Prepreg or semipreg comprising thermosetting resin

A benzoxazine ring-structured thermosetting resin impregnated prepreg or semi-preg provides superior repeated deformability, addressing the limitations of conventional resins by maintaining shape integrity during repeated deformation and curing processes.

JP2024137349APending Publication Date: 2024-10-07KANEKA CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023048842
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

Conventional thermosetting resins, such as epoxy resins, suffer from breakage during repeated remolding and deformation processes, lacking the ability to be repeatedly deformed without losing shape.

Method used

A prepreg or semi-preg containing a thermosetting resin with a benzoxazine ring structure in its main chain, represented by a specific formula, allowing for repeated deformability and shape retention upon curing.

Benefits of technology

The prepreg or semi-preg exhibits excellent repeated deformability, maintaining shape after deformation and curing, even under high temperatures and multiple cycles, without embrittlement or cracking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137349000007
    Figure 2024137349000007
  • Figure 2024137349000001
    Figure 2024137349000001
  • Figure 2024137349000002
    Figure 2024137349000002
Patent Text Reader

Abstract

To provide a prepreg or semipreg comprising thermosetting resin that exhibits superior repeated deformability.SOLUTION: A prepreg or semipreg according to one embodiment comprises reinforced fibers impregnated with a thermosetting resin that comprises a benzoxazine ring structure represented by a specific formula in its main chain or a composition comprising the thermosetting resin.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a prepreg or semipreg comprising a thermosetting resin. [Background technology]

[0002] It is known that benzoxazine compounds undergo ring-opening polymerization and reaction of benzoxazine rings by heat or the like, and are cured without generating volatile matter. Therefore, thermosetting resins mainly composed of low molecular weight compounds or polymers having a benzoxazine structure have various advantages such as low dielectric constant and low curing shrinkage in addition to the basic characteristics of thermosetting resins such as heat resistance, water resistance, chemical resistance, mechanical strength, and long-term reliability, and have attracted attention. For example, Patent Document 1 discloses a thermosetting resin having a dihydrobenzoxazine ring structure in the main chain by reacting a bifunctional phenolic compound, an aliphatic diamine or aromatic diamine, and an aldehyde compound.

[0003] Additionally, prepregs and / or semipregs using epoxy resin as a thermosetting resin are known. For example, Patent Document 2 discloses a laminate using a prepreg in which a glass fiber substrate is impregnated with an epoxy resin. Patent Document 3 discloses an epoxy prepreg using an epoxy resin blend. Patent Document 4 discloses a laminate including a prepreg in which a glass fiber woven fabric is impregnated with an epoxy resin and dried by heating. Patent Document 5 discloses a molding material comprising an epoxy resin composition and carbon fiber and / or glass fiber. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2008-291070 A [Patent Document 2] JP 2002-264157 A [Patent Document 3] Special Publication No. 2021-535941 [Patent Document 4] JP 2002-200633 A [Patent Document 5] International Publication No. 2021 / 157442 Summary of the Invention [Problem to be solved by the invention]

[0005] However, the above-mentioned conventional techniques have problems such as breakage when the remolding process, which includes a deformation step, is repeated, and there is room for improvement in terms of the property of being able to be repeatedly deformed (repeated deformability).

[0006] An object of one aspect of the present invention is to provide a prepreg or semipreg containing a thermosetting resin, which has excellent repeated deformability. [Means for solving the problem]

[0007] In order to solve the above problems, the prepreg or semipreg according to one embodiment of the present disclosure is formed by impregnating reinforcing fibers with a thermosetting resin having a benzoxazine ring structure in its main chain, as represented by general formula (I), or a composition containing the thermosetting resin, and has the property of being capable of being repeatedly deformed.

[0008] [ka]

[0009] [In the formula (I), Ar 1 and Ar 2 may be the same or different, and each represents a tetravalent aromatic group derived from a bifunctional phenol compound (A), R 1 represents a linear alkylene group having 6 to 12 carbon atoms derived from the aliphatic diamine compound (B), R 2 represents a (poly)oxyalkylene group derived from the (poly)oxyalkylenediamine compound (C), m represents an integer of 1 or more, n is an integer of 1 or more, The repeating unit represented by m and the repeating unit represented by n are repeated randomly, in blocks, or are alternately copolymerized. In order to solve the above problems, a method for molding a fiber composite material obtained from a prepreg or semipreg according to one embodiment of the present disclosure includes the steps of: A step of impregnating a reinforcing fiber with a thermosetting resin having a benzoxazine ring structure in its main chain represented by general formula (I) or a composition containing the thermosetting resin to obtain a prepreg or semipreg; curing the prepreg or semipreg to obtain a fiber composite material; Includes. Effect of the Invention

[0010] According to one aspect of the present invention, a prepreg or semipreg containing a thermosetting resin and having excellent repeated deformability can be provided. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is a diagram showing a procedure for evaluating repeated deformability in Examples and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an example of an embodiment of the present invention will be described in detail, but the present invention is not limited thereto. Unless otherwise specified in this specification, "A to B" representing a numerical range means "A or more and B or less."

[0013] 1. Overview of the Invention Prepregs and / or semipregs containing thermosetting resins are used in various applications. In recent years, there has been an increasing demand for new prepregs or semipregs that have the property of being able to deform a prepreg or semipreg once molded and then remolded. However, prepregs and / or semipregs using epoxy resins as thermosetting resins as disclosed in Patent Documents 2 to 5 break when repeatedly remolded, so there is room for improvement in terms of the property of being able to be repeatedly deformed. In addition, prepregs and / or semipregs using epoxy resins as thermosetting resins can be deformed before curing if they have a high grade of flexibility, but it is thought that they cannot maintain the shape after deformation due to their high flexibility.

[0014] Therefore, as a result of intensive research by the present inventors to solve the above problems, it has been found that a prepreg and / or semipreg having excellent properties of being repeatedly deformed can be obtained by using a thermosetting resin having a benzoxazine ring structure in the main chain represented by a certain formula, or a composition containing the thermosetting resin. It has also been found that a prepreg and / or semipreg that can maintain the shape after deformation can be obtained even when it is deformed and heated at a low temperature such as 60°C and cured. In this specification, the "property of being repeatedly deformed" is also referred to as "repeated deformability". The repeated deformability also includes the property that the prepreg or semipreg can be deformed into a different shape and cured by heating. It also includes the property that the laminate can be deformed into a different shape after laminating the prepreg or semipreg once to obtain a prepreg laminate and a semipreg laminate, respectively. Furthermore, the prepreg, semipreg, prepreg laminate, or semipreg laminate can be cured and molded, and then deformed into a different shape and re-cured by heating. Repeating this series of processes is also called remolding.

[0015] [2. Prepreg and / or Semipreg] In this specification, the term "semipreg" refers to a composite in which a thermosetting resin or a composition containing the thermosetting resin is partially impregnated (semi-impregnated) into reinforcing fibers and integrated. In addition, in this specification, the term "prepreg" refers to a composite obtained by impregnating reinforcing fibers with a resin by further heating and melting the semipreg. In other words, in this specification, the term "prepreg" refers to a composite in which the degree of impregnation of reinforcing fibers with resin is more advanced than that of semipreg.

[0016] A prepreg or semipreg according to one embodiment of the present invention is formed by impregnating reinforcing fibers with a thermosetting resin having a benzoxazine ring structure in its main chain, as represented by general formula (I), or a composition containing the thermosetting resin, and has the property of being capable of being repeatedly deformed.

[0017] [ka]

[0018] [In the formula (I), Ar 1 and Ar 2 may be the same or different, and each represents a tetravalent aromatic group derived from a bifunctional phenol compound (A), R 1 represents a linear alkylene group having 6 to 12 carbon atoms derived from the aliphatic diamine compound (B), R 2 represents a (poly)oxyalkylene group derived from the (poly)oxyalkylenediamine compound (C), m represents an integer of 1 or more, n represents an integer of 1 or more, The repeating unit represented by m and the repeating unit represented by n are repeated randomly, in blocks, or are alternately copolymerized. In formula (I), Ar 1 and Ar 2represents a tetravalent aromatic group derived from a bifunctional phenolic compound (A). As the bifunctional phenolic compound (A), a compound having a structure in which its OH group and the ortho position relative to the OH group can be incorporated into a benzoxazine ring is preferable. Examples of the bifunctional phenolic compound (A) include dihydroxydiphenylmethane compounds, dihydroxydiphenylethane compounds, dihydroxydiphenylpropane compounds, dihydroxydiphenylbutane compounds, dihydroxydiphenylcyclohexane compounds, and other dihydroxydiphenyl compounds.

[0019] Examples of the dihydroxydiphenylmethane compound include bis(4-hydroxyphenyl)diphenylmethane and bis(4-hydroxyphenyl)methane (commonly known as bisphenol F).

[0020] Examples of dihydroxydiphenylethane compounds include 1,1-bis(4-hydroxyphenyl)-1-phenylethane and 1,1-bis(4-hydroxyphenyl)ethane (commonly known as bisphenol E).

[0021] Examples of dihydroxydiphenylpropane compounds include 2,2-bis(4-hydroxyphenyl)propane (commonly known as bisphenol A or BPA), 2,2-bis(4-hydroxyphenyl)hexafluoropropane, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-isopropylphenyl)propane, and 5,5'-(1-methylethylidene)-bis[1,1'-(bisphenyl)-2-ol]propane.

[0022] An example of the dihydroxydiphenylbutane compound is 2,2-bis(4-hydroxyphenyl)butane (commonly known as bisphenol B).

[0023] Examples of the dihydroxydiphenylcyclohexane compound include 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane and 1,1-bis(4-hydroxyphenyl)cyclohexane.

[0024] Other dihydroxydiphenyl compounds include bis(4-hydroxyphenyl)-2,2-dichloroethylene, bis(4-hydroxyphenyl)sulfone, 1,3-bis(2-(4-hydroxyphenyl)-2-propyl)benzene, and 1,4-bis(2-(4-hydroxyphenyl)-2-propyl)benzene.

[0025] Of these, bis(4-hydroxyphenyl)methane, 2,2-bis(4-hydroxyphenyl)propane and the like are preferred, and 2,2-bis(4-hydroxyphenyl)propane is more preferred.

[0026] In formula (I), R 1 represents a linear alkylene group having 6 to 12 carbon atoms derived from the aliphatic diamine compound (B). That is, examples of the aliphatic diamine compound (B) include diamine compounds having a linear alkylene group having 6 to 12 carbon atoms. Among them, a diamine compound having a linear alkylene group having 6 carbon atoms, for example, 1,6-hexanediamine (hexamethylenediamine), is preferred.

[0027] In formula (I), R 2represents a divalent (poly)oxyalkylene group derived from a (poly)oxyalkylene diamine compound (C) having a (poly)oxyalkylene skeleton and two amino group terminals. In this specification, the (poly)oxyalkylene group includes a monooxyalkylene group (comprising one oxyalkylene group) and a polyoxyalkylene group (comprising multiple oxyalkylene groups). The (poly)oxyalkylene diamine compound (C) preferably has a (poly)oxyethylene group and / or a (poly)oxypropylene group as the (poly)oxyalkylene group. Examples of the (poly)oxyalkylene diamine compound (C) include Jeffamine D-230, Jeffamine D-400, Jeffamine D-2000, and Jeffamine D-4000 of the Jeffamine (registered trademark) D-series. Jeffamine D-2000 is particularly preferred. The thermosetting resin of the present disclosure contains a divalent (poly)oxyalkylene group derived from a (poly)oxyalkylenediamine compound, and thus the toughness of the thermosetting resin before and after curing can be improved.

[0028] In addition, an aldehyde compound may be used to synthesize the thermosetting resin of the present disclosure. The aldehyde compound is not particularly limited, but formaldehyde is preferred, and the formaldehyde can be used in the form of paraformaldehyde, which is a polymer thereof, or formalin, which is an aqueous solution thereof.

[0029] In formula (I), m is the degree of polymerization and is an integer of 1 or more, but from the viewpoint of improving mechanical properties before and after curing, m is preferably 2 or more, more preferably 3 or more, and even more preferably 5 or more. Moreover, from the viewpoint of maintaining fluidity during molding, m is preferably 500 or less, more preferably 300 or less, even more preferably 200 or less, and particularly preferably 100 or less.

[0030] In formula (I), n is the degree of polymerization and is an integer of 1 or more, but from the viewpoint of improving mechanical properties before and after curing, n is preferably 2 or more, more preferably 3 or more, and even more preferably 5 or more. Moreover, from the viewpoint of maintaining fluidity during molding, n is preferably 500 or less, more preferably 300 or less, even more preferably 200 or less, and particularly preferably 100 or less.

[0031] The ratio of m to n is preferably n / m=1 / 0.1 to 1 / 100. When the ratio of m to n is within the above range, a thermosetting resin having excellent decomposition temperature and toughness before and after curing can be obtained.

[0032] The thermosetting resin of the present disclosure may contain a structure other than the benzoxazine ring structure represented by formula (I). For example, it may have a structure derived from a monocyclic phenol compound for sealing the end of the structure represented by formula (I). In addition, the thermosetting resin of the present disclosure may contain a structure derived from an aliphatic monoamine or a (poly)oxyalkylene monoamine compound.

[0033] The thermosetting resin of the present disclosure preferably has a weight average molecular weight (Mw) measured by GPC of 10,000 or more, and from the viewpoint of improving mechanical properties before and after curing, Mw is more preferably 15,000 or more. In addition, the weight average molecular weight (Mw) is preferably 100,000 or less.

[0034] The method for producing the thermosetting resin of the present disclosure is not particularly limited, but for example, the thermosetting resin can be produced by a method including a step (s1) of reacting a bifunctional phenol compound (A), an aliphatic diamine compound (B), and an aldehyde compound, and a step (s2) of reacting a bifunctional phenol compound (A), a (poly)oxyalkylenediamine compound (C), and an aldehyde compound. The bifunctional phenol compound (A), the aliphatic diamine compound (B), the (poly)oxyalkylenediamine compound (C), and the aldehyde compound are as described above.

[0035] According to step (s1), a unit represented by formula (I) with a degree of polymerization m is produced. According to step (s2), a unit represented by formula (I) with a degree of polymerization n is produced.

[0036] Step (s1) and step (s2) may be performed simultaneously, step (s1) may be performed first and step (s2) may be performed later, or step (s2) may be performed first and step (s1) may be performed later. That is, step (s2) may be performed by adding the material for step (s2) to the system after the reaction of step (s1) has progressed, or vice versa. Also, step (s1) and step (s2) may be performed in separate systems, and then the respective products obtained may be reacted in one system. In other words, the manufacturing method of the present disclosure includes a step of reacting a bifunctional phenol compound (A), an aliphatic diamine compound (B), a (poly)oxyalkylenediamine compound (C), and an aldehyde compound. Also, in the manufacturing method of the present disclosure, the aliphatic diamine compound (B) and the (poly)oxyalkylenediamine compound (C) may be added simultaneously or sequentially. From the viewpoint of ease of operation, it is preferable that step (s1) and step (s2) are performed simultaneously.

[0037] In the production method of the present disclosure, the molar ratio of the bifunctional phenol (A), the aliphatic diamine compound (B), and the (poly)oxyalkylenediamine compound (C) in combination is preferably bifunctional phenol (A) / (aliphatic diamine compound (B)+(poly)oxyalkylenediamine compound (C))=10 / 1 to 1 / 10, more preferably 2 / 1 to 1 / 2. If the molar ratio of the bifunctional phenol (A), the aliphatic diamine compound (B), and the (poly)oxyalkylenediamine compound (C) in combination is within the above range, a high molecular weight thermosetting resin that is less likely to gel during production can be obtained.

[0038] In the production method of the present disclosure, the molar ratio of the (poly)oxyalkylenediamine compound (C) to the aliphatic diamine compound (B) is preferably (poly)oxyalkylenediamine compound (C) / aliphatic diamine compound (B)=1 / 0.1 to 1 / 100, more preferably 1 / 1 to 1 / 9. When the molar ratio of the (poly)oxyalkylenediamine compound (C) to the aliphatic diamine compound (B) is within the above range, a thermosetting resin excellent in decomposition temperature and toughness before and after curing can be obtained.

[0039] In the production method of the present disclosure, the molar ratio of the bifunctional phenol compound (A) to the aldehyde compound is preferably 1 / 1 to 1 / 20, and more preferably 1 / 2 to 1 / 6. When the molar ratio of the bifunctional phenol compound (A) to the aldehyde compound is within the above range, a benzoxazine ring can be suitably produced.

[0040] In the production method of the present disclosure, the solvent is not particularly limited as long as it can dissolve the raw materials, and examples thereof include chloroform, toluene, a mixed solvent of toluene and methanol, a mixed solvent of toluene and ethanol, a mixed solvent of toluene and isobutanol, and tetrahydrofuran.

[0041] The reaction temperature in step (s1) and / or step (s2) is preferably 25 to 150° C., more preferably 40 to 120° C. The reaction time in step (s1) and / or step (s2) is preferably 0.5 to 10 hours, more preferably 1 to 5 hours. In the production method of the present disclosure, the obtained product may be washed with an aqueous sodium bicarbonate solution or the like. After washing, dehydration may be performed with sodium sulfate or the like.

[0042] It is also possible to prepare and use a thermosetting composition that contains the thermosetting resin of the present disclosure as a main component and other thermosetting resins, thermoplastic resins, and compounding agents as minor components.

[0043] Examples of other thermosetting resins include epoxy resins, thermosetting modified polyphenylene ether resins, thermosetting polyimide resins, silicon resins, melamine resins, urea resins, allyl resins, phenol resins, unsaturated polyester resins, bismaleimide resins, alkyd resins, furan resins, polyurethane resins, and aniline resins.

[0044] Examples of the thermoplastic resin include a thermoplastic epoxy resin and a thermoplastic polyimide resin.

[0045] Examples of compounding agents include flame retardants, nucleating agents, antioxidants, antiaging agents, heat stabilizers, light stabilizers, ultraviolet absorbers, lubricants, flame retardant assistants, antistatic agents, antifogging agents, fillers, softeners, plasticizers, colorants, etc., as required. These may be used alone or in combination of two or more. Reactive or non-reactive solvents may also be used.

[0046] The prepreg or semipreg according to one embodiment of the present invention has repeated deformation properties. In addition, it has superior repeated deformation properties compared to conventional prepregs or semipregs using epoxy resin as a thermosetting resin. Here, the definition of "repeated deformation properties" is as described above. Repeated deformation can be performed by repeating deformation and curing by heat treatment. The lower limit of the temperature of the heat treatment may be, for example, 50°C or more, 60°C or more, 80°C or more, 100°C or more, or 120°C or more. The upper limit of the temperature of the heat treatment may be, for example, 400°C or less, 300°C or less, or 200°C or less. In addition, the number of repeated deformations (also referred to as the number of cycles) is not particularly limited, but may be 1 or more, for example, 2, 3, 4, 5, 6, 7, 10, 20, 30, or 50 times. In the present specification, "excellent repeated deformability" means that the prepreg or semipreg according to one embodiment of the present invention can be repeatedly deformed more times under the same heat treatment conditions than a prepreg or semipreg using a conventional epoxy resin. For example, when the prepreg or semipreg according to one embodiment of the present invention is subjected to repeated deformation seven or more times at a heat treatment temperature of 100°C or more and less than 120°C, or when the prepreg or semipreg is subjected to repeated deformation three or more times at a heat treatment temperature of 120°C or more, none of the states such as embrittlement, breakage, or cracking can be confirmed in the prepreg or semipreg.

[0047] The prepreg or semipreg according to one embodiment of the present invention may be present in a state in which a plurality of prepregs are laminated together. A laminate of a plurality of prepregs is also called a prepreg laminate, and a laminate of a plurality of semipregs is also called a semipreg laminate.

[0048] Furthermore, the prepreg or semipreg according to one embodiment of the present invention preferably has adhesiveness to other substrates (metals) etc. By having the adhesiveness, the prepreg or semipreg can be adhered to other substrates without the need for an adhesive.

[0049] Furthermore, the prepreg or semipreg according to one embodiment of the present invention preferably has self-supporting properties. In this specification, "self-supporting properties" refers to the property of maintaining a shape that is desired to be imparted after molding, for example, a curved shape, even after heating in an oven or the like without requiring a physical support. To explain this property in more detail, when one end of a prepreg laminate is fixed to the main surface of a flat object and the other end is left floating in the air, the pre-heating shape (for example, a curved shape) is maintained even after heating.

[0050] By having self-supporting properties, it is possible to switch from molding using an autoclave to molding using an oven halfway through molding the composite material. Unlike molding using an autoclave, molding using an oven allows the use of general-purpose auxiliary materials (heat resistance of about 180°C to match the epoxy). Therefore, having self-supporting properties is preferable because it allows the molding of a composite material without the need for expensive auxiliary materials.

[0051] The prepreg or semipreg according to one embodiment of the present invention can be used for aircraft members, automobile members, building members, electronic parts, and electronic devices, as well as materials thereof.

[0052] <Method of manufacturing prepreg or semipreg> The method for producing the prepreg or semipreg according to one embodiment of the present invention is not particularly limited, but it can be obtained by layering the thermosetting resin or a composition containing the thermosetting resin on the front and back of a sheet in which the reinforcing fibers are previously impregnated with a resin, and pressing at a predetermined temperature and a predetermined pressure. Examples of the reinforcing fibers include inorganic fibers, organic fibers, metal fibers, and hybrid reinforcing fibers that combine these. The reinforcing fibers may be one type or two or more types.

[0053] Examples of inorganic fibers include carbon fibers, graphite fibers, silicon carbide fibers, alumina fibers, tungsten carbide fibers, boron fibers, and glass fibers. Examples of organic fibers include aramid fibers, high-density polyethylene fibers, and other general nylon fibers and polyester fibers. Examples of metal fibers include stainless steel and iron fibers. Examples of metal fibers include carbon-coated metal fibers in which metal fibers are coated with carbon. Among these, from the viewpoint of increasing the strength of the cured product, it is preferable that the reinforcing fibers are carbon fibers.

[0054] Generally, the carbon fibers are subjected to a sizing treatment, but they may be used as they are, or, if necessary, fibers using a small amount of sizing agent may be used, or the sizing agent may be removed by an existing method such as an organic solvent treatment or heat treatment. Alternatively, the carbon fiber bundles may be opened in advance using air or a roller, and a treatment may be performed to facilitate impregnation of the resin between the single fibers of the carbon fibers. By reducing the amount of sizing agent used or removing the sizing agent, it is possible to suppress the formation of voids and discoloration of the resin caused by decomposition of the sizing agent at high temperatures.

[0055] [3. Fiber Composite Materials] An embodiment of the present invention also includes a fiber composite material obtained by curing a prepreg or semipreg. A method for molding a fiber composite material includes the steps of: A step of impregnating a reinforcing fiber with a thermosetting resin having a benzoxazine ring structure in its main chain represented by the above general formula (I), or a composition containing the thermosetting resin, to obtain a prepreg or semipreg; curing the prepreg or semipreg to obtain a fiber composite material; In the general formula (I), Ar 1 , Ar 2 , R 1 , R 2 The definitions of , m, and n are as described above.

[0056] The molding method may also include a step of pre-curing the prepreg or semipreg before curing the prepreg or semipreg to obtain a pre-cured prepreg or pre-cured semipreg having a degree of cure of more than 0% to 99%. Here, in this specification, pre-curing means partially curing the prepreg or semipreg. Therefore, the pre-cured prepreg and the pre-cured semipreg mean partially cured prepreg and semipreg, respectively. The degree of cure of the pre-cured prepreg or the pre-cured semipreg may be 99% or less, preferably 90% or less, and more preferably 80% or less.

[0057] Furthermore, the molding method may further include a step of repeatedly deforming the prepreg or semipreg before pre-curing the prepreg or semipreg. Furthermore, the molding method may further include a step of repeatedly deforming the pre-cured prepreg before curing the pre-cured prepreg. The repeated deformation can be performed by repeating deformation and curing by heat treatment as described above. The lower limit of the temperature of the heat treatment may be, for example, 50°C or more, 60°C or more, 80°C or more, 100°C or more, or 120°C or more. The upper limit of the temperature of the heat treatment may be, for example, 400°C or less, 300°C or less, or 200°C or less. In addition, the number of repeated deformations is not particularly limited, but may be 1 or more, for example, 2, 3, 4, 5, 6, 7, 10, 20, 30, or 50 times.

[0058] Furthermore, the molding method may include a step of curing and molding the prepreg or semipreg, deforming it again, and then curing it again by heating. In this specification, this molding method is also called a remolding method.

[0059] The fiber composite material may be a fiber composite material obtained by using only the semipreg or prepreg according to one embodiment of the present invention, or may be a fiber composite material obtained by laminating together the semipreg or prepreg according to one embodiment of the present invention and a prepreg or semipreg obtained by impregnating reinforcing fibers with another resin or a composition thereof.

[0060] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention.

[0061] [4. Summary] An embodiment of the present invention may have the following configuration. <1> A prepreg or semipreg is obtained by impregnating reinforcing fibers with a thermosetting resin having a benzoxazine ring structure in its main chain, as represented by general formula (I), or a composition containing the thermosetting resin, and has the property of being capable of being repeatedly deformed.

[0062] [ka]

[0063] [In the formula (I), Ar 1 and Ar 2 may be the same or different, and each represents a tetravalent aromatic group derived from a bifunctional phenol compound (A), R 1 represents a linear alkylene group having 6 to 12 carbon atoms derived from the aliphatic diamine compound (B), R 2 represents a (poly)oxyalkylene group derived from the (poly)oxyalkylenediamine compound (C), m represents an integer of 1 or more, n represents an integer of 1 or more, The repeating unit represented by m and the repeating unit represented by n are repeated randomly, in blocks, or are alternately copolymerized. <2> The bifunctional phenol compound (A) is 2,2-bis(4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 2,2-bis(4-hydroxyphenyl)hexafluoropropane, 2,2-bis(4-hydroxyphenyl)butane, bis(4-hydroxyphenyl)diphenylmethane, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, bis(4-hydroxyphenyl)-2,2-dichloroethylene, 1,1-bis(4-hydroxyphenyl)ethane, bis(4-hydroxyphenyl)methane, 2,2-bis(4- at least one bifunctional phenol compound selected from the group consisting of 1,3-bis(2-(4-hydroxyphenyl)-2-propyl)benzene, bis(4-hydroxyphenyl)sulfone, 1,4-bis(2-(4-hydroxyphenyl)-2-propyl)benzene, 5,5'-(1-methylethylidene)-bis[1,1'-(bisphenyl)-2-ol]propane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, and 1,1-bis(4-hydroxyphenyl)cyclohexane; <1> The prepreg or semipreg according to claim 1. <3> The (poly)oxyalkylenediamine compound (C) has a (poly)oxyethylene group and / or a (poly)oxypropylene group. <1> or <2> The prepreg or semipreg according to claim 1. <4> In the formula (I), the ratio of m to n is n / m=1 / 0.1 to 1 / 100. <1> ~ <3> 13. The prepreg or semipreg according to claim 12, <5> <1> ~ <4> A fiber composite material obtained by curing the prepreg or semipreg described in any one of the above items. <6> A step of impregnating a reinforcing fiber with a thermosetting resin having a benzoxazine ring structure in its main chain represented by general formula (I) or a composition containing the thermosetting resin to obtain a prepreg or semipreg;

[0064] [ka]

[0065] [In the formula (I), Ar 1 and Ar 2 may be the same or different, and each represents a tetravalent aromatic group derived from a bifunctional phenol compound (A), R 1 represents a linear alkylene group having 6 to 12 carbon atoms derived from the aliphatic diamine compound (B), R 2 represents a (poly)oxyalkylene group derived from the (poly)oxyalkylenediamine compound (C), m represents an integer of 1 or more, n represents an integer of 1 or more, The repeating unit represented by m and the repeating unit represented by n are repeated randomly, in blocks, or are alternately copolymerized. curing the prepreg or semipreg to obtain a fiber composite material; A method for molding a fiber composite material, comprising: <7> The method further includes a step of pre-curing the prepreg or semipreg before curing the prepreg or semipreg to obtain a pre-cured prepreg or pre-cured semipreg having a degree of cure of more than 0% to 99%. <6> The method according to <8> The method further includes a step of repeatedly deforming the prepreg or semipreg at a temperature of 50° C. or higher one or more times before pre-curing the prepreg or semipreg; <7> The method according to <9> <1> ~ <4> 2. A remolding method comprising curing and molding the prepreg or semipreg according to any one of 1 to 11, deforming it again, and then curing it again by heating. EXAMPLES

[0066] The present invention will be described in detail based on examples, but the present invention is not limited to these.

[0067] Example 1 (JD19) 〔material〕 The materials used in the preparation of the benzoxazine resin are listed below.

[0068] (Bifunctional phenol compound (A)) 2,2-Bis(4-hydroxyphenyl)propane (bisphenol A, BisA) (Tokyo Chemical Industry Co., Ltd.) (Aliphatic diamine compound (B)) Hexamethylenediamine (HMD) (Tokyo Chemical Industry Co., Ltd.) (Poly)oxyalkylenediamine compound (C) Jeffamine D-2000 (Hentsman) [Production of benzoxazine resin] Bisphenol A (4.5666 g, 0.02 mol), hexamethylenediamine (2.0923 g, 0.018 mol), Jeffamine D2000 (4.0000 g, 0.002 mol), and paraformaldehyde (2.5840 g, 0.086 mol) were added to chloroform (40 mL) and reacted at 60°C. The reaction was stopped after 5 hours. After cooling the reaction solution to room temperature, separation was performed three times using 60 mL of 0.1 N sodium bicarbonate solution. The reaction solution was dehydrated after washing with sodium sulfate and filtered. The solvent was removed using an evaporator under heating and reduced pressure, and the powder of benzoxazine resin, the target compound, was obtained by drying under reduced pressure at 40°C using a vacuum oven.

[0069] The number average molecular weight (Mn) and weight average molecular weight (Mw) of the compound obtained were determined using gel permeation chromatography (GPC, Shimadzu Corporation) in terms of standard polystyrene. The number average molecular weight (Mn) of the compound was 6063 and the weight average molecular weight (Mw) was 17414 in terms of standard polystyrene.

[0070] [Forming of benzoxazine resin film] A release PET spacer with a hole (50 μm thick, 8 cm square or 10 cm square) in the center was placed on top of the release PET (50 μm thick), the resin powder obtained above was placed in the hole, and the release PET was placed on top of that. This laminate was sandwiched between stainless steel plates, heated at 60°C for 5 minutes in a press molding machine, and then press molded at a pressure of 10 MPa for 10 minutes to obtain a film with a thickness of 0.05 mm.

[0071] [Molding of benzoxazine resin prepreg] Two of the films obtained above (one side of the release PET was peeled off and the other side of the release PET remained) were placed on a 8 cm square piece of carbon fiber plain weave material (product name: CO6343B (manufactured by Toray Industries, Inc.), fiber weight: 198 g / m 2 , Density: 1.76g / cm 3 ) on the front and back of one sheet, and the laminate (which is composed of release PET, film, carbon fiber plain weave material, film, and release PET in that order) is sandwiched between stainless steel plates, heated for 5 minutes at 60°C using a press molding machine, and then press molded for 10 minutes at a pressure of 1 MPa to obtain a prepreg with an 8 cm square and a thickness of 0.2 to 0.3 mm. The prepreg was obtained by stacking an 8 cm square film on the front side of the carbon fiber plain weave material and a 10 cm square film on the back side. Next, two sheets of the obtained prepreg were prepared, the release PET on one side of each was peeled off, and the peeled surfaces of the prepregs were bonded together. The prepreg was heated for 5 minutes at 60°C, and then press molded for 10 minutes at 60°C and a pressure of 1 MPa to obtain a prepreg laminate with an 8 cm square and a thickness of 0.4 to 0.6 mm (with release PET laminated on both the top and bottom sides).

[0072] <Repeated deformation evaluation> The prepreg laminate obtained was evaluated for its repetitive remoldability according to the procedure shown in FIG. 1. The prepreg laminate was cut into 2 x 8 cm strips and the release PET on the top and bottom was removed. 2. The prepreg laminate strip that had been through step 1 above was attached to the corner of a metal bat to give it a curved shape, and was heated in a convection oven for 5 minutes at 100°C. After heating, it was removed from the oven and the prepreg laminate strip was peeled off from the metal bat, leaving a prepreg laminate strip that maintained its curved shape. 3. The strip of prepreg laminate obtained in step 2 above was tape-attached at both ends to fit the bottom surface of the metal bat, leaving it in an unbent shape (i.e., the flat shape before bending in step 2 above). While maintaining this shape, it was heated in a convection oven at 100°C for 5 minutes. After heating, it was removed from the oven and the prepreg laminate strip was peeled off from the metal bat, leaving a strip of prepreg laminate that had maintained its unbent shape. In other words, in step 3, the shape of the prepreg laminate strip was restored to the same shape as in step 1 above. 4. The above steps 2 and 3 constituted one cycle, and seven cycles were performed.

[0073] As a result of the repeated deformation evaluation, no embrittlement, breakage, or cracking was confirmed in the prepreg laminate after seven cycles.

[0074] Comparative Example 1 A commercially available UD (Uni-Directional) epoxy prepreg was used as the carbon fiber composite material (CFRP). Two 8 cm square epoxy prepregs were laminated perpendicularly and cut into 2 x 8 cm strips to obtain a prepreg laminate (quasi-plain weave material). The quasi-plain weave material means that the fibers of two UD prepregs are perpendicular to each other, so that the fibers are not woven together, but have an arrangement similar to that of a plain weave material.

[0075] The obtained prepreg laminate was subjected to a cycle consisting of steps 2 and 3 in the repeated deformation evaluation as in Example 1. Up to the sixth cycle, no embrittlement, breakage, or cracking was observed in the prepreg laminate. However, when the prepreg laminate was checked after the seventh cycle, the fibers were found to have broken.

[0076] Example 2 (JD19) A prepreg was molded in the same manner as in Example 1. Thereafter, the repeated deformation properties of the obtained prepreg were evaluated in the same manner as in Example 1, except that the heat treatment temperature in steps 2 and 3 in the repeated deformation property evaluation was changed to 120°C.

[0077] As a result of the repeated deformation evaluation, no embrittlement, breakage, or cracking was confirmed in the prepreg laminate after seven cycles.

[0078] Comparative Example 2 A prepreg laminate was obtained in the same manner as in Comparative Example 1. The repeated deformation property of the obtained prepreg laminate was evaluated in the same manner as in Example 2. Up to the second cycle, no state such as embrittlement, breakage, or cracking was confirmed in the prepreg laminate. On the other hand, when the prepreg laminate was checked after the third cycle, the fibers were broken. As described above, since fiber breakage was confirmed in the check after the third cycle, the fourth cycle and subsequent cycles were not performed.

[0079] Example 3 (JD19) A prepreg was molded in the same manner as in Example 1. Thereafter, the repeated deformation properties of the obtained prepreg were evaluated in the same manner as in Example 1, except that the heat treatment temperature in steps 2 and 3 in the repeated deformation property evaluation was changed to 60°C.

[0080] As a result of the repeated deformation evaluation, the prepreg laminate after one cycle was not found to be embrittled, broken, or cracked. In other words, it was confirmed that the prepreg laminate maintained the deformed shape even when it was deformed and then heated at a low temperature such as 60°C to harden it.

[0081] 〔summary〕 From the above repeated deformation evaluation results, it was confirmed that the prepreg laminates of the Examples have excellent repeated deformability compared to the prepreg laminates of the Comparative Examples. That is, it was revealed that the prepreg laminates produced using the prepreg according to one embodiment of the present invention have repeated deformability even when the heat treatment temperature is high and / or the number of cycles is large, and are excellent in repeated deformability compared to prepreg laminates using conventional epoxy prepregs. It was also revealed that the prepreg laminates produced using the prepreg according to one embodiment of the present invention maintain the deformed shape even when deformed and then heated at a low temperature such as 60°C to harden. [Industrial Applicability]

[0082] The present invention can be utilized in fields using prepregs or semipregs obtained by impregnating reinforcing fibers with a thermosetting resin or a composition containing the thermosetting resin.

Claims

1. A prepreg or semipreg is obtained by impregnating reinforcing fibers with a thermosetting resin having a benzoxazine ring structure in its main chain, as represented by general formula (I), or a composition containing the thermosetting resin, and has the property of being capable of being repeatedly deformed. 【Chemistry 1】 [In the formula (I), Ar 1 and Ar 2 may be the same or different, and each represents a tetravalent aromatic group derived from a bifunctional phenol compound (A), R 1 represents a linear alkylene group having 6 to 12 carbon atoms derived from the aliphatic diamine compound (B), R 2 represents a (poly)oxyalkylene group derived from the (poly)oxyalkylenediamine compound (C), m represents an integer of 1 or more; n represents an integer of 1 or more; The repeating unit represented by m and the repeating unit represented by n are repeated randomly, repeated as a block, or are an alternating copolymer.

2. The bifunctional phenol compound (A) is 2,2-bis(4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 2,2-bis(4-hydroxyphenyl)hexafluoropropane, 2,2-bis(4-hydroxyphenyl)butane, bis(4-hydroxyphenyl)diphenylmethane, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, bis(4-hydroxyphenyl)-2,2-dichloroethylene, 1,1-bis(4-hydroxyphenyl)ethane, bis(4-hydroxyphenyl)methane, 2,2-bis(4-hydroxy-3-isopropyl)propane, bis(4-hydroxyphenyl)butane, bis(4-hydroxyphenyl)diphenylmethane, bis(4-hydroxyphenyl)-2,2-dichloroethylene, bis(4-hydroxyphenyl)ethane, bis(4-hydroxyphenyl)methane, bis(4-hydroxyphenyl)methane, bis(4-hydroxy-3-isopropyl)propane, bis(4-hydroxyphenyl)butane, bis(4-hydroxyphenyl)diphenylmethane ... The prepreg or semipreg according to claim 1, which is at least one bifunctional phenol compound selected from the group consisting of 1,3-bis(2-(4-hydroxyphenyl)-2-propyl)propane, 1,3-bis(2-(4-hydroxyphenyl)-2-propyl)benzene, bis(4-hydroxyphenyl)sulfone, 1,4-bis(2-(4-hydroxyphenyl)-2-propyl)benzene, 5,5'-(1-methylethylidene)-bis[1,1'-(bisphenyl)-2-ol]propane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, and 1,1-bis(4-hydroxyphenyl)cyclohexane.

3. 2. The prepreg or semipreg according to claim 1, wherein the (poly)oxyalkylenediamine compound (C) has a (poly)oxyethylene group and / or a (poly)oxypropylene group.

4. The prepreg or semipreg according to claim 1, wherein in the formula (I), the ratio of m to n is n / m = 1 / 0.1 to 1 / 100.

5. A fiber composite material obtained by curing the prepreg or semipreg according to any one of claims 1 to 4.

6. A step of impregnating a reinforcing fiber with a thermosetting resin having a benzoxazine ring structure in its main chain represented by general formula (I) or a composition containing the thermosetting resin to obtain a prepreg or semipreg; 【Chemistry 2】 [In the formula (I), Ar 1 and Ar 2 may be the same or different, and each represents a tetravalent aromatic group derived from a bifunctional phenol compound (A), R 1 represents a linear alkylene group having 6 to 12 carbon atoms derived from the aliphatic diamine compound (B), R 2 represents a (poly)oxyalkylene group derived from the (poly)oxyalkylenediamine compound (C), m represents an integer of 1 or more; n represents an integer of 1 or more; The repeating unit represented by m and the repeating unit represented by n are repeated randomly, repeated as a block, or are an alternating copolymer. curing the prepreg or semipreg to obtain a fiber composite material; A method for molding a fiber composite material, comprising:

7. 7. The method of claim 6, further comprising the step of pre-curing the pre-preg or semi-preg prior to curing the pre-preg or semi-preg to obtain a pre-cured pre-preg or pre-cured semi-preg having a degree of cure of greater than 0% to 99%.

8. 8. The method of claim 7, further comprising the step of deforming the prepreg or semipreg at a temperature of 50° C. or higher one or more times before precuring the prepreg or semipreg.

9. A remolding method comprising curing and molding the prepreg or semipreg according to any one of claims 1 to 4, deforming it again, and then curing it by heating.

Citation Information

Patent Citations

  • Amide-ether amide copolymer and its production

    JP1989193320A

  • Cyano group-containing thermosetting benzoxazine resin, thermosetting resin composition and its application

    JP2006257286A

  • Manufacturing method for thermosetting resin having benzoxazine ring, and thermosetting resin having benzoxazine ring

    JP2011057961A

  • Polybenzoxazine resin for compounding epoxy resin, and epoxy resin composition containing the same

    JP2012077243A

  • Resin material and multilayer printed wiring board

    JP2021025051A