Epoxy resin composition for molding semiconductor, and molding film and semiconductor package that employ the same
A specialized epoxy resin composition with specific epoxy polymers and high inorganic filler content addresses visibility and warping issues in semiconductor molding, improving heat resistance and mechanical properties while maintaining transparency.
Patent Information
- Application Number
- JP2024098039
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-01-07
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-07
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing epoxy resin compositions for semiconductor molding, when used in thinner packages, suffer from reduced visibility due to the addition of excessive inorganic fillers, while also experiencing issues with heat shrinkage and warping.
A new epoxy resin composition containing specific epoxy polymers and compounds, along with a high content of inorganic filler, is developed to maintain low thermal expansion and improve mechanical properties and visibility.
The new composition enhances heat resistance, mechanical properties, and reduces warpage in semiconductor packages while maintaining high transparency, making defect identification easier.
Smart Images

Figure 2024137950000001 
Figure 2024137950000002 
Figure 2024137950000003
Abstract
Description
[Technical field]
[0001] [CROSS REFERENCE TO RELATED APPLICATIONS] This application claims the benefit of priority based on Korean Patent Application No. 10-2018-0004041, filed January 11, 2018, and Korean Patent Application No. 10-2019-0001976, filed January 7, 2019, and all contents disclosed in the documents of said Korean patent applications are incorporated herein by reference.
[0002] The present invention relates to an epoxy resin composition for semiconductor molding, and a molding film and a semiconductor package using the same. More specifically, the present invention relates to an epoxy resin composition for semiconductor molding which has excellent heat resistance and mechanical properties, a low thermal expansion coefficient and improved warpage characteristics, and improved visibility, and a molding film and a semiconductor package using the epoxy resin composition for semiconductor molding. [Background technology]
[0003] In general, the manufacturing process of semiconductor chips includes a process of forming fine patterns on a wafer, polishing the wafer to meet the specifications of the final device, and packaging the wafer.
[0004] The packaging process mentioned above includes a wafer inspection process to inspect semiconductor chips for defects; a dicing process to cut the wafer and separate it into individual chips; a die bonding process to attach the separated chips to a mounting plate of a circuit film or a lead frame; a wire bonding process to connect chip pads on the semiconductor chip to the circuit pattern of the circuit film or lead frame with electrical connection means such as wires; a molding process to wrap the outside of the semiconductor chip with an encapsulant to protect the internal circuitry and other components; a trim process to cut the dam bars connecting the leads; a forming process to bend the leads into a desired shape; and a finished product inspection process to inspect the completed package for defects.
[0005] In particular, the molding process is essential to prevent the internal circuits and other components of the semiconductor chip from being exposed to the outside and causing a sudden deterioration in performance due to moisture, impact, heat, etc. Generally, epoxy resin is used as a sealant in the molding process because it is economical and easy to mold.
[0006] However, as electronic devices have become smaller, lighter, and more functional in recent years, semiconductor packages are also being manufactured to be smaller, lighter, and thinner. As a result, in a process for manufacturing a thinner semiconductor package compared to the existing semiconductor packaging process, there is a problem that the package bends due to thermal shrinkage, curing shrinkage, etc. of the epoxy resin composition during the molding process.
[0007] To solve this problem, there have been attempts to improve warpage characteristics by adding a large amount of inorganic filler to the epoxy resin used in the molding process to reduce the difference between the thermal expansion coefficient of the epoxy resin composition and the thermal expansion coefficient of the semiconductor chip.
[0008] However, the addition of such an excessive amount of inorganic filler causes a limit in that visibility is reduced in the final semiconductor package even though no separate pigment or dye is added.
[0009] Therefore, there is a demand for development of an epoxy resin composition for semiconductor molding that has a low thermal expansion coefficient, improved warpage characteristics, and improved visibility. Summary of the Invention [Problem to be solved by the invention]
[0010] An object of the present invention is to provide an epoxy resin composition for semiconductor molding which has excellent heat resistance and mechanical properties, a low thermal expansion coefficient and improved warpage characteristics, while improving visibility.
[0011] Another object of the present invention is to provide a molding film obtained by using the epoxy resin composition for semiconductor molding.
[0012] It is also an object of the present invention to provide a semiconductor package including a semiconductor sealed with the molding film. [Means for solving the problem]
[0013] The present invention provides an epoxy resin composition for semiconductor molding, comprising: an epoxy resin containing an epoxy polymer represented by the following chemical formula 1 and an epoxy compound represented by the following chemical formula 2; and 50% by weight or more and 90% by weight or less of an inorganic filler.
[0014] [ka]
[0015] In the above chemical formula 1, R is an alkyl group having 1 to 20 carbon atoms or a cycloalkyl group having 3 to 20 carbon atoms, n is an integer of 1 to 30, and C 1 is a cycloalkane having 3 to 10 carbon atoms, and L 1 is a direct bond or an alkylene group having 1 to 10 carbon atoms,
[0016] [ka]
[0017] In the above chemical formula 2, C 2 ~C 3 are each independently a cycloalkane having 3 to 10 carbon atoms and having an epoxy group bonded thereto; L 2 is a direct bond or an alkylene group having 1 to 10 carbon atoms.
[0018] The present invention also provides a molding film comprising: a polymer including a repeating unit represented by the following chemical formula 3 and a repeating unit represented by the following chemical formula 4; and 50% by weight or more and 90% by weight or less of an inorganic filler dispersed in the polymer.
[0019] [ka]
[0020] In the above chemical formulas 3 to 4, C 4 ~C 8 are each independently a cycloalkane having 3 to 10 carbon atoms; L 3 ~L 5 each independently represents a direct bond or an alkylene group having 1 to 10 carbon atoms.
[0021] The present invention also provides a semiconductor package including a semiconductor sealed with the molding film of the other embodiment.
[0022] Hereinafter, an epoxy resin composition for semiconductor molding, a molding film and a semiconductor package using the same according to a specific embodiment of the present invention will be described in more detail.
[0023] In this specification, when a part "comprises" certain elements, this means that it can further include other elements, rather than excluding other elements, unless specifically stated to the contrary.
[0024] In this specification, the weight average molecular weight means the weight average molecular weight in terms of polystyrene measured by the GPC method. In the process of measuring the weight average molecular weight in terms of polystyrene measured by the GPC method, a commonly known analyzer, a detector such as a refractive index detector, and an analytical column can be used, and commonly applied temperature conditions, solvents, and flow rates can be applied. Specific examples of the measurement conditions include using a Polymer Laboratories PLgel MIX-B 300 mm long column and a Waters PL-GPC220 instrument, the evaluation temperature is 160° C., 1,2,4-trichlorobenzene is used as a solvent, the flow rate is 1 mL / min, the sample is prepared to a concentration of 10 mg / 10 mL, and then supplied in an amount of 200 μL, and the Mw value can be obtained using a calibration curve formed using a polystyrene standard. Nine types of polystyrene standards with molecular weights of 2,000 / 10,000 / 30,000 / 70,000 / 200,000 / 700,000 / 2,000,000 / 4,000,000 / 10,000,000 were used.
[0025] In this specification, [ka] means a bond that is connected to another substituent, and a direct bond means that there are no other atoms present in the moiety represented by L.
[0026] In this specification, the alkyl group is linear or branched, and the number of carbon atoms is not particularly limited, but is preferably 1 to 40. According to one embodiment, the alkyl group has 1 to 20 carbon atoms. According to another embodiment, the alkyl group has 1 to 10 carbon atoms. According to yet another embodiment, the alkyl group has 1 to 6 carbon atoms. Specific examples of alkyl groups include, but are not limited to, methyl, ethyl, propyl, n-propyl, isopropyl, butyl, n-butyl, isobutyl, tert-butyl, sec-butyl, 1-methyl-butyl, 1-ethyl-butyl, pentyl, n-pentyl, isopentyl, neopentyl, tert-pentyl, hexyl, n-hexyl, 1-methylpentyl, 2-methylpentyl, 4-methyl-2-pentyl, 3,3-dimethylbutyl, 2-ethylbutyl, heptyl, n-heptyl, 1-methylhexyl, cyclopentylmethyl, cycloheptylmethyl, octyl, n-octyl, tert-octyl, 1-methylheptyl, 2-ethylhexyl, 2-propylpentyl, n-nonyl, 2,2-dimethylheptyl, 1-ethyl-propyl, 1,1-dimethyl-propyl, isohexyl, 2-methylpentyl, 4-methylhexyl, 5-methylhexyl, and the like.
[0027] In the present specification, the cycloalkyl group is not particularly limited, but preferably has 3 to 60 carbon atoms, and according to one embodiment, the cycloalkyl group has 3 to 30 carbon atoms. According to another embodiment, the cycloalkyl group has 3 to 20 carbon atoms. According to yet another embodiment, the cycloalkyl group has 3 to 6 carbon atoms. Specific examples include, but are not limited to, cyclopropyl, cyclobutyl, cyclopentyl, 3-methylcyclopentyl, 2,3-dimethylcyclopentyl, cyclohexyl, 3-methylcyclohexyl, 4-methylcyclohexyl, 2,3-dimethylcyclohexyl, 3,4,5-trimethylcyclohexyl, 4-tert-butylcyclohexyl, cycloheptyl, and cyclooctyl.
[0028] In the present specification, the aryl group is not particularly limited, but preferably has 6 to 60 carbon atoms, and may be a monocyclic aryl group or a polycyclic aryl group. According to one embodiment, the aryl group has 6 to 30 carbon atoms. According to one embodiment, the aryl group has 6 to 20 carbon atoms. The monocyclic aryl group may be, but is not limited to, a phenyl group, a biphenyl group, a terphenyl group, etc. The polycyclic aryl group may be, but is not limited to, a naphthyl group, an anthracenyl group, a phenanthryl group, a pyrenyl group, a perylenyl group, a chrysenyl group, a fluorenyl group, etc.
[0029] As used herein, cycloalkane refers to a cyclic hydrocarbon having a C n H 2n The molecular formula is: wherein the carbon number n may be 3 to 20, or 3 to 10, or 4 to 8, or 5 to 6. Specific examples include cyclopropane, cyclobutane, cyclopentane, cyclohexane, cycloheptane, and cyclooctane.
[0030] As used herein, an alkylene group is a divalent functional group derived from an alkane, and may be, for example, linear, branched, or cyclic, such as a methylene group, an ethylene group, a propylene group, an isobutylene group, a sec-butylene group, a tert-butylene group, a pentylene group, a hexylene group, and the like.
[0031] In this specification, an 'adjacent' group may mean a substituent substituted on an atom directly connected to the atom on which the substituent is substituted, a substituent sterically closest to the substituent, or another substituent substituted on the atom on which the substituent is substituted. For example, two substituents substituted at ortho positions on a benzene ring and two substituents substituted on the same carbon atom on an aliphatic ring may be interpreted as 'adjacent' groups to each other.
[0032] 1. Epoxy resin composition for semiconductor molding According to one embodiment of the present invention, there may be provided an epoxy resin composition for semiconductor molding, comprising: an epoxy resin including an epoxy polymer represented by Chemical Formula 1 above and an epoxy compound represented by Chemical Formula 2 below; and 50% by weight or more and 90% by weight or less of an inorganic filler.
[0033] The present inventors have found that the existing epoxy resin composition for semiconductor molding containing an excess inorganic filler together with an epoxy resin has a limit of reduced visibility, and in order to improve this, have developed a method of introducing a new epoxy resin containing an epoxy polymer represented by Chemical Formula 1 and an epoxy compound represented by the following Chemical Formula 2. In this way, in the case of a molding film obtained from a composition containing 50% by weight to 90% by weight of an inorganic filler together with the new epoxy resin having the specific structure represented by Chemical Formula 1 and Chemical Formula 2, it has been confirmed through experiments that the molding film has excellent visibility due to increased transparency, while at the same time achieving the effects of improving mechanical properties, heat resistance, and warpage properties due to the addition of an excess inorganic filler, thereby completing the invention.
[0034] The epoxy resin is made by mixing an epoxy polymer of Chemical Formula 1, which has excellent heat resistance and modulus, and an epoxy compound of Chemical Formula 2, which exists in a liquid state at room temperature and is advantageous for containing a high content of inorganic filler. The liquid epoxy compound improves the solubility of the inorganic filler, thereby preventing the inorganic filler from leaching out from the epoxy resin surface and reducing visibility. The polymerized epoxy structure significantly improves heat resistance, mechanical properties, and warpage properties, and the two different materials are uniformly dispersed to show overall uniform properties.
[0035] Unlike typical epoxy resins, the epoxy resin does not contain an unsaturated aliphatic functional group but contains a cyclic aliphatic functional group, and thus may have a refractive index very similar to that of the silica filler itself used as an inorganic filler, thereby achieving uniformly high transmittance within the molding film.
[0036] In particular, when a molding process of a semiconductor chip is performed using an epoxy resin composition containing a high content of inorganic filler together with the epoxy resin, the warpage characteristics of the semiconductor chip and the circuit board inside the semiconductor package after molding are minimized, thereby improving the durability of the thin semiconductor package, and the heat resistance and mechanical properties of the external molding film of the semiconductor package are improved, thereby improving the performance as a protective film for the semiconductor package. In addition, the solubility of the inorganic filler is increased to improve visibility, so that defects of the semiconductor chip and the circuit board inside the semiconductor package can be easily detected, and a desired color can be clearly achieved by blending pigments, dyes, etc.
[0037] Hereinafter, each component of the epoxy resin composition for semiconductor molding of the present invention will be described in detail.
[0038] (1) Epoxy resin The epoxy resin is a binder resin, and is a thermosetting resin that can be thermally cured by an epoxy curing agent that is further applied to the epoxy resin composition.
[0039] In the above chemical formula 1, R is an alkyl group having 1 to 20 carbon atoms or a cycloalkyl group having 3 to 20 carbon atoms, n is an integer of 1 to 30, and C 1 is a cycloalkane having 3 to 10 carbon atoms, and L 1 is a direct bond or an alkylene group having 1 to 10 carbon atoms.
[0040] In particular, the epoxy polymer represented by the above formula 1 is 1 The epoxy functional group is bonded to a cycloalkane having 3 to 10 carbon atoms represented by the following formula: and due to the chemical structural feature of not containing any double bonds in the molecule, it can have high weather resistance and transparency.
[0041] Specifically, the epoxy polymer represented by the above Chemical Formula 1 does not contain a general unsaturated aliphatic functional group, but contains a cyclic aliphatic functional group, and the epoxy resin synthesized therefrom can have a refractive index very similar to that of the silica filler itself used as an inorganic filler, thereby realizing a uniformly high transmittance within the molding film.
[0042] On the other hand, bisphenol-based epoxy polymers, which are epoxy polymers that have been used in conventional molding films, exhibit relatively low weather resistance and transparency due to the inclusion of double bonds in the molecule.
[0043] In addition, the epoxy polymer represented by Chemical Formula 1 has low viscosity characteristics, which is very advantageous for adding an excess filler, and since the synthesis of the polymer is carried out by an oxidation reaction of the double bond of cycloalkyne, it can have an effect of significantly reducing ionic impurities (e.g., chloride ions) in the finally synthesized epoxy polymer, compared to the synthesis process of a general bisphenol-based epoxy polymer.
[0044] On the other hand, in the above chemical formula 2, C 2 ~C 3 are each independently a cycloalkane having 3 to 10 carbon atoms and having an epoxy group bonded thereto; L 2 is a direct bond or an alkylene group having 1 to 10 carbon atoms.
[0045] In the above Chemical Formula 2, the cycloalkane having 3 to 10 carbon atoms to which an epoxy group is bonded may have an epoxy group bonded via two adjacent carbon atoms of the cycloalkane having 3 to 10 carbon atoms.
[0046] Preferably, in the above Chemical Formula 1, R is an alkyl group having 1 to 20 carbon atoms or a cycloalkyl group having 3 to 20 carbon atoms, n is an integer of 1 to 20, and C 1 is cyclohexane with 6 carbon atoms, and L 1 is a direct bond.
[0047] Specifically, the above Chemical Formula 1 is represented by the following Chemical Formula 1-1.
[0048] [ka]
[0049] In the above chemical formula 1-1, R, n, and L 1 The content relating to includes all of the content described above in Chemical Formula 1.
[0050] In addition, in the above chemical formula 2, preferably, 2 ~C 3 are each independently a cyclohexane having 6 carbon atoms and an epoxy group bonded thereto, and L 2 is an alkylene group having 1 to 5 carbon atoms (for example, a methylene group having 1 carbon atom).
[0051] The epoxy compound represented by the above formula 2 does not contain a general unsaturated aliphatic functional group, but contains a cyclic aliphatic functional group, and the epoxy resin synthesized therefrom can have a refractive index very similar to that of the silica filler itself used as an inorganic filler, thereby realizing uniformly high transmittance within the molding film.
[0052] Specifically, the above chemical formula 2 is represented by the following chemical formula 2-1.
[0053] [ka]
[0054] In the above chemical formula 2-1, L 2 The content relating to includes all the content described above in Chemical Formula 2.
[0055] The epoxy polymer represented by Formula 1 may have a weight average molecular weight (measured by GPC) of 100 g / mol to 5,000 g / mol. The epoxy polymer represented by Formula 1 can improve the transparency, heat resistance, and modulus of the epoxy resin, which is the reaction product produced, and can enhance the dispersibility of a high content of inorganic filler due to its low viscosity.
[0056] The epoxy compound represented by Chemical Formula 2 may be in a liquid state at room temperature (20° C. to 30° C.), and the epoxy resin produced as a reaction product may contain a high content of inorganic filler.
[0057] Meanwhile, the epoxy compound represented by the above Chemical Formula 2 may be contained in an amount of 50 to 90 parts by weight, or 60 to 85 parts by weight, or 65 to 85 parts by weight, based on 100 parts by weight of the epoxy polymer represented by the above Chemical Formula 1. If the epoxy compound represented by the above Chemical Formula 2 is reduced too much, the epoxy resin produced cannot contain a high content of inorganic filler sufficiently, and the mechanical properties and warpage characteristics of the molding film may deteriorate, and if the epoxy compound represented by the above Chemical Formula 2 is increased too much, the heat resistance and mechanical properties of the final molding film may decrease.
[0058] Meanwhile, the epoxy resin may be included in an amount of 5 wt % to 40 wt %, or 5 wt % to 30 wt %, or 5 wt % to 25 wt %, based on the total weight of the epoxy resin composition.
[0059] (2) Inorganic filler The epoxy resin composition for semiconductor molding may contain 50% by weight to 90% by weight, or 60% by weight to 80% by weight, or 70% by weight to 90% by weight of inorganic filler based on the total composition weight. Specifically, the inorganic filler may be contained in an amount of 200 parts by weight to 1,000 parts by weight, or 220 parts by weight to 700 parts by weight, or 230 parts by weight to 620 parts by weight, based on 100 parts by weight of the epoxy resin. By adding the inorganic filler in a high content, the thermal expansion coefficient of the molding film obtained from the epoxy resin composition for semiconductor molding is lowered, and the difference in thermal expansion coefficient with the semiconductor chip is reduced, thereby reducing the degree of warping of the final semiconductor package and improving the mechanical properties of the molding film.
[0060] The inorganic filler can be added to improve the handling property, heat resistance, and heat conduction of the composition, and to adjust the melt viscosity. Examples of the inorganic filler include, but are not limited to, one or a mixture of two or more of silicon dioxide, titanium dioxide, aluminum hydroxide, calcium carbonate, magnesium hydroxide, aluminum oxide, talc, and aluminum nitride.
[0061] However, preferably, silica can be used as the inorganic filler, particularly silica having an average particle size of 100 μm or less, or 10 μm or less, or 0.1 μm to 100 μm, or 0.1 μm to 10 μm.
[0062] The average particle size of the silica can be determined by checking the particle size of the entire silica, and the particle size of the silica can be checked on the cross section of the molding film described later. The average particle size of the silica can also be checked by the particle size of the entire silica used in manufacturing the molding film and the average particle size thereof.
[0063] The silica is a group of individual particles having an average particle size of 100 μm or less, or 10 μm or less, or from 0.1 μm to 100 μm, or from 0.1 μm to 10 μm, and the individual particles contained in such a group may have an average particle size of 100 μm or less, or 10 μm or less, or from 0.1 μm to 100 μm, or from 0.1 μm to 10 μm. More specifically, 95% or 99% of the individual particles contained in the group may have a particle size of 100 μm or less, or 10 μm or less, or from 0.1 μm to 100 μm, or from 0.1 μm to 10 μm.
[0064] (3) Epoxy resin composition The epoxy resin composition includes the above-mentioned epoxy resin and inorganic filler, and a method for producing the epoxy resin composition is not particularly limited, and various methods, for example, a method of mixing the epoxy resin and the inorganic filler using a mixer, may be used.
[0065] In addition, the epoxy resin composition may further include a heat curing catalyst, an epoxy curing agent, a leveling agent, a dispersing agent, or a solvent, if necessary.
[0066] The heat curing catalyst also plays a role in promoting the curing of the epoxy resin of the heat curable binder during heat curing. The heat curing catalyst that can be added is not particularly limited, and examples thereof include imidazole compounds such as imidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 4-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-(2-cyanoethyl)-2-ethyl-4-methylimidazole; amine compounds such as dicyandiamide, benzyldimethylamine, 4-(dimethylamino)-N,N-dimethylbenzylamine, 4-methoxy-N,N-dimethylbenzylamine, and 4-methyl-N,N-dimethylbenzylamine; hydrazine compounds such as adipic acid dihydrazide and sebacic acid dihydrazide; and compounds such as triphenylphosphine.
[0067] Other commercially available compounds include, for example, 2MZ-A, 2MZ-OK, 2PHZ, 2P4BHZ, and 2P4MHZ (all trade names of imidazole-based compounds) manufactured by Shikoku Chemical Industry Co., Ltd., and U-CAT3503N and UCAT3502T (all trade names of dimethylamine blocked isocyanate compounds), DBU, DBN, U-CATSA102, and U-CAT5002 (all bicyclic amidine compounds and salts thereof) manufactured by San-Apro Co., Ltd.
[0068] However, usable thermosetting catalysts are not limited to the above-mentioned examples, and any compound known as a thermosetting catalyst for epoxy resins or oxetane compounds, or a compound that promotes the reaction of an epoxy group and / or an oxetanyl group with a carboxyl group, can be used without any particular restrictions.
[0069] In addition, as the guanamine, S-triazine derivatives such as acetoguanamine, benzoguanamine, melamine, 2,4-diamino-6-methacryloyloxyethyl-S-triazine, 2-vinyl-4,6-diamino-S-triazine, 2-vinyl-4,6-diamino-S-triazine isocyanuric acid adduct, and 2,4-diamino-6-methacryloyloxyethyl-S-triazine isocyanuric acid adduct can also be used.
[0070] The thermosetting catalyst may be used in an appropriate amount in consideration of the degree of curing of the epoxy resin. For example, the epoxy resin composition may include 0.1 wt % to 20 wt %, or 0.1 wt % to 10 wt %, of the thermosetting catalyst.
[0071] The epoxy curing agent may be an amine compound, an acid anhydride compound, an amide compound, a phenol compound, or the like. The amine compound may be diaminodiphenylmethane, diethylenetriamine, triethylenetetramine, diaminodiphenylsulfone, isophoronediamine, or the like. The acid anhydride compound may be phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, maleic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylnadic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, or the like. The amide compound may be dicyandiamide, a polyamide resin synthesized from a dimer of linoleic acid and ethylenediamine, or the like. Examples of phenolic compounds that can be used include polyhydric phenols such as bisphenol A, bisphenol F, bisphenol S, fluorene bisphenol, and terpene diphenol; phenolic resins obtained by condensation of phenols with aldehydes, ketones, dienes, and the like; modified phenols and / or phenolic resins; halogenated phenols such as tetrabromobisphenol A and brominated phenolic resins; and other imidazoles, BF3-amine complexes, and guanidine derivatives.
[0072] The epoxy curing agent may be used in an appropriate amount in consideration of the mechanical properties of the molding film to be manufactured. For example, the epoxy resin composition may include 0.01 wt % to 10 wt %, or 0.1 wt % to 5 wt % of the epoxy curing agent.
[0073] The solvent can be used for the purpose of dissolving the epoxy resin composition and imparting a suitable degree of viscosity for application of the composition. Specific examples of the solvent include ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers (cellosolves) such as ethylene glycol monoethyl ether, ethylene glycol monomethyl ether, ethylene glycol monobutyl ether, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; acetates such as ethyl acetate, butyl acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, and dipropylene glycol monomethyl ether acetate; alcohols such as ethanol, propanol, ethylene glycol, propylene glycol, and carbitol; aliphatic hydrocarbons such as octane and decane; petroleum solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent naphtha; and amides such as dimethylacetamide and dimethylformamide (DMF). These solvents can be used alone or in combination of two or more.
[0074] The solvent may be used in an appropriate amount in consideration of the dispersibility, solubility, or viscosity of the epoxy resin composition, and for example, the epoxy resin composition may contain 0.1% to 50% by weight of the solvent, or 1% to 30% by weight of the solvent. If the content of the solvent is too low, the viscosity of the epoxy resin composition may increase, resulting in reduced coatability, and if the content of the solvent is too high, drying may not be performed well, resulting in increased adhesion of the formed film.
[0075] 2. Molding film for semiconductor molding According to another embodiment of the present invention, there is provided a molding film comprising: a polymer including a repeating unit represented by the above chemical formula 3 and a repeating unit represented by the above chemical formula 4; and 50% by weight or more and 90% by weight or less of an inorganic filler dispersed in the polymer.
[0076] The inorganic filler contained in the molding film of the other embodiment includes all of the contents described above in the epoxy resin composition for semiconductor molding of the one embodiment.
[0077] The polymer may include all of the repeating units represented by Formula 3 and Formula 4, and may include a cured product of the epoxy resin of the embodiment, thereby making it possible to uniformly realize the physical properties embodied by each of the two repeating units throughout the film.
[0078] Specifically, the repeating unit represented by chemical formula 3 contained in the polymer is C 4 ~C 5 are each independently a cycloalkane having 3 to 10 carbon atoms; L 3 ~L 4 each independently represents a direct bond or an alkylene group having 1 to 10 carbon atoms.
[0079] In this way, the repeating unit represented by Chemical Formula 3 contained in the polymer does not contain an unsaturated aliphatic functional group but contains a cyclic aliphatic functional group, and the epoxy polymer containing the same can have a refractive index very similar to that of the silica filler itself used as an inorganic filler, thereby achieving uniformly high transmittance within the molding film.
[0080] Preferably, the repeating unit represented by chemical formula 3 contained in the polymer is 4 ~C 5 are each independently a cyclohexane having 6 carbon atoms, and L 3 is a direct bond, and L 4 is an alkylene group having 1 to 5 carbon atoms (for example, a methylene group having 1 carbon atom).
[0081] The repeating unit represented by the above chemical formula 3 is more specifically a repeating unit represented by the following chemical formula 3-1.
[0082] [ka]
[0083] In the above chemical formula 3-1, L 3 ~L 4 The content of may include the content described above in Chemical Formula 3.
[0084] The repeating unit represented by Chemical Formula 3 contained in the polymer contained in the molding film is obtained by an epoxy crosslinking reaction of the epoxy polymer represented by Chemical Formula 1 of the above-mentioned embodiment, and the crosslinked structure formed by the repeating unit represented by Chemical Formula 3 can improve heat resistance and mechanical properties.
[0085] On the other hand, the repeating unit represented by chemical formula 4 contained in the polymer is C 6 ~C 8 are each independently a cycloalkane having 3 to 10 carbon atoms; L 5 is a direct bond or an alkylene group having 1 to 10 carbon atoms.
[0086] Preferably, the repeating unit represented by chemical formula 4 contained in the polymer is 6 ~C 8 are each independently a cyclohexane having 6 carbon atoms, and L 5 is an alkylene group having 1 to 5 carbon atoms (for example, a methylene group having 1 carbon atom).
[0087] In this way, the repeating unit represented by Chemical Formula 4 contained in the polymer does not contain an unsaturated aliphatic functional group but contains a cyclic aliphatic functional group, and the epoxy polymer containing the same can have a refractive index very similar to that of the silica filler itself used as an inorganic filler, thereby achieving uniformly high transmittance within the molding film.
[0088] The repeating unit represented by Chemical Formula 4 contained in the polymer is more specifically a repeating unit represented by Chemical Formula 4-1 below.
[0089] [ka]
[0090] In the above chemical formula 4-1, L 5 The content of may include the content described above in Chemical Formula 4.
[0091] The repeating unit represented by Chemical Formula 4 contained in the polymer contained in the molding film is obtained by an epoxy crosslinking reaction between the epoxy polymer represented by Chemical Formula 1 of the above-mentioned embodiment and the epoxy compound represented by Chemical Formula 2. The crosslinked structure formed by the repeating unit represented by Chemical Formula 4 increases the solubility of a high content of inorganic filler, thereby improving visibility.
[0092] Meanwhile, the polymer included in the molding film may further include a repeating unit represented by the following Chemical Formula 5:
[0093] [ka]
[0094] In the above chemical formula 5, C 9 ~C 10 are each independently a cycloalkane having 3 to 10 carbon atoms; L 6 is a direct bond or an alkylene group having 1 to 10 carbon atoms.
[0095] Preferably, the repeating unit represented by Chemical Formula 5 contained in the molding film is C 9 ~C 10 are each independently a cyclohexane having 6 carbon atoms, and L 6is an alkylene group having 1 to 5 carbon atoms (for example, a methylene group having 1 carbon atom).
[0096] The repeating unit represented by the above chemical formula 5 is more specifically a repeating unit represented by the following chemical formula 5-1.
[0097] [ka]
[0098] In the above chemical formula 5-1, L 6 The content of may include the content described above in Chemical Formula 5.
[0099] When the polymer contained in the molding film further includes a repeating unit represented by Chemical Formula 5 in addition to the repeating units represented by Chemical Formula 3 and Chemical Formula 4, the repeating unit represented by Chemical Formula 4 can be crosslinked via the repeating unit represented by Chemical Formula 5. Specifically, at least two repeating units represented by Chemical Formula 4 can be crosslinked via the repeating unit represented by Chemical Formula 5.
[0100] In this way, by forming cross-links between the repeating units present inside the polymer, the polymer can have better heat resistance and mechanical properties, and can achieve a low thermal expansion coefficient and improved warpage characteristics.
[0101] More specifically, the structure in which the repeating units represented by Chemical Formula 4 are crosslinked via the repeating units represented by Chemical Formula 5 above is represented by Chemical Formula 6 below.
[0102] [ka]
[0103] In the above chemical formula 6, C 6 ~C 10 are each independently a cycloalkane having 3 to 10 carbon atoms; L 5 ~L 6are each independently a direct bond or an alkylene group having 1 to 10 carbon atoms. 6 ~C 10 , L 5 ~L 6 The content relating to may include all of the contents described above in Chemical Formula 3 to Chemical Formula 5.
[0104] More specifically, the repeating unit represented by the above formula 6 is represented by the following formula 6-1.
[0105] [ka]
[0106] In the above chemical formula 6-1, L 5 ~L 6 The content relating to may include all of the contents described above in Chemical Formula 3 to Chemical Formula 5.
[0107] Meanwhile, the polymer may include a reaction product of an epoxy polymer represented by Chemical Formula 1 of the embodiment and an epoxy compound represented by Chemical Formula 2. The details of the epoxy polymer represented by Chemical Formula 1 and the epoxy compound represented by Chemical Formula 2 include all the details described above in the embodiment.
[0108] That is, the molding film of the other embodiment means a fully cured film obtained by applying, drying, and curing the epoxy resin composition for semiconductor molding of the one embodiment, and the polymer contained in the molding film may include a reaction product obtained by an epoxy crosslinking reaction between an epoxy polymer contained in the epoxy resin composition for semiconductor molding and an epoxy compound.
[0109] In the coating step, a known method and device that can be used to coat the resin composition can be used. For example, a comma coater, a blade coater, a lip coater, a rod coater, a squeeze coater, a reverse coater, a transfer roll coater, a gravure coater, a spray coater, etc. can be used.
[0110] The drying temperature may be 50° C. or higher and 130° C. or lower, or 70° C. or higher and 100° C. or lower. The curing conditions are not particularly limited, and for example, the composition may be heated and cured in an oven at 140° C. or higher and 200° C. or lower for 0.5 hours or higher and 2 hours or lower.
[0111] The molding film may include 50% by weight to 90% by weight, or 60% by weight to 80% by weight, or 70% by weight to 90% by weight, based on the total weight of the molding film.
[0112] Meanwhile, the transmittance of the molding film (measured at 550 nm) may be 60% to 90%, or 70% to 85%. The molding film has a high transmittance in such a range, and thus has excellent transparency, and can improve visibility when applied to a semiconductor package.
[0113] In addition, the modulus of the molding film (measured at 25° C.) may be 10.0 GPa to 20.0 GPa, or 15.0 GPa to 20.0 GPa. The molding film has a high modulus in this range, and thus can improve the durability of the semiconductor package based on its high mechanical properties when applied to the semiconductor package.
[0114] Meanwhile, the molding film may have an average coefficient of thermal expansion (CTE) of 1.00 ppm / K to 25.00 ppm / K or 1.00 ppm / K to 8.00 ppm / K measured in a temperature range of 0° C. to 50° C. Since the molding film has a low CTE in this range, when applied to a semiconductor package, the difference in CTE between the molding film and a semiconductor substrate is reduced, thereby reducing warpage characteristics of the semiconductor package and improving durability.
[0115] The thickness of the molding film is not particularly limited and can be freely adjusted within a range of, for example, 0.01 μm to 1,000 μm. When the thickness of the molding film increases or decreases by a certain value, the physical properties measured from the molding film can also change by a certain value. In the present invention, the thickness used to measure the physical properties of the molding film may be, for example, 95 μm to 105 μm, or 98 μm to 102 μm.
[0116] Meanwhile, the molding film includes a cycloaliphatic epoxy resin matrix; and an inorganic filler dispersed in the cycloaliphatic epoxy resin; and the absolute value of the difference between the refractive index of the cycloaliphatic epoxy resin matrix and the refractive index of the inorganic filler may be 0.1 or less, or 0.01 to 0.1, or 0.05 to 0.1, or 0.06 to 0.08. As a result, the molding film has excellent optical performance and can achieve high transmittance since the refractive index of the cycloaliphatic epoxy resin matrix and the refractive index of the inorganic filler have similar values in the final cured state.
[0117] The absolute value of the difference between the refractive index of the cycloaliphatic epoxy resin matrix and the refractive index of the inorganic filler means the difference between the larger one of the refractive index of the cycloaliphatic epoxy resin matrix and the refractive index of the inorganic filler and the smaller one of the refractive index of the cycloaliphatic epoxy resin matrix and the refractive index of the inorganic filler.
[0118] Specifically, in the molding film, when the absolute value of the difference between the refractive index of the cycloaliphatic epoxy resin matrix and the refractive index of the inorganic filler satisfies 0.1 or less, the refractive index of the cycloaliphatic epoxy resin matrix and the refractive index of the inorganic filler may have similar values, so that the transmittance (measured at 550 nm) may be 60% to 90%, or 70% to 85%. The molding film has a high transmittance in such a range, so that it has excellent transparency and can improve visibility when applied to a semiconductor package.
[0119] On the other hand, when the absolute value of the difference between the refractive index of the cycloaliphatic epoxy resin matrix and the refractive index of the inorganic filler in the molding film exceeds 0.1 and is too large, the refractive index of the cycloaliphatic epoxy resin matrix and the refractive index of the inorganic filler have significantly different values, and therefore the transmittance (measured at 550 nm) decreases to less than 60%, decreasing transparency, which may cause poor visibility when applied to a semiconductor package.
[0120] In particular, the absolute value of the difference between the refractive index of the cycloaliphatic epoxy resin matrix and the refractive index of the inorganic filler in the molding film is similar and is less than 0.1, because the cycloaliphatic epoxy resin, which does not contain unsaturated aliphatic moieties, is used as a binder resin, thereby achieving better optical performance than that of general epoxy resins.
[0121] Therefore, in the molding film, it is easy to adjust the refractive index of the cycloaliphatic epoxy resin matrix and the refractive index of the silica filler itself used as the inorganic filler to a similar level, thereby achieving a uniformly high transmittance within the molding film.
[0122] The refractive index of the cycloaliphatic epoxy resin matrix is 1.6 or less, or 1.4 to 1.6 or 1.5 to 1.6 or 1.5 to 1.55 or 1.51 to 1.53, and the refractive index of the inorganic filler is 1.5 or less, or 1.3 to 1.5 or 1.4 to 1.5 or 1.42 to 1.48 or 1.44 to 1.46.
[0123] The inorganic filler contained in the molding film may include all of the contents described above in the epoxy resin composition for semiconductor molding according to the embodiment.
[0124] The cycloaliphatic epoxy resin matrix includes a cycloaliphatic epoxy resin containing a cycloaliphatic functional group in its molecular structure or a cured product of the cycloaliphatic epoxy resin, and the description of the polymer contained in the molding film described above is equally applicable to the cycloaliphatic epoxy resin.
[0125] The cycloaliphatic epoxy resin matrix may be formed by photocuring the epoxy resin composition for semiconductor molding according to the embodiment described above by irradiating it with light such as UV or by thermal curing.
[0126] The cycloaliphatic epoxy resin contained in the cycloaliphatic epoxy resin matrix does not contain an unsaturated aliphatic functional group, unlike general epoxy resins, and may have a refractive index very similar to that of the silica filler itself used as an inorganic filler, thereby achieving uniformly high transmittance within the molding film.
[0127] Therefore, the cycloaliphatic epoxy resin matrix may include a cycloaliphatic epoxy resin or a cured product thereof, which includes a repeating unit represented by Chemical Formula 3 and a repeating unit represented by Chemical Formula 4. The cycloaliphatic epoxy resin may further include a repeating unit represented by Chemical Formula 5. The cycloaliphatic epoxy resin may include a repeating unit represented by Chemical Formula 6, which has a structure in which the repeating unit represented by Chemical Formula 4 is crosslinked via the repeating unit represented by Chemical Formula 5.
[0128] The contents of Formula 3, Formula 4, Formula 5, and Formula 6 include all the contents described above regarding the polymer contained in the molding film.
[0129] The molding film includes the cycloaliphatic epoxy resin matrix; and an inorganic filler dispersed in the cycloaliphatic epoxy resin; and the absolute value of the difference between the refractive index of the cycloaliphatic epoxy resin matrix and the refractive index of the inorganic filler is 0.1 or less. The details of the manufacturing method, transmittance, modulus, thermal expansion coefficient, and thickness of the molding film are the same as those described above for the molding film including a polymer including a repeating unit represented by Chemical Formula 3 and a repeating unit represented by Chemical Formula 4; and 50% by weight or more and 90% by weight or less of inorganic filler dispersed in the polymer.
[0130] Meanwhile, the cycloaliphatic epoxy resin matrix may include a cycloaliphatic epoxy resin including a reaction product of an epoxy polymer represented by Chemical Formula 1 and an epoxy compound represented by Chemical Formula 2, or a cured product thereof. The details of the epoxy polymer represented by Chemical Formula 1 and the epoxy compound represented by Chemical Formula 2 each include all the details described above in the above embodiment.
[0131] The molding film may include 50% by weight to 90% by weight, or 60% by weight to 80% by weight, or 70% by weight to 90% by weight, based on the total weight of the molding film.
[0132] 3.Semiconductor Package According to yet another embodiment of the present invention, a semiconductor package may be provided that includes a semiconductor sealed with the molding film of the other embodiment.
[0133] That is, the molding film of the other embodiment can be used for sealing a semiconductor, and the semiconductor can include a circuit board and a semiconductor chip. The circuit board can be a printed circuit board (PCB), a semiconductor package board, or a flexible semiconductor package board (FPCB).
[0134] More specifically, the molding film of the other embodiment can be laminated on a semiconductor package substrate to seal the semiconductor chip or the circuit board mounted on the circuit board, thereby preventing the circuit board or the semiconductor chip from being exposed to the outside by the molding film, thereby achieving high reliability of the semiconductor package. Effect of the Invention
[0135] According to the present invention, there can be provided an epoxy resin composition for semiconductor molding which has excellent heat resistance and mechanical properties, a low thermal expansion coefficient and improved warpage characteristics, while improving visibility, and a molding film and a semiconductor package which use such an epoxy resin composition for semiconductor molding. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0136] Hereinafter, the functions and effects of the present invention will be described in more detail with reference to specific embodiments of the present invention, however, these embodiments are merely presented as examples of the present invention and do not limit the scope of the present invention. EXAMPLES
[0137] [Production Examples and Comparative Production Examples] Production of epoxy resin [Production Example 1] A solid polymer (weight average molecular weight: 1874 g / mol) represented by the following chemical formula A and a liquid compound (3',4'-epoxycyclohexane)methyl 3,4-epoxycyclohexylcarboxylate (manufactured by Daicel Chemical Industries, Ltd., Celloxide 2021P) represented by the following chemical formula B were mixed in a weight ratio of 5:4 to produce an epoxy resin.
[0138] [ka]
[0139] In the above chemical formula A, R is a butyl group and n is an integer of 15.
[0140] [ka]
[0141] [Production Example 2] An epoxy resin was produced in the same manner as in Production Example 1, except that the weight ratio of the solid polymer represented by the above chemical formula A to the liquid compound represented by the above chemical formula B [3',4'-epoxycyclohexane)methyl 3,4-epoxycyclohexylcarboxylate (manufactured by Daicel Chemical Industries, Ltd., Celloxide 2021P)] was changed to 6:4.
[0142] [Comparative Manufacturing Example 1] An epoxy resin was produced by mixing 31 parts by weight of bisphenol F type epoxy resin (manufactured by Tohto Kasei Co., Ltd., product number "Epotohto YDF-8170", epoxy equivalent 160) and 78.6 parts by weight of (3',4'-epoxycyclohexane) methyl 3,4-epoxycyclohexyl carboxylate (manufactured by Daicel Chemical Industries, Ltd., Celloxide2021P).
[0143] [Examples and Comparative Examples] [Example 1] (1) Manufacture of epoxy resin compositions for semiconductor molding An epoxy resin composition for semiconductor molding was prepared by mixing and stirring each component using 25 wt% of the epoxy resin obtained in Preparation Example 1 as a binder resin, 60 wt% of silica (average particle size 5 μm) as a filler, 2 wt% of 2-phenylimidazole as a thermosetting catalyst, 3 wt% of a leveling agent, and 10 wt% of MEK as a solvent. The components were then dispersed using a three-roll mill.
[0144] (2) Molding film / semiconductor package manufacturing A semiconductor package substrate on which a semiconductor chip was mounted was placed in a molding device including a mold having a specific shape, and the epoxy resin composition for semiconductor molding obtained above was supplied to the mold and heat cured at 175°C for 1 hour to manufacture a semiconductor package including a molding film having a thickness of 100 μm.
[0145] Meanwhile, the semiconductor package substrate on which the semiconductor chip is mounted was prepared by cutting a copper foil laminate LG-T-500GA manufactured by LG Chem Co., Ltd., having a thickness of 0.1 mm and a copper foil thickness of 12 μm, into a substrate measuring 5 cm wide and 5 cm long, with the semiconductor chip mounted on the surface.
[0146] The molding film contains repeating unit structures of the following chemical formulas C and D.
[0147] [ka]
[0148] [Example 2] An epoxy resin composition for semiconductor molding, a molding film, and a semiconductor package were prepared in the same manner as in Example 1, except that the epoxy resin obtained in Preparation Example 2 was used as a binder resin.
[0149] [Example 3] The epoxy resin obtained in Preparation Example 1 was used as a binder resin in an amount of 13 wt%, silica (average particle size 5 μm) as a filler in an amount of 80 wt%, 2-phenylimidazole as a thermosetting catalyst in an amount of 1 wt%, a leveling agent in an amount of 1 wt%, and MEK as a solvent in an amount of 5 wt%, and the components were mixed and stirred, and then dispersed using a three-roll mill to prepare an epoxy resin composition for semiconductor molding. The epoxy resin composition for semiconductor molding, a molding film, and a semiconductor package were prepared in the same manner as in Example 1.
[0150] [Example 4] An epoxy resin composition for semiconductor molding, a molding film, and a semiconductor package were prepared in the same manner as in Example 3, except that the epoxy resin obtained in Preparation Example 2 was used as the binder resin.
[0151] [Comparative Example 1] An epoxy resin composition for semiconductor molding, a molding film, and a semiconductor package were prepared in the same manner as in Example 1, except that the epoxy resin obtained in Comparative Preparation Example 1 was used as the binder resin.
[0152] [Comparative Example 2] An epoxy resin composition for semiconductor molding, a molding film, and a semiconductor package were prepared in the same manner as in Example 3, except that the epoxy resin obtained in Comparative Preparation Example 1 was used as the binder resin.
[0153] [Test example] 1. Heat resistance reliability evaluation The semiconductor package specimens obtained in Examples 1 to 4 and Comparative Examples 1 and 2 were left in a Pressure Cooker Test Chamber at 146°C and 100RH% for 14 hours, then removed and the moisture on the surface was removed. The specimens were then floated with the film side facing up on a solder bath at 288°C. The test specimens were visually inspected for peeling or deformation of the film to evaluate the heat resistance reliability. OK: 288, no explosion due to solder floating NG:288, Explosion due to floating solder
[0154] 2. Modulus rating The molding films having a thickness of 100 μm obtained in Examples 1 to 4 and Comparative Examples 1 to 2 were cut into specimens having a width of 5.3 mm and a length of 17.2 to 17.9 mm. The modulus was measured using a TA DMA Q800 under the conditions of a frequency of 1 Hz, an amplitude of 5 μm, and a static stress of 0.1 N, with a temperature rise rate of 10°C to 300°C at 10°C / min. The modulus at room temperature (25°C) was shown in Table 1 below.
[0155] 3. Transparency assessment The molding films having a thickness of 100 μm obtained in Examples 1 to 4 and Comparative Examples 1 to 2 were cut into specimens having a length of 3 cm and a width of 3 cm. The transmittance was measured at 550 nm using a UV-3600plus device manufactured by SHIMADZU.
[0156] 4. Warpage characteristics evaluation The molding films having a thickness of 100 μm obtained in Examples 1 to 4 and Comparative Examples 1 to 2 were cut into specimens having a width of 4.8 mm and a length of 16 mm. The thermal expansion coefficients (CTEs) were then measured at a temperature rise rate of 5° C. / min from -20° C. to 300° C. using a Q400EM manufactured by TA Corporation under a static stress of 0.1 N. The average values of the CTEs measured in the temperature range of 0° C. to 50° C. were calculated and shown in Table 1 below.
[0157] The measurement results of Experimental Examples 1 to 4 are shown in Table 1 below.
[0158] 5. Refractive index evaluation The refractive index of the epoxy resin matrix and the filler dispersed therein of the 100 μm thick molding films obtained in Examples 1 to 4 and Comparative Examples 1 and 2 was measured using a prism coupler manufactured by Sairon Technology, and the results are shown in Table 2 below.
[0159] The measurement results of Experimental Example 5 are shown in Table 2 below.
[0160] [Table 1]
[0161] As shown in Table 1 above, the molding films of Examples 1 to 4 obtained from compositions containing 60% by weight or more and 80% by weight or less of silica filler together with the epoxy resin synthesized in Preparation Example 1 or Preparation Example 2 showed high transmittance of 72.55% to 83.23% at 550 nm, confirming that transparency was greatly improved.
[0162] On the other hand, the molding films of Comparative Examples 1 and 2 obtained from compositions containing 60% by weight or more and 80% by weight or less of silica filler together with the epoxy resin synthesized in Comparative Preparation Example 1 showed significantly lower transmittance of 49.13% to 59.11% at 550 nm compared to the Examples, and were confirmed to have poor transparency.
[0163] As described above, the molding films of Examples 1 to 4 exhibited significantly improved transparency compared to the molding films of Comparative Examples 1 and 2, while also exhibiting excellent mechanical properties due to a high modulus equivalent to or higher than the comparative examples, as well as excellent warpage properties corresponding to a low thermal expansion coefficient.
[0164] In particular, the molding films of Examples 3 and 4 obtained from compositions containing 80% by weight of silica filler together with the epoxy resin synthesized in Preparation Example 1 or Preparation Example 2 had a modulus of 17.0 GPa to 18.5 GPa, which was significantly higher than that of the comparative example, and a coefficient of thermal expansion (CTE) of 4.62 ppm / K to 5.68 ppm / K, which was significantly lower than that of the comparative example, demonstrating the improved effect of increasing the content of silica filler.
[0165] [Table 2]
[0166] As shown in Table 2 above, in the molding films of Examples 1 to 4, the absolute difference between the refractive index of the epoxy resin matrix and the refractive index of the inorganic filler was small, ranging from 0.06 to 0.08, and it was confirmed that the epoxy resin matrix and the inorganic filler had refractive indices at approximately the same level.
[0167] On the other hand, in the molding films of Comparative Examples 1 and 2, the absolute value of the difference between the refractive index of the epoxy resin matrix and the refractive index of the inorganic filler was 0.17, which was significantly increased compared to the Examples, confirming that the refractive indexes of the epoxy resin matrix and the inorganic filler were different from each other.
[0168] In this way, the molding films of Examples 1 to 4 can achieve uniformly high transmittance within the molding film by adjusting the refractive index of the epoxy resin matrix and the refractive index of the inorganic filler to a similar level.
Claims
1. An epoxy resin comprising an epoxy polymer represented by the following Chemical Formula 1 and an epoxy compound represented by the following Chemical Formula 2: An epoxy resin composition for semiconductor molding comprising 50% by weight or more and 90% by weight or less of an inorganic filler: [Formula 1] In the above Chemical Formula 1, R is an alkyl group having 1 to 20 carbon atoms or a cycloalkyl group having 3 to 20 carbon atoms, n is an integer of 1 to 30, and C 1 is a cycloalkane having 3 to 10 carbon atoms, and L 1 is a direct bond or an alkylene group having 1 to 10 carbon atoms, [chemical 2] In the above chemical formula 2, C 2 ~C 3 each independently represents a cycloalkane having 3 to 10 carbon atoms and having an epoxy group bonded thereto; L 2 is a direct bond or an alkylene group having 1 to 10 carbon atoms.
2. In the above chemical formulas 1 and 2, C 1 ~C 2 The epoxy resin composition for semiconductor molding according to claim 1, wherein each of the is independently a cyclohexane having 6 carbon atoms.
3. In the above chemical formulas 1 and 2, L 1 is a direct bond, L 2 3. The epoxy resin composition for semiconductor molding according to claim 1, wherein is an alkylene group having 1 to 5 carbon atoms.
4. 4. The epoxy resin composition for semiconductor molding according to claim 1, comprising 50 parts by weight or more and 90 parts by weight or less of an epoxy compound based on 100 parts by weight of the epoxy polymer.
5. 5. The epoxy resin composition for semiconductor molding according to claim 1, further comprising 200 parts by weight or more and 1,000 parts by weight or less of an inorganic filler relative to 100 parts by weight of the epoxy resin.
6. 6. The epoxy resin composition for semiconductor molding according to claim 1, wherein the inorganic filler comprises silica.
7. 7. The epoxy resin composition for semiconductor molding according to claim 6, wherein the silica has an average particle size of 100 μm or less.
8. The epoxy resin composition for semiconductor molding according to any one of claims 1 to 7, further comprising a heat curing catalyst, an epoxy curing agent, a leveling agent, a dispersant or a solvent.
9. A molding film comprising: a polymer including a repeating unit represented by the following chemical formula 3 and a repeating unit represented by the following chemical formula 4; and 50% by weight to 90% by weight of an inorganic filler dispersed in the polymer: [C3] In the above chemical formulas 3 to 4, C 4 ~C 8 are each independently a cycloalkane having 3 to 10 carbon atoms; L 3 ~L 5 are each independently a direct bond or an alkylene group having 1 to 10 carbon atoms.
10. The molding film according to claim 9, wherein the polymer further comprises a repeating unit represented by the following formula 5: [C4] In the above chemical formula 5, C 9 ~C 10 are each independently a cycloalkane having 3 to 10 carbon atoms; L 6 is a direct bond or an alkylene group having 1 to 10 carbon atoms.
11. The molding film according to claim 10, wherein the repeating unit represented by Chemical Formula 4 is crosslinked via the repeating unit represented by Chemical Formula 5.
12. The molding film according to claim 11, wherein the repeating unit represented by Chemical Formula 4 is crosslinked via the repeating unit represented by Chemical Formula 5, the structure being represented by the following Chemical Formula 6: [C5] In the above chemical formula 6, C 6 ~C 10 are each independently a cycloalkane having 3 to 10 carbon atoms; L 5 ~L 6 are each independently a direct bond or an alkylene group having 1 to 10 carbon atoms.
13. The molding film according to any one of claims 9 to 12, wherein the polymer comprises a reaction product of an epoxy polymer represented by Chemical Formula 1 of claim 1 and an epoxy compound represented by Chemical Formula 2.
14. The molding film according to any one of claims 9 to 13, wherein the transmittance of the molding film (measured at 550 nm) is 60% or more and 90% or less.
15. A molding film comprising: a cycloaliphatic epoxy resin matrix; and an inorganic filler dispersed in the cycloaliphatic epoxy resin; wherein the absolute value of the difference between the refractive index of the cycloaliphatic epoxy resin matrix and the refractive index of the inorganic filler is 0.1 or less.
16. 16. The molding film of claim 15, wherein the transmittance of the molding film (measured at 550 nm) is 60% or more and 90% or less.
17. The cycloaliphatic epoxy resin matrix comprises a cycloaliphatic epoxy resin containing a repeating unit represented by Chemical Formula 3 of claim 9 and a repeating unit represented by Chemical Formula 4 of claim 9, or a cured product thereof. The molding film according to claim 15 or 16.
18. The cycloaliphatic epoxy resin matrix comprises a cycloaliphatic epoxy resin comprising a reaction product of an epoxy polymer represented by Chemical Formula 1 of claim 1 and an epoxy compound represented by Chemical Formula 2, or a cured product thereof. The molding film according to any one of claims 15 to 17.
19. The molding film according to any one of claims 15 to 18, wherein the content of the inorganic filler dispersed in the cycloaliphatic epoxy resin matrix is 50% by weight or more and 90% by weight or less based on the total weight of the molding film.
20. A semiconductor package comprising a semiconductor sealed with the molding film according to any one of claims 9 to 19.
Citation Information
Patent Citations
Epoxy resin composition for semiconductor molding, molding film and semiconductor package using the same