Semiconductor device

Highly purified oxide semiconductors, especially In-Ga-Zn-O-based materials, are used in switching transistors to address high leakage currents in CMOS circuits, achieving significant reductions in standby power consumption and maintaining operational efficiency.

JP2024138162AActive Publication Date: 2024-10-07SEMICON ENERGY LAB CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024123305
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2009-12-11
Filing Date
2024-07-30
Publication Date
2024-10-07
Estimated Expiration
2030-12-09

AI Technical Summary

Technical Problem

Existing CMOS circuits face challenges in reducing standby power consumption due to high leakage currents in switching transistors, which become significant in miniaturized MOS transistors, leading to increased electricity consumption and potential thermal issues.

Method used

The use of highly purified oxide semiconductors, particularly In-Ga-Zn-O-based materials, in switching transistors to minimize leakage currents, ensuring low off-state current and high on-state current drive capability, thereby reducing standby power.

Benefits of technology

This approach effectively suppresses standby power consumption to nearly zero levels, even in complex integrated circuits, maintaining proper operation and reducing overall power usage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138162000001_ABST
    Figure 2024138162000001_ABST
Patent Text Reader

Abstract

To provide a novel semiconductor device with sufficiently reduced standby power.SOLUTION: A semiconductor device comprises: a first power supply terminal; a second power supply terminal; a switching transistor using oxide semiconductor material; and an integrated circuit. The first power supply terminal and one of a source terminal and a drain terminal of the switching transistor are electrically connected with each other. The other of the source terminal and the drain terminal of the switching transistor and one of terminals of the integrated circuit are electrically connected with each other. The other one of the terminals of the integrated circuit and the second power supply terminal are electrically connected with each other.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The technical field of the disclosed invention relates to a semiconductor device including an oxide semiconductor. A semiconductor device generally refers to any device that functions by utilizing semiconductor properties. Semiconductor elements such as transistors, diodes, and thyristors (including so-called power devices) (including image sensors, memories, converters, and other integrated circuits; integrated circuits including these; liquid crystal displays, Display devices, such as liquid crystal display devices, are broadly included in the category of semiconductor devices. [Background technology]

[0002] CMOS circuits consume little power, are capable of high-speed operation, and can be highly integrated. Due to these characteristics, it is an essential component of semiconductor integrated circuits. With the miniaturization of MOS transistors, leakage current (off-state current, subthreshold voltage The power consumption during non-operation (standby power consumption, hereafter referred to as standby power consumption) caused by the increase in For example, the increase in the channel length to less than 0.1 μm has become a problem. In miniaturized silicon MOS transistors, the gate-source potential is set to a value lower than the threshold voltage. Even if the drain current is reduced, it is not possible to make the drain current zero.

[0003] In order to suppress the increase in standby power caused by the leakage current as described above, A technique using a transistor has been proposed (see, for example, Patent Document 1). This technology uses a switch between the power supply and the CMOS circuit, which has a smaller leakage current than the CMOS circuit. A switching transistor is provided, and when the CMOS circuit is not in operation, the switching transistor is turned on. The aim is to reduce standby power consumption by turning off the starter. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 5-210976 Summary of the Invention [Problem to be solved by the invention]

[0005] In the technology disclosed in Patent Document 1, standby power is the leakage current of a switching transistor. In other words, the leakage current of the switching transistor must be kept small enough. This allows standby power consumption to be sufficiently reduced.

[0006] On the other hand, to ensure proper operation of the CMOS circuit, it is necessary to have sufficient For this reason, a switching transistor such as that disclosed in Patent Document 1 is required. When a transistor is provided, it is necessary to supply sufficient current to the CMOS circuit to ensure its operation. In order to achieve this, the channel width of the switching transistor is set to the Therefore, it becomes necessary to make the width of the signal line equal to or larger than the channel width of the star.

[0007] For the above reasons, the channel width of the switching transistor is set to 1. The transistor channel width is made smaller to prevent leakage current from the switching transistor itself. It is not a realistic way to suppress it.

[0008] In this way, the technology disclosed in Patent Document 1 makes the standby power consumption of the CMOS circuit substantially zero. For this reason, in an integrated circuit that is made up of a large number of circuits, In the case of an integrated circuit, the small standby power consumption of each circuit is accumulated to become a large standby power consumption. There may be a problem with the

[0009] In view of the above problems, the object of the present invention is to provide a new semiconductor device that sufficiently reduces standby power consumption. It shall be one. [Means for solving the problem]

[0010] In the disclosed invention, a semiconductor device (e.g., a transistor) is manufactured using a highly purified oxide semiconductor. A transistor using a highly purified oxide semiconductor has a Since the transistor current is extremely small, it is possible to sufficiently increase the on-off ratio. Even if the current drive capacity of the transistor is sufficiently secured, the leakage current cannot be suppressed to an extremely low level. It is possible.

[0011] By using the oxide semiconductor as described above in the following configuration, the standby power of the semiconductor device can be reduced. It is possible to sufficiently suppress it.

[0012] For example, one embodiment of the disclosed invention is a semiconductor device including a first power supply terminal, a second power supply terminal, and an oxide semiconductor. a switching transistor using the material and an integrated circuit, One of the source terminal and the drain terminal of the switching transistor is electrically connected The other of the source terminal or the drain terminal of the switching transistor and the integrated One of the terminals of the circuit is electrically connected to the other terminal of the integrated circuit and the second power supply terminal are electrically connected semiconductor devices.

[0013] Another embodiment of the disclosed invention is a semiconductor device including a first power supply terminal, a second power supply terminal, and an oxide semiconductor a switching transistor having a first control terminal and a second control terminal, the switching transistor being made of a dielectric material; an integrated circuit, the first power supply terminal and a source terminal of the switching transistor One of the drain terminals of the switching transistor is electrically connected to the source terminal of the switching transistor. The other of the terminals or the drain terminal is electrically connected to one of the terminals of the integrated circuit. The other terminal of the circuit is electrically connected to the second power supply terminal of the semiconductor device.

[0014] The switching transistor includes an oxide semiconductor layer made of an oxide semiconductor material and an oxide semiconductor A gate electrode that applies an electric field to the conductor layer, and a gate insulating layer between the oxide semiconductor layer and the gate electrode. and a source electrode and a drain electrode electrically connected to the oxide semiconductor layer. Also, a gate electrode for controlling the threshold voltage of the switching transistor may be provided. Here, the gate electrode is an electrode corresponding to a control terminal, and the source electrode is a The drain electrode is an electrode that corresponds to a drain terminal. As long as the circuit operation is not impeded, the various electrodes and the various terminals do not have to be the same. For example, if there is some element ( Wiring, switching elements, resistor elements, inductors, capacitors, and other various functions In some cases, elements such as

[0015] The oxide semiconductor material may be an In-Ga-Zn-O-based oxide semiconductor material. stomach.

[0016] In addition, the leakage current of the switching transistor is 1×10 -13 A or less can.

[0017] The integrated circuit may be formed using a semiconductor material other than an oxide semiconductor material. The semiconductor material other than the oxide semiconductor material may be silicon.

[0018] Additionally, integrated circuits include CMOS circuits.

[0019] In this specification, the terms "above" and "below" refer to the positional relationship of a component. For example, the term "gate electrode on a gate insulating layer" does not necessarily mean "directly under" the gate insulating layer. If the expression "gate electrode" is used, it excludes those that include other components between the gate insulating layer and the gate electrode. In addition, the terms "upper" and "lower" are merely used for the convenience of explanation, and Unless otherwise stated, this also includes reversed versions.

[0020] In addition, the terms "electrode" and "wiring" used in this specification refer to these components functionally. This is not intended to be limiting. For example, an "electrode" may be used as a part of a "wire." , and vice versa. Furthermore, the terms "electrode" and "wiring" are used interchangeably to refer to the plural "electrodes". This also includes cases where the "wiring" is formed integrally.

[0021] In addition, the functions of the "source" and "drain" may differ depending on whether transistors of different polarities are used or not. However, they may be swapped when the direction of the current changes during circuit operation. In this specification, the terms "source" and "drain" are used interchangeably. It is assumed that this is possible.

[0022] In this specification, "electrically connected" means "something that has some electrical effect." This includes cases where the device is connected via a wire. is not subject to any particular restriction as long as it enables transmission of electrical signals between connected objects.

[0023] For example, "things that have some kind of electrical function" include electrodes, wiring, and transistors. These include switching elements, resistor elements, inductors, capacitors, and other various functions. This includes elements such as Effect of the Invention

[0024] In the disclosed invention, a highly purified oxide semiconductor is used for a semiconductor device. Hydrogen in the oxide semiconductor is removed from the oxide semiconductor layer as much as possible, or Supplying oxygen to the body and filling the energy gap caused by oxygen deficiency in oxide semiconductors and reducing the defect level in the semiconductor.

[0025] The above-mentioned purification is performed in order to make the oxide semiconductor layer intrinsic (i-type). Since nitride semiconductors are generally n-type, transistors made using them tend to have leakage current In one embodiment of the disclosed invention, in order to sufficiently reduce the leakage current, The compound semiconductor is highly purified to become i-type or close to it.

[0026] A semiconductor device is manufactured by using the oxide semiconductor highly purified as described above as at least a part of the semiconductor device. By configuring the above, a semiconductor device that sufficiently suppresses standby power consumption can be realized. It can be said that the effect of power reduction becomes greater as the circuit becomes more complex. [Brief description of the drawings]

[0027] [Figure 1] FIG. 1 is a circuit diagram of an example of a semiconductor device. [Diagram 2] 1A and 1B are a cross-sectional view and a plan view of an example of a semiconductor device. [Diagram 3] 1A to 1C are cross-sectional views relating to a manufacturing process of a semiconductor device. [Figure 4] 1A to 1C are cross-sectional views relating to a manufacturing process of a semiconductor device. [Diagram 5] 1A to 1C are cross-sectional views relating to a manufacturing process of a semiconductor device. [Figure 6] FIG. 1 is a circuit diagram of an example of a semiconductor device. [Figure 7] FIG. 1 is a cross-sectional view of an example of a semiconductor device. [Figure 8] FIG. 1 is a block diagram illustrating an example of a semiconductor device. [Figure 9] 1A to 1C are cross-sectional views relating to a manufacturing process of a semiconductor device. [Figure 10] 1A to 1C are cross-sectional views relating to a manufacturing process of a semiconductor device. [Figure 11] 1A to 1C are diagrams for explaining electronic devices. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] The embodiments of the present invention will be described below with reference to the drawings. However, the present invention is not limited to the following description. The present invention is not limited to the above, and may be modified in various forms and details without departing from the spirit and scope of the present invention. It will be easily understood by those skilled in the art that the above-mentioned invention can be obtained by the following embodiments. It should not be construed as being limited to the contents described.

[0029] In addition, the position, size, range, etc. of each component shown in the drawings are not necessarily shown in order to facilitate understanding. The actual position, size, range, etc. may not be shown. The present invention is not necessarily limited to the positions, sizes, ranges, etc. disclosed in the drawings.

[0030] In this specification, ordinal numbers such as "first," "second," and "third" are used to avoid confusion of components. It should be noted that the numbers are added to avoid any unnecessary errors and are not intended to limit the number of errors.

[0031] (Embodiment 1) In this embodiment, a structure and a manufacturing method of a semiconductor device according to one embodiment of the disclosed invention will be described. 1 to 5. Note that in the circuit diagrams, To indicate that it is a transistor, the symbol OS may also be added.

[0032] <Circuit Configuration and Operation of Semiconductor Device> FIG. 1 shows an example of a circuit configuration of a semiconductor device. FIG. 1(A) shows the simplest CMOS circuit. FIG. 1(B) shows an example of a semiconductor device using a CMOS inverter circuit. 1 is an example of a semiconductor device having a plurality of inverter circuits.

[0033] The semiconductor device shown in FIG. 1A includes a power supply terminal VH, a power supply terminal VL, and a The switching transistor S1 and the CMOS inverter circuit C1 are used. The switching transistor S1 is typically an n-channel transistor using an oxide semiconductor. A high potential is supplied to the power supply terminal VH, and a low potential is supplied to the power supply terminal VL. do.

[0034] Here, the power supply terminal VH and the solenoid of the p-channel transistor of the CMOS inverter circuit C1 The p-channel of the CMOS inverter circuit C1 is electrically connected to the source terminal. The drain terminal of the n-channel transistor of the CMOS inverter circuit C1 The drain terminal of the CMOS inverter circuit C1 is electrically connected to the output terminal OU In addition, the source of the n-channel transistor of the CMOS inverter circuit C1 is The drain terminal of the switching transistor S1 is electrically connected to the drain terminal of the switching transistor S2. In addition, the source terminal of the switching transistor S1 and the power supply terminal VL are electrically connected. The gate terminal of the p-channel transistor of the CMOS inverter circuit C1 is The gate terminal of the n-channel transistor of the CMOS inverter circuit C1 is electrically connected to and serves as the input terminal IN of the CMOS inverter circuit C1.

[0035] When the semiconductor device is in operation, a high potential is applied to the control terminal S_IN of the switching transistor S1. In this state, a high voltage is applied to the input terminal IN, and the switching transistor S1 turns on. When either high or low potential is input, high or low potential is generated depending on the potential. For example, when the potential input to the input terminal IN is high, In this case, the p-channel transistor of the CMOS inverter circuit C1 is turned off, and the Since the n-channel transistor of the inverter circuit C1 is turned on, The input terminal I When the potential input to N is low, the p-channel transistor of the CMOS inverter circuit C1 This causes the n-channel transistor in the CMOS inverter circuit C1 to turn off. Therefore, the CMOS inverter circuit C1 outputs a voltage corresponding to the potential supplied to the power supply terminal VH. It outputs a high voltage.

[0036] When the semiconductor device is not in operation, a low voltage is applied to the control terminal S_IN of the switching transistor S1. The switching transistor S1 is turned off. The current (leakage current) flowing through the CMOS inverter circuit C1 and the switching transistor Since it is controlled by the combined resistance of S1, the resistance of the switching transistor S1 when it is off By sufficiently increasing the leakage current of the switching transistor S1, This allows the power consumption during non-operation (standby power consumption, hereafter also referred to as standby power) to be sufficiently small. It is possible.

[0037] A transistor using an oxide semiconductor material has an extremely low off-state current. For example, in a fully intrinsic (i-type) oxide semiconductor, the carrier density is, for example, , 1×10 12 / cm 3 Less than 1.45×10 10 / cm 3 Less than For example, when the drain voltage Vd is +1 V or +10 V, the off-current of the transistor is Therefore, when the gate voltage Vg is in the range of -5V to -20V, -13 It will be A or below. Therefore, by configuring the switching transistor S1 using an oxide semiconductor, It is possible to sufficiently reduce the leakage current of the semiconductor device. When using a compound semiconductor, the leakage current at room temperature is set to 1×10 -20 A(10zA(Zepto Ampere) to 1 × 10 -19 A (100zA). That is, it is even possible to make the leakage current substantially zero. Even if the channel width of the transistor S1 is relatively large, the magnitude of the leakage current does not change. That is, a transistor using an oxide semiconductor material does not have sufficient current driving capability. It is possible to suppress leakage current while ensuring a sufficient power, and reduce power consumption of the semiconductor device.

[0038] The semiconductor device shown in FIG. 1B is a semiconductor device shown in FIG. 1A, in which a CMOS inverter is added. The inverter circuit C1 is replaced with a plurality of CMOS inverter circuits C1 to Cn. do.

[0039] That is, the semiconductor device shown in FIG. 1B includes a power supply terminal VH, a power supply terminal VL, and an oxide semiconductor A switching transistor S1 using a conductive material and CMOS inverter circuits C1 to Cn (also simply referred to as an integrated circuit). Each CMOS inverter circuit is The input terminals I1 to In and the output terminals O1 to On are connected as follows: The difference from FIG. 1(A) is that the multiple CMOS inverter circuits C1 to Cn are connected in parallel, and each CMOS inverter circuit is connected to the power supply terminal VH and the switch The switching transistor S1 is connected to the multiple CMOS inverter circuits C If the circuit in which 1 to Cn are connected in parallel is considered as one integrated circuit, the switching transistor S The drain terminal of the first transistor is electrically connected to one of the terminals of the integrated circuit, and the other terminal of the integrated circuit is electrically connected to the drain terminal of the first transistor. It can also be said that the power supply terminal VH is electrically connected to the power supply terminal VL.

[0040] The operation of the above circuit is the same as that of FIG. 1(A). However, each input terminal has At the point where a potential is input to the output terminal and a corresponding potential is output from the output terminal, ) is different from

[0041] As described above, the present invention uses an oxide semiconductor, particularly a highly purified oxide semiconductor, at least in part. By configuring the semiconductor device in this way, a semiconductor device in which standby power consumption is sufficiently suppressed can be realized. Previous technology has made it possible to ensure proper operation of a semiconductor device while reducing leakage current to essentially zero. degree (e.g. 1×10 -13 It was difficult to reduce the amount of the In this respect, the disclosed invention is excellent. In particular, in a circuit in which many circuits are integrated and complicated, Even if the standby power consumption of each circuit is small, the total amount becomes large. The effect of reducing standby power consumption to a level that can be called substantially zero is achieved by the circuit This tendency becomes more pronounced as the circuit becomes more integrated and complex.

[0042] Although an example of a semiconductor device using a CMOS inverter circuit has been described here, One aspect of the disclosed invention is not limited to this. One aspect of the disclosed invention is consumption during non-operation. It can be used for any circuit (integrated circuit) where power is an issue. .

[0043] The above explanation is for the case where an n-channel switching transistor S1 is used. However, a p-channel transistor is used for the switching transistor S1. In this case, for example, the switching transistor S1 may be It is preferable to electrically connect the transistor to a p-channel type transistor of the OS inverter circuit.

[0044] <Plane and cross-sectional configurations of semiconductor device> FIG. 2 is a diagram showing an example of the configuration of the semiconductor device shown in FIG. FIG. 2(A) shows a cross section of the semiconductor device, and FIG. 2(B) shows a plan view of the semiconductor device. , which corresponds to the cross section taken along the line A1-A2-A3 in FIG. 2(B). The semiconductor device shown in FIG. 1 includes a transistor 160 ( The transistor that constitutes the CMOS inverter circuit C1 is made of an oxide semiconductor. A transistor 162 (a transistor that functions as a switching transistor S1) The transistor 160 and the transistor 162 each have The explanation will be given assuming that the transistor is an n-channel type, but the CMOS inverter circuit has a p It goes without saying that a channel type transistor is also used. The technical idea of ​​the invention is to switch transistors using oxide semiconductors in order to reduce power consumption. Since the purpose of the present invention is to use the semiconductor device as a switching transistor, the specific configuration of the semiconductor device is shown here. There is no need to limit it to anything.

[0045] The transistor 160 includes a channel forming region 11 provided in a substrate 100 including a semiconductor material. 6, and the impurity region 114 and the high concentration impurity region 115 are provided so as to sandwich the channel forming region 116. A pure region 120 (collectively referred to as an impurity region) and a channel forming region 11 6, and a gate electrode provided on the gate insulating layer 108. 110 and a source or drain electrode 130a electrically connected to the impurity region 114. , and a source or drain electrode 130b.

[0046] Here, a sidewall insulating layer 118 is provided on the side surface of the gate electrode 110. In addition, in the region of the substrate 100 that does not overlap with the sidewall insulating layer 118 in a plan view, A high concentration impurity region 120 is provided on the substrate 100, and a metal compound region 124 is provided on the high concentration impurity region 120. In addition, an element isolation insulating layer 106 is formed on the substrate 100 so as to surround the transistor 160. , and an interlayer insulating layer 126 and an interlayer insulating A source or drain electrode 130a, a source electrode or The drain electrode 130b is formed through an opening formed in the interlayer insulating layer 126 and the interlayer insulating layer 128. That is, the source electrode or the drain electrode is electrically connected to the metal compound region 124. The source or drain electrode 130a and the source or drain electrode 130b are formed on the metal compound region 124. The semiconductor laser 100 is electrically connected to the high concentration impurity region 120 and the impurity region 114 via the junction.

[0047] The transistor 162 includes a gate electrode 136c provided on the interlayer insulating layer 128 and a gate A gate insulating layer 138 is provided on the electrode 136c. An oxide semiconductor layer 140 and a second insulating film provided on the oxide semiconductor layer 140. A source electrode or drain electrode 142a, which is electrically connected to the source electrode or drain electrode 142b, and an in-electrode 142b.

[0048] Here, the gate electrode 136c is embedded in the insulating layer 132 formed on the interlayer insulating layer 128. Similarly to the gate electrode 136c, the source electrode An electrode 136a is in contact with the drain electrode 130a, and a source or drain electrode 130b is in contact with the drain electrode 130b. Electrodes 136b are formed in contact with the respective electrodes 136a and 136b.

[0049] In addition, a protective layer is provided on the transistor 162 so as to be in contact with part of the oxide semiconductor layer 140. An insulating layer 144 is provided, and an interlayer insulating layer 146 is provided on the protective insulating layer 144. Here, the protective insulating layer 144 and the interlayer insulating layer 146 are provided with a source electrode or a drain electrode. The openings reach the source electrode 142a and the source or drain electrode 142b. Through the opening, the electrode 150c and the electrode 150d are connected to the source electrode or the drain electrode. The electrode 142a is formed in contact with the source electrode or the drain electrode 142b. As well as the electrode 150c and electrode 150d, the gate insulating layer 138, the protective insulating layer 144, the interlayer insulating An electrode 150a contacts the electrodes 136a and 136b through an opening in the layer 146. , electrode 150b is formed.

[0050] Here, the oxide semiconductor layer 140 is a layer in which impurities such as hydrogen have been sufficiently removed or in which there is sufficient oxidation. It is preferable that the raw material is highly purified by supplying the raw material. The hydrogen concentration in the oxide semiconductor layer 140 is 5×10 19 atoms / cm 3 The following is preferable: 5×10 18 atoms / cm 3 Less than or equal to 5×10 17 atoms / cm 3 The hydrogen concentration is sufficiently reduced to achieve high purification, and sufficient oxygen is supplied to prevent oxygen deficiency. In the oxide semiconductor layer 140 in which the defect levels in the energy gap caused by the deficiency are reduced, Carrier concentration is 1×10 12 / cm 3 Less than 1×10 11 / cm 3 Less than, More preferably 1.45 x 10 10 / cm3 For example, if the drain voltage Vd is +1 When the gate voltage Vg is in the range of -5V to -20V, the on-state current The current is 1×10 -13 The off-resistance is 1×10 9 Ω·m or more, desired Or 1×10 10 In this way, the intrinsic (i-type) or substantially intrinsic By using a functionalized oxide semiconductor, a transistor with excellent off-state current characteristics was developed. The hydrogen concentration in the oxide semiconductor layer 140 can be calculated by the secondary ion Secondary ion mass spectrometry (SIMS) py).

[0051] An insulating layer 152 is provided on the interlayer insulating layer 146, and a buried insulating film is formed in the insulating layer 152. Electrodes 154a, 154b, and 154c are provided so that the electrodes 154a, 154b, and 154c are embedded in the liquid. Electrode 154a is in contact with electrode 150a, electrode 154b is in contact with electrode 150b and electrode 1 Electrode 154c contacts electrode 150d.

[0052] That is, in the semiconductor device shown in FIG. The source electrode 130b and the source or drain electrode 142a of the transistor 162 are Electrically connected via electrodes 136b, 150b, 154b and 150c It is being done.

[0053] <Method for Manufacturing Semiconductor Device> Next, an example of a method for manufacturing the above semiconductor device will be described. A method for fabricating the transistor 160 will be described with reference to FIG. A method for producing the heater 162 will be described with reference to FIGS.

[0054] <Method of manufacturing the lower transistor> First, a substrate 100 containing a semiconductor material is prepared (see FIG. 3(A)). The plate 100 may be a single crystal semiconductor substrate such as silicon or silicon carbide, or a polycrystalline semiconductor substrate. Compound semiconductor substrates such as silicon germanium, SOI substrates, etc. can be used. Here, a single crystal silicon substrate is used as the substrate 100 containing a semiconductor material. In general, an "SOI substrate" is a substrate that has a silicon semiconductor on an insulating surface. A substrate having a conductor layer formed thereon is referred to as a substrate having a silicon layer formed on an insulating surface. The term "substrate" is used as a concept including a substrate having a semiconductor layer made of a material other than silicon. The semiconductor layer of the "SOI substrate" is not limited to a silicon semiconductor layer. The substrate is a structure in which a semiconductor layer is provided on an insulating substrate such as a glass substrate via an insulating layer. This includes the following:

[0055] A protective layer 102 is formed on the substrate 100 to serve as a mask for forming an element isolation insulating layer. (See FIG. 3(A)). The protective layer 102 is made of, for example, silicon oxide, silicon nitride, An insulating layer made of silicon oxynitride or the like can be used. In order to control the threshold voltage of a transistor, an impurity that imparts n-type conductivity is added. The substrate 100 may be doped with an element or an impurity element that imparts p-type conductivity. In the case of a capacitor, impurities that give it n-type conductivity include, for example, phosphorus and arsenic. In addition, examples of impurities that impart p-type conductivity include boron and aluminum. Umium, gallium, etc. can be used.

[0056] Next, etching is performed using the protective layer 102 as a mask, and the The part of the substrate 100 in the area where the semiconductor device is not attached (the exposed area) is removed. The conductor region 104 is formed (see FIG. 3(B)). It is preferable to use an etching gas or an etchant, but wet etching may also be used. The etching liquid can be appropriately selected depending on the material to be etched.

[0057] Next, an insulating layer is formed so as to cover the semiconductor region 104, and a region overlapping the semiconductor region 104 is The insulating layer is selectively removed to form an element isolation insulating layer 106 (see FIG. 3(B)). The insulating layer is formed using silicon oxide, silicon nitride, silicon oxynitride, etc. Methods for removing the insulating layer include polishing such as CMP and etching. Either of them may be used. After the semiconductor region 104 is formed or after the element isolation insulating layer After the formation of 106, the protective layer 102 is removed.

[0058] Next, an insulating layer is formed on the semiconductor region 104, and a layer containing a conductive material is formed on the insulating layer. do.

[0059] The insulating layer will later become the gate insulating layer and is obtained using a method such as CVD or sputtering. Silicon oxide, silicon oxynitride, silicon nitride, hafnium oxide, aluminum oxide, oxide It is preferable to use a single layer or a multilayer structure of a film containing tantalum chloride or the like. The surface of the semiconductor region 104 is oxidized or nitrided by thermal oxidation or heat treatment. An insulating layer may be formed. The high density plasma treatment may be performed using, for example, He, Ar, Kr, Xe, etc. This is done using a mixture of rare gases such as oxygen, nitrogen oxide, ammonia, nitrogen, and hydrogen. The thickness of the insulating layer is not particularly limited, but may be, for example, 1 nm or more and 100 nm or less. It can be below.

[0060] The layer containing a conductive material is a metal material such as aluminum, copper, titanium, tantalum, or tungsten. Also, the insulating layer can be formed using a semiconductor material such as polycrystalline silicon containing a conductive material. The method of formation is not particularly limited, and examples of the method include deposition, C Various film formation methods such as VD method, sputtering method, and spin coating method can be used. In this embodiment, an example of forming a layer containing a conductive material using a metal material will be described. This shall be shown.

[0061] Thereafter, the insulating layer and the layer containing the conductive material are selectively etched to form the gate insulating layer 108. Then, a gate electrode 110 is formed (see FIG. 3(C)).

[0062] Next, an insulating layer 112 is formed to cover the gate electrode 110 (see FIG. 3(C)). Phosphorus (P) or arsenic (As) is added to the conductive region 104 to form a shallow junction with the substrate 100. In this case, an impurity region 114 having a thickness of 100 nm is formed (see FIG. 3(C)). However, when forming a p-type transistor, Impurity elements such as boron (B) and aluminum (Al) may be added. By forming the gate insulating layer 108, a channel forming region 114 is formed below the gate insulating layer 108 of the semiconductor region 104. A region 116 is formed (see FIG. 3(C)). Here, the concentration of the added impurity is appropriately set. However, when semiconductor elements are highly miniaturized, the concentration can be increased. In this embodiment, the impurity region 114 is formed after the insulating layer 112 is formed. The process includes forming the insulating layer 112 after forming the impurity region 114. You can do that.

[0063] Next, a sidewall insulating layer 118 is formed (see FIG. 3(D)). The layer 118 is formed by forming an insulating layer to cover the insulating layer 112 and then applying a highly anisotropic By applying a simple etching process, the film can be formed in a self-aligned manner. Then, the insulating layer 112 is partially etched to expose the upper surface of the gate electrode 110 and the impurity region 1 It is a good idea to expose the top surface of 14.

[0064] Next, a semiconductor device is formed so as to cover the gate electrode 110, the impurity region 114, the sidewall insulating layer 118, etc. Then, an insulating layer is formed in the region where the insulating layer contacts the impurity region 114. By doping the silicon substrate with ions such as phosphorus (P) or arsenic (As), a high-concentration impurity region 120 is formed (see FIG. 3(E)). After that, the insulating layer is removed, and the gate electrode 110, the sidewall insulating layer 118, A metal layer 122 is formed so as to cover the high concentration impurity region 120 and the like (see FIG. 3(E)). The metal layer 122 is formed by using various film forming methods such as vacuum deposition, sputtering, and spin coating. The metal layer 122 can be formed by reacting with the semiconductor material that constitutes the semiconductor region 104. It is preferable to form the insulating layer using a metal material that reacts with the insulating layer to form a low-resistance metal compound. Examples of metal materials include titanium, tantalum, tungsten, nickel, cobalt, and white. There is gold etc.

[0065] Next, a heat treatment is performed to react the metal layer 122 with the semiconductor material. A metal compound region 124 is formed in contact with the high concentration impurity region 120 (see FIG. 3(F)). When polycrystalline silicon or the like is used as the gate electrode 110, the gate electrode 110 A metal compound region is also formed in the portion in contact with the metal layer 122.

[0066] The heat treatment may be, for example, a heat treatment by irradiation with a flash lamp. Of course, other heat treatment methods may be used, but the chemical reaction involved in the formation of metal compounds is In order to improve the controllability of the heat treatment, it is desirable to use a method that can realize a very short heat treatment. The metal compound region is preferably formed by a reaction between a metal material and a semiconductor material. The metal compound region is formed in the region, and the conductivity is sufficiently increased. This sufficiently reduces the electrical resistance and improves the device characteristics. After forming region 124, metal layer 122 is removed.

[0067] Next, an interlayer insulating layer 126 and an interlayer insulating layer 127 are formed to cover the respective components formed by the above-mentioned steps. The interlayer insulating layer 126 and the interlayer insulating layer 128 are formed by using silicon oxide. Silicon, silicon oxynitride, silicon nitride, hafnium oxide, aluminum oxide, tungsten oxide The insulating layer can be formed using a material containing an inorganic insulating material such as aluminum. It is also possible to form the insulating film by using an organic insulating material such as acrylic. Although the present embodiment has a two-layer structure of the layer 126 and the interlayer insulating layer 128, the configuration of the interlayer insulating layer is not limited to this. After the interlayer insulating layer 128 is formed, the surface is polished by CMP, etching, or the like. It is desirable to flatten the surface by

[0068] Thereafter, an opening is formed in the interlayer insulating layer so as to reach the metal compound region 124. A source electrode or drain electrode 130a and a source electrode or drain electrode 130b are provided on the The source electrode or drain electrode 130a and the source electrode or The drain electrode 130b is formed by, for example, depositing a layer on a region including an opening using a PVD method, a CVD method, or the like. After forming the conductive layer, a part of the conductive layer is removed by a method such as etching or CMP. It can be formed by removing

[0069] In addition, a part of the conductive layer is removed to form the source electrode or drain electrode 130a and the source electrode Alternatively, when forming the drain electrode 130b, the surface of the electrode is processed to be flat. For example, after forming a thin titanium film or titanium nitride film in the region including the opening, When a tungsten film is formed to fill the opening, the inclusions are removed by the subsequent CMP. The necessary tungsten film, titanium film, titanium nitride film, etc. are removed, and the flatness of the surface is improved. In this way, the source electrode or drain electrode 130a, By planarizing the surface including the source or drain electrode 130b, This makes it possible to form good electrodes, wiring, insulating layers, semiconductor layers, and the like.

[0070] In this case, the source electrode or drain electrode 130 in contact with the metal compound region 124 Although only the source electrode 130a or the drain electrode 130b is shown, in this process, An electrode in contact with the source electrode 110 may also be formed. The drain electrode 130a can be used as a source electrode or a drain electrode 130b. There is no particular limitation on the material, and various conductive materials can be used. For example, molybdenum Titanium, Chromium, Tantalum, Tungsten, Aluminum, Copper, Neodymium, Scandium For example, a conductive material such as aluminum can be used.

[0071] In this manner, a transistor 160 is formed using the substrate 100 containing a semiconductor material. After the above steps, electrodes, wiring, an insulating layer, etc. may be further formed. In addition, by adopting a multilayer wiring structure consisting of a laminated structure of interlayer insulating layers and conductive layers, Therefore, it is possible to provide a highly integrated semiconductor device.

[0072] <How to make the upper transistor> Next, referring to FIG. 4 and FIG. 5, a process for forming a transistor 162 on the interlayer insulating layer 128 will be described. 4 and 5 show various electrodes and transistors on the interlayer insulating layer 128. Since the figure shows the manufacturing process of the transistor 162, the The transistor 160 and other components that correspond to it are omitted.

[0073] First, an interlayer insulating layer 128, a source electrode or drain electrode 130a, An insulating layer 132 is formed on the drain electrode 130b (see FIG. 4(A)). It can be formed by using a VD method, a CVD method, or the like. Inorganic insulating materials such as silicon nitride, hafnium oxide, aluminum oxide, and tantalum oxide The material may be formed using a material containing the metal.

[0074] Next, the source or drain electrode 130a, the source or An opening is formed that reaches the drain electrode 130b. At this time, the gate electrode 136c is An opening is also formed in the region where the conductive layer is to be formed. 134 is formed (see FIG. 4(B)). The opening is formed by a method such as etching using a mask. The mask can be formed by a method such as exposure using a photomask. The etching method can be wet etching or dry etching. From the viewpoint of fine processing, however, it is preferable to use dry etching. The conductive layer 134 can be formed by a film forming method such as a PVD method or a CVD method. Materials that can be used to form the conductive layer 134 include molybdenum, titanium, Conductors such as chromium, tantalum, tungsten, aluminum, copper, neodymium, and scandium Examples of the conductive materials include conductive materials, alloys thereof, and compounds (eg, nitrides).

[0075] More specifically, for example, a thin titanium film is formed by PVD in the area including the opening, and then CV After forming a thin titanium nitride film by the D method, a tungsten film is formed to fill the opening. Here, the titanium film formed by the PVD method is The oxide film (such as the native oxide film) on the formation surface is reduced, and the lower electrode (here, the source electrode or drain electrode) is The contact resistance between the electrode and the source or drain electrode (e.g., the source electrode 130a, the source electrode or the drain electrode 130b, etc.) is reduced. In addition, the titanium nitride film formed afterwards suppresses the diffusion of the conductive material. In addition, after forming a barrier film made of titanium or titanium nitride, A copper film may be formed on the conductive layer by plating.

[0076] After the conductive layer 134 is formed, the conductive layer 134 is etched or CMP is performed. 34 is removed to expose the insulating layer 132, and the electrodes 136a, 136b, and the gate An electrode 136c is formed (see FIG. 4C). Note that a part of the conductive layer 134 is removed. When the electrodes 136a, 136b, and gate electrode 136c are formed, the surfaces are flattened. In this manner, the insulating layer 132, the electrode 136a, the electrode 136 b. By planarizing the surface of the gate electrode 136c, a good electrode can be obtained in a later process. It becomes possible to form wiring, insulating layers, semiconductor layers, and the like.

[0077] Next, the insulating layer 132, the electrode 136a, the electrode 136b, and the gate electrode 136c are covered with A gate insulating layer 138 is formed (see FIG. 4(D)). The gate insulating layer 138 is formed by a CVD method or the like. The gate insulating layer 138 can be formed by a sputtering method or the like. Silicon nitride, silicon oxynitride, aluminum oxide, hafnium oxide, tantalum oxide It is preferable that the gate insulating layer 138 is formed to include a single layer structure. The thickness of the gate insulating layer 138 is not particularly limited, but For example, the thickness can be set to 10 nm or more and 500 nm or less. In the case of a laminated structure, for example, A first gate insulating layer having a thickness of 50 nm to 200 nm, and a film thickness on the first gate insulating layer It is preferable to laminate the second gate insulating layer with a thickness of 5 nm to 300 nm.

[0078] Note that an oxide semiconductor (high Since the purified oxide semiconductor is extremely sensitive to the interface states and the interface charges, When using such an oxide semiconductor for the oxide semiconductor layer, the interface with the gate insulating layer is important. Therefore, the gate insulating layer 138 in contact with the highly purified oxide semiconductor layer has a high This will require higher quality.

[0079] For example, the high-density plasma CVD method using microwaves (2.45 GHz) produces dense, high-insulation-voltage This is advantageous in that a high quality gate insulating layer 138 can be formed. The intimate contact between the conductor layer and the high-quality gate insulating layer reduces the interface state and improves the interface characteristics. Because it can be made to be a good thing.

[0080] Of course, if it can form a good insulating layer as a gate insulating layer, highly purified Even when an oxide semiconductor layer is used, other methods such as sputtering and plasma CVD are used. In addition, the film quality and the interface with the oxide semiconductor layer can be improved by heat treatment after the formation. An insulating layer whose characteristics are modified may also be applied. In either case, the film quality is good and The gate insulating layer 138 capable of reducing the interface state with the oxide semiconductor layer may be formed.

[0081] Next, an oxide semiconductor layer is formed over the gate insulating layer 138 and etched using a mask. The oxide semiconductor layer is processed by a method such as the above to form an island-shaped oxide semiconductor layer 140. (See FIG. 4(E)).

[0082] The oxide semiconductor layer is preferably formed by a sputtering method. The In-Sn-Ga-Zn-O system, which is a binary metal oxide, and the In- Ga-Zn-O system, In-Sn-Zn-O system, In-Al-Zn-O system, Sn-Ga-Z nO system, Al-Ga-Zn-O system, Sn-Al-Zn-O system, and binary metal oxides. In-Zn-O series, Sn-Zn-O series, Al-Zn-O series, Zn-Mg-O series, Sn- Mg-O, In-Mg-O, and single-element metal oxides such as In-O, Sn-O, and Z The film can be formed using a metal oxide such as nO. For example, a target containing 2% to 10% by weight of SiO2 may be used. A semiconductor layer may be formed.

[0083] In particular, by using In-Ga-Zn-O metal oxides, the resistance in the absence of an electric field is sufficiently low. To provide a semiconductor device having a sufficiently high off-state current and a sufficiently low field-effect mobility, Therefore, the In-Ga-Zn-O metal oxide is suitable for semiconductor devices. It is suitable as a semiconductor material to be used.

[0084] A representative example of In-Ga-Zn-O metal oxide is InGaO3(ZnO). m (m >0). Also, M is used instead of Ga, resulting in InMO3(ZnO). m There are metal oxides that are written as (m>0), where M is gallium (Ga), Aluminum (Al), Iron (Fe), Nickel (Ni), Manganese (Mn), Cobalt (C) o) represents one or more metal elements selected from the following. For example, M is Ga, Ga and Al, Ga and Fe, Ga and Ni, Ga and Mn, Ga and Co, etc. can be applied. Note that the above composition is derived from the crystal structure. However, it should be noted that this is merely one example.

[0085] In this embodiment, the oxide semiconductor layer is formed using an In-Ga-Zn-O oxide semiconductor film forming tube. The film is formed by sputtering using a target.

[0086] The oxide semiconductor layer is formed by holding a substrate in a treatment chamber that is kept in a reduced pressure state and controlling the substrate temperature to The temperature is preferably 100°C or higher and 600°C or lower, and more preferably 200°C or higher and 400°C or lower. Here, the oxide semiconductor layer is formed while the substrate is heated, so that the oxide semiconductor The impurity concentration in the oxide semiconductor layer can be reduced, and damage to the oxide semiconductor layer caused by sputtering can be prevented. can be alleviated.

[0087] Then, the remaining moisture in the processing chamber is removed and a sputtering gas from which hydrogen, water, etc. have been removed is introduced. The oxide semiconductor layer is formed in a deposition atmosphere using a metal oxide as a target. The atmosphere may be a rare gas (typically argon) atmosphere, an oxygen atmosphere, or a rare gas (typically It is preferable to use a mixed atmosphere of oxygen and hydrogen (e.g., argon). The concentration of impurities such as water, hydroxyl groups, and hydrides is on the order of several ppm (preferably on the order of several ppb). It is preferable to use a high-purity gas atmosphere in which even the smallest amount of oxygen has been removed.

[0088] In order to remove the residual moisture in the processing chamber, it is preferable to use an adsorption type vacuum pump. For example, a cryopump, an ion pump, or a titanium sublimation pump is used. The exhaust means is a turbo pump with a cold trap. The deposition chamber evacuated using a cryopump may be filled with, for example, hydrogen atoms, water ( Compounds containing hydrogen atoms (and more preferably compounds containing carbon atoms) such as HO are exhausted. Therefore, the concentration of impurities in the oxide semiconductor layer formed in the deposition chamber can be reduced. .

[0089] The thickness of the oxide semiconductor layer is 2 nm to 200 nm, preferably 5 nm to 30 nm. The appropriate thickness of the oxide semiconductor film varies depending on the oxide semiconductor material used. Therefore, the thickness may be appropriately selected depending on the material used.

[0090] In addition, by using a pulsed direct current (DC) power supply in the deposition of the oxide semiconductor layer, the deposition This reduces the amount of powdery material (also called particles or dust) that sometimes occurs, and also ensures uniform film thickness distribution. It can be said that:

[0091] The sputtering conditions for the oxide semiconductor layer are, for example, Distance: 170 mm, pressure: 0.4 Pa, DC power: 0.5 kW, atmosphere: oxygen ( The conditions that can be applied are an atmosphere with a flow rate of 100% oxygen.

[0092] Before forming the oxide semiconductor layer by sputtering, argon gas was introduced to the plasma A reverse sputtering process is performed to generate a smear, and dust adhering to the surface of the gate insulating layer 138 is removed. Here, the reverse sputtering is a method of removing the sputtering. Instead of bombarding the target with ions, the treatment surface is bombarded with ions. The method of modifying the surface by bombarding the surface with ions is as follows: A high-frequency voltage is applied to the processing surface side in an argon atmosphere to generate plasma near the substrate. In addition, the argon atmosphere can be replaced by a nitrogen atmosphere, a helium atmosphere, or an oxygen atmosphere. An atmosphere or the like may also be used.

[0093] The etching of the oxide semiconductor layer can be performed by either dry etching or wet etching. Of course, both can be used in combination. In order to match the etching conditions (etching gas, etching solution, etc.) to the material, The etching time, temperature, etc. may be appropriately set.

[0094] The etching gas used in dry etching is, for example, a gas containing chlorine (chlorine-based gas, For example, chlorine (Cl2), boron trichloride (BCl3), silicon tetrachloride (SiCl4), carbon tetrachloride In addition, gases containing fluorine (fluorine-based gases, for example, tetrafluoroethylene (CCl4)) Carbon fluoride (CF4), sulfur hexafluoride (SF6), nitrogen trifluoride (NF3), trifluoromethane (CHF3), hydrogen bromide (HBr), oxygen (O2), and helium (H e) or a gas containing a rare gas such as argon (Ar), etc. may also be used.

[0095] As a dry etching method, parallel plate type RIE (Reactive Ion Etch) ing method and ICP (Inductively Coupled Plasma) A method of etching a silicon wafer using a plasma-coupled plasma (PPS) can be used. As shown in the figure, the etching conditions (the amount of power applied to the coil-shaped electrode, the amount of power applied to the electrode on the substrate side) The power consumption, electrode temperature on the substrate side, etc. are set appropriately.

[0096] The etching solution used for wet etching is a mixture of phosphoric acid, acetic acid, and nitric acid. Alternatively, an etching solution such as ITO07N (manufactured by Kanto Chemical Co., Ltd.) can be used. This is also fine.

[0097] Next, the oxide semiconductor layer is preferably subjected to a first heat treatment. The temperature of the first heat treatment can be set to The temperature is set to 300°C or higher and 750°C or lower, preferably 400°C or higher and 700°C or lower. The substrate is placed in an electric furnace using a heating element or the like, and the oxide semiconductor layer 140 is heated in a nitrogen atmosphere. A heat treatment is performed for 1 hour at 450° C. During this time, the oxide semiconductor layer 140 is not exposed to the air. Ensure that hydrogen (including water, etc.) is not re-mixed.

[0098] The heat treatment device is not limited to an electric furnace, and may be any device that uses heat conduction from a medium such as a heated gas, or It may be a device that heats the workpiece by thermal radiation. For example, LRTA (Lamp Rapid Thermal Annealing Equipment, GRTA (Gas Rapid RTA (Rapid Thermal Anneal) equipment etc. The LRTA device can be equipped with halogen lamps, metal halide lamps, etc. Lamps, xenon arc lamps, carbon arc lamps, high pressure sodium lamps, high pressure water A device that heats the workpiece by radiating light (electromagnetic waves) emitted from a lamp such as a silver lamp. The GRTA device is a device that performs heat treatment using high-temperature gas. An inert gas that does not react with the workpiece during heat treatment, such as a rare gas such as argon or nitrogen. A gas is used.

[0099] For example, in the first heat treatment, the substrate is immersed in an inert gas heated to a high temperature of 650° C. to 700° C. After heating for a few minutes, the substrate is taken out of the inert gas (GRTA process). GRTA treatment allows high-temperature heat treatment in a short time. Since this is a heat treatment, when using a substrate with low heat resistance such as a glass substrate, distortion of the substrate may occur. This makes it possible to apply the method even under temperature conditions exceeding the melting point.

[0100] The first heat treatment is performed in a vacuum chamber mainly containing nitrogen or a rare gas (helium, neon, argon, etc.). It is preferable to carry out the process in an atmosphere that does not contain hydrogen, water, etc. The purity of nitrogen or rare gas such as helium, neon, or argon introduced into the heat treatment device is 6N (99.9999%) or more, preferably 7N (99.99999%) or more (i.e. , the impurity concentration is 1 ppm or less, preferably 0.1 ppm or less.

[0101] Depending on the conditions of the first heat treatment or the material of the oxide semiconductor layer, the oxide semiconductor layer may be crystallized. In addition, the semiconductor layer may contain crystals. Depending on the material of the conductor layer, it may become an amorphous oxide semiconductor layer that does not contain crystalline components. .

[0102] In addition, by providing a crystal layer on an amorphous surface, the electrical characteristics of the oxide semiconductor layer are changed. For example, it is possible to form a crystal layer in which crystal grains having electrical anisotropy are oriented. By this, the electrical properties of the oxide semiconductor layer can be changed. Because of their shape, they are sometimes called plate crystals.

[0103] The first heat treatment for the oxide semiconductor layer 140 is performed to process the oxide semiconductor layer 140 into an island-shaped oxide semiconductor layer 140. In that case, the first heat treatment is performed on the oxide semiconductor layer. The substrate is then removed and subjected to a photolithography process.

[0104] Note that the first heat treatment has a dehydrogenation (dehydration) effect on the oxide semiconductor layer 140. This type of treatment can also be called dehydrogenation treatment (dehydration treatment). After the oxide semiconductor layer is formed, a source electrode or a drain electrode is laminated on the oxide semiconductor layer 140. After forming a protective insulating layer on the source electrode or drain electrode, In addition, such a process can be carried out not only once but multiple times. is also good.

[0105] In addition, by controlling the deposition atmosphere, it is possible to obtain an oxide semiconductor layer in which hydrogen is sufficiently reduced. In such a case, the first heat treatment may be omitted.

[0106] Next, a source electrode or drain electrode 142a, The source or drain electrode 142b is formed (see FIG. 4(F)). The drain electrode 142a and the source or drain electrode 142b are formed on the oxide semiconductor layer 1 After forming a conductive layer so as to cover 40, the conductive layer is selectively etched. Depending on the material and etching conditions, A part of the oxide semiconductor layer 140 is etched to form a groove (a recess). This can also happen.

[0107] The conductive layer is formed by using PVD methods such as sputtering and CVD methods such as plasma CVD. The conductive layer can be formed of a material such as aluminum, chromium, copper, Tantalum, titanium, molybdenum, tungsten, or any of the above elements. Manganese, magnesium, zirconium, beryllium, etc. can be used. Alternatively, one or more materials selected from the group consisting of aluminum, thorium, and aluminum alloy may be used. Titanium, tantalum, tungsten, molybdenum, chromium, neodymium, scandium Alternatively, a material containing a single element selected from the group consisting of aluminum and a combination of multiple elements may be used. It may have a single layer structure or a laminated structure of two or more layers. For example, Single-layer aluminum film structure, two-layer aluminum film with titanium film laminated on top, titanium and a three-layer structure in which a film, an aluminum film, and a titanium film are laminated.

[0108] The conductive layer may be formed using a conductive metal oxide. Indium oxide (In2O3), tin oxide (SnO2), zinc oxide (ZnO), Indium tin oxide alloy (In2O3-SnO2, sometimes abbreviated as ITO), oxide Indium zinc oxide alloy (In2O3-ZnO), or a combination of these metal oxide materials It is possible to use one containing silicon or silicon oxide.

[0109] The channel length (L) of the transistor is defined as the distance between the bottom end of the source or drain electrode 142a and the The distance between the bottom end of the source electrode or drain electrode 142b and the channel When exposure is performed with a length (L) of less than 25 nm, the wavelength is extremely low, ranging from a few nm to a few tens of nm. Extreme ultraviolet light with short length is used for etching. Exposure to extreme ultraviolet light provides high resolution and a large depth of focus. Therefore, the channel length (L) of the formed transistor is set to 10 nm or more and 1000 nm or less. It is also possible to increase the operating speed of the circuit and reduce power consumption. do.

[0110] After the above process, plasma treatment using gas such as N2O, N2, or Ar may be performed. It is preferable that the plasma treatment is performed on the exposed surface of the oxide semiconductor layer. Adherent water and other substances are removed. In addition, gases containing oxygen, such as a mixture of oxygen and argon, In this case, oxygen is supplied to the oxide semiconductor layer, and then a plasma treatment using a gas is performed. It is possible to reduce defect levels in the energy gap caused by oxygen deficiency.

[0111] Next, the protective insulating layer 14 in contact with a part of the oxide semiconductor layer 140 is removed without exposing it to the air. Form 4 (see Figure 4(G)).

[0112] The protective insulating layer 144 is formed by mixing impurities such as hydrogen and water into the protective insulating layer 144 using a method such as sputtering. The thickness of the layer is 1 nm or more. Materials that can be used for the protective insulating layer 144 include silicon oxide, silicon nitride, Silicon oxynitride and the like. The structure may be a single layer structure or a multilayer structure. The substrate temperature when forming the protective insulating layer 144 is set to be equal to or higher than room temperature and equal to or lower than 300° C. The atmosphere is preferably a rare gas (typically argon) atmosphere, an oxygen atmosphere, or a rare gas atmosphere. It is preferable to use a mixed atmosphere of nitrogen (typically argon) and oxygen.

[0113] If hydrogen is contained in the protective insulating layer 144, the hydrogen may penetrate into the oxide semiconductor layer 140 or may be decomposed by water. The oxygen in the oxide semiconductor layer 140 is extracted by the hydrogen, and the oxide semiconductor layer 140 The back channel side of the gate insulating film becomes low in resistance, and a parasitic channel may be formed. Therefore, in order to prevent the protective insulating layer 144 from containing hydrogen as much as possible, the method for forming the protective insulating layer 144 is carried out so as not to include hydrogen. It is preferable not to use it.

[0114] For example, when the protective insulating layer 144 is formed by sputtering, the sputtering gas is water. The concentration of impurities such as nitrogen, water, hydroxyl groups, and hydrides is on the order of several ppm (preferably on the order of several ppb). ) high-purity gas is used. Also, any residual moisture in the processing chamber must be removed. is desirable.

[0115] In this embodiment, an insulating layer containing silicon oxide is formed as the protective insulating layer 144 by a sputtering method. Thus, it is formed.

[0116] Then, a second heat treatment (preferably for 20 It is preferable to carry out the heating at a temperature between 0°C and 400°C, for example between 250°C and 350°C. The second heat treatment is performed at 250° C. for 1 hour in a nitrogen atmosphere. The second heat treatment can reduce the variation in the electrical characteristics of the transistors. Oxygen is supplied from the insulating layer containing oxygen to the oxide semiconductor layer, and energy due to oxygen deficiency is generated. It is also possible to reduce the defect level in the gap. However, the atmosphere may be air. In that case, the oxide semiconductor layer may be It is preferable to use an atmosphere that is free of hydrogen and water so that hydrogen is not mixed in. The heat treatment in step 2 is not an essential step and may be omitted.

[0117] Next, an interlayer insulating layer 146 is formed on the protective insulating layer 144 (see FIG. 5(A)). The edge layer 146 can be formed by using a PVD method, a CVD method, or the like. Silicon oxynitride, silicon nitride, hafnium oxide, aluminum oxide, tantalum oxide After the interlayer insulating layer 146 is formed, a material containing an inorganic insulating material such as SiO 2 can be used. In order to achieve this, it is desirable to flatten the surface by a method such as CMP or etching. stomach.

[0118] Next, an electrode 1 is formed on the interlayer insulating layer 146, the protective insulating layer 144, and the gate insulating layer 138. 36a, electrode 136b, source or drain electrode 142a, An opening is formed that reaches the inner electrode 142b, and the conductive layer 148 is formed so as to fill the opening. (See FIG. 5(B)). The opening is formed by a method such as etching using a mask. The mask can be formed by a method such as exposure using a photomask. Etching can be either wet etching or dry etching. However, from the viewpoint of fine processing, it is preferable to use dry etching. The material used for the conductive layer 148 and the method for forming the conductive layer 148 are the same as those for the conductive layer 134. Therefore, the description of the conductive layer 134 can be referred to.

[0119] After the conductive layer 148 is formed, the conductive layer 148 is etched or CMPed. Electrodes 150a, 150b, and 150c are then removed to expose the interlayer insulating layer 146. 50c, and an electrode 150d are formed (see FIG. 5(C)). When forming the electrodes 150a, 150b, 150c, and 150d by removing the It is desirable to process the surface so that it is flat. By flattening the surfaces of the electrodes 150a, 150b, 150c, and 150d, In the subsequent steps, it becomes possible to form good electrodes, wiring, insulating layers, semiconductor layers, etc. do.

[0120] Thereafter, an insulating layer 152 is formed, and the electrodes 150a, 150b, and 150c are attached to the insulating layer 152. 50c, an opening is formed that reaches the electrode 150d. After the conductive layer is formed, a part of the conductive layer is removed by a method such as etching or CMP to form an insulating layer. The edge layer 152 is exposed to form electrodes 154a, 154b, and 154c (FIG. 5). (D)). This process is the same as that for forming the electrodes 136a, 150a, etc. Therefore, details will be omitted.

[0121] In the case where the transistor 162 is manufactured by the above-described method, the hydrogen concentration in the oxide semiconductor layer 140 is Degree is 5 x 10 19 atoms / cm 3 Less than 5×10 18 atoms / cm 3 Less than or equal to 5×10 17 atoms / cm 3 The following is also true: The off current of 162 is 1×10 -13 A or less, and the off-resistance is 1×10 9 Ω m or more ( or 1×10 10 In this way, the hydrogen concentration is sufficiently reduced to produce a high-purity The oxide semiconductor is improved in that the defect level in the energy gap caused by oxygen deficiency is reduced. By using such a material, the transistor 162 can have excellent characteristics.

[0122] Note that in this embodiment, a transistor using a material other than an oxide semiconductor and a The semiconductor device having a stacked structure with a transistor using a semiconductor device has been described. The structure that can be clearly used is not limited to the laminated structure. A single layer structure may also be used. For example, an oxide semiconductor has a relatively high field-effect mobility. Therefore, semiconductor devices with a single-layer structure or a multilayer structure using only oxide semiconductors as semiconductor materials are In particular, when a crystalline oxide semiconductor is used, the field effect Mobility μ is μ>100cm 2 / V s is possible, and the semiconductor is made only of oxide semiconductors. The device is also realistic. In this case, a semiconductor is formed using a substrate such as a glass substrate. It is possible to form a device.

[0123] In addition, the arrangement and connection of electrodes (wiring), insulating layers, semiconductor layers, etc., wiring width, channel width, Various parameters such as channel length and other conditions are required for semiconductor integrated circuits. For example, the semiconductor device may be formed in a single layer structure. The configuration of electrodes, wiring, etc. in such a case is significantly different from that in the case of a laminated structure.

[0124] As described above, the configurations, methods, etc. described in this embodiment may be used in conjunction with the configurations, methods, etc. described in other embodiments. They can be used in any suitable combination.

[0125] (Embodiment 2) In this embodiment, a semiconductor device having a different configuration from the semiconductor device shown in the previous embodiment is used. The arrangement will be described with reference to FIG. 6 and FIG.

[0126] <Circuit Configuration and Operation of Semiconductor Device> FIG. 6 shows an example of a circuit configuration of a semiconductor device according to this embodiment. This is an example of a semiconductor device using a CMOS inverter circuit, which is a simple CMOS circuit. B) is an example of a semiconductor device having a plurality of CMOS inverter circuits.

[0127] The difference between the semiconductor device shown in FIG. 6 and the semiconductor device shown in FIG. 1 is that the semiconductor device shown in FIG. The difference between the two is whether the switching transistor S1 has a back gate or not. In this device, the switching transistor S1 has a back gate. By controlling the potential of the gate, the threshold voltage of the switching transistor S1 is controlled. This reduces the leakage current when the device is off to a level that can be said to be virtually zero. It becomes easier to control.

[0128] In this embodiment, as described above, the switching transistor S1 has a back gate. Therefore, there are two control terminals, control terminal S_IN_1 and control terminal S_IN_2. A high potential or a low potential is input to the control terminal S_IN_1 in the same manner as in the previous embodiment. The control terminal S_IN_ The potential input to 2 is set so that the threshold voltage of the switching transistor S1 becomes the desired value. There is no particular limitation as long as the potential is such that the potential is constant. A constant potential or a fluctuating potential may be input. Alternatively, a potential such as a ground potential may be used.

[0129] Other configurations and operations are the same as those shown in the previous embodiment. Omitted.

[0130] <Plane and cross-sectional configurations of semiconductor device> FIG. 7 is a cross-sectional view showing an example of the configuration of the semiconductor device shown in FIG. The device has a transistor 160 (CMOS inverter) using a material other than an oxide semiconductor in the lower part. The transistor that constitutes the data circuit C1 is a transistor using an oxide semiconductor on the upper part. 162 (a transistor that functions as a switching transistor S1). The semiconductor device shown in FIG. 2 and the semiconductor device shown in FIG. The difference between the semiconductor device is whether or not the semiconductor device has a gate electrode 145 in addition to the gate electrode 136c. Either way.

[0131] The details of each component are similar to those of the semiconductor device described in the previous embodiment. The gate electrode 145 provided on the insulating layer 144 in a region overlapping with the oxide semiconductor layer 140 is , has the function of generating an electric field for controlling the threshold voltage of the transistor 162 . This reduces the leakage current of the transistor 162 when it is off to a level that can be said to be substantially zero. In this case, the gate electrode 136c is used to suppress the transistor The gate electrode 145 controls the threshold voltage of the transistor 162 by switching it on and off. The protective insulating layer 14 is also preferably made of a fluorine-containing material. 4 also functions as a gate insulating layer.

[0132] The structures, methods, and the like described in this embodiment may be combined as appropriate with the structures, methods, and the like described in other embodiments. They can be used in combination.

[0133] (Embodiment 3) In this embodiment, an integrated semiconductor device which is another embodiment of the disclosed invention will be described. The following description will be given with reference to FIG.

[0134] FIG. 8 shows an integrated semiconductor device which is a modification of the semiconductor device shown in the previous embodiment (for example, embodiment 1). The semiconductor device 170 shown in FIG. 1 is a CP Examples include U and MPU.

[0135] The semiconductor device 170 includes a plurality of circuit blocks such as a circuit block 171 to a circuit block 174. Each circuit block is composed of a switching element 181, a switch The current is supplied to the semiconductor device 182 via an element that uses an oxide semiconductor at least in part. are electrically connected.

[0136] The circuit blocks 171 to 174 include, for example, the above-mentioned CMOS inverter circuit. An integrated circuit including C1 to Cn can be applied. Each circuit block may be provided with an appropriate function according to requirements. It is necessary to give them the ability.

[0137] The switching element 181 and the switching element 182 are, for example, the above-mentioned switching transistors. A switching element 181, a switching transistor S1, etc. can be applied. The element 182 is made of an oxide semiconductor, particularly a highly purified oxide semiconductor. It is preferable to form the

[0138] The semiconductor device 170 shown in FIG. 8 is merely an example showing a simplified configuration. It has a wide variety of configurations depending on its application.

[0139] The semiconductor device 170 is made of at least one oxide semiconductor, particularly a highly purified oxide semiconductor. The semiconductor device is formed by using the above-mentioned parts, and the standby power consumption is sufficiently suppressed. As described in the embodiment, in an integrated and complicated semiconductor device, standby power consumption The effect of inhibition is very large.

[0140] The structures, methods, and the like described in this embodiment may be combined as appropriate with the structures, methods, and the like described in other embodiments. They can be used in combination.

[0141] (Embodiment 4) Next, as the switching transistor S1 in the previous embodiment (such as the first embodiment), Another example of a method for manufacturing a transistor including an oxide semiconductor that can be used in the present invention is described below. In this embodiment, a highly purified oxide semiconductor (particularly, a non-purified oxide semiconductor) will be described. In the following, we will explain in detail the case where a top-gate type We will use a transistor as an example to explain this, but there is no need to limit the transistor structure to top-gate type. There is none.

[0142] First, an insulating layer 202 is formed on a lower substrate 200. Then, an oxide layer is formed on the insulating layer 202. A semiconductor layer 206 is formed (see FIG. 9(A)).

[0143] For example, the lower layer substrate 200 may be an interlayer insulating substrate in the semiconductor device of the previous embodiment (FIG. 2, etc.). The structure below the edge layer 128 can be described in detail in the previous embodiment. can be taken into consideration.

[0144] The insulating layer 202 functions as a base and is the same as the gate insulating layer 1 in the previous embodiment. The insulating layer 38 and the protective insulating layer 144 can be formed in the same manner as described in the previous embodiment. Note that the insulating layer 202 is formed so as not to contain hydrogen or water as much as possible. It is desirable to form

[0145] The oxide semiconductor layer 206 is made of a quaternary metal oxide such as In-Sn-Ga-Zn-O or a ternary The In-Ga-Zn-O system, In-Sn-Zn-O system, In-Al- Zn-O series, Sn-Ga-Zn-O series, Al-Ga-Zn-O series, Sn-Al-Zn-O and binary metal oxides such as In-Zn-O, Sn-Zn-O, and Al-Zn-O. , Zn-Mg-O, Sn-Mg-O, In-Mg-O, and single-element metal oxides. It can be formed using In-O, Sn-O, Zn-O, or other materials.

[0146] Among them, In-Ga-Zn-O oxide semiconductor materials have a sufficiently high resistance when no electric field is present, Since it is possible to sufficiently reduce the field current and the field effect mobility is high, It is suitable as a semiconductor material for use in devices.

[0147] The oxide semiconductor layer is InMO3(ZnO) m (m>0 and m is not a natural number) The thin film described below can be used, where M is selected from Ga, Al, Mn, and Co. For example, M may be Ga, Ga and Al, Ga and Mn, Ga and Co. Also, InGa x Zinc y O z Using the material represented by Here, x, y, and z can be any number. Also, x, y, and z can be integers. It is not necessary for x to be 0, and it may be a non-integer. Note that x may be 0, but y must not be 0. For example, the notation includes In-Zn-O where x is 0. The oxide semiconductor material represented by In-Ga-Zn-O in this specification is InGaO3 ( ZnO) m (m>0 and m is not a natural number), and the fact that m is not a natural number is an ICP -MS analysis and RBS analysis can be used to confirm this. Also, the formula is expressed as x=1 and y=1. This includes cases where the composition is expressed as x = 1 and y = 0.5. It should be noted that these are merely examples derived from the crystal structure.

[0148] In this embodiment, the oxide semiconductor layer 206 having an amorphous structure is formed using an In-Ga-Zn-O oxide. The film is formed by sputtering using a compound semiconductor film-forming target.

[0149] A target for forming an In-Ga-Zn-O oxide semiconductor layer 206 by a sputtering method. The compound is In:Ga:Zn=1:x:y (x is 0 or more, y is 0.5 to 5). For example, In:Ga:Zn=1:1:1[atom ratio] (x = 1, y = 1), i.e., In2O3:Ga2O3:ZnO = 1:1:2 [m Alternatively, a target having a composition ratio of In:Ga:Zn=1.0 or 1.0 may be used. A target having a composition ratio of I:1:0.5 (x=1, y=0.5) A target having a composition ratio of n:Ga:Zn=1:1:2 [atom ratio] (x=1, y=2) and In:Ga:Zn=1:0:1 [atom ratio] (x=0, y=1) A target that does not change the polarization state can also be used.

[0150] The relative density of the metal oxide in the oxide semiconductor film forming target is 80% or more, preferably 95% or more. % or more, and more preferably 99.9% or more. By using the target, the oxide semiconductor layer 206 can be formed with a dense structure. It is.

[0151] The oxide semiconductor layer 206 is formed in a rare gas (typically, argon) atmosphere or an oxygen atmosphere. It is preferable to use a mixed atmosphere of oxygen or a rare gas (typically argon) and oxygen. Specifically, for example, the concentration of impurities such as hydrogen, water, hydroxyl groups, and hydrides is about several ppm. It is preferable to use a high-purity gas atmosphere in which the concentration is reduced to a level of a few ppb. .

[0152] When the oxide semiconductor layer 206 is formed, for example, the substrate is placed in a processing chamber maintained in a reduced pressure state. The temperature of the substrate is maintained at 100° C. or higher and 600° C. or lower, preferably 200° C. or higher and 400° C. or lower. The substrate is heated so that the moisture in the processing chamber is removed, and hydrogen, water, etc. are removed. The oxide semiconductor layer 206 is formed by using the above target. The oxide semiconductor layer 206 is formed while the substrate is heated. In addition, impurities contained in the oxide semiconductor layer 206 by sputtering can be reduced. In order to remove moisture from inside the processing chamber, a suction type vacuum pump is used. For example, a cryopump, an ion pump, a titanium sublimation pump, etc. A cold trap can be added to the turbo pump. By using a cryopump to evacuate the processing chamber, hydrogen, water, etc. can be removed. Since the impurities and the like are removed, the impurity concentration in the oxide semiconductor layer 206 can be reduced.

[0153] The oxide semiconductor layer 206 is formed under the following conditions: the distance between the substrate and the target is 1 70 mm, pressure 0.4 Pa, direct current (DC) power 0.5 kW, atmosphere oxygen (oxygen 10 0%) atmosphere, or argon (100% argon) atmosphere, or a mixture of oxygen and argon In addition, a pulsed direct current (DC) power supply is used. This reduces the amount of powdery material (also called particles or dust) that is generated during film formation, and improves the film thickness. The thickness of the oxide semiconductor layer 206 is preferably greater than or equal to 2 nm and less than or equal to 200 nm. m or less, preferably 5 nm to 30 nm. The appropriate thickness varies depending on the material and application of the semiconductor device. The method may be selected depending on the purpose.

[0154] Note that before the oxide semiconductor layer 206 is formed by a sputtering method, argon gas is introduced. The deposition on the surface of the insulating layer 202 is removed by reverse sputtering, which generates plasma using the Here, the reverse sputtering is a method of sputtering a sputter target in a normal sputtering process. By bombarding the surface with ions, the surface is deformed by bombarding the surface with ions. The method of modifying the surface by bombarding the surface with ions is called argon bombardment. A method of applying a high-frequency voltage to the processing surface in an atmosphere to generate plasma near the substrate. In addition, nitrogen atmosphere, helium atmosphere, oxygen atmosphere, etc. can be used instead of argon atmosphere. You may use it.

[0155] Next, the oxide semiconductor layer 206 is processed by a method such as etching using a mask. An island-shaped oxide semiconductor layer 206a is formed.

[0156] The oxide semiconductor layer 206 can be etched by either dry etching or wet etching. Of course, both of them can be used in combination. The etching conditions (etching temperature) are adjusted according to the material so that the layer can be etched into the desired shape. The gas, etching solution, etching time, temperature, etc. are set appropriately. For details, see The oxide semiconductor layer 206 is etched in the same manner as in the above embodiment. The etching of the oxide semiconductor layer can be performed in the same manner as in the etching of the oxide semiconductor layer in the embodiment. The above embodiment may be referred to.

[0157] After that, the oxide semiconductor layer 206a is preferably subjected to heat treatment (first heat treatment). The first heat treatment removes excess hydrogen (water or a hydroxyl group) from the oxide semiconductor layer 206a. The structure of the oxide semiconductor layer is adjusted, and the energy The defect level in the gap can be reduced. The temperature of the first heat treatment is, for example, 300 ℃ or higher and 750℃ or lower, or 400℃ or higher and 700℃ or lower.

[0158] In the first heat treatment, for example, the lower substrate 200 is placed in an electric furnace using a resistance heating element, and nitrogen is heated. The treatment can be performed under conditions of a nitrogen atmosphere at 450° C. for one hour. During this time, the oxide semiconductor layer 20 6a should not be exposed to the atmosphere and should not be contaminated with water or hydrogen.

[0159] The heat treatment device is not limited to an electric furnace, and may be any type of heat treatment device, such as heat conduction from a medium such as a heated gas, or A device that heats the workpiece by thermal radiation may be used. For example, a LRTA (Lamp Rapid Thermal Annealing Equipment, GRTA (Gas Rapid RTA (Rapid Thermal Anneal) equipment etc. The LRTA device can be equipped with halogen lamps, metal halide lamps, etc. Lamps, xenon arc lamps, carbon arc lamps, high pressure sodium lamps, high pressure water A device that heats the workpiece by radiating light (electromagnetic waves) emitted from a lamp such as a silver lamp. The GRTA device is a device that performs heat treatment using high-temperature gas. An inert gas that does not react with the workpiece during heat treatment, such as a rare gas such as argon or nitrogen. A gas is used.

[0160] For example, in the first heat treatment, the substrate is placed in an inert gas atmosphere at 650° C. to 700° C. After heating for a few minutes, the substrate may be removed from the inert gas atmosphere and subjected to a GRTA process. GRTA treatment allows high-temperature heat treatment in a short time. Therefore, it can be applied even under temperature conditions that exceed the heat resistance temperature of the substrate. During the heating, the inert gas may be replaced with a gas containing oxygen. By carrying out the heat treatment of step 1, the defect level in the energy gap caused by oxygen vacancies is reduced. This is because it is possible to do so.

[0161] The inert gas atmosphere is nitrogen or a rare gas (helium, neon, argon, etc.). It is desirable to use an atmosphere containing 1,2-dichloroethane (CO), which is the main component, and does not contain water, hydrogen, etc. For example, nitrogen and rare gases such as helium, neon, and argon introduced into heat treatment equipment Purity should be 6N (99.9999%) or more, preferably 7N (99.99999%) or more ( That is, the impurity concentration is set to 1 ppm or less, preferably 0.1 ppm or less.

[0162] In any case, the first heat treatment reduces impurities and makes the semiconductor i-type or substantially i-type. By forming the oxide semiconductor layer 206a, a transistor with excellent characteristics can be realized. It is possible.

[0163] Note that the first heat treatment is performed on the oxide semiconductor layer 2 before it is processed into the island-shaped oxide semiconductor layer 206a. In that case, the lower substrate 20 is removed from the heating device after the first heat treatment. 0 and undergoes a photolithography process.

[0164] The first heat treatment has the effect of removing hydrogen and water, so the first heat treatment is also called dehydration treatment or dehydration treatment. The dehydration or dehydrogenation treatment may be called hydrogenation treatment or the like. After the formation of the oxide semiconductor layer 206a, a source electrode or a drain electrode is stacked on the oxide semiconductor layer 206a. In addition, such dehydration treatment and dehydrogenation can be performed at the following timing. The chemical treatment may be carried out not only once but also multiple times.

[0165] Next, a conductive layer is formed in contact with the oxide semiconductor layer 206a. By selectively etching the source or drain electrode 208a, the source or drain In this step, the source electrode 208b is formed (see FIG. 9(B)). The process is similar to that for the electrode 142a, drain electrode 142b, etc. The form of implementation can be taken into consideration.

[0166] Next, a gate insulating layer 212 is formed in contact with a part of the oxide semiconductor layer 206a (FIG. 9( For details, please refer to the description of the gate insulating layer 138 in the previous embodiment. It is possible.

[0167] After the gate insulating layer 212 is formed, a second thermal annealing is performed in an inert gas atmosphere or an oxygen atmosphere. The temperature of the second heat treatment is preferably 200° C. or more and 450° C. or less. The temperature is 250° C. or higher and 350° C. or lower. For example, the second heating is performed in a nitrogen atmosphere at 250° C. for 1 hour. By performing the second heat treatment, the electrical characteristics of the transistor can be improved. In addition, when the gate insulating layer 212 contains oxygen, the oxide semiconductor Oxygen is supplied to the conductor layer 206a to compensate for oxygen vacancies in the oxide semiconductor layer 206a, thereby forming an i-type It is also possible to form an oxide semiconductor layer that is an intrinsic semiconductor or an oxide semiconductor layer that is extremely close to i-type.

[0168] In this embodiment, the second heat treatment is performed after the gate insulating layer 212 is formed. The timing of the second heat treatment is not particularly limited to this.

[0169] Next, a gate electrode 21 is formed on the gate insulating layer 212 in a region overlapping with the oxide semiconductor layer 206a. The gate electrode 214 is formed by depositing a conductive layer on the gate insulating layer 212. After forming the conductive layer, the conductive layer can be selectively patterned. For details, see the description of the gate electrode 136c and the gate electrode 145 of the previous embodiment. The descriptions therein may be taken into consideration.

[0170] Next, an interlayer insulating layer 216 and an interlayer insulating film 217 are formed on the gate insulating layer 212 and the gate electrode 214. The interlayer insulating layer 216 and the interlayer insulating layer 218 are formed (see FIG. 9(E)). The film can be formed by using a PVD method, a CVD method, or the like. Inorganic insulators such as silicon, silicon nitride, hafnium oxide, aluminum oxide, and tantalum oxide In this embodiment, the interlayer insulating layer can be formed using a material containing an insulating material. However, one embodiment of the disclosed invention is not limited to this. It may be a single layer or a laminated structure of two or more layers.

[0171] It is preferable that the interlayer insulating layer 218 is formed so that its surface is flat. By forming the interlayer insulating layer 218 so as to have a flat surface, a conductive layer is formed on the interlayer insulating layer 218. This is because electrodes, wiring, etc. can be formed suitably.

[0172] Through the above steps, the transistor 250 including the highly purified oxide semiconductor layer 206a is completed. do.

[0173] The transistor 250 shown in FIG. 9(E) is provided on the lower substrate 200 via an insulating layer 202. The oxide semiconductor layer 206a is electrically connected to a source electrode 206b. a source or drain electrode 208a, a source or drain electrode 208b, and an oxide semiconductor layer 206a, source or drain electrode 208a, source or drain electrode A gate insulating layer 212 covering 208b, a gate electrode 214 on the gate insulating layer 212, and a gate electrode An interlayer insulating layer 216 on the gate insulating layer 212 and the gate electrode 214; and an interlayer insulating layer 218.

[0174] In the transistor 250 described in this embodiment, the oxide semiconductor layer 206a is highly purified. Therefore, the hydrogen concentration is 5×10 19 atoms / cm 3 Below 5, preferably ×10 18 atoms / cm 3 Less than or equal to 5×10 17 atoms / cm 3 Below The carrier density of the oxide semiconductor layer 206a is lower than that of a general silicon wafer. Carrier density (1×10 14 / cm 3 A sufficiently small value (e.g., , 1×10 12 / cm 3 less than 1.45×10 10 / cm 3 (less than) This makes the off-current sufficiently small. For example, when the channel length is 10 μm, When the thickness of the oxide semiconductor layer is 30 nm, the drain voltage is 1 V to 10 V. When the gate-source voltage is in the range of about 0 V, the off-state current (the drain current when the gate-source voltage is 0 V or less) The input current is 1×10 -13 A or less. Or, the off-current density at room temperature (off-current divided by the channel width of the transistor) is 100aA (1aA (attoampere) is 10 -18 A (ampere) / μm or less (preferably, 10 aA / μm or less, more preferably or less than 1aA / μm).

[0175] In addition to the off-state current and off-state current density, the characteristics of the above-mentioned transistors include the off-state resistance (transistor The resistance value when the transistor is off and the off resistivity (resistivity when the transistor is off) Here, the off-resistance R can be expressed using the off-current and drain voltage as The off-resistivity ρ is the value calculated from Ohm's law. This value can be calculated by using the area A and the channel length L, and is expressed as ρ=RA / L. In the above case, the off-resistance is 1×10 9 Ω·m or more (or 1×10 10 Ω·m or more) The cross-sectional area A is expressed as A=dW, where d is the thickness of the oxide semiconductor layer and W is the channel width. will be done.

[0176] By using the oxide semiconductor layer 206a which has been highly purified and made intrinsic, Therefore, the off-state current of the transistor can be sufficiently reduced.

[0177] In this embodiment, a transistor Although the present invention has been described with reference to the embodiment using the stencil 250, it is not necessary to interpret the present invention as being limited to this embodiment. For example, by sufficiently improving the electrical properties of oxide semiconductors, It is also possible to use an oxide semiconductor for all the transistors including the transistor. In such a case, it is not necessary to have a laminated structure as shown in the previous embodiment. In order to realize favorable circuit operation, the field-effect mobility μ is μ>100cm 2 In this case, it is preferable to use a glass substrate, etc. A semiconductor device can be formed using such a substrate.

[0178] As described above, the configurations, methods, etc. described in this embodiment may be used in conjunction with the configurations, methods, etc. described in other embodiments. They can be used in any suitable combination.

[0179] (Embodiment 5) Next, as the switching transistor S1 in the previous embodiment (such as the first embodiment), Another example of a method for manufacturing a transistor including an oxide semiconductor that can be used in the present invention is described below. In this embodiment, a crystalline region is formed in the oxide semiconductor layer. a first oxide semiconductor layer having a first crystal region and a second crystal region formed by crystal growth from the first oxide semiconductor layer; The case where the oxide semiconductor layer of the top gate electrode 2 is used will be described in detail. We will explain this using a top-gate transistor as an example, but if the transistor configuration is changed to a top-gate type, There's no need to limit it.

[0180] First, an insulating layer 302 is formed on a lower substrate 300. Then, a first An oxide semiconductor layer is formed, and at least a surface of the first oxide semiconductor layer is subjected to a first heat treatment. The region containing the oxide semiconductor layer is crystallized to form a first oxide semiconductor layer 304 (see FIG. 10A). ).

[0181] For example, the lower layer substrate 300 may be an interlayer insulating substrate in the semiconductor device of the previous embodiment (FIG. 2, etc.). The structure below the edge layer 128 can be described in detail in the previous embodiment. can be taken into consideration.

[0182] The insulating layer 302 functions as a base and is the same as the gate insulating layer 1 in the previous embodiment. The insulating layer 38 and the protective insulating layer 144 can be formed in the same manner as described in the previous embodiment. Note that the insulating layer 302 is formed so as not to contain hydrogen or water as much as possible. It is desirable to form

[0183] The first oxide semiconductor layer 304 is formed in the same manner as the oxide semiconductor layer 206 in the above embodiment. The first oxide semiconductor layer 304 and a method for forming the first oxide semiconductor layer 304 can be described in detail below. However, in this embodiment, the first heat treatment is performed. In order to intentionally crystallize the first oxide semiconductor layer 304, It is preferable to form the first oxide semiconductor layer 304 using a semiconductor film formation target. The thickness of the first oxide semiconductor layer 304 is preferably greater than or equal to 3 nm and less than or equal to 15 nm. In this embodiment, the thickness is set to 5 nm as an example. The appropriate thickness varies depending on the material and the application of the semiconductor device, so the thickness should be determined according to the material and the application of the semiconductor device. The selection may be made according to the application.

[0184] The temperature of the first heat treatment is 450° C. or higher and 850° C. or lower, preferably 550° C. or higher and 750° C. or lower. The heat treatment time is preferably 1 minute or more and 24 hours or less. The atmosphere for the first heat treatment is preferably an atmosphere that does not contain hydrogen, water, etc. , water is sufficiently removed, nitrogen atmosphere, oxygen atmosphere, rare gas (helium, neon, argon) The atmosphere may be, for example, a room temperature (such as a sauna) or a room temperature (such as a sauna).

[0185] Heat treatment equipment includes electric furnaces, as well as equipment that uses heat conduction from a medium such as heated gas or heat radiation. For example, a Lamp Radiation Atomic Energy Transmitter (LRTA) can be used to heat the object to be treated. Rapid Thermal Anneal (GRTA) equipment, Gas Rapid Thermal Anneal (GRTA) equipment RTA (Rapid Thermal Anneal) equipment l) Equipment can be used. LRTA equipment includes halogen lamps, metal halide lamps, etc. xenon arc lamp, carbon arc lamp, high pressure sodium lamp, high pressure mercury lamp It is a device that heats the workpiece by radiating light (electromagnetic waves) emitted from a lamp such as a The GRTA device is a device that performs heat treatment using high-temperature gas. An inert gas that does not react with the workpiece during heat treatment, such as a rare gas such as benzene or nitrogen. is used.

[0186] By the above-mentioned first heat treatment, a region including at least the surface of the first oxide semiconductor layer 304 is The crystalline region is formed by crystallizing the first oxide semiconductor layer 304 from the surface of the first oxide semiconductor layer 304. This is a region formed by the progress of crystal growth toward the inside of the semiconductor layer 304 . The crystalline region may include plate-like crystals having an average thickness of 2 nm to 10 nm. In addition, the crystalline region is a crystal having a c-axis oriented in a direction perpendicular to the surface of the oxide semiconductor layer. May include:

[0187] In addition, the first heat treatment forms a crystalline region and also causes a crystal structure in the first oxide semiconductor layer 304. It is desirable to remove hydrogen (including water and hydroxyl groups) from the water. The purity of nitrogen is 6N (99.9999%) or more (i.e., the concentration of impurities is 1 ppm or less). In nitrogen atmosphere, oxygen atmosphere, rare gas atmosphere (helium, neon, argon, etc.), etc. It is preferable to carry out the heat treatment of 1. It is more preferable to use a material with a purity of 7N (99.99999%) or higher (i.e. The atmosphere is one with an impurity concentration of 0.1 ppm or less. In addition, the H2O concentration is 20 ppm or less. The first heat treatment is carried out in ultra-dry air, preferably in ultra-dry air having an H2O content of 1 ppm or less. You can go.

[0188] In addition, a crystalline region is formed by the first heat treatment, and an oxide is added to the first oxide semiconductor layer 304. For example, it is desirable to change the atmosphere of the heat treatment to an oxygen atmosphere. Thus, oxygen can be supplied to the first oxide semiconductor layer 304.

[0189] In this embodiment, the first heat treatment is performed in a nitrogen atmosphere at 700° C. for 1 hour. After removing hydrogen and the like from the oxide semiconductor layer, the atmosphere is switched to an oxygen atmosphere. In this case, oxygen is supplied to the inside of the first oxide semiconductor layer 304. The objective is to form crystalline regions, so the removal of hydrogen and other substances and the supply of oxygen are separate. For example, heat treatment to remove hydrogen and other substances, or treatment to supply oxygen can be performed. After that, a heat treatment for crystallization can be performed.

[0190] By such a first heat treatment, a crystalline region is formed and hydrogen (including water and hydroxyl groups) is removed. Thus, the first oxide semiconductor layer 304 to which oxygen is supplied is obtained.

[0191] Next, a first oxide semiconductor layer 304 having a crystalline region at least in a region including a surface thereof is formed with A second oxide semiconductor layer 306 is formed (see FIG. 10B).

[0192] The second oxide semiconductor layer 306 is formed in the same manner as the oxide semiconductor layer 206 in the above embodiment. The second oxide semiconductor layer 306 and a method for forming the second oxide semiconductor layer 306 can be described in detail below. The above embodiment may be referred to for the description of the second oxide semiconductor layer 306. It is preferable that the first oxide semiconductor layer 302 is thicker than the first oxide semiconductor layer 304. The sum of the thicknesses of the oxide semiconductor layer 304 and the second oxide semiconductor layer 306 is 3 nm to 50 nm. It is preferable to form a second oxide semiconductor layer 306. The appropriate thickness varies depending on the material and the application of the semiconductor device. The selection may be made according to the application.

[0193] The second oxide semiconductor layer 306 is made of a material having the same main component as the first oxide semiconductor layer 304, e.g. For example, use materials with close lattice constants after crystallization (lattice constant mismatch of 1% or less). In the case where the same main component material is used, the junction of the second oxide semiconductor layer 306 is preferably made of the same material. In the crystallization, crystal growth is likely to proceed using the crystalline regions of the first oxide semiconductor layer 304 as seeds. Furthermore, when the first oxide semiconductor layer 304 and the second oxide semiconductor layer 305 are made of the same main component material, The interface properties and electrical characteristics with the second oxide semiconductor layer 306 are also improved.

[0194] In addition, if the desired film quality can be obtained by crystallization, a second film may be formed using a material with a different main component. Alternatively, the oxide semiconductor layer 306 may be formed as described above.

[0195] Next, the second oxide semiconductor layer 306 is subjected to a second heat treatment, and the first oxide semiconductor layer 304 is The crystalline region is used as a seed for crystal growth to form a second oxide semiconductor layer 306a (FIG. 1 0(C)).

[0196] The temperature of the second heat treatment is 450° C. or higher and 850° C. or lower, preferably 600° C. or higher and 700° C. or lower. The heating time of the second heat treatment is from 1 minute to 100 hours, preferably from 5 hours to 100 hours. The heat treatment time is set to 20 hours or less, typically 10 hours. It is preferable that the atmosphere during the process does not contain hydrogen, water, etc.

[0197] The details of the atmosphere and the effects of the heat treatment are the same as those of the first heat treatment. The heat treatment apparatus that can perform this is the same as that for the first heat treatment. By sometimes placing the inside of the furnace in a nitrogen atmosphere and sometimes placing the inside of the furnace in an oxygen atmosphere during cooling, Hydrogen and the like can be removed in the atmosphere, and oxygen can be supplied in the oxygen atmosphere.

[0198] By performing the above-described second heat treatment, the oxide semiconductor layer 304 is formed. The crystal growth is caused to proceed from the crystalline region to the entire second oxide semiconductor layer 306, so that the second oxide semiconductor layer A conductor layer 306a can be formed. In addition, hydrogen (including water and hydroxyl groups) and the like are removed. In this way, the second oxide semiconductor layer 306a to which oxygen is supplied can be formed. The heat treatment in step 2 can improve the orientation of the crystalline region of the first oxide semiconductor layer 304. It is Noh.

[0199] For example, an In-Ga-Zn-O-based oxide semiconductor material is used for the second oxide semiconductor layer 306a. When used, the second oxide semiconductor layer 306a is InGaO3(ZnO). m (m>0, and and In2Ga2ZnO7 (In:Ga:Zn:O Such crystals may include crystals represented by the following formula: ##EQU1## where R is the ratio of the crystals to the crystals in the second heat treatment. Therefore, the c-axis is perpendicular to the surface of the second oxide semiconductor layer 306b. The orientation is such that

[0200] Here, the above-mentioned crystal contains any one of In, Ga, and Zn, and has an a-axis and It can be considered as a laminated structure of layers parallel to the a-axis and b-axis. In general, the above crystals are made up of layers containing In and layers not containing In (Ga or The oxide semiconductor has a structure in which a layer containing Zn or a layer containing Zn is laminated in the c-axis direction. The membrane layer includes a region having crystallinity, and the crystalline region has an ab plane approximately adjacent to the membrane surface. The oxide semiconductor is made of crystals whose c-axes are approximately parallel to each other and whose c-axes are approximately perpendicular to the film surface. The crystalline regions in the layer are c-axis oriented. Since the oxide semiconductor layer includes a region having crystallinity, the oxide semiconductor layer is ligated Crystalline Oxide Semiconductor) That is, the oxide semiconductor layer including the region having crystallinity is non-single-crystal, and The entire film does not become amorphous.

[0201] In the In-Ga-Zn-O oxide semiconductor crystal, the a-axis and The conductivity in the direction parallel to the a-axis is good. In semiconductor crystals, the electrical conduction is mainly controlled by In. The 5s orbital of In overlaps with the 5s orbital of the adjacent In, forming a carrier path. This is achieved by:

[0202] In addition, the first oxide semiconductor layer 304 may have an amorphous region at the interface with the insulating layer 302. In the case of the structure, the second heat treatment is performed to form a thin film on the surface of the first oxide semiconductor layer 304. Crystal growth proceeds from the crystalline region toward the bottom of the first oxide semiconductor layer 304. In some cases, the amorphous region may be crystallized. Depending on the conditions of the heat treatment, the amorphous regions may remain.

[0203] The first oxide semiconductor layer 304 and the second oxide semiconductor layer 306 are made of oxide semiconductors having the same main component. In the case where a dielectric material is used, as shown in FIG. 10C, a first oxide semiconductor layer 304 and a second oxide semiconductor layer 305 are formed. In some cases, the oxide semiconductor layer 306a may have the same crystal structure as the oxide semiconductor layer 306b. As indicated by the dotted line in FIG. 1C, the first oxide semiconductor layer 304 and the second oxide semiconductor layer 306 The boundary between the first oxide semiconductor layer 304 and the second oxide semiconductor layer 30 a becomes indistinguishable. In some cases, 6a can be considered the same layer.

[0204] Next, the first oxide semiconductor layer 304 and the The second oxide semiconductor layer 306a is processed to form the island-shaped first oxide semiconductor layer 304a and A second oxide semiconductor layer 306b is formed (see FIG. 10D).

[0205] The first oxide semiconductor layer 304 and the second oxide semiconductor layer 306a are etched using a dopant. Either dry etching or wet etching may be used. Of course, both methods may be combined. In order to etch the oxide semiconductor layer into a desired shape, Etching conditions (etching gas, etching solution, etching time, temperature) are adjusted according to the material. The first oxide semiconductor layer 304 and the second oxide semiconductor layer 306a The etching may be performed in a similar manner to the etching of the oxide semiconductor layer in the above embodiment. For details, please refer to the above embodiment.

[0206] Note that a region to be a channel formation region in the oxide semiconductor layer has a flat surface. For example, it is preferable that the height difference of the surface of the second oxide semiconductor layer 306b is equal to or smaller than that of the gate electrode. In the region overlapping with the above (channel formation region), the thickness is 1 nm or less (preferably 0.2 nm or less) ) is preferable.

[0207] Next, a conductive layer is formed in contact with the second oxide semiconductor layer 306b. The conductive layer is selectively etched to form the source or drain electrode 308a, The source or drain electrode 308b is formed (see FIG. 10(D)). The electrode 308a and the source or drain electrode 308b are the same as those in the previous embodiment. The source or drain electrode 142a has a shape similar to that of the source or drain electrode 142b. For details, the above embodiment may be referred to.

[0208] In the step shown in FIG. 10D, the first oxide semiconductor layer 304a and the second oxide semiconductor layer On the side of the conductor layer 306b, a source electrode or drain electrode 308a, Alternatively, the crystal layer in contact with the drain electrode 308b may become amorphous. The entire region of the first oxide semiconductor layer 304a and the second oxide semiconductor layer 306b is crystalline. It is not necessarily a structure.

[0209] Next, a gate insulating layer 312 is formed in contact with part of the second oxide semiconductor layer 306b. The gate insulating layer 312 can be formed by using a CVD method, a sputtering method, or the like. The first oxide semiconductor layer 304a and the second oxide semiconductor layer 304b on the gate insulating layer 312 A gate electrode 314 is formed in a region overlapping with the gate insulating layer 312 and the gate insulating layer 313. An interlayer insulating layer 316 and an interlayer insulating layer 318 are formed on the gate electrode 314 (FIG. 10). (E)). A gate insulating layer 312, a gate electrode 314, an interlayer insulating layer 316 and an interlayer insulating film 317 are formed. The edge layer 318 is the same as the gate insulating layer 138, the gate electrode 136c, and the gate The insulating layer 216 and the insulating layer 218 can be formed in the same manner as the insulating layer 145 and the insulating layer 216. For details, please refer to the above embodiment.

[0210] After the gate insulating layer 312 is formed, a third heat treatment is performed in an inert gas atmosphere or an oxygen atmosphere. The temperature of the third heat treatment is preferably 200° C. or more and 450° C. or less. For example, in an oxygen-containing atmosphere at 250°C for 1 hour, By performing the third heat treatment, the electrical characteristics of the transistor are improved. In addition, when the gate insulating layer 312 is an insulating layer containing oxygen, In this case, oxygen is supplied to the second oxide semiconductor layer 306b, and the oxygen of the second oxide semiconductor layer 306b is Compensating for elemental deficiencies to form an i-type (intrinsic semiconductor) or an oxide semiconductor layer that is as close to i-type as possible It is also possible.

[0211] In this embodiment, the third heat treatment is performed after the gate insulating layer 312 is formed. The timing of the third heat treatment is not limited to this. In addition, the timing of the third heat treatment may be different from that of the second heat treatment. Therefore, when oxygen is supplied to the second oxide semiconductor layer, the third heat treatment can be omitted. good.

[0212] As a result of the above, the first oxide semiconductor layer 304a and A transistor 350 including a second oxide semiconductor layer 306b grown from a crystalline region is completed.

[0213] The transistor 350 shown in FIG. 10(E) is disposed on the lower substrate 300 via the insulating layer 302. The first oxide semiconductor layer 304a is provided on the first oxide semiconductor layer 304a. The second oxide semiconductor layer 306b is electrically connected to the second oxide semiconductor layer 306b. A source or drain electrode 308a, a source or drain electrode 308b, and a the second oxide semiconductor layer 306b, the source or drain electrode 308a, The gate insulating layer 312 covers the drain electrode 308b, and the gate electrode 308a on the gate insulating layer 312 is An interlayer insulating layer 316 is formed on the gate electrode 314 and the gate insulating layer 312. An interlayer insulating layer 318 is provided on the insulating layer 316 .

[0214] In the transistor 350 described in this embodiment, the first oxide semiconductor layer 304a and Since the second oxide semiconductor layer 306b is highly purified, the hydrogen concentration is 5×10 19 atoms / cm 3 Less than 5×10 18 atoms / cm 3 More hopes below Preferably 5 x 10 17 atoms / cm 3 In addition, the oxide semiconductor layer 206a The carrier density is the carrier density in a typical silicon wafer (1×10 14 / cm 3 A sufficiently small value (e.g., 1×10 12 / cm 3Less than, more preferably is 1.45 x 10 10 / cm 3 This allows the off-current to be sufficiently For example, when the channel length is 10 μm and the thickness of the oxide semiconductor layer is 30 nm, In this case, when the drain voltage is in the range of about 1V to 10V, the off-current (gate- The drain current when the source voltage is set to 0V or less is 1×10 -13 A or lower Or, the off-current density at room temperature (off-current divided by the channel width of the transistor) is 100aA (1aA (attoampere) is 10 -18 A (ampere) / μm or less ( Preferably, it is 10 aA / μm or less, and more preferably, it is 1 aA / μm or less.

[0215] In addition to the off-state current and off-state current density, the characteristics of the above-mentioned transistors include the off-state resistance (transistor The resistance value when the transistor is off and the off resistivity (resistivity when the transistor is off) Here, the off-resistance R can be expressed using the off-current and drain voltage as The off-resistivity ρ is the value calculated from Ohm's law. This value can be calculated by using the area A and the channel length L, and is expressed as ρ=RA / L. In the above case, the off-resistance is 1×10 9 Ω·m or more (or 1×10 10 Ω·m or more) The cross-sectional area A is expressed as A=dW, where d is the thickness of the oxide semiconductor layer and W is the channel width. will be done.

[0216] The first oxide semiconductor layer 304a and the second oxide semiconductor layer 304b are thus highly purified and intrinsic. By using the compound semiconductor layer 306b, the off-state current of the transistor can be sufficiently reduced. Cut.

[0217] Further, in this embodiment, a first oxide semiconductor having a crystalline region is used as the oxide semiconductor layer. The first oxide semiconductor layer 304a and the second oxide semiconductor layer 304b are crystal-grown from the crystalline region of the first oxide semiconductor layer 304a. The use of the oxide semiconductor layer 306b improves the field effect mobility and provides good electrical characteristics. It is possible to realize a transistor having the above structure.

[0218] In this embodiment, a transistor Although the present invention has been described with reference to the embodiment using the stencil 350, it is not necessary to interpret the present invention as being limited to this embodiment. For example, the transistor 350 described in this embodiment has a first oxide film having a crystalline region. The first oxide semiconductor layer 304a and the second oxide semiconductor layer 304b are grown from the crystalline region of the first oxide semiconductor layer 304a. Since the second oxide semiconductor layer 306b has a good field-effect mobility, it is possible to integrate the It is possible to use oxide semiconductors for all transistors, including those that constitute circuits. In such a case, the laminated structure shown in the above embodiment is However, in order to realize good circuit operation, the field effect mobility of the oxide semiconductor is required. μ is μ>100cm 2 / V·s. In this case, the glass substrate A semiconductor device can be formed using a substrate such as a silicon substrate.

[0219] As described above, the configurations, methods, etc. described in this embodiment may be used in conjunction with the configurations, methods, etc. described in other embodiments. They can be used in any suitable combination.

[0220] (Embodiment 6) In this embodiment, when the semiconductor device described in the above embodiment is applied to an electronic device, This will be described with reference to FIG. 11. In this embodiment, Telephones, mobile phone devices, portable information terminals (including portable game consoles, audio playback devices, etc.) (including), digital cameras, digital video cameras, electronic paper, television equipment (television The above-described semiconductor device is applied to electronic devices such as a television receiver. This section explains what happens when

[0221] FIG. 11A shows a notebook personal computer, which includes a housing 401, a housing 402, The display unit 403 and the keyboard 404 are included. The semiconductor device described in the above embodiment is provided inside the semiconductor device. This realizes a notebook type personal computer with reduced processing power.

[0222] FIG. 11B shows a portable digital assistant (PDA), and a main body 411 includes a display unit 413 and an external The terminal 415 includes an external interface, an operation button 414, and the like. The main body 411 includes a stylus 412 for operating the terminal. Therefore, a portable information terminal with sufficiently reduced power consumption can be provided. It will be realized.

[0223] FIG. 11C shows an electronic book 420 equipped with electronic paper. The electronic book 420 is made up of a housing 421 and a housing 422. The housing 421 and the housing 423 are connected by a shaft portion 437. The shaft portion 437 is an axis around which the opening and closing operation can be performed. The case 421 also includes a power supply 431, an operation key, and a keyboard. At least one of the housings 421 and 423 is provided with a keyboard 433 and a speaker 435. The semiconductor device described in the above embodiment is provided in the This allows for a reduced reading size of electronic books.

[0224] FIG. 11D shows a mobile phone that is configured with two housings, a housing 440 and a housing 441. Furthermore, the housing 440 and the housing 441 slide and are unfolded as shown in FIG. 11(D). It can be folded up and folded up, making it possible to make it compact and suitable for carrying. The housing 441 also includes a display panel 442, a speaker 443, a microphone 444, and a pointing device. The camera includes a display device 446, a camera lens 447, and an external connection terminal 448. The display panel 442 has a touch panel function, and the image display shown in FIG. The multiple operation keys 445 shown are indicated by dotted lines. The device is also equipped with a solar cell 449 for charging the device, an external memory slot 450, etc. The antenna is built into the housing 441. At least one of the housings 440 and 441 The semiconductor device described in the above embodiment is provided. This allows for a mobile phone with reduced power consumption to be realized.

[0225] FIG. 11E shows a digital camera, which includes a main body 461, a display unit 467, an eyepiece unit 463, and an operation unit. It is composed of an operation switch 464, a display unit 465, a battery 466, etc. The semiconductor device described in the above embodiment is provided in the inside of 461. Thus, a digital camera in which the above-mentioned noise is sufficiently reduced can be realized.

[0226] FIG. 11F shows a television device 470, which includes a housing 471, a display unit 473, a stand, and the like. The television device 470 is operated by a switch provided in the housing 471. The operation can be performed by a switch or a remote control 480. The semiconductor device described in the above embodiment is mounted on the device 480. A television apparatus with sufficiently reduced forces is realized.

[0227] As described above, the electronic device shown in this embodiment mode includes the integrated circuit according to the above embodiment. As a result, standby power consumption has been sufficiently suppressed, and electronic devices with low power consumption have been realized. can be. [Explanation of symbols]

[0228] 100 Substrates 102 Protective layer 104 Semiconductor area 106 Element isolation insulating layer 108 Gate Insulation Layer 110 Gate electrode 112 Insulating layer 114 Impurity region 116 Channel formation region 118 Sidewall insulating layer 120 High concentration impurity region 122 Metal layer 124 Metal compound area 126 Interlayer Insulation Layer 128 Interlayer Insulation Layer 130a source electrode or drain electrode 130b Source electrode or drain electrode 132 Insulating layer 134 Conductive Layer 136a electrode 136b Electrode 136c Gate electrode 138 Gate Insulation Layer 140 Oxide semiconductor layer 142a Source electrode or drain electrode 142b Source or drain electrode 144 Protective Insulation Layer 145 Gate electrode 146 Interlayer Insulation Layer 148 Conductive Layer 150a electrode 150b electrode 150c electrode 150d electrode 152 Insulating layer 154a electrode 154b electrode 154c electrode 160 Transistors 162 Transistor 170 Semiconductor Devices 171 Circuit Block 172 Circuit Block 173 Circuit Block 174 Circuit Block 181 Switching elements 182 Switching element 200 Lower layer board 202 Insulating layer 206 Oxide semiconductor layer 206a Oxide semiconductor layer 208a Source electrode or drain electrode 208b Source electrode or drain electrode 212 Gate insulating layer 214 Gate electrode 216 Interlayer Insulation Layer 218 Interlayer Insulation Layer 250 Transistors 300 Lower layer board 302 Insulating layer 304 First oxide semiconductor layer 304a First oxide semiconductor layer 306 Second oxide semiconductor layer 306a Second oxide semiconductor layer 306b Second oxide semiconductor layer 308a Source electrode or drain electrode 308b Source electrode or drain electrode 312 Gate insulation layer 314 Gate electrode 316 Interlayer Insulation Layer 318 Interlayer Insulation Layer 350 Transistors 401 Case 402 Case 403 Display section 404 Keyboard 411 Main unit 412 Stylus 413 Display section 414 Operation button 415 External Interface 420 e-books 421 Case 423 Case 431 Power supply 433 Operation Key 435 Speaker 437 Shaft 440 Case 441 Case 442 Display Panel 443 Speaker 444 Microphone 445 Operation Key 446 Pointing Device 447 Camera Lenses 448 External connection terminal 449 Solar Cells 450 external memory slot 461 Main unit 463 Eyepiece 464 Operation Switch 465 Display section 466 Battery 467 Display section 470 Television Equipment 471 Case 473 Display section 475 Stand 480 Remote Controlled Device

Claims

1. A semiconductor device having a first transistor and a second transistor, a first insulating layer having a region located above a channel formation region of the first transistor; a first conductive layer having a region located above the first insulating layer and functioning as a first gate electrode of the second transistor; a second insulating layer having a region located above the first conductive layer and functioning as a first gate insulating layer of the second transistor; an oxide semiconductor layer having a region located above the second insulating layer and functioning as a channel formation region of the second transistor; a second conductive layer having a region in contact with a top surface of the oxide semiconductor layer and functioning as one of a source electrode and a drain electrode of the second transistor; a third conductive layer having a region in contact with a top surface of the oxide semiconductor layer and functioning as the other of the source electrode and the drain electrode of the second transistor; a third insulating layer having a region located above the oxide semiconductor layer, a region located above the second conductive layer, and a region located above the third conductive layer and functioning as a second gate insulating layer of the second transistor; a fourth conductive layer having a region located above the third insulating layer and functioning as a second gate electrode of the second transistor; a fourth insulating layer having a region located above the fourth conductive layer; a channel formation region of the first transistor includes silicon; the oxide semiconductor layer contains In, Ga, and Zn; the first conductive layer comprises molybdenum; the second conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the third conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the second conductive layer is electrically connected to a source or a drain of the first transistor; the fourth conductive layer has a region overlapping with the second conductive layer via the third insulating layer, The fourth conductive layer has a region overlapping with the third conductive layer via the third insulating layer.

2. A semiconductor device having a first transistor and a second transistor, a first insulating layer having a region located above a channel formation region of the first transistor; a first conductive layer having a region located above the first insulating layer and functioning as a first gate electrode of the second transistor; a second insulating layer having a region located above the first conductive layer and functioning as a first gate insulating layer of the second transistor; an oxide semiconductor layer having a region located above the second insulating layer and functioning as a channel formation region of the second transistor; a second conductive layer having a region in contact with a top surface of the oxide semiconductor layer and functioning as one of a source electrode and a drain electrode of the second transistor; a third conductive layer having a region in contact with a top surface of the oxide semiconductor layer and functioning as the other of the source electrode and the drain electrode of the second transistor; a third insulating layer having a region located above the oxide semiconductor layer, a region located above the second conductive layer, and a region located above the third conductive layer and functioning as a second gate insulating layer of the second transistor; a fourth conductive layer having a region located above the third insulating layer and functioning as a second gate electrode of the second transistor; a fourth insulating layer having a region located above the fourth conductive layer; a channel formation region of the first transistor includes silicon; the oxide semiconductor layer contains In, Ga, and Zn; the first conductive layer comprises molybdenum; the second conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the third conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the oxide semiconductor layer does not have a region overlapping with a channel formation region of the first transistor, the second conductive layer is electrically connected to a source or a drain of the first transistor; the fourth conductive layer has a region overlapping with the second conductive layer via the third insulating layer, The fourth conductive layer has a region overlapping with the third conductive layer via the third insulating layer.

3. A semiconductor device having a first transistor and a second transistor, a first insulating layer having a region located above a channel formation region of the first transistor; a first conductive layer having a region located above the first insulating layer and functioning as a first gate electrode of the second transistor; a second insulating layer having a region located above the first conductive layer and functioning as a first gate insulating layer of the second transistor; an oxide semiconductor layer having a region located above the second insulating layer and functioning as a channel formation region of the second transistor; a second conductive layer having a region in contact with a top surface of the oxide semiconductor layer and functioning as one of a source electrode and a drain electrode of the second transistor; a third conductive layer having a region in contact with a top surface of the oxide semiconductor layer and functioning as the other of the source electrode and the drain electrode of the second transistor; a third insulating layer having a region located above the oxide semiconductor layer, a region located above the second conductive layer, and a region located above the third conductive layer and functioning as a second gate insulating layer of the second transistor; a fourth conductive layer having a region located above the third insulating layer and functioning as a second gate electrode of the second transistor; a fourth insulating layer having a region located above the fourth conductive layer; a channel formation region of the first transistor includes silicon; the oxide semiconductor layer contains In, Ga, and Zn; the first conductive layer comprises molybdenum; the second conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the third conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the first conductive layer does not have a region overlapping a channel formation region of the first transistor, the second conductive layer is electrically connected to a source or a drain of the first transistor; the fourth conductive layer has a region overlapping with the second conductive layer via the third insulating layer, The fourth conductive layer has a region overlapping with the third conductive layer via the third insulating layer.

4. A semiconductor device having a first transistor and a second transistor, a first insulating layer having a region located above a channel formation region of the first transistor; a first conductive layer having a region located above the first insulating layer and functioning as a first gate electrode of the second transistor; a second insulating layer having a region located above the first conductive layer and functioning as a first gate insulating layer of the second transistor; an oxide semiconductor layer having a region located above the second insulating layer and functioning as a channel formation region of the second transistor; a second conductive layer having a region in contact with a top surface of the oxide semiconductor layer and functioning as one of a source electrode and a drain electrode of the second transistor; a third conductive layer having a region in contact with a top surface of the oxide semiconductor layer and functioning as the other of the source electrode and the drain electrode of the second transistor; a third insulating layer having a region located above the oxide semiconductor layer, a region located above the second conductive layer, and a region located above the third conductive layer and functioning as a second gate insulating layer of the second transistor; a fourth conductive layer having a region located above the third insulating layer and functioning as a second gate electrode of the second transistor; a fourth insulating layer having a region located above the fourth conductive layer; a channel formation region of the first transistor includes silicon; the oxide semiconductor layer contains In, Ga, and Zn; the first conductive layer comprises molybdenum; the second conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the third conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the oxide semiconductor layer does not have a region overlapping with a channel formation region of the first transistor, the first conductive layer does not have a region overlapping a channel formation region of the first transistor, the second conductive layer is electrically connected to a source or a drain of the first transistor; the fourth conductive layer has a region overlapping with the second conductive layer via the third insulating layer, The fourth conductive layer has a region overlapping with the third conductive layer via the third insulating layer.

5. A semiconductor device having a first transistor and a second transistor, a first insulating layer having a region located above a channel formation region of the first transistor; a first conductive layer having a region located above the first insulating layer and functioning as a first gate electrode of the second transistor; a second insulating layer having a region located above the first conductive layer and functioning as a first gate insulating layer of the second transistor; an oxide semiconductor layer having a region located above the second insulating layer and functioning as a channel formation region of the second transistor; a second conductive layer having a region in contact with a top surface of the oxide semiconductor layer and a region in contact with a top surface of the second insulating layer and functioning as one of a source electrode and a drain electrode of the second transistor; a third conductive layer having a region in contact with a top surface of the oxide semiconductor layer and a region in contact with a top surface of the second insulating layer and functioning as the other of the source electrode and the drain electrode of the second transistor; a third insulating layer having a region located above the oxide semiconductor layer, a region located above the second conductive layer, and a region located above the third conductive layer and functioning as a second gate insulating layer of the second transistor; a fourth conductive layer having a region located above the third insulating layer and functioning as a second gate electrode of the second transistor; a fourth insulating layer having a region located above the fourth conductive layer; a channel formation region of the first transistor includes silicon; the oxide semiconductor layer contains In, Ga, and Zn; the first conductive layer comprises molybdenum; the second conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the third conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the second conductive layer is electrically connected to a source or a drain of the first transistor; the fourth conductive layer has a region overlapping with the second conductive layer via the third insulating layer, The fourth conductive layer has a region overlapping with the third conductive layer via the third insulating layer.

6. A semiconductor device having a first transistor and a second transistor, a first insulating layer having a region located above a channel formation region of the first transistor; a first conductive layer having a region located above the first insulating layer and functioning as a first gate electrode of the second transistor; a second insulating layer having a region located above the first conductive layer and functioning as a first gate insulating layer of the second transistor; an oxide semiconductor layer having a region located above the second insulating layer and functioning as a channel formation region of the second transistor; a second conductive layer having a region in contact with a top surface of the oxide semiconductor layer and a region in contact with a top surface of the second insulating layer and functioning as one of a source electrode and a drain electrode of the second transistor; a third conductive layer having a region in contact with a top surface of the oxide semiconductor layer and a region in contact with a top surface of the second insulating layer and functioning as the other of the source electrode and the drain electrode of the second transistor; a third insulating layer having a region located above the oxide semiconductor layer, a region located above the second conductive layer, and a region located above the third conductive layer and functioning as a second gate insulating layer of the second transistor; a fourth conductive layer having a region located above the third insulating layer and functioning as a second gate electrode of the second transistor; a fourth insulating layer having a region located above the fourth conductive layer; a channel formation region of the first transistor includes silicon; the oxide semiconductor layer contains In, Ga, and Zn; the first conductive layer comprises molybdenum; the second conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the third conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the oxide semiconductor layer does not have a region overlapping with a channel formation region of the first transistor, the second conductive layer is electrically connected to a source or a drain of the first transistor; the fourth conductive layer has a region overlapping with the second conductive layer via the third insulating layer, The fourth conductive layer has a region overlapping with the third conductive layer via the third insulating layer.

7. A semiconductor device having a first transistor and a second transistor, a first insulating layer having a region located above a channel formation region of the first transistor; a first conductive layer having a region located above the first insulating layer and functioning as a first gate electrode of the second transistor; a second insulating layer having a region located above the first conductive layer and functioning as a first gate insulating layer of the second transistor; an oxide semiconductor layer having a region located above the second insulating layer and functioning as a channel formation region of the second transistor; a second conductive layer having a region in contact with a top surface of the oxide semiconductor layer and a region in contact with a top surface of the second insulating layer and functioning as one of a source electrode and a drain electrode of the second transistor; a third conductive layer having a region in contact with a top surface of the oxide semiconductor layer and a region in contact with a top surface of the second insulating layer and functioning as the other of the source electrode and the drain electrode of the second transistor; a third insulating layer having a region located above the oxide semiconductor layer, a region located above the second conductive layer, and a region located above the third conductive layer and functioning as a second gate insulating layer of the second transistor; a fourth conductive layer having a region located above the third insulating layer and functioning as a second gate electrode of the second transistor; a fourth insulating layer having a region located above the fourth conductive layer; a channel formation region of the first transistor includes silicon; the oxide semiconductor layer contains In, Ga, and Zn; the first conductive layer comprises molybdenum; the second conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the third conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the first conductive layer does not have a region overlapping a channel formation region of the first transistor, the second conductive layer is electrically connected to a source or a drain of the first transistor; the fourth conductive layer has a region overlapping with the second conductive layer via the third insulating layer, The fourth conductive layer has a region overlapping with the third conductive layer via the third insulating layer.

8. A semiconductor device having a first transistor and a second transistor, a first insulating layer having a region located above a channel formation region of the first transistor; a first conductive layer having a region located above the first insulating layer and functioning as a first gate electrode of the second transistor; a second insulating layer having a region located above the first conductive layer and functioning as a first gate insulating layer of the second transistor; an oxide semiconductor layer having a region located above the second insulating layer and functioning as a channel formation region of the second transistor; a second conductive layer having a region in contact with a top surface of the oxide semiconductor layer and a region in contact with a top surface of the second insulating layer and functioning as one of a source electrode and a drain electrode of the second transistor; a third conductive layer having a region in contact with a top surface of the oxide semiconductor layer and a region in contact with a top surface of the second insulating layer and functioning as the other of the source electrode and the drain electrode of the second transistor; a third insulating layer having a region located above the oxide semiconductor layer, a region located above the second conductive layer, and a region located above the third conductive layer and functioning as a second gate insulating layer of the second transistor; a fourth conductive layer having a region located above the third insulating layer and functioning as a second gate electrode of the second transistor; a fourth insulating layer having a region located above the fourth conductive layer; a channel formation region of the first transistor includes silicon; the oxide semiconductor layer contains In, Ga, and Zn; the first conductive layer comprises molybdenum; the second conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the third conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the oxide semiconductor layer does not have a region overlapping with a channel formation region of the first transistor, the first conductive layer does not have a region overlapping a channel formation region of the first transistor, the second conductive layer is electrically connected to a source or a drain of the first transistor; the fourth conductive layer has a region overlapping with the second conductive layer via the third insulating layer, The fourth conductive layer has a region overlapping with the third conductive layer via the third insulating layer.

9. A semiconductor device having a first transistor and a second transistor, a first insulating layer having a region located above a channel formation region of the first transistor; a first conductive layer having a region located above the first insulating layer and functioning as a first gate electrode of the second transistor; a second insulating layer having a region located above the first conductive layer and functioning as a first gate insulating layer of the second transistor; an oxide semiconductor layer having a region located above the second insulating layer and functioning as a channel formation region of the second transistor; a second conductive layer having a region in contact with a top surface of the oxide semiconductor layer and functioning as one of a source electrode and a drain electrode of the second transistor; a third conductive layer having a region in contact with a top surface of the oxide semiconductor layer and functioning as the other of the source electrode and the drain electrode of the second transistor; a third insulating layer having a region located above the oxide semiconductor layer, a region located above the second conductive layer, and a region located above the third conductive layer and functioning as a second gate insulating layer of the second transistor; a fourth conductive layer having a region located above the third insulating layer and functioning as a second gate electrode of the second transistor; a fourth insulating layer having a region located above the fourth conductive layer; a channel formation region of the first transistor includes silicon; the first conductive layer comprises molybdenum; the second conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the third conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the second conductive layer is electrically connected to a source or a drain of the first transistor; the fourth conductive layer has a region overlapping with the second conductive layer via the third insulating layer, The fourth conductive layer has a region overlapping with the third conductive layer via the third insulating layer.

10. A semiconductor device having a first transistor and a second transistor, a first insulating layer having a region located above a channel formation region of the first transistor; a first conductive layer having a region located above the first insulating layer and functioning as a first gate electrode of the second transistor; a second insulating layer having a region located above the first conductive layer and functioning as a first gate insulating layer of the second transistor; an oxide semiconductor layer having a region located above the second insulating layer and functioning as a channel formation region of the second transistor; a second conductive layer having a region in contact with a top surface of the oxide semiconductor layer and functioning as one of a source electrode and a drain electrode of the second transistor; a third conductive layer having a region in contact with a top surface of the oxide semiconductor layer and functioning as the other of the source electrode and the drain electrode of the second transistor; a third insulating layer having a region located above the oxide semiconductor layer, a region located above the second conductive layer, and a region located above the third conductive layer and functioning as a second gate insulating layer of the second transistor; a fourth conductive layer having a region located above the third insulating layer and functioning as a second gate electrode of the second transistor; a fourth insulating layer having a region located above the fourth conductive layer; a channel formation region of the first transistor includes silicon; the first conductive layer comprises molybdenum; the second conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the third conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the oxide semiconductor layer does not have a region overlapping with a channel formation region of the first transistor, the second conductive layer is electrically connected to a source or a drain of the first transistor; the fourth conductive layer has a region overlapping with the second conductive layer via the third insulating layer, The fourth conductive layer has a region overlapping with the third conductive layer via the third insulating layer.

11. A semiconductor device having a first transistor and a second transistor, a first insulating layer having a region located above a channel formation region of the first transistor; a first conductive layer having a region located above the first insulating layer and functioning as a first gate electrode of the second transistor; a second insulating layer having a region located above the first conductive layer and functioning as a first gate insulating layer of the second transistor; an oxide semiconductor layer having a region located above the second insulating layer and functioning as a channel formation region of the second transistor; a second conductive layer having a region in contact with a top surface of the oxide semiconductor layer and functioning as one of a source electrode and a drain electrode of the second transistor; a third conductive layer having a region in contact with a top surface of the oxide semiconductor layer and functioning as the other of the source electrode and the drain electrode of the second transistor; a third insulating layer having a region located above the oxide semiconductor layer, a region located above the second conductive layer, and a region located above the third conductive layer and functioning as a second gate insulating layer of the second transistor; a fourth conductive layer having a region located above the third insulating layer and functioning as a second gate electrode of the second transistor; a fourth insulating layer having a region located above the fourth conductive layer; a channel formation region of the first transistor includes silicon; the first conductive layer comprises molybdenum; the second conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the third conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the first conductive layer does not have a region overlapping a channel formation region of the first transistor, the second conductive layer is electrically connected to a source or a drain of the first transistor; the fourth conductive layer has a region overlapping with the second conductive layer via the third insulating layer, The fourth conductive layer has a region overlapping with the third conductive layer via the third insulating layer.

12. A semiconductor device having a first transistor and a second transistor, a first insulating layer having a region located above a channel formation region of the first transistor; a first conductive layer having a region located above the first insulating layer and functioning as a first gate electrode of the second transistor; a second insulating layer having a region located above the first conductive layer and functioning as a first gate insulating layer of the second transistor; an oxide semiconductor layer having a region located above the second insulating layer and functioning as a channel formation region of the second transistor; a second conductive layer having a region in contact with a top surface of the oxide semiconductor layer and functioning as one of a source electrode and a drain electrode of the second transistor; a third conductive layer having a region in contact with a top surface of the oxide semiconductor layer and functioning as the other of the source electrode and the drain electrode of the second transistor; a third insulating layer having a region located above the oxide semiconductor layer, a region located above the second conductive layer, and a region located above the third conductive layer and functioning as a second gate insulating layer of the second transistor; a fourth conductive layer having a region located above the third insulating layer and functioning as a second gate electrode of the second transistor; a fourth insulating layer having a region located above the fourth conductive layer; a channel formation region of the first transistor includes silicon; the first conductive layer comprises molybdenum; the second conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the third conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the oxide semiconductor layer does not have a region overlapping with a channel formation region of the first transistor, the first conductive layer does not have a region overlapping a channel formation region of the first transistor, the second conductive layer is electrically connected to a source or a drain of the first transistor; the fourth conductive layer has a region overlapping with the second conductive layer via the third insulating layer, The fourth conductive layer has a region overlapping with the third conductive layer via the third insulating layer.

13. A semiconductor device having a first transistor and a second transistor, a first insulating layer having a region located above a channel formation region of the first transistor; a first conductive layer having a region located above the first insulating layer and functioning as a first gate electrode of the second transistor; a second insulating layer having a region located above the first conductive layer and functioning as a first gate insulating layer of the second transistor; an oxide semiconductor layer having a region located above the second insulating layer and functioning as a channel formation region of the second transistor; a second conductive layer having a region in contact with a top surface of the oxide semiconductor layer and a region in contact with a top surface of the second insulating layer and functioning as one of a source electrode and a drain electrode of the second transistor; a third conductive layer having a region in contact with a top surface of the oxide semiconductor layer and a region in contact with a top surface of the second insulating layer and functioning as the other of the source electrode and the drain electrode of the second transistor; a third insulating layer having a region located above the oxide semiconductor layer, a region located above the second conductive layer, and a region located above the third conductive layer and functioning as a second gate insulating layer of the second transistor; a fourth conductive layer having a region located above the third insulating layer and functioning as a second gate electrode of the second transistor; a fourth insulating layer having a region located above the fourth conductive layer; the first conductive layer comprises molybdenum; the second conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the third conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; a channel formation region of the first transistor includes silicon; the second conductive layer is electrically connected to a source or a drain of the first transistor; the fourth conductive layer has a region overlapping with the second conductive layer via the third insulating layer, The fourth conductive layer has a region overlapping with the third conductive layer via the third insulating layer.

14. A semiconductor device having a first transistor and a second transistor, a first insulating layer having a region located above a channel formation region of the first transistor; a first conductive layer having a region located above the first insulating layer and functioning as a first gate electrode of the second transistor; a second insulating layer having a region located above the first conductive layer and functioning as a first gate insulating layer of the second transistor; an oxide semiconductor layer having a region located above the second insulating layer and functioning as a channel formation region of the second transistor; a second conductive layer having a region in contact with a top surface of the oxide semiconductor layer and a region in contact with a top surface of the second insulating layer and functioning as one of a source electrode and a drain electrode of the second transistor; a third conductive layer having a region in contact with a top surface of the oxide semiconductor layer and a region in contact with a top surface of the second insulating layer and functioning as the other of the source electrode and the drain electrode of the second transistor; a third insulating layer having a region located above the oxide semiconductor layer, a region located above the second conductive layer, and a region located above the third conductive layer and functioning as a second gate insulating layer of the second transistor; a fourth conductive layer having a region located above the third insulating layer and functioning as a second gate electrode of the second transistor; a fourth insulating layer having a region located above the fourth conductive layer; a channel formation region of the first transistor includes silicon; the first conductive layer comprises molybdenum; the second conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the third conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the oxide semiconductor layer does not have a region overlapping with a channel formation region of the first transistor, the second conductive layer is electrically connected to a source or a drain of the first transistor; the fourth conductive layer has a region overlapping with the second conductive layer via the third insulating layer, The fourth conductive layer has a region overlapping with the third conductive layer via the third insulating layer.

15. A semiconductor device having a first transistor and a second transistor, a first insulating layer having a region located above a channel formation region of the first transistor; a first conductive layer having a region located above the first insulating layer and functioning as a first gate electrode of the second transistor; a second insulating layer having a region located above the first conductive layer and functioning as a first gate insulating layer of the second transistor; an oxide semiconductor layer having a region located above the second insulating layer and functioning as a channel formation region of the second transistor; a second conductive layer having a region in contact with a top surface of the oxide semiconductor layer and a region in contact with a top surface of the second insulating layer and functioning as one of a source electrode and a drain electrode of the second transistor; a third conductive layer having a region in contact with a top surface of the oxide semiconductor layer and a region in contact with a top surface of the second insulating layer and functioning as the other of the source electrode and the drain electrode of the second transistor; a third insulating layer having a region located above the oxide semiconductor layer, a region located above the second conductive layer, and a region located above the third conductive layer and functioning as a second gate insulating layer of the second transistor; a fourth conductive layer having a region located above the third insulating layer and functioning as a second gate electrode of the second transistor; a fourth insulating layer having a region located above the fourth conductive layer; a channel formation region of the first transistor includes silicon; the first conductive layer comprises molybdenum; the second conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the third conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the first conductive layer does not have a region overlapping a channel formation region of the first transistor, the second conductive layer is electrically connected to a source or a drain of the first transistor; the fourth conductive layer has a region overlapping with the second conductive layer via the third insulating layer, The fourth conductive layer has a region overlapping with the third conductive layer via the third insulating layer.

16. A semiconductor device having a first transistor and a second transistor, a first insulating layer having a region located above a channel formation region of the first transistor; a first conductive layer having a region located above the first insulating layer and functioning as a first gate electrode of the second transistor; a second insulating layer having a region located above the first conductive layer and functioning as a first gate insulating layer of the second transistor; an oxide semiconductor layer having a region located above the second insulating layer and functioning as a channel formation region of the second transistor; a second conductive layer having a region in contact with a top surface of the oxide semiconductor layer and a region in contact with a top surface of the second insulating layer and functioning as one of a source electrode and a drain electrode of the second transistor; a third conductive layer having a region in contact with a top surface of the oxide semiconductor layer and a region in contact with a top surface of the second insulating layer and functioning as the other of the source electrode and the drain electrode of the second transistor; a third insulating layer having a region located above the oxide semiconductor layer, a region located above the second conductive layer, and a region located above the third conductive layer and functioning as a second gate insulating layer of the second transistor; a fourth conductive layer having a region located above the third insulating layer and functioning as a second gate electrode of the second transistor; a fourth insulating layer having a region located above the fourth conductive layer; a channel formation region of the first transistor includes silicon; the first conductive layer comprises molybdenum; the second conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the third conductive layer has a laminated structure in which a titanium film, an aluminum film, and a titanium film are laminated in this order; the oxide semiconductor layer does not have a region overlapping with a channel formation region of the first transistor, the first conductive layer does not have a region overlapping a channel formation region of the first transistor, the second conductive layer is electrically connected to a source or a drain of the first transistor; the fourth conductive layer has a region overlapping with the second conductive layer via the third insulating layer, The fourth conductive layer has a region overlapping with the third conductive layer via the third insulating layer.

17. In any one of claims 1 to 16, the second insulating layer has a laminated structure of a first layer having nitrogen and silicon and a second layer having oxygen and silicon; The third insulating layer has a laminated structure of a first layer containing oxygen and silicon, and a second layer containing nitrogen and silicon.

Citation Information

Patent Citations

  • Semiconductor device, semiconductor memory device and manufacturing method, and portable information equipment

    JP2002368226A

  • Semiconductor device and method of manufacturing the same

    JP2008218786A

  • Semiconductor device

    JP2009076879A

  • Fabricating method of semiconductor device

    JP2009135350A

  • Semiconductor device and method of manufacturing the same

    JP2009239196A