoloration after sintering, and has sufficient brightness, and thus completed the present invention. Furthermore, in one preferred embodiment, the present invention was completed based on the discovery that when firing a molded body made from a raw material paste containing boron nitride raw material powder, at least one boron nitride ceramic plate is placed on the molded body, thereby producing a boron nitride ceramic sheet sintered body with minimal warping after firing.
[0012] The various aspects included in the present invention are as follows. [1]. A method for producing a boron nitride ceramic sheet sintered body, comprising the steps of: (1) A molding process for producing a compact from a raw material paste containing raw material powder of boron nitride, a sintering aid, and a medium, A first stripe coated body having a plurality of stripes arranged at given intervals and each stripe being stretched in one direction; and A molding step of producing a molded body including a plurality of second linear coated bodies arranged at given intervals so as to be in contact with and cross each of the first linear coated bodies, each of which is stretched in one direction; and (2) A firing step of firing the molded body using a firing tool having a surface exposed to a firing atmosphere containing boron nitride to obtain a boron nitride ceramic sheet sintered body, This boron nitride ceramic sheet sintered body is A first striated portion layer including a plurality of first striated portions arranged at given intervals and each of the first striated portions extending in one direction; and A firing step including a second filament layer composed of a plurality of second filament sections each extending in one direction, the second filament sections being arranged at a given interval so as to contact and cross each of the first filament sections. A method for producing a boron nitride ceramic sheet sintered body, comprising: [2]. A boron nitride ceramic sheet sintered body, (i) a first striated portion layer composed of a plurality of first striated portions arranged at given intervals and each striated portion extending in one direction; and (ii) a second linear portion layer including a plurality of second linear portions arranged at given intervals so as to be in contact with and cross each of the first linear portions, each of which extends in one direction; The first filamentary layer and the second filamentary layer are integrally formed, The surface lightness L* of the boron nitride ceramic sheet sintered body is 80 or more. Sintered boron nitride ceramic sheet. Effect of the Invention
[0013] According to the boron nitride ceramic sheet sintered body and the manufacturing method thereof of the present invention, it is possible to obtain a boron nitride ceramic sheet sintered body that does not collapse after firing, has a uniform color tone with little discoloration, and has sufficient brightness. As described above, the occurrence of discoloration and a decrease in brightness after firing during the production of a fired product correlates with a decrease in the physical strength and durability of the fired product, but the boron nitride ceramic sheet sintered body obtained by the present invention has sufficient brightness and therefore can exhibit extremely high durability even when placed in conditions where it is subjected to severe handling, including being dropped, or when it is stored and transported on a table or stacked in multiple layers. According to a preferred embodiment of the boron nitride ceramic sheet sintered body and its manufacturing method of the present invention, a boron nitride ceramic sheet sintered body can be obtained that does not collapse after firing, has a uniform color tone with little discoloration, has sufficient brightness, and further has little warping after firing. By using a setter for firing a ceramic sheet sintered body with little warping, it is possible to greatly improve the stability when firing the object to be fired. The boron nitride ceramic sheet sintered body obtained by the present invention does not collapse after firing, has a uniform color tone with little discoloration, has sufficient brightness, and preferably also has little warping after firing, and can be suitably used as a ceramic setter for firing a ceramic substrate. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a schematic diagram showing the process of placing a boron nitride ceramic plate on a molded body including a plurality of first filamentary coated bodies and a plurality of second filamentary coated bodies and firing the molded body in a crucible, which is a firing jig containing boron nitride. [Diagram 2] FIG. 2 is a schematic diagram of a boron nitride ceramic sheet sintered body (setter for firing) according to one embodiment of the present invention. [Diagram 3] FIG. 3(a) is a perspective view showing a boron nitride ceramic sheet sintered body (setter for sintering) having a so-called point contact configuration according to one embodiment of the present invention, and FIG. 3(b) is a perspective view of the sintered body shown in FIG. 3(a) as seen from the opposite side. [Figure 4] FIG. 4 is a cross-sectional view taken along line II-II in FIG. [Diagram 5] FIG. 5 is a cross-sectional view taken along line III-III in FIG. [Figure 6] FIG. 6 is a cross-sectional view taken along line IV-IV in FIG. [Figure 7] FIG. 7 is a cross-sectional view taken along line VV in FIG. [Figure 8] FIG. 8 is a projection view of the vicinity of the intersection in the sintered body shown in FIG. 3, as viewed from the second linear portion side. [Figure 9] FIG. 9 is a projection view of the vicinity of the intersection in the sintered body shown in FIG. 3, as viewed from the first linear portion side. [Figure 10] FIG. 10 is a schematic diagram showing the shape of a through hole in the sintered body shown in FIG. [Figure 11] FIG. 11(a) is a perspective view showing a boron nitride ceramic sheet sintered body (setter for sintering) having a so-called surface contact configuration according to one embodiment of the present invention, and FIG. 11(b) is a perspective view of the sintered body shown in FIG. 11(a) as seen from the opposite side. [Figure 12] FIG. 12 is a cross-sectional view taken along line II-II in FIG. [Figure 13] FIG. 13 is a cross-sectional view taken along line III-III in FIG. [Figure 14] FIG. 14 is a cross-sectional view taken along line IV-IV in FIG. [Figure 15] FIG. 15 is a cross-sectional view taken along line VV in FIG. [Figure 16] FIG. 16 is a projection view of the vicinity of the intersection in the sintered body shown in FIG. 11, viewed from the second linear portion side. [Figure 17] FIG. 17 is a projection view of the vicinity of the intersection in the sintered body shown in FIG. 11, viewed from the first linear portion side. [Figure 18] FIG. 18 is a schematic diagram showing the shape of a through hole in the sintered body shown in FIG. [Figure 19] FIG. 19 is a photograph comparing the appearance of the sintered body obtained after firing in the example (normal appearance without discoloration) with the appearance of the sintered body obtained after firing in the comparative example (discolored). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] 1. Manufacturing method for sintered boron nitride ceramic sheet The method for producing a boron nitride ceramic sheet sintered body according to the present invention comprises: (1) a molding step of producing a molded body from a raw material paste containing raw material powder of boron nitride, a sintering aid, and a medium; and (2) a firing step of firing the molded body using a firing tool whose surface exposed to the firing atmosphere comprises boron nitride, to obtain a boron nitride ceramic sheet sintered body. These steps may be simply referred to as the molding step and the firing step in the following description.
[0016] In the molding process, a raw material paste containing boron nitride raw material powder, a sintering aid and a medium is used to create a molded body including a first linear coated body having multiple stripes arranged at given intervals and each stripe extending in one direction, and a second linear coated body having multiple stripes arranged at given intervals so as to be in contact with and intersect with each stripe of the first linear coated body, each stripe extending in one direction.
[0017] A boron nitride sintered body can be obtained by preparing a green body from a raw material paste using raw material powder of boron nitride in combination with a medium and a sintering aid, and then firing this green body under appropriate conditions.
[0018] Examples of the boron nitride raw powder used in the raw paste include hexagonal boron nitride powder, cubic boron nitride powder, and amorphous boron nitride powder. The average particle size of the boron nitride raw powder is preferably within the range of 0.1 to 50 μm. This average particle size is determined by the volume reference value D50 using a laser diffraction / scattering type particle size distribution measuring device. By having the average particle size of the boron nitride raw powder within the above range, it is possible to obtain a boron nitride ceramic sheet sintered body that has excellent structural strength and stability after firing.
[0019] Water is usually used as a medium for the raw material paste for producing the molded body. As a medium other than water, alcohol, acetone, ethyl acetate, etc. can also be used. Two or more of these media may be mixed. The mass ratio of the medium in the raw material paste may usually be 10 mass% or more and 60 mass% or less, and preferably 15 mass% or more and 55 mass% or less, based on the mass of the entire paste.
[0020] The raw material paste for producing the molded body contains a sintering aid. Well-known examples of sintering aids used in producing a boron nitride sintered body include, but are not limited to, silicon nitride, silicon carbide, boron, boron oxide, yttrium oxide, aluminum oxide, calcium fluoride, magnesium oxide, strontium oxide, calcium oxide, silicon, calcium boride, magnesium boride, magnesium oxide, boric acid, calcium carbonate, and the like. These sintering aids can be used alone or in combination of two or more. By using a sintering aid, it is possible to obtain a boron nitride ceramic sheet sintered body having excellent strength stability after firing. Among these sintering aids, it is preferable to use a boron compound (including boron simple substance) and a calcium compound from the viewpoint of sufficiently bonding the primary particles of boron nitride.
[0021] The mass ratio of the sintering aid to the boron nitride raw powder in the raw material paste may usually be 0.1 to 20%, and preferably 8 to 20%. By adding the sintering aid in the mass ratio to the boron nitride raw powder within the above range, it becomes possible to more easily obtain a boron nitride ceramic sheet sintered body that does not collapse after firing, has little discoloration, and has sufficient brightness.
[0022] The raw material paste may contain a binder. Examples of binders include, but are not limited to, polyvinyl alcohol, polyethylene glycol, polyethylene oxide, dextrin, sodium and ammonium lignin sulfonate, carboxymethylcellulose, ethylcellulose, hydroxypropylmethylcellulose, carboxymethylcellulose, hydroxyethylcellulose, hydroxyethylmethylcellulose, sodium and ammonium alginate, epoxy resin, phenolic resin, gum arabic, polyvinyl butyral, acrylic polymers such as polyacrylic acid and polyacrylamide, thickening polysaccharides such as xanthan gum and guar gum, gelling agents such as gelatin, agar and pectin, vinyl acetate resin emulsion, wax emulsion, and inorganic binders such as alumina sol and silica sol. Two or more of these may be mixed and used. The mass ratio of the binder in the raw material paste may be, for example, 0% by mass or more and 40% by mass or less, preferably 1% by mass or more and 40% by mass or less, and more preferably 3% by mass or more and 30% by mass or less, based on the total mass of the raw material paste.
[0023] The viscosity of the raw material paste is preferably high at the temperature during application of the filamentary coated body in order to successfully produce the filamentary coated body. The viscosity of the raw material paste is not particularly limited, but is preferably 1.5 MPa·s or more and 5.0 MPa·s or less, and more preferably 1.7 MPa·s or more and 3.0 MPa·s or less, at the temperature during application (typically room temperature such as about 25°C). The viscosity of the raw material paste here refers to the value measured 4 minutes after the start of measurement at a rotational speed of 0.3 rpm using a cone-plate type rotational viscometer or rheometer.
[0024] The raw material paste may contain a viscosity adjusting agent such as a thickening agent, a flocculating agent, or a thixotropic agent. Examples of thickeners include, but are not limited to, polyethylene glycol fatty acid esters, alkylarylsulfonic acid, alkylammonium salts, ethyl vinyl ether-maleic anhydride copolymers, fumed silica, proteins such as albumin, etc. In many cases, binders are classified as thickeners because they have a thickening effect, but when more precise viscosity adjustment is required, a thickener that is not classified as a binder can be used. Examples of the flocculant include, but are not limited to, polyacrylamide, polyacrylic acid ester, aluminum sulfate, polyaluminum chloride, etc. Examples of the thixotropic agent include fatty acid amide, polyolefin oxide, polyether ester type surfactant, etc.
[0025] In order to stabilize the amount of material discharged from the discharge device, the raw material paste may contain, for example, a plasticizer, a lubricant, a dispersant, a sedimentation inhibitor, a pH adjuster, and the like. Examples of the plasticizer include, but are not limited to, glycols such as trimethylene glycol and tetramethylene glycol, glycerin, butanediol, phthalic acids, adipic acids, and phosphoric acids. Examples of lubricants include, but are not limited to, hydrocarbons such as liquid paraffin, microwax, and synthetic paraffin, higher fatty acids, and fatty acid amides. Examples of dispersants include, but are not limited to, sodium or ammonium polycarboxylates, acrylic acid-based, polyethyleneimine, and phosphoric acid-based dispersants. Examples of the settling inhibitor include, but are not limited to, polyamide amine salts, bentonite, aluminum stearate, and the like. Examples of the pH adjuster include, but are not limited to, sodium hydroxide, aqueous ammonia, oxalic acid, acetic acid, and hydrochloric acid.
[0026] The raw material paste thus obtained is discharged from a discharge device onto a flat substrate to form a first linear coated body having a plurality of stripes arranged at given intervals and each stripe extending in one direction. The first linear coated body corresponds to the first linear portion of the boron nitride ceramic sheet sintered body. As the discharge device, various known devices such as a small extruder or a printer can be used. These discharge devices may typically be equipped with a dispenser having a nozzle. After the first striated coated body is discharged, the medium contained in the first striated coated body can be removed and dried to increase the viscosity. The medium can be removed by blowing hot air or irradiating infrared rays onto the first striated coated body. The ratio of the medium in the first striated coated body after the medium removal operation may be reduced to preferably 50% by mass or less, more preferably 30% by mass or less. By such a medium removal operation, the viscosity of the first striated coated body becomes extremely high, and its shape retention is further improved.
[0027] Next, using the raw material paste, a second filamentary coated body is formed, each filament extending in one direction, arranged at a given interval so as to contact and cross each filament of the first filamentary coated body. The second filamentary coated body corresponds to the second filamentary portion of the boron nitride ceramic sheet sintered body. The raw material paste for forming the second filamentary coated body may be the same as or different from the raw material paste for forming the first filamentary coated body, but it is more preferable that they are the same from the viewpoints of efficiency in forming the filamentary coated body and integrity of the structure and physical properties of the ceramic sheet sintered body to be produced.
[0028] The specific shapes of the first multiple filamentary coated body and the second multiple filamentary coated body formed as a molded body can be constructed to match the desired shape of a boron nitride ceramic sheet sintered body including a first filamentary layer composed of a plurality of first filament portions and a second filamentary layer composed of a plurality of second filament portions according to various embodiments described below.
[0029] In an additional embodiment, the raw material paste may be used to optionally form a plurality of third filamentary coated bodies, each of which is arranged at a given interval so as to be in contact with each stripe of the second filamentary coated body and intersect with the first filamentary coated body and the second filamentary coated body in a plan view, and each stripe is extended in one direction. The raw material paste for forming the optional third filamentary coated body may be the same as or different from the raw material paste for forming the first / second filamentary coated bodies, but it is more preferable that they are the same from the viewpoints of efficiency of forming the filamentary coated bodies and integrity of the structure and physical properties of the ceramic sheet sintered body to be produced.
[0030] The thus obtained molded body including the first filament coated body and the second filament coated body can be peeled off from the substrate and placed in a firing jig (firing furnace) for firing. The firing produces the desired boron nitride ceramic sheet sintered body. The obtained boron nitride ceramic sheet sintered body includes a first filament layer (a fired product of the first filament coated body) consisting of a plurality of first filament parts arranged at a given interval and stretched in one direction, and a second filament layer (a fired product of the second filament coated body) consisting of a plurality of second filament parts arranged at a given interval so as to be in contact with and intersect with each of the first filament parts and stretched in one direction. The boron nitride ceramic sheet sintered body including the first filament layer consisting of a plurality of first filament parts and the second filament layer consisting of a plurality of second filament parts is constructed as an integral structure by firing. Such construction of an integral structure of a sintered boron nitride ceramic sheet generally does not involve physical bonding of the individual components with an adhesive.
[0031] Firing may be performed in an air atmosphere (atmospheric pressure) or under pressure with an inert gas such as nitrogen, as necessary. The firing temperature may be selected appropriately depending on the type of raw powder of the ceramic material. The same applies to the firing time. Non-limiting examples of the firing temperature may be 500°C or higher, 800°C or higher, or 1000°C or higher, and 4000°C or lower, 3500°C or lower, or 3000°C or lower. Non-limiting examples of the firing time may be 30 minutes or more, 1 hour or more, or 2 hours or more, and 24 hours or less, 12 hours or less, or 6 hours or less.
[0032] In the firing process, an apparatus whose surface exposed to the firing atmosphere comprises boron nitride, and which is usually called a "firing furnace" or "firing kiln", is used. In this firing process, when firing is mainly performed in an inert atmosphere, a jig called a "crucible" is more preferably used to prevent contamination occurring within the apparatus. The crucible is usually composed of a storage body (forming a storage space for the material to be fired) and a furnace cover (lid body). In addition to the main body and the furnace cover, the crucible may have accessories such as a sealer. The outline of the storage space of the crucible is not particularly limited and may take various forms such as a cube, a rectangular parallelepiped, a cylinder, an elliptical cylinder, etc., but it is preferable that the inner bottom surface is substantially flat. The crucible may have an inlet for inert gas such as nitrogen.
[0033] The material of the member in the firing jig that includes the surface exposed to the firing atmosphere may contain elements other than boron nitride, for example, may contain a ceramic material other than the boron nitride raw powder that may be mixed in the raw paste described above. The material of the member in the firing jig that includes the surface exposed to the firing atmosphere may usually have a boron nitride content of 50 mass% or more, preferably 70 mass% or more, more preferably 90 mass% or more, and in one typical example, may be substantially 100 mass%. The surface of the storage body and furnace lid (cover body) of the firing jig such as a crucible exposed to the firing atmosphere at the furnace top may be made of the same material or different materials from the other parts. When a crucible is used as the firing jig, preferably, substantially all of the storage body and furnace lid (cover body) may be made of boron nitride. By using a firing tool whose surface exposed to the firing atmosphere contains boron nitride and whose component including the exposed surface has a boron nitride content of typically 50 mass% or more, and preferably 70 mass% or more, it becomes easy to produce a boron nitride ceramic sheet sintered body that does not collapse after firing, has a uniform color tone with little discoloration, and has sufficient brightness.
[0034] The carbon content in the firing jig (typically a crucible) may usually be in the range of 0 to 10% by mass, and preferably in the range of 0 to 3% by mass. The carbon content in the firing jig here is a value measured in accordance with JSS-152-19 using a carbon and sulfur simultaneous analyzer (CS-844) manufactured by LECO after crushing using an agate mortar. By having the carbon content in the firing jig within the above range, it becomes possible to more easily obtain a boron nitride ceramic sheet sintered body that has little discoloration after firing and has sufficient brightness.
[0035] In the step of firing a molded body including a plurality of first filamentary coated bodies and a plurality of second filamentary coated bodies, it is also preferable to place at least one boron nitride ceramic plate on the second filamentary coated body (or the third filamentary coated body if formed). By placing at least one boron nitride ceramic plate on the second filamentary coated body in this manner in the firing step of the molded body, it becomes possible to produce a boron nitride ceramic sheet sintered body in which warpage occurring after firing is effectively suppressed (warpage is sufficiently reduced).
[0036] The constituent material of the boron nitride ceramic plate used in the firing step may contain elements other than boron nitride, for example, ceramic materials other than the boron nitride raw material powder that may be mixed into the raw material paste described above. The material of the boron nitride ceramic plate may usually have a boron nitride content of 50 mass% or more, preferably 70 mass% or more, more preferably 90 mass% or more, and in one typical example, substantially 100 mass%. Preferably, substantially all of the ceramic plate may be formed from boron nitride. By using a ceramic plate that contains boron nitride and has a boron nitride content of usually 50 mass% or more, preferably 70 mass% or more, it becomes easier to manufacture a boron nitride ceramic sheet sintered body in which warping after firing is effectively suppressed (warping is sufficiently reduced).
[0037] The carbon content in the boron nitride ceramic plate may usually be in the range of 0 to 10% by mass, and preferably in the range of 0 to 3% by mass. The carbon content in the ceramic plate here is a value measured in accordance with JSS-152-19 using a carbon and sulfur simultaneous analyzer (CS-844) manufactured by LECO after crushing using an agate mortar. By having the carbon content in the ceramic plate within the above range, it becomes possible to more easily obtain a boron nitride ceramic sheet sintered body that has little discoloration after firing and has sufficient brightness.
[0038] The boron nitride ceramic plate used in the firing step of the molded body is not particularly limited, but from the viewpoint of applying an even load to the entire molded body and maximizing the effect of suppressing warping of the sintered body, it is more preferable that the plate has a substantially uniform thickness. The average thickness of one boron nitride ceramic plate is not particularly limited, but may be, for example, 1 mm or more and 20 mm or less, or 1.5 mm or more and 10 mm or less. The boron nitride ceramic plate may be used alone or in a plurality of layers, for example, 2 to 5 layers, stacked together. The average thickness range of the ceramic plate when stacked together may be the same as that exemplified above. The size of the boron nitride ceramic plate is not particularly limited, but it is desirable that the plate is large enough to cover substantially the entire second filamentary coated body (or the third filamentary coated body if formed) on which it is placed in order to apply a uniform load to the entire molded body. In one embodiment, the boron nitride ceramic plate may be large enough to cover about 90% or more of the second filamentary coated body (or the third filamentary coated body if formed) on which it is placed, preferably about 100% or more, and most preferably about 100%. In a preferred embodiment, the boron nitride ceramic plate and the second filamentary coated body (or the third filamentary coated body if formed) on which it is placed may have substantially the same shape and may be substantially the same size.
[0039] In the firing process, the pressure applied when placing the boron nitride ceramic plate on the second line-coated body (or the third line-coated body if formed) is usually 0.02 N / mm 2 It may be 1.0 N / mm or more and preferably 0.05 N / mm 2 More than 0.5N / mm 2 By controlling the pressure of the boron nitride ceramic plate within such a range, the effect of suppressing warping of the resulting sintered body can be further improved.
[0040] The pressure applied when the boron nitride ceramic plate is placed here means a value approximately calculated by the following method. After applying ink to the topmost filamentary portion of a molded body including a plurality of first filamentary coatings and a plurality of second filamentary coatings (and optionally a plurality of third filamentary coatings), a boron nitride ceramic plate (one or more) is placed on the molded body and the width of the ink-colored area on the plate is measured to estimate the contact width W (mm) between the topmost filamentary portion of the molded body and the plate. The contact area (mm ) between the topmost filament of the compact and the plate is calculated by multiplying the length L (mm), the number N, and the contact width W (mm) of the topmost filament of the compact. 2 ) to calculate Calculate the load F (unit: Newton, N) from the total mass of the boron nitride ceramic plate (one or more plates) by unit conversion. The load F (N) is calculated by dividing the contact area (mm 2 ) to obtain the applied pressure (unit: N / mm 2 ) can be calculated.
[0041] Fig. 1 shows a schematic diagram of a process in which a boron nitride ceramic plate is placed on a molded body containing a first filamentary coated body and a second filamentary coated body in a crucible, which is a firing jig containing boron nitride. In Fig. 1, 1 is a crucible, which is a firing jig containing boron nitride, 1a is a main body of the crucible (a storage section for the material to be fired), 1b is a furnace cover (a lid) of the crucible, 2 is a first filamentary coated body, 3 is a second filamentary coated body arranged so as to perpendicularly intersect with the first filamentary coated body of 2 (a structural example in which a stack of the first filamentary coated body of 2 and the first filamentary coated body of 3 are combined in two stages), 4 is a stack of boron nitride ceramic plates (weights), and 4a and 4b are each a boron nitride ceramic plate. Although not shown, this crucible is designed to enable firing under atmospheric pressure, and may be provided with an inlet for inert gas such as nitrogen gas in the main body or the lid.
[0042] 2. Sintered boron nitride ceramic sheet The boron nitride ceramic sheet sintered body according to the present invention is (i) a first striated portion layer composed of a plurality of first striated portions arranged at given intervals and each striated portion extending in one direction; and (ii) a second linear portion layer including a plurality of second linear portions arranged at given intervals so as to be in contact with and cross each of the first linear portions, each of which extends in one direction; The first filamentary layer and the second filamentary layer are integrally formed, The surface of the boron nitride ceramic sheet sintered body has a lightness L* value of 80 or more.
[0043] The boron nitride ceramic sheet sintered body can be produced by, but is not limited to, combining one or more of the embodiments of the production method described above.
[0044] The given spacing between each of the filaments of the multiple first filament portion may be designed to be at least partially different or substantially equal when the first filament portion is composed of three or more filaments, i.e., when there are two or more spacings. In addition, when the second filamentary portion is composed of three or more filaments, i.e., when there are two or more intervals, the given intervals between the filaments may be designed to be at least partially different or substantially equal. The given intervals between the filaments of the first filamentary portion and the given intervals between the filaments of the second filamentary portion may be designed independently of each other.
[0045] The above-mentioned first filamentary layer and the second filamentary layer being integrally formed means that the group of filaments constituting the first filamentary layer and the group of filaments constituting the second filamentary layer are sintered and connected at their contact points to form an integral structure and are formed in such a way that they cannot be easily separated. In one embodiment, the first filamentary layer and the second filamentary layer are formed such that the filaments constituting the first filamentary layer and the filaments constituting the second filamentary layer are sintered and connected to each other at their contact points to form an integral structure and are not easily separated, and the first filamentary layer and the second filamentary layer, or different portions of each filamentary layer, may be formed from a single composition. In another embodiment, the first filamentary layer and the second filamentary layer are formed such that the filaments constituting the first filamentary layer and the filaments constituting the second filamentary layer are sintered and connected to each other at the contact points to form an integral structure and cannot be easily separated, and the first filamentary layer and the second filamentary layer, or different portions of each filamentary layer, may be formed from a plurality of different compositions.
[0046] The lightness L* value of the surface of the boron nitride ceramic sheet sintered body may be 80 or more, preferably 85 or more, more preferably 90 or more, even more preferably 92 or more, and most preferably 95 or more. A boron nitride ceramic sheet sintered body having such a high lightness L* value on the surface can exhibit extremely high durability even when placed in conditions of severe handling, including being dropped, or when stored and transported in multiple layers. The lightness of the sintered body surface here is the lightness L* of CIE1976, and the lightness L* can be obtained by measuring the XYZ coordinates under geometric condition c using the SCI method including regular reflection (specular reflection) light using the D65 light source, which is considered as the standard light, in accordance with JIS Z8722 (2009), and converting them into L*a*b* coordinates. A commercially available spectrophotometer (a typical example of the device is the spectrophotometer "CM-600d" manufactured by Konica Minolta) can be used to measure the lightness L*.
[0047] In a preferred embodiment, the warpage rate per unit length, calculated by dividing the amount of warpage at the longest part of the main surface of the boron nitride ceramic sheet sintered body by the length of the longest part, is typically 5×10 -3 The warpage rate is preferably 4.5×10 -3 mm / mm or less, more preferably 4×10 -3 mm / mm or less, and even more preferably 3.5×10 -3 mm / mm or less, and even more preferably 3×10 -3 mm / mm or less, and even more preferably 2.5×10 -3 mm / mm or less, and most preferably 2×10-3 By using a ceramic sheet sintered body with such small warpage as a firing setter, it is possible to significantly improve the stability when firing an object to be fired (such as a ceramic substrate).
[0048] Specifically, the warpage rate here can be calculated as follows when the boron nitride ceramic sheet sintered body has a substantially rectangular shape in a plan view. With a metal ruler placed against one diagonal of a boron nitride ceramic sheet sintered body, the amount of warping of the other diagonal that is the longest is measured using a gap gauge. The amount of warping (mm) at the diagonal with the larger value is divided by the length of the diagonal (maximum length) to calculate the "Maximum warping ratio = amount of warping / maximum length (mm / mm)".
[0049] In a preferred embodiment, the boron nitride ceramic sheet sintered body may be one that does not crack when it is held above the SUS plate at a position 20 mm from the plate surface in a substantially parallel state and then dropped. It is more preferable that the boron nitride ceramic sheet sintered body is one that does not crack when it is held above the SUS plate at a position 25 mm from the plate surface in a substantially parallel state and then dropped, and it is even more preferable that it is one that does not crack when it is held above the SUS plate at a position 30 mm from the plate surface in a substantially parallel state and then dropped. In this way, by being one that does not crack when it is held above the SUS plate at a position 20 mm or more from the plate surface in a substantially parallel state and then dropped, the boron nitride ceramic sheet sintered body can have sufficient strength and durability even under severe handling conditions such as dropping.
[0050] The boron nitride ceramic sheet sintered body may, in addition to a first filament layer composed of a plurality of first filament portions and a second filament layer composed of a plurality of second filament portions, optionally include a third filament layer composed of a plurality of third filament portions, each of which extends in one direction and is arranged at given intervals so as to be in contact with each filament of the second filament portion and intersect with the first filament portions and the second filament portions.
[0051] Specific structural examples of the boron nitride ceramic sheet sintered body of the present invention are given below, but these are merely examples and the boron nitride ceramic sheet sintered body is not limited to these. Those skilled in the art will be able to modify or change part of these specific structural examples as necessary, or combine part or all of a plurality of structural examples to the extent possible.
[0052] Structural example 1 of boron nitride ceramic sheet sintered body In one embodiment, the boron nitride ceramic sheet sintered body is configured as a ladder-shaped sintered body (sintering setter) that forms a first striated layer (support layer) consisting of two striated bodies (supports) extending approximately parallel to each other at a given interval, and a second striated layer consisting of a plurality of striated bodies extending approximately parallel to each other at a given interval on the first striated layer so as to intersect with the two striated bodies of the first striated layer as both ends. Such a ladder-shaped sintered body is formed by integrally firing the first striated layer and the second striated layer.
[0053] An example of the sintered body (sintering setter) of Structural Example 1 is illustrated in Fig. 2. In Fig. 2, 5 denotes a ceramic sheet sintered body, 6 (6a and 6b) denote lines constituting the first striated layer, and 7 denotes lines constituting the second striated layer. Here, each line constituting the second striated layer is disposed approximately perpendicular to each line (i.e., each support) constituting the first striated layer. The cross-sectional shape of each filament of the first filament layer and the second filament layer may be a circle, an ellipse, a triangle, a rectangle, etc., and is not particularly limited. When the cross-sectional shape of each filament is a circle, an ellipse, a triangle, or a rectangle, the filaments form a cylinder, an elliptical cylinder, a triangular prism, or a quadrangular prism. For example, as shown in FIG. 2, each filament constituting the second filament layer and each filament constituting the first filament layer may be formed in a cylindrical shape except for the bottom, and the bottom of each filament constituting the first filament layer may form a flat surface. The thickness of the first filament layer and the second filament layer is not particularly limited, and may be, for example, 0.5 mm or more and 5 mm or less. The thickness of the first filament layer and the second filament layer may be substantially the same or different. From the viewpoint of structural strength and stability, the thickness of the first filament layer constituting the bottom of the sheet sintered body of Structural Example 1 may be greater than the thickness of the second filament layer.
[0054] As one modified embodiment, when each filament of the sintered body (sintering setter) of Structural Example 1 forms a square pillar as illustrated in FIG. 2, one of the two filaments (supports) of the first filament layer of one sintered body is a longitudinal side a and the corresponding end faces b1 to b2 of each filament of the second filament layer arranged substantially perpendicularly thereon. x and one of the longitudinal side surfaces ac of the two filaments (supports) of the first filament layer of the other sintered body and the corresponding end surfaces b of each filament of the second filament layer arranged thereon. 1c ~b xc Between the end faces b1 to b2, the side face a and the side face ac are joined to each other. x and end face b 1c ~b xc The sintered body may have a structure in which two or three or more sintered bodies are bonded to each other and integrally joined together.
[0055] Structural example 2 of boron nitride ceramic sheet sintered body: Lattice (mesh) sintered body In a preferred embodiment, the boron nitride ceramic sheet sintered body has, at any intersection between the first and second striated portions, a cross section of the first striated portion having a shape composed of a straight portion and a convex curved portion having both ends of the straight portion as ends, and the cross section of the second striated portion having a circular or elliptical shape, and further, when viewed in vertical cross section at the intersection, a configuration in which only the apex of the convex curved portion of the first striated portion and the downwardly convex apex of the circle or ellipse of the second striated portion are in contact (a so-called point contact configuration).
[0056] An example of a boron nitride ceramic sheet sintered body (sintering setter) having such a so-called point contact configuration is illustrated in FIG. 3. A boron nitride ceramic sheet sintered body 11 (hereinafter, simply referred to as "ceramic sheet sintered body 11") shown in FIG. 3(a) and FIG. 3(b) has a plurality of first linear stripes 20 made of ceramic extending in one direction X. Each of the first linear stripes 20 is straight and extends parallel to each other. The ceramic sheet sintered body 11 also has a plurality of second linear stripes 30 made of ceramic extending in a Y direction different from the X direction. Each of the second linear stripes 30 is straight and extends parallel to each other. Since the X direction and the Y direction are different directions, the first linear stripes 20 and the second linear stripes 30 cross each other. The crossing angle between the two linear stripes 20, 30 can be set according to the specific application of the ceramic sheet sintered body 11. For example, the crossing angle of the second linear portion 30 with respect to the first linear portion 20 can be set to 90 degrees. Alternatively, the crossing angle of the second linear portion 30 with respect to the first linear portion 20 can be changed within a range of 90 degrees ± 10 degrees. The ceramic sheet sintered body 11 is formed by the crossing of a plurality of first linear portions 20 and a plurality of second linear portions 30.
[0057] The ceramic sheet sintered body 11 has a plate-like shape in which a lattice is formed by the intersection of first linear portions 20 and second linear portions 30, and the lattice defines a plurality of through holes 13. As shown in Fig. 4, the ceramic sheet sintered body 11 has a first surface 11a and a second surface 11b facing the first surface 11a.
[0058] The ceramic sheet sintered body 11 has intersections 12 at locations where each of the first linear portions 20 intersects with each of the second linear portions 30. The intersections 12 are locations where the first linear portions 20 and the second linear portions 30 overlap with each other in a projected image of the ceramic sheet sintered body 11 in a plan view.
[0059] The first linear portion 20 has a constant width W1 (see FIG. 4) in plan view at a position other than the intersection 12 of both linear portions 20, 30. The cross-sectional shape of the first linear portion 20 along the thickness direction in a direction perpendicular to the longitudinal direction is defined by a first surface 20a located on the first surface 11a side of the ceramic sheet sintered body 11 and a second surface 20b located on the second surface 11b side of the ceramic sheet sintered body 11, as shown in FIG. 4 and FIG. 5. In detail, the cross-section of the first linear portion 20 along the thickness direction in a direction perpendicular to the longitudinal direction has a shape composed of a straight portion 20A and a convex curved portion 20B having both ends of the straight portion 20A as ends at a position other than the intersection 12. As a result, the first surface 20a of the first linear portion 20 has a cross-section along the thickness direction of the linear portion 20 as a flat surface. The flat surface is approximately parallel to the in-plane direction of the ceramic sheet sintered body 11. On the other hand, the second surface 20b of the first linear portion 20 has a cross section in the thickness direction of the linear portion 20 that has a convex curved shape extending from the first surface 11a to the second surface 11b of the ceramic sheet sintered body 11.
[0060] Like the first linear portion 20, the second linear portion 30 also has a constant width W2 (see FIG. 7) in plan view at a position other than the intersection 12 of both linear portions 20, 30. The width W2 may be the same as the width W1 of the first linear portion 20, or may be different. The cross-sectional shape of the second linear portion 30 along the thickness direction in a direction perpendicular to the longitudinal direction is defined by a first surface 30a located on the first surface 11a side of the ceramic sheet sintered body 11 and a second surface 30b located on the second surface 11b side of the ceramic sheet sintered body 11, as shown in FIG. 6 and FIG. 7. The first surface 30a of the second linear portion 30 has a convex curved shape extending from the second surface 11b of the ceramic sheet sintered body 11 toward the first surface 11a. On the other hand, the second surface 30b of the second linear portion 30 has a cross section in the thickness direction of the linear portion 30 that is convexly curved from the first surface 11a to the second surface 11b of the ceramic sheet sintered body 11. This curved shape may be the same as or different from the curved shape of the first linear portion 20. The first surface 30a and the second surface 30b of the second linear portion 30 are symmetrical, and as a result, the cross section of the second linear portion 30 along the thickness direction in a direction perpendicular to the longitudinal direction may be circular or elliptical.
[0061] 5 and 6, when the straight line portion 20A of the first linear portion 20, i.e., the first surface 20a, is placed on a plane P as a placement surface, all of the first surfaces 20a are located on the plane P. Since the first surfaces 20a form the first surfaces 21a of the ceramic sheet sintered body 11, the fact that all of the first surfaces 20a are located on the plane P means that the first surface 11a of the ceramic sheet sintered body 11 is a flat surface. Therefore, when the ceramic sheet sintered body 11 is placed so that the first surface 11a is in contact with a flat placement surface, the entire area of the first surface 11a is in contact with the placement surface.
[0062] 5, when the straight line portion 20A of the first linear portion 20, i.e., the first surface 20a, is placed on a plane P as a placement surface, the second linear portion 30 has a shape that is spaced apart from the plane P between two adjacent intersections 12. Therefore, a space S is formed between the second linear portion 30 and the plane P between the two adjacent intersections 12.
[0063] On the other hand, the second surface 11b of the ceramic sheet sintered body 11 is formed from the second surface 30b of the second linear portion 30, which has a convex curved shape, as shown in Figure 6, and is therefore not a flat surface but an uneven surface.
[0064] At the intersection 12 between the first linear portion 20 and the second linear portion 30 in the ceramic sheet sintered body 11, the two linear portions 20, 30 are integrated. "Integrated" means that, when observing the cross section of the intersection 12, the two linear portions 20, 30 form a continuous ceramic structure. Each through hole 13 formed in the ceramic sheet sintered body 11 by the intersection of the two linear portions 20, 30 has the same size and shape. Each through hole 13 is approximately rectangular. The through holes 13 are regularly arranged.
[0065] 3, 5 and 6, at each intersection 12 between the first linear portion 20 and the second linear portion 30, the second linear portion 30 is disposed on the first linear portion 20. That is, at each intersection 12 between the first linear portion 20 and the second linear portion 30, the second linear portion 30 is disposed on the first linear portion 20 located relatively closer to the first surface 11a of the two surfaces 11a and 11b of the ceramic sheet sintered body 11. The thickness at the intersection 12 is larger than both the thickness of the first linear portion and the thickness of the second linear portion at the portions other than the intersection. That is, when the thickness of the first linear portion 20 at a position other than the intersection 12 of both linear portions 20, 30 is T1 (see FIG. 4), the thickness of the second linear portion 30 at a position other than the intersection 12 of both linear portions 20, 30 is T2 (see FIG. 7), and the thickness at the intersection is Tc (see FIG. 5 and FIG. 6), Tc>T1 and Tc>T2. Therefore, on the second surface 11b of the ceramic sheet sintered body 11, the intersection of both linear portions 20, 30 is the highest. The thickness Tc of the intersection 12 is also the thickness of the ceramic sheet sintered body 11.
[0066] As shown in Fig. 6, in the first linear portion 20, the highest position of the second surface 20b of the first linear portion 20, i.e., the position of the apex, is the same along the extension direction of the first linear portion 20 at the intersections 12 and at other positions. As for the second linear portion 30, as shown in Fig. 5, the highest positions of the second surfaces 30b of the second linear portion 30 are the same along the extension direction of the first linear portion 20 at the intersections 12 and other positions. The lowest positions of the first surfaces 30a of the second linear portion 30 are the same along the extension direction of the second linear portion 30 at the intersections 12 and other positions.
[0067] 5 and 6, when the intersection 12 of the ceramic sheet sintered body 11 is viewed in vertical cross section, the first linear portion 20 and the second linear portion 30 are in contact only at the apex of the convex curved portion 20B of the first linear portion 20 and the apex of the downwardly convex curve of the circle or ellipse of the second linear portion 30, i.e., the apex of the first surface 30a. In other words, the first linear portion 20 and the second linear portion 30 are in point contact or surface contact close to point contact. Such contact between the first linear portion 20 and the second linear portion 30 enhances the spalling resistance of the ceramic sheet sintered body 11. This is believed to be because the first linear portion 20 and the second linear portion 30 are bonded through point contact or surface contact close thereto, so that the two linear portions 20, 30 are unlikely to be bonded too strongly, and volume change that occurs during rapid heating and / or cooling due to this can be mitigated. From this viewpoint, the intersection 12 is in a point contact state such that its thickness Tc is preferably 0.5 to 1.0, more preferably 0.8 to 1.0, and even more preferably 0.9 to 1.0, relative to the sum (T1+T2) of the thickness T1 of the first linear portion 20 at a position other than the intersection 12 and the thickness T2 of the second linear portion 30 at a position other than the intersection 12.
[0068] The ceramic sheet sintered body 11 is composed of one layer of a first linear portion 20 and one layer of a second linear portion 30. When the ceramic sheet sintered body 11 is composed of n layers of the first linear portion 20 and m layers of the second linear portion 30 (n and m are each independently an integer of 1 or more, but n and m are not both 1 at the same time), the intersection 12 is in a point contact state such that the thickness T of the ceramic sheet sintered body 11 is preferably 0.5 or more and 1.0 or less, more preferably 0.8 or more and 1.0 or less, and even more preferably 0.9 or more and 1.0 or less, relative to (nT1+mT2).
[0069] As shown in FIG. 3(a) and FIG. 8, the width W2a of the projected image of the second linear portion 30 in plan view at the intersection 12 is approximately the same as the width W2b of the projected image in plan view at a portion other than the intersection 12, or is slightly larger than W2b. In detail, the second linear portion 30 (i) has a contour along the longitudinal direction of the projected image in plan view that is approximately straight lines 31, 31 at the intersection 12, or (ii) has a very gentle convex curve (not shown) toward the outside in the width direction X. In the case of (ii), the contour along the longitudinal direction of the projected image of the second linear portion 30 in plan view has a maximum width portion having a width W2a, and the width gradually decreases as it moves away from the maximum width portion, and becomes the width W2b at a position between the intersections 12. The width W2b is the same as the width W2 described above. W2a is preferably 1 to 1.5 times W2b, more preferably 1 to 1.3 times, and even more preferably 1 to 1.1 times.
[0070] On the other hand, as shown in Fig. 3(b) and Fig. 9, the width W1a of the projected image at the intersection 12 in plan view of the first linear portion 20 is approximately the same as the width W1b of the projected image at a portion other than the intersection 12 in plan view, or is slightly larger than W1b. In detail, the first linear portion 20 (i) has a contour along the longitudinal direction of the projected image in plan view that is approximately straight lines 21, 21 at the intersection 12, or (ii) has a very gentle convex curve (not shown) toward the outside in the width direction Y. In the case of (ii), the contour along the longitudinal direction of the projected image of the first linear portion 20 in plan view has a maximum width portion having a width W1a, and the width gradually decreases as it moves away from the maximum width portion, and becomes width W1b at a position between the intersections 12. The width W1b is the same as the width W1 described above. W1a is preferably 1 to 1.5 times W1b, more preferably 1 to 1.3 times, and even more preferably 1 to 1.1 times W1b.
[0071] FIG. 10 shows a plan view of the ceramic sheet sintered body 11. As shown in the figure, the ceramic sheet sintered body 11 has a plurality of through holes 13 that are substantially rectangular in plan view of the lattice body, with the plurality of first linear stripes 20 and the plurality of second linear stripes 30 being substantially perpendicular to each other. The substantially rectangular through hole 13 has a first side 13a, 13a that is a pair of opposing sides. In addition, the through hole 13 has a second side 13b, 13b that is another pair of opposing sides. The first side 13a, 13a is a side that corresponds to both side edges of the first linear stripe 20. On the other hand, the second side 13b, 13b is a side that corresponds to both side edges of the second linear stripe 30. The through hole 13 is defined by these four sides. The opposing first sides 13a, 13a are straight lines that extend parallel to each other. Similarly, the opposing second sides 13b, 13b are also straight and extend parallel to each other. Since the first linear portion 20 and the second linear portion 30 have the above-mentioned substantially straight shape at their intersection 12, the through hole 13 formed by the first linear portion 20 and the second linear portion 30 intersecting substantially at right angles has a rectangular shape with corners 40 at substantially right angles, as shown in the schematic diagram of FIG.
[0072] When the ceramic sheet sintered body 11 having the above configuration is used as a setter for firing an object to be fired, the first surface 11a of the ceramic sheet sintered body 11 is flat, and the object to be fired is placed on the first surface 11a of the ceramic sheet sintered body 11. The first surface 11a is flat, and is suitable for placing the object to be fired that requires flatness. Examples of the object to be fired that require flatness include ceramic substrates made of boron nitride. In addition, the object to be fired is in contact with only the first linear portion 20, which is a member constituting the first surface 11a, so that the contact area between the ceramic sheet sintered body 11 and the object to be fired is greatly reduced, and this makes it easier to rapidly heat and cool the object to be fired. In addition, the ceramic sheet sintered body 11 is formed by the intersection of the first and second linear portions 20 and 30, and has a plurality of through holes 13, so that the thermal capacity is small, and from this point of view, it is easy to rapidly heat and cool the object to be fired. Furthermore, the ceramic sheet sintered body 11 has good air permeability due to the presence of a plurality of through holes 13, which also facilitates rapid cooling of the sintered body. The good air permeability is further enhanced by the fact that the second linear portions 30 are floating between the adjacent intersections 12. Moreover, in the ceramic sheet sintered body 11, the first and second linear portions 20, 30 are integrated at the intersections 12, so that the ceramic sheet sintered body 11 has sufficient strength.
[0073] In order to make the above-mentioned various advantageous effects more prominent, the value of T1 is preferably 50 μm or more and 3 mm or less, and more preferably 100 μm or more and 2 mm or less. On the other hand, the value of T2 is preferably 50 μm or more and 3 mm or less, and more preferably 100 μm or more and 2 mm or less. There is no particular restriction on the magnitude relationship between the values of T1 and T2, and T1 may be greater than T2, or conversely, T1 may be greater than T2. <T2であってもよく、あるいはT1=T2であってもよい。
[0074] From the same viewpoint, the thickness Tc at the intersection 12 is preferably 20 μm or more and 5 mm or less, and more preferably 50 μm or more and 2 mm or less, provided that the thickness Tc is preferably 0.5 or more and 1.0 or less with respect to (T1+T2).
[0075] Furthermore, when the cross-sectional shape in the thickness direction of the second linear portion 30 (see FIG. 7) is elliptical, it is preferable that the minor axis of the ellipse coincides with the thickness direction of the ceramic sheet sintered body 11 and the major axis of the ellipse coincides with the planar direction of the ceramic sheet sintered body 11, in order to ensure that the object to be sintered can be placed successfully. In this case, the major axis / minor axis ratio is preferably 1 to 5, and more preferably 1 to 3. Furthermore, the fact that the cross-sectional shape in the thickness direction of the second linear portion 30 is elliptical or circular also contributes to improving the strength of the ceramic sheet sintered body 11.
[0076] The through-hole 13 formed in the ceramic sheet sintered body 11 has an area of 100 μm 2 More than 100mm 2 Below, especially 2500μm 2 More than 1mm 2 It is preferable that the ratio of the total area of the through holes 13 to the apparent area of the ceramic sheet sintered body 11 in a plan view is 1% or more and 80% or less, more preferably 3% or more and 70% or less, and even more preferably 10% or more and 70% or less. This ratio is calculated by cutting the ceramic sheet sintered body 11 into a rectangle of any size in a plan view, calculating the total area of the through holes 13 contained in the rectangle, dividing the total by the area of the rectangle, and multiplying by 100. The area of each through hole 13 can be measured by image analysis of a microscope observation image of the ceramic sheet sintered body 11.
[0077] In relation to the area of the through-hole 13, the width W1 of the first linear portion 20 is preferably 50 μm or more and 4 mm or less, and more preferably 75 μm or more and 2 mm or less. On the other hand, the width W2 of the second linear portion 30 is preferably 50 μm or more and 4 mm or less, and more preferably 75 μm or more and 2 mm or less. There is no particular restriction on the magnitude relationship between the values of W1 and W2, and W1 may be greater than W2, or conversely, W1 may be greater than W2. <W2であってもよく、あるいはW1=W2であってもよい。
[0078] In relation to the widths W1, W2 of the first and second linear portions 20, 30, the pitch P1, which is the gap (space) between adjacent first linear portions 20, is preferably 0.1 mm to 10 mm, more preferably 0.15 mm to 5 mm. On the other hand, the pitch P2 between adjacent second linear portions 30 is preferably 0.1 mm to 10 mm, more preferably 0.15 mm to 5 mm.
[0079] As a modified embodiment (not shown) of this structural example, the sintered body may use three or more types of linear portions, such as a third linear portion, a fourth linear portion, and a fifth linear portion in addition to the first linear portion and the second linear portion. When using three or more types of linear portions, it is preferable that the linear portions after the third linear portion have the same configuration as the first and second linear portions as described above in terms of thickness T1, width W1, and pitch P1. It is also preferable that the configuration of the intersection formed by the linear portions after the third linear portion has the same configuration as the intersection formed by the first and second linear portions as described above. As another modified embodiment (not shown), the sintered body may be laminated in a plurality of stages. In this embodiment, for example, in the case of a two-stage laminate, the first filament portion of one sintered body and the first filament portion of the other sintered body may be arranged at the same pitch, and the second filament portion of one sintered body and the second filament portion of the other sintered body may be arranged at the same pitch.
[0080] Structural examples 3a and 3b of boron nitride ceramic sheet sintered body: lattice (mesh) sintered body In one embodiment, the boron nitride ceramic sheet sintered body may have a structure in which the first striated portion has a cross section consisting of a straight portion and a convex curved portion having both ends of the straight portion as ends at a portion other than the intersection between the first striated portion and the second striated portion, the cross section of the second striated portion has a circular or elliptical shape at a portion other than the intersection, and the first striated portion and the second striated portion form an intersection where they are in contact with each other not at a single point but over a surface (Structural Example 3a). This structure may be called a surface contact structure as opposed to the above-mentioned so-called point contact.
[0081] In a preferred embodiment corresponding to a sub-concept of the above Structural Example 3a based on such surface contact, the boron nitride ceramic sheet sintered body has a cross section of the first striated portion that has a shape consisting of a straight portion and a convex curved portion having both ends of the straight portion as ends at a portion other than the intersection between the first striated portion and the second striated portion, and has a cross section of the second striated portion that has a circular or elliptical shape at a portion other than the intersection, and further, the projected image of the second striated portion in a plan view has a shape that is curved and bulged outward in the width direction at the intersection, so that the width of the projected image at the intersection is larger than the width of the projected image at the portions other than the intersection (Structural Example 3b). That is, the boron nitride ceramic sheet sintered body of Structural Example 3a by surface contact includes those that do not have the configuration of Structural Example 3b (subordinate concept) in which "the projected image of the second striated portion in a plan view is curved and bulged outward in the width direction at the intersection, and the width of the projected image at the intersection is larger than the width of the projected image at the intersection. In this case, the boron nitride ceramic sheet sintered body of Structural Example 3a by surface contact has a configuration in which the projected image of the second striated portion in a plan view is not curved and bulged outward in the width direction at the intersection, and the width of the projected image at the intersection is substantially the same as the width of the projected image at the intersection.
[0082] An example of the boron nitride ceramic sheet sintered body of Structural Example 3b will be described below with reference to the drawings. The boron nitride ceramic sheet sintered body 41 (hereinafter, simply referred to as the "ceramic sheet sintered body 41") shown in FIG. 11(a) and FIG. 11(b) has a plurality of first linear portions 50 made of ceramic extending in one direction X. Each of the first linear portions 50 is straight and extends parallel to each other. The ceramic sheet sintered body 41 also has a plurality of second linear portions 60 made of ceramic extending in a Y direction different from the X direction. Each of the second linear portions 60 is straight and extends parallel to each other. Since the X direction and the Y direction are different directions, the first linear portions 50 and the second linear portions 60 intersect. The intersection angle between the linear portions 50 and 60 can be set according to the specific application of the ceramic sheet sintered body 41.
[0083] The ceramic sheet sintered body 41 has a plate-like shape in which a lattice is formed by the intersection of first linear portions 50 and second linear portions 60, and the lattice defines a plurality of through holes 43. The ceramic sheet sintered body 41 has a first surface 41a and a second surface 41b facing the first surface 41a.
[0084] The ceramic sheet sintered body 41 has intersections 42 at locations where the first linear portions 50 and the second linear portions 60 intersect. The intersections 42 are locations where the first linear portions 50 and the second linear portions 60 overlap in a projected image of the ceramic sheet sintered body 41 in a plan view.
[0085] The first linear portion 50 has a constant width W1 (see FIG. 12) in plan view at a position other than the intersection 42 of both linear portions 50, 60. The cross-sectional shape of the first linear portion 50 along the thickness direction in a direction perpendicular to the longitudinal direction is defined by a first surface 50a located on the first surface 41a side of the ceramic sheet sintered body 41 and a second surface 50b located on the second surface 41b side of the ceramic sheet sintered body 41, as shown in FIG. 12 and FIG. 13. In detail, the cross-section of the first linear portion 50 along the thickness direction in a direction perpendicular to the longitudinal direction has a shape composed of a straight portion 50A and a convex curved portion 50B having both ends of the straight portion 50A as ends at a position other than the intersection 42. As a result, the first surface 50a of the first linear portion 50 has a cross-section along the thickness direction of the linear portion 50 as a flat surface. The flat surface is approximately parallel to the in-plane direction of the ceramic sheet sintered body 41. On the other hand, the second surface 50b of the first linear portion 50 has a cross section in the thickness direction of the linear portion 50 that has a convex curved shape extending from the first surface 41a to the second surface 41b of the ceramic sheet sintered body 41.
[0086] Like the first linear portion 50, the second linear portion 60 has a constant width W2 (see FIG. 15) in plan view at a position other than the intersection 42 of both linear portions 50, 60. The width W2 may be the same as the width W1 of the first linear portion 50, or may be different. The cross-sectional shape of the second linear portion 60 along the thickness direction in a direction perpendicular to the longitudinal direction is defined by a first surface 60a located on the first surface 41a side of the ceramic sheet sintered body 41 and a second surface 60b located on the second surface 41b side of the ceramic sheet sintered body 41, as shown in FIG. 14 and FIG. 15. The first surface 60a of the second linear portion 60 has a convex curved shape extending from the second surface 41b of the ceramic sheet sintered body 41 toward the first surface 41a. On the other hand, the second surface 60b of the second linear portion 60 has a cross section in the thickness direction of the linear portion 60 that is convexly curved from the first surface 41a to the second surface 41b of the ceramic sheet sintered body 41. This curved shape may be the same as or different from the curved shape of the first linear portion 50. In this embodiment, the first surface 60a and the second surface 60b of the second linear portion 60 are symmetrical, and as a result, the cross section of the second linear portion 60 along the thickness direction in a direction perpendicular to the longitudinal direction is circular or elliptical.
[0087] 13 and 14, when the straight line portion 50A of the first linear portion 50, i.e., the first surface 50a, is placed on a plane P as a placement surface, all of the first surfaces 50a are located on the plane P. Since the first surfaces 50a form the first surfaces 41a of the ceramic sheet sintered body 41, the fact that all of the first surfaces 50a are located on the plane P means that the first surfaces 41a of the ceramic sheet sintered body 41 are flat surfaces. Therefore, when the ceramic sheet sintered body 41 is placed so that the first surfaces 41a are in contact with a flat placement surface, the entire area of the first surfaces 41a is in contact with the placement surface.
[0088] 13, when the straight line portion 50A of the first linear portion 50, i.e., the first surface 50a, is placed on a plane P as a placement surface, the second linear portion 60 has a shape that is spaced apart from the plane P between two adjacent intersections 42. Therefore, a space S is formed between the second linear portion 60 and the plane P between the two adjacent intersections 42.
[0089] On the other hand, the second surface 41b of the sintered ceramic sheet 41 is configured from the second surface 60b of the second linear portion 60 having a convex curved shape, and therefore is not a flat surface but an uneven surface.
[0090] At the intersection 42 between the first linear portion 50 and the second linear portion 60 in the ceramic sheet sintered body 41, the two linear portions 50, 60 are integrated. "Integrated" means that, when observing the cross section of the intersection 42, the two linear portions 50, 60 form a continuous ceramic structure. Each through hole 43 formed in the ceramic sheet sintered body 41 by the intersection of the two linear portions 50, 60 has the same size and shape. Each through hole 43 is approximately rectangular. The through holes 43 are regularly arranged.
[0091] 11, 13 and 14, at each intersection 42 between the first linear portion 50 and the second linear portion 60, the second linear portion 60 is disposed on the first linear portion 50. That is, at each intersection 42 between the first linear portion 50 and the second linear portion 60, the second linear portion 60 is disposed on the first linear portion 50 located relatively closer to the first surface 41a of the two surfaces 41a and 41b of the ceramic sheet sintered body 41. The thickness at the intersection 42 is larger than both the thickness of the first linear portion and the thickness of the second linear portion at the portions other than the intersection. That is, when the thickness of the first linear portion 50 at a position other than the intersection 42 of both linear portions 50, 60 is T1 (see FIG. 12), the thickness of the second linear portion 60 at a position other than the intersection 42 of both linear portions 50, 60 is T2 (see FIG. 15), and further the thickness at the intersection is Tc (see FIGS. 13 and 14), Tc>T1 and Tc>T2. Therefore, on the second surface 41b of the ceramic sheet sintered body 41, the position of the intersection of both linear portions 50, 60 is the highest.
[0092] As shown in Fig. 14, in the first linear portion 50, the highest position of the second surface 50b of the first linear portion 50, i.e., the position of the apex, is the same along the extension direction of the first linear portion 50 at the intersection 42 and at other positions. As for the second linear portion 60, as shown in Fig. 13, the highest positions of the second surfaces 60b of the second linear portion 60 are the same along the extension direction of the first linear portion 50 at both the intersection 42 and other positions. The lowest positions of the first surfaces 60a of the second linear portion 60 are the same along the extension direction of the second linear portion 60 at the intersection 42 and other positions.
[0093] As shown in FIG. 11(a) and FIG. 16, the second linear portion 60 has a projected image in a plan view that is curved and bulged outward in the width direction X at the intersection 42. As a result, the width W2a of the projected image at the intersection 42 is larger than the width W2b of the projected image at a portion other than the intersection 42 (the embodiment of the above structural example 3a includes a case where such an expansion in width does not occur). In detail, the second linear portion 60 has a contour along the longitudinal direction of the projected image in a plan view that draws gentle convex curves 61, 61 outward in the width direction X at the intersection 42. The contour along the longitudinal direction of the projected image of the second linear portion 60 in a plan view has a maximum width portion having a width W2a, and the width gradually decreases as it moves away from the maximum width portion, and becomes width W2b at a position between the intersections 42. The width W2b is the same as the width W2 described above.
[0094] On the other hand, as shown in FIG. 11(b) and FIG. 17, the first linear portion 50 has a projected image in plan view that is curved and bulged outward in the width direction Y at the intersection 42. As a result, the width W1a of the projected image at the intersection 42 is larger than the width W1b of the projected image at the portion other than the intersection 42 (the embodiment of the above-mentioned structural example 3a includes a case where such an expansion in width does not occur). In detail, the first linear portion 50 has a contour along the longitudinal direction of the projected image in plan view that draws gentle convex curves 51, 51 outward in the width direction Y at the intersection 42. The contour along the longitudinal direction of the projected image of the first linear portion 50 in plan view has a maximum width portion having a width W1a, and the width gradually decreases as it moves away from the maximum width portion, and becomes width W1b at a position between the intersections 42. The width W1b is the same as the width W1 described above.
[0095] FIG. 18 shows a plan view of the ceramic sheet sintered body 41. As shown in the figure, the ceramic sheet sintered body 41 has a plurality of through holes 43 that are substantially rectangular in plan view, as a result of the plurality of first linear portions 50 and the plurality of second linear portions 60 being substantially perpendicular to each other. The substantially rectangular through hole 43 has a first side 43a, 43a that is a pair of opposing sides. In addition, the through hole 43 has a second side 43b, 43b that is another pair of opposing sides. The first side 43a, 43a is a side that corresponds to both side edges of the first linear portion 50. On the other hand, the second side 43b, 43b is a side that corresponds to both side edges of the second linear portion 60. The through hole 43 is defined by these four sides. The opposing first sides 43a, 43a are straight lines that extend parallel to each other. Similarly, the opposing second sides 43b, 43b are also straight and extend parallel to each other. Since the first linear portion 50 and the second linear portion 60 have the above-mentioned curved bulging shape at the intersection 42 thereof, the through hole 43 formed by the first linear portion 50 and the second linear portion 60 intersecting at substantially right angles has a slightly rounded rectangular corner 70 as shown in the schematic diagram of Fig. 18 (the embodiment of the above structural example 3a includes the case where the corners of the through hole are substantially right angles).
[0096] When the ceramic sheet sintered body 41 having the above configuration is used, for example, as a firing setter for a sintered body, the strength and spalling resistance are improved due to the rounded corners 70 of the rectangular through-holes 43. The reason for this is that, although the corners 70 of the through-holes 43 are the parts of the ceramic sheet sintered body 41 where defects such as cracks are most likely to occur, cracks are less likely to occur at the corners 70 due to the rounded corners 70.
[0097] The above-mentioned improvement in strength and spalling resistance is sufficiently achieved if at least the second filamentary portion 60 has the above-mentioned convex curve 61 on the outline along the longitudinal direction of the projected image in a plan view at the intersection 42 between the first filamentary portion 50 and the second filamentary portion 60. In particular, if both the first filamentary portion 50 and the second filamentary portion 60 have the above-mentioned convex curves 51, 61 on the outline along the longitudinal direction of the projected image in a plan view, the strength and spalling resistance are further improved.
[0098] As described above, the ceramic sheet sintered body 41 of this embodiment has one flat surface and the other uneven surface, which is advantageous in that the mounting surface can be selected depending on the type of body to be sintered.
[0099] In order to make the above-mentioned various advantageous effects more prominent, the value of T1 is preferably 50 μm or more and 3 mm or less, and more preferably 100 μm or more and 2 mm or less. On the other hand, the value of T2 is preferably 50 μm or more and 3 mm or less, and more preferably 100 μm or more and 2 mm or less. There is no particular restriction on the magnitude relationship between the values of T1 and T2, and T1 may be greater than T2, or conversely, T1 may be greater than T2. <T2であってもよく、あるいはT1=T2であってもよい。
[0100] From the same viewpoint, the thickness Tc at the intersection 42 is preferably 0.1 mm or more and 2 mm or less, and more preferably 0.3 mm or more and 1.5 mm or less. The thickness Tc at the intersection 42 is smaller than T1+T2, which is the sum of T1 and T2.
[0101] Furthermore, when the cross-sectional shape in the thickness direction of the second linear portion 60 (see FIG. 15) is elliptical, it is preferable that the minor axis of the ellipse coincides with the thickness direction of the ceramic sheet sintered body 41 and the major axis of the ellipse coincides with the planar direction of the ceramic sheet sintered body 41, in order to facilitate the placement of the object to be fired. In this case, the major axis / minor axis ratio is preferably 1 to 5, and more preferably 1 to 3. Furthermore, the fact that the cross-sectional shape in the thickness direction of the second linear portion 60 is elliptical or circular also contributes to improving the strength of the ceramic sheet sintered body 41.
[0102] The through-holes 43 formed in the ceramic sheet sintered body 41 have an area of 100 μm 2 More than 100mm 2 Below, especially 2500μm 2 More than 1mm 2 It is preferable that the total area of the through holes 43 is 1% or more and 80% or less in terms of reducing the heat capacity of the sintered ceramic sheet 41, improving the breathability, and maintaining the strength of the sintered ceramic sheet 41. Moreover, the ratio (this value) of the total area of the through holes 43 to the apparent area of the sintered ceramic sheet 41 in a plan view is preferably 1% or more and 80% or less, more preferably 3% or more and 70% or less, and even more preferably 10% or more and 70% or less. The method of calculating and measuring this ratio is as described above.
[0103] In relation to the area of the through-hole 43, the width W1 of the first linear portion 50 is preferably 50 μm or more and 4 mm or less, and more preferably 75 μm or more and 2 mm or less. On the other hand, the width W2 of the second linear portion 60 is preferably 50 μm or more and 4 mm or less, and more preferably 75 μm or more and 2 mm or less. There is no particular restriction on the magnitude relationship between the values of W1 and W2, and W1 may be greater than W2, or conversely, W1 may be greater than W2. <W2であってもよく、あるいはW1=W2であってもよい。
[0104] In relation to the widths W1, W2 of the first and second linear portions 50, 60, the pitch P1, which is the gap between adjacent first linear portions 50, is preferably 0.1 mm to 10 mm, more preferably 0.15 mm to 5 mm. On the other hand, the pitch P2 between adjacent second linear portions 60 is preferably 0.1 mm to 10 mm, more preferably 0.15 mm to 5 mm.
[0105] As a modified embodiment (not shown) of this structural example, the sintered body may use three or more types of linear portions, such as a third linear portion, a fourth linear portion, and a fifth linear portion in addition to the first linear portion and the second linear portion. When using three or more types of linear portions, it is preferable that the linear portions after the third linear portion have the same configuration as the first and second linear portions as described above in terms of thickness T1, width W1, and pitch P1. It is also preferable that the configuration of the intersection formed by the linear portions after the third linear portion has the same configuration as the intersection formed by the first and second linear portions as described above. As another modified embodiment (not shown), the sintered body may be laminated in a plurality of stages. In this embodiment, for example, in the case of a two-stage laminate, the first filament portion of one sintered body and the first filament portion of the other sintered body may be arranged at the same pitch, and the second filament portion of one sintered body and the second filament portion of the other sintered body may be arranged at the same pitch.
[0106] Structural example 4 of boron nitride ceramic sheet sintered body: Lattice (mesh) sintered body In one embodiment, the boron nitride ceramic sheet sintered body may have a first filamentary portion having a cross section that is shaped at a location other than the intersection of the first filamentary portion and the second filamentary portion and is composed of a straight portion and a convex curved portion having both ends of the straight portion as ends, and the second filamentary portion having a cross section that is circular or elliptical at a location other than the intersection of the first filamentary portion and the second filamentary portion, and the sintered body may have a straight side portion in at least a part of its outline in a plan view, and the first filamentary portion and the second filamentary portion may each independently intersect with this straight side portion (outer side) at an angle of 10 degrees or more and 170 degrees or less (i.e., within a wide angle range including an angle that is not a right angle).
[0107] The sintered body according to this embodiment has a rectangular outline having opposing first and second sides and opposing third and fourth sides, and the first and second linear portions may intersect with the first and second sides independently at an angle of 10 degrees or more and 170 degrees or less. This sintered body may have a contact form in which the first and second filamentary portions are in so-called surface contact, as in the above structural example 3a or 3b, or may further have a configuration in which the projected image of the second filamentary portion in a plan view is curved and bulged outward in the width direction at the intersection between the first and second filamentary portions, so that the width of the projected image at the intersection is larger than the width of the projected image at the other locations. Also, instead of or in addition to such a configuration of the second filamentary portion, this sintered body may have a projected image of the first filamentary portion in a plan view is curved and bulged outward in the width direction at the intersection between the first and second filamentary portions, so that the width of the projected image at the intersection is larger than the width of the projected image at the other locations. This sintered body may have a shape such that when the straight line portions of the first linear portions are placed on a plane as a placement surface, the second linear portions are spaced from the plane between two adjacent intersections.
[0108] Structural example 5 of boron nitride ceramic sheet sintered body: Lattice (mesh) sintered body In one embodiment, the boron nitride ceramic sheet sintered body may be a plate-shaped ceramic structure having, in addition to a plurality of first linear portions and a plurality of second linear portions, a plurality of third linear portions made of ceramic passing on the diagonals of a quadrilateral defined by the intersection of the first linear portions and the second linear portions, and having a plurality of triangular through holes defined by the first linear portions, the second linear portions and the third linear portions.
[0109] The sintered body according to this structural example may be configured such that the first line portion, the second line portion, and the third line portion intersect at one intersection portion. In this sintered body, each of the filamentary portions of the filamentary portion layers constituting the upper two layers may have a circular or elliptical cross section at locations other than the intersections. The sintered body may have a straight side portion in at least a part of the outline in a plan view, and any one of the first, second and third linear portions may be arranged parallel to the straight side portion. Also, the sintered body may have the first or third linear portion arranged parallel to the straight side portion. This sintered body may form a structure in which two or more repeating units each consisting of a first striated portion, a second striated portion and a third striated portion are laminated. EXAMPLES
[0110] Example 1: Production example of mesh-shaped boron nitride sheet sintered body As the raw powder of boron nitride, a mixture of 40.0 parts of cubic boron nitride powder with an average particle size of 8.0 μm and 60.0 parts of cubic boron nitride powder with an average particle size of 13.0 μm was used. As the sintering aid, a mixture of 100 parts of powdered boron and 60 parts of calcium carbonate was used. Then, 14 parts of the sintering aid were mixed with 100 parts of the raw powder of boron nitride. 15.0 parts of hydroxypropyl methylcellulose, 2.5 parts of glycerin, 5.0 parts of polycarboxylic acid dispersant, and 60.0 parts of water were mixed with 100 parts of this mixture, and degassed to prepare a raw paste. In addition, the amounts and ratios of substances in the examples refer to numerical values by mass unless otherwise specified.
[0111] Using a dispenser with a nozzle having a diameter of 1.4 mm, a molded body consisting of a filamentary coated body, which is a four-layer lattice body of the above-mentioned so-called point contact form, was formed from the raw material paste prepared as described above. The four-layer lattice molded body had a structure (similar to the structure illustrated in FIG. 1) in which two laminates of a first filamentary coated body and a second filamentary coated body perpendicularly crossed each other were stacked so that the openings were aligned. After the first filamentary coated body was formed, hot air was blown using a dryer to remove water and dry the first filamentary coated body until the water content of the first filamentary coated body reached 10%, after which a second filamentary coated body was formed. In addition, after the second filamentary coated body was formed, hot air was blown using a dryer to remove water and dry the second filamentary coated body until the water content of the second filamentary coated body reached 8%. The four-layer lattice compact thus obtained was degreased and fired for 4 hours at 2000°C under normal pressure in a crucible of a firing jig entirely made of boron nitride and having a carbon content of 1.0% by mass. During firing, a weight of a boron nitride ceramic plate having a size of 50 mm length x 50 mm width x 2.0 mm thickness x 2 sheets, a total thickness of 4.0 mm, and a carbon content of 1.0% by mass was placed on the compact. In this way, a four-layer mesh-like boron nitride sheet of so-called point contact form was produced, having a size of 50 mm x 50 mm, a pitch of 0.5 mm, a width of the striated part of 1.2 mm, and a total thickness of 3.0 mm after firing.
[0112] Example 2: Production example of mesh-shaped boron nitride sheet sintered body Except for placing a boron nitride ceramic plate weight measuring 50 mm length x 50 mm width x 2.0 mm thickness x 1 sheet, with a total thickness of 2.0 mm, on the molded body instead of the above weight, firing was carried out in the same manner as in Example 1 above, to produce a four-layer mesh-like boron nitride sheet with a so-called point contact configuration, with a size of 50 mm x 50 mm, a pitch of 0.5 mm, a width of 1.2 mm for the linear portion, and a total thickness of 3.0 mm after firing.
[0113] Method for converting the pressure of the boron nitride plate (weight plate) in Examples 1 and 2 The pressure caused by placing a boron nitride ceramic plate during firing was calculated as follows. The mass of one boron nitride ceramic plate was 8g, so the load for one plate was 78.5N, and for two plates was 156.9N. Ink was applied to the filamentous portion at the top of the molded body, and then a weight was placed on the boron nitride ceramic plate. The width of the ink-colored area on the plate was measured to estimate the contact width W (mm) between the filamentous portion at the top of the molded body and the plate. In both the case of one plate and the case of two plates, the contact width W was 0.545mm. The length of the filamentous portion at the top of the molded body was 50mm, and there were 30 filaments, so the contact area between the filamentous portion at the top of the molded body and the plate was 0.545mm x 50mm x 30 (filaments) = 817.5mm 2 It was calculated that: Therefore, the pressure caused by placing the plate is 78.5N for one plate and 817.5mm for the contact area in Example 1. 2 =0.096×10 -2 N / mm 2 In Example 2, the load on two plates was 156.9 N / contact area was 817.5 mm 2 =0.192×10 -2 N / mm 2 It was calculated that:
[0114] Example 3: Production example of mesh-shaped boron nitride sheet sintered body Firing was carried out in the same manner as in Example 1 above, except that the weight of the boron nitride ceramic plate was not placed on the molded body, to produce a four-layer mesh-like boron nitride sheet with a so-called point contact configuration having a post-firing size of 50 mm x 50 mm, a pitch of 0.5 mm, a linear width of 1.2 mm, and a total thickness of 3.0 mm.
[0115] Comparative Example 1: Comparative production example of mesh-shaped boron nitride sheet sintered body A sintering aid was not used, and 100 parts of boron nitride raw material powder was mixed with 15.0 parts of hydroxypropyl methylcellulose, 2.5 parts of glycerin, 5.0 parts of a polycarboxylic acid dispersant, and 60.0 parts of water, followed by degassing to prepare a raw material paste, and the boron nitride ceramic plate weight was not placed on the molded body. Firing was performed in the same manner as in Example 1 above, except that a four-layer mesh-like boron nitride sheet with a point contact configuration was attempted. However, the fired product collapsed, and the desired four-layer mesh-like boron nitride sheet could not be produced.
[0116] Comparative Example 2: Comparative production example of mesh-shaped boron nitride sheet sintered body Firing was carried out in the same manner as in Example 1 above, except that the boron nitride ceramic plate weight was not placed on the molded body, and a crucible made entirely of carbon was used as the firing jig instead of a crucible made entirely of boron nitride, to produce a four-layer mesh-like boron nitride sheet with a so-called point contact configuration having a size after firing of 50 mm x 50 mm, a pitch of 0.5 mm, a width of the linear portion of 1.2 mm, and a total thickness of 3.0 mm.
[0117] A. Characterization of mesh-shaped boron nitride sheet sintered body The boron nitride sheet sintered bodies of Examples 1 to 3 and Comparative Examples 1 and 2 were evaluated for various characteristics such as appearance, warpage and brightness as follows.
[0118] 1) Appearance observation The appearance of the boron nitride sheet sintered body was evaluated according to the following three-level criteria. A (good): The appearance of the sintered body was normal with no discoloration. B (unusable): The sintered body collapsed when removed from the furnace. C (unusable): The sintered body showed a gray discoloration.
[0119] 2) Warpage evaluation With a metal ruler placed against one diagonal (length 70.7 mm) of the boron nitride sheet sintered compact, the amount of warping at the other diagonal (length 70.7 mm), which was the longest part, was measured by placing a gap gauge against it. The amount of warping (mm) at the diagonal part with the larger value was divided by the length of the diagonal to calculate the "maximum warping ratio = amount of warping / maximum length (mm / mm)". The evaluation criteria for this maximum warping ratio were as follows: A (best): Maximum warpage ratio is 2×10 -3 The results were as follows. B (Good): Maximum warpage ratio is 2×10 -3 Larger than 3×10 -3 The results were as follows. U (available): Maximum warpage ratio is 3 x 10 -3 Larger than 5×10 -3 The results were as follows. D (unavailable): Maximum warpage ratio is 5 x 10 -3 It was greater.
[0120] 3) Measurement of lightness L* In accordance with JIS Z8722 (2009), a Konica Minolta spectrophotometer "CM-600d" was used to measure the XYZ coordinates under geometric condition c using the SCI method including specular reflection light with a D65 light source (standard light), and these were converted to L*a*b* coordinates to obtain the lightness L* (CIE1976 lightness L*) of the surface of the boron nitride ceramic sheet sintered compact.
[0121] B. Durability evaluation of mesh-shaped boron nitride sheet sintered body The mesh-like boron nitride sheet sintered bodies obtained using the sintering aids in Examples 1 to 3 and Comparative Example 2 were evaluated for durability against dropping, stacking in multiple layers, and transportation, as described below, assuming a severe transportation process.
[0122] 4) Drop durability evaluation The mesh-shaped boron nitride sheet sintered body was held approximately parallel to the surface of the SUS plate at a position 20 mm from the plate surface and then dropped. The durability of the mesh-shaped boron nitride sheet sintered body was evaluated based on the presence or absence of cracks.
[0123] 5) Durability evaluation for multi-stack Ten mesh-like boron nitride sheet sintered bodies were stacked in layers, with 10x10x10mm boron nitride supports (hereafter referred to as "BN supports") placed at the four corners of a 50mm square. The stacked mesh-like boron nitride sheet sintered bodies were vibrated for 180 seconds at level 5 intensity using a 60Hz vibration tester (SINFONIA TECHNOLOGY VIBRATORY PACKER, TYPE VP-40) to observe whether the stacked state could be maintained, and the amount of protrusion from the mullite supports was measured and evaluated according to the following criteria. ◎ (Best): The multi-tiered stacking state was maintained and did not fall over, and the BN pillars protruded less than 1 mm from the setter. ○ (Good): The stacked state was maintained and did not fall over, and the BN pillars protruded from the setter by 1 mm to less than 3 mm. △ (Acceptable): The stacked state was maintained and did not fall over, and the BN pillars protruded 3mm to less than 5mm from the setter. × (Not acceptable): The cargo collapsed and multiple layers of the cargo were torn apart.
[0124] 6) Durability evaluation for transportation A mesh-like boron nitride sheet sintered body was placed on a 1m long roller conveyor and moved along it. The distance of lateral deviation / wandering was measured at the start position and at a position 90cm ahead, and evaluated according to the following criteria. ◎ (best): The lateral displacement distance was less than 10 mm. ○ (Good): The lateral displacement distance was 10 mm or more but less than 30 mm. △ (Acceptable): The lateral displacement distance was between 30mm and 50mm. × (Not acceptable): The lateral displacement distance was 50 m or more.
[0125] The characteristics and durability evaluation results of the above mesh-shaped boron nitride sheet sintered body are shown in Table 1 below, along with the presence or absence of sintering aids, the type of sintering jig (crucible), and the number of boron nitride plate weights used during sintering and the converted pressure. FIG. 19 shows a photograph comparing the appearance of the sintered body obtained after firing in each of the Examples (Examples 1 to 3) (normal appearance without discoloration) with the appearance of the sintered body obtained after firing in Comparative Example 2 (with discoloration).
[0126] [Table 1]
[0127] These results demonstrate that the sintered body obtained by the manufacturing method of the present invention does not collapse after firing, has a uniform color tone with little discoloration, has sufficient brightness, and is highly durable and stable against dropping, stacking in multiple layers, and transportation. Furthermore, it was found that by placing a boron nitride ceramic plate on the second striated coated body during the firing process, in addition to the above advantages, it is possible to produce a sintered body with little warping after firing.
Claims
1. A method for producing a boron nitride ceramic sheet sintered body, comprising the steps of: (1) A molding process for producing a compact from a raw material paste containing raw material powder of boron nitride, a sintering aid, and a medium, A first stripe coated body having a plurality of stripes arranged at given intervals and each stripe being stretched in one direction; and A molding step of producing a molded body including a plurality of second linear coated bodies arranged at given intervals so as to be in contact with and cross each of the first linear coated bodies, each of the second linear coated bodies being stretched in one direction; (2) A firing step of firing the molded body using a firing tool having a surface exposed to a firing atmosphere containing boron nitride to obtain a boron nitride ceramic sheet sintered body, This boron nitride ceramic sheet sintered body is A first striated portion layer including a plurality of first striated portions arranged at given intervals and each of the first striated portions extending in one direction; and A firing step including a second filament layer composed of a plurality of second filament sections each extending in one direction, the second filament sections being arranged at a given interval so as to be in contact with and cross each of the first filament sections. A method for producing a boron nitride ceramic sheet sintered body, comprising:
2. The method of claim 1 , further comprising the step of placing at least one ceramic plate made of boron nitride on the second filamentary coating during the firing step.
3. The method according to claim 1 or 2, wherein the firing jig is a crucible having a surface exposed to the firing atmosphere comprising boron nitride.
4. In the firing step, the pressure applied when placing the boron nitride ceramic plate on the second filamentary coated body is 0.05 N / mm 2 0.5N / mm or more 2 The method according to any one of claims 1 to 3, wherein:
5. A boron nitride ceramic sheet sintered body, (i) a first striated portion layer including a plurality of first striated portions arranged at given intervals and each of the first striated portions extending in one direction; and (ii) a second linear portion layer including a plurality of second linear portions arranged at given intervals so as to be in contact with and cross each of the first linear portions, each of the second linear portions being extended in one direction; The first filamentary layer and the second filamentary layer are integrally formed, The lightness L* value of the surface of the boron nitride ceramic sheet sintered body is 80 or more. Sintered boron nitride ceramic sheet.
6. The warpage rate per unit length obtained by dividing the amount of warpage at the longest part of the main surface of the boron nitride ceramic sheet sintered body by the length of the longest part is 5×10 -3 6. The boron nitride ceramic sheet sintered body according to claim 5, wherein the surface roughness is 0.05 mm / mm or less.
7. 7. The boron nitride ceramic sheet sintered body according to claim 5 or 6, which does not crack when the boron nitride ceramic sheet sintered body is held in a substantially parallel state above a stainless steel plate at a position 20 mm from the plate surface and then dropped.
Citation Information
Patent Citations
Ceramic lattice body
JP2018193274A
Cited By
High-performance corundum-based repairing material and preparation method thereof
CN120864873A
High-performance corundum-based repair material and method for producing same
CN120864873B