Taking-up method for hot rolled steel sheet, taking-up device for hot rolled steel sheet, and manufacturing method of hot rolled steel sheet

By optimizing the cooling process to maximize the temperature difference between the outer and inner coil surfaces, the method and device effectively reduce springback, enhancing the manufacturability and safety of high-strength, thick-walled hot-rolled steel sheets.

JP2024137348AActive Publication Date: 2024-10-07JFE STEEL CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023048840
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-07
Estimated Expiration
2043-03-24

AI Technical Summary

Technical Problem

Existing methods for winding high-strength, thick-walled hot-rolled steel sheets fail to accurately determine the cooling time to maximize the temperature difference between the outer and inner surfaces of the coil, leading to insufficient reduction of springback, which can cause lifting, equipment damage, and band tearing during transportation.

Method used

A method and device that control the cooling process by injecting water from nozzles while rotating the mandrel, optimizing the installation position, nozzle direction, and flow rate to set the cooling time at the maximum temperature difference between the outer and inner coil surfaces, using a computer system to calculate and control these parameters.

Benefits of technology

Accurately reduces springback at the outermost part of the coil, preventing lifting and band tearing, ensuring safe handling and manufacturing of high-strength steel sheets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137348000001_ABST
    Figure 2024137348000001_ABST
Patent Text Reader

Abstract

To provide a taking-up method for a hot rolled steel sheet, etc., capable of accurately presenting a spring-back reduction effect in an outermost peripheral part of a coil by accurately determining a cooling time, with which a temperature difference between an outer peripheral surface and an inner peripheral surface of an outermost peripheral plate of the coil becomes maximum, from an outer diameter, a plate thickness, etc., of the coil for each coil when determining the cooling time.SOLUTION: A spray control step (step S2) in a taking-up method for a hot rolled steel sheet includes a cooling time calculation step (step S23) of calculating a cooling time τ, with which a temperature difference between an outer peripheral surface and an inner peripheral surface of an outermost peripheral plate of a coil C for an arc length Lc of a cooling range in the coil C becomes maximum, on the basis of an installation position of the coil C, an outer diameter D of the coil C, a plate thickness t of the coil C, positions of nozzles 4a and 4b, a direction α of the nozzles 4a and 4b, an injection angle β of cooling water from the nozzles 4a and 4b, a cooling width Wc in the coil C by the cooling water from the nozzles 4a and 4b, a flow quantity Q of the cooling water from the nozzles 4a and 4b, and a surface temperature T0 of the coil C before cooling when taking up the coil.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for winding a hot-rolled steel sheet, in particular a high-strength thick-walled hot-rolled steel sheet that is used as a material for steel pipe piles and square columns, for stably producing the hot-rolled steel sheet, a winding device for the hot-rolled steel sheet, and a method for manufacturing the hot-rolled steel sheet. [Background technology]

[0002] In recent years, there has been an increasing demand for steel pipe piles, which are mainly used as foundation piles for port buildings, and square columns, which are used as pillars for buildings. The materials used for these steel pipe piles and square columns are required to have properties such as high strength and high toughness. For this reason, steel pipe piles and square columns are manufactured using high-strength thick hot-rolled steel plates. These high-strength thick hot-rolled steel plates have a thickness of about 12 to 30 mm and a width of about 1100 to 2200 mm.

[0003] Incidentally, the hot-rolled steel sheet after passing through the hot rolling line is wound up by a winding device (down coiler). At this time, in the case of a high-strength thick material, the elastic deformation (springback) of the outermost periphery of the hot-rolled steel sheet wound up in a coil shape (hereinafter, the hot-rolled steel sheet wound up in a coil shape is referred to as a coil) becomes large. In the winding device, the elastic deformation force of the outermost periphery of the coil is larger than the coil's own weight, so that the coil C is lifted up by the elastic deformation force of the outermost periphery C1 of the coil C (the coil C is lifted up from the cradle rolls 107a, 107b supporting the coil C) as shown in FIG. 15. This causes the coil C to come into contact with the reduced diameter mandrel 102, and the coil C may not be able to come out of the mandrel 102. In addition, there is a risk that the mandrel 102 may be damaged due to the contact between the coil C and the mandrel 102. Furthermore, after the hot-rolled steel sheet is wound up, the elastic deformation force of the outermost periphery C1 of the coil C is large, so that there is a risk that the restraining band (not shown) that restrains the outer periphery of the coil C will be torn off during transportation, and the coil C will fly off at that moment. In addition, steel pipe pile and column materials are required to have strength and toughness, so it is necessary to take samples for material testing. When taking these samples, the hot-rolled steel sheet that has been wound into a coil is cooled and then gas-cut by hand, but at the moment the restraining band that restrains the coil C is removed, the hot-rolled steel sheet jumps up due to the elastic deformation force of the outermost periphery C1 of the coil C, which is very dangerous. For this reason, it can be said that it is essential to suppress the elastic deformation of the outermost periphery C1 of the coil C in manufacturing the hot-rolled steel sheet.

[0004] As a method for suppressing elastic deformation at the outermost periphery of a coil, for example, a coiling method for a hot-rolled steel sheet as shown in Patent Document 1 has been proposed. In the method of winding a hot-rolled steel sheet shown in Patent Document 1, after winding the hot-rolled steel sheet from the leading end to the trailing end into a coil, cooling water is sprayed onto the outer periphery of the coil while a wrapper roll arranged in a planetary fashion is pressed against the coil. Then, after cooling the outer periphery of the coil for a predetermined cooling time, the cooling is stopped and the coil is retained in the winding device for a predetermined retention time, after which the wrapper roll is released and the coil is removed from the winding device.

[0005] Furthermore, as a method for suppressing elastic deformation of the outermost periphery of a coil, for example, a coiling method for a high-strength thick hot-rolled steel sheet as shown in Patent Document 2 has been proposed. The coiling method of high-strength thick hot-rolled steel sheet shown in Patent Document 2 involves winding the high-strength thick hot-rolled steel sheet from the leading end to the trailing end around a mandrel in the form of a coil, and then spraying cooling water onto the outer periphery of the coil while multiple wrapper rolls are pressed against the coil, thereby rapidly cooling the outer periphery of the coil to a predetermined temperature, and then pulling out the coil from the coiling device. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2012-24793 A [Patent Document 2] JP 2010-162594 A Summary of the Invention [Problem to be solved by the invention]

[0007] Incidentally, in the coiling method of hot-rolled steel sheet shown in Patent Document 1, it is said that the springback reduction effect is achieved when the cooling time of the outer peripheral plate of the coil is approximately equal to the time when the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost plate of the coil becomes maximum. In the coiling method of hot-rolled steel sheet shown in Patent Document 1, coil winding experiments, etc. were conducted to determine the cooling time at which the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost sheet of the coil becomes maximum, and the cooling time was set to 5 seconds or more for materials that meet API standard X65 or higher and have a product thickness of 19 mm or higher.

[0008] However, when determining the cooling time at which the temperature difference between the outer and inner surfaces of the outermost coil plate will be maximized, for materials that meet API standards of X65 or higher and have a product thickness of 19 mm or more, it is not enough to simply set the cooling time at 5 seconds or more; it must be accurately determined for each coil based on the outer diameter and plate thickness of the coil, the position and direction of the nozzle that sprays the cooling water, the flow rate of the cooling water, etc. In addition, in the coiling method of high-strength thick hot-rolled steel sheet shown in Patent Document 2, cooling water is sprayed onto the outer periphery of the coil to rapidly cool it down to a predetermined temperature. However, there is no description of setting the cooling time of the outer periphery sheet of the coil to the time that maximizes the temperature difference between the outer periphery surface and the inner periphery surface of the outermost sheet of the coil in order to exert the effect of reducing springback.

[0009] Therefore, the present invention has been made to solve the conventional problems, and has an object to provide a coiling method for hot-rolled steel sheet, a coiling device for hot-rolled steel sheet, and a manufacturing method for hot-rolled steel sheet, which can accurately determine the cooling time at which the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost sheet of a coil is maximized for each coil based on the outer diameter and sheet thickness of the coil, the position and direction of the nozzle for spraying cooling water, the flow rate of cooling water, etc., and can accurately demonstrate the effect of reducing springback in the outermost portion of the coil. [Means for solving the problem]

[0010] In order to solve the above problems, a method for winding a hot-rolled steel sheet according to one aspect of the present invention comprises winding a hot-rolled steel sheet from its leading end to its trailing end into a coil shape on a mandrel of a winding device, and then rotating the mandrel while pressing a plurality of wrapper rolls arranged in a planetary pattern against the coil against the coil, spraying cooling water from a nozzle against an outer peripheral sheet of the coil, thereby cooling the outer peripheral portion of the coil for a predetermined cooling time, wherein the predetermined cooling time for the outer peripheral portion of the coil is set equal to the time at which the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost sheet of the coil becomes maximum. The method includes a spray control step of controlling the rotation of the mandrel and the spray of cooling water from the nozzle so as to spray cooling water from the nozzle onto the peripheral plate, and the spray control step includes a cooling time calculation step of calculating a cooling time at which a temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost plate of the coil over an arc length of a cooling range in the coil is maximized, based on an installation position of the coil, an outer diameter of the coil, a plate thickness of the coil, a position of the nozzle, an orientation of the nozzle, an angle of spray of cooling water from the nozzle, a cooling width in the coil by cooling water from the nozzle, a flow rate of cooling water from the nozzle, and a surface temperature of the coil before cooling when winding the coil.

[0011] A hot-rolled steel sheet winding device according to another aspect of the present invention is a hot-rolled steel sheet winding device which winds up the hot-rolled steel sheet from the leading end to the trailing end into a coil shape around a mandrel, and then rotates the mandrel while pressing a plurality of wrapper rolls arranged in a planetary fashion against the coil against the coil, and sprays cooling water from a nozzle against the outer peripheral plate of the coil to cool the outer peripheral portion of the coil for a predetermined cooling time, in which the predetermined cooling time for the outer peripheral portion of the coil is set to be equal to the time at which the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost plate of the coil becomes maximum. The method includes a spray control unit that controls the rotation of the mandrel and the spray of cooling water from the nozzle so as to spray cooling water from the nozzle onto the coil, and the spray control unit includes a cooling time calculation unit that calculates the cooling time at which the temperature difference between the outer surface and the inner surface of the outermost plate of the coil over the arc length of the cooling range of the coil is maximized, based on the installation position of the coil, the outer diameter of the coil, the plate thickness of the coil, the position of the nozzle, the orientation of the nozzle, the spray angle of cooling water from the nozzle, the cooling width of the coil by the cooling water from the nozzle, the flow rate of cooling water from the nozzle, and the surface temperature of the coil before cooling when winding the coil.

[0012] A method for producing a hot-rolled steel sheet according to another aspect of the present invention is characterized in that it includes a winding step of winding the hot-rolled steel sheet into a coil shape by a winding device using the above-mentioned method for winding the hot-rolled steel sheet. Effect of the Invention

[0013] According to the coiling method for hot-rolled steel sheet, the coiling device for hot-rolled steel sheet, and the manufacturing method for hot-rolled steel sheet of the present invention, it is possible to provide a coiling method for hot-rolled steel sheet, a coiling device for hot-rolled steel sheet, and a manufacturing method for hot-rolled steel sheet, which can accurately determine the cooling time at which the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost sheet of the coil is maximized for each coil based on the outer diameter and sheet thickness of the coil, the position and orientation of the nozzle for spraying cooling water, the flow rate of cooling water, etc., and can accurately demonstrate the effect of reducing springback in the outermost portion of the coil. [Brief description of the drawings]

[0014] [Figure 1] 1 is a schematic configuration diagram of a coiling device for a hot-rolled steel sheet according to an embodiment of the present invention. [Diagram 2] 2 is a schematic diagram of a spray control unit in the winding device shown in FIG. 1. [Diagram 3] 3 is a schematic configuration diagram of a cooling time calculation unit in the spray control unit shown in FIG. 2. [Figure 4] 2 is a flowchart showing a process flow in a winding control device in the winding device shown in FIG. [Diagram 5] 5 is a flowchart showing details of the process flow in step S2 (spray control step) in the flowchart showing the process flow in the take-up control device shown in FIG. [Figure 6] 6 is a flowchart showing details of the process flow in step S23 (cooling time calculation step) in the flowchart showing the process flow in step S2 (spray control step) shown in FIG. 5. [Figure 7] 1 shows the control contents by the winding control device, where (a) is wrapper roll control, (b) is spray control, (c) is air cooling control, and (d) is tail end stop control. [Figure 8] 11 is a diagram for explaining the plastic bending moment of the outermost plate of the coil. FIG. [Figure 9] FIG. 13 is a diagram for explaining a coil's own weight moment. [Figure 10] FIG. 13 is a diagram for explaining calculation of the arc length of the cooling range in a coil. [Figure 11] This is a graph showing the relationship between the temperature difference between the outer surface and the inner surface of the outermost plate of the coil and the cooling time for each plate thickness (t = 12, 15 mm). [Figure 12] This is a graph showing the relationship between the time until the maximum temperature difference is reached between the outer surface and the inner surface of the outermost plate of the coil and the plate thickness of the coil for each heat transfer coefficient (h = 6000, 10000, 20000 kcal (m2.hr·℃)-1). [Figure 13]1 is a graph showing the relationship between the time until the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost plate of the coil reaches a maximum and the heat transfer coefficient for each plate thickness (t = 10, 15, 20, 25.4 mm). [Figure 14] 13 is a diagram for explaining an ejection nozzle pattern selection unit and the process in step S25 (ejection nozzle pattern selection step). FIG. [Figure 15] 13 is a diagram illustrating how the coil is lifted up due to springback at the outermost portion of the coil when the coil is removed from the mandrel. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, embodiments of the present invention will be described with reference to the drawings. The embodiments shown below are merely examples of devices and methods for embodying the technical concept of the present invention, and the technical concept of the present invention is not limited to the following embodiments in terms of the materials, shapes, structures, arrangements, etc. of the components. In addition, the drawings are schematic, and therefore, it should be noted that the relationship between thickness and planar dimensions, ratios, etc. may differ from the actual relationship between thickness and planar dimensions, and the drawings may include parts in which the relationship between dimensions and ratios differ from one another.

[0016] FIG. 1 shows a schematic configuration of a coiling device for a hot-rolled steel sheet according to one embodiment of the present invention. A coiling device 1 for a hot-rolled steel sheet shown in FIG. 1 is provided in a hot rolling line (not shown), and is equipment for coiling a hot-rolled steel sheet after it has been hot-rolled. The hot-rolled steel sheet winding device 1 winds up the hot-rolled steel sheet S from its leading end to its trailing end into a coil shape (the hot-rolled steel sheet S wound into a coil shape will hereinafter be referred to as a coil C).

[0017] The hot-rolled steel plate S is a high-strength, thick-walled hot-rolled steel plate with a thickness of about 12 to 30 mm and a width of about 1100 to 2200 mm. Steel pipe piles and square columns are manufactured using this high-strength, thick-walled hot-rolled steel plate as a material. As described above, when the hot-rolled steel sheet S is a high-strength thick material, the springback of the outermost portion C1 of the coil C (see FIG. 15) is larger than the weight of the coil C, so that the coil C is lifted by the springback of the outermost portion C1 of the coil C as shown in FIG. 15 (the coil C is lifted from the cradle rolls 107a, 107b supporting the coil C). This causes the coil C to come into contact with the reduced diameter mandrel 102, and the coil C may not be able to come out of the mandrel 102. There is also a risk that the mandrel 102 may be damaged by the contact between the coil C and the mandrel 102. Furthermore, since the springback of the outermost portion C1 of the coil C is large after the hot-rolled steel sheet is wound, there is a risk that the restraining band (not shown) that restrains the outer periphery of the coil C may be torn off during transportation, causing the coil C to fly off at that moment.

[0018] For this reason, it is important to reduce the springback of the outermost portion C1 of the coil C. In this embodiment, the winding device 1 winds the hot-rolled steel sheet S into a coil shape around the mandrel 2, and then rotates the mandrel 2 while pressing a plurality of (four in this embodiment) wrapper rolls 3a to 3d arranged in a planetary fashion against the coil C against the coil C, and sprays cooling water from nozzles 4a and 4b against the outer peripheral plate of the coil C to cool the outer peripheral portion of the coil C for a predetermined cooling time. This makes it possible to reduce the springback of the outermost portion C1 of the coil C. This is done by cooling the outer peripheral plate of the coil C to generate a temperature difference in the plate thickness direction and increase the plastic deformation region, and then the outside of the coil C is reheated and thermally expanded by heat conduction from the inside of the coil C, and the thermal expansion of the outer peripheral portion generates a force that deforms the inside of the coil C, thereby reducing the springback.

[0019] The predetermined cooling time for the outer periphery of the coil C by the nozzles 4a and 4b is set to be equal to the time when the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost plate of the coil C is maximum. The reason for this is that the effects of the plastic deformation and thermal expansion described above are greatest at the maximum temperature difference when the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost plate of the coil C is maximum, and the springback reduction effect is maximized. The aforementioned plastic deformation region is determined by the maximum temperature difference when the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost plate of the coil C is maximum, so the springback reduction effect remains unchanged even if cooling is performed for a long period of time, and the cooling time when the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost plate of the coil C is maximum is sufficient.

[0020] In order to achieve cooling of the outer periphery of the coil C by such nozzles 4a, 4b, in this embodiment, the winding device 1 is equipped with a winding control device 10 that controls the winding of the hot-rolled steel sheet S by the mandrel 2, as shown in Figure 1, and has a wrapper roll control unit 11, a spray control unit 12, an air cooling control unit 13, and a tail end stop control unit 14.

[0021] The winding control device 10 is a computer system having a calculation function, and executes various dedicated computer programs pre-stored in the hardware. This allows the functions of the wrapper roll control unit 11, the spray control unit 12, the air-cooling control unit 13, and the tail end stop control unit 14 (steps S1 to S4 described later, see FIG. 4) to be realized on the software.

[0022] When the tail end Sa of the hot-rolled steel sheet S passes through the pinch rolls 5a, 5b, the wrapper roll control unit 11 of the winding control device 10 controls the movement of the wrapper rolls 3a-3d so as to press the wrapper rolls 3a-3d against the coil C, as shown in Fig. 7(a). A signal indicating that the tail end Sa of the hot-rolled steel sheet S has passed through the pinch rolls 5a, 5b is detected by a tail end detection sensor (not shown) provided on the wrapper rolls 3a-3d, and when the wrapper roll control unit 11 receives the signal from the tail end detection sensor, it controls the movement of the wrapper rolls 3a-3d so as to press the wrapper rolls 3a-3d against the coil C.

[0023] The wrapper roll control unit 11 is connected to a host computer 15. The host computer 15 stores various information, such as the installation position of the coil C (coil center position CP(x0, y0) in FIG. 10), the outer diameter of the coil C (D in FIG. 10), the thickness of the coil C (hot-rolled steel sheet S) (t in FIG. 8), the width of the coil C (hot-rolled steel sheet S) (not shown), and the unit weight P W , yield stress σ of coil C (hot-rolled steel sheet S) y The host computer 15 also stores information about the coil C, such as the positions of the nozzles 4a and 4b (N in FIG. 10). i (x i ,y i 10), the direction of the nozzles 4a, 4b (the tilt angle α from the horizontal state in FIG. 10), the spray angle of the cooling water from the nozzles 4a, 4b (the angle β that defines the spray width of the cooling water in FIG. 10), the cooling width Wc of the coil C by the cooling water from the nozzles 4a, 4b, and the flow rate Q of the cooling water from the nozzles 4a, 4b are stored.

[0024] In addition, after the wrapper rolls 3a to 3d are pressed against the coil C under the control of the wrapper roll control unit 11, the spray control unit 12 controls the rotation of the mandrel 2 and the spraying of cooling water from the nozzles 4a, 4b so that cooling water is sprayed from the nozzles 4a, 4b onto the outer peripheral plate of the coil C while rotating the mandrel 2, as shown in Fig. 7(b). The spray control unit 12 is also connected to the host computer 15. Here, a detailed configuration of the spray control unit 12 will be described with reference to Fig. 2. Fig. 2 is a schematic configuration diagram of the spray control unit 12 in the winding device 1 shown in Fig. 1.

[0025] As shown in FIG. 2, the spray control unit 12 includes a material information acquisition unit 12a, a cooling necessity determination unit 12b, a cooling time calculation unit 12c, a total coil cooling time calculation unit 12d, an injection nozzle pattern selection unit 12e, and a drive control unit 12f. The material information acquisition unit 12a acquires information about the coil C, such as the outer diameter D of the coil C, the thickness t of the coil C, the width of the coil C, and the unit weight P of the coil C. W , yield stress σ of coil C (hot-rolled steel sheet S) y In addition, information on the Young's modulus E of coil C (hot-rolled steel sheet S), the radius of curvature ρ of the outermost sheet in coil C, and the second moment of area I of the outermost sheet in coil C are obtained from the host computer 15.

[0026] Further, the cooling necessity determining unit 12b determines whether or not it is necessary to spray cooling water onto the outer periphery of the coil C for cooling, based on the information on the coil C acquired from the material information acquiring unit 12a. The cooling necessity determination unit 12b determines whether the plastic bending moment M of the outermost plate of the coil C is equal to the coil weight moment (=P W The coil extraction feasibility judgment is based on whether the plastic bending moment M of the outermost plate of coil C is less than the band securing moment (= σ bt w g D N) using the following formula (2) for judging whether the plastic bending moment M of the outermost plate of coil C is less than the band securing moment (= σ bt w g D N).

[0027] When the following equation (1) is satisfied, the aforementioned plastic bending moment M is smaller than the coil's own weight moment, and the coil C does not float up from the cradle rolls 7a, 7b, thereby preventing the coil C from coming into contact with the mandrel 2 when it is removed from the mandrel 2. Furthermore, when the following formula (2) is satisfied, the aforementioned plastic bending moment M is smaller than the band fastening moment, and there is no risk of the restraining band restraining the outer periphery of the coil C being torn off.

[0028]

number

[0029] M<σ bt w g D N (2) In the above formula (1), λ e is the elastic deformation rate and is expressed by the following equation (3). λ e =2δ / t=2 ρ σ y / E·t··(3) In equation (1), E is the Young's modulus E of coil C (hot-rolled steel sheet S), I is the second moment of area of ​​the outermost sheet in coil C, ρ is the radius of curvature of the outermost sheet in coil C, and in equation (3), ρ is the radius of curvature of the outermost sheet in coil C, σ y is the yield stress of the coil C (hot-rolled steel sheet S), E is the Young's modulus of the coil C (hot-rolled steel sheet S), and t is the sheet thickness of the coil C (hot-rolled steel sheet S). The cooling necessity determination unit 12b acquires this information from the material information acquisition unit 12a.

[0030] In addition, in the above formula (1), P W is the unit weight of the coil C, and this information is acquired by the cooling necessity determination unit 12b from the material information acquisition unit 12a. In addition, in formula (1), L is the distance between the centers 7a1 and 7b1 of the cradle rolls 7a and 7b that support the coil C, as shown in FIG. 9, and this information is acquired by the cooling necessity determination unit 12b from the host computer 15.

[0031] In addition, in the above-mentioned formula (2), σ is the band strength of the restraint band that restrains the outer periphery of coil C, bt is the plate thickness of the restraint band, w is the plate width of the restraint band, g is the gravitational acceleration, and N is the number of restraint bands, and these pieces of information are acquired by the cooling necessity determination unit 12b from the host computer 15. In addition, in the above-mentioned formula (2), D is the outer diameter of coil C, and this information is acquired by the cooling necessity determination unit 12b from the material information acquisition unit 12a.

[0032] If the plastic bending moment M of the outermost plate of coil C does not satisfy at least one of equations (1) and (2), it is determined that it is necessary to spray cooling water onto the outer periphery of coil C to cool it, and if the plastic bending moment M satisfies both equations (1) and (2), it is determined that it is not necessary to spray cooling water onto the outer periphery of coil C to cool it.

[0033] In addition, when the cooling necessity determination unit 12b determines that it is necessary to inject cooling water onto the outer periphery of the coil C for cooling, the cooling time calculation unit 12c calculates the cooling time based on the installation position of the coil (the coil center position CP(x0, y0) in FIG. 10), the outer diameter D of the coil C, the plate thickness t of the coil C (the hot-rolled steel plate S), the positions of the nozzles 4a and 4b (the N i (x i ,y i )), the direction of the nozzles 4a, 4b (the tilt angle α from the horizontal state in Figure 10), the spray angle of the cooling water from the nozzles 4a, 4b (the angle β that determines the spray width of the cooling water in Figure 10), the cooling width Wc of the coil C by the cooling water from the nozzles 4a, 4b, the flow rate Q of the cooling water from the nozzles 4a, 4b, and the surface temperature T0 of the coil C before cooling when winding the coil, a cooling time τ at which the temperature difference between the outer surface and the inner surface of the outermost plate of the coil C over the arc length Lc of the cooling range in the coil C is maximized is calculated.

[0034] Here, the cooling time calculation unit 12c will be described in detail. Fig. 3 shows a schematic configuration of the cooling time calculation unit 12c. As shown in FIG. 3, the cooling time calculation unit 12c includes a cooling range arc length calculation unit 12ca, a flow rate density calculation unit 12cb, a heat transfer coefficient calculation unit 12cd, and a maximum temperature difference cooling time calculation unit 12ce. The cooling range arc length calculation unit 12ca calculates the coil installation position (coil center position CP (x0, y0) in FIG. 10), the outer diameter D of the coil C, the positions of the nozzles 4a and 4b (N in FIG. 10), i (x i ,y i 10), the orientation of the nozzles 4a, 4b (the tilt angle α from the horizontal state in FIG. 10), and the spray angle of the cooling water from the nozzles 4a, 4b (the angle β that determines the spray width of the cooling water in FIG. 10). Based on this, the arc length Lc of the cooling range in the coil C is calculated.

[0035] In FIG. 10, the arc length Lc of the cooling range in the coil C is determined by the nozzles 4a and 4b (position N) which are inclined by α. i (x i ,y i )) at a spray angle β, and the length on the outer periphery of the coil is from end point P2 of the cooling water W where the cooling water W comes into contact with the outer periphery plate of the coil C to end point P1 of the cooling water W. The positions of the end points P1 and P2 of the cooling water W are the positions of the nozzles 4a and 4b (N in FIG. 10). i (x i ,y i 10), the direction of the nozzles 4a, 4b (the tilt angle α from the horizontal state in FIG. 10), the spray angle of the cooling water from the nozzles 4a, 4b (the angle β that determines the spray width of the cooling water in FIG. 10), the installation position of the coil (the coil center position CP(x0, y0) in FIG. 10), and the outer diameter D of the coil C.

[0036] The length of the cooling water W on the outer circumference of the coil from end point P2 to end point P1 is expressed as D / 2×(θ1-θ2), where θ1 is the rotation angle from a predetermined point P0 on the outer circumference of the coil C to end point P1, and θ2 is the rotation angle from the predetermined point P0 on the outer circumference of the coil C to end point P2, and D is the outer diameter of the coil C. Therefore, the arc length Lc of the cooling range in the coil C can be calculated by the following formula (4). Lc = D / 2 × (θ1 - θ2) (4) Here, Lc is the arc length (mm) of the cooling range in coil C, D is the outer diameter (mm) of coil C, and θ1 and θ2 are the rotation angles (rad).

[0037] The coil installation position (coil center position CP (x0, y0) in FIG. 10), the outer diameter D of the coil C, the positions of the nozzles 4a and 4b (N in FIG. 10) i (x i ,y i 10), the orientation of the nozzles 4a, 4b (tilt angle α from the horizontal state in FIG. 10), and the spray angle of the cooling water from the nozzles 4a, 4b (angle β that defines the spray width of the cooling water in FIG. 10) are acquired by the cooling range arc length calculation unit 12ca from the host computer 15.

[0038] Furthermore, the flow density calculation unit 12cb calculates a flow density w based on the arc length Lc of the cooling range calculated by the cooling range arc length calculation unit 12ca, the cooling width Wc in the coil C by the cooling water from the nozzles 4a and 4b, and the flow rate Q of the cooling water from the nozzles 4a and 4b. The flow density w of the cooling water is calculated by the following formula (5). w=Q / (Ac×10 -6 )=Q / (Lc×Wc×10 -6 ) ···(5)

[0039] where w is the flow density of the cooling water (L / (min m 2 ), Q is the flow rate of cooling water from the nozzles 4a and 4b (L / min), and Ac is the specific cooling area (mm 2 ), Lc is the arc length of the cooling range in coil C (mm), and Wc is the cooling width in coil C by the cooling water from nozzles 4a and 4b (the width cooled by the cooling water in the width direction of C) (mm). The flow density calculation unit 12cb obtains information on the cooling width Wc and the flow rate Q of the cooling water from the host computer 15.

[0040] Further, the heat transfer coefficient calculation unit 12cd calculates the heat transfer coefficient h based on the flow density w calculated by the flow density calculation unit 12cb and the surface temperature T0 of the coil C before cooling during coil winding. The heat transfer coefficient h is calculated using the following equation (6). h=494.3w 0.595 ×10 -0.00179T0 (6) where h is the heat transfer coefficient (kcal(m 2 .hr·℃) -1 ), w is the flow density of the cooling water (L / (min m 2 ), T0 is the surface temperature of coil C before cooling during coil winding (℃).

[0041] The surface temperature T0 of the coil C before cooling during coil winding is measured by a thermometer 6 installed on the exit side of the pinch rolls 5a and 5b as shown in Fig. 1. Information on the measured surface temperature T0 of the coil C before cooling during coil winding is sent from the thermometer 6 to the heat transfer coefficient calculation unit 12cd. In addition, the surface temperature T0 of the coil C before cooling during coil winding may be actually measured by the thermometer 6, or a target surface temperature T0 may be determined in advance and stored in the host computer 15, and the heat transfer coefficient calculation unit 12cd may obtain information on the target surface temperature T0 from the host computer 15.

[0042] In addition, the maximum temperature difference cooling time calculation unit 12ce calculates the cooling time τ at which the temperature difference between the outer surface and the inner surface of the outermost plate of coil C over the arc length Lc of the cooling range is maximized based on the heat transfer coefficient h calculated by the heat transfer coefficient calculation unit 12cd and the plate thickness t of coil C. FIG. 11 shows the relationship between the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost plate of coil C and the cooling time for each plate thickness (t=15, 25 mm). Also, FIG. 12 shows the relationship between the time until the maximum temperature difference is reached between the outer peripheral surface and the inner peripheral surface of the outermost plate of the coil and the plate thickness of the coil, as a function of the heat transfer coefficient (h=6000, 10000, 20000 kcal(m 2 .hr·℃) -1 Furthermore, Fig. 13 shows the relationship between the time until the maximum temperature difference is reached between the outer peripheral surface and the inner peripheral surface of the outermost plate of the coil and the heat transfer coefficient for each plate thickness (t = 10, 15, 20, 25.4 mm).

[0043] As shown in FIG. 11, the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost plate of coil C increases as the cooling time increases, and then gradually decreases after the temperature difference reaches a maximum. In FIG. 11, when the plate thickness t of coil C is 12 mm, the cooling time until the aforementioned temperature difference reaches a maximum is 1.5 sec, and when the plate thickness t of coil C is 25 mm, the cooling time until the aforementioned temperature difference reaches a maximum is 5.5 sec. In the graph of FIG. 11, when the heat transfer coefficient is 20,000 kcal (m 2 .hr·℃) -1 The data shown is for the time.

[0044] The time until the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost plate of coil C becomes maximum (maximum temperature difference) increases with an increase in plate thickness t of coil C, as shown in Figs. 11 and 12. Also, the time until the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost plate of coil C becomes maximum (maximum temperature difference) decreases with an increase in heat transfer coefficient h, as shown in Fig. 13. In the graph of Fig. 12, when the heat transfer coefficient is 6000 kcal (m 2 .hr·℃) -1 , 10000kcal(m 2 .hr·℃) -1 , 20000kcal(m 2 .hr·℃) -1 13 shows data when the thickness t of the coil C is 10 mm, 15 mm, 20 mm, and 25.4 mm.

[0045] The time until the temperature difference between the outer surface and the inner surface of the outermost plate of coil C reaches its maximum (maximum temperature difference), derived from the graphs shown in Figures 12 and 13, is proportional to the power of the plate thickness t and inversely proportional to the power of the heat transfer coefficient h, and is expressed by the following equation (7). Therefore, the maximum temperature difference cooling time calculation unit 12ce calculates the cooling time τ at which the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost plate of the coil C over the arc length Lc of the cooling range is maximized based on the following equation (7).

[0046]

number

[0047] Here, τ is the cooling time (sec) at which the temperature difference between the outer and inner surfaces of the outermost sheet of coil C over the arc length Lc of the cooling range becomes maximum, t is the sheet thickness (mm) of coil C (hot-rolled steel sheet S), and h is the heat transfer coefficient (kcal (m 2 .hr·℃) -1 The maximum temperature difference cooling time calculation unit 12ce acquires information on the thickness t of the coil C (hot-rolled steel sheet S) from the host computer 15.

[0048] Next, the total coil cooling time calculation unit 12d of the spray control unit 12 shown in FIG. 2 calculates the total coil cooling time T when cooling water is sprayed from the nozzles 4a and 4b to cool the outer periphery of the coil C for one revolution based on the cooling time τ at which the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost plate of the coil C over the arc length Lc of the cooling range calculated by the cooling time calculation unit 12c, the arc length Lc of the cooling range, and the outer diameter D of the coil C. total The information on the outer diameter D of the coil C is obtained by the coil total cooling time calculation unit 12d from the host computer 15. The rotation speed ω of the mandrel 2 can be calculated by the following equation (8).

[0049]

number

[0050] Here, ω is the rotational speed (rpm) of mandrel 2, Lc is the arc length (mm) of the cooling range in coil C, τ is the cooling time (sec) at which the temperature difference between the outer surface and the inner surface of the outermost plate of coil C over the arc length Lc of the cooling range becomes maximum, and D is the outer diameter of coil C (mm). The total coil cooling time T when cooling the outer periphery of the coil C by one revolution by injecting cooling water from the nozzles 4a and 4b is total can be calculated using the following formula (9). T total =1 / ω (9)

[0051] Here, T totalis the total coil cooling time (min) when cooling water is sprayed from the nozzles 4a and 4b to cool the outer periphery of the coil C for one revolution, and ω is the rotation speed (rpm) of the mandrel 2. Here, since multiple nozzles (in this embodiment, two nozzles, nozzle 4a and nozzle 4b) are installed along the outer periphery of coil C, it is assumed that cooling water is sprayed from each of the multiple nozzles 4a, 4b onto the outer periphery of coil C, and the processing in the cooling time calculation unit 12c and total coil cooling time calculation unit 12d described above is carried out for each of the multiple nozzles 4a, 4b.

[0052] Then, in the coil total cooling time calculation unit 12d, the rotation speed ω of the mandrel 2 and the total coil cooling time T when cooling the outer periphery of the coil C for one revolution are calculated for each of the multiple nozzles 4a and 4b. total Calculate the following: In addition, the spray nozzle pattern selection unit 12e of the spray control unit 12 shown in Figure 2 selects the spray nozzle from which cooling water is sprayed (only nozzle 4a, only nozzle 4b, or both nozzle 4a and nozzle 4b), the rotational speed ω of the mandrel 2 (ω2, ω1, or ω2 and ω1, whichever is faster), and the rotational angle of the mandrel 2 (360°, 360°, or θ1), as shown in Figure 14.

[0053] The ejection nozzle pattern selection unit 12e will now be described in detail. The injection nozzle pattern selection unit 12e selects the total coil cooling time T total Compare the shortest time among the above with the time in case B below. And the total coil cooling time T in the case of A below total When the shortest time among the plurality of nozzles 4a and 4b is shorter than the time in the case of B described below, the injection nozzle pattern selection unit 12e selects one of the nozzles 4a and 4b that is the shortest in the total coil cooling time T totalThe injection nozzle pattern selection unit 12e selects the nozzle having the shortest length (only nozzle 4a or only nozzle 4b). Furthermore, the injection nozzle pattern selection unit 12e selects the rotation speed (ω2 or ω1) of the mandrel 2 for the selected nozzle (only nozzle 4a or only nozzle 4b) as the rotation speed ω of the mandrel 2. Furthermore, the injection nozzle pattern selection unit 12e selects the rotation angle of the mandrel for one revolution of the coil C (360° or 360°) for the selected nozzle (only nozzle 4a or only nozzle 4b) as the rotation angle of the mandrel 2.

[0054] On the other hand, the time in the case of B below is the total coil cooling time T total If the time is shorter than the shortest time among the above, the injection nozzle pattern selection unit 12e selects all of the nozzles 4a, 4b as injection nozzles for injecting cooling water. Furthermore, the injection nozzle pattern selection unit 12e selects, as the rotation speed of the mandrel 2, the rotation speed (ω2 or ω1) of the mandrel 2 that has the faster rotation speed out of the rotation speed ω2 of the mandrel 2 for any one nozzle 4a and the rotation speed ω1 of the mandrel 2 for the adjacent nozzle 4b. Furthermore, the injection nozzle pattern selection unit 12e selects, as the rotation angle of the mandrel 2, the rotation angle (θ1) from point a in the cooling range on the outer periphery of the coil C by any one nozzle 4a to point b in the cooling range on the outer periphery of the coil C by the adjacent nozzle 4b.

[0055] A: The total coil cooling time T calculated by the total coil cooling time calculation unit 12d when cooling one revolution of the outer periphery of the coil C for each of the multiple nozzles 4a and 4b total B: Assume any one of the multiple nozzles 4a, 4b, that has the largest rotation angle θ1 from point a in the cooling range on the outer periphery of the coil C by any one of the nozzles 4a to point b in the cooling range on the outer periphery of the coil C by the adjacent nozzle 4b adjacent to that nozzle 4a in the rotation direction of the mandrel 2. Then, the time when the mandrel is rotated by the rotation angle θ1 from point a in the cooling range by any one of the nozzles 4a to point b in the cooling range by the adjacent nozzle 4b at the rotation speed of the mandrel 2 (ω2 or ω1) which is faster between the rotation speed ω1 of the mandrel 2 for any one of the nozzles 4a and the rotation speed ω2 of the mandrel 2 for the adjacent nozzle 4b

[0056] In addition, when only one nozzle is installed, specifically, for example, when only nozzle 4a is installed on the outer periphery of coil C, processing is performed in cooling time calculation unit 12c and total coil cooling time calculation unit 12d for nozzle 4a, assuming that cooling water is sprayed from nozzle 4a onto the outer periphery of coil C. Then, in the coil total cooling time calculation unit 12d, the rotation speed ω2 of the mandrel 2 and the total coil cooling time T total Calculate the following: Then, the jet nozzle pattern selection unit 12e selects the nozzle 4a as the jet nozzle for jetting cooling water, the rotation speed ω2 of the mandrel 2, and the rotation angle of the mandrel 2, 360°.

[0057] 2 controls the rotation of the mandrel 2 and the injection of the injection nozzle based on the injection nozzle (only nozzle 4a, only nozzle 4b, or both nozzles 4a and 4b) that injects cooling water, the rotation speed ω of the mandrel 2 (ω2, ω1, or ω2 and ω1, whichever is faster), and the rotation angle (360°, 360°, or θ1) of the mandrel 2. A control signal from the drive control unit 12f is sent to a drive device of the mandrel 2 and an injection device of the injection nozzle (not shown), and these drive device of the mandrel 2 and the injection device of the injection nozzle control the rotation of the mandrel 2 and the injection of the injection nozzle (flow rate Q described above) based on the control signal from the drive control unit 12f.

[0058] In addition, the control signal from the drive control unit 12f is also transmitted to the drive devices of the wrapper rolls 3a to 3d, and the drive devices of the wrapper rolls 3a to 3d control the rotation of the wrapper rolls 3a to 3d to be synchronized with the rotation of the mandrel 2 based on the control signal from the drive control unit 12f. The time for spraying cooling water from the nozzles 4a and 4b by the spray control unit 12 is the total coil cooling time T total This is the shortest time when compared with the time in case B.

[0059] 7(c), after the spray control unit 12 has finished controlling the spraying of cooling water from the nozzles 4a, 4b, the air-cooling control unit 13 of the winding control device 10 shown in Fig. 1 rotates the mandrel 2 and the wrapper rolls 3a-3d for a preset time to air-cool the coil C. The air-cooling control unit 13 is also connected to the host computer 15. After the air-cooling control of the coil C by the air-cooling control unit 13 is completed, the tail end stop control unit 14 of the winding control device 10 controls the rotation of the mandrel 2 and the wrapper rolls 3a to 3d to stop the tail end Sa of the coil C at the designated tail end position P, as shown in Fig. 7(d). Then, the tail end stop control unit 14 controls the wrapper rolls 3a to 3d to be released after the cradle rolls 7a, 7b support the lower side of the coil C. The tail end stop control unit 14 is also connected to the host computer 15.

[0060] Thereafter, when the coil C is to be removed from the mandrel 2, the mandrel 2 contracts in diameter as shown in FIG. 7(d), allowing the coil C to be removed from the mandrel 2. Here, according to the hot-rolled steel sheet winding device 1 according to the present embodiment, the spray control unit 12 determines the coil installation position (coil center position CP(x0, y0) in FIG. 10), the outer diameter D of the coil C, the sheet thickness t of the coil C (hot-rolled steel sheet S), the positions of the nozzles 4a and 4b (N in FIG. 10), i (x i ,y i 10), the direction of the nozzles 4a, 4b (the tilt angle α from the horizontal state in FIG. 10), the spray angle of the cooling water from the nozzles 4a, 4b (the angle β that determines the spray width of the cooling water in FIG. 10), the cooling width Wc of the coil C by the cooling water from the nozzles 4a, 4b, the flow rate Q of the cooling water from the nozzles 4a, 4b, and the surface temperature T0 of the coil C before cooling when winding the coil.

[0061] In this way, when determining the cooling time τ at which the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost plate of the coil C is maximized, the outer diameter D of the coil C, the plate thickness t, and the positions N of the nozzles 4a and 4b for injecting the cooling water are taken into consideration. i (x i ,y i ), direction α, flow rate Q of cooling water, etc., can be accurately determined for each coil C, thereby providing a coiling device 1 for hot-rolled steel sheet that can accurately reduce springback at the outermost periphery of the coil C. Because the effect of reducing springback of the outermost portion of the coil C can be achieved with high precision, it is possible to avoid the risk of the coil C being lifted by the springback of the outermost portion C1 of the coil C when the coil C is removed from the mandrel 2, causing the coil C to come into contact with the reduced-diameter mandrel 102. In addition, because the springback of the outermost portion C1 of the coil C is reduced after the hot-rolled steel sheet S is wound, it is possible to avoid the risk of the restraining band restraining the outer periphery of the coil C being torn off during transportation.

[0062] In addition, according to the hot-rolled steel sheet winding device 1 according to the present embodiment, the cooling time calculation unit 12c calculates the cooling time by calculating the coil installation position CP (x0, y0), the outer diameter D of the coil C, the sheet thickness t of the coil C, the positions N of the nozzles 4a and 4b, i (x i ,y i 10), the direction of the nozzles 4a, 4b (tilt angle α from the horizontal state in FIG. 10), and the spray angle of the cooling water from the nozzles 4a, 4b (angle β that defines the spray width of the cooling water in FIG. 10). The cooling time calculation unit 12c also includes a flow density calculation unit 12cb that calculates a flow density w based on the arc length Lc of the cooling range calculated by the cooling range arc length calculation unit 12ca, the cooling width Wc of the coil C by the cooling water from the nozzles 4a, 4b, and the flow rate Q of the cooling water from the nozzles 4a, 4b. The cooling time calculation unit 12c also includes a heat transfer coefficient calculation unit 12cd that calculates a heat transfer coefficient h based on the flow density w calculated by the flow density calculation unit 12cb and the surface temperature T0 of the coil C before cooling when winding the coil. Furthermore, the cooling time calculation unit 12c is equipped with a maximum temperature difference cooling time calculation unit 12ce that calculates the cooling time τ at which the temperature difference between the outer surface and the inner surface of the outermost plate of the coil C over the arc length Lc of the cooling range is maximized, based on the heat transfer coefficient h calculated by the heat transfer coefficient calculation unit 12cd and the plate thickness t of the coil C. This makes it possible to determine with greater accuracy the cooling time τ at which the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost plate of the coil C becomes maximum.

[0063] Further, according to the hot-rolled steel sheet winding device 1 according to the present embodiment, the spray control unit 12 calculates the cooling time τ at which the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost sheet of the coil C over the arc length Lc of the cooling range is maximized, based on the arc length Lc of the cooling range, and the outer diameter D of the coil C, and calculates the rotation speed ω of the mandrel 2 and the total coil cooling time T when cooling water is sprayed from the nozzles 4a and 4b to cool the outer peripheral portion of the coil C for one revolution. total The coil total cooling time calculation unit 12d calculates the following: As a result, the rotation speed ω of the mandrel 2 and the total coil cooling time T when cooling the outer periphery of the coil C for one revolution by injecting cooling water from the nozzles 4a and 4b are total It is possible to calculate with high accuracy.

[0064] According to the hot-rolled steel sheet winding device 1 of this embodiment, a plurality of nozzles 4a, 4b are installed along the outer periphery of the coil C. Then, assuming that cooling water is sprayed from each of the plurality of nozzles 4a, 4b onto the outer periphery of the coil, the cooling time calculation unit 12c and the total coil cooling time calculation unit 12d perform processing for each of the plurality of nozzles 4a, 4b, and the total coil cooling time calculation unit 12d calculates the rotation speed ω of the mandrel 2 and the total coil cooling time T when cooling the outer periphery of the coil C for one revolution for each of the plurality of nozzles 4a, 4b. total Calculate the following: As a result, for each of the multiple nozzles 4a and 4b, the rotation speed ω of the mandrel 2 and the total coil cooling time T when cooling the outer periphery of the coil C for one revolution by spraying cooling water from the nozzles 4a and 4b are total It is possible to calculate with high accuracy.

[0065] In addition, according to the hot-rolled steel sheet winding device 1 of this embodiment, the spray control unit 12 is equipped with a spray nozzle pattern selection unit 12e that selects the spray nozzle (only nozzle 4a, only nozzle 4b, or both nozzle 4a and nozzle 4b) from which cooling water is sprayed, the rotational speed ω of the mandrel 2 (ω2, ω1, or ω2 and ω1, whichever is the faster rotational speed), and the rotational angle of the mandrel 2 (360°, 360°, or θ1).

[0066] The injection nozzle pattern selection unit 12e selects the total coil cooling time T total The shortest time among these is compared with the time in case B described above. And the total coil cooling time T in the above case A total When the shortest time among the multiple nozzles 4a and 4b is shorter than the time in the case of B, the injection nozzle pattern selection unit 12e selects the nozzle that is the shortest among the multiple nozzles 4a and 4b for injecting the cooling water and that is the shortest among the multiple nozzles 4a and 4b for injecting the cooling water. total The injection nozzle pattern selection unit 12e selects the nozzle having the shortest length (only nozzle 4a or only nozzle 4b). Furthermore, the injection nozzle pattern selection unit 12e selects the rotation speed (ω2 or ω1) of the mandrel 2 for the selected nozzle (only nozzle 4a or only nozzle 4b) as the rotation speed ω of the mandrel 2. Furthermore, the injection nozzle pattern selection unit 12e selects the rotation angle (360° or 360°) of the mandrel 2 for one revolution of the coil C for the selected nozzle (only nozzle 4a or only nozzle 4b) as the rotation angle of the mandrel 2.

[0067] On the other hand, the time in the case of B is the total coil cooling time T total If the time is shorter than the shortest time among the above, the injection nozzle pattern selection unit 12e selects all of the nozzles 4a, 4b as injection nozzles for injecting cooling water. Furthermore, the injection nozzle pattern selection unit 12e selects, as the rotation speed of the mandrel 2, the rotation speed (ω2 or ω1) of the mandrel 2 that has the faster rotation speed out of the rotation speed ω2 of the mandrel 2 for any one nozzle 4a and the rotation speed ω1 of the mandrel 2 for the adjacent nozzle 4b. Furthermore, the injection nozzle pattern selection unit 12e selects, as the rotation angle of the mandrel 2, the rotation angle (θ1) from point a in the cooling range on the outer periphery of the coil C by any one nozzle 4a to point b in the cooling range on the outer periphery of the coil C by the adjacent nozzle 4b.

[0068] As a result, when multiple nozzles 4a, 4b are installed, the nozzle that sprays the cooling water (only nozzle 4a, only nozzle 4b, or both nozzle 4a and nozzle 4b), the rotation speed ω of the mandrel 2 (ω2, ω1, or ω2 and ω1, whichever is the faster rotation speed), and the rotation angle of the mandrel 2 (360°, 360°, or θ1) can be selected so as to shorten the cooling time, thereby shortening the cooling time of the coil.

[0069] Next, the process flow in the winding control device 10 will be described with reference to Figs. 4 to 6. Fig. 4 is a flowchart showing the process flow in the winding control device 10. Fig. 5 is a flowchart showing details of the process flow in step S2 (spray control step) in the flowchart showing the process flow in the winding control device shown in Fig. 4. Fig. 6 is a flowchart showing details of the process flow in step S23 (cooling time calculation step) in the flowchart showing the process flow in step S2 (spray control step) shown in Fig. 5.

[0070] First, in step S1, the wrapper roll control unit 11 of the winding control device 10 controls the movement of the multiple wrapper rolls 3a to 3d so as to press the wrapper rolls 3a to 3d against the coil C, as shown in Figure 7(a), when the tail end portion Sa of the hot-rolled steel sheet S passes through the pinch rolls 5a, 5b (wrapper roll control step). Next, in step S2, after the multiple wrapper rolls 3a to 3d are pressed against the coil C in step S1 (wrapper roll control step), the spray control unit 12 of the winding control device 10 controls the rotation of the mandrel 2 and the spraying of cooling water from the nozzles 4a, 4b so as to spray cooling water from the nozzles 4a, 4b onto the outer plate of the coil C while rotating the mandrel 2, as shown in Figure 7 (b) (spray control step).

[0071] The details of this step S2 (spray control step) will be described with reference to FIG. First, in step S21, the material information acquisition unit 12a of the spray control unit 12 acquires information about the coil C, such as the outer diameter D of the coil C, the plate thickness t of the coil C, the plate width of the coil C, and the unit weight P of the coil C. W , yield stress σ of coil C (hot-rolled steel sheet S) y In addition, information on the Young's modulus E of coil C (hot-rolled steel sheet S), the radius of curvature ρ of the outermost sheet in coil C, and the second moment of area I of the outermost sheet in coil C are obtained from the host computer 15 (material information acquisition step).

[0072] Next, in step S22, the cooling necessity determining unit 12b determines whether or not it is necessary to spray cooling water onto the outer periphery of the coil C to cool it, based on the information about the coil C acquired in step S21 (cooling necessity determining step). The cooling necessity determination unit 12b determines whether the plastic bending moment M of the outermost plate of the coil C is equal to the coil weight moment (=P W The second is a band fastening feasibility judgment that judges whether the plastic bending moment M of the outermost plate of coil C is less than the band fastening moment (= σ bt w g D N) using the band fastening feasibility judgment formula (2) described above.

[0073] Then, when the plastic bending moment M of the outermost plate of the coil C does not satisfy at least one of the formulas (1) and (2), it is determined that it is necessary to spray cooling water onto the outer periphery of the coil C for cooling, and the process proceeds to step S23. On the other hand, when the plastic bending moment M satisfies both the formulas (1) and (2), it is determined that it is not necessary to spray cooling water onto the outer periphery of the coil C for cooling, and the process in step S2 (spray control step) ends.

[0074] Next, in step S23, the cooling time calculation unit 12c calculates the installation position of the coil (the coil center position CP (x0, y0) in FIG. 10), the outer diameter D of the coil C, the plate thickness t of the coil C (hot-rolled steel sheet S), the positions of the nozzles 4a and 4b (N in FIG. 10), i (x i,y i )), the direction of the nozzles 4a, 4b (the tilt angle α from the horizontal state in Figure 10), the spray angle of cooling water from the nozzles 4a, 4b (the angle β that determines the spray width of the cooling water in Figure 10), the cooling width Wc of the coil C by the cooling water from the nozzles 4a, 4b, the flow rate Q of the cooling water from the nozzles 4a, 4b, and the surface temperature T0 of the coil C before cooling when winding the coil, a cooling time τ at which the temperature difference between the outer surface and the inner surface of the outermost plate of the coil C over the arc length Lc of the cooling range in the coil C is maximized (cooling time calculation step).

[0075] The details of the process flow in step S23 will be described with reference to FIG. First, in step S231, the cooling range arc length calculation unit 12ca of the cooling time calculation unit 12c calculates the coil installation position (coil center position CP(x0, y0) in FIG. 10), the outer diameter D of the coil C, the positions of the nozzles 4a and 4b (N in FIG. 10), i (x i ,y i 10), the direction of the nozzles 4a, 4b (tilt angle α from the horizontal state in FIG. 10), and the spray angle of the cooling water from the nozzles 4a, 4b (angle β that determines the spray width of the cooling water in FIG. 10), the arc length Lc of the cooling range in the coil C is calculated as described above in (4) (cooling range arc length calculation step).

[0076] Next, in step S232, the flow density calculation unit 12cb calculates the flow density w using the aforementioned equation (5) based on the arc length Lc of the cooling range calculated in step S231, the cooling width Wc in the coil C by the cooling water from the nozzles 4a, 4b, and the flow rate Q of the cooling water from the nozzles 4a, 4b (flow density calculation step). Next, in step S233, the heat transfer coefficient calculation unit 12cd calculates the heat transfer coefficient h using the aforementioned equation (6) based on the flow rate density w calculated in step S232 and the surface temperature T0 of the coil C before cooling during coil winding (heat transfer coefficient calculation step).

[0077] Next, in step S234, the maximum temperature difference cooling time calculation unit 12ce calculates the cooling time τ at which the temperature difference between the outer surface and the inner surface of the outermost plate of coil C over the arc length Lc of the cooling range is maximized based on the heat transfer coefficient h calculated by the heat transfer coefficient calculation unit 12cd and the plate thickness t of coil C using the aforementioned equation (7) (maximum temperature difference cooling time calculation step). This ends the process in step S23. When the process in step S23 is completed, the process proceeds to step S24.

[0078] In step S24, the total coil cooling time calculation unit 12d of the spray control unit 12 calculates the rotation speed ω of the mandrel 2 and the total coil cooling time T when cooling water is sprayed from the nozzles 4a and 4b to cool one revolution of the outer periphery of the coil C based on the cooling time τ at which the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost plate of the coil C over the arc length Lc of the cooling range is maximized, the arc length Lc of the cooling range, and the outer diameter D of the coil C, which are calculated in step S23 (cooling time calculation step). total (total coil cooling time calculation step).

[0079] The rotation speed ω of the mandrel 2 can be calculated by the above-mentioned formula (8). In addition, the total coil cooling time T when cooling the outer periphery of the coil C by one revolution by injecting cooling water from the nozzles 4a and 4b is total can be calculated using the above formula (9). Here, since multiple nozzles (in this embodiment, two nozzles, nozzle 4a and nozzle 4b) are installed along the outer periphery of coil C, it is assumed that cooling water is sprayed from each of the multiple nozzles 4a, 4b onto the outer periphery of coil C, and the above-mentioned steps S23 and S24 are performed for each of the multiple nozzles 4a, 4b.

[0080] Then, in step S24, the rotation speed ω of the mandrel 2 and the total coil cooling time T when cooling the outer periphery of the coil C for one revolution are calculated for each of the nozzles 4a and 4b. total Calculate the following: Next, in step S25, the spray nozzle pattern selection unit 12e of the spray control unit 12 selects the injection nozzle from which the cooling water will be injected (only nozzle 4a, only nozzle 4b, or both nozzle 4a and nozzle 4b), the rotational speed ω of the mandrel 2 (ω2, ω1, or ω2 and ω1, whichever is the faster rotational speed), and the rotational angle of the mandrel 2 (360°, 360°, or θ1) (injection nozzle pattern selection step).

[0081] In step S25, the injection nozzle pattern selection unit 12e first selects the total coil cooling time T total The shortest time among these is compared with the time in case B described above. And the total coil cooling time T in the above case A total If the shortest time among the multiple nozzles 4a and 4b is shorter than the time in the above-mentioned case B, the injection nozzle pattern selection unit 12e selects the nozzle that is the shortest among the multiple nozzles 4a and 4b for injecting the cooling water and that is the shortest among the multiple nozzles 4a and 4b for injecting the cooling water. total The injection nozzle pattern selection unit 12e selects the nozzle having the shortest length (only nozzle 4a or only nozzle 4b). Furthermore, the injection nozzle pattern selection unit 12e selects the rotation speed (ω2 or ω1) of the mandrel 2 for the selected nozzle (only nozzle 4a or only nozzle 4b) as the rotation speed ω of the mandrel 2. Furthermore, the injection nozzle pattern selection unit 12e selects the rotation angle of the mandrel for one revolution of the coil C (360° or 360°) for the selected nozzle (only nozzle 4a or only nozzle 4b) as the rotation angle of the mandrel 2.

[0082] On the other hand, the time in the case of B is the total coil cooling time T totalIf the time is shorter than the shortest time among the above, the injection nozzle pattern selection unit 12e selects all of the nozzles 4a, 4b as injection nozzles for injecting cooling water. Furthermore, the injection nozzle pattern selection unit 12e selects, as the rotation speed of the mandrel 2, the rotation speed (ω2 or ω1) of the mandrel 2 that has the faster rotation speed out of the rotation speed ω2 of the mandrel 2 for any one nozzle 4a and the rotation speed ω1 of the mandrel 2 for the adjacent nozzle 4b. Furthermore, the injection nozzle pattern selection unit 12e selects, as the rotation angle of the mandrel 2, the rotation angle (θ1) from point a in the cooling range on the outer periphery of the coil C by any one nozzle 4a to point b in the cooling range on the outer periphery of the coil C by the adjacent nozzle 4b.

[0083] In addition, when only one nozzle is installed, specifically, for example, when only the nozzle 4a is installed on the outer periphery of the coil C, steps S23 and S24 are performed for the nozzle 4a, assuming that cooling water is sprayed from the nozzle 4a onto the outer periphery of the coil C. Then, in step S24, the total coil cooling time calculation unit 12d calculates, for the nozzle 4a, the rotation speed ω2 of the mandrel 2 and the total coil cooling time T total Then, in step S25, the jet nozzle pattern selection unit 12e selects the nozzle 4a as the jet nozzle for jetting cooling water, the rotation speed ω2 of the mandrel 2, and the rotation angle of the mandrel 2, 360°.

[0084] Next, in step S26, the drive control unit 12f of the spray control unit 12 controls the rotation of the mandrel 2 and the spray of the spray nozzle based on the spray nozzle (only nozzle 4a, only nozzle 4b, or both nozzle 4a and nozzle 4b) that sprays cooling water selected in step S25 (spray nozzle pattern selection step), the rotation speed ω of the mandrel 2 (ω2, ω1, or ω2 and ω1, whichever is the faster rotational speed), and the rotation angle of the mandrel 2 (360°, 360°, or θ1) (drive control step).

[0085] The control signal from the drive control unit 12f is transmitted to the drive device of the mandrel 2 and the injection device of the injection nozzle (not shown), and these drive device of the mandrel 2 and the injection device of the injection nozzle control the rotation of the mandrel 2 and the injection of the injection nozzle (flow rate is Q as described above) based on the control signal from the drive control unit 12f. In addition, the control signal from the drive control unit 12f is also transmitted to the drive devices of the wrapper rolls 3a to 3d, and the drive devices of the wrapper rolls 3a to 3d control the rotation of the wrapper rolls 3a to 3d to be synchronized with the rotation of the mandrel 2 based on the control signal from the drive control unit 12f.

[0086] The time for spraying cooling water from the nozzles 4a and 4b by the spray control unit 12 is the total coil cooling time T total This is the shortest time when compared with the time in case B. This ends the process in step S2, and the process proceeds to the next step S3. In step S3, after the processing in step S2 is completed, the air-cooling control unit 13 of the winding control device 10 rotates the mandrel 2 and the wrapper rolls 3a to 3d for a preset time as shown in FIG. 7(c) to air-cool the coil C (air-cooling control step).

[0087] Finally, in step S4, after the processing in step S3 is completed, the tail end stop control unit 14 of the winding control device 10 controls the rotation of the mandrel 2 and the wrapper rolls 3a to 3d so as to stop the tail end Sa of the coil C at the designated tail end position P, as shown in Figure 7 (d) (tail end stop control step). Then, in step S24, the tail end stop control unit 14 controls the cradle rolls 7a, 7b to support the lower side of the coil C, and then releases the wrapper rolls 3a to 3d. Thereafter, when the coil C is to be removed from the mandrel 2, the mandrel 2 contracts in diameter as shown in FIG. 7(d), allowing the coil C to be removed from the mandrel 2.

[0088] In this way, according to the coiling method of the hot-rolled steel sheet according to the present embodiment, the spray control step (step S2) is carried out based on the coil installation position (coil center position CP(x0, y0) in FIG. 10), the outer diameter D of the coil C, the thickness t of the coil C (hot-rolled steel sheet S), the positions of the nozzles 4a and 4b (N in FIG. 10), i (x i ,y i 10), the direction of the nozzles 4a, 4b (the tilt angle α from the horizontal state in FIG. 10), the spray angle of the cooling water from the nozzles 4a, 4b (the angle β that determines the spray width of the cooling water in FIG. 10), the cooling width Wc of the coil C by the cooling water from the nozzles 4a, 4b, the flow rate Q of the cooling water from the nozzles 4a, 4b, and the surface temperature T0 of the coil C before cooling when winding the coil.

[0089] In this way, when determining the cooling time τ at which the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost plate of the coil C is maximized, the outer diameter D of the coil C, the plate thickness t, and the positions N of the nozzles 4a and 4b for injecting the cooling water are taken into consideration. i (x i ,y i ), direction α, flow rate Q of cooling water, etc., can be accurately determined for each coil C, thereby providing a coiling method for hot-rolled steel sheet that can accurately reduce springback at the outermost periphery of the coil C. Because the effect of reducing springback of the outermost portion of the coil C can be achieved with high precision, it is possible to avoid the risk of the coil C being lifted by the springback of the outermost portion C1 of the coil C when the coil C is removed from the mandrel 2, causing the coil C to come into contact with the reduced-diameter mandrel 102. In addition, because the springback of the outermost portion C1 of the coil C is reduced after the hot-rolled steel sheet S is wound, it is possible to avoid the risk of the restraining band restraining the outer periphery of the coil C being torn off during transportation.

[0090] According to the coiling method of the hot-rolled steel sheet according to the present embodiment, the cooling time calculation step (step S23) is carried out by calculating the cooling time from the coil installation position CP (x0, y0), the outer diameter D of the coil C, the sheet thickness t of the coil C, the positions N of the nozzles 4a and 4b, i (x i ,y i 10), the direction of the nozzles 4a, 4b (tilt angle α from the horizontal state in FIG. 10), and the spray angle of the cooling water from the nozzles 4a, 4b (angle β that defines the spray width of the cooling water in FIG. 10). The cooling time calculation step (step S23) also includes a flow density calculation step (step S232) for calculating a flow density w based on the arc length Lc of the cooling range calculated in the cooling range arc length calculation step (step S231), the cooling width Wc of the coil C by the cooling water from the nozzles 4a, 4b, and the flow rate Q of the cooling water from the nozzles 4a, 4b. The cooling time calculation step (step S23) also includes a heat transfer coefficient calculation step (step S233) for calculating a heat transfer coefficient h based on the flow density w calculated in the flow density calculation step (step S232) and the surface temperature T0 of the coil C before cooling when winding the coil. Furthermore, the cooling time calculation step (step S23) includes a maximum temperature difference cooling time calculation step (step S234) for calculating the cooling time τ at which the temperature difference between the outer surface and the inner surface of the outermost plate of coil C over the arc length Lc of the cooling range is maximized, based on the heat transfer coefficient h calculated in the heat transfer coefficient calculation step (step S233) and the plate thickness t of coil C. This makes it possible to determine with greater accuracy the cooling time τ at which the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost plate of the coil C becomes maximum.

[0091] According to the coiling method of the hot-rolled steel sheet according to the present embodiment, the spray control step (step S2) calculates the cooling time τ at which the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost sheet of the coil C over the arc length Lc of the cooling range is maximized, based on the arc length Lc of the cooling range, and the outer diameter D of the coil C, and calculates the rotation speed ω of the mandrel 2 and the total coil cooling time T when cooling water is sprayed from the nozzles 4a and 4b to cool the outer peripheral portion of the coil C for one revolution. total The method includes a coil total cooling time calculation step (step S24) for calculating: As a result, the rotation speed ω of the mandrel 2 and the total coil cooling time T when cooling the outer periphery of the coil C for one revolution by injecting cooling water from the nozzles 4a and 4b are total It is possible to calculate with high accuracy.

[0092] According to the coiling method of the hot-rolled steel sheet according to the present embodiment, a plurality of nozzles 4a, 4b are installed along the outer periphery of the coil C. Then, assuming that cooling water is sprayed from each of the plurality of nozzles 4a, 4b onto the outer periphery of the coil, a cooling time calculation step (step S23) and a total coil cooling time calculation step (step S24) are performed for each of the plurality of nozzles 4a, 4b, and in the total coil cooling time calculation step (step S24), the rotation speed ω of the mandrel 2 and the total coil cooling time T when cooling the outer periphery of the coil C for one revolution are calculated for each of the plurality of nozzles 4a, 4b. total Calculate the following: As a result, for each of the multiple nozzles 4a and 4b, the rotation speed ω of the mandrel 2 and the total coil cooling time T when cooling the outer periphery of the coil C for one revolution by spraying cooling water from the nozzles 4a and 4b are total It is possible to calculate with high accuracy.

[0093] Furthermore, according to the method for winding hot-rolled steel sheet of this embodiment, the spray control step (step S2) includes a spray nozzle pattern selection step (step S25) for selecting the spray nozzle (only nozzle 4a, only nozzle 4b, or both nozzle 4a and nozzle 4b) for spraying cooling water, the rotational speed ω of the mandrel 2 (ω2, ω1, or ω2 and ω1, whichever is the faster rotational speed), and the rotational angle of the mandrel 2 (360°, 360°, or θ1).

[0094] Then, in the injection nozzle pattern selection step (step S25), the injection nozzle pattern selection unit 12e selects the total coil cooling time T total The shortest time among these is compared with the time in case B described above. And the total coil cooling time T in the above case A total When the shortest time among the multiple nozzles 4a and 4b is shorter than the time in the case of B, the injection nozzle pattern selection unit 12e selects the nozzle that is the shortest among the multiple nozzles 4a and 4b for injecting the cooling water and that is the shortest among the multiple nozzles 4a and 4b for injecting the cooling water. total The shortest nozzle (only nozzle 4a or only nozzle 4b) is selected, and as the rotation speed ω of the mandrel 2, the rotation speed (ω2 or ω1) of the mandrel 2 for the selected nozzle (only nozzle 4a or only nozzle 4b) is selected, and as the rotation angle of the mandrel 2, the rotation angle (360° or 360°) of the mandrel 2 for one revolution of the coil C for the selected nozzle (only nozzle 4a or only nozzle 4b) is selected.

[0095] On the other hand, the time in the case of B is the total coil cooling time T totalIf the time is shorter than the shortest time among the above, the injection nozzle pattern selection unit 12e selects all of the multiple nozzles 4a, 4b as the injection nozzles for injecting cooling water, and selects, as the rotation speed of the mandrel 2, the rotation speed (ω2 or ω1) of the mandrel 2 which has the faster rotation speed between the rotation speed ω2 of the mandrel 2 for any one of the nozzles 4a and the rotation speed ω1 of the mandrel 2 for the adjacent nozzle 4b, and selects, as the rotation angle of the mandrel 2, the rotation angle (θ1) from point a in the cooling range on the outer periphery of the coil C by any one of the nozzles 4a to point b in the cooling range on the outer periphery of the coil C by the adjacent nozzle 4b.

[0096] As a result, when multiple nozzles 4a, 4b are installed, the nozzle that sprays the cooling water (only nozzle 4a, only nozzle 4b, or both nozzle 4a and nozzle 4b), the rotation speed ω of the mandrel 2 (ω2, ω1, or ω2 and ω1, whichever is the faster rotation speed), and the rotation angle of the mandrel 2 (360°, 360°, or θ1) can be selected so as to shorten the cooling time, thereby shortening the cooling time of the coil.

[0097] Then, by using this hot-rolled steel sheet winding method, a hot-rolled steel sheet can be manufactured by providing a winding process in which the hot-rolled steel sheet S is wound into a coil by a winding device 1. That is, by using the hot-rolled steel sheet winding method and the hot-rolled steel sheet winding device according to the present invention, the effect of reducing springback of the outermost peripheral part C1 of the coil C can be accurately achieved, and even during the manufacture of the hot-rolled steel sheet S, a manufacturing method can be provided that can solve the problems of impaired manufacturability and damage to equipment due to increased springback of the outermost peripheral part C1 of the coil C.

[0098] Although the embodiment of the present invention has been described above, the present invention is not limited to this and various modifications and improvements can be made. For example, the number of nozzles 4a, 4b is not limited to two, but may be one, or three or more. Moreover, the air-cooling control by the air-cooling control unit 13 does not necessarily have to be performed. [Explanation of symbols]

[0099] 1. Hot-rolled steel sheet winding equipment 2 Mandrels 3a, 3b, 3c, 3d Wrapper roll 4a, 4b Nozzle 5a, 5b Pinch roll 6 thermometer 7a,7b Cradle Roll 10 Winding control device 11 Wrapper roll control section 12 Spray control unit 13 Air cooling control section 14 Tail end stop control unit 15 Upper computer C coil S hot rolled steel plate Sa caudal end

Claims

1. A method for winding a hot-rolled steel sheet, comprising winding a hot-rolled steel sheet from its leading end to its trailing end into a coil shape on a mandrel of a winding device, and then rotating the mandrel while pressing a plurality of wrapper rolls arranged in a planetary fashion against the coil against the coil, spraying cooling water from a nozzle against an outer peripheral plate of the coil, thereby cooling the outer peripheral portion of the coil for a predetermined cooling time, wherein the predetermined cooling time for the outer peripheral portion of the coil is set equal to the time when the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost plate of the coil becomes maximum, a spray control step of controlling the rotation of the mandrel and the spray of cooling water from the nozzle so as to spray cooling water from the nozzle onto the outer peripheral plate of the coil while rotating the mandrel; The method for winding hot-rolled steel sheet, characterized in that the spray control step includes a cooling time calculation step of calculating a cooling time at which a temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost sheet of the coil over an arc length of a cooling range in the coil is maximized, based on the installation position of the coil, the outer diameter of the coil, the sheet thickness of the coil, the position of the nozzle, the orientation of the nozzle, the spray angle of cooling water from the nozzle, the cooling width of the coil by the cooling water from the nozzle, the flow rate of cooling water from the nozzle, and the surface temperature of the coil before cooling when winding the coil.

2. 2. The coiling method for hot-rolled steel sheet according to claim 1, wherein the cooling time calculation step includes: a cooling range arc length calculation step of calculating an arc length of a cooling range in the coil based on an installation position of the coil, an outer diameter of the coil, a position of the nozzle, an orientation of the nozzle, and a spray angle of the cooling water from the nozzle; a flow density calculation step of calculating a flow density based on the arc length of the cooling range calculated in the cooling range arc length calculation step, a cooling width in the coil by the cooling water from the nozzle, and a flow rate of the cooling water from the nozzle; a heat transfer coefficient calculation step of calculating a heat transfer coefficient based on the flow density calculated in the flow density calculation step and a surface temperature of the coil before cooling at the time of coiling; and a maximum temperature difference cooling time calculation step of calculating a cooling time at which a temperature difference between an outer peripheral surface and an inner peripheral surface of an outermost plate of the coil for the arc length of the cooling range is maximum based on the heat transfer coefficient calculated in the heat transfer coefficient calculation step and a plate thickness of the coil.

3. 3. The method for winding a hot-rolled steel sheet according to claim 2, characterized in that the spray control step includes a total coil cooling time calculation step of calculating a rotational speed of the mandrel and a total coil cooling time when cooling water is sprayed from the nozzle to cool one revolution of the outer periphery of the coil, based on the cooling time at which the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost plate of the coil for the arc length of the cooling range is maximized, the arc length of the cooling range, and the outer diameter of the coil.

4. The nozzles are provided along the outer periphery of the coil, 4. The method for coiling hot-rolled steel sheet according to claim 3, characterized in that, assuming that cooling water is sprayed from each of the plurality of nozzles onto the outer periphery of the coil, the cooling time calculation step and the total coil cooling time calculation step are performed for each of the plurality of nozzles, and, in the total coil cooling time calculation step, the rotation speed of the mandrel and the total coil cooling time required to cool the outer periphery of the coil for one revolution are calculated for each of the plurality of nozzles.

5. the spray control step includes a spray nozzle pattern selection step of selecting a spray nozzle for spraying cooling water, a rotation speed of the mandrel, and a rotation angle of the mandrel when spraying the cooling water; In the injection nozzle pattern selection step, the shortest time among the total coil cooling times in case A below is compared with the time in case B below, and if the shortest time among the total coil cooling times in case A below is shorter than the time in case B below, a nozzle having the shortest total coil cooling time among the multiple nozzles is selected as the injection nozzle for injecting cooling water, the mandrel rotation speed for the selected nozzle is selected as the mandrel rotation speed, the mandrel rotation angle for one revolution of the coil for the selected nozzle is selected as the mandrel rotation angle, and the time in case B below is compared with the time in case A below. The method for coiling a hot-rolled steel sheet according to claim 4, characterized in that, when the cooling time is shorter than the shortest time among the total cooling times, all of the plurality of nozzles are selected as the injection nozzles for injecting cooling water, and the mandrel rotation speed is selected as the mandrel rotation speed, whichever is faster, out of the mandrel rotation speed for any one of the following nozzles and the mandrel rotation speed for the following adjacent nozzle, and the mandrel rotation angle is selected as the mandrel rotation angle from a point within the cooling range on the outer periphery of the coil by any one of the following nozzles to a point within the cooling range on the outer periphery of the coil by the following adjacent nozzle: A: The total coil cooling time calculated in the total coil cooling time calculation step when cooling one revolution of the outer periphery of the coil for each of the plurality of nozzles. B: Assuming one of a plurality of nozzles and the adjacent nozzle that have the largest rotation angle from a point in the cooling range on the coil outer periphery by one of the nozzles to a point in the cooling range on the coil outer periphery by an adjacent nozzle that is adjacent to the nozzle in the mandrel rotation direction, the time when the mandrel is rotated by the rotation angle from a point in the cooling range by one of the nozzles to a point in the cooling range by the adjacent nozzle at the mandrel rotation speed for the one of the nozzles and the mandrel rotation speed for the adjacent nozzle, whichever is faster.

6. A hot-rolled steel sheet winding device winds up a hot-rolled steel sheet from its leading end to its trailing end into a coil shape around a mandrel, and then, while rotating the mandrel in a state in which a plurality of wrapper rolls arranged in a planetary fashion with respect to the coil are pressed against the coil, cooling water is sprayed from a nozzle onto an outer peripheral sheet of the coil to cool the outer peripheral portion of the coil for a predetermined cooling time, wherein the predetermined cooling time for the outer peripheral portion of the coil is set equal to the time when the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost sheet of the coil becomes maximum. a spray control unit that controls the rotation of the mandrel and the spray of cooling water from the nozzle so as to spray cooling water from the nozzle onto the outer peripheral plate of the coil while rotating the mandrel; The spray control unit is characterized in that it includes a cooling time calculation unit that calculates the cooling time at which the temperature difference between the outer surface and the inner surface of the outermost plate of the coil over the arc length of the cooling range in the coil is maximized, based on the installation position of the coil, the outer diameter of the coil, the plate thickness of the coil, the position of the nozzle, the orientation of the nozzle, the spray angle of cooling water from the nozzle, the cooling width of the coil by the cooling water from the nozzle, the flow rate of cooling water from the nozzle, and the surface temperature of the coil before cooling when winding the coil.

7. 7. The coiling device for hot-rolled steel sheet according to claim 6, characterized in that the cooling time calculation unit includes a cooling range arc length calculation unit that calculates an arc length of a cooling range in the coil based on an installation position of the coil, an outer diameter of the coil, a position of the nozzle, an orientation of the nozzle, and a spray angle of cooling water from the nozzle; a flow density calculation unit that calculates a flow density based on the arc length of the cooling range calculated by the cooling range arc length calculation unit, a cooling width of the coil by the cooling water from the nozzle, and a flow rate of the cooling water from the nozzle; a heat transfer coefficient calculation unit that calculates a heat transfer coefficient based on the flow density calculated by the flow density calculation unit and a surface temperature of the coil before cooling at the time of coiling; and a maximum temperature difference cooling time calculation unit that calculates a cooling time at which a temperature difference between an outer peripheral surface and an inner peripheral surface of an outermost plate of the coil for the arc length of the cooling range is maximum based on the heat transfer coefficient calculated by the heat transfer coefficient calculation unit and a plate thickness of the coil.

8. The hot-rolled steel sheet winding device according to claim 7, characterized in that the spray control unit includes a coil total cooling time calculation unit that calculates the rotational speed of the mandrel and the total coil cooling time when cooling water is sprayed from the nozzle to cool the outer peripheral portion of the coil for one revolution, based on the cooling time calculated by the cooling time calculation unit at which the temperature difference between the outer peripheral surface and the inner peripheral surface of the outermost plate of the coil for the arc length of the cooling range is maximized, the arc length of the cooling range, and the outer diameter of the coil.

9. The nozzles are provided along the outer periphery of the coil, 9. A hot-rolled steel sheet winding device as described in claim 8, characterized in that, assuming that cooling water is sprayed from each of the plurality of nozzles onto the outer periphery of the coil, processing is carried out for each of the plurality of nozzles in the cooling time calculation unit and the total coil cooling time calculation unit, and the rotation speed of the mandrel and the total coil cooling time required to cool the outer periphery of the coil for one revolution are calculated in the total coil cooling time calculation unit for each of the plurality of nozzles.

10. the spray control unit includes a spray nozzle pattern selection unit that selects a spray nozzle for spraying cooling water, a rotation speed of the mandrel, and a rotation angle of the mandrel when spraying the cooling water, The injection nozzle pattern selection unit compares the shortest time among the total coil cooling times in case A below with the time in case B below, and if the shortest time among the total coil cooling times in case A below is shorter than the time in case B below, selects a nozzle from among the multiple nozzles that has the shortest total coil cooling time as an injection nozzle for injecting cooling water, selects a mandrel rotation speed for the selected nozzle as the mandrel rotation speed, selects a mandrel rotation angle for one revolution of the coil for the selected nozzle as the mandrel rotation angle, and determines whether the time in case B below is shorter than the total coil cooling time in case A below.

10. The coiling device for hot-rolled steel sheet according to claim 9, characterized in that, when the cooling time is shorter than the shortest time among the cooling times, all of the plurality of nozzles are selected as the injection nozzles for injecting cooling water, and the mandrel rotation speed is selected as the mandrel rotation speed, whichever is faster, out of the mandrel rotation speed for any one of the following nozzles and the mandrel rotation speed for the following adjacent nozzle, and the mandrel rotation angle is selected as the mandrel rotation angle from a point in the cooling range on the outer periphery of the coil by any one of the following nozzles to a point in the cooling range on the outer periphery of the coil by the following adjacent nozzle: A: The total coil cooling time calculated in the total coil cooling time calculation step when cooling one revolution of the outer periphery of the coil for each of the plurality of nozzles. B: Assuming one of a plurality of nozzles and the adjacent nozzle that have the largest rotation angle from a point in the cooling range on the coil outer periphery by one of the nozzles to a point in the cooling range on the coil outer periphery by an adjacent nozzle that is adjacent to the nozzle in the mandrel rotation direction, the time when the mandrel is rotated by the rotation angle from a point in the cooling range by one of the nozzles to a point in the cooling range by the adjacent nozzle at the mandrel rotation speed for the one of the nozzles and the mandrel rotation speed for the adjacent nozzle, whichever is faster.

11. A method for producing a hot-rolled steel sheet, comprising: a winding step of winding the hot-rolled steel sheet into a coil shape by a winding device using the method for winding the hot-rolled steel sheet according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Down-equipped with cooling mechanism

    JP1983018608U

  • Winding method for pure ti plate after hot rolling

    JP1988194818A

  • Method for coiling thick-walled high-tensile hot-rolled stock

    JP2002263734A

  • Method and device for coiling thick high strength hot-rolled steel sheet

    JP2010162594A

  • Method of winding and carrying away thick high-strength hot-rolled steel plate

    JP2010253482A