Piezoelectric device, manufacturing method thereof and piezoelectric device array

The piezoelectric device structure addresses crack formation in pMUT devices by employing a void and varying grain sizes and compositions in the piezoelectric layer, enhancing crack resistance and energy conversion efficiency.

JP2024137404APending Publication Date: 2024-10-07TAIYO YUDEN KK
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023048915
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

Piezoelectric layers in pMUT devices experience cracks near the outer periphery of the vibration region due to stress concentration, particularly when using single crystal PZT as the piezoelectric material.

Method used

A piezoelectric device structure is designed with a void in the substrate, an intermediate layer covering the void, a lower electrode, and a piezoelectric layer divided into regions with different grain sizes and compositions, including a second region with smaller grain size and potentially higher magnesium or oxygen concentration to reduce stress concentration.

Benefits of technology

The structure effectively suppresses cracks in the piezoelectric layer while maintaining high piezoelectricity and improving electromechanical energy conversion efficiency by reducing grain size and altering material composition.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137404000001_ABST
    Figure 2024137404000001_ABST
Patent Text Reader

Abstract

To provide a piezoelectric device capable of suppressing cracks.SOLUTION: A piezoelectric device comprises: a substrate 10a including a cavity 28; an intermediate layer which is provided on the substrate so as to cover the cavity in a planar view; a lower electrode 12 which is provided on the intermediate layer; a piezoelectric layer 14 which is provided on the lower electrode; and an upper electrode 16 of which the first region holding the piezoelectric layer together with the lower electrode is provided on the piezoelectric layer inside of a contour of the cavity 28 in the planar view and the area in the planar view is smaller than an area of a region enclosed by the contour of the cavity in the planar view. Outside of an outer periphery of the first region in the planar view, an average grain size of crystal grains of the piezoelectric layer in a second region, which is provided from the inside to the outside of the contour of the cavity is provided smaller than an average grain size of crystal grains of the piezoelectric layer in the first region.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to piezoelectric devices and methods for making the same, and to piezoelectric device arrays. [Background technology]

[0002] A piezoelectric micromachined ultrasonic transducer (pMUT) using a piezoelectric body is known. An ultrasonic transducer in which a plurality of pMUT elements are arranged in an array is known (for example, Patent Document 1, Non-Patent Document 1). It is also known to add magnesium to a piezoelectric layer of an aluminum nitride film (for example, Patent Document 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] US Patent Publication No. 2020 / 0194658 [Patent Document 2] JP 2021-150920 A [Non-patent literature]

[0004] [Non-Patent Document 1] P. Ngoc, et al., Micromachines, vol 9, no.9 p.455 (2018) Summary of the Invention [Problem to be solved by the invention]

[0005] In a pMUT, a gap is provided in a substrate, and a laminated film including a piezoelectric layer is provided on the gap. The laminated film in the vibration region that overlaps with the gap in a plan view flexes and vibrates. At this time, the laminated film on the substrate is fixed, and stress is concentrated on the periphery of the vibration region. Non-Patent Document 1 describes that when single crystal PZT (Lead Zirconate titanate) is used as the piezoelectric layer, cracks are formed in the piezoelectric layer near the periphery of the vibration region.

[0006] The present invention has been made in consideration of the above problems, and has an object to suppress cracks. [Means for solving the problem]

[0007] The present invention is a piezoelectric device comprising: a substrate having a gap; an intermediate layer provided on the substrate so as to cover the gap in a planar view; a lower electrode provided on the intermediate layer; a piezoelectric layer provided on the lower electrode; and an upper electrode having a first region that sandwiches the piezoelectric layer together with the lower electrode and is provided on the piezoelectric layer inside the outer periphery of the gap in a planar view, and an area in a planar view smaller than the area in a planar view of the region surrounded by the outer periphery of the gap, wherein the average grain size of the crystal grains of the piezoelectric layer in a second region that is provided outside the periphery of the first region in a planar view, spanning from the inside to the outside of the outer periphery of the gap, is smaller than the average grain size of the crystal grains of the piezoelectric layer in the first region.

[0008] In the above configuration, the piezoelectric layer may be mainly composed of aluminum nitride, and the piezoelectric layer in the second region may contain magnesium.

[0009] In the above configuration, the magnesium concentration of the piezoelectric layer in the second region can be set to 1 atomic % or more and 10 atomic % or less when the total of aluminum, magnesium and other additive elements is taken as 100 atomic %.

[0010] In the above configuration, the piezoelectric layer may be mainly composed of aluminum nitride, and the oxygen concentration of the piezoelectric layer in the second region may be higher than the oxygen concentration in the first region.

[0011] In the above configuration, the oxygen concentration of the piezoelectric layer in the second region can be set to 1 atomic % or more and 10 atomic % or less when the total of aluminum, nitrogen and other added elements is taken as 100 atomic %.

[0012] In the above configuration, the average grain size of the crystal grains in the second region at a position 1 μm from the lower surface of the piezoelectric layer can be 30 nm or less.

[0013] In the aforementioned configuration, the surface roughness of the lower surface of the piezoelectric layer in the second region can be greater than the surface roughness of the lower surface of the piezoelectric layer in the first region.

[0014] In the above configuration, in a planar view, the surface roughness of the underside of the piezoelectric layer in a third region having the outer periphery of the first region as its inner periphery and the inner periphery of the second region as its outer periphery can be configured to increase from the outer periphery of the first region toward the inner periphery of the second region.

[0015] In the above configuration, a seed layer having the same main component as the main component of the piezoelectric layer may be provided between the lower electrode and the piezoelectric layer in the first region.

[0016] In the above configuration, a main component of the piezoelectric layer in the first region and a main component of the piezoelectric layer in the second region can be the same.

[0017] The present invention is a piezoelectric device comprising: a substrate having a gap; an intermediate layer provided on the substrate so as to cover the gap in a planar view; a lower electrode provided on the intermediate layer; a piezoelectric layer provided on the lower electrode; and an upper electrode having a first region that sandwiches the piezoelectric layer together with the lower electrode and is provided on the piezoelectric layer inside the outer periphery of the gap in a planar view, and an area in a planar view smaller than the area in a planar view of the region surrounded by the outer periphery of the gap; and an amorphous layer provided on the substrate and the gap in a second region that is provided from the inside to the outside of the outer periphery of the gap in a planar view, without the piezoelectric layer interposed, and surrounding the piezoelectric layer.

[0018] The present invention also relates to a piezoelectric device array in which a plurality of the piezoelectric devices as described above are provided, and the substrates of the plurality of piezoelectric devices are provided as an integral unit.

[0019] The present invention is a method for manufacturing a piezoelectric device, including the steps of: forming a first piezoelectric layer mainly composed of aluminum nitride on a lower electrode provided on a substrate using a sputtering method; removing the first piezoelectric layer in a second region provided outside the first region while leaving the first piezoelectric layer in a first region; forming a second piezoelectric layer mainly composed of aluminum nitride and containing magnesium on the lower electrode in the second region provided outside the outer periphery of the first region using a sputtering method with a power density lower than the power density used to form the first piezoelectric layer; forming an upper electrode on the first piezoelectric layer in the first region; and forming the void in the substrate so that the upper electrode is provided inside the outer periphery of the void in a planar view, the area of ​​the upper electrode in a planar view is smaller than the area in a planar view of the region surrounded by the outer periphery of the void, and the second region extends from the inside to the outside of the outer periphery of the void.

[0020] The present invention is a method for manufacturing a piezoelectric device, including the steps of: using a sputtering method to form a first piezoelectric layer mainly composed of aluminum nitride on a lower electrode provided on a substrate; removing the first piezoelectric layer in a second region provided outside the first region, leaving the first piezoelectric layer in a first region; using a sputtering method to form a second piezoelectric layer mainly composed of aluminum nitride and having a higher oxygen concentration than the first piezoelectric layer on the lower electrode in the second region provided outside the periphery of the first region; forming an upper electrode on the first piezoelectric layer in the first region; and forming the void in the substrate so that the upper electrode is provided inside the periphery of the void in a planar view, the area of ​​the upper electrode in a planar view is smaller than the area in a planar view of the region surrounded by the periphery of the void, and the second region extends from the inside to the outside of the periphery of the void outside the periphery of the first region.

[0021] The present invention is a method for manufacturing a piezoelectric device, comprising the steps of: roughening an upper surface of a lower electrode provided on a substrate in a first region so that the surface roughness of the upper surface of the lower electrode in the second region provided outside the periphery of the first region is smaller than the surface roughness of the upper surface of the lower electrode in a second region provided outside the periphery of the first region; forming a piezoelectric layer on the lower electrode in the first region and the second region; forming an upper electrode on the piezoelectric layer in the first region; and forming the gap in the substrate so that the upper electrode is provided inside the outer periphery of the gap in a planar view, the area of ​​the upper electrode in a planar view is smaller than the area in a planar view of the region surrounded by the outer periphery of the gap, and the second region extends from the inside to the outside of the outer periphery of the gap.

[0022] In the above configuration, the process of roughening the upper surface of the lower electrode can be configured to include a process of roughening the upper surface of the lower electrode in a third region located between the first region and the second region so that the surface roughness of the upper surface of the lower electrode increases from the first region toward the second region.

[0023] The present invention is a method for manufacturing a piezoelectric device, including the steps of: forming a seed layer on a lower electrode provided on a substrate in a first region; forming a piezoelectric layer on the seed layer in the first region and on the lower electrode in a second region provided outside the periphery of the first region; forming an upper electrode on the piezoelectric layer in the first region; and forming the gap in the substrate so that the upper electrode is provided inside the periphery of a gap in a planar view, the area of ​​the upper electrode in a planar view is smaller than the area of ​​the region surrounded by the periphery of the gap in a planar view, and the second region extends from the inside to the outside of the periphery of the gap outside the periphery of the first region. Effect of the Invention

[0024] According to the present invention, it is possible to suppress cracks. [Brief description of the drawings]

[0025] [Figure 1] FIG. 1(a) is a plan view of an ultrasonic transducer according to a first embodiment, and FIG. 1(b) is a cross-sectional view taken along line AA of FIG. 1(a). [Diagram 2] 2(a) and 2(b) are schematic cross-sectional views of the piezoelectric layer in FIG. 1(b). [Diagram 3] 3(a) and 3(b) are cross-sectional views showing the operation of an ultrasonic transducer. [Figure 4] 4(a) to 4(c) are cross-sectional views showing a manufacturing method of the ultrasonic transducer according to the first embodiment. [Diagram 5] 5(a) to 5(c) are cross-sectional views showing a manufacturing method of the ultrasonic transducer according to the first embodiment. [Figure 6] 6(a) and 6(b) are cross-sectional views showing a manufacturing method of the ultrasonic transducer according to the first embodiment. [Figure 7] FIG. 7 is a graph showing the average grain size of crystal grains versus power density in Experiment 1. [Figure 8] FIG. 8 is a graph showing the average grain size of crystal grains versus the oxygen concentration in Experiment 2. [Figure 9] FIG. 9 is a cross-sectional view of an ultrasonic transducer according to the second embodiment. [Figure 10] 10(a) and 10(b) are cross-sectional views showing a method for manufacturing an ultrasonic transducer according to the second embodiment. [Figure 11] FIG. 11 is a cross-sectional view of an ultrasonic transducer according to a first modified example of the second embodiment. [Figure 12] 12(a) and 12(b) are cross-sectional views showing a first manufacturing method of an ultrasonic transducer according to a first modified example of the second embodiment. [Figure 13] 13(a) and 13(b) are cross-sectional views showing a second manufacturing method of an ultrasonic transducer according to a first modified example of the second embodiment. [Figure 14] FIG. 14 is a cross-sectional view of the ultrasonic transducer according to the third embodiment. [Figure 15] 15(a) and 15(b) are cross-sectional views showing a manufacturing method of the ultrasonic transducer according to the third embodiment. [Figure 16] FIG. 16 is a cross-sectional view of an ultrasonic transducer according to a fourth embodiment. [Figure 17] FIG. 17 is a plan view of the ultrasonic transducer according to the fifth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The following embodiments will be described with reference to the accompanying drawings. In the following embodiments, an ultrasonic transducer will be described as an example of a piezoelectric device. EXAMPLES

[0027] Fig. 1(a) is a plan view of an ultrasonic transducer 100 according to a first embodiment, and Fig. 1(b) is a cross-sectional view taken along line AA of Fig. 1(a). In Fig. 1(a), a gap 28 is indicated by a dashed line, and an upper electrode 16 is indicated by cross-hatching. The stacking direction of each layer is the Z direction, and the extension directions of the sides of the substrate 10 in a plan view are the X direction and the Y direction.

[0028] The ultrasonic transducer 100 has a substrate 10 having a certain thickness and a rectangular planar shape. The substrate 10 is made of, for example, an SOI (Semiconductor On Insulator) substrate, and a substrate 10a, a stopper layer 10b, and an active layer 10c are provided in this order from the bottom. The substrate 10a is, for example, a silicon substrate. The stopper layer 10b is, for example, a silicon oxide layer. The active layer 10c is, for example, a silicon layer.

[0029] The substrate 10a has a gap 28 penetrating the substrate 10a. The gap 28 is also called a cavity. The laminated film of the stopper layer 10b and the active layer 10c is layered, and when viewed in a plan view, the approximate center of the stopper layer 10b contacts the gap 28, and the periphery is supported by the substrate 10a. The stopper layer 10b functions as an etching stopper when the gap 28 is formed. The active layer 10c is a support layer that supports the piezoelectric layer 14.

[0030] An insulating layer 11 is provided on the active layer 10c. The insulating layer 11 does not necessarily have to be provided. The layers between the gap 28 and the lower electrode 12 (i.e., the stopper layer 10b, the active layer 10c, and the insulating layer 11) are intermediate layers. The lower electrode 12 is provided so as to cover the entire upper surface of the active layer 10c. The piezoelectric layer 14 is provided so as to cover the entire upper surface of the lower electrode 12. An upper electrode 16 is provided on the piezoelectric layer 14.

[0031] 1(a), in a plan view, the upper electrode 16 is provided so as to substantially coincide with the center of the substrate 10a. Pads 24a and 24b are provided on the piezoelectric layer 14. In a plan view, the pads 24a and 24b are provided around the gap 28. The pad 24a is connected to the lower electrode 12 via a hole 22 penetrating the piezoelectric layer 14. The pad 24b is integrally connected to the upper electrode 16 via a wiring 16a. A pad 24b made of gold for bonding is provided on the pad receiving portion 16b.

[0032] When a voltage is applied to the lower electrode 12 and the upper electrode 16, electrical energy is converted into mechanical energy by the inverse piezoelectric effect in the piezoelectric layer 14, generating compressive or tensile stress in the left-right direction. As a result, the region where the gap 28 is located bends and vibrates in the up-down direction, generating ultrasonic waves.

[0033] Here, the film in which the stopper layer 10b, the active layer 10c, the insulating layer 11, the lower electrode 12, the piezoelectric layer 14, and the upper electrode 16 are provided in this order is called the laminated film 18. The region where the gap 28 contacts the stopper layer 10b (intermediate layer) is the vibration region 50. The laminated film 18 in the vibration region 50 flexurally vibrates. The region where the lower electrode 12 and the upper electrode 16 overlap with the piezoelectric layer 14 sandwiched therebetween is called the S region 52, taking the initial letter of "stack." The S region 52 is smaller than the vibration region 50 (i.e., the gap 28) in a plan view, and is provided so as to be included in the vibration region 50. That is, the area of ​​the upper electrode 16 in a plan view is smaller than the area of ​​the vibration region 50 surrounded by the outer periphery of the gap 28 in a plan view. The planar shapes of the vibration region 50 and the S region 52 are, for example, approximately circular. The center of the S region 52 approximately coincides with the center 55 of the vibration region 50.

[0034] In the following, the piezoelectric layer 14 will be described by dividing it into a plurality of regions when viewed from a plan view. When viewed from a plan view, a region larger than the S region 52 and smaller than the vibration region 50 is defined as a region 54. The piezoelectric layer 14 in this region 54 is defined as a first piezoelectric layer 15a. A region outside this region 54, which is in contact with the outer periphery of the region 54, includes the inner and outer peripheries of the vibration region 50, and extends to the periphery of the substrate 10 is defined as a second region 56. That is, the second region 56 is provided from the inside to the outside of the contour of the gap 28 when viewed from a plan view. The piezoelectric layer 14 in the second region 56 is defined as a second piezoelectric layer 15b.

[0035] Using these names, the average grain size of the crystal grains in the second piezoelectric layer 15b is smaller than the average grain size of the crystal grains in the first piezoelectric layer 15a. That is, the average grain size is smaller in the periphery of the piezoelectric layer 14 than in the center.

[0036] Figures 2(a) and 2(b) are schematic cross-sectional views of piezoelectric layers 15a and 15b in Figure 1(b). Since piezoelectric layers 15a and 15b have a columnar polycrystalline structure, a plurality of crystal grains 34 are provided. The interfaces between crystal grains 34 are grain boundaries 35. As shown in Figures 2(a) and 2(b), the second piezoelectric layer 15b is characterized in that the average grain size of the crystal grains is smaller than the average grain size of the crystal grains in the first piezoelectric layer 15a.

[0037] The operation of the ultrasonic transducer 100 will be described below. Figures 3(a) and 3(b) are cross-sectional views showing the operation of the ultrasonic transducer. The insulating layer 11 and the stopper layer 10b are omitted from the illustration.

[0038] An example of transmitting ultrasonic waves will be described. As shown in Figures 3(a) and 3(b), a control unit 30 is provided that applies an AC voltage between the lower electrode 12 and the upper electrode 16. When this AC voltage is applied between the lower electrode 12 and the upper electrode 16, strains 31a and 31b are generated in the piezoelectric layer 14 due to the inverse piezoelectric effect. As a result, stresses 32a and 32b are applied to the active layer 10c, and the laminated film 18 vibrates in the up-down directions 33a and 33b. This AC voltage causes the states of Figures 3(a) and 3(b) to be repeated, causing the vibration region 50 to vibrate alternately in the up-down directions 33a and 33b, and ultrasonic waves are emitted from the vibration region 50.

[0039] When ultrasonic waves are received by the vibration region 50 from the outside, the vibration region 50 vibrates in the vertical directions 33a and 33b. This applies stresses 32a and 32b to the active layer 10c of the vibration region 50. This causes strains 31a and 31b to occur in the piezoelectric layer 14. An AC voltage is generated between the lower electrode 12 and the upper electrode 16 due to the piezoelectric effect. By measuring this AC voltage (AC signal), ultrasonic waves can be received.

[0040] As shown in Figures 3(a) and 3(b), when the laminated film 18 in the vibration region 50 flexurally vibrates, stress is concentrated in an area 58 near the outer periphery of the vibration region 50, that is, in the base of the ring shape and its vicinity. This phenomenon occurs because the area 58 is the fixed end of the vibration. The piezoelectric material used for the piezoelectric layer 14 has a large Young's modulus and is hard. For this reason, cracks are likely to occur in the piezoelectric layer 14. When the crystal grains 34 are large, the portion of the hard crystal grains 34 increases, and the piezoelectric layer 14 becomes relatively hard. When the crystal grains 34 are small, the portion of the hard crystal grains 34 decreases, and the piezoelectric layer 14 becomes relatively soft.

[0041] Therefore, in the first embodiment, the average grain size of the crystal grains 34 in the second region 56 of the second piezoelectric layer 15b is smaller than the average grain size of the crystal grains 34 in the first piezoelectric layer 15a in the S region 52 (first region).

[0042] As a result, the second piezoelectric layer 15b in the second region 56 including the area 58 where cracks are likely to occur becomes relatively soft, and cracks are suppressed. On the other hand, the first piezoelectric layer 15a in the S region 52 has a large grain size, so that mechanical friction at the grain boundaries is small and the mechanical quality factor Qm is large. In addition, the first piezoelectric layer 15a has a large grain size, so that the piezoelectric transverse effect (d31) is large and the piezoelectricity is high. This improves the electromechanical energy conversion efficiency.

[0043] The average grain size of the crystal grains 34 in the second piezoelectric layer 15b is preferably 0.9 times or less, more preferably 0.8 times or less, and further preferably 0.7 times or less, the average grain size of the crystal grains 34 in the first piezoelectric layer 15a in the S region 52.

[0044] From this viewpoint, the average grain size of the crystal grains 34 in the second piezoelectric layer 15b is preferably 0.1 times or more, and more preferably 0.2 times or more, the average grain size of the crystal grains 34 in the first piezoelectric layer 15a in the S region 52.

[0045] An example of how to determine the average grain size of the crystal grains 34 in the first piezoelectric layer 15a and the second piezoelectric layer 15b will be described. In the piezoelectric layers 15a and 15b, cross sections in the XY plane at the same height (Z position) from the bottom surface are observed. Note that the height at which the cross sections of the piezoelectric layers 15a and 15b are observed can tolerate an error of about 5% of the thickness of the piezoelectric layers 15a and 15b.

[0046] An example of how to determine the average grain size of the crystal grains 34 in the first piezoelectric layer 15a and the second piezoelectric layer 15b will be described. In the piezoelectric layers 15a and 15b, cross sections in the XY plane at the same height (Z position) from the bottom surface are observed. Note that the height at which the cross sections of the piezoelectric layers 15a and 15b are observed can tolerate an error of about 5% of the thickness of the piezoelectric layers 15a and 15b.

[0047] The cross sections of the piezoelectric layers 15a and 15b are observed, for example, using a TEM (Transmission Electron Microscope). The diffraction contrast of the TEM makes it easier to observe the crystal grains and to define them on the image. Those in which the crystal grains cannot be defined are not sampled, and those in which the crystal grains can be defined are sampled. For example, crystal grains are sampled from a TEM image of 500 nm x 500 nm. It is preferable to sample 60 or more crystal grains. If the number of sampled crystal grains is less than 60, the number of TEM images is increased.

[0048] The area of ​​the sampled crystal grains 34 is measured. The measured area of ​​the crystal grains 34 is converted into the diameter of a circle. If the area of ​​the crystal grains 34 is S, the grain size R can be expressed as 2×√(S / π). The average of these grain sizes R gives the average grain size of the crystal grains 34.

[0049] Since the main components of the first piezoelectric layer 15a and the second piezoelectric layer 15b are the same, the acoustic impedances of the two layers are almost equal. Therefore, no impedance difference occurs at the boundary between the piezoelectric layers 15a and 15b, and the reflection of vibrations can be suppressed, and as a result, unwanted vibration modes can be suppressed.

[0050] The main components of the piezoelectric layers 15a and 15b are elements that function as piezoelectric layers. The piezoelectric layers 15a and 15b are allowed to contain elements other than the main components unintentionally or intentionally. For example, the element concentration of the main components of the piezoelectric layers 15a and 15b is 50 atomic % or more, 80 atomic % or more, or 90 atomic % or more. For example, when the main component of the piezoelectric layers 15a and 15b is aluminum nitride, the total concentration of aluminum and nitrogen is 50 atomic % or more, 80 atomic % or more, or 90 atomic % or more. Furthermore, the concentration of aluminum in the piezoelectric layers 15a and 15b is 10 atomic % or more or 20 atomic % or more, and the concentration of nitrogen is 10 atomic % or more or 20 atomic % or more.

[0051] The materials of each component will be specifically described below. Other than the SOI substrate mentioned above, a silicon substrate can be used as the substrate. The lower electrode 12 and the upper electrode 16 are films selected from metals such as ruthenium, molybdenum, gold, titanium, platinum, aluminum, copper, chromium, silver, palladium, or nickel, or laminated films in which a plurality of metals are selected from these. For example, the lower electrode 12 is a chromium film and a ruthenium film from the active layer 10c side. The upper electrode 16 is a ruthenium film and a chromium film from the piezoelectric layer 14 side.

[0052] The material of the piezoelectric layer 14 is, for example, AlN (aluminum nitride), PZT (lead zirconate titanate), KNN (potassium sodium niobate), BaFeO3 (barium ferrate), BaTiO3 (barium titanate), LiNbO3 (lithium niobate), LiTaO3 (lithium tantalate), ZnO (zinc oxide) or pVDF (polyvinylidene fluoride). The material of the protective film is, for example, an inorganic insulator such as silicon oxide, silicon nitride, aluminum oxide or aluminum nitride. The pads 24a and 24b are, for example, a gold layer, a copper layer or an aluminum layer.

[0053] The substrate 10a has a thickness of 100 μm to 500 μm, the stopper layer 10b has a thickness of 0.1 μm to 3 μm, and the active layer 10c has a thickness of 1 μm to 20 μm. The lower electrode 12 and the upper electrode 16 have a thickness of, for example, 100 nm to 300 nm. The piezoelectric layer 14 has a thickness of, for example, 100 nm to 300 nm.

[0054] The planar shape of the vibrating region 50 and the S region 52 is a circle. The center 55 of the vibrating region 50 and the center of the S region 52 coincide with each other. The diameter of the vibrating region 50 is 200 μm to 2000 μm, and the diameter of the S region 52 is smaller than the diameter of the vibrating region 50, being 100 μm to 1500 μm. The planar shapes and areas of the vibrating region 50 and the S region 52 can be set appropriately. The planar shapes of the vibrating region 50 and the S region 52 may be, for example, approximately elliptical or approximately polygonal.

[0055] [Production method of Example 1] Hereinafter, a description will be given of a method for manufacturing the ultrasonic transducer of Example 1. Figures 4(a) to 6(b) are cross-sectional views showing a method for manufacturing the ultrasonic transducer 100 according to Example 1.

[0056] 4(a), as described in the first half of Example 1, the substrate 10 is an SOI substrate, and an insulating layer 11 is formed on the entire surface of the substrate 10 by, for example, a chemical vapor deposition (CVD) method or a thermal oxidation method. A conductive material is deposited on the insulating layer 11 by, for example, a sputtering method to form a lower electrode 12.

[0057] Next, as shown in FIG. 4(b), a piezoelectric material is deposited on the lower electrode 12 by, for example, sputtering to form a piezoelectric layer 15a.

[0058] 4(c), the piezoelectric layer 15a is patterned using photolithography and etching. As a result, the piezoelectric layer 15a in the second region 56 is removed, and the piezoelectric layer 15a remains in the region 54. For etching the piezoelectric layer 15a, a dry etching method such as an ion milling method or a RIE (Reactive Ion Etching) method or a wet etching method is used.

[0059] 5(a), the piezoelectric layer 15b is formed by sputtering so as to cover the lower electrode 12 and the piezoelectric layer 15a. The grain sizes of the crystal grains in the first piezoelectric layer 15a and the second piezoelectric layer 15b will be described later.

[0060] Next, as shown in FIG. 5(b), the upper surface of the piezoelectric layer 15a is removed by using a chemical mechanical polishing (CMP) method to form a flat surface. The central piezoelectric layer 15a and the piezoelectric layer 15b surrounding the piezoelectric layer 15a form an integrated piezoelectric layer 14 with a flat upper surface. Thus, two types of piezoelectric layers 15a and 15b can be prepared, and piezoelectric layers with different average grain sizes can be formed by appropriately setting the process conditions from FIG. 4(c) to FIG. 5(b). Alternatively, after this process, piezoelectric layers with different average grain sizes can be formed by using light irradiation or the like. This will be described in detail later.

[0061] 5(c), a conductive material is deposited on the piezoelectric layer 14 by, for example, sputtering. The conductive material is patterned to form the upper electrode 16 on the first piezoelectric layer 15a. As a result, the region where the upper electrode 16 remains becomes the S region 52. At this time, the wiring 16a and the pad receiving portion 16b in FIG. 1(a) are also formed simultaneously with the upper electrode 16.

[0062] Next, holes 22 are formed in the piezoelectric layer 14, as shown in FIG. 6(a).

[0063] 6(b), pad 24a is formed to connect to lower electrode 12 through hole 22. At this time, pad 24b in FIG. 1(a) is also formed at the same time as pad 24a. To bond thin metal wires (bonding wires) to pads 24a and 24b, the surfaces of pads 24a and 24b are coated with a conductive film by gold plating or sputtering, etc.

[0064] Thereafter, the void 28 is formed from the lower surface of the substrate 10a by, for example, a DRIE (Deep RIE) method. The stopper layer 10b functions as an etching stopper. In this manner, the ultrasonic transducer 100 according to the first embodiment is manufactured. Therefore, as shown in FIG. 1(b), the laminated film 18 from the etching stopper layer 10b to the upper electrode 16 is laminated in a portion corresponding to the roof of the void 28 so as to cover the void 28. Note that, for example, the void 28 may be formed by providing a sacrificial layer in the portion of the substrate 10a corresponding to the void 28 and removing it by etching.

[0065] Next, the deposition conditions for the piezoelectric layers 15a and 15b will be described based on experiments. [Experiment 1] An aluminum nitride film with no additives was formed as film A, and a film B with magnesium (Mg) and hafnium (Hf) added was formed.

[0066] Film A deposition method Film formation was performed by AC (Alternating Current) magnetron sputtering. Two Al targets were used. Argon (Ar) and nitrogen (N2) were used as sputtering gases.

[0067] Film B deposition method The deposition was performed by AC magnetron sputtering. An Al target and an Al76MgHf12 alloy target were used. Argon and oxygen / nitrogen were used as process gases. Al76, Mg12, and Hf12 are in atomic %. Note that the Mg concentration is the concentration of Mg relative to the total of Al, Mg, and Hf, and the Hf concentration is the concentration of Hf relative to the total of Al, Mg, and Hf.

[0068] The AC power densities for depositing films A and B were 10.0, 17.5, and 20.0 W / cm 2 7 is a diagram showing the average grain size of crystal grains versus power density in Experiment 1. The average grain size of crystal grains 34 was measured by the above-mentioned method using TEM images of the surfaces of films A and B after they were formed to a thickness of 1 μm.

[0069] For film A, the power density is 10 W / cm 2 , 17.5W / cm 2 and 20W / cm 2 The average particle size at the power density of 10 W / cm2 is 43.8 nm, 39.8 nm and 40.8 nm, respectively. 2 , 17.5W / cm 2 and 20W / cm 2 The average particle size at the power density of 10 W / cm is 25.2 nm, 33.7 nm, and 38.1 nm, respectively. 2 The average concentrations of Mg and Hf in the 17.5 W / cm3 are 3.36 atomic % and 2.97 atomic %, respectively. 2 The average concentrations of Mg and Hf in the 20 W / cm3 are 4.47 atomic % and 4.86 atomic %, respectively. 2 The average concentrations of Mg and Hf in the alloy are 3.89 atomic % and 5.25 atomic %, respectively.

[0070] For film A, the average grain size remains almost unchanged even when the power density is changed. On the other hand, for film B, the average grain size becomes smaller when the power density is reduced.

[0071] The reason for this was presumed. Patent Document 2 describes that in an aluminum nitride film to which Mg and Hf are added, the Hf concentration is almost uniform throughout the film, whereas the Mg concentration is higher near the grain boundaries 35 than within the crystal grains 34. When an aluminum nitride film is formed using a sputtering method, it undergoes Volmer-Weber growth. It is known that in Volmer-Weber growth, the grain size of the crystal grains increases as the film thickness increases. It is presumed that the growth of the crystal grains 34 is suppressed by the fact that Mg segregates at the grain boundaries 35 of the crystal grains 34 and that the mobility of the sputtered particles decreases due to film formation at a low power density. For this reason, if magnesium is contained in the aluminum nitride film, the average grain size of the crystal grains 34 can be reduced by lowering the power density.

[0072] Therefore, in FIG. 4(b), a piezoelectric material mainly composed of aluminum nitride is deposited on the lower electrode 12 provided on the substrate 10 by sputtering to form a piezoelectric layer 15a (first piezoelectric layer). In FIG. 4(c), the piezoelectric layer 15a in the S region 52 (first region) is left, and the piezoelectric layer 15a in the region 56 (second region) provided outside the S region 52 is removed. Thereafter, in FIG. 5(a), a piezoelectric material mainly composed of aluminum nitride and containing magnesium is deposited on the lower electrode 12 in the range 58 by sputtering using a power density smaller than the power density used to form the piezoelectric layer 15a, to form a piezoelectric layer 15b (second piezoelectric layer). This allows the average grain size of the crystal grains 34 of the piezoelectric layer 15b to be smaller than the average grain size of the crystal grains 34 of the piezoelectric layer 15a.

[0073] This suppresses the occurrence of cracks in the piezoelectric layer 15b in the range 58. On the other hand, the piezoelectric layer 15a in the S region 52 has high piezoelectricity, and the electromechanical energy conversion efficiency is improved. The piezoelectric layer 15a may or may not contain magnesium.

[0074] In the ultrasonic transducer 100 thus manufactured, the piezoelectric layer 14 is mainly composed of aluminum nitride. The piezoelectric layer 15b in the region 56 contains magnesium.

[0075] From Fig. 7, the film A without Mg addition and the film B with a power density of 20 W / cm 2 In the case of film B, the average grain size is about 40 nm. In contrast, the power density is about 10 W / cm 2 When film B is formed using the above conditions, the average grain size is about 25 nm.

[0076] In order to reduce the average grain size of the crystal grains 34, the average Mg concentration in the piezoelectric layer 15b is preferably 10 atomic % or less, and more preferably 5 atomic % or less. The average Mg concentration in the piezoelectric layer 15b is preferably 1 atomic % or more. Note that the Mg concentration is the magnesium concentration when the total of aluminum, magnesium, and other added elements (excluding nitrogen) is taken as 100 atomic %.

[0077] Aluminum nitride containing magnesium is softer than aluminum nitride not containing magnesium. Therefore, the average Mg concentration in piezoelectric layer 15b is set higher than the average Mg concentration in piezoelectric layer 15a. This makes it possible to further suppress the occurrence of cracks in piezoelectric layer 15b in range 58.

[0078] [Experiment 2] An aluminum nitride film with added oxygen (O) was deposited. The deposition was performed using AC magnetron sputtering. Two Al targets were used. Argon (Ar), nitrogen (N2), and oxygen (O2) were used as the sputtering gases. By changing the mixture ratio of nitrogen and oxygen, aluminum nitride films with different oxygen concentrations were deposited. The average oxygen concentration from 0.7 μm to 1 μm from the surface was measured using SIMS (Secondary Ion Mass Spectrometry) and used as the oxygen concentration of the film.

[0079] 8 is a diagram showing the average grain size versus oxygen concentration in Experiment 2. When the oxygen concentration in the aluminum nitride film is 0.0018 atomic %, 0.67 atomic %, and 5.5 atomic %, the average grain size of the crystal grains 34 is 38.4 nm, 33.3 nm, and 26.6 nm, respectively. In this way, the average grain size can be reduced by increasing the oxygen concentration in the aluminum nitride film.

[0080] Therefore, in FIG. 4(b), a piezoelectric material mainly composed of aluminum nitride is deposited on the lower electrode 12 by sputtering to form the piezoelectric layer 15a. In FIG. 4(c), the piezoelectric layer 15a in the S region 52 (first region) remains, and the piezoelectric layer 15a in the region 56 (second region) provided outside the S region 52 is removed. In FIG. 5(a), a piezoelectric material mainly composed of aluminum nitride and having a higher oxygen concentration than the piezoelectric layer 15a is deposited on the lower electrode 12 in a range 58 by sputtering to form the piezoelectric layer 15b. This allows the average grain size of the crystal grains 34 of the piezoelectric layer 15b to be smaller than the average grain size of the crystal grains 34 of the piezoelectric layer 15a. Therefore, the occurrence of cracks in the piezoelectric layer 15b in the range 58 is suppressed. On the other hand, the piezoelectric layer 15a in the S region 52 has high piezoelectricity and improves efficiency.

[0081] In the ultrasonic transducer 100 thus manufactured, the piezoelectric layer 14 is mainly composed of aluminum nitride. The oxygen concentration of the piezoelectric layer 15b in the region 56 is lower than the oxygen concentration of the piezoelectric layer 15a in the S region 52.

[0082] The oxygen concentration of piezoelectric layer 15b is preferably 1 atomic % or more, and more preferably 2 atomic % or more. The oxygen concentration of piezoelectric layer 15a is preferably 10 atomic % or less, and more preferably 8 atomic % or less. The oxygen concentration of piezoelectric layer 15b is preferably at least twice the oxygen concentration of piezoelectric layer 15a, and more preferably at least 5 times. The oxygen concentration is the concentration of oxygen when the total of aluminum, nitrogen and other added elements is 100 atomic %.

[0083] From the results of Experiments 1 and 2, the average grain size of the crystal grains 34 at a location 1 μm from the lower surface of the piezoelectric layer 15b in the region 56 is preferably 30 nm or less, and more preferably 25 nm or less. The average grain size of the crystal grains 34 at a location 1 μm from the lower surface of the piezoelectric layer 15a in the S region 52 is preferably 35 nm or more. EXAMPLES

[0084] Example 2 is an example in which the surface roughness of the lower surface of the piezoelectric layer 14 is different. Fig. 9 is a cross-sectional view of an ultrasonic transducer according to Example 2.

[0085] In the ultrasonic transducer 102 of Example 2, the surface roughness of the lower surface 40 of the piezoelectric layer 15b in the region 56 is greater than the surface roughness of the lower surface 40 of the piezoelectric layer 15a in the region 54. The other configurations are the same as those of Example 1, and therefore description thereof will be omitted.

[0086] [Method of manufacturing ultrasonic transducer according to embodiment 2] 10(a) and 10(b) are cross-sectional views showing a method for manufacturing an ultrasonic transducer according to the second embodiment.

[0087] As shown in FIG. 10(a), after performing the process of FIG. 4(a) of Example 1, a mask layer 46 is formed in the region that will become the region 54. The mask layer 46 is, for example, a thin metal film. Using an ion milling method, the lower electrode 12 is irradiated with argon ions 48 using the mask layer 46 as a mask. As a result, unevenness is formed on the upper surface 41 of the lower electrode 12 in the region that will become the region 56, and the surface roughness of the upper surface 41 is increased. The inclination angle of the ion beam from the Z direction is, for example, 0° to 5°. If redeposits adhere to the side surface of the mask layer 46 after the ion beam irradiation, the inclination angle of the ion beam from the Z direction may be set to 80°, and the ion beam may be irradiated. As a result, the redeposits adhered to the side surface of the mask layer 46 can be removed. The surface roughness of the upper surface 41 of the lower electrode 12 in the region 56 is greater than the surface roughness of the upper surface 41 in the region 54.

[0088] As shown in FIG. 10(b), after removing the mask layer 46, the piezoelectric layer 14 is formed on the lower electrode 12 by, for example, sputtering. In the region 54 with small surface roughness, a piezoelectric layer 15a with a large average grain size is formed, and in the region 56 with large surface roughness, a piezoelectric layer 15b with a small average grain size is formed. Then, the steps from FIG. 5(c) onwards are performed. In this way, the ultrasonic transducer 102 of the second embodiment is manufactured.

[0089] In the second embodiment, as shown in FIG. 10(a), the upper surface 41 of the lower electrode 12 in the region 56 is roughened so that the surface roughness of the upper surface 41 of the lower electrode 12 in the S region 52 is smaller than the surface roughness of the upper surface 41 of the lower electrode 12 in the region 56. The average grain size of the crystal grains 34 of the piezoelectric layer 15b can be made smaller than the average grain size of the crystal grains 34 of the piezoelectric layer 15a. Therefore, the occurrence of cracks in the piezoelectric layer 15b in the range 58 is suppressed. On the other hand, the piezoelectric layer 15a in the S region 52 has a large grain size, so that the mechanical friction at the grain boundary is small and the mechanical quality factor Qm is large. In addition, the first piezoelectric layer 15a has a large grain size, so that the piezoelectric transverse effect (d31) is large and the piezoelectricity is high. Therefore, the electromechanical energy conversion efficiency is improved. In addition, by forming the piezoelectric layer 14, the piezoelectric layers 15a and 15b can be formed simultaneously, so that the manufacturing man-hours can be reduced compared to the first embodiment. Thus, the steps of etching the piezoelectric layer 15a in FIG. 4(c) and CMP in FIG. 5(b) are omitted.

[0090] From the viewpoint of making the average grain size of the piezoelectric layer 15a about 40 nm, the arithmetic mean roughness of the lower surface 40 of the piezoelectric layer 15a is preferably 5 nm or less, more preferably 2 nm or less. From the viewpoint of making the average grain size of the piezoelectric layer 15b 35 nm or less, the arithmetic mean roughness of the lower surface 40 of the piezoelectric layer 15b is preferably 5 nm or more, more preferably 10 nm or more. If the arithmetic mean roughness is too large compared to the average grain size, the average grain size will not become small. From this viewpoint, the arithmetic mean roughness of the lower surface 40 of the piezoelectric layer 15a is preferably 50 nm or less, more preferably 20 nm or less.

[0091] [Modification 1 of Example 2] FIG. 11 is a cross-sectional view of an ultrasonic transducer according to a first modified example of the second embodiment.

[0092] In the ultrasonic transducer 104 of the first modified example of the second embodiment, a region 56 including a range 58 and a region 57 located between the region 54 and the region 56 are provided outside the region 54. The surface roughness of the lower surface 40 of the piezoelectric layer 15c in the region 57 is greater than the surface roughness of the lower surface 40 of the piezoelectric layer 15a in the region 54. The surface roughness of the lower surface 40 of the piezoelectric layer 15b in the region 56 is greater than the surface roughness of the lower surface 40 of the piezoelectric layer 15c in the region 57. In the region 57, the surface roughness of the lower surface 40 gradually increases from the region 54 to the region 56. The average grain size of the crystal grains 34 of the piezoelectric layer 15c is smaller than the average grain size of the crystal grains 34 of the piezoelectric layer 15a. The average grain size of the crystal grains 34 of the piezoelectric layer 15b is smaller than the average grain size of the crystal grains 34 of the piezoelectric layer 15c. In the piezoelectric layer 15c, the average grain size of the crystal grains 34 gradually decreases from the piezoelectric layer 15a to 15b. The other configurations are the same as those in the second embodiment, and therefore the description will be omitted.

[0093] [Method 1 of manufacturing ultrasonic transducer according to modified example 1 of embodiment 2] 12(a) and 12(b) are cross-sectional views showing a first manufacturing method of an ultrasonic transducer according to a first modified example of the second embodiment.

[0094] As shown in FIG. 12(a), after the process of FIG. 4(a) is performed, a mask layer 46 is formed in a region that will become the region 54. The mask layer 46 is, for example, a thin metal film. Using an ion milling method, the lower electrode 12 is irradiated with argon ions 48 using the mask layer 46 as a mask. The inclination angle of the ion beam from the Z direction is, for example, 30° to 60°. The wafer is rotated. The ion beam is not irradiated to the region 54 where the mask layer 46 is provided. In the region 56 that is not in the shadow of the mask layer 46, the upper surface 41 of the lower electrode 12 is irradiated with the ion beam, and the surface roughness increases. In the region 57, the amount of irradiation of the ion beam increases in a portion far from the mask layer 46, and the amount of irradiation of the ion beam decreases in a portion close to the mask layer 46. As a result, the surface roughness of the upper surface 41 in the region 57 increases from the region 54 to the region 56.

[0095] As shown in FIG. 12(b), after removing the mask layer 46, the piezoelectric layer 14 is formed on the lower electrode 12 by, for example, sputtering. In the region 54 with small surface roughness, a piezoelectric layer 15a with a large average grain size is formed, and in the region 56 with large surface roughness, a piezoelectric layer 15b with a small average grain size is formed. In the region 57, a piezoelectric layer 15c with a gradually decreasing average grain size from the piezoelectric layer 15a to 15b is formed. Then, the steps from FIG. 5(c) onwards are carried out. In this way, the ultrasonic transducer 104 of the first modified example of the second embodiment is manufactured.

[0096] [Method 2 of manufacturing ultrasonic transducer according to modified example 1 of embodiment 2] 13(a) and 13(b) are cross-sectional views showing a second manufacturing method of an ultrasonic transducer according to a first modified example of the second embodiment.

[0097] As shown in FIG. 13(a), after the process of FIG. 4(a) is performed, a sacrificial layer 47 is formed on the lower electrode 12. The sacrificial layer 47 is, for example, an insulating film such as a silicon oxide film. A mask layer 46 is formed in a region that will become the region 54 on the sacrificial layer 47. The mask layer 46 is, for example, a thin metal film. Using the mask layer 46 as a mask, argon ions 48 are irradiated by ion milling. The inclination angle of the ion beam from the Z direction is, for example, 80° to 85°. The wafer is rotated. The ion beam is not irradiated to the region 54 where the mask layer 46 is provided. In the regions 57 and 56, the amount of irradiation of the ion beam is large in the area far from the mask layer 46, and the amount of irradiation of the ion beam is small in the area close to the mask layer 46. As a result, the sacrificial layer 47 becomes thinner as it moves away from the region 54. The irradiation of the ion beam is terminated when the sacrificial layer 47 in the region 56 is removed and the sacrificial layer 47 in the region 57 remains.

[0098] As shown in FIG. 13(b), the mask layer 46 is removed. In the region 56, the sacrificial layer 47 is not formed, and in the region 54, the thickness of the sacrificial layer 47 is constant. In the region 57, the sacrificial layer 47 gradually becomes thinner from the region 54 to the region 56. Argon ions 48 are irradiated using an ion milling method. The inclination angle of the ion beam from the Z direction is, for example, 0° to 5°. When the sacrificial layer 47 is etched, the sacrificial layer 47 is removed from the periphery of the region 57. Therefore, in the region 57, the time during which the ion beam is irradiated to the lower electrode 12 becomes longer from the region 54 to the region 56. As a result, the surface roughness of the upper surface 41 of the lower electrode 12 in the region 57 becomes larger from the region 54 to the region 56. Thereafter, the process of FIG. 12(b) and subsequent steps of the modified example 1 of the embodiment 2 is performed. In this way, the ultrasonic transducer 104 of the modified example 1 of the embodiment 2 is manufactured.

[0099] 12(a) to 13(b), in region 57 (third region) whose inner circumference is the outer periphery of region 54 and whose outer periphery is the inner periphery of region 56, upper surface 41 of lower electrode 12 is roughened so that the surface roughness of upper surface 41 of lower electrode 12 increases from the outer periphery of region 54 toward the inner periphery of region 56. As a result, the average grain size of crystal grains 34 in piezoelectric layer 15c in region 57 increases from region 54 toward region 56.

[0100] In Examples 1 and 2, the average grain size changes abruptly between regions 54 and 56. Therefore, an interface is generated at the boundary between piezoelectric layers 15a and 15b. This may cause vibrations to be reflected at the interface between piezoelectric layers 15a and 15b, resulting in unwanted vibrations. This may cause unwanted vibrations to become noise. In addition, if the average grain size changes abruptly between regions 54 and 56, it is believed that there is also abrupt difference in acoustic impedance. This may cause unwanted vibrations.

[0101] In the first modification of the second embodiment, the average grain size of the crystal grains 34 in the piezoelectric layer 15c in the region 57 becomes smaller from the region 54 to the region 56. This causes a gradual change in the acoustic impedance between the piezoelectric layers 15a and 15b. This suppresses the reflection of vibrations, thereby suppressing unnecessary vibrations. EXAMPLES

[0102] Example 3 is an example in which a seed layer is provided on the piezoelectric layer 15a. Fig. 14 is a cross-sectional view of an ultrasonic transducer according to Example 3.

[0103] In the ultrasonic transducer 106 of the third embodiment, a seed layer 15d is provided between the piezoelectric layer 15a in the region 54 and the lower electrode 12. The seed layer 15d mainly contains the same main component as the piezoelectric layer 15b. The other configurations are the same as those of the first embodiment, and therefore the description will be omitted.

[0104] [Method of manufacturing ultrasonic transducer according to embodiment 3] 15(a) and 15(b) are cross-sectional views showing a manufacturing method of the ultrasonic transducer according to the third embodiment.

[0105] As shown in FIG. 15(a), after performing the step of FIG. 4(a) of Example 1, a seed layer 15d is formed in a region that will become the region 54. The seed layer 15d is formed, for example, by ALD (Atomic Layer Deposition). The seed layer 15d formed by the ALD method has high crystallinity. When an aluminum nitride film is formed as the seed layer 15d, the seed layer 15d has a crystal structure with high c-axis orientation.

[0106] As shown in Fig. 15(b), the piezoelectric layer 14 is formed on the lower electrode 12 and the seed layer 15d by sputtering. Since the seed layer 15d has good crystallinity, the average grain size of the crystal grains 34 of the piezoelectric layer 15a formed on the seed layer 15d is larger than the average grain size of the crystal grains 34 of the piezoelectric layer 15b formed on the lower electrode 12. Then, the steps from Fig. 5(c) onward in Example 1 are performed. In this way, the ultrasonic transducer 106 of Example 3 is manufactured.

[0107] In the third embodiment, as shown in FIG. 15(a), a seed layer 15d is formed on the lower electrode 12 so as to be provided in the region 54 and not provided in the region 56. As shown in FIG. 15(b), a piezoelectric layer 14 is formed on the seed layer 15d in the region 54 and on the lower electrode 12 in the region 56. This allows the average grain size of the crystal grains 34 in the piezoelectric layer 15b to be smaller than the average grain size of the crystal grains 34 in the piezoelectric layer 15a. Furthermore, by forming the piezoelectric layer 14, the piezoelectric layers 15a and 15b can be formed simultaneously, so that the number of manufacturing steps can be reduced compared to the first embodiment. The CMP process in FIG. 5(b) can be omitted. EXAMPLES

[0108] Example 4 is an example in which an amorphous layer is provided instead of the piezoelectric layer 15b. Fig. 16 is a cross-sectional view of an ultrasonic transducer according to Example 4.

[0109] In the ultrasonic transducer 108 of the fourth embodiment, an amorphous layer 17 is provided in place of the piezoelectric layer 15b in the region 56. The amorphous layer 17 is a layer whose crystal structure is amorphous, for example, an insulating layer. For example, silicon oxide (SiO2), aluminum oxide (Al2O3), tantalum oxide (Ta2O5), zirconium oxide (ZrO2), titanium oxide (TiO2), or hafnium oxide (HfO2) can be used as the amorphous layer 17.

[0110] [Method of manufacturing ultrasonic transducer according to embodiment 4] 5(a) of the manufacturing method of the first embodiment, instead of forming the piezoelectric layer 15b, the amorphous layer 17 is formed by sputtering, CVD or vacuum deposition. The amorphous layer 17 may be made of silicon oxide (SiO2), silicon nitride (Si3N4), aluminum oxide (Al2O3), titanium oxide (TiO2), zirconium oxide (ZrO2) or hafnium oxide (HfO2). The other manufacturing methods are the same as those of the first embodiment.

[0111] In the fourth embodiment, an amorphous layer 17 is provided on the substrate 10 and the gap 28 in the region 56 to surround the piezoelectric layer 15a. The amorphous layer 17 is less susceptible to cracks. Therefore, the occurrence of cracks in the piezoelectric layer 15b in the range 58 can be suppressed. EXAMPLES

[0112] Example 5 is an example of a piezoelectric device array in which the ultrasonic transducers of Examples 1 to 4 are arranged in an array. Fig. 17 is a plan view of the ultrasonic transducer according to Example 5.

[0113] In the ultrasonic transducer 110, a plurality of pMUT elements 20 are arranged in an array on the substrate 10. That is, the substrate of the pMUT elements 20 is integrally provided in common. Each pMUT element 20 has a vibration region 50, an S region 52, and regions 54 and 56, and is an ultrasonic transducer according to the first to fourth embodiments. By operating the plurality of pMUT elements 20 at approximately the same frequency, the sound pressure of the transmitted ultrasonic waves can be increased. In addition, the sensitivity of receiving ultrasonic waves can be improved. An ultrasonic transducer with a high sound pressure can be used in aerial tactile sensing, which requires high output, or in a molecular emission control device for an olfactory display that reproduces scents by atomization.

[0114] In piezoelectric devices other than ultrasonic transducers, cracks may occur in the piezoelectric layer 14 in the area 58. Therefore, it is preferable to use the techniques of the first to fifth embodiments.

[0115] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to such specific embodiments, and various modifications and variations are possible within the scope of the gist of the present invention described in the claims. [Explanation of symbols]

[0116] 10 SOI substrate 10a Substrate 10b Stopper layer 10c active layer 11 Insulating layer 12 Lower electrode 14, 15a, 15b, 15c Piezoelectric layers 15d Seed layer 16 Upper electrode 17 Amorphous layer 18 Laminated Film 20 pMUT element 28 void 34 Grains 35 grain boundaries 40 Bottom side 41 Top side 50 vibration area 52, 54, 56, 57 areas 55 center 58 Range

Claims

1. a substrate having an air gap; an intermediate layer provided on the substrate so as to cover the gap in a plan view; a lower electrode provided on the intermediate layer; a piezoelectric layer provided on the lower electrode; an upper electrode, a first region sandwiching the piezoelectric layer together with the lower electrode being provided on the piezoelectric layer on the inner side of the periphery of the gap in a plan view, the area of ​​which in a plan view is smaller than the area of ​​a region surrounded by the periphery of the gap in a plan view; Equipped with A piezoelectric device in which, in a planar view, outside the outer periphery of the first region, the average grain size of the crystal grains of the piezoelectric layer in a second region extending from the inside to the outside of the outer contour of the gap, is smaller than the average grain size of the crystal grains of the piezoelectric layer in the first region.

2. The piezoelectric layer is mainly composed of aluminum nitride, The piezoelectric device of claim 1 , wherein the piezoelectric layer in the second region contains magnesium.

3. 3. The piezoelectric device according to claim 2, wherein the magnesium concentration of the piezoelectric layer in the second region is equal to or greater than 1 atomic % and equal to or less than 10 atomic % when the total of aluminum, magnesium and other additive elements is taken as 100 atomic %.

4. The piezoelectric layer is mainly composed of aluminum nitride, The piezoelectric device of claim 1 , wherein the oxygen concentration of the piezoelectric layer in the second region is higher than the oxygen concentration in the first region.

5. 5. The piezoelectric device according to claim 4, wherein the oxygen concentration of the piezoelectric layer in the second region is 1 atomic % or more and 10 atomic % or less when the total of aluminum, nitrogen and other additive elements is taken as 100 atomic %.

6. The piezoelectric device according to claim 2 , wherein the average grain size of crystal grains in the second region at a position 1 μm from the lower surface of the piezoelectric layer is 30 nm or less.

7. The piezoelectric device according to claim 1 , wherein a surface roughness of the lower surface of the piezoelectric layer in the second region is greater than a surface roughness of the lower surface of the piezoelectric layer in the first region.

8. 8. The piezoelectric device of claim 7, wherein in a planar view, the surface roughness of the underside of the piezoelectric layer in a third region having an inner circumference equal to the outer periphery of the first region and an inner circumference equal to the inner circumference of the second region increases from the outer periphery of the first region toward the inner circumference of the second region.

9. The piezoelectric device according to claim 1 , wherein a seed layer having the same main component as the main component of the piezoelectric layer is provided between the lower electrode and the piezoelectric layer in the first region.

10. The piezoelectric device according to claim 1 , wherein a main component of the piezoelectric layer in the first region is the same as a main component of the piezoelectric layer in the second region.

11. a substrate having an air gap; an intermediate layer provided on the substrate so as to cover the gap in a plan view; a lower electrode provided on the intermediate layer; a piezoelectric layer provided on the lower electrode; an upper electrode, a first region sandwiching the piezoelectric layer together with the lower electrode being provided on the piezoelectric layer on the inner side of the periphery of the gap in a plan view, the area of ​​which in a plan view is smaller than the area of ​​a region surrounded by the periphery of the gap in a plan view; Equipped with an amorphous layer provided on the substrate and the gap in a second region provided outside the outer periphery of the first region in a plan view, the second region being provided from the inside to the outside of the contour of the gap, without the piezoelectric layer therebetween, and surrounding the piezoelectric layer; A piezoelectric device comprising:

12. A piezoelectric device array comprising a plurality of piezoelectric devices according to claim 1 , the substrate being integrally formed with the plurality of piezoelectric devices.

13. forming a first piezoelectric layer mainly made of aluminum nitride on a lower electrode provided on a substrate by sputtering; removing the first piezoelectric layer in a second region provided outside the first region while leaving the first piezoelectric layer in a first region; forming a second piezoelectric layer, the second piezoelectric layer being mainly composed of aluminum nitride and containing magnesium, on the lower electrode in a second region provided outside the outer periphery of the first region by using a sputtering method with a power density lower than the power density used for forming the first piezoelectric layer; forming a top electrode on the first piezoelectric layer in the first region; forming the gap in the substrate such that the upper electrode is provided inside an outer periphery of the gap in a plan view, the area of ​​the upper electrode in a plan view is smaller than the area of ​​a region surrounded by the outer periphery of the gap in a plan view, and the second region extends from the inside to the outside of the outer periphery of the gap outside the periphery of the first region; A method for manufacturing a piezoelectric device comprising the steps of:

14. forming a first piezoelectric layer mainly made of aluminum nitride on a lower electrode provided on a substrate by sputtering; removing the first piezoelectric layer in a second region provided outside the first region while leaving the first piezoelectric layer in a first region; forming a second piezoelectric layer, which is mainly composed of aluminum nitride and has a higher oxygen concentration than the first piezoelectric layer, on the lower electrode in a second region provided outside the periphery of the first region by using a sputtering method; forming a top electrode on the first piezoelectric layer in the first region; forming the gap in the substrate such that the upper electrode is provided inside an outer periphery of the gap in a plan view, the area of ​​the upper electrode in a plan view is smaller than the area of ​​a region surrounded by the outer periphery of the gap in a plan view, and the second region extends from the inside to the outside of the outer periphery of the gap outside the periphery of the first region; A method for manufacturing a piezoelectric device comprising the steps of:

15. roughening an upper surface of the lower electrode in a second region provided on the substrate such that a surface roughness of the upper surface of the lower electrode in a first region is smaller than a surface roughness of the upper surface of the lower electrode in a second region provided outside an outer periphery of the first region; forming a piezoelectric layer on the bottom electrode in the first region and the second region; forming a top electrode on the piezoelectric layer in the first region; forming the gap in the substrate such that the upper electrode is provided inside an outer periphery of the gap in a plan view, the area of ​​the upper electrode in a plan view is smaller than the area of ​​a region surrounded by the outer periphery of the gap in a plan view, and the second region extends from the inside to the outside of the outer periphery of the gap outside the periphery of the first region; A method for manufacturing a piezoelectric device comprising the steps of:

16. 16. The method for manufacturing a piezoelectric device according to claim 15, wherein the step of roughening the upper surface of the lower electrode includes a step of roughening the upper surface of the lower electrode in a third region located between the first region and the second region such that the surface roughness of the upper surface of the lower electrode increases from the first region toward the second region.

17. forming a seed layer on a lower electrode provided on the substrate in a first region; forming a piezoelectric layer on the seed layer in the first region and on the bottom electrode in a second region disposed outside an outer periphery of the first region; forming a top electrode on the piezoelectric layer in the first region; forming the gap in the substrate such that the upper electrode is provided inside an outer periphery of the gap in a plan view, the area of ​​the upper electrode in a plan view is smaller than the area of ​​a region surrounded by the outer periphery of the gap in a plan view, and the second region extends from the inside to the outside of the outer periphery of the gap outside the periphery of the first region; A method for manufacturing a piezoelectric device comprising the steps of:

Citation Information

Patent Citations

  • Aluminum nitride film, piezoelectric device, resonator, filter and multiplexer

    JP2021150920A

  • Piezoelectric micromachined ultrasonic transducer with a patterned membrane structure

    US20200194658A1