Stainless steel having excellent cold forgeability and, hydrogen embrittlement resistance

A stainless steel with controlled borides and sulfides addresses the challenges of cold forgeability and hydrogen embrittlement resistance, improving tool life and mechanical properties through optimized chemical composition and manufacturing processes.

JP2024138419AActive Publication Date: 2024-10-08NIPPON STEEL CORPORATION
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024111005
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-02-09
Filing Date
2024-07-10
Publication Date
2024-10-08
Estimated Expiration
2042-08-03

AI Technical Summary

Technical Problem

Conventional stainless steels face challenges in simultaneously achieving cold forgeability, machinability, and hydrogen embrittlement resistance after cold working, with high material strength leading to short tool life and increased forging loads, and processing limits being reached during high-strain operations.

Method used

A stainless steel composition with controlled amounts of borides and sulfides, optimized through specific chemical elements and manufacturing processes like inclined rolling, ensuring a critical compression ratio of 60% or more, relative tensile strength of 80% or more, and drilling life index of 1 m/min or more.

Benefits of technology

The solution enhances cold forgeability, machinability, and hydrogen embrittlement resistance by improving tool life and reducing the risk of cracking, while maintaining mechanical strength and corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138419000001
    Figure 2024138419000001
  • Figure 2024138419000002
    Figure 2024138419000002
  • Figure 2024138419000003
    Figure 2024138419000003
Patent Text Reader

Abstract

To provide a stainless steel which can satisfy all of cold forgeability, machinability and hydrogen embrittlement resistance after being cold worked.SOLUTION: A stainless steel is provided, containing, by mass%, 0.0010-0.15% of C, 0.01-2.00% of Si, 0.01-10.00% of Mn, 8.00-30.00% of Ni, 9.0-21.0% of Cr, 0.01-3.00% of Mo, 0.01-5.00% of Cu, 0.0010-0.10%, of N, 0.0001-0.05% of B, and 0.0001-0.50% of S, and further containing one or more selected from 0.001-2.0% of Al and 0.0001-0.05% of Ca, wherein an A value represented by formula (a) is -100 or less, an amount of precipitated B as a boride is 0.0001% or more, and an aspect ratio of a sulfide is 50 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a stainless steel, and more particularly to a stainless steel that can satisfy all of the requirements for cold forgeability, machinability, and hydrogen embrittlement resistance after cold working. [Background technology]

[0002] Fuel cell vehicles and hydrogen stations that handle hydrogen fuel use many metal parts that come into contact with hydrogen in a high-pressure gas state. Metal parts that come into contact with high-pressure hydrogen gas are prone to hydrogen embrittlement, as hydrogen penetrates into the metal. Therefore, metal parts are required to have mechanical strength and corrosion resistance in a high-pressure hydrogen environment, as well as hydrogen embrittlement resistance.

[0003] Conventionally, austenitic stainless steels such as SUS316 and SUS316L are generally used as stainless steels in contact with high-pressure hydrogen gas. SUS316 and SUS316L contain Mo. In contrast, Patent Document 1 discloses an austenitic stainless steel for high-pressure hydrogen that is inexpensive and has excellent mechanical strength and corrosion resistance and low hydrogen embrittlement susceptibility even at a low temperature of -40°C, and does not contain Mo. In the examples, test pieces that have been cold drawn at a cold working rate of 0 to 25% are evaluated for hydrogen embrittlement susceptibility by SSRT (Slow Strain Rate Test).

[0004] Patent Document 2 discloses a hydrogen-resistant spring stainless steel wire that is made of austenitic stainless steel having a specified composition, that has been subjected to a specified cold working, and that has a face-centered cubic (fcc) lattice crystal structure after the working. In the examples, after solution heat treatment, cold drawing is performed with a final working ratio of 0 to 75%, and the test pieces are charged with hydrogen before evaluation of bending stress and tensile stress.

[0005] Non-Patent Document 1 presents Md30 as an evaluation index of the austenite stability of austenitic stainless steel. Md30 is the temperature (°C) at which the structure transforms to 50% martensite phase when a tensile true strain of 0.30 is applied to a single-phase austenite sample. The higher this value, the more unstable the material is. Non-Patent Document 1 presents the formula for Md30 as a function of the component composition.

[0006] Patent Document 3 describes a steel having a predetermined composition including C: 0.15-0.80%, Ni: 8.0-20.0%, Cr: 8.0-18.0%, Mo: 0.05-0.50%, V: 0.50-3.00%, and Al: 0.001-1.000%, in which the value of formula (3) obtained by modifying the above Md30 formula described in Non-Patent Document 1 is set to -100 or less, and the number of V(C,N) precipitates of 50 nm or less is 3.5 × 10 -2 μm 2 The document discloses a low-cost, high-hardness non-magnetic steel that is characterized by having 50 or more dispersed particles therein, and that has excellent hydrogen embrittlement resistance, mechanical properties, and corrosion resistance.

[0007] Patent Document 4 discloses tilt rolling. In tilt rolling, three work rolls are arranged on a roll axis that is twisted and tilted in the same direction around the material to be rolled. Each work roll revolves around the material to be rolled while rotating on its own axis. As a result, the material to be rolled is rolled in a spiral shape while moving forward.

[0008] Conventionally, austenitic stainless steels such as SUS316 and SUS316L have been generally used as stainless steels for nonmagnetic parts. In contrast, Patent Documents 3 and 5 disclose a steel having a predetermined composition including C: 0.15-0.80%, Ni: 8.0-20.0%, Cr: 8.0-18.0%, Mo: 0.05-0.50%, V: 0.50-3.00%, and Al: 0.001-1.000%, in which the value of formula (3) obtained by modifying the above Md30 formula described in Non-Patent Document 1 is set to -100 or less, and the number of V(C,N) precipitates of 50 nm or less is 3.5×10 -2 μm 2The document discloses a low-cost, high-hardness non-magnetic steel that is characterized by having 50 or more dispersed particles therein, and that has excellent hydrogen embrittlement resistance, mechanical properties, and corrosion resistance. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2014-114471 A [Patent Document 2] JP 2009-84597 A [Patent Document 3] JP 2019-49036 A [Patent Document 4] Japanese Patent Application Publication No. 05-329510 [Patent Document 5] JP 2016-183372 A [Non-patent literature]

[0010] [Non-Patent Document 1] Nohara et al., "Dependence of Composition and Grain Size on the Strain-Induced Martensitic Transformation in Metastable Austenitic Stainless Steels," Iron and Steel, No. 5, 63 (1977), pp. 772-782 Summary of the Invention [Problem to be solved by the invention]

[0011] By using SUS316, SUS316L, or the austenitic stainless steels described in Patent Documents 1 to 3, steels that are excellent in hydrogen embrittlement resistance as well as mechanical strength and corrosion resistance are realized. These steels have excellent hydrogen embrittlement resistance after hot working or after cold working and then solid solution heat treatment. Patent Document 1 shows that steels that have been cold worked to a cold working rate of 25% or less, and Patent Document 2 shows that steels that have been cold worked to a final working rate of 75% or less, have excellent hydrogen embrittlement resistance even after cold working.

[0012] It was also found that it was difficult for the above-mentioned conventional steels to satisfy all of the requirements for cold forgeability, machinability, and hydrogen embrittlement resistance after cold working. In particular, in conventional techniques, the material strength before cold forging is high, resulting in a short tool life and an increased forging load for large-diameter steel bars. As a result, it was found that these factors caused the cold forgeability to deteriorate, as well as the machinability to deteriorate. It was also found that in processing with high strain such as cold forging, the conventional steels reached their material processing limit (cracks).

[0013] A second object of the present invention is to provide a stainless steel which has reduced tensile strength, increased cold forgeability, improved machinability, and further increased resistance to hydrogen embrittlement after cold working. [Means for solving the problem]

[0014] In the invention related to the original application, three inventions were created: a first invention corresponding to the first objective, a second invention corresponding to the second objective, and a third invention corresponding to the third objective. In the invention related to the present application, which is a divisional application of the original application, the following second invention is defined. That is, the gist of the present invention is as follows.

[0015] [7] <Second Invention> Chemical composition, in mass%, C:0.0010~0.15%, Si:0.01~2.00%, Mn:0.01~10.00%, Ni:8.00~30.00%, Cr:9.0~21.0%, Mo:0.01~3.00%, Cu:0.01~5.00%, N:0.0010~0.10%, B:0.0001~0.05%, S:0.0001~0.50%, Ti:0~2.00%, Nb:0~2.00%, Sn:0~2.5%, V:0~2.0%, W:0~3.0%, Ga:0~0.05%, Co:0~2.5%, Sb:0~2.5%, Ta:0~2.5% , Mg:0~0.012%, Zr:0~0.012%, REM:0~0.05%, Pb:0~0.30%, Se:0~0.80%, Te:0~0.30%, Bi:0~0.50%, P:0~0.30%, and further comprising Contains one or more selected from Al: 0.001 to 2.0%, Ca: 0.0001 to 0.05%, and the balance: Fe and impurities; The A value represented by the following formula (a) is -100 or less, A stainless steel characterized in that the amount of B precipitated as borides is 0.0001% or more and the aspect ratio of sulfides is 50 or less. A value=551-462(C+N)-9.2Si―8.1Mn―29(Ni+Cu)-13.7Cr―18.5Mo (a) However, the element symbol in formula (a) means the content (mass%) of the element in the steel. When the content of an element in formula (a) is 0%, "0" is substituted for the corresponding symbol in the calculation.

[0016] [8] The chemical composition further comprises, in mass %, Group A: one or more selected from Ti: 0.01-2.00%, Nb: 0.01-2.00%, Sn: 0.0001-2.5%, V: 0.001-2.0%, W: 0.05-3.0%, Ga: 0.0004-0.05%, Co: 0.05-2.5%, Sb: 0.01-2.5%, and Ta: 0.01-2.5%; As group B, one or more selected from Mg: 0.0002 to 0.012%, Zr: 0.0002 to 0.012%, and REM: 0.0002 to 0.05%; As group C, one or more selected from Pb: 0.0001 to 0.30%, Se: 0.0001 to 0.80%, Te: 0.0001 to 0.30%, Bi: 0.0001 to 0.50%, and P: 0.0001 to 0.30%; The stainless steel according to [7], which contains one or more of Groups A to C.

[0017] [9] The stainless steel according to [7] or [8], having a tensile strength of 700 MPa or less.

[10] The stainless steel according to any one of [7] to [9], having a limiting compressibility of 60% or more.

[11] The stainless steel according to any one of [7] to

[10] , having a drilling life index VL-1000 of 1 m / min or more.

[12] The stainless steel according to any one of [7] to

[11] , having a relative tensile strength in high-pressure hydrogen after cold working of 80% or more.

[13] The stainless steel according to any one of [7] to

[12] , having a relative reduction in area in high pressure hydrogen after cold working of 50% or more. Effect of the Invention

[0018] The stainless steel of the second invention contains specified components, and further contains one or both of Al and Ca, the amount of B precipitated as borides is 0.0001% or more, and the aspect ratio of the sulfides is 50 or less, thereby making it possible to satisfy all of the cold forgeability, machinability, and hydrogen embrittlement resistance after cold working. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The stainless steel of the present invention can be applied in either a bar shape or a plate shape. In particular, it is particularly suitable for use as a bar-shaped steel material. The bar-shaped steel material includes "steel bar," "wire rod," "steel wire," "deformed wire," "deformed steel bar," and the like. The stainless steel of the present invention is an austenitic stainless steel.

[0020] As described above, the second invention has an object to provide a stainless steel, particularly a bar-shaped steel material, which is capable of satisfying all of the requirements for cold forgeability, machinability, and hydrogen embrittlement resistance after cold working.

[0021] Regarding cold forgeability, a φ8 × 12 mm test piece is used, and an end-constrained compression test (processing temperature: RT (room temperature), strain rate: 10 / s) is performed. The maximum compression ratio at which no cracks occur on the side of the test piece after compression is defined as the limit compression ratio, and the target limit compression ratio is 60% or more.

[0022] To evaluate hydrogen embrittlement resistance after cold working, a sample was prepared by first performing solution heat treatment and then performing cold working with a cold working ratio of 80%. Two test pieces were prepared under the same processing conditions, one as a hydrogen test piece and the other as an air test piece. The hydrogen test piece was subjected to strain rate of 1×10 in a hydrogen atmosphere at -40°C and 70 MPa. -5 A tensile test is performed at a strain rate of 1 / s. For air test pieces, a tensile test is performed in air at the same strain rate. The strength and reduction of area are evaluated for each, and the evaluation result for the hydrogen test piece is divided by the evaluation result for the air test piece, and the percentage values ​​are the "relative strength" and "relative reduction of area," respectively. The goal of the first and second inventions is to achieve a relative strength of 80% or more and a relative reduction of area of ​​50% or more.

[0023] Machinability is evaluated based on the drill processing life index VL-1000 (the maximum peripheral speed (m / min) that can drill a hole with a cumulative hole depth of 1000 mm). The goal of the second invention is to achieve a VL-1000 of 1 m / min or more.

[0024] The second aspect of the invention will now be described in detail.

[0025] <Second Invention> Amount of B precipitated as boride in the steel material of the second invention The inventors came up with the idea of ​​controlling the amount of B precipitated as borides in a steel material as a means of satisfying all of the cold forgeability, machinability, and hydrogen embrittlement resistance after cold working in a stainless steel material. Regarding cold forgeability, the formation of borides reduces solid solution elements (such as N) and softens the material, improving the limit compression ratio during cold forging and improving cold forgeability. In addition, the borides precipitate finely, making them less likely to become the starting point of cracks, which also improves cold forgeability in this respect. Regarding machinability, the lubricating action of the borides extends the tool life during cutting. Regarding hydrogen embrittlement resistance, in addition to the softening caused by the formation of borides increasing dislocation mobility, the borides contribute as hydrogen trapping sites, improving hydrogen embrittlement resistance. Furthermore, by setting the amount of B precipitated as borides to 0.0001 mass% or more, in combination with the specification of the aspect ratio of sulfides described below, it is possible to satisfy all of the cold forgeability, machinability, and hydrogen embrittlement resistance after cold working.

[0026] The amount of B precipitated as borides in steel can be evaluated by subjecting the steel to electrolytic extraction residue, extracting the borides, and measuring the amount of B in the borides (Bpre).

[0027] <<Aspect ratio of sulfides in the steel material of the second invention>> The present inventors came up with the idea of ​​controlling the aspect ratio of sulfides in steel as a means for satisfying all of the cold forgeability, machinability, and hydrogen embrittlement resistance after cold working in stainless steel. If the aspect ratio of sulfides in steel is small, they are less likely to become fracture starting points, improving cold forgeability and hydrogen embrittlement resistance. In addition, if the aspect ratio of sulfides is small, the lubricating action increases, the tool life increases, and the machinability improves. And, if the aspect ratio of sulfides is 50 or less, in combination with the above-mentioned regulation of the amount of precipitated B as boride, all of the cold forgeability, machinability, and hydrogen embrittlement resistance after cold working can be satisfied. The aspect ratio means a value calculated as L / W from the length (L) of the sulfide in the rolling direction and the length (W) of the sulfide in the direction perpendicular to the rolling direction.

[0028] The aspect ratio of sulfides can be evaluated by measuring at least one field of view at 200x magnification in the L section of the steel (a section including the center line of the steel) at the surface layer, the center, and the 1 / 4 depth position between the surface layer and the center, and calculating the average value of the aspect ratios L / W of sulfides in the same field of view using an optical microscope.

[0029] <<Composition of the stainless steel according to the second invention>> Next, the chemical composition of the stainless steel according to the second aspect of the present invention will be described. In the chemical composition, % means mass %.

[0030] (B: 0.0001~0.05%) B is necessary to ensure the amount of B precipitated as the boride. By containing 0.0001% or more of B, in combination with the regulations of the manufacturing method described below, the amount of B precipitated as the boride can be ensured. The B content is more preferably 0.0005% or more. It is even more preferably 0.0020% or more. On the other hand, if the B content exceeds 0.05%, coarse borides are formed in the steel, and the coarse borides become the starting points of fracture, which deteriorates cold forgeability, machinability, and hydrogen embrittlement resistance, so the upper limit is 0.05%. The B content is more preferably 0.02% or less. It is even more preferably 0.015% or less.

[0031] (S:0.0001~0.50%) S is an element that forms sulfides in steel and improves machinability, and is contained at 0.0001% or more. On the other hand, excessive addition of S deteriorates cold forgeability, machinability, and hydrogen embrittlement resistance, so the upper limit is set to 0.50%, preferably 0.1% or less, and more preferably 0.05% or less. Note that S is usually contained in steel as an impurity mixed in from the steelmaking raw materials.

[0032] (Al: 0.001-2.0%, Ca: 0.0001-0.05%) The stainless steel of the second invention contains one or more selected from Al: 0.001-2.0% and Ca: 0.0001-0.05%. By containing one or more of Al and Ca at the above lower limit or more, Al- or Ca-based oxides are formed, which, in combination with the above-mentioned S content and the regulations of the production method described below, act as nuclei for sulfides, forming fine sulfides, and the aspect ratio of the sulfides after rolling can be set to 50 or less. Excessive addition of Al forms coarse AlN and the like, deteriorating cold forgeability, machinability, and hydrogen embrittlement resistance, and therefore the upper limit of the Al content is set to 2.0%, preferably 1.0% or less, more preferably 0.5% or less, and even more preferably 0.05% or less. Excessive addition of Ca forms coarse Ca-based inclusions, and the sulfides formed around them also become larger. The aspect ratio of the sulfides increases due to the expansion of the sulfides during rolling, and the cold forgeability, machinability, and hydrogen embrittlement resistance deteriorate. Therefore, the upper limit of the Ca content is set to 0.05%. Ca is preferably 0.010% or less, and more preferably 0.005% or less. If neither Al nor Ca is contained, or if the contents are outside the lower limit, the aspect ratio of the sulfides will deviate from the range of the present invention, resulting in poor tensile strength, limiting compression rate, machinability, and relative tensile strength and reduction in area after cold working.

[0033] (C:0.0010~0.15%) C suppresses the formation of processing-induced martensite and enhances hydrogen embrittlement resistance, so the content is set to 0.0010% or more. Excessive addition of C deteriorates cold forgeability, machinability, and hydrogen embrittlement resistance. Therefore, the upper limit of the C content is set to 0.15%, preferably 0.12% or less, more preferably 0.05% or less, and even more preferably 0.02% or less. It is preferable to set the upper limit of C to less than 0.15%.

[0034] (Si: 0.01 to 2.00%) Silicon is added as a deoxidizing element, and is set to 0.01% or more. Excessive addition of silicon deteriorates cold forgeability, machinability, and hydrogen embrittlement resistance. Therefore, the upper limit of the silicon content is set to 2.0%, preferably 1.2%, more preferably 0.6%, and even more preferably 0.5%.

[0035] (Mn: 0.01 to 10.00%) Mn suppresses the formation of processing-induced martensite and enhances hydrogen embrittlement resistance, so the content is set to 0.01% or more. Excessive addition of Mn deteriorates cold forgeability, machinability, and hydrogen embrittlement resistance. Therefore, the upper limit of the Mn content is set to 10.0%, preferably 2.5% or less, more preferably 1.5% or less, and even more preferably 1.0% or less.

[0036] (Ni: 8.00~30.00%) Ni suppresses the formation of processing-induced martensite and improves hydrogen embrittlement resistance. In addition, in order to improve cold forgeability, the Ni content is set to 8.00% or more. It is preferably 10.00% or more, more preferably 13.00% or more, and even more preferably 15.00% or more. Adding excessive Ni will adversely deteriorate cold forgeability, machinability, and hydrogen embrittlement resistance. Therefore, the upper limit of the Ni content is set to 30.00%, and preferably 25.00% or less.

[0037] (Cr: 9.0~21.0%) Cr suppresses the formation of processing-induced martensite and improves hydrogen embrittlement resistance. In order to improve corrosion resistance, the Cr content is set to 9.0% or more, preferably 10.5% or more. Excessive addition of Cr deteriorates cold forgeability, machinability, and hydrogen embrittlement resistance. Therefore, the upper limit of the Cr content is set to 21.0%, preferably 19.5% or less, and more preferably 15.0% or less.

[0038] (Mo: 0.01 to 3.00%) Mo suppresses the formation of processing-induced martensite and enhances hydrogen embrittlement resistance. In addition to enhancing corrosion resistance, Mo content is set to 0.01% or more in order to enhance cold forgeability. Excessive addition of Mo deteriorates cold forgeability, machinability, and hydrogen embrittlement resistance. Therefore, the upper limit of Mo content is set to 3.0%, preferably 2.8% or less, more preferably 2.5% or less, and even more preferably 1.0% or less.

[0039] (Cu: 0.01 to 5.00%) Cu suppresses the formation of processing-induced martensite and improves hydrogen embrittlement resistance. In order to improve cold forgeability, the Cu content is set to 0.01% or more. It is preferably set to 1.00% or more, and more preferably set to 2.00% or more. Excessive addition of Cu deteriorates cold forgeability, machinability, and hydrogen embrittlement resistance, and also causes hot embrittlement. Therefore, the upper limit of the Cu content is set to 5.00%, and preferably set to 3.50% or less.

[0040] (N:0.0010~0.10%) N suppresses the formation of processing-induced martensite and enhances hydrogen embrittlement resistance, so the content is set to 0.0010% or more. Excessive addition of N deteriorates cold forgeability, machinability, and hydrogen embrittlement resistance. Therefore, the upper limit of the N content is set to 0.10%, preferably 0.08% or less, more preferably 0.05% or less, and even more preferably 0.03% or less.

[0041] The stainless steel of the second invention contains the above-mentioned components, with the balance being Fe and impurities. It may further contain one or more components selected from the following components:

[0042] (Ti: 0-2.00%) Ti may be added to fix C and N, which increase microstrain. On the other hand, excessive addition of Ti forms coarse Ti-based precipitates, which deteriorates cold forgeability, machinability, and hydrogen embrittlement resistance. Therefore, the upper limit of the Ti content is set to 2.00%, preferably 1.0% or less, more preferably 0.7% or less, and even more preferably 0.5% or less. The preferred lower limit of Ti is 0.01% or more, and even more preferably 0.05% or more.

[0043] (Nb: 0-2.00%) Nb may be added to fix C and N. On the other hand, excessive addition of Nb forms coarse Nb-based precipitates, which deteriorates cold forgeability, machinability, and hydrogen embrittlement resistance. Therefore, the upper limit of the Nb content is set to 2.00%, preferably 1.0% or less, more preferably 0.7% or less, and even more preferably 0.5% or less. The preferred lower limit of Nb is 0.01% or more, and even more preferably 0.05% or more.

[0044] (Sn: 0-2.5%) Sn is an effective element for improving corrosion resistance, so it may be contained. However, if Sn is contained in excess, the effect is saturated, and conversely, there is a risk of deterioration in cold forgeability, machinability, and hydrogen embrittlement resistance. Therefore, the upper limit of Sn content is set to 2.5%. More preferably, it is 1.0% or less, and even more preferably, it is 0.2% or less. In order to exert the above effect, the Sn content is preferably 0.0001% or more, and even more preferably, it is 0.01% or more. More preferably, it is 0.05% or more.

[0045] (V:0~2.0%) V may be added to fix C and N. On the other hand, excessive V addition forms coarse V-based precipitates, which deteriorates cold forgeability, machinability, and hydrogen embrittlement resistance. Therefore, the upper limit of the V content is set to 2.0%, preferably 1.0% or less, more preferably 0.7% or less, and even more preferably 0.5% or less. The preferable lower limit of V is 0.001%.

[0046] (W:0~3.0%) W may be contained since it is an effective element for improving corrosion resistance. However, if W is contained in excess, the effect is saturated, and conversely, there is a risk of deterioration in cold forgeability, machinability, and hydrogen embrittlement resistance. Therefore, the upper limit of W content is set to 3.0%. More preferably, it is 2.0% or less, and further preferably, it is 1.5% or less. In order to exert the above effect, it is preferable that the W content is 0.05% or more. More preferably, it is 0.10% or more.

[0047] (Ga: 0~0.05%) Ga is an effective element for improving corrosion resistance, so it may be contained. However, if Ga is contained in excess, the effect is saturated, and there is a risk that cold forgeability, machinability, and hydrogen embrittlement resistance may be deteriorated. Therefore, the upper limit of Ga content is set to 0.05%. To achieve the above effect, it is preferable that the Ga content is 0.0004% or more.

[0048] (Co: 0-2.5%) Co may be contained since it has the effect of improving corrosion resistance. However, if Co is contained in excess, the effect is saturated, and conversely, there is a risk of deterioration in cold forgeability, machinability, and hydrogen embrittlement resistance. Therefore, the upper limit of Co content is set to 2.5%. More preferably, it is 1.0% or less, and even more preferably, it is 0.8% or less. In order to exert the above effect, it is preferable that the Co content is 0.05% or more, and more preferably, it is 0.10% or more.

[0049] (Sb: 0-2.5%) Sb may be contained since it has the effect of improving corrosion resistance. However, if Sb is contained in excess, the effect is saturated, and conversely, there is a risk of deterioration in cold forgeability, machinability, and hydrogen embrittlement resistance. Therefore, the upper limit of Sb content is set to 2.5%. More preferably, it is 1.0% or less, and even more preferably, it is 0.8% or less. In order to exert the above effect, the Sb content is preferably 0.01% or more, and more preferably 0.05% or more.

[0050] (Ta: 0~2.5%) Ta may be added to fix C and N. On the other hand, excessive Ta addition forms coarse Ta-based precipitates, which deteriorates cold forgeability, machinability, and hydrogen embrittlement resistance. Therefore, the upper limit of the Ta content is set to 2.5%, preferably 1.0% or less, more preferably 0.7% or less, and even more preferably 0.5% or less. The preferred lower limit of Ta is 0.01%.

[0051] (Mg: 0~0.012%) Mg may be added as necessary for deoxidation. On the other hand, excessive addition of Mg forms coarse Mg-based inclusions, which deteriorates cold forgeability, machinability, and hydrogen embrittlement resistance. Therefore, the upper limit of the Mg content is set to 0.012%, preferably 0.010% or less, and more preferably 0.005% or less. The preferable lower limit of Mg is 0.0002%.

[0052] (Zr: 0~0.012%) Zr may be added as necessary for deoxidation. On the other hand, excessive addition of Zr forms coarse Zr-based inclusions, which deteriorates cold forgeability, machinability, and hydrogen embrittlement resistance. Therefore, the upper limit of the Zr content is set to 0.012%, preferably 0.010% or less, and more preferably 0.005% or less. The preferable lower limit of Zr is 0.0002%.

[0053] (REM: 0~0.05%) REM may be added as necessary for deoxidization. On the other hand, excessive addition of REM will form coarse REM inclusions, deteriorating cold forgeability, machinability, and hydrogen embrittlement resistance. Therefore, the upper limit of the REM content is set to 0.05%, preferably 0.010% or less, and more preferably 0.005% or less. The preferred lower limit of REM is 0.0002%.

[0054] (Pb: 0~0.30%) Pb is an element that improves machinability and may be contained as necessary. On the other hand, excessive addition of Pb deteriorates cold forgeability, machinability, and hydrogen embrittlement resistance. Therefore, the upper limit of the Pb content is set to 0.30%, preferably 0.10% or less, and more preferably 0.05% or less. The preferred lower limit of Pb is 0.0001%.

[0055] (Se:0~0.80%) Se is an element that improves machinability and may be contained as necessary. On the other hand, excessive addition of Se deteriorates cold forgeability, machinability, and hydrogen embrittlement resistance. Therefore, the upper limit of the Se content is set to 0.80%, preferably 0.1% or less, and more preferably 0.05% or less. The preferable lower limit of Se is 0.0001%.

[0056] (Te:0~0.30%) Te is an element that improves machinability and may be contained as necessary. On the other hand, excessive addition of Te deteriorates cold forgeability, machinability, and hydrogen embrittlement resistance. Therefore, the upper limit of the Te content is set to 0.30%, preferably 0.1% or less, and more preferably 0.05% or less. The preferred lower limit of Te is 0.0001%.

[0057] (Bi: 0~0.50%) Bi is an element that improves machinability and may be contained as necessary. On the other hand, excessive addition of Bi deteriorates cold forgeability, machinability, and hydrogen embrittlement resistance. Therefore, the upper limit of the Bi content is set to 0.50%, preferably 0.1% or less, and more preferably 0.05% or less. The preferred lower limit of Bi is 0.0001%.

[0058] (P:0~0.30%) P is an element that improves machinability and may be contained as necessary. On the other hand, excessive addition of P deteriorates cold forgeability, machinability, and hydrogen embrittlement resistance. Therefore, the upper limit of the P content is set to 0.30%, preferably 0.1% or less, and more preferably 0.05% or less. The preferable lower limit of P is 0.0001%.

[0059] <Common to the first to third inventions> <<A value in formula (a)>> Based on the formula for Md30 described in Non-Patent Document 1, the following formula (a) was introduced. A value=551-462(C+N)-9.2Si―8.1Mn―29(Ni+Cu)-13.7Cr―18.5Mo (a) The element symbol in formula (a) means the content (mass%) of the element in the steel. When the content of an element in formula (a) is 0%, the corresponding symbol is substituted with "0" for the calculation. The above formula (a) corresponds to the formula for Md30 described in Non-Patent Document 1 with the Nb term deleted. The reason for deleting the Nb term is that the addition ratio of Nb is small and its contribution to Md30 is small. In the first to third inventions, the A value shown in the above formula (a) is -100 or less. By making the A value -100 or less, the formation of processing-induced martensite is suppressed, and work hardening is reduced, resulting in softening and suppressing the occurrence of cracks, thereby improving cold forgeability. Furthermore, the first invention can obtain the effect of reducing microstrain and improving hydrogen embrittlement resistance. The second invention can obtain the effect of reducing cutting resistance and improving machinability by softening. As for hydrogen embrittlement resistance, processing-induced martensite at the fracture origin is reduced, improving hydrogen embrittlement resistance. The third invention can obtain the effect of improving non-magnetic properties.

[0060] Quality of the steel materials according to the first to third inventions The stainless steel of the present invention, particularly the bar-shaped steel material, can achieve the following qualities as a result of having the above-mentioned component composition, and further, as a result of having a microstrain of D / 4 in the steel material surface layer in the first invention, as a result of having an amount of B precipitated as borides and an aspect ratio of sulfides in the second invention, and as a result of having a B grain boundary occupancy rate in the steel material in the third invention.

[0061] <Common to the first to third inventions> The stainless steel may have a tensile strength of 700 MPa or less. <Common to the first to third inventions> The stainless steel may have a limit compression ratio of 60% or more. Here, the evaluation of the limit compression ratio shall be performed in the same manner as described above, with respect to the shape of the test piece, the content of the compression test, and the definition of the limit compression ratio.

[0062] <Common to the first and second inventions> The stainless steel may have a relative tensile strength in high-pressure hydrogen after cold working of 80% or more. <Common to the first and second inventions> The stainless steel may have a relative reduction in area of ​​50% or more in high-pressure hydrogen after cold working. Here, the cold working rate (reduction of area) of the above cold working is 80%. The tensile strength and reduction of area in high-pressure hydrogen were evaluated in a hydrogen atmosphere, -40°C, 70 MPa environment, and strain rate of 1×10 -5 The tensile strength and reduction of area in the hydrogen atmosphere thus obtained are divided by the tensile strength and reduction of area evaluated at the same strain rate in the air atmosphere, and the percentage values ​​are the relative tensile strength and relative reduction of area in high pressure hydrogen.

[0063] <Second Invention> The stainless steel may have a drilling life index VL-1000 of 1 m / min or more.

[0064] <<Method of manufacturing steel material according to the second invention>> The method for producing the steel material according to the second aspect of the present invention will be described below.

[0065] <Second Invention> In producing the stainless steel of the second invention, particularly a steel bar, it is preferable to employ tilt rolling as the hot working method and to use induction heating for heating the material before tilt rolling.

[0066] A set temperature is provided in an induction heating device for heating a steel material to be rolled. The set temperature is specified to 1000 to 1400°C, and the speed at which the rolling material passes through the induction heating device is set to a range of 0.003 to 4.0 m / s. It is more preferable that the set temperature is within a range of 1000 to 1300°C, and the speed at which the rolling material passes is within a range of 0.005 to 2.0 m / s. The set temperature is more preferably 1050 to 1300°C, and even more preferably 1100 to 1300°C. The speed at which the material passes is more preferably 0.01 to 2.0 m / s, and even more preferably 0.1 to 1.0 m / s. By setting the induction heating device temperature and material passing speed within the above ranges, in combination with the inclusion of B in the steel, the amount of B precipitated as borides in the steel can be made 0.0001% or more. In addition, by setting the temperature of the induction heating device and the material passing speed within the above ranges, in combination with the inclusion of S in the steel and at least one of Al and Ca, the aspect ratio of the sulfides can be made 50 or less.

[0067] If the set temperature of the induction heating device is less than 1000°C, the amount of precipitated B decreases, the aspect ratio of the sulfides increases, and coarse undissolved precipitates remain, resulting in deterioration of cold forgeability, machinability, and hydrogen embrittlement resistance. If the temperature exceeds 1400°C, the amount of precipitated B decreases and the aspect ratio increases due to the elongation of the sulfides, resulting in deterioration of cold forgeability, machinability, and hydrogen embrittlement resistance. In addition, high-temperature heating causes oxidation of the steel material, resulting in a decrease in yield, or the steel material creeps and deforms during passage, resulting in poor rolling. In addition, if the speed of the rolling material passing through the induction heating device is less than 0.003 m / s, the amount of precipitated B decreases and the sulfides elongate, resulting in a high aspect ratio of the sulfides, resulting in deterioration of cold forgeability, machinability, and hydrogen embrittlement resistance. When the speed of the material passing through the induction heating device exceeds 4.0 m / s, the amount of precipitated B decreases, the aspect ratio of the sulfides increases, and coarse undissolved precipitates remain, resulting in deterioration of cold forgeability, machinability, and hydrogen embrittlement resistance. In addition, high-temperature heating causes oxidation of the steel material, resulting in a decrease in yield, or the steel material creeps and deforms during passage, resulting in poor rolling. The set temperature of the induction heating device specifically means the output temperature within the induction heating device through which the steel material passes.

[0068] After the rolling material is heated in this way, tilt rolling is performed. As disclosed in Patent Document 4, for example, in the tilt rolling, three work rolls are arranged on a roll axis that is twisted and tilted in the same direction around the rolled material, and each work roll revolves around the rolled material while rotating. As a result, the rolled material is rolled in a spiral shape while moving forward. Regarding the temperature distribution of the rolling material when performing tilt rolling, the temperature distribution is set so that the steel temperature from the steel surface layer to the D / 4 position uniformly coincides with the set temperature. As a result, the amount of precipitated B is reduced and the elongation of sulfides is suppressed, thereby improving cold forgeability, machinability, and hydrogen embrittlement resistance. In addition, the above process causes coarse undissolved precipitates to disappear and precipitates to become finer, which also contributes to improving cold forgeability, machinability, and hydrogen embrittlement resistance.

[0069] After the tilt rolling, it is preferable to carry out in-line heat treatment, hot rolling, heat treatment, pickling, etc. After that, the shape of the steel material may be adjusted by peeling, drawing, etc.

[0070] In the manufacturing method of the steel material according to the second aspect of the present invention, it is preferable to perform hot working by using tilt rolling as described above. Note that the hot working is not limited to tilt rolling, and any method that follows a similar thermal processing history may be used, for example, blooming (breakdown) rolling may be used as long as it provides a similar thermal processing history. EXAMPLES

[0071] <Second Invention> (Example 2-1) The steel was melted in a 100 kg vacuum melting furnace, assuming AOD melting, which is an inexpensive process for melting stainless steel, and cast into a slab with a diameter of 180 mm. Then, stainless steel bars with a diameter of 20.0 mm and chemical compositions shown in Tables 1 to 3 were manufactured under the manufacturing conditions below. In Tables 1 to 6, items outside the range of the second invention and items outside the preferred manufacturing conditions of the second invention are underlined.

[0072] [Table 1]

[0073] [Table 2]

[0074] [Table 3]

[0075] The cast slab was heated to 1130°C in a heating furnace, and then induction heating was used to heat the rolling material before tilt rolling. The induction heating device was set to a temperature of 1210°C and the material passing speed through the induction heating device was 0.3 m / s. The material was then tilt rolled, subjected to in-line heat treatment and bar wire rolling, and then subjected to offline heat treatment at 1100°C for 30 minutes (water cooling). The material was then pickled and produced into a bar-shaped steel material with a diameter of 20.0 mm.

[0076] The methods used for measuring the amount of precipitated B as borides in the bar-shaped steel material, the aspect ratio of sulfides, the limiting compression ratio, the VL-1000 drilling life index evaluation method, and the relative tensile strength and relative reduction in area after cold working were as described above.

[0077] The amount of B precipitated as borides was rated by mass as AA for 0.0010% or more, A for 0.0005% or more but less than 0.0010%, B for 0.0001% or more but less than 0.0005%, and C for less than 0.0001%. Note that when coarse borides were formed due to an excessive B content, they were rated as CC. Regarding the aspect ratio of sulfides, 5 or less was rated as AA, more than 5 and less than 30 was rated as A, more than 30 and less than 50 was rated as B, and more than 50 was rated as C. Regarding tensile strength, 500 MPa or less was rated AA, between 500 MPa and 620 MPa was rated A, between 620 MPa and 700 MPa was rated B, and over 700 MPa was rated C. Regarding the limiting compression rate, 80% or more was rated AA, 70% or more but less than 80% was rated A, 60% or more but less than 70% was rated B, and less than 60% was rated C. For the VL-1000 drilling life index, 20 m / min or more was rated AA, 10 m / min to less than 20 m / min was rated A, 1 m / min to less than 10 m / min was rated B, and less than 1 m / min was rated C. Regarding the relative tensile strength in high-pressure hydrogen after cold working, 95% or more was rated AA, 90% or more but less than 95% was rated A, 80% or more but less than 90% was rated B, and less than 80% was rated C. Regarding the relative reduction in area in high pressure hydrogen after cold working, 70% or more was rated AA, 60% or more but less than 70% was rated A, 50% or more but less than 60% was rated B, and less than 50% was rated C. The evaluation results are shown in Tables 4 and 5.

[0078] [Table 4]

[0079] [Table 5]

[0080] The bar-shaped steel materials described in Inventive Examples No. 1 to 39 had the chemical composition, the amount of precipitated B as borides, and the aspect ratio of sulfides specified in the second invention, and were good in terms of tensile strength, limit compression ratio, VL-1000, relative tensile strength after cold working, and reduction in area, all of which were AA, A, or B.

[0081] On the other hand, in Comparative Examples 40 to 50 and 52 to 56, any of the components was outside the range of the second invention, and the amount of precipitated B as borides and the aspect ratio of sulfides were outside the range of the second invention, and as a result, the tensile strength, the limit compression ratio, VL-1000, the relative tensile strength and the reduction in area after cold working were all C. In Comparative Example 51, coarse borides were formed due to the excessive B content, and the coarse borides became the starting point of fracture, and as a result, the tensile strength, the limit compression ratio, VL-1000, the relative tensile strength and the reduction in area after cold working were all C.

[0082] (Example 2-2) Steel type P in Table 1 was used as the component composition, the induction heating conditions before tilt rolling were as shown in Table 6, and the other manufacturing conditions were the same as in Example 2-1 above to manufacture steel bars.

[0083] [Table 6]

[0084] As shown in Table 6, inventive examples Nos. 55 to 64, the manufacturing method was performed under the preferred conditions of the second invention, and they had the component composition, the amount of precipitated B as borides, and the aspect ratio of sulfides specified in the second invention. The tensile strength, limit compression ratio, relative tensile strength and reduction of area after cold working were all either AA, A, or B, and were good.

[0085] On the other hand, for Comparative Examples 65 to 70, any of the manufacturing conditions was outside the preferred range of the second invention, and the amount of precipitated B as borides and the aspect ratio of sulfides were outside the range of the second invention. As a result, the tensile strength, limit compression rate, VL-1000, relative tensile strength and reduction of area after cold working were all C.

Claims

1. The chemical composition, in mass%, is C: 0.0010 to 0.15%, Si: 0.01-2.00%, Mn: 0.01-10.00%, Ni: 8.00-30.00%, Cr: 9.0-21.0%, Mo: 0.01-3.00%, Cu: 0.01-5.00%, N: 0.0010 to 0.10%, B: 0.0001 to 0.05%, S: 0.0001-0.50%, Ti: 0-2.00%, Nb: 0 to 2.00%, Sn: 0 to 2.5%, V: 0 to 2.0%, W: 0 to 3.0%, Ga: 0-0.05%, Co: 0 to 2.5%, Sb: 0 to 2.5%, Ta: 0 to 2.5%, Mg: 0 to 0.012%, Zr: 0 to 0.012%, REM: 0-0.05%, Pb: 0 to 0.30%, Se: 0-0.80%, Te: 0 to 0.30%, Bi: 0 to 0.50%, P: 0-0.30%, and further comprising Al: 0.001-2.0%, Ca: 0.0001-0.05%, Contains one or more selected from The balance is Fe and impurities. The A value represented by the following formula (a) is −100 or less, A stainless steel characterized in that the amount of precipitated B as borides is 0.0001% or more and the aspect ratio of sulfides is 50 or less. A value=551-462(C+N)-9.2Si-8.1Mn-29(Ni+Cu)-13.7Cr-18.5Mo (a) In the formula (a), the symbol of an element means the content (mass%) of the element in the steel. When the content of an element in the formula (a) is 0%, "0" is substituted for the corresponding symbol in the calculation.

2. The chemical composition further comprises, in mass %, As group A, Ti: 0.01-2.00%, Nb: 0.01-2.00%, Sn: 0.0001 to 2.5%, V: 0.001-2.0%, W: 0.05-3.0%, Ga: 0.0004-0.05%, Co: 0.05-2.5%, Sb: 0.01 to 2.5%, and Ta: 0.01-2.5%, One or more selected from As group B, Mg: 0.0002-0.012%, Zr: 0.0002 to 0.012%, and REM: 0.0002-0.05%, One or more selected from As group C, Pb: 0.0001 to 0.30%, Se: 0.0001-0.80%, Te: 0.0001 to 0.30%, Bi: 0.0001 to 0.50%, and P: 0.0001-0.30%, One or more selected from Contains one or more of groups A to C of The stainless steel of claim 1.

3. 3. The stainless steel according to claim 1 or 2, having a tensile strength of 700 MPa or less.

4. 3. The stainless steel according to claim 1, wherein the limit compression ratio is 60% or more.

5. The stainless steel according to claim 1 or 2, having a drilling life index VL-1000 of 1 m / min or more.

6. 3. The stainless steel according to claim 1, which has a relative tensile strength in high-pressure hydrogen after cold working of 80% or more.

7. 3. The stainless steel according to claim 1, which has a relative reduction in area in high pressure hydrogen after cold working of 50% or more.

8. The stainless steel according to claim 3, having a limiting compressibility of 60% or more.

9. The stainless steel according to claim 3, having a drilling life index VL-1000 of 1 m / min or more.

10. The stainless steel according to claim 4, having a drilling life index VL-1000 of 1 m / min or more.

11. The stainless steel according to claim 8, having a drilling life index VL-1000 of 1 m / min or more.

12. 4. The stainless steel according to claim 3, having a relative tensile strength in high pressure hydrogen after cold working of 80% or more.

13. 5. The stainless steel according to claim 4, which has a relative tensile strength in high pressure hydrogen after cold working of 80% or more.

14. 6. The stainless steel according to claim 5, having a relative tensile strength in high pressure hydrogen after cold working of 80% or more.

15. 9. The stainless steel according to claim 8, having a relative tensile strength in high pressure hydrogen after cold working of 80% or more.

16. 10. The stainless steel according to claim 9, having a relative tensile strength in high pressure hydrogen after cold working of 80% or more.

17. 11. The stainless steel according to claim 10, having a relative tensile strength in high pressure hydrogen after cold working of 80% or more.

18. 12. The stainless steel according to claim 11, having a relative tensile strength in high pressure hydrogen after cold working of 80% or more.

19. 4. The stainless steel according to claim 3, which has a relative reduction in pressure in high pressure hydrogen after cold working of 50% or more.

20. 5. The stainless steel according to claim 4, which has a relative reduction in area in high pressure hydrogen after cold working of 50% or more.

21. 6. The stainless steel according to claim 5, which has a relative reduction in area in high pressure hydrogen after cold working of 50% or more.

22. 9. The stainless steel according to claim 8, having a relative reduction in pressure in high pressure hydrogen after cold working of 50% or more.

23. 10. The stainless steel according to claim 9, having a relative reduction in pressure in high pressure hydrogen after cold working of 50% or more.

24. The stainless steel according to claim 10, having a relative reduction in pressure in high pressure hydrogen after cold working of 50% or more.

25. The stainless steel according to claim 11, having a relative reduction in pressure in high pressure hydrogen after cold working of 50% or more.

Citation Information

Patent Citations

  • Wire rod of nonmagnetic sulfur free-cutting stainless steel superior in cold drawability and corrosion resistance

    JP2004307977A

  • Soft austenitic stainless steel and manufacturing method therefor

    JP2008208430A

  • Austenitic stainless free-cutting steel having excellent cold forgeability and machinability

    JP2008240053A

  • Austenitic stainless steel

    JP2017160520A

  • Nonmagnetic austenitic stainless steel sheet and method for producing nonmagnetic member

    JP2018109215A