Flux composition, solder composition, and electronic board
The flux composition with controlled solvents and additives addresses void formation and storage stability issues in solder compositions, enhancing solderability and printability for large electronic components.
Patent Information
- Application Number
- JP2023048825
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2043-03-24
AI Technical Summary
Existing solder compositions face issues with void formation and storage stability, particularly when used with large electronic components, due to the use of high viscosity and polar diol solvents.
A flux composition containing specific solvents with controlled boiling points and viscosities, along with diol-based solvents having two hydroxy groups, thixotropic agents, and additives like hindered amines and antioxidants, which suppress voids and enhance storage stability.
The solution effectively reduces voids and maintains storage stability, ensuring excellent solderability and printability for large electronic components.
Smart Images

Figure 2024137337000001 
Figure 2024137337000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a flux composition, a solder composition, and an electronic board. [Background technology]
[0002] The solder composition is a mixture of solder powder and flux composition (rosin resin, activator, solvent, etc.) kneaded into a paste (for example, Patent Document 1). This solder composition is required to have solderability such as solder meltability and the property that solder easily wets and spreads (solder wettability), as well as void suppression, printability, etc. On the other hand, as the functions of electronic devices become more diverse, larger electronic components are being mounted on electronic boards. Some large electronic components have large electrode terminal areas (e.g., QFN (Quad Flatpack No Lead) and power transistors). In such electronic components, the printing area of the solder composition is large, so voids tend to occur easily. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 5756067 Summary of the Invention [Problem to be solved by the invention]
[0004] In order to reduce voids in solder compositions, the use of high-viscosity solvents such as diol-based solvents has been considered. However, diol-based solvents tend to have relatively high viscosity and high polarity, which tends to reduce the storage stability of the solder composition.
[0005] An object of the present invention is to provide a flux composition, a solder composition, and an electronic board that can sufficiently suppress voids and have excellent storage stability. [Means for solving the problem]
[0006] According to the present invention, there are provided a flux composition, a solder composition, and an electronic board as described below. [1] A flux composition comprising: (A) a resin; (B) an activator; and (C) a solvent, the component (C) contains (C1) a solvent having a boiling point of more than 250°C and a viscosity at 20°C of more than 10 mPa s, and (C2) a diol solvent having a boiling point of 250°C or less, a resistance value of 60 MΩ or more and 80 MΩ or less, and two hydroxyl groups in one molecule; Flux composition. [2] The flux composition according to [1], The component (B) contains (B1) a dicarboxylic acid having 6 or more carbon atoms. Flux composition. [3] The flux composition according to [1] or [2], the component (C) further contains (C3) a solvent having a boiling point of 210°C or higher and 275°C or lower and a viscosity at 20°C of 10 mPa s or lower; Flux composition. [4] The flux composition according to any one of [1] to [3], The component (C1) is diethylene glycol mono 2-ethylhexyl ether. Flux composition. [5] The flux composition according to any one of [1] to [4], Further, (D) a thixotropic agent is contained, The component (D) contains an amide. Flux composition. [6] The flux composition according to any one of [1] to [5], Further, (E) a hindered amine compound is contained, Flux composition. [7] The flux composition according to any one of [1] to [6], Further, (F) a hindered phenol-based antioxidant is contained, Flux composition. [8] A flux composition according to any one of [1] to [7] and (G) a solder powder. Solder composition. [9] [8] A soldered portion using the solder composition according to the present invention. Electronic board. Effect of the Invention
[0007] According to one aspect of the present invention, it is possible to provide a flux composition, a solder composition, and an electronic substrate that can sufficiently suppress voids and have excellent storage stability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] [Flux composition] First, the flux composition according to this embodiment will be described. The flux composition according to this embodiment is a component other than the solder powder in the solder composition, and contains (A) a resin, (B) an activator, and (C) a solvent, which will be described below. In addition, it is necessary for the (C) component to contain (C1) a solvent having a boiling point of more than 250°C and a viscosity at 20°C of more than 10 mPa·s, and (C2) a diol-based solvent having a boiling point of 250°C or less, a resistance value of 60 MΩ or more and 80 MΩ or less, and two hydroxyl groups in one molecule.
[0009] The reason why the flux composition according to the present embodiment can sufficiently suppress voids and improve printability is not necessarily clear, but the inventors speculate as follows. That is, in the flux composition of the present invention, as the (C) solvent, a diol-based solvent (C2) having a boiling point of 250°C or less, a resistance value of 60MΩ to 80MΩ, and two hydroxyl groups in one molecule is used. A part of the (C2) component volatilizes and becomes a gas before or when the solder melts, and this gas has the effect of pushing the gas in the solder composition to the outside. The solder composition containing the (C2) component that has not volatilized has a certain degree of fluidity even when the solder melts, so that the gas in the solder composition gradually gathers and is released to the outside. In this way, voids can be sufficiently suppressed. In addition, the (C2) component tends to have low polarity among diol-based solvents. As a result, even though a diol-based solvent is used, the viscosity change during storage of the solder composition can be suppressed. In this way, excellent storage stability can be ensured. The present inventors presume that the above-mentioned effects of the present invention are achieved in the above-mentioned manner.
[0010] [Component (A)] Examples of the (A) resin used in this embodiment include rosin resin, acrylic resin, epoxy resin, and phenol resin. These may be used alone or in combination of two or more. Among these, rosin resin or acrylic resin is preferred from the viewpoint of viscosity stability. Examples of the rosin-based resin include rosins and rosin-based modified resins. Examples of the rosins include gum rosin, wood rosin, and tall oil rosin. Examples of the rosin-based modified resin include disproportionated rosin, polymerized rosin, hydrogenated rosin, and derivatives thereof. Examples of the hydrogenated rosin include fully hydrogenated rosin, partially hydrogenated rosin, and hydrogenated products of unsaturated organic acid-modified rosins (also called "hydrogenated acid-modified rosin"), which are modified rosins of unsaturated organic acids (aliphatic unsaturated monobasic acids such as (meth)acrylic acid, aliphatic unsaturated dibasic acids such as α,β-unsaturated carboxylic acids such as fumaric acid and maleic acid, unsaturated carboxylic acids having aromatic rings such as cinnamic acid, etc.). These rosin-based resins may be used alone or in combination of two or more. Among these rosin-based resins, it is preferable to use fully hydrogenated rosin and hydrogenated acid-modified rosin, and it is more preferable to use fully hydrogenated rosin and hydrogenated acid-modified rosin in combination. The acrylic resin is obtained by polymerizing at least one monomer such as acrylic acid, methacrylic acid, various esters of acrylic acid, various esters of methacrylic acid, crotonic acid, itaconic acid, maleic acid, maleic anhydride, esters of maleic acid, esters of maleic anhydride, acrylonitrile, methacrylonitrile, acrylamide, methacrylamide, vinyl chloride, and vinyl acetate. The acrylic resin is useful in that it can prevent cracks from occurring in the flux residue even in an environment with a large temperature difference and a large thermal shock. Among these acrylic resins, acrylic resins obtained by polymerizing monomers containing methacrylic acid and a monomer having an alkyl group with 2 to 6 carbon atoms, and further acrylic resins obtained by polymerizing monomers containing methacrylic acid and a monomer having an alkyl group with 2 carbon atoms are preferred. Such acrylic resins are preferred in that they suppress the stickiness of the flux residue (flux solidified product) formed and have a good crack suppression effect.
[0011] The amount of the (A) component is preferably 25% by mass or more and 60% by mass or less, and more preferably 30% by mass or more and 50% by mass or less, based on 100% by mass of the flux composition. If the amount of the (A) component is more than the lower limit, the oxidation of the copper foil surface of the soldering land is prevented, making the surface more easily wetted with molten solder, so that the so-called solderability can be improved and solder balls can be sufficiently suppressed. Also, if the amount of the (A) component is less than the upper limit, the amount of flux residue can be sufficiently suppressed.
[0012] [(B) Component] The (B) activator used in this embodiment preferably contains (B1) a dicarboxylic acid having 6 or more carbon atoms. This component (B1) can improve solderability. Examples of the (B1) component include adipic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, eicosanedioic acid, and 8,13-dimethyl-8,12-eicosadienedioic acid. These may be used alone or in combination of two or more.
[0013] The blending amount of the (B1) component is preferably 0.1% by mass or more and 15% by mass or less, more preferably 1% by mass or more and 12% by mass or less, even more preferably 3% by mass or more and 10% by mass or less, and particularly preferably 5% by mass or more and 8% by mass or less, based on 100% by mass of the flux composition. If the blending amount of the (B1) component is equal to or more than the lower limit, the solderability tends to be improved without deteriorating other physical properties, while if it is equal to or less than the upper limit, the insulating properties of the flux composition tend to be maintained.
[0014] The component (B) may further contain an amine-based activator (B2), which can further improve the solderability. Examples of the (B2) component include benzotriazoles (benzotriazole, 2-(2-hydroxy-5-methylphenyl), etc.), imidazolines (2-phenylimidazoline, 2-benzylimidazoline, etc.), amines (polyamines such as ethylenediamine, etc.), amine salts (organic acid salts or inorganic acid salts (hydrochloric acid, sulfuric acid, hydrobromic acid, etc.) of amines and aminoalcohols such as trimethylolamine, cyclohexylamine, diethylamine, etc.), amino acids (glycine, alanine, aspartic acid, glutamic acid, valine, etc.), amide compounds, etc. Among these, imidazolines are preferred from the viewpoint of activity.
[0015] The blending amount of the (B2) component is preferably 0.1% by mass to 10% by mass, more preferably 0.5% by mass to 8% by mass, even more preferably 1% by mass to 7% by mass, and particularly preferably 3% by mass to 6% by mass, based on 100% by mass of the flux composition. If the blending amount of the (B2) component is equal to or more than the lower limit, the solderability tends to be improved, whereas if the blending amount is equal to or less than the upper limit, the insulating properties of the flux composition tends to be maintained.
[0016] The component (B) may further contain an organic acid other than the component (B1) (hereinafter sometimes referred to as the component (B3)). Examples of the (B3) component include monocarboxylic acids, dicarboxylic acids other than the (B1) component, and other organic acids. These may be used alone or in combination of two or more. Monocarboxylic acids include formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, enanthic acid, capric acid, lauric acid, myristic acid, pentadecylic acid, palmitic acid, margaric acid, stearic acid, tuberculostearic acid, arachidic acid, behenic acid, lignoceric acid, and glycolic acid. Dicarboxylic acids include succinic acid, dimer acid, tartaric acid, and diglycolic acid. Other organic acids include trimer acid, levulinic acid, lactic acid, acrylic acid, benzoic acid, salicylic acid, anisic acid, citric acid, and picolinic acid, etc. Among these, it is more preferable to use picolinic acid.
[0017] When the (B3) component is used, its amount is preferably 0.1% by mass or more and 8% by mass or less, more preferably 0.2% by mass or more and 5% by mass or less, and particularly preferably 0.3% by mass or more and 3% by mass or less, based on 100% by mass of the flux composition. If the (B3) component is added in an amount equal to or more than the lower limit, the activation action tends to be improved, whereas if the amount is equal to or less than the upper limit, the insulating properties of the flux composition tend to be maintained.
[0018] In addition to the components (B1) to (B3), the component (B) may further contain another activator (hereinafter also referred to as the component (B4)) within the scope of the present invention. Examples of the component (B4) include halogen-based activators.
[0019] The blending amount of the (B) component is preferably 1% by mass or more and 20% by mass or less, and more preferably 2% by mass or more and 15% by mass or less, based on 100% by mass of the flux composition. If the blending amount of the (B) component is equal to or more than the lower limit, the activation action tends to be improved, whereas if the blending amount is equal to or less than the upper limit, the insulating property of the flux composition tends to be maintained.
[0020] [(C) component] The (C) solvent used in this embodiment must contain (C1) a solvent having a boiling point of more than 250° C. and a viscosity of more than 10 mPa s at 20° C. Such component (C1) is the main solvent, which allows the viscosity of the solder composition to be within an appropriate range during printing and after reflow. Examples of the (C1) component include diethylene glycol mono 2-ethylhexyl ether (boiling point 272°C, viscosity 11.8 mPa·s) and polyethylene glycol monomethyl ether (boiling point 290 to 310°C, viscosity 12.8 mPa·s). Among these, diethylene glycol mono 2-ethylhexyl ether is preferred from the viewpoint of printability. These may be used alone or in combination of two or more. The viscosity in parentheses is the viscosity at 20°C.
[0021] The blending amount of the (C1) component, relative to 100% by mass of the (C) component, is preferably 40% by mass or more and 85% by mass or less, more preferably 45% by mass or more and 80% by mass or less, and particularly preferably 50% by mass or more and 75% by mass or less.
[0022] The solvent (C) used in this embodiment must contain a diol solvent (C2) having a boiling point of 250° C. or less, a resistance value of 60 MΩ or more and 80 MΩ or less, and two hydroxyl groups in one molecule. Such a component (C2) has a high effect of suppressing voids and has little adverse effect on storage stability. The resistance value of the solvent can be measured using a milliohm high tester (manufactured by Hioki E.E. Corp.) The temperature of the solvent during the measurement may be room temperature (for example, 25° C.). Examples of the (C2) component include 1,2-butanediol (resistance value 65 MΩ), 1,2-pentanediol (resistance value 70 MΩ), and 1,2-hexanediol (resistance value 70 MΩ). These may be used alone or in combination of two or more.
[0023] The blending amount of the (C2) component is preferably 10% by mass or more and 50% by mass or less, more preferably 15% by mass or more and 45% by mass or less, and particularly preferably 20% by mass or more and 40% by mass or less, based on 100% by mass of the (C) component. If the blending amount of the (C2) component is equal to or more than the lower limit, the effect of suppressing voids can be further improved. On the other hand, if the blending amount of the (C2) component is equal to or less than the upper limit, adverse effects on storage stability can be suppressed.
[0024] The (C) solvent used in this embodiment preferably contains (C3) a solvent having a boiling point of 210° C. or more and 275° C. or less and a viscosity of 10 mPa s or less at 20° C. Such a (C3) component can improve printability. Examples of components (C3) include diethylene glycol dibutyl ether (boiling point 256°C, viscosity 2.4 mPa·s), diethylene glycol butyl methyl ether (boiling point 212°C, viscosity 1.6 mPa·s), tetraethylene glycol dimethyl ether (boiling point 275°C, viscosity 3.8 mPa·s), diethylene glycol monobutyl ether (boiling point 230°C, viscosity 5.85 mPa·s), and diethylene glycol monobutyl ether acetate (boiling point 247°C, viscosity 3.56 mPa·s). Note that the viscosity in parentheses is the viscosity at 20°C.
[0025] From the viewpoint of printability, the blending amount of the (C3) component, relative to 100% by mass of the (C) component, is preferably 5% by mass or more and 30% by mass or less, more preferably 8% by mass or more and 22% by mass or less, and particularly preferably 10% by mass or more and 15% by mass or less.
[0026] From the viewpoint of the balance between the void suppression effect and printability, the mass ratio of the (C2) component to the (C3) component ((C2) / (C3)) is preferably from 1 / 2 to 6, more preferably from 1 to 5, and particularly preferably from 3 / 2 to 4.
[0027] The (C) component may contain a solvent other than the (C1), (C2) and (C3) components (hereinafter also referred to as the (C4) component). As the (C4) component, a known solvent can be appropriately used. As such a solvent, it is preferable to use a solvent having a boiling point of 170°C or more and 250°C or less. Examples of such solvents include hexylene glycol (boiling point 197° C.) and methyl carbitol (boiling point 194° C.). These may be used alone or in combination of two or more. From the viewpoint of storage stability, it is preferable not to use a diol solvent other than the component (C2) as the component (C).
[0028] The blending amount of the (C) component is preferably 20% by mass or more and 60% by mass or less, and more preferably 30% by mass or more and 50% by mass or less, based on 100% by mass of the flux composition. When the blending amount of the solvent is within the above range, the viscosity of the obtained solder composition can be appropriately adjusted to an appropriate range.
[0029] [(D) component] The flux composition according to the present embodiment preferably contains (D) a thixotropic agent from the viewpoint of suppressing sagging during printing or heating. As the component (D), a known thixotropic agent can be appropriately used. Examples of the thixotropic agent used here include hardened castor oil, amides, kaolin, colloidal silica, organic bentonite, and glass frit. Among these, amides are preferred from the viewpoint of storage stability. These may be used alone or in combination of two or more. From the viewpoint of storage stability, it is preferable not to use a thixotropic agent other than an amide (especially hydrogenated castor oil) as component (D).
[0030] The blending amount of the (D) component is preferably 2% by mass or more and 20% by mass or less, more preferably 3% by mass or more and 15% by mass or less, and particularly preferably 5% by mass or more and 10% by mass or less, based on 100% by mass of the flux composition. If the blending amount is equal to or more than the lower limit, sufficient thixotropy is obtained and sagging tends to be suppressed. On the other hand, if the blending amount is equal to or less than the upper limit, the thixotropy is not too high and printing defects tend not to occur.
[0031] [(E) component] From the viewpoint of suppressing voids, the flux composition according to the present embodiment preferably contains a hindered amine compound (E). The component (E) has a structure represented by the following general formula (E1).
[0032] [ka]
[0033] In general formula (E1), R 1 are independently a methyl group or an ethyl group, and are preferably a methyl group. X is hydrogen, an alkyl group having 1 to 12 carbon atoms, or an alkoxy group having 1 to 12 carbon atoms. In addition, there are no particular limitations on the structure of the portion beyond the wavy line in component (E). The number of structures represented by general formula (E1) in one molecule of the component (E) is preferably 1 or more and 10 or less, and more preferably 2 or more and 4 or less.
[0034] The (E) component includes bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate, tetrakis(2,2,6,6-tetramethyl-4-piperidyl)butane-1,2,3,4-tetracarboxylate, 2,2,6,6-tetramethyl-4-piperidyl methacrylate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)-[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]ethyl]butylmalonate, and bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacic acid. cate, 1-(methyl)-8-(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)butane-1,2,3,4-tetracarboxylate, 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate, bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidyl)sebacate, and bis(1-undecaoxy-2,2,6,6-tetramethylpiperidin-4-yl)carbonate. These may be used alone or in combination of two or more.
[0035] From the viewpoint of suppressing voids, the blending amount of the (E) component is preferably 0.1 mass % or more and 20 mass % or less, more preferably 0.5 mass % or more and 10 mass % or less, further preferably 1 mass % or more and 7 mass % or less, and particularly preferably 1.5 mass % or more and 4 mass % or less, based on 100 mass % of the flux composition.
[0036] [Component (F)] From the viewpoint of storage stability, the flux composition according to this embodiment preferably further contains (F) a hindered phenol-based antioxidant.
[0037] Examples of the (F) component include pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], bis(3-tert-butyl-4-hydroxy-5-methylbenzenepropanoic acid)ethylene bis(oxyethylene), N,N'-bis[2-[2-(3,5-di-tert-butyl-4-hydroxyphenyl)ethylcarbonyloxy]ethyl]oxamide, and N,N'-bis{3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl}hydrazine. Among these, from the viewpoint of storage stability, bis(3-tert-butyl-4-hydroxy-5-methylbenzenepropanoic acid)ethylene bis(oxyethylene) is more preferred. These may be used alone or in combination of two or more.
[0038] The blending amount of the (F) component is preferably 0.1% by mass or more and 7% by mass or less, more preferably 1% by mass or more and 6% by mass or less, and particularly preferably 2% by mass or more and 5% by mass or less, based on 100% by mass of the flux composition. If the blending amount of the antioxidant is equal to or more than the lower limit, the solder melting property and the storage stability tend to be improved, while if it is equal to or less than the upper limit, the insulation property of the flux composition tends to be maintained.
[0039] [Other ingredients] In addition to the components (A), (B), (C), (D), (E), and (F), other additives may be added to the flux composition used in this embodiment as necessary. Examples of the other additives include imidazole compounds, antifoaming agents, modifiers, matting agents, and foaming agents. The amount of these additives is preferably 0.01% by mass or more and 5% by mass or less with respect to 100% by mass of the flux composition.
[0040] [Solder composition] Next, the solder composition according to the present embodiment will be described. The solder composition according to the present embodiment contains the flux composition according to the present embodiment described above and the solder powder (G) described below. The amount of the flux composition is preferably 5% by mass or more and 35% by mass or less, more preferably 7% by mass or more and 15% by mass or less, and particularly preferably 8% by mass or more and 12% by mass or less, relative to 100% by mass of the solder composition. When the amount of the flux composition is less than 5% by mass (when the amount of the solder powder exceeds 95% by mass), the flux composition as a binder is insufficient, so that it tends to be difficult to mix the flux composition and the solder powder. On the other hand, when the amount of the flux composition is more than 35% by mass (when the amount of the solder powder is less than 65% by mass), when the obtained solder composition is used, it tends to be difficult to form a sufficient solder joint.
[0041] [(G) component] The solder powder (G) used in this embodiment is preferably made of only lead-free solder powder, but may be lead-containing solder powder. The solder alloy in this solder powder preferably contains at least one selected from the group consisting of tin (Sn), copper (Cu), zinc (Zn), silver (Ag), gold (Au), antimony (Sb), lead (Pb), indium (In), bismuth (Bi), nickel (Ni), cobalt (Co) and germanium (Ge). The solder alloy in the solder powder is preferably an alloy mainly composed of tin, more preferably containing tin, silver and copper, and may further contain at least one of antimony, bismuth and nickel as an additive element. Here, lead-free solder powder refers to a powder of solder metal or alloy to which no lead is added. However, the presence of lead as an unavoidable impurity in the lead-free solder powder is permitted, but in this case, the amount of lead is preferably 300 ppm by mass or less.
[0042] Specific examples of alloy systems for lead-free solder powder include Sn-Ag-Cu systems, Sn-Cu systems, Sn-Ag systems, Sn-Bi systems, Sn-Ag-Bi systems, Sn-Ag-Cu-Bi systems, Sn-Ag-Cu-Ni systems, Sn-Ag-Cu-Bi-Sb systems, Sn-Ag-Bi-In systems, and Sn-Ag-Cu-Bi-In-Sb systems.
[0043] The average particle size of component (G) is usually 1 μm or more and 40 μm or less, but from the viewpoint of being compatible with electronic boards having narrow pitches of solder pads, it is more preferably 1 μm or more and 35 μm or less, even more preferably 2 μm or more and 35 μm or less, and particularly preferably 3 μm or more and 32 μm or less. The average particle size can be measured by a dynamic light scattering type particle size measuring device.
[0044] [Method of manufacturing solder composition] The solder composition of this embodiment can be produced by blending the above-described flux composition and the above-described (G) solder powder in the above-described predetermined ratio, and stirring and mixing them.
[0045] [Electronic board] Next, the electronic board according to the present embodiment will be described. The electronic board according to the present embodiment is characterized by having a soldered portion using the solder composition according to the present embodiment. The electronic board according to the present embodiment can be manufactured by mounting electronic components on an electronic board (such as a printed wiring board) using the solder composition. Examples of the coating device used here include a screen printer, a metal mask printer, a dispenser, and a jet dispenser. In addition, electronic components can be mounted on an electronic board by a reflow process in which electronic components are placed on the solder composition applied by an application device and heated under specified conditions in a reflow furnace to mount the electronic components on a printed wiring board.
[0046] In the reflow process, an electronic component is placed on the solder composition and heated in a reflow furnace under predetermined conditions. This reflow process allows a sufficient solder joint to be formed between the electronic component and the printed wiring board. As a result, the electronic component can be mounted on the printed wiring board. The reflow conditions may be appropriately set according to the melting point of the solder. For example, the preheat temperature is preferably 140°C or higher and 200°C or lower, and more preferably 150°C or higher and 160°C or lower. The preheat time is preferably 60 seconds or higher and 120 seconds or lower. The peak temperature is preferably 230°C or higher and 270°C or lower, and more preferably 240°C or higher and 255°C or lower. The holding time at a temperature of 220°C or higher is preferably 20 seconds or higher and 60 seconds or lower.
[0047] Furthermore, the flux composition, the solder composition, and the electronic board according to the present embodiment are not limited to the above-described embodiment, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention. For example, in the electronic substrate, the printed wiring board and the electronic component are bonded by a reflow process, but the present invention is not limited thereto. For example, instead of the reflow process, the printed wiring board and the electronic component may be bonded by a process (laser heating process) of heating the solder composition using laser light. In this case, the laser light source is not particularly limited and can be appropriately adopted according to the wavelength that matches the absorption band of the metal. Examples of the laser light source include solid lasers (ruby, glass, YAG, etc.), semiconductor lasers (GaAs, InGaAsP, etc.), liquid lasers (dye, etc.), and gas lasers (He-Ne, Ar, CO2, excimer, etc.). EXAMPLES
[0048] The present invention will now be described in more detail with reference to examples and comparative examples, but the present invention is not limited to these examples. The materials used in the examples and comparative examples are shown below. (Component (A)) Rosin resin A: Acrylic acid modified hydrogenated rosin, product name "Pine Crystal KE-604", manufactured by Arakawa Chemical Industries Co., Ltd. Rosin resin B: fully hydrogenated rosin, trade name "Foral AXE", manufactured by Eastman Chemical Company ((B1) component) Dicarboxylic acid A: Dodecanedioic acid Dicarboxylic acid B: Adipic acid ((B2) component) Amine surfactant: 2-phenylimidazoline ((C1) component) Solvent A: Diethylene glycol mono 2-ethylhexyl ether (boiling point 272°C, viscosity 11.8 mPa·s), product name "EHDG", manufactured by Nippon Nyukazai Co., Ltd. ((C2) component) Solvent B: 1,2-butanediol (resistance value 65MΩ) Solvent C: 1,2-pentanediol (resistance value 70MΩ) Solvent D: 1,2-Hexanediol (resistance value 70MΩ) ((C3) component) Solvent E: Diethylene glycol dibutyl ether (boiling point 256°C, viscosity 2.4 mPa·s) ((C4) component) Solvent F: 1,4-butanediol (resistance value 50MΩ) Solvent G: 1,3-butanediol (resistance value 36MΩ) Solvent H: 1,5-pentanediol (resistance value 50MΩ) Solvent I: 2,4-pentanediol (resistance value cannot be measured because it is a solid) Solvent J: 1,6-Hexanediol (resistance value cannot be measured because it is a solid) Solvent K: 1,2,4-butanetriol (resistance value 20MΩ) ((D) component) Thixotropic agent A: higher fatty acid polyamide, product name "Talen VA-79", manufactured by Kyoeisha Chemical Co., Ltd. Thixotropic agent B: fatty acid amide, product name "Slipax H", manufactured by Nippon Kasei Co., Ltd. Thixotropic agent C: fatty acid amide, product name "Slipax ZHH", manufactured by Nippon Kasei Co., Ltd. Thixotropic agent D: Trade name "Himako", manufactured by KF Trading Co., Ltd. ((E) component) Hindered amine compound: bis(1,2,2,6,6-pentamethyl-4-piperidyl)-[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]ethyl]butyl malonate, trade name "Tinuvin 144", manufactured by BASF (Component (F)) Antioxidant A: bis(3-tert-butyl-4-hydroxy-5-methylbenzenepropanoic acid) ethylene bis(oxyethylene), trade name "Irganox 245", manufactured by BASF Antioxidant B: Pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], trade name "ANOX20", manufactured by SI Group Antioxidant C: N,N'-bis{3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl}hydrazine, trade name "Irganox MD1024", manufactured by BASF ((G) component) Solder powder: alloy composition is Sn-3.0Ag-0.5Cu, particle size distribution is 15~25μm
[0049] [Example 1] 28.5 mass% of rosin-based resin A, 14.5 mass% of rosin-based resin B, 5 mass% of dicarboxylic acid A, 3 mass% of dicarboxylic acid B, 5 mass% of amine-based activator, 2 mass% of antioxidant A, 23 mass% of solvent A, 9 mass% of solvent B, 4.5 mass% of solvent E, and 5.5 mass% of thixotropic agent A were charged into a container and mixed using a planetary mixer to obtain a flux composition. Thereafter, 11.5% by mass of the obtained flux composition and 88.5% by mass of solder powder (total of 100% by mass) were placed in a container and mixed with a planetary mixer to prepare a solder composition.
[0050] [Examples 2 to 13] A solder composition was obtained in the same manner as in Example 1, except that the materials were mixed according to the composition shown in Table 1. [Comparative Examples 1 to 8] A solder composition was obtained in the same manner as in Example 1, except that the materials were mixed according to the composition shown in Table 1.
[0051] <Evaluation of solder composition> The solder compositions were evaluated (void area ratio, storage stability) by the following methods. The results are shown in Table 1. (1) Void area ratio A solder composition was printed on a board capable of mounting QFN components, and a Sn-plated QFN (6 mm x 6 mm) was mounted on it. The solder composition was melted in a reflow furnace (manufactured by Tamura Corporation) and soldered to obtain a board for evaluation. The reflow conditions were a preheat temperature of 130 to 180°C (approximately 80 seconds), a time at a temperature of 220°C or higher for approximately 50 seconds, a peak temperature of 248°C, and air. An X-ray photograph was taken of the bonded portion of the evaluation substrate, and the void area ratio of the lower electrode portion [(void area ÷ land area) × 100] (unit: %) was measured. The void area ratio was then calculated and evaluated according to the following criteria. A: The void area ratio is less than 10%. ◯: The void area ratio is 10% or more and less than 20%. Δ: The void area ratio is 20% or more and less than 30%. ×: The void area ratio is 30% or more. (2) Storage stability The solder composition was used as a sample, and a stability test was performed in which the sample was stored in (i) a thermostatic chamber at 30°C and (ii) a thermostatic chamber at 40°C for 30 days. The viscosity of the sample was measured before and after the stability test. The difference (η2-η1) between the initial viscosity value (η1) and the viscosity value (η2) after the stability test was calculated, and the viscosity change rate [{(η2-η1) / η1}×100] (unit: %) was calculated. The viscosity was measured by a spiral viscosity measurement (Malcom Co., Ltd., PCU-II type, measurement temperature: 25°C, rotation speed: 10 rpm, after stirring for 3 minutes). The appearance of the sample after the stability test was also observed. The storage stability was evaluated according to the following criteria. ⊚: The viscosity change rate is -15% or more and 15% or less. ◯: The viscosity change rate is −25% or more and less than −15%, or more than 15% and 25% or less. Δ: The viscosity change rate is −50% or more and less than −25%, or more than 25% and 50% or less. ×: The viscosity change rate is less than −50% or more than 50%, or the appearance of the sample after the stability test is dull and gritty.
[0052] [Table 1]
[0053] As is clear from the results shown in Table 1, it was confirmed that the solder compositions of the present invention (Examples 1 to 13) were excellent in both void area ratio and storage stability. Therefore, it was confirmed that the solder composition of the present invention can sufficiently suppress voids and has excellent storage stability. [Industrial Applicability]
[0054] The flux composition and solder composition of the present invention can be suitably used as a technique for mounting electronic components on electronic substrates such as printed wiring boards of electronic devices.
Claims
1. A flux composition comprising: (A) a resin; (B) an activator; and (C) a solvent, the component (C) contains (C1) a solvent having a boiling point of more than 250° C. and a viscosity at 20° C. of more than 10 mPa·s, and (C2) a diol solvent having a boiling point of 250° C. or less, a resistance value of 60 MΩ or more and 80 MΩ or less, and having two hydroxyl groups in one molecule; Flux composition.
2. 2. The flux composition according to claim 1, The component (B) contains (B1) a dicarboxylic acid having 6 or more carbon atoms. Flux composition.
3. The flux composition according to claim 1 or 2, The component (C) further contains (C3) a solvent having a boiling point of 210° C. or higher and 275° C. or lower and a viscosity at 20° C. of 10 mPa s or lower. Flux composition.
4. The flux composition according to claim 1 or 2, The component (C1) is diethylene glycol mono 2-ethylhexyl ether. Flux composition.
5. The flux composition according to claim 1 or 2, Further, (D) a thixotropic agent is contained, The component (D) contains an amide. Flux composition.
6. The flux composition according to claim 1 or 2, Further, the composition contains (E) a hindered amine compound, Flux composition.
7. The flux composition according to claim 1 or 2, Further, (F) a hindered phenol-based antioxidant is contained, Flux composition.
8. A flux composition according to claim 1 or 2, and (G) a solder powder. Solder composition.
9. A soldered portion comprising the solder composition according to claim 8. Electronic board.
Citation Information
Patent Citations
Solder paste composition and reflow soldering method
JP2002283097A
Flux composition, and solder composition, and method for producing electronic board
JP2022073104A
Flux composition, and solder composition, and method for producing electronic board
JP2022188686A
Agent for suppressing viscosity increase in solder flux