Method for manufacturing water-repellent layer for fuel cell, water-repellent layer for fuel cell and gas diffusion layer for fuel cell using the same

By employing hydrophilic carbon particles and thermosetting resin particles with controlled processing, the method enhances bonding strength and energy efficiency in the production of a water-repellent layer for fuel cells, addressing the inefficiencies of conventional high-temperature methods.

JP2024137772APending Publication Date: 2024-10-07KK TOYOTA CHUO KENKYUSHO

Patent Information

Application Number
JP2024032124
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-10-17
Filing Date
2024-03-04
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

Conventional methods for manufacturing a water-repellent layer for fuel cells face challenges in achieving sufficient bonding strength between the water-repellent layer and the porous base material, and they are energy inefficient due to high temperature heating processes, particularly when using thermoplastic resins like PTFE.

Method used

A method involving the use of hydrophilic carbon particles and thermosetting resin particles, with a specific content ratio and processing conditions, including dry film forming, pressure application, and lower temperature firing, to create a mixed bonded body with enhanced bonding strength and energy efficiency.

Benefits of technology

The method results in a water-repellent layer with improved bonding strength to the porous base material, achieved with higher energy efficiency and reduced manufacturing costs, suitable for use in fuel cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137772000008
    Figure 2024137772000008
  • Figure 2024137772000009
    Figure 2024137772000009
  • Figure 2024137772000010
    Figure 2024137772000010
Patent Text Reader

Abstract

To provide a method for manufacturing a water-repellent layer for a fuel cell which can efficiently manufacture a water-repellent layer for a fuel cell with high energy efficiency, and can make joint strength between the water-repellent layer and a porous base material higher, when the water-repellent layer is formed on the surface of a porous base material for a gas diffusion layer.SOLUTION: A method for manufacturing a water-repellent layer for a fuel cell includes the steps of: forming mixed powder of powder (A) of specific hydrophilic carbon particles, and powder (B) of specific resin raw material particles composed of a raw material of a thermosetting resin, in which a content of the powder (B) is in a specific ratio, by a dry film-formation method, and forming a mixed powder layer; pressurizing the mixed powder layer under a specific condition, and compacting it; baking the mixed powder layer after the compaction under a specific condition, and thereby obtaining a water-repellent layer for a fuel cell composed of a mixed joined body of the powder (A) of the hydrophilic carbon particles and a water-resistant resin (C) composed of a thermosetting resin that is a polycondensation of the raw material.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a water-repellent layer for a fuel cell, a water-repellent layer for a fuel cell, and a gas diffusion layer for a fuel cell using the same. [Background technology]

[0002] A fuel cell generally comprises a membrane electrode assembly (MEA) as a basic unit, in which electrodes including a catalyst layer are bonded to both sides of an electrolyte membrane. Here, the electrodes generally have a two-layer structure of a gas diffusion layer and a catalyst layer. Such a gas diffusion layer is used to supply reactant gases and electrons to the catalyst layer, which is the reaction field of the electrode reaction, and therefore has been required to have gas permeability and properties that enable water management (e.g., water repellency). For this reason, a gas diffusion layer that generally comprises a porous substrate such as carbon paper or carbon cloth and a water-repellent layer laminated on the surface of the porous substrate is used. As a manufacturing method for such a water-repellent layer for a fuel cell, for example, JP 2021-2444 A (Patent Document 1) discloses a method comprising the steps of preparing a granule comprising first particles made of spheroidized graphite, second particles containing fine carbon having a particle size smaller than that of the first particles, and a water-repellent polymer, and in which the second particles are bonded to the surface of the first particles via the water-repellent polymer, applying the granule to a substrate surface using a powder coating device, and heat-treating the resulting coating film. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2021-2444 Summary of the Invention [Problem to be solved by the invention]

[0004] However, when the conventional method for producing a water-repellent layer as described in Patent Document 1 is adopted, the bonding strength between the water-repellent layer and the porous substrate cannot be necessarily made sufficient. In Patent Document 1, the use of a fluorine-based resin (thermoplastic resin) such as polytetrafluoroethylene (PTFE) as a polymer used in the water-repellent layer is specifically disclosed, but the use of other resins (for example, thermosetting resins, etc.) as raw materials is not specifically described. In addition, in the examples of Patent Document 1, a specific example is disclosed in which a granule is produced using PTFE as a polymer used in the water-repellent layer, the granule is applied to the surface of a substrate, and the granule is pressed under conditions of 1.0 MPa, 1 minute, and room temperature, and then a heat treatment (baking) is performed at a high temperature such as 350°C, but a specific example of heat treatment at another temperature is not specifically disclosed. The conventional method actually adopted in the examples of Patent Document 1 is a method in which heating is performed at a relatively high temperature during production due to the type of resin, etc., and there is room for improvement in terms of energy efficiency.

[0005] The present invention has been made in consideration of the problems associated with the above-mentioned conventional technology, and aims to provide a method for producing a water-repellent layer for a fuel cell, which makes it possible to efficiently produce a water-repellent layer for a fuel cell with high energy efficiency, and which makes it possible to increase the bonding strength between the water-repellent layer and a porous substrate when the water-repellent layer is formed on the surface of a porous substrate for a gas diffusion layer; a water-repellent layer for a fuel cell that can be efficiently produced by adopting this manufacturing method and which makes it possible to increase the bonding strength between the water-repellent layer and a porous substrate; and a gas diffusion layer for a fuel cell comprising this water-repellent layer for a fuel cell. [Means for solving the problem]

[0006] As a result of intensive research by the inventors in order to achieve the above object, they have discovered a method for producing a water-repellent layer for a fuel cell, comprising the steps of: utilizing a mixed powder containing a powder (A) of hydrophilic carbon particles having an average particle size of 0.002 to 50 μm and a powder (B) of resin raw material particles made of a thermosetting resin raw material and having an average particle size of 0.01 to 50 μm, such that the content of the powder (B) is 15 to 60 mass % based on the total amount of the powders (A) and (B), forming the mixed powder into a film by a dry film forming method, compressing the obtained mixed powder layer under a pressure of 0.2 to 50 MPa, and then compressing the compressed mixed powder layer by applying a pressure of 0.2 to 50 MPa to the thermosetting resin (a polycondensate of the raw materials). The inventors have found that by using a method for obtaining a water-repellent layer for a fuel cell comprising a mixed bond of a powder of hydrophilic carbon particles (A) and a water-resistant resin (C) made of a thermosetting resin which is a polycondensation product of the raw materials, the water-repellent layer can be produced efficiently with high energy efficiency, and when a water-repellent layer is formed on the surface of a porous substrate for a gas diffusion layer, the bonding strength between the water-repellent layer and the porous substrate can be increased, thereby completing the present invention.

[0007] That is, the present invention provides the following aspects.

[0008] [1] A film-forming process of forming a mixed powder layer by forming a film of a mixed powder containing a powder (A) of hydrophilic carbon particles having an average particle size of 0.002 to 50 μm and a powder (B) of resin raw material particles made of a thermosetting resin raw material and having an average particle size of 0.01 to 50 μm, the mixed powder having a content of the powder (B) of 15 to 60 mass% based on the total amount of the powders (A) and (B) by a dry film-forming method; a consolidation step of compressing the mixed powder layer under a pressure of 0.2 to 50 MPa; a water-repellent layer forming step of calcining the mixed powder layer after the consolidation step at a temperature 10 to 130° C. lower than the decomposition temperature of the thermosetting resin to obtain a water-repellent layer for a fuel cell made of a mixed bond of the hydrophilic carbon particle powder (A) and a water-resistant resin (C) made of a thermosetting resin which is a polycondensate of the raw materials; The method for producing a water-repellent layer for a fuel cell includes the steps of:

[0009] [2] The method for producing a water-repellent layer for a fuel cell according to [1], wherein the thermosetting resin is at least one resin selected from the group consisting of phenolic resin, silicone resin, polyurethane resin, urea resin, melamine resin, and acrylic resin.

[0010] [3] The method for producing a water-repellent layer for a fuel cell according to [1] or [2], wherein the thermosetting resin is a melamine resin.

[0011] [4] The method for producing a water-repellent layer for a fuel cell according to any one of [1] to [3], wherein in the film-forming step, a film is formed on a surface of a substrate to be film-formed by using at least one raw material of the resin constituting the thermosetting resin (at least one raw material of the thermosetting resin) and / or a porous substrate having at least one resin constituting the thermosetting resin on its surface.

[0012] [5] A layer made of a sintered product of a mixed powder, comprising: a powder (A) of hydrophilic carbon particles having an average particle size of 0.002 to 50 μm; and a powder (B) of resin raw material particles made of a thermosetting resin raw material having an average particle size of 0.01 to 50 μm, the powder (B) having a content of 15 to 60 mass% based on the total amount of the powders (A) and (B); The layer is a layer made of a mixed bond of the hydrophilic carbon particle powder (A) and a water-resistant resin (C) made of a thermosetting resin which is a polycondensation product of the raw materials, and The water-repellent layer for a fuel cell, wherein the content of the water-resistant resin (C) in the mixed bonded body is 13 to 57 mass % based on the total amount of the powder (A) and the water-resistant resin (C).

[0013] [6] A gas diffusion layer for a fuel cell, comprising: a porous substrate; and the water-repellent layer for a fuel cell according to [5] laminated on a surface of the porous substrate.

[0014] [7] The gas diffusion layer for a fuel cell according to [6], wherein the porous substrate is a porous substrate having at least one of the resins constituting the thermosetting resin on a surface thereof. Effect of the Invention

[0015] According to the present invention, it is possible to provide a method for producing a water-repellent layer for a fuel cell that can efficiently produce a water-repellent layer for a fuel cell with high energy efficiency, and that can increase the bonding strength between the water-repellent layer and a porous substrate when the water-repellent layer is formed on the surface of a porous substrate for a gas diffusion layer; a water-repellent layer for a fuel cell that can be efficiently produced by adopting this manufacturing method and that can increase the bonding strength between the water-repellent layer and a porous substrate; and a gas diffusion layer for a fuel cell that includes this water-repellent layer for a fuel cell. [Brief description of the drawings]

[0016] [Figure 1] 1 is a photograph showing the dispersion state when the hydrophilic carbon particles and the hydrophobic carbon particles used in the examples and comparative examples are added to water (methanol concentration: 0 mass %). [Diagram 2] 1 is a graph showing the bonding strength of the water-repellent layers produced in Examples 1 to 11 and Comparative Examples 1 to 3 to carbon paper. [Diagram 3] Photographs of the appearance of resin at each firing temperature. [Figure 4] 2 is a graph showing a TG curve and a DTA curve of a powder of resin raw material particles of a melamine resin used in the examples. [Diagram 5] 1 is an electron microscope photograph (SEM image) of the water-repellent layer produced in Example 7. [Figure 6] 1 is an electron microscope photograph (SEM-EDS image) of the water-repellent layer produced in Example 7. [Figure 7] 1 is an electron microscope photograph (SEM image) of the mixed powder used to produce the water-repellent layer in Example 7. [Figure 8] 1 is an electron microscope photograph (SEM-EDS image) of the mixed powder used to produce the water-repellent layer in Example 7. [Figure 9] 1 is a photograph of the peeled surface of the laminate obtained in Example 8 after a 90 degree peel strength test. [Figure 10] 1 is a photograph of the peeled surface of the laminate obtained in Example 13 after a 90 degree peel strength test. [Figure 11] 1 is a graph showing a TG curve and a DTA curve of the same powder as the powder of resin raw material particles used in producing the water-repellent layer in Example 16. [Figure 12] 1 is a graph showing the bonding strength of the water-repellent layers produced in Examples 12 to 15, Examples 16 to 22, and Comparative Example 5 to carbon paper. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The present invention will be described in detail below based on preferred embodiments thereof.

[0018] [Method for producing water-repellent layer for fuel cell] The method for producing a water-repellent layer for a fuel cell of the present invention includes the steps of: a film-forming step of forming a mixed powder layer by forming a film of a mixed powder, the mixed powder including a powder (A) of hydrophilic carbon particles having an average particle size of 0.002 to 50 μm and a powder (B) of resin raw material particles made of a thermosetting resin raw material having an average particle size of 0.01 to 50 μm, the content of the powder (B) being 15 to 60 mass % based on the total amount of the powders (A) and (B), by a dry film-forming method; a consolidation step of compressing the mixed powder layer under a pressure of 0.2 to 50 MPa; a water-repellent layer-forming step of baking the mixed powder layer after the consolidation step at a temperature 10 to 130° C. lower (more preferably a temperature 50 to 110° C. lower) than the decomposition temperature of the thermosetting resin to obtain a water-repellent layer for a fuel cell made of a mixed bond of the hydrophilic carbon particle powder (A) and a water-resistant resin (C) made of a thermosetting resin which is a polycondensate of the raw materials; Each step will be described below separately.

[0019] <Film formation process> The film-forming process according to the present invention is a process for forming a mixed powder layer by forming a film of a mixed powder containing the powder (A) and the powder (B), and in which the content of the powder (B) is 15 to 60 mass % based on the total amount of the powders (A) and (B), by a dry film-forming method.

[0020] The powder (A) is a powder of hydrophilic carbon particles having an average particle size of 0.002 to 50 μm. Thus, the powder (A) is composed of hydrophilic carbon particles. The properties of such carbon particles, such as "hydrophilic" and "hydrophobic", can be evaluated by the so-called Methanol Wettability method (see Mitsuru Ochiai, Aerosol Research, vol. 5, 1990, pp. 32-43). Specifically, water and methanol aqueous solutions with different methanol concentrations are prepared, and carbon particles are gently added to the water and each aqueous solution. The methanol concentration at which the carbon particles disperse in the methanol aqueous solution (the methanol concentration in the aqueous solution with the lowest methanol concentration among the aqueous solutions in which the carbon particles disperse: 0 in the case of water) is obtained. If the methanol concentration is less than 2% by mass, the carbon particles are evaluated as "hydrophilic", and if the methanol concentration is 2% by mass or more (if the carbon particles are dispersed in the methanol aqueous solution when the carbon particles are added to the methanol aqueous solution with a methanol concentration of 2% by mass or more), the carbon particles are evaluated as "hydrophobic". Such hydrophilic carbon particles can be obtained, for example, by subjecting carbon particles to a known hydrophilic treatment (open corona discharge treatment, steam oxidation treatment, acid treatment, etc.).

[0021] The powder (A) is a powder made of the hydrophilic carbon particles and has an average particle size of 0.002 to 50 μm (more preferably 0.002 to 30 μm, even more preferably 0.002 to 10 μm, and particularly preferably 0.002 to 1 μm). By setting the average particle size to be equal to or more than the lower limit, gas diffusibility can be improved compared to the case where the average particle size is less than the lower limit, and power generation performance can be improved. On the other hand, by setting the average particle size to be equal to or less than the upper limit, electronic resistance can be reduced compared to the case where the average particle size exceeds the upper limit, and power generation performance can be improved. Note that, as the powder (A) of hydrophilic carbon particles having an average particle size of 0.002 to 50 μm, a commercially available product may be used. The average particle size of such powder (A) can be measured by measuring the particle size of 500 randomly selected particles using a particle size distribution measuring device or an electron microscope and calculating the average. The average particle size of the primary particles is adopted as the average particle size of such powder (A).

[0022] Moreover, the powder (B) is a powder of resin raw material particles made of the thermosetting resin raw material and having an average particle size of 0.01 to 50 μm. That is, the powder (B) is composed of particles of the thermosetting resin raw material (resin raw material particles). In this way, the present invention uses a powder made of particles of the thermosetting resin raw material as a material used in manufacturing the water-repellent layer without using a powder of a fluororesin (thermoplastic resin) such as PTFE, which is expensive and has a high melting temperature, and therefore the baking temperature during heat treatment can be lowered, which makes it possible to form the water-repellent layer with high energy efficiency and reduce the manufacturing cost.

[0023] The raw material of the thermosetting resin forming the resin raw material particles constituting such powder (B) is not particularly limited as long as it is capable of expressing water resistance in the thermosetting resin obtained after polycondensation (curing by heat treatment) of the raw material (in other words, it is sufficient as long as it is a raw material of a thermosetting resin having water resistance), and a component (precursor of a thermosetting resin) that is a raw material of a thermosetting resin having water resistance, such as a monomer of a thermosetting resin (water-resistant resin) having water resistance formed after baking or a low condensate of the monomer, can be appropriately used. In addition, the raw material of the thermosetting resin is sufficient as long as it can form a water-resistant resin (C) made of a thermosetting resin when the water-repellent layer is finally formed, and even if the raw material itself is in a condensation state, it can be used (as long as the condensation product can be further polycondensed (cured by heat treatment) to form a water-resistant resin (C), it can be used). Thus, the form of the "thermosetting resin raw material" is not particularly limited as long as it can be used as a raw material of the thermosetting resin constituting the water-resistant resin (C) to be finally formed, and a monomer or a (low) condensate of the monomer can be appropriately used. That is, the "thermosetting resin raw material" is not limited to a so-called monomer, and even if it is in a condensation state (polymer: resin), it can be appropriately used as long as it has a functional group or the like and can be further polycondensed to form the water-resistant resin (C). As such a thermosetting resin raw material (thermosetting resin precursor), from the viewpoint that the polymerization temperature can be relatively low and that it has a high affinity with carbon particles, a phenol resin raw material, a silicone resin raw material, a polyurethane resin raw material, a urea resin raw material, a melamine resin raw material, and an acrylic resin raw material are preferable. That is, the thermosetting resin raw material is preferably at least one thermosetting resin raw material selected from the group consisting of a phenol resin, a silicone resin, a polyurethane resin, a urea resin, a melamine resin, and an acrylic resin. As the raw material for such a thermosetting resin, any known material (monomer of each resin or its low condensate: it may be a commercially available product) that can exhibit water resistance after polycondensation (thermosetting) can be appropriately used.The resin raw material particles made of such thermosetting resin raw materials may be used alone or in combination of two or more kinds.

[0024] As the raw material of the thermosetting resin, it is preferable to use a raw material of a melamine resin (monomer or its low condensate) from the viewpoint that the polymerization can be sufficiently progressed even at a low polymerization temperature, the affinity with carbon particles is high, and in addition, a high effect can be obtained in terms of cost. As the raw material of such a melamine resin, it is preferable to use methylol melamine, a low condensate of methylol melamine (an initial condensate of melamine and formaldehyde), and methylated melamine from the viewpoint of lowering the polymerization temperature, high affinity with carbon particles, cost, and higher effects can be obtained in terms of workability, and a low condensate of methylol melamine (an initial condensate of melamine and formaldehyde) is more preferable. As such a low condensate of methylol melamine, it is also possible to use one obtained by appropriately carrying out an etherification process, etc., and among them, a low condensate of methylol melamine having an amino group, an imino group, a methylol group, and an alkyl ether group can be preferably used. As such a low condensate of methylol melamine (melamine resin), a commercially available product (for example, "Nikaresin S260" manufactured by Nippon Carbide Industries Co., Ltd.) may be used. By polycondensing resin raw material particles made of such a low condensate of methylol melamine, it is possible to form a water-resistant resin made of melamine resin, which is a polycondensate of methylol melamine. As the methylated melamine (melamine resin), methylated melamine (melamine resin) having an amino group, an imino group, a methylol group, and an alkyl ether group can be suitably used. By using such a raw material of a thermosetting resin having a functional group such as an amino group, an imino group, or a methylol group, it is possible to easily react with other components having an amino group, an amide group, a carboxyl group, a hydroxyl group, or the like (other thermosetting resin materials having a functional group that reacts with an amino group, an amide group, a carboxyl group, a hydroxyl group, or the like) to harden the resin. In addition, as such methylated melamine, a commercially available product (for example, "Nicalac MX035" manufactured by Nippon Carbide Industries Co., Ltd.) may be used. When a commercially available product is used and the commercially available product is in liquid form, it may be used in particulate form by drying and then pulverizing the product.In addition, when the raw material (commercial product, etc.) used for the thermosetting resin is liquid, for example, the raw material may be supported (attached) to the surface of hydrophilic carbon particles constituting the powder (A), dried, and the surface of the carbon particles may be coated (composite) with the raw material of the thermosetting resin to obtain resin raw material-coated carbon particles (composite particles of carbon and resin raw material). (Note that in this specification, the term "coated" with respect to "resin raw material-coated carbon particles" is used as a term including a state in which the whole particle is covered with the raw material, as well as a state in which only a part of the surface is covered with the raw material (supported state), that is, a state in which the raw material is supported (attached) to a part of the surface). Here, the carbon particles (coated object coated with the resin raw material) present in the resin raw material-coated carbon particles are regarded as carbon particles constituting the powder (A) in the present invention.

[0025] In addition, when two or more kinds of raw materials for the thermosetting resin are mixed and used, it is preferable to use a combination of a raw material for melamine resin (monomer or its low condensation product, methylated melamine, etc.) and a raw material for acrylic resin (one that can be further polycondensed) from the viewpoint of improving durability such as weather resistance, corrosion resistance, contamination resistance, and chemical resistance. As described above, the raw material for the thermosetting resin is more preferably one that contains a raw material for melamine resin, and it is preferable to use one that consists only of a raw material for melamine resin, or a combination of a raw material for melamine resin and a raw material for acrylic resin. In addition, when two or more kinds of raw materials for the thermosetting resin are mixed and used, one resin raw material may be a powder consisting of particles of the resin raw material alone, and the other resin raw material may be a powder of carbon particles coated with the resin raw material, and these may be mixed.

[0026] The powder (B) is a powder made of the resin raw material particles and has an average particle size of 0.01 to 50 μm (more preferably 0.01 to 40 μm, and even more preferably 0.01 to 30 μm). By making the average particle size equal to or less than the upper limit, the dispersibility of the resin in the mixed powder is higher than when the average particle size exceeds the upper limit, and the water-resistant resin and the carbon particles can be more uniformly dispersed and mixed in the finally obtained water-repellent layer, thereby improving the power generation performance of the fuel cell. The average particle size of such powder (B) can be measured by measuring the particle size of 500 particles randomly selected by a particle size distribution measuring device or an electron microscope and calculating the average. The average particle size of the primary particles of the resin raw material particles constituting the powder is adopted as the average particle size of such powder (B). Furthermore, when using a powder of the resin raw material coated carbon particles (particles obtained by supporting the thermosetting resin raw material on the surfaces of hydrophilic carbon particles constituting the powder (A), drying the particles, and coating the surfaces of the carbon particles with the thermosetting resin raw material), the average particle diameter of the resin raw material coated carbon particles is assumed to be the average particle diameter of the primary particles of the resin raw material. In this way, when using a powder of the resin raw material coated carbon particles, the average particle diameter of the resin raw material coated carbon particles is adopted as the average primary particle diameter of the particles of the thermosetting resin raw material coated on the surfaces of the hydrophilic carbon particles. The average particle diameter of the carbon particles contained in the resin raw material coated carbon particles can be adopted as the average particle diameter of the powder of hydrophilic carbon particles constituting the powder (A) as it is.

[0027] The mixed powder used in the film forming step contains the powder (A) and the powder (B). When the powder of the resin raw material coated carbon particles is used, the inclusion of the powder of the resin raw material coated carbon particles results in the system containing the powder of carbon particles (the powder of carbon particles present in the resin raw material coated carbon particles) and the powder of the raw material of the thermosetting resin. Therefore, in the present invention, when the powder of the resin raw material coated carbon particles is included, it is considered that the powder (A) and the powder (B) are included. That is, in the present invention, when the powder of the resin raw material coated carbon particles is used, the powder of the resin raw material coated carbon particles itself is considered to be a mixed powder containing the powder (A) and the powder (B), and the powder of the resin raw material coated carbon particles is judged to be a powder (mixed powder) that satisfies the condition that it contains the powder (A) and the powder (B).

[0028] In such a mixed powder, the content of the powder (B) is 15 to 60% by mass (more preferably 15 to 50% by mass, and even more preferably 25 to 35% by mass) based on the total amount of the powders (A) and (B). By setting the content of the powder (B) to be equal to or more than the lower limit, it is possible to improve the bonding strength of the water-repellent layer to the porous substrate compared to when it is less than the lower limit, and on the other hand, by setting the content of the powder (B) to be equal to or less than the upper limit, it is possible to make the bonding strength higher compared to when it exceeds the upper limit, and it is possible to form a water-repellent layer with higher convenience without increasing the electronic resistance of the water-repellent layer to such an extent that it becomes difficult to use it for fuel cell applications. In addition, when the powder (B) is composed of the powder of the resin raw material coated carbon particles and other types of resin raw material particles, the content of the powder (B) is calculated by regarding the total amount of the mass of only the resin in the powder of the resin raw material coated carbon particles and the mass of the powder of the other types of resin raw material particles as the mass of the powder (B).

[0029] Furthermore, the mixed powder may contain other components, if necessary, in addition to the powder (A) and the powder (B). Such other components are not particularly limited as long as they do not impair the function of the water-repellent layer formed after firing, and examples thereof include components for promoting the curing of the thermosetting resin constituting the particles in the powder (B).

[0030] Furthermore, with respect to the powder (A) and the powder (B) contained in the mixed powder, the ratio of the average particle diameter of the powder (B) to the average particle diameter of the powder (A) ([average particle diameter of the powder (B)] / [average particle diameter of the powder (A)]) is preferably 0.01 / 0.002 to 50 / 50, more preferably 0.01 / 0.002 to 40 / 30. By setting such a ratio to be equal to or greater than the lower limit, the bonding strength of the water-repellent layer to the porous substrate tends to be improved compared to when the ratio is less than the lower limit, and on the other hand, by setting the ratio to be equal to or less than the upper limit, the bonding strength of the water-repellent layer to the porous substrate tends to be improved compared to when the ratio exceeds the upper limit.

[0031] In addition, such a mixed powder can be obtained by mixing (stirring) the powder (A) and the powder (B) so that the content of the powder (B) is 15 to 60 mass% with respect to the total amount of the powders (A) and (B). The method of mixing (stirring) is not particularly limited, and any known method that can sufficiently uniformly mix the powder (A) and the powder (B) can be appropriately adopted, such as using a commercially available stirrer and mixing under appropriately set stirring conditions. In addition, when other components are to be contained in the mixed powder as necessary, the components may be mixed together during the mixing. In addition, other methods for producing such a mixed powder are not particularly limited, and for example, a method of mixing (stirring) and pulverizing the powder (A) and the raw material of the thermosetting resin that is not particulate (for example, lump-shaped, film-shaped, etc.) with a commercially available stirrer that can also be used as a pulverizer to satisfy the conditions of the mixed powder may be adopted. As another method for producing such a mixed powder, for example, a method may be adopted in which the powder (A) is added to the liquid thermosetting resin raw material, dispersed, and then dried to coat the surfaces of the carbon particles constituting the powder (A) with the raw material to obtain resin raw material-coated carbon particles, and then resin raw material particles made of a different type of thermosetting resin raw material from the raw material are added thereto and mixed to produce a mixed powder.

[0032] In the film-forming step, the mixed powder is formed into a film by a dry film-forming method to form a layer (mixed powder layer) made of the mixed powder. In this way, in the present invention, the mixed powder is formed into a film by a dry film-forming method. There is no particular limitation on such a dry film-forming method, and known methods (for example, electrostatic screen printing, electrostatic painting, etc.) can be appropriately used. In addition, as such a dry film-forming method, it is preferable to adopt a film-forming method by electrostatic screen printing. Among them, it is preferable to adopt an electrostatic screen printing method in which a screen is placed above a film-forming substrate (such as a porous substrate for a gas diffusion layer) on which a coating film is to be formed, the mixed powder is placed on the screen, and the mixed powder is rubbed into the screen using a pressing member (such as a squeegee) to coat the mixed powder and form a film, because the mixed powder having a desired particle size can be more easily applied (formed into a film) and the thickness of the mixed powder layer obtained after application can be more easily adjusted to a desired thickness. In addition, when electrostatic screen printing is used as the dry film formation method, various film formation conditions such as the type of screen (mesh) and the voltage magnitude can be set appropriately depending on the design of the water-repellent layer to be produced, and conditions used in known electrostatic screen printing methods can be appropriately adopted.

[0033] In addition, in such a film-forming process, the substrate on which the mixed powder is formed can be appropriately selected depending on the intended use and is not particularly limited, but when the laminate of the substrate and the water-repellent layer obtained after the water-repellent layer is finally formed is used as a gas diffusion layer, it is preferable that the substrate is a porous substrate for the gas diffusion layer. Examples of such porous substrates include carbon paper and carbon cloth.

[0034] In addition, in such a film-forming process, it is preferable to use a porous substrate having at least one raw material of the resin constituting the thermosetting resin (at least one raw material of the thermosetting resin) and / or at least one resin constituting the thermosetting resin (polycondensate of the raw material) on its surface as the substrate on which the mixed powder is formed. In this way, in the film-forming process, by using a "porous substrate having at least one raw material of the resin constituting the thermosetting resin and / or at least one resin constituting the thermosetting resin on its surface" as the substrate on which the mixed powder is formed, it is possible to dramatically improve the bonding strength between the finally obtained water-repellent layer and the porous substrate (substrate having at least the thermosetting resin on its surface). As the "at least one kind of raw material of the resin constituting the thermosetting resin (at least one kind of raw material of the thermosetting resin)" on the surface of such a porous substrate, the same as that described as the "raw material of the thermosetting resin" forming the resin raw material particles constituting the powder (B) can be appropriately used. For example, since it is possible to increase the bonding strength between the porous substrate and the water-repellent layer, a suitable example is to use at least one kind of the raw material of the thermosetting resin used as the powder (B) and at least one kind of the raw material of the thermosetting resin possessed by the porous substrate. In addition, when the substrate to be coated is a porous substrate having at least one kind of raw material of the resin constituting the thermosetting resin (raw material of the thermosetting resin) on the surface, the raw material of the thermosetting resin is preferably methylol melamine or a low condensate of methylol melamine (initial condensate of melamine and formaldehyde), and more preferably a low condensate of methylol melamine (initial condensate of melamine and formaldehyde).In addition, as the "at least one type of resin constituting the thermosetting resin" on the surface of the porous substrate, the same as the thermosetting resin which is a polycondensate of the raw material (the thermosetting resin described below as "water-resistant resin (C)") or the same as at least one of the resins constituting the composite resin when the polycondensate of the raw material is a composite resin can be appropriately used, and for example, since it is possible to increase the bonding strength between the porous substrate and the water-repellent layer, it is possible to cite at least one type of resin constituting the water-resistant resin (C) in the water-repellent layer and at least one type of resin constituting the thermosetting resin possessed by the porous substrate as a suitable example (for example, when the water-resistant resin (C) in the water-repellent layer is made of melamine resin, or when the water-resistant resin (C) in the water-repellent layer is made of a composite of melamine resin and acrylic resin, at least one type of resin constituting the thermosetting resin possessed by the porous substrate on the surface is made of melamine resin (the thermosetting resin possessed by the porous substrate on the surface is made of melamine resin). Furthermore, when the substrate on which the film is formed is a porous substrate having at least one of the resins constituting the thermosetting resin on its surface, it is particularly preferable that the thermosetting resin on the surface is a melamine resin.

[0035] Furthermore, when the substrate to be coated with a film is a porous substrate (e.g., carbon paper) having at least one of the raw materials constituting the thermosetting resin and / or at least one of the resins constituting the thermosetting resin on its surface, the raw materials are simultaneously polycondensed to become the thermosetting resin by baking in the water-repellent layer formation process described below, so that the substrate to be finally obtained (substrate to be coated with a film after baking) is a porous substrate having at least one of the resins constituting the thermosetting resin (e.g., a polycondensate of at least one of the raw materials constituting the thermosetting resin) on its surface. In addition, when the substrate to be coated is a porous substrate (e.g., carbon paper) having at least one of the raw materials of the resin constituting the thermosetting resin and / or at least one of the resins constituting the thermosetting resin on the surface, the content (total amount) of at least one of the raw materials of the resin constituting the thermosetting resin and at least one of the resins constituting the thermosetting resin is preferably such that the amount of the thermosetting resin in the substrate to be coated after the baking (the "porous substrate having at least one of the resins constituting the thermosetting resin on the surface" obtained after the baking) is 13 to 23 mass% (more preferably 13 to 21 mass%). If the content (total amount) of the raw materials of the thermosetting resin and the thermosetting resin is less than the lower limit, the bonding strength at the interface between the water-repellent layer and the porous substrate tends to decrease, while if it exceeds the upper limit, the electronic resistance tends to increase.

[0036] In addition, the method for producing a porous substrate having at least one of the raw materials of the resin constituting the thermosetting resin and / or at least one of the resin constituting the thermosetting resin on the surface is not particularly limited, and at least one of the raw materials of the resin constituting the thermosetting resin (at least one of the raw materials of the thermosetting resin) and / or at least one of the resins constituting the thermosetting resin can be appropriately used. For example, when the raw materials of the thermosetting resin are attached to obtain a porous substrate, a method of producing a porous substrate having the raw materials of the thermosetting resin at least on the surface by attaching the raw materials of the thermosetting resin to at least the surface of the porous substrate by preparing an aqueous solution containing the same type of raw materials as the "raw materials of the thermosetting resin" described in the powder (B) and immersing the porous substrate in the aqueous solution and then vacuum drying the porous substrate can be adopted. In this way, when the raw materials are coated (applied) to the porous substrate by performing a process of immersing the porous substrate in the aqueous solution, a coating film of the raw materials can be formed on the porous substrate. In addition, in the case where a porous substrate having at least the thermosetting resin raw material on its surface is produced in this manner, the mixed powder layer is dry-formed on the porous substrate, and then the mixed powder layer is baked by carrying out the water-repellent layer forming process described later, so that the raw material on the surface of the porous substrate is simultaneously baked (polycondensed), which is presumably capable of further improving the bonding strength at the interface between the water-repellent layer and the porous substrate. In addition, when a porous substrate having at least one of the resins constituting the thermosetting resin on its surface is produced as a substrate to be coated, it is sufficient to bake the substrate so that the raw material is polycondensed after attaching at least one of the raw materials of the thermosetting resin. The baking temperature in this case is not particularly limited, but the same temperature as the baking temperature described in the water-repellent layer forming process described later can be adopted. Furthermore, when manufacturing a porous substrate so that the content of the thermosetting resin in the final substrate (substrate to be coated after firing) is 13 to 23 mass %, it is preferable to set the amount of raw material before polycondensation to be attached to the porous substrate to 15 to 25 mass %, taking into consideration, for example, the amount of components that evaporate due to condensation, etc.

[0037] In the film-forming step, the thickness of the mixed powder layer obtained is preferably 5 to 100 μm (more preferably 5 to 50 μm). By making the thickness of the mixed powder layer equal to or greater than the lower limit, the drainage of the finally formed water-repellent layer is improved and the power generation performance of the fuel cell tends to be improved compared to when the thickness is less than the lower limit, while by making the thickness equal to or less than the upper limit, a higher effect in terms of reducing the electronic resistance of the finally formed water-repellent layer is obtained and the power generation performance of the fuel cell tends to be improved compared to when the thickness exceeds the upper limit.

[0038] <Consolidation process> The consolidation step according to the present invention is a step of compressing the mixed powder layer under a pressure of 0.2 to 50 MPa.

[0039] In such a consolidation step, the pressure condition when the mixed powder layer is pressed needs to be 0.2 to 50 MPa. By setting the pressure at the time of pressing to the lower limit or more, it is possible to achieve more efficient consolidation compared to the case where the pressure is less than the lower limit, and it is possible to improve the contact between carbon particles and reduce the electronic resistance, and it is possible to manufacture a structure of a desired design. On the other hand, by setting the pressure to the upper limit or less, compared to the case where the pressure exceeds the upper limit, it is possible to sufficiently prevent the destruction of the carbon fibers constituting the porous substrate, and it is possible to sufficiently maintain the characteristics of the structure during the consolidation step, so that it is possible to further improve both the bonding strength between the water-repellent layer and the porous substrate and the power generation performance of the fuel cell. In addition, since a higher effect can be obtained from the same viewpoint, the pressure condition when pressing the mixed powder layer is more preferably 0.3 to 30 MPa, further preferably 0.4 to 10 MPa, and particularly preferably 1.5 to 10 MPa.

[0040] In addition, the pressurizing time when the mixed powder layer is pressed is preferably 10 to 600 seconds (more preferably 20 to 300 seconds). By setting the pressurizing time to the lower limit or more, the contact between the carbon particles is improved and the electronic resistance can be reduced compared to the case where the pressurizing time is less than the lower limit, and the bond strength between the water-repellent layer and the porous substrate and the power generation performance of the fuel cell tend to be improved. On the other hand, by setting the pressurizing time to the upper limit or less, the destruction of the carbon fibers constituting the porous substrate can be sufficiently prevented compared to the case where the pressurizing time exceeds the upper limit, and the characteristics of the structure can be sufficiently maintained during the consolidation process, so that the bond strength between the water-repellent layer and the porous substrate and the power generation performance of the fuel cell tend to be improved.

[0041] The method of pressing the mixed powder layer is not particularly limited, and known methods can be appropriately adopted. For example, pressing methods (pressing methods) such as plate pressing and roll pressing may be adopted. The temperature conditions when pressing the mixed powder layer are not particularly limited, but from the viewpoint of energy efficiency, it is preferable to use room temperature. As a method of pressing the mixed powder layer, hot pressing, in which pressing (pressing) is performed while heating, may be adopted.

[0042] In the consolidation step, the mixed powder layer is consolidated by the above-mentioned pressure. The thickness and porosity of the mixed powder layer after consolidation are determined so that the properties of the water-repellent layer finally obtained are desired (for example, a BET specific surface area of ​​5 m 2 / g~50m 2 / g) depending on the intended design and the types of powders (A) and (B), etc. Therefore, the consolidation step can be carried out by selecting the pressing conditions within the range of 0.2 to 50 MPa and adjusting the pressing time, etc., depending on the desired design.

[0043] <Water-repellent layer forming process> The water-repellent layer forming process according to the present invention is a process in which the mixed powder layer after the compaction process is baked at a temperature 10 to 130°C lower (preferably a temperature 20 to 130°C, more preferably a temperature 30 to 130°C lower) than the decomposition temperature of the thermosetting resin (polycondensate of the raw materials: thermosetting resin obtained by polycondensing the raw materials (raw materials of the thermosetting resin) constituting the resin raw material particles in the powder (B)), to obtain a water-repellent layer for a fuel cell made of a mixed assembly of the powder of hydrophilic carbon particles (A) and a water-resistant resin (C) made of a thermosetting resin which is a polycondensate of the raw materials.

[0044] Thus, in the present invention, the mixed powder layer after the consolidation step is baked at a temperature (preferably 20 to 130°C, more preferably 30 to 130°C) lower than the decomposition temperature of the water-resistant resin (C) (the decomposition temperature of the thermosetting resin, which is a polycondensate of the raw material) (hereinafter, such a step of baking the mixed powder layer may be simply referred to as a "baking step" in some cases). Note that such a baking temperature may be appropriately set depending on the type of raw material constituting the resin raw material particles in the powder (B) and, in the case of using a substrate to be coated, the type of the substrate. For example, when the substrate to be coated is a porous substrate having at least the raw material of a thermosetting resin and / or the thermosetting resin on the surface (more preferably, when the substrate has at least the raw material of a thermosetting resin on the surface), the bonding strength tends to be higher in a relatively high temperature range within the temperature range (for example, a temperature range 10 to 70 ° C lower than the decomposition temperature). Therefore, when the porous substrate is a porous substrate having at least the raw material of a thermosetting resin and / or the thermosetting resin on the surface, and when it is necessary to use the substrate with a higher bonding strength depending on the application, a relatively high temperature range may be selected. In addition, when a certain level of bonding strength is required, the energy required for the firing process can be reduced by selecting a relatively low temperature range, and energy efficiency can be further improved. On the other hand, from the viewpoint of achieving a better balance between the improvement of the bonding strength and the improvement of the energy efficiency, it is preferable to adopt a temperature 20 to 130 ° C (more preferably 30 to 130 ° C) lower than the decomposition temperature of the water-resistant resin (C) as the firing temperature. By setting the baking temperature at or above the lower limit (a temperature 130°C lower than the decomposition temperature of the thermosetting resin), the polycondensation reaction proceeds sufficiently and the bonding strength is improved compared to when the baking temperature is below the lower limit. On the other hand, by setting the baking temperature at or below the upper limit, it is possible to impart a high bonding strength to the substrate to the obtained water-repellent layer compared to when the baking temperature exceeds the upper limit.Furthermore, when the upper limit of the baking temperature is set to a temperature 50°C lower than the decomposition temperature of the thermosetting resin, structural collapse accompanied by weight loss of the water-repellent layer due to volatilization, decomposition, etc. of carbon particles and resin can be more reliably prevented compared to the case where the upper limit is exceeded, and a higher level of bonding strength to the substrate can be imparted to the obtained water-repellent layer (a decrease in bonding strength associated with structural collapse can be prevented, and a high level of bonding strength can be maintained). Furthermore, since a higher effect can be obtained from the same viewpoint, it is more preferable that the baking temperature is set to a temperature 50 to 110°C (more preferably 50 to 90°C, particularly preferably 50 to 70°C) lower than the decomposition temperature of the thermosetting resin.

[0045] In addition, regarding the "decomposition temperature of the water-resistant resin (C)" mentioned here, when the water-resistant resin (C) is made of only one type of resin, the decomposition temperature is measured by a known thermal analyzer (for example, "Thermoplus" manufactured by Rigaku Corporation). A TG curve is obtained by measuring the thermogravimetric change at a heating rate of 1° C. / min using a thermogravimetric analyzer (such as "Thermoplus TG8120") at a heating rate of 1° C. / min., and then, from the obtained TG curve, the temperature at which the resin raw material would have sufficiently polycondensed (reacted) or higher is determined as the decomposition temperature, within a temperature range above the temperature at which the resin raw material would have sufficiently polycondensed (reacted) (for example, referring to FIG. 4 (a graph showing the TG curve and DTA curve of the powder of the resin raw material particles of the melamine resin used in the examples) described later, in FIG. 4, the temperature at which the weight loss changes from abrupt to gradual weight loss occurs). In addition, when the water-resistant resin (C) is a composite (composite resin) of two or more resins or a copolymer of two or more resins (obtained by using a mixed powder of multiple resin raw materials), the mixed powder of multiple resin raw materials constituting the water-resistant resin (C) is subjected to a thermal analysis using a known thermal analyzer (for example, a thermoplus TG8120, a product of Rigaku Corporation). A TG curve is obtained by measuring the thermogravimetric change at a heating rate of 1°C / min using a thermogravimetric analyzer (such as "TG8120"), and then, from the obtained TG curve, an inflection point at which the weight loss changes from a rapid one to a gradual one in a temperature range equal to or higher than the temperature at which the mixture of raw materials would have sufficiently polycondensed (reacted) is obtained, and the temperature at the inflection point is adopted as the decomposition temperature.

[0046] In addition, in the firing step, when firing the mixed powder layer formed on the surface of the substrate to be coated, if the substrate to be coated is a "porous substrate having at least one raw material of a thermosetting resin and / or at least one resin of a thermosetting resin on its surface", the bonding strength between the water-repellent layer and the porous substrate can be made higher in a wide temperature range. Therefore, it is preferable to set the firing temperature at 10 to 130°C (more preferably 40 to 120°C, even more preferably 50 to 110°C) lower than the decomposition temperature of the water-resistant resin (C). On the other hand, if the substrate to be coated is a porous substrate other than a "porous substrate having at least a raw material of a thermosetting resin and / or a thermosetting resin on its surface" (more preferably a porous substrate having at least a thermoplastic resin (PTFE, etc.) on its surface), it is preferable to set the firing temperature at 50 to 110°C (more preferably 50 to 90°C, even more preferably 50 to 70°C) lower than the decomposition temperature of the water-resistant resin (C).

[0047] The thermosetting resin (water-resistant resin (C)) which is a polycondensate of the raw materials obtained by such baking is preferably at least one selected from the group consisting of phenolic resin, silicone resin, polyurethane resin, urea resin, melamine resin, and acrylic resin, more preferably melamine resin or a composite resin of melamine resin and acrylic resin, and among them, melamine resin is particularly preferred from the viewpoint of obtaining a higher effect in terms of energy efficiency during production, and a composite resin of melamine resin and acrylic resin is particularly preferred from the viewpoint of obtaining a higher effect in terms of bonding strength. In the baking step, the temperature rise rate when heating from room temperature to the baking temperature is not particularly limited, but is preferably 1 to 100°C / min (more preferably 1 to 50°C / min) from the viewpoint of more fully maintaining the shape of the resin raw material particles constituting the powder (B). That is, when the temperature is raised to the firing temperature at such a heating rate, even if the raw material melts once, the reaction can be made to proceed more efficiently during firing and solidified, and this tends to form a polycondensation product while more fully maintaining the shape of the particles in the powder (B).

[0048] In addition, the baking time in the baking step may be adjusted appropriately according to the type of thermosetting resin formed after baking and the baking temperature set so that the polycondensation reaction of the raw materials in the mixed powder layer can be sufficiently advanced and the resulting polycondensate can be imparted with water resistance. Although not particularly limited, the baking time is preferably 1 to 120 minutes, and more preferably 1 to 60 minutes. By setting the baking time to the lower limit or more, the polycondensation reaction can be sufficiently advanced compared to the case where the baking time is less than the lower limit, so that the bonding strength tends to be improved. On the other hand, by setting the baking time to the upper limit or less, it is possible to further improve the energy efficiency during the production of the water-repellent layer compared to the case where the baking time exceeds the upper limit.

[0049] In addition, in such a firing step, the gas atmosphere during firing is not particularly limited, and may be an oxidizing gas atmosphere containing oxygen or an inert gas atmosphere such as nitrogen, but from the viewpoint of reducing costs and improving workability, it is more preferable to use air. In such a firing step, the pressure conditions during firing are not particularly limited, but from the viewpoint of reducing costs and improving workability, it is preferable to use atmospheric pressure (normal pressure). The heating means used in such firing is not particularly limited, and known heating means can be appropriately used, for example, a heating furnace such as a hot air furnace or an electric furnace may be used.

[0050] By carrying out such a firing process, the mixed powder layer after the consolidation process is fired, and the thermosetting resin raw material in the resin raw material particles in the mixed powder layer is polycondensed, making it possible to form a layer (layer imparted with water resistance) consisting of a mixed bond of the powder (A) and the water-resistant resin (C) consisting of the thermosetting resin which is a polycondensation product of the raw material. In addition, when the resin raw material coated carbon particles are used, it can be said that the carbon particles and the resin raw material are originally composited in the state of the mixed powder layer, so it is clear that the water-repellent layer obtained by carrying out the firing process is a layer consisting of a mixed bond in which the powder (A) and the water-resistant resin (C) are bonded to each other. In addition, since the layer consisting of the mixed bond formed in this way contains the water-resistant resin, the layer is imparted with water resistance.

[0051] In this way, the water-repellent layer obtained by carrying out the baking process is a layer formed from a mixed bond of the powder (A) and the water-resistant resin (C). Here, the average particle diameter of the constituent particles of the powder (A) in the water-repellent layer is the same as that of the powder (A) in the mixed powder used as a material. The water-resistant resin (C) is made of a thermosetting resin obtained by baking and polycondensing the raw material (thermosetting resin raw material) in each particle constituting the powder (B) used in its production. Depending on the type of raw material, even if it is melted once and then solidified again in the polycondensation process, it is possible to polycondense while maintaining the dispersion state of the powder (A) in the mixed bond after compaction, so that the powder (A) and powder (B) are basically polymerized without causing a large change in the dispersion state before and after the polycondensation. In this way, when polymerization is carried out without causing a large change in the dispersion state of the resin, even if some particles are bonded to adjacent particles, there is no large change in the dispersion state or the average particle diameter, and the shape tends to be basically maintained. In this way, when the water-resistant resin (C) in the water-repellent layer sufficiently maintains the particle shape and dispersion state of the raw material, the average particle size can be almost the same as the average particle size of the powder (B) in the mixed powder. Therefore, when the water-resistant resin (C) in the water-repellent layer sufficiently maintains the particle shape and dispersion state of the raw material (when it is particulate), the average particle size of the powder (C) is preferably 0.01 to 50 μm (more preferably 0.01 to 40 μm, and even more preferably 0.01 to 30 μm). By setting the average particle size to the upper limit or less, the dispersibility of the powder (C) is further improved compared to when the average particle size exceeds the upper limit, and the power generation performance of the fuel cell using the obtained water-repellent layer can be further improved. The average particle size of such powder (C) can be measured by measuring the particle size of 500 particles randomly selected by a particle size distribution measuring device or an electron microscope and calculating the average.

[0052] The water-repellent layer obtained by the firing process is formed from a mixed bond in which the powder (A) and the water-resistant resin (C) are bonded together. In addition, since the water-repellent layer is formed in this manner, the present invention can also be said to be a method for forming a water-repellent layer by using the raw material of the thermosetting resin constituting the powder (B) as the raw material of the binding resin.

[0053] By forming the water-repellent layer in this manner, for example, when a porous substrate for a gas diffusion layer is used as the substrate during film formation (when a mixed powder layer is formed on the substrate, and a water-repellent layer is finally formed on the substrate), the resulting laminate of the substrate and the water-repellent layer can be used as is as a gas diffusion layer for a fuel cell. When a substrate on which a film is to be formed is used in the film formation process, and the substrate is a "porous substrate having at least one type of raw material of a resin constituting a thermosetting resin on its surface," the raw material on the substrate on which the film is to be formed is also polycondensed at the same time in the firing process, and the substrate after firing becomes a porous substrate having at least a thermosetting resin, which is a polycondensate of the raw material, on its surface. Therefore, when a "porous substrate having at least one raw material of the resin constituting the thermosetting resin and / or at least one of the resins constituting the thermosetting resin on its surface" is used as the substrate to be coated, the substrate in the laminate (a laminate of the substrate and the water-repellent layer) obtained after firing will be a "porous substrate having at least one of the resins constituting the thermosetting resin on its surface (for example, when the resin on the surface is of one type, the substrate will be a porous substrate having at least that one type of thermosetting resin (e.g., melamine resin) on its surface)."

[0054] In addition, the thickness of the obtained water-repellent layer is not particularly limited, but is preferably 5 to 100 μm (more preferably 5 to 50 μm). By making the thickness of such a water-repellent layer equal to or greater than the lower limit, the water-repellent layer can be sandwiched more reliably between the catalyst layer and the substrate, compared to a thickness below the lower limit, so that the bonding strength of the water-repellent layer tends to be improved, and the power generation performance tends to be improved by reducing the electronic resistance. On the other hand, by making the thickness equal to or less than the upper limit, the power generation performance tends to be improved by reducing the electronic resistance, compared to a thickness exceeding the upper limit.

[0055] In addition, in the method for producing a water-repellent layer for a fuel cell of the present invention, the obtained water-repellent layer can be the same as the water-repellent layer for a fuel cell of the present invention described below, and can be a layer made of a fired product of the mixed powder, a layer made of a mixed assembly of the hydrophilic carbon particle powder (A) and the water-resistant resin (C), and the content of the water-resistant resin (C) in the mixed assembly is 13 to 57 mass% with respect to the total amount of the powders (A) and (C). Therefore, the method for producing a water-repellent layer for a fuel cell of the present invention can be suitably adopted as a method for producing a water-repellent layer for a fuel cell of the present invention described below.

[0056] [Water-repellent layer for fuel cells] The water-repellent layer for a fuel cell of the present invention is a layer made of a sintered product of a mixed powder, the layer comprising: a powder (A) of hydrophilic carbon particles having an average particle size of 0.002 to 50 μm; and a powder (B) of resin raw material particles made of a thermosetting resin raw material having an average particle size of 0.01 to 50 μm, the powder (B) having a content of 15 to 60 mass% based on the total amount of the powders (A) and (B); The layer is a layer made of a mixed bond of the hydrophilic carbon particle powder (A) and a water-resistant resin (C) made of a thermosetting resin which is a polycondensation product of the raw materials, and The content of the water-resistant resin (C) in the mixed bonded body is 13 to 57% by mass based on the total amount of the powder (A) and the water-resistant resin (C).

[0057] In the present invention, the components in the mixed composite constituting the water-repellent layer for a fuel cell, namely, "powder of hydrophilic carbon particles (A) having an average particle size of 0.02 to 50 μm," "powder of resin raw material particles (B) made of a thermosetting resin raw material and having an average particle size of 0.01 to 50 μm," "mixed powder," "water-resistant resin (C)," and "mixed composite," are each the same as those explained in the above-mentioned "Method for manufacturing a water-repellent layer for a fuel cell of the present invention" (the preferred conditions, etc. are also the same).

[0058] In the present invention, the water-repellent layer for a fuel cell is a layer made of the sintered product of the mixed powder. Therefore, the layer is made of the mixed conjugate. In the mixed conjugate, the powder (A) and the water-resistant resin (C) are bonded to each other. The sintered product of the mixed powder and the bonded state of the components in the mixed conjugate can be efficiently formed by adopting the above-mentioned "method for manufacturing a water-repellent layer for a fuel cell of the present invention". Therefore, the water-repellent layer for a fuel cell of the present invention is preferably obtained by the above-mentioned "method for manufacturing a water-repellent layer for a fuel cell of the present invention" (for example, the sintered product of the mixed powder is preferably obtained by carrying out the sintering process explained in the above-mentioned "method for manufacturing a water-repellent layer for a fuel cell of the present invention").

[0059] In the water-repellent layer (mixed composite layer) for fuel cells according to the present invention, the content of the water-resistant resin (C) in the mixed composite is 13 to 57% by mass (more preferably 13 to 47% by mass, and even more preferably 22 to 31% by mass) based on the total amount of the powder (A) and the water-resistant resin (C). By setting the content of the water-resistant resin (C) to be equal to or greater than the lower limit, it is possible to improve the bonding strength of the water-repellent layer to various substrates and the like compared to when the content is less than the lower limit. On the other hand, by setting the content of the water-resistant resin (C) to be equal to or less than the upper limit, it is possible to make the bonding strength higher compared to when the content exceeds the upper limit, and it is possible to form a more convenient water-repellent layer without increasing the electronic resistance of the water-repellent layer to such an extent that it becomes difficult to use the water-repellent layer for fuel cell applications. When the "method of manufacturing a water-repellent layer for a fuel cell of the present invention" is adopted, the mixed powder used as the material for the water-repellent layer has a content of the powder (B) of 15 to 60 mass% relative to the total amount of the powders (A) and (B). By using such a mixed powder, when the thermosetting resin is polycondensed and cured in the baking step, the reaction proceeds accompanied by the elimination of compounds such as water due to a condensation reaction. Therefore, in the water-repellent layer obtained by the baking step, the content of the powder (C) in the mixed assembly can be easily adjusted to 13 to 57 mass% depending on the type of the thermosetting resin.

[0060] The thickness of such a water-repellent layer for a fuel cell is not particularly limited, but it is preferable that the thickness is the same as the thickness of the water-repellent layer described in the above "Method for producing a water-repellent layer for a fuel cell of the present invention." In addition, such a water-repellent layer for a fuel cell has a BET specific surface area of ​​5 m 2 / g~100m 2 / g (preferably 10 to 50 m 2 By setting the BET specific surface area to be equal to or greater than the lower limit, gas diffusibility is improved and power generation performance can be further improved compared to when the BET specific surface area is below the lower limit, while by setting the BET specific surface area to be equal to or less than the upper limit, the strength of the structure is increased and the bonding strength can be further improved compared to when the BET specific surface area exceeds the upper limit.

[0061] In addition, such a water-repellent layer for a fuel cell has a pore volume of 0.01 to 0.2 cm 2 / g (more preferably 0.01 to 0.1 cm 2 By making the pore volume equal to or greater than the lower limit, gas diffusibility is improved and power generation performance can be further improved compared to when the pore volume is below the lower limit, while by making the pore volume equal to or less than the upper limit, the strength of the structure can be increased and the bonding strength can be further improved compared to when the pore volume exceeds the upper limit.

[0062] The BET specific surface area and pore volume of the water-repellent layer for the fuel cell can be obtained by the following method. That is, first, the water-repellent layer for the fuel cell to be measured is cooled to the liquid nitrogen temperature (-196°C), nitrogen gas is introduced at a predetermined pressure, and the nitrogen adsorption amount at the equilibrium pressure is obtained by a constant volume gas adsorption method or a gravimetric method. Next, the pressure of the introduced nitrogen gas is gradually increased, and the nitrogen adsorption amount at each equilibrium pressure is obtained. Next, a nitrogen adsorption isotherm is obtained by plotting the obtained nitrogen adsorption amount against the equilibrium pressure. Thereafter, the specific surface area of ​​the gas diffusion layer for the fuel cell is obtained from the obtained nitrogen adsorption isotherm by the BET isothermal adsorption formula. In addition, the pore volume of the gas diffusion layer for the fuel cell is obtained by calculating from the nitrogen adsorption amount at P (adsorption equilibrium pressure) / P0 (saturated vapor pressure) = 0.95 of the nitrogen adsorption isotherm. In addition, when the water-repellent layer for the fuel cell to be measured is in a state of being laminated on a porous substrate or the like, the water-repellent layer may be scraped off from the laminate and used as a measurement sample to measure the BET specific surface area and pore volume.

[0063] The water-repellent layer for a fuel cell of the present invention has been described above. Hereinafter, the gas diffusion layer for a fuel cell of the present invention, which includes such a water-repellent layer for a fuel cell of the present invention, will be described.

[0064] [Gas diffusion layer for fuel cells] The gas diffusion layer for a fuel cell of the present invention is characterized by comprising a porous substrate and the water-repellent layer for a fuel cell of the present invention laminated on the surface of the porous substrate.

[0065] Such a porous substrate may be any substrate that can be used for a gas diffusion layer for a fuel cell, and is not particularly limited, and examples thereof include carbon paper, carbon cloth, etc. As such a porous substrate, it is preferable that the substrate is a porous substrate having at least one of the resins constituting the thermosetting resin (similar to the thermosetting resin described in the water-repellent layer for a fuel cell of the present invention) on its surface, since it is possible to increase the bonding strength between the water-repellent layer and the porous substrate (for example, carbon paper having at least one of the resins constituting the thermosetting resin on its surface). As such a thermosetting resin, the same as the "thermosetting resin" described as the water-resistant resin (C) can be appropriately used. For example, since it is possible to increase the bonding strength between the porous substrate and the water-repellent layer, a suitable example is to make at least one type of resin constituting the thermosetting resin of the water-resistant resin (C) constituting the water-repellent layer the same as at least one type of thermosetting resin possessed by the porous substrate (for example, when the water-resistant resin (C) is made of a melamine resin, or when the water-resistant resin (C) in the water-repellent layer is made of a composite of melamine resin and acrylic resin, at least one type of resin constituting the thermosetting resin possessed by the porous substrate on the surface is made of melamine resin (the thermosetting resin possessed by the porous substrate on the surface is made of melamine resin). In addition, when the porous substrate is a porous substrate having at least one type of resin constituting the thermosetting resin on the surface, it is particularly preferable that the thermosetting resin is a melamine resin. That is, as the porous substrate, a porous substrate having a melamine resin on the surface is particularly preferable. In addition, when the substrate to be coated is a porous substrate having at least one of the resins constituting the thermosetting resin on its surface (for example, when the thermosetting resin of the water-resistant resin (C) constituting the water-repellent layer is a composite resin of melamine resin and acrylic resin, carbon paper having melamine resin on its surface, which is one of the resins constituting the composite resin), the content of the thermosetting resin is preferably 13 to 23 mass% (more preferably 12 to 21 mass%) with respect to the total amount of the porous substrate having at least one of the resins constituting the thermosetting resin on its surface (total amount of substrate).

[0066] The thickness of such a porous substrate is not particularly limited, and may be appropriately changed within a range that can be used in a fuel cell, for example, may be 100 to 300 μm. The "water-repellent layer for fuel cells" laminated on the surface of the porous substrate is the water-repellent layer for fuel cells of the present invention (preferable conditions (e.g., film thickness, etc.) are also the same). The "water-repellent layer for fuel cells" laminated on the surface of such a porous substrate can be easily formed by carrying out the film formation process on the porous substrate by employing the manufacturing method for the water-repellent layer for fuel cells of the present invention described above.

[0067] The gas diffusion layer for a fuel cell of the present invention may be any one that includes a porous substrate and the water-repellent layer for a fuel cell of the present invention laminated on the surface of the porous substrate, and other configurations (e.g., conditions of BET specific surface area, etc.) are not particularly limited. Such a gas diffusion layer for a fuel cell of the present invention can be suitably applied to a gas diffusion layer used in an electrode of a fuel cell, for example. EXAMPLES

[0068] The present invention will be described in more detail below based on examples and comparative examples, but the present invention is not limited to the following examples.

[0069] [Ingredients used in each example] The types of carbon particles (hereinafter, sometimes simply referred to as "CB particles") and the types of raw material resins used in each example are described below. The types of CB particles used in each example are shown in Table 1.

[0070] About CB particles Hydrophilic carbon particles (manufactured by Nishimura Graphite Co., Ltd., product name: hydrophilic graphite MC2, average primary particle size: 46 nm (0.046 μm), in Tables 1 to 2 and Tables 4 to 7, such a type of CB particles is simply referred to as "hydrophilic") Hydrophobic carbon particles (manufactured by Denka Company, product name: Denka Black Li400, average primary particle diameter: 48 nm (0.048 μm), in Tables 1 to 2 and Tables 4 to 7, such a type of CB particles is simply referred to as "hydrophobic").

[0071] The properties of the CB particles, such as "hydrophilicity" or "hydrophobicity," were evaluated by the so-called Methanol Wettability method (see Mitsuru Ochiai, Aerosol Research, vol. 5, 1990, pp. 32-43). Specifically, methanol aqueous solutions with different methanol concentrations or water (methanol concentration: 0% by mass) were prepared, and the CB particles used in each example were gently added to the water or each aqueous solution to confirm whether the CB particles were dispersed or not, and the methanol concentration at which the CB particles were dispersed was determined (to confirm dispersibility in water or aqueous solution) (the properties of hydrophilicity or hydrophobicity were evaluated using the methanol concentration (% by mass) required to completely wet the CB particles floating on the water or solution surface as a scale. Note that the lower the value of the methanol concentration at which the CB particles are dispersed, the higher the hydrophilicity). In the evaluation, when the methanol concentration in the aqueous solution in which the CB particles are dispersed is less than 2% by mass (Methanol Wettability: <2), the CB particles are evaluated as “hydrophilic” particles, and when the CB particles are not dispersed in an aqueous solution of methanol with a concentration of less than 2% by mass, but are dispersed in an aqueous solution of methanol with a concentration of 2% by mass or more (Methanol Wettability: 2≦), the CB particles are evaluated as “hydrophobic” particles. When such an evaluation method was adopted, the aforementioned “hydrophilic carbon particles” were dispersed in water with a methanol concentration of 0% by mass. On the other hand, the aforementioned “hydrophobic carbon particles” were not dispersed in an aqueous solution of methanol with a concentration of less than 2% by mass, but were dispersed in an aqueous solution of methanol with a concentration of 2% by mass. As a result of such evaluation, photographs showing the state when the aforementioned hydrophilic carbon particles and the aforementioned hydrophobic carbon particles were added to water (methanol concentration: 0% by mass) are shown in FIG. 1. The left side of the photograph in FIG. 1 is a photograph when the hydrophilic carbon particles are added to water, and it can be confirmed that the hydrophilic carbon particles are dispersed in water. In contrast, the photograph on the right side of Figure 1 shows what happens when hydrophobic carbon particles are added to water, and in this case, it can be seen that the particles float on the water and are not dispersed at all in the water.

[0072] <About resin raw material particles> Low condensation product of methylol melamine (raw material for melamine resin (melamine resin having amino group, imino group, methylol group, and alkyl ether group), manufactured by Nippon Carbide Industries Co., Ltd., product name "Nikaresin S260", average primary particle size: 20 μm, decomposition temperature of resin (melamine resin) after polycondensation: 280°C) PTFE (Kitamura Co., Ltd., product name: KTL-500F, average primary particle size: 0.2 μm, decomposition temperature: 500 to 600°C) Methylated melamine (raw material for thermosetting resin constituting the water-repellent layer (melamine resin having amino group, imino group, methylol group, and alkyl ether group), manufactured by Nippon Carbide Industries Co., Ltd., product name "Nicalac MX035"; in Examples 16 to 22, CB particles (hydrophilic) were dispersed in the product (aqueous solution), and then dried to obtain particles (carbon particles coated with resin raw material) in which the CB particles were coated with methylated melamine.) Acrylic resin (raw material for the thermosetting resin that constitutes the water-repellent layer, manufactured by Nippon Carbide Industries Co., Ltd., product name "Nikasol RX1033", in Examples 16 to 22, the dried product (aggregate of primary particles) was pulverized with a mixer and used, the average primary particle diameter of the acrylic resin obtained in each Example: 0.1 μm, the average secondary particle diameter: 30 μm or less).

[0073] [Examples and Comparative Examples in which "carbon paper having PTFE on the surface" is used as the porous substrate of the laminate for the gas diffusion layer] (Examples 1 to 11 and Comparative Examples 1 to 2) The CB particles of the type shown in Table 1 and the resin raw material particles (low condensation product of methylol melamine) of the type shown in Table 1 were mixed in the compounding ratio (compounding ratio based on mass) shown in Table 1 with a mixer (manufactured by Tescom Denki Co., Ltd., product name: OML-2) at 20,000 revolutions for 5 minutes to obtain a mixed powder. Next, the obtained mixed powder was applied to the surface of a porous substrate, carbon paper (carbon paper having PTFE on the surface (hereinafter, for convenience, sometimes referred to as "PTFE-treated product"), manufactured by Chemix, product name: TGP-H-060H, PTFE: 5 mass%, film thickness: about 200 μm), to form a film by electrostatic screen printing (dry film formation method), to form a layer of the mixed powder. The electrostatic screen printing method used was to use an electrostatic screen printing device (manufactured by Berg Kogyo, product name: T-1) and a screen mesh (manufactured by Berg Kogyo, product name: electrostatic screen plate), and with a voltage of 16 kV applied between the carbon paper and the screen mesh, the mixed powder was placed on the screen mesh and rubbed with a squeegee, causing the mixed powder to fall from the mesh onto the carbon paper, forming a film.

[0074] Next, the layer of the mixed powder laminated on the surface of the carbon paper (carbon paper having PTFE on the surface) was compressed by pressing at 3 MPa for 1 minute using a flat press. Then, the layer of the mixed powder after such compression was heated and baked using an electric furnace under the conditions of pressure: normal pressure, heating temperature: temperature shown in Table 1, and time: 30 minutes (the temperature was raised from room temperature at a rate of 10°C per minute up to the heating temperature), thereby forming a water-repellent layer on the carbon paper, which was made of CB particles and a thermosetting resin (melamine resin) which was a polycondensate of the resin raw material (low condensation product of methylol melamine) constituting the resin raw material particles, and a laminate of the carbon paper and the water-repellent layer (a laminate for a gas diffusion layer of a fuel cell) was obtained. The mass ratio of the carbon particles in the water-repellent layer to the fired product of the resin raw material particles (resin made of a polycondensate of the resin raw material) is shown in Table 2 (in Table 2, the resin content after firing was calculated from the charge ratio (mixture ratio) of the CB particles and the raw material resin using the results of the thermogravimetric measurement described below). In addition, it is clear from the firing conditions (heating temperature and heating time) that all of the formed water-repellent layers contain melamine resin (water-resistant resin) obtained by sufficient progress of the polycondensation reaction of the resin raw material (low condensation product of methylol melamine), and therefore it is clear that the layers are water-resistant.

[0075] Comparative Example 3 Instead of the above-mentioned mixed powder, a mixed powder was used in which the type of carbon particles (CB particles) shown in Table 1 and the type of resin raw material particles (PTFE) shown in Table 1 were mixed at 20,000 rpm for 5 minutes using a mixer (manufactured by Tescom Electric Co., Ltd., product name: OML-2) so that the content ratio of the carbon particles in the water-repellent layer to the baked resin (baked PTFE) was 85 / 15 (carbon particles / baked resin particles). A water-repellent layer was formed on carbon paper using a method similar to that described in the above-mentioned "Examples 1 to 11 and Comparative Examples 1 and 2", and a laminate of carbon paper (carbon paper having PTFE on the surface) and a water-repellent layer (laminate for a gas diffusion layer of a fuel cell) was obtained.

[0076] [Table 1]

[0077] [Evaluation of properties of laminates obtained in Examples 1 to 11 and Comparative Examples 1 to 3] <Bonding strength test: Measurement of the bonding strength between the carbon paper and the water-repellent layer> Using the laminate of carbon paper and water-repellent layer obtained in each Example as a measurement sample, a 90 degree peel strength test of the water-repellent layer was performed using an electric test stand (manufactured by Imada Co., Ltd., product name: MX2-500N-L-FA) to measure the bonding strength (unit: N / m) of the water-repellent layer to the carbon paper. The obtained results are shown in Table 2 and Figure 2.

[0078] [Table 2]

[0079] As is clear from the results shown in Tables 1-2 and Fig. 2, in the laminates (laminates for gas diffusion layers of fuel cells) obtained in Examples 1-11 using carbon paper having PTFE on the surface as the porous substrate, the bonding strength of the water-repellent layer to the porous substrate was 1.38 N / m or more in all cases, even though the heating temperature (firing temperature) during firing was a relatively low temperature of 210°C or less. In contrast, in Comparative Example 3 using PTFE, which is the resin raw material particle also used in Patent Document 1, the bonding strength of the water-repellent layer to the porous substrate was 0.62 N / m, even though a high firing temperature of 350°C, which is the firing temperature employed in the examples of Patent Document 1, was used. In this way, when comparing the results in the system using carbon paper having PTFE on the surface, it was confirmed from the results shown in Tables 1 and 2 that when the water-repellent layer was produced under the conditions adopted in each example, at least twice as much bonding strength (for example, about six times as much as Example 3) was obtained compared to the case where the water-repellent layer was produced by firing PTFE at a high firing temperature such as 350 ° C. (Comparative Example 3). From these results, it was found that according to the present invention, a relatively low temperature can be used as the heating temperature in the firing step, and it is possible to lower the firing temperature (heat treatment temperature) (for example, it is possible to lower the temperature by 150 ° C. compared to Example 3 and Comparative Example 3), and therefore it is possible to efficiently produce a water-repellent layer with higher energy efficiency, and it was also found that when a water-repellent layer is formed on the surface of a porous substrate (carbon paper having PTFE on the surface) for a gas diffusion layer, it is possible to make the bonding strength between the water-repellent layer and the porous substrate higher than the conventional technology described in Patent Document 1.

[0080] In addition, when comparing the results among Examples 1 to 11 in which carbon paper having PTFE on the surface was used as a porous substrate, it was confirmed that the bonding strength changed depending on the baking temperature when comparing Examples having the same raw material charge amount (charge ratio). When a low condensate of methylolmelamine (a raw material for melamine resin) was used as the resin raw material particle, it was also found that the bonding strength was maximized when the baking temperature was 200°C, as in Examples 3 and 7. In addition, considering the relationship between the baking temperature and the bonding temperature from the results shown in Tables 1 to 2 and FIG. 2, it can be understood that in the system (Examples 1 to 11) in which carbon paper having PTFE on the surface (manufactured by Chemix, product name: TGP-H-060H) was used as a porous substrate, if the baking temperature was set within a range of 50 to 110°C lower than the decomposition temperature of melamine resin (280°C), a sufficiently high bonding strength can be obtained more reliably.

[0081] 2, it is also clear that a sufficiently high level of bonding strength can be obtained when the content of the resin raw material particles is in the range of 15 to 60 mass% with respect to the total amount of the CB particles and the resin raw material particles, when Examples 1 to 11 are compared with Comparative Example 1. In addition, when the firing temperature is 200°C (Examples 3, 7, and 9 to 11), the bonding strength is extremely high when the content of the resin raw material particles is 30 mass% with respect to the total amount of the CB particles and the resin raw material particles (Example 7), and it is also found that a higher effect can be obtained when the content of the resin raw material particles in the mixed powder is around 30 mass%.

[0082] Furthermore, from the results shown in Tables 1 and 2 and FIG. 2, it was also found that when focusing on the type of carbon particles, the bonding strength was 0 when hydrophobic carbon particles were used (Comparative Example 2), and therefore the bonding strength of the resulting water-repellent layer was further improved by using hydrophilic carbon particles.

[0083] <Measurement of BET specific surface area and pore volume of water-repellent layer> Only the water-repellent layer was scraped off from the laminate of carbon paper and water-repellent layer obtained in Example 3 to prepare a measurement sample, and the nitrogen adsorption amount at equilibrium pressure was determined for the measurement sample by a constant volume gas adsorption method at liquid nitrogen temperature (-196°C) using a specific surface area / pore distribution measurement device (manufactured by Quantachrome, product name: Autosorb-1) to obtain a nitrogen adsorption isotherm.The specific surface area was calculated from the nitrogen adsorption isotherm using the BET isotherm, and the pore volume was calculated from the nitrogen adsorption amount at P (adsorption equilibrium pressure) / P0 (saturated vapor pressure) = 0.95 on the nitrogen adsorption isotherm.The results are shown in Table 3.

[0084] [Table 3]

[0085] The results shown in Table 3 indicate that the pores in the gaps between the CB particles in the water-repellent layer are not blocked by the polycondensate (thermosetting resin: melamine resin) of the raw material (low condensation product of methylol melamine) (they are not blocked by the adhesion of the polycondensate).

[0086] <Considerations on resin raw material particles> Observation of changes in state of resin raw material particles due to heating temperature A powder of resin raw material particles identical to the resin raw material particles of melamine resin used in manufacturing the water-repellent layer in Example 1 was used, and the resin raw material particles were heated from room temperature to 400°C at a temperature increase rate of 1°C per minute. The appearance of the powder was photographed when heating began (room temperature) and when it reached each of the thermal temperatures (baking temperatures) of 100°C, 200°C, 300°C, and 400°C, and the shape and color were observed. The photographs obtained are shown in Figure 3.

[0087] <Thermogravimetry (TG) and differential thermal analysis (DTA) of resin raw material particles> Using the same resin raw material particles (melamine resin raw material) as those used in the production of the water-repellent layer in Example 1, the thermogravimetric change of the melamine resin raw material constituting the resin raw material particles was measured at a temperature rise rate of 1°C / min using a thermal analyzer (manufactured by Rigaku Corporation, product name: Thermoplus TG8120) to obtain a TG curve. In addition, differential thermal analysis (DTA) of the melamine resin raw material was performed under the same conditions using the thermal analyzer to obtain a DTA curve. The thermogravimetric change measurement results (TG curve) and the differential thermal analysis results (DTA curve) are shown in Figure 4.

[0088] <Measurement results of resin raw material particles> From the results shown in Fig. 3, when the resin raw material particles were baked at the same temperature of 200°C, which was the baking temperature at which the water-repellent layer in the above example showed high bonding strength, traces of foaming could be confirmed from the external photograph of the resin raw material particles, and it is believed that dehydration occurred due to polycondensation. Furthermore, as shown in Fig. 3, it can also be seen that the resin raw material particles used were melted once at 100°C.

[0089] In addition, from the results shown in FIG. 4, it can be seen that a rapid weight loss occurs from about 250°C in the TG curve (FIG. 4), but when heated at a temperature rise rate of 1°C / min, it can be understood that thermal decomposition occurs in the region above about 250°C. On the other hand, when heated at a temperature rise rate of 1°C / min, it can be considered that the polycondensation reaction has progressed sufficiently by heating to a temperature of about 250°C, at which the powder of the resin raw material particles serving as the sample undergoes a rapid weight loss. Therefore, the proportion of the mass lost due to the reaction (weight loss rate) was calculated from the amount of mass lost between the temperature (100°C) at which the condensation reaction begins to proceed and the temperature (250°C) at which the rapid weight loss occurs in the TG curve (FIG. 4), and the weight loss rate due to the reaction was found to be about 12.5% ​​by mass. Considering the results shown in Figures 3 and 4, the mass reduction of the resin raw material (low condensation product of methylol melamine) is considered to be due to water molecules generated by polycondensation, and is considered to be equivalent to two water molecules generated by polycondensation. From this viewpoint, the above-mentioned weight reduction rate is calculated assuming that it is equivalent to the mass ratio of the resin raw material particles reduced in the baking process in each example, and the resin content after baking contained in the water-repellent layer manufactured in each example can be obtained. In the above examples, the resin content after baking (13 to 57% by mass) shown in Table 2 is obtained based on the amount of resin raw material particles charged (15 to 60% by mass) and the weight reduction rate obtained from the TG curve shown in Figure 4. In the TG curve shown in FIG. 4, a reduction in mass is confirmed even in the temperature region lower than the temperature (100° C.) at which the condensation reaction begins to proceed. However, this is thought to be due to moisture absorbed in the air and is thought to be the amount of water molecules that are not involved in the condensation reaction. Therefore, this amount does not have a significant effect on the change in mass before and after baking and can be ignored in calculating the mass of the resin after baking. Therefore, the amount of the resin after baking is calculated using the weight loss rate.

[0090] Also, referring to Table 2, in a system using carbon paper having PTFE on the surface as a porous substrate, the bonding strength of the water-repellent layer is lower when the water-repellent layer is produced by baking at 210°C or 220°C (Examples 4 and 5) than when the water-repellent layer is produced by baking at 200°C (Example 3). Taking into consideration the results of Examples 12 to 15 described later, this is presumed to be due to the type of porous substrate and the occurrence of thermal decomposition of the melamine resin structure in a part of the water-repellent layer. In addition, the TG curve shown in Figure 4 does not show any mass change due to thermal decomposition at temperatures of 210°C or 220°C, but this is considered to be due to the fact that the TG curve was obtained when the temperature was increased at a rate of 1°C / min. Considering the relationship between such thermal decomposition and temperature, the water-repellent layers of Examples 4 and 5 listed in Table 2 were formed by firing under conditions of a heating rate of 10°C / min and a holding temperature of 210 to 220°C for 30 minutes, and the heating conditions (thermal history) are different from those in the experiment when the TG curve shown in Figure 4 was obtained. Therefore, a mass reduction that is likely due to thermal decomposition was confirmed at a position of about 250°C in Figure 4, but it is considered that thermal decomposition occurs partially even at temperatures of 210°C or 220°C due to long-term heating under actual firing conditions. On the other hand, even when the firing temperature is 220°C (Example 5), at least twice the bonding strength was obtained compared to the case where the water-repellent layer was produced by firing at a high firing temperature of 350°C using PTFE (Comparative Example 3). Considering these points, in a system using carbon paper having PTFE on the surface as the porous substrate, the upper limit of the heating temperature during baking is considered to be a temperature 50°C lower than the decomposition temperature (280°C) of the raw resin (thermosetting resin: melamine resin), taking into consideration both the viewpoint that a higher bonding strength can be more reliably obtained between the porous substrate and the water-repellent layer compared to Comparative Examples 1 to 3, etc., and the viewpoint that a sufficient improvement in energy efficiency can be achieved compared to the case where baking is performed at a high temperature of 350°C as actually adopted in the examples of Patent Document 1.

[0091] <Measurement of water-repellent layer by SEM> In order to confirm the dispersion state of the resin (melamine resin) after baking in the water-repellent layer, the surface state of the water-repellent layer of the laminate obtained in Example 7 was measured using a scanning electron microscope (SEM, Hitachi High-Tech Corporation, product name: Regulus8230). That is, using the SEM as a measuring device, an SEM image of the surface of the water-repellent layer (Example 7) was obtained under the condition of an acceleration voltage of 3 kV, and an element detector (EDS, Bruker, product name: QUANTAXFlatQUAD) was used to obtain an SEM-EDS image (element mapping image) of the portion where the SEM image was obtained. In addition, for reference, an SEM image and an SEM-EDS image of the mixed powder (before film formation) prepared in Example 7 were also obtained under the same conditions. The SEM image of the surface of the water-repellent layer (Example 7) is shown in FIG. 5, and the SEM-EDS image of the surface of the water-repellent layer (Example 7) is shown in FIG. 6. FIG. 7 shows an SEM image of the mixed powder (before film formation: Example 7), and FIG. 8 shows an SEM-EDS image.

[0092] From the SEM image shown in FIG. 5 and the EDS mapping results shown in FIG. 6, it was confirmed that the white areas in the SEM image shown in FIG. 5 are composed of melamine resin (thermosetting resin: polycondensate of resin raw material (low condensation product of methylol melamine)) (this was confirmed by the fact that in the image (FIG. 6) in which the map of N element contained in the polycondensate of the resin raw material (low condensation product of methylol melamine) is superimposed, the area where N element exists (in the color drawing, the area corresponding to N element contained in melamine resin (thermosetting resin) is orange) overlaps with the white areas in the SEM image shown in FIG. 5). From the results shown in FIG. 5 and FIG. 6, it was found that the polycondensate of the thermosetting resin raw material was dispersed throughout the water-repellent layer produced in Example 7. In addition, in Fig. 5 and Fig. 6, it is confirmed that there are some parts where the melamine resin (thermosetting resin) is in a lump form, but the dispersion state of the melamine resin (thermosetting resin) in such a water-repellent layer is formed due to the dispersion state of the resin raw material particles in the mixed powder, since the resin raw material particles already exist in a lump form in the mixed powder state before film formation can be confirmed from the results shown in Fig. 7 and Fig. 8. From these results, it was confirmed that the water-repellent layer is formed by a bonded body in which the CB particles and the melamine resin obtained after the resin raw material particles are baked are bonded in a sufficiently dispersed state. In addition, from the results shown in Figs. 5 to 8 (dispersion state of the resin raw material particles and the melamine resin (thermosetting resin) in the mixed powder shown in the figures), it can be recognized that the resin after baking has a particle shape, and its particle size is basically equivalent to the particle size of the resin raw material particles in the mixed powder, and it can be seen that there is no significant change in the shape or average particle size before and after baking.

[0093] From the evaluation results of the properties of the laminates obtained in Examples 1 to 11 and Comparative Examples 1 to 3 (evaluation results of the properties of the water-repellent layer in the laminate), etc., when carbon paper having PTFE on the surface is used as a porous substrate, a mixed powder containing a powder of hydrophilic carbon particles (A) and a powder of resin raw material particles (B) made of a thermosetting resin raw material, the content of the powder (B) being 15 to 60 mass% relative to the total amount of the powders (A) and (B), is formed on the porous substrate by a dry film formation method, and then compacted, and then baked at a temperature 50 to 110 ° C. lower than the decomposition temperature of the polycondensate of the thermosetting resin raw material (thermosetting resin formed after baking), thereby efficiently forming a water-repellent layer consisting of a mixed bond of the hydrophilic carbon particle powder (A) and the water-resistant resin (C). It was also confirmed that when a water-repellent layer is formed on the surface of a porous substrate made of carbon paper having PTFE on the surface in this way, the resulting water-repellent layer has excellent bonding strength to the porous substrate. As described above, in the method adopted in each example using a porous substrate made of carbon paper having PTFE on the surface, a water-repellent layer is formed at a relatively low baking temperature of around 200°C (180 to 220°C). Therefore, according to the present invention, it is possible to achieve sufficiently high energy efficiency during the production of a water-repellent layer.

[0094] [Examples and Comparative Examples in which "carbon paper having melamine resin on the surface" is used as the porous substrate of the laminate for the gas diffusion layer] (Examples 12 to 15) <Preparation process of carbon paper (porous substrate) having melamine resin raw material on the surface> First, a low condensate of methylol melamine (a raw material for melamine resin, manufactured by Nippon Carbide Industries Co., Ltd., trade name "Nikaresin S260", average particle size: 20 μm, decomposition temperature: 280 ° C.) was dissolved in water to obtain an aqueous solution with a methylol melamine content of 30% by mass. Next, carbon paper (manufactured by Chemix, trade name: TGP-H-060, a product not treated with resins such as PTFE) was immersed in the aqueous solution for 5 minutes, then removed, air-dried for several hours, and vacuum-dried by leaving it to stand for 12 hours under vacuum conditions (pressure of 10 Pa or less) at a temperature condition of 25 ° C. to obtain carbon paper having a raw material for melamine resin (low condensate of methylol melamine) on its surface (a surface-treated product with raw material for melamine resin: a content of raw material for melamine resin of 20% by mass relative to the total amount of the porous substrate).

[0095] <Preparation process of laminate for gas diffusion layer of fuel cell> The type of carbon paper, which is a porous substrate used as a substrate to be coated, was changed from carbon paper having PTFE on its surface (PTFE-treated product, manufactured by Chemix, product name: TGP-H-060H) to "carbon paper having melamine resin raw material on its surface (surface-treated product with melamine resin raw material)" obtained by the preparation process described above, the types and compounding ratios of the CB particles and resin raw material particles were changed as shown in Table 4, and the firing temperature shown in Table 4 was adopted. Except for this, a laminate of carbon paper (carbon paper having melamine resin on its surface) and a water-repellent layer (laminate for a gas diffusion layer of a fuel cell) was obtained in the same manner as in Example 1.

[0096] In addition, it is clear that the water-repellent layers formed in Examples 12 to 15 contain melamine resin (water-resistant resin) obtained by sufficient polycondensation reaction of the resin raw material (low condensation product of methylol melamine) from the adopted baking conditions (heating temperature and heating time), and therefore it is clear that they are layers having water resistance. In addition, considering the above-mentioned baking conditions (heating temperature and heating time), it is also clear that the polycondensation reaction of the melamine resin raw material (low condensation product of methylol melamine) present on the surface of the carbon paper (film-forming substrate) has sufficiently progressed, and the porous substrate (porous substrate of the laminate) after baking is carbon paper having melamine resin on the surface.

[0097] Comparative Example 4 A laminate (laminate for a gas diffusion layer of a fuel cell) of carbon paper (carbon paper having melamine resin on its surface) and a water-repellent layer was obtained in the same manner as in Example 12, except that the type of resin raw material particles (PTFE) shown in Table 4 was used and the amount of CB particles and resin raw material particles used was changed so that the content ratio (carbon particles / resin particles after baking) of the carbon particles in the water-repellent layer and the baked resin (baked PTFE) was 70 / 30.

[0098] Comparative Example 5 A laminate of carbon paper (carbon paper having PTFE on its surface) and a water-repellent layer (laminate for a gas diffusion layer of a fuel cell) was obtained in the same manner as in Comparative Example 3, except that the amounts of CB particles and resin raw material particles used were changed so that the content ratio (carbon particles / resin particles after baking) of the carbon particles in the water-repellent layer to the baked resin (baked PTFE) was 70 / 30.

[0099] [Table 4]

[0100] [Evaluation of properties of laminates obtained in Examples 12 to 15 and Comparative Examples 4 to 5] <Bonding strength test: Measurement of the bonding strength between the carbon paper and the water-repellent layer> The same test (90 degree peel strength test) as the "bonding strength test" conducted to evaluate the properties of the laminates obtained in Examples 1 to 11 and Comparative Examples 1 to 3 was conducted to measure the bonding strength (unit: N / m) of the water-repellent layer to the carbon paper. The obtained results are shown in Table 5.

[0101] For reference, Table 5 also shows the properties of the laminates obtained in Examples 6 to 8, in which the types and amounts of the CB particles and the resin raw material particles are the same as those in Examples 12 to 15. Table 5 also lists the values ​​(mass ratios) of "CB particles / resin after baking" for each Example, etc., but for Examples 12 to 13, the values ​​(mass ratios) were calculated from the charge ratio (compounding ratio) of the CB particles and the raw material resin by considering the baking temperature and, for convenience, referring to FIG. 4 in the same manner as in Table 2, assuming that the resin weight loss rate due to the reaction is 11.0% by mass in Example 12 and 12.5% ​​by mass in Example 13. For Examples 14 to 15, in which the baking temperature is relatively high (240°C or 260°C), the values ​​were calculated from the charge ratio (compounding ratio) of the CB particles and the raw material resin by considering the progress of thermal decomposition during baking and the like and assuming that the resin weight loss rate is 20.0% by mass in Example 14 and 21.0% by mass in Example 15. In addition, taking into consideration the relationship between the firing temperature and the amount of mass reduction of the resin shown in FIG. 4, the results shown in Table 5, and the charge ratio (mixture ratio) of the CB particles and raw resin, it is clear that the content of the resin after firing relative to the total amount of the CB particles and the resin after firing in the water-repellent layers obtained in Examples 12 to 15 was in the range of 13 to 57 mass%.

[0102] [Table 5]

[0103] As is clear from the results shown in Table 5, the laminates obtained in Examples 12 to 15 (laminates for gas diffusion layers of fuel cells) having carbon paper with melamine resin on the surface as a porous substrate have a bonding strength of 17.9 N / m or more, whereas the laminate obtained in Comparative Example 4, which has carbon paper with melamine resin on the surface as a porous substrate but uses the conventionally used PTFE (thermoplastic resin) as the resin in the water-repellent layer, has a bonding strength of 1.1 N / m, and furthermore, the laminate obtained in Comparative Example 5, in which the firing temperature was 350°C as in the conventional manufacturing method, has a bonding strength of 0.62 N / m. From these and other factors, it was found that it is possible to improve the bonding strength by using melamine resin, which is a thermosetting resin, as the resin (resin as a constituent component) for the water-repellent layer. In addition, it was also confirmed that the laminates obtained in Examples 6 to 8, which include carbon paper having PTFE on the surface as a porous substrate, in Examples 12 to 15, which include carbon paper having melamine resin on the surface as a porous substrate, have a dramatically improved bonding strength of the water-repellent layer to the porous substrate. From such a comparison between Examples 6 to 8 and Examples 12 to 15 (particularly the comparison between Example 12 and Example 6, which have the same baking temperature, or the comparison between Example 13 and Example 8, which have the same baking temperature), it was found that by using carbon paper having melamine resin on the surface as the porous substrate of the laminate, it is possible to make the bonding strength with the water-repellent layer extremely high. In addition, in Examples 6 to 8, in which the porous substrate was carbon paper having PTFE on its surface, the bonding strength was maximum when the baking temperature was 220°C, whereas in Examples 12 to 15, in which the porous substrate was carbon paper having melamine resin on its surface, the bonding strength was maximum when the baking temperature was 240°C. This shows that, in terms of the manufacturing method, the baking temperature at which the bonding strength is maximum varies depending on the type of porous substrate.In addition, when the result of the TG curve shown in FIG. 4 is taken into consideration, it seems that the decomposition of the melamine resin proceeds at 250°C or higher. However, when carbon paper having a melamine resin raw material on its surface is used as the substrate to be coated (when the porous substrate after baking becomes carbon paper having melamine resin on its surface), the bonding strength is 30.3 N / m even when the baking temperature is 260°C (Example 15), and since a very high bonding strength is achieved even at a baking temperature of 260°C, it is clear that a sufficiently high bonding strength can be obtained even when the baking temperature is 10°C lower than the decomposition temperature of the melamine resin (280°C). In addition, even at a temperature (about 270°C) 10°C lower than the decomposition temperature of the melamine resin (280°C), it can be lowered by 80°C compared to the case where the baking temperature is 350°C in the same manner as in the conventional manufacturing method, so that according to the present invention, the energy efficiency during manufacturing is sufficiently improved. Considering that the bonding strength is 33.7 N / m even in Example 13 where the baking temperature is 220°C, it is clear that in a system using carbon paper having a melamine resin raw material on the surface as a porous substrate as a substrate to be coated, a sufficiently high level of bonding strength can be obtained even at a temperature 50°C lower than the decomposition temperature of the thermosetting resin. In addition, considering the bonding strength values ​​of Examples 13 and 14 together with the results shown in Table 2, from the viewpoint of achieving a better balance between further improvement in energy efficiency and improvement in bonding strength, it can be said that it is more preferable to set the baking temperature at a temperature 40°C (more preferably 50°C) lower than the decomposition temperature of the thermosetting resin, since the lower the baking temperature, the more energy efficiency is improved.

[0104] Furthermore, considering that the bonding strength was 17.9 N / m even in Example 12, where the firing temperature was 180°C, and that the bonding strength of the laminates produced by conventional manufacturing methods (Comparative Example 3 and Comparative Example 5) was 0.62 N / m or less, it is clear that a sufficiently high level of bonding strength can be obtained even when the lower limit of the firing temperature is set to a temperature 130°C (more preferably 110°C) lower than the decomposition temperature of melamine resin (280°C).

[0105] <Check the peeling surface> Regarding the laminate obtained in Example 8 and the laminate obtained in Example 13, after the water-repellent layer was peeled off in the above-mentioned "90 degree peel strength test", the surface of the peeled surface was visually observed and the state of the peeled surface was evaluated. A photograph of the peeled surface of the laminate obtained in Example 8 after the 90 degree peel strength test is shown in Figure 9, and a photograph of the peeled surface of the laminate obtained in Example 13 after the 90 degree peel strength test is shown in Figure 10.

[0106] As is clear from the results shown in Figures 9 to 10, when the porous substrate has PTFE on its surface (Example 8), the peeling surface is mainly the interface between the water-repellent layer and the substrate, and peeling occurs at the interface. In contrast, when the same raw material (low condensation product of methylol melamine) as the raw material of the thermosetting resin used in the water-repellent layer was attached to the surface of the porous substrate as the substrate to be film-formed (Example 13), it was revealed by observation of the peeling surface that peeling of the obtained laminate occurs mainly due to cohesive failure. From these results, the inventors infer that by using a porous substrate having the same raw material (low condensation product of methylol melamine) as the raw material of the thermosetting resin used in the water-repellent layer on its surface instead of a porous substrate having PTFE on its surface as the substrate to be film-formed, the melting temperatures of the resin present on the surface of the porous substrate after firing and the resin in the water-repellent layer become close to each other, and the bonding strength at the interface between the water-repellent layer and the substrate can be further improved, thereby further improving the peel strength.

[0107] (Examples 16 to 22) <Preparation process of carbon paper (porous substrate) having melamine resin raw material on the surface> A process similar to the "process for preparing carbon paper (porous substrate) having melamine resin raw material on its surface" employed in Examples 12 to 15 was employed to obtain carbon paper having melamine resin raw material (low condensation product of methylol melamine) on its surface (surface-treated product using melamine resin raw material: content of melamine resin raw material relative to the total amount of porous substrate is 20 mass%; hereinafter, sometimes referred to as "carbon paper having melamine resin raw material on its surface").

[0108] <Preparation process of laminate for gas diffusion layer of fuel cell> The type of CB particles (hydrophilic) shown in Table 6 was dispersed in methylated melamine (manufactured by Nippon Carbide Industries Co., Ltd., product name "Nikarac MX035", colorless and transparent liquid, solvent: water) so that the mass ratio of the CB particles to the methylated melamine (CB particles / methylated melamine) was 83 / 17 in terms of solid content, and then the dispersion was dried to adhere (coat) the methylated melamine to the surfaces of the CB particles, thereby obtaining a powder of resin raw material-coated carbon particles (particles in which the CB particles are coated with methylated melamine: methylated melamine / CB composite particles).

[0109] Separately, a commercially available acrylic resin (manufactured by Nippon Carbide Industries Co., Ltd., product name "Nikasol RX1033") was prepared and dried to obtain a dried acrylic resin. The average primary particle diameter of the acrylic resin particles was determined by measuring the dried acrylic resin with a scanning electron microscope, and the average primary particle diameter of the acrylic resin was 0.1 μm. The dried acrylic resin was in the form of an aggregate of acrylic resin particles (primary particles) resembling plastic pieces.

[0110] Next, the resin raw material coated carbon particles (methylated melamine / CB composite particles) obtained as described above and the dried acrylic resin were introduced into a mixer (manufactured by Tescom Electric Co., Ltd., product name: OML-2) so that the mass ratio of the solid content of the CB particles, methylated melamine, and acrylic resin (CB particles / methylated melamine / acrylic resin) was 70 / 7.5 / 22.5, and the mixture was stirred at 20,000 revolutions for 5 minutes to mix the resin raw material coated carbon particles (methylated melamine / CB composite particles) and acrylic resin while crushing the dried acrylic resin, thereby obtaining a mixed powder of resin raw material coated carbon particles and acrylic resin particles (note that the resin raw material coated carbon particles are regarded as particles of methylated melamine contained in the mixed powder, and the CB particles contained therein are regarded as CB particles contained in the mixed powder. Therefore, the mixed powder can be said to be a mixed powder containing CB particles, particles of methylated melamine, and particles of acrylic resin). That is, by such a process, a mixed powder containing CB particles (particles in resin raw material coated carbon particles), methylated melamine particles (particles in a coated state), and acrylic resin particles was prepared. In addition, the resin raw material coated carbon particles (methylated melamine / coated CB particles) and acrylic resin particles in the mixed powder obtained after stirring were printed (filmed) with a screen mesh with an opening of 30 μm in the electrostatic screen printing described later, so it is clear that their average particle diameters (secondary particle diameter for acrylic resin particles) are 30 μm or less. In addition, it is clear that the average particle diameter of the resin raw material coated carbon particles (methylated melamine / coated CB particles) is 10 nm or more, considering that the average primary particle diameter of the CB particles (hydrophilic) is 46 nm. Therefore, it is clear that the powder of the resin raw material coated carbon particles in the mixed powder is a powder with an average particle diameter of 0.01 to 30 μm (the average particle diameter of such resin raw material coated carbon particles (composite particles) is considered to be the average primary particle diameter of the methylated melamine particles).

[0111] Next, the obtained mixed powder was applied to the surface of carbon paper (a surface-treated product with a melamine resin raw material) having a surface of the raw material of melamine resin on the surface by electrostatic screen printing (dry film formation method) to form a film, and a layer of the mixed powder was formed. Note that, as the electrostatic screen printing method, an electrostatic screen printing device (manufactured by Belc Kogyo, product name: T-1) and a screen mesh (manufactured by Belc Kogyo, product name: electrostatic screen plate, mesh size: 30 μm) were used, and a voltage of 1.75 kV was applied between the carbon paper and the screen mesh, and the mixed powder was placed on the screen mesh and rubbed with a squeegee to drop the mixed powder from the mesh onto the carbon paper to form a film.

[0112] Next, the laminated mixed powder layer was compressed by pressing at 3 MPa for 1 minute using a flat press. Then, the compressed mixed powder layer was heated and baked using an electric furnace under the conditions of pressure: normal pressure, heating temperature: temperature shown in Table 6, and time: 30 minutes (the temperature was raised from room temperature at a rate of 10°C per minute up to the heating temperature), thereby forming a water-repellent layer on the carbon paper containing CB particles and a thermosetting resin (composite resin of melamine resin and acrylic resin) which is a polycondensation product of the resin raw material (methylated melamine and acrylic resin) constituting the resin raw material particles, and a laminate of carbon paper and a water-repellent layer (laminate for gas diffusion layer of fuel cell) was obtained. Note that, from the above-mentioned baking conditions (heating temperature and heating time), it is clear that each of the formed water-repellent layers contains a composite resin of melamine resin and acrylic resin (water-resistant resin) obtained by sufficient progress of the polycondensation reaction of the resin raw material (methylated melamine and acrylic resin), and therefore it is clear that the layer has water resistance. In addition, before and after firing the water-repellent layer of the laminate obtained in Example 20, SEM-EDS analysis was performed on the water-repellent layer (and its precursor) to obtain SEM-EDS images (element mapping images). In the element mapping images before and after firing, the positions of the C element (constituent element of the carbon particles), the O element (constituent element of the acrylic resin), and the N element (constituent element of the melamine resin) were confirmed, and it was found that each element was uniformly dispersed overall after firing as before firing. From the results of such SEM-EDS analysis, it can be understood that each particle is uniformly dispersed in the formed water-repellent layer.

[0113] [Table 6]

[0114] [Evaluation of properties of laminates obtained in Examples 16 to 22] <Thermogravimetry (TG) and Differential Thermal Analysis (DTA) of Resin Raw Material Particles: Measurement of Decomposition Temperature of Thermosetting Resin> Using the same resin raw material particles as those used in the manufacture of the water-repellent layer in Example 16 (a mixture of resin raw material coated carbon particles (assumed to be methylated melamine particles) and acrylic resin particles), the thermogravimetric change of the thermosetting resin raw material constituting the resin raw material particles was measured with a thermal analyzer (manufactured by Rigaku Corporation, product name: Thermoplus TG8120) at a temperature rise rate of 1°C / min, and a TG curve was obtained. In addition, differential thermal analysis (DTA) of the resin raw material particles was performed under the same conditions using the thermal analyzer, and a DTA curve was obtained. The thermogravimetric change measurement results (TG curve) and the differential thermal analysis results (DTA curve) are both shown in Figure 11.

[0115] From the results shown in Fig. 11, it was confirmed that there is an inflection point at 290°C in the TG curve (Fig. 11), and therefore it was found that the decomposition temperature of the resin (composite resin of melamine resin and acrylic resin) formed as a fired product of the mixed particles of methylated melamine particles (carbon particles coated with resin raw material) and acrylic resin particles is 290°C. When heating was performed at a temperature rise rate of 1°C / min, it can be considered that the polycondensation reaction had progressed sufficiently by heating up to 290°C.

[0116] For Examples 16 to 22, the mass of the resin after baking was calculated from the amount of resin raw material charged (30% by mass) and the relationship between the heating temperature and the weight loss rate (%) calculated from the TG curve shown in Figure 11, and the value (mass ratio) of "CB particles / resin after baking" for each Example is shown in Table 7. Here, for the value (mass ratio), taking into account the baking temperature of each Example, for convenience, based on Figure 11, the weight loss rate of the resin due to the reaction was assumed to be 2.8% by mass in Example 16, 3.1% by mass in Example 17, 3.4% by mass in Example 18, 3.8% by mass in Example 19, 4.7% by mass in Example 20, 5.5% by mass in Example 21, and 7.9% by mass in Example 22, and the value calculated from the charge ratio (mixture ratio) of the CB particles and the raw resin was adopted. In addition, taking into consideration the relationship between the firing temperature and the amount of mass reduction of the resin shown in FIG. 11, the results shown in Table 7, and the charge ratio (mixture ratio) of the CB particles and raw resin, it is clear that the water-repellent layers obtained in Examples 16 to 22 all had a post-fired resin content in the range of 13 to 57 mass% relative to the total amount of the CB particles and post-fired resin in the layer.

[0117] <Bonding strength test: Measurement of the bonding strength between the carbon paper and the water-repellent layer> The laminates obtained in Examples 16 to 22 were subjected to the same test (90 degree peel strength test) as the "bonding strength test" performed to evaluate the properties of the laminates obtained in Examples 1 to 11 and Comparative Examples 1 to 3, and the bonding strength (unit: N / m) of the water-repellent layer to the carbon paper was measured. The obtained results are shown in Table 7 and Fig. 12. For reference, Table 7 and Fig. 12 also show the results of Examples 12 to 15 and Comparative Example 5.

[0118] [Table 7]

[0119] As is clear from the results shown in Table 7, the laminates (laminates for gas diffusion layers of fuel cells) obtained in Examples 16 to 22, which have carbon paper having melamine resin on the surface as a porous substrate and the type of resin constituting the water-repellent layer is a composite resin of melamine resin and acrylic resin, have a bonding strength of 17.8 N / m or more, whereas the laminate obtained in Comparative Example 5, in which the baking temperature was 350 ° C. in the same manner as in the conventional manufacturing method, has a bonding strength of 0.62 N / m. Therefore, it was found that the bonding strength can be greatly improved by using a composite resin of melamine resin and acrylic resin, which are thermosetting resins, as the resin (resin as a component) used for the water-repellent layer. In addition, from the results shown in Table 7 and FIG. 12, even when the baking temperature was 280 ° C., a very high bonding strength of 36.5 N / m was achieved, so it is clear that a sufficiently high bonding strength can be obtained even when the baking temperature is 10 ° C. lower than the decomposition temperature (290 ° C.) of the composite resin of melamine resin and acrylic resin. In addition, even if the temperature (about 280°C) is 10°C lower than the decomposition temperature (290°C) of the composite resin, the temperature can be lowered by 60°C compared to the case where the baking temperature is 350°C in the same manner as in the conventional manufacturing method, so it is understood that the energy efficiency during manufacturing is sufficiently improved according to the present invention. In addition, when the baking temperature is 220°C to 260°C (Examples 19 to 21), the bonding strength is 76.9 N / m or more, and it was confirmed that a very high level of bonding strength can be achieved. Furthermore, even when the temperature (160°C) is 130°C lower than the decomposition temperature (290°C) of the composite resin (Example 16), the bonding strength of the water-repellent layer is 17.8 N / m, and it was found that a sufficiently high level of bonding strength can be obtained.

[0120] As described above, from the evaluation results of the properties of the laminate shown in Tables 2, 5 and 7 (evaluation results of the properties of the water-repellent layer in the laminate), a mixed powder containing a powder (A) of hydrophilic carbon particles and a powder (B) of resin raw material particles made of a thermosetting resin raw material such that the content of the powder (B) is 15 to 60 mass% relative to the total amount of the powders (A) and (B) is formed on the porous substrate by a dry film formation method, compacted, and then baked at a temperature 10 to 130 ° C (preferably 40 to 120 ° C, more preferably 50 to 110 ° C) lower than the decomposition temperature of the polycondensate of the thermosetting resin raw material (thermosetting resin formed after baking), It became clear that a water-repellent layer consisting of a mixed bond of the powder (A) of hydrophilic carbon particles and the water-resistant resin (C) can be formed with energy efficiency. It was also revealed that when a water-repellent layer is formed in this way, the resulting water-repellent layer has excellent bonding strength to the porous substrate. In addition, from the evaluation results of the properties of the laminate shown in Tables 2 and 5 (evaluation results of the properties of the water-repellent layer in the laminate) and the results shown in Figures 9 to 10, it was also found that when the porous substrate after firing has a thermosetting resin at least on its surface (Example 13, etc.), it is possible to further improve the bonding strength between the water-repellent layer and the porous substrate. [Industrial Applicability]

[0121] As described above, according to the present invention, it is possible to provide a method for producing a water-repellent layer for a fuel cell that can efficiently produce a water-repellent layer for a fuel cell with high energy efficiency and can increase the bonding strength between the water-repellent layer and the porous substrate when the water-repellent layer is formed on the surface of a porous substrate for a gas diffusion layer; a water-repellent layer for a fuel cell that can be efficiently produced by adopting the production method and can increase the bonding strength between the water-repellent layer and the porous substrate; and a gas diffusion layer for a fuel cell that includes the water-repellent layer for a fuel cell. Therefore, the method for producing a water-repellent layer for a fuel cell of the present invention can be suitably used as a method for producing a water-repellent layer to be used in a gas diffusion layer for a fuel cell.

Claims

1. a film-forming step of forming a mixed powder layer by forming a film of a mixed powder, the mixed powder including a powder (A) of hydrophilic carbon particles having an average particle size of 0.002 to 50 μm and a powder (B) of resin raw material particles made of a thermosetting resin raw material and having an average particle size of 0.01 to 50 μm, the content of the powder (B) being 15 to 60 mass % based on the total amount of the powders (A) and (B), by a dry film-forming method; a consolidation step of compressing the mixed powder layer under a pressure of 0.2 to 50 MPa; a water-repellent layer forming step of baking the mixed powder layer after the consolidation step at a temperature 10 to 130° C. lower than the decomposition temperature of the thermosetting resin to obtain a water-repellent layer for a fuel cell made of a mixed bond of the hydrophilic carbon particle powder (A) and a water-resistant resin (C) made of a thermosetting resin which is a polycondensate of the raw materials; A method for producing a water-repellent layer for a fuel cell, comprising:

2. 2. The method for manufacturing a water-repellent layer for a fuel cell according to claim 1, wherein the thermosetting resin is at least one resin selected from the group consisting of phenolic resin, silicone resin, polyurethane resin, urea resin, melamine resin, and acrylic resin.

3. 2. The method for producing a water-repellent layer for a fuel cell according to claim 1, wherein the thermosetting resin is a melamine resin.

4. The method for manufacturing a water-repellent layer for a fuel cell, as described in claim 1, characterized in that in the film-forming process, a porous substrate having at least one raw material of the resin that constitutes the thermosetting resin and / or at least one of the resins that constitute the thermosetting resin on its surface is used as the film-forming substrate, and the mixed powder is formed on the surface of the film-forming substrate.

5. a layer made of a sintered product of a mixed powder, the layer comprising: a powder (A) of hydrophilic carbon particles having an average particle size of 0.002 to 50 μm; and a powder (B) of resin raw material particles made of a thermosetting resin raw material having an average particle size of 0.01 to 50 μm, the content of the powder (B) being 15 to 60 mass % based on the total amount of the powders (A) and (B); the layer is a layer made of a mixed bond of the hydrophilic carbon particle powder (A) and a water-resistant resin (C) made of a thermosetting resin which is a polycondensation product of the raw materials, and A water-repellent layer for a fuel cell, wherein the content of the water-resistant resin (C) in the mixed assembly is 13 to 57 mass % based on the total amount of the powder (A) and the water-resistant resin (C).

6. A gas diffusion layer for a fuel cell, comprising: a porous substrate; and the water-repellent layer for a fuel cell according to claim 5 laminated on a surface of the porous substrate.

7. 7. The gas diffusion layer for a fuel cell according to claim 6, wherein the porous substrate is a porous substrate having at least one of the resins constituting the thermosetting resin on a surface thereof.

Citation Information

Patent Citations

  • Granular material, water-repellent layer, and manufacturing method thereof

    JP2021002444A