Processing method of wafer

The method addresses improper modified layer formation by incorporating protective tape, unevenness detection, and foreign material removal to ensure precise wafer separation into device chips, enhancing the dicing process's reliability and quality.

JP2024138636APending Publication Date: 2024-10-09DISCO CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023049225
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

The formation of an inappropriate modified layer along the dividing line of a wafer due to foreign matter on the chuck table causes improper wafer separation, leading to potential damage or chipping of device chips during the dicing process.

Method used

A method involving protective tape disposal, wafer holding, unevenness detection, and foreign material removal steps to ensure proper formation of a modified layer by positioning a laser beam within the wafer, followed by grinding to separate the wafer into individual device chips.

Benefits of technology

Ensures accurate division of wafers into device chips without damage by addressing unevenness and foreign matter, thereby improving the quality and reliability of the dicing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138636000001_ABST
    Figure 2024138636000001_ABST
Patent Text Reader

Abstract

To provide a processing method of a wafer, for forming a proper modified layer along a division schedule line of the wafer, and dividing the wafer into individual device chips.SOLUTION: A method executes steps of: distributing a protection tape T1 onto a front surface of a wafer 10; holding the protection tape side to a holding surface of a chuck table 35, and exposing a back surface 10b of the wafer; and detecting unevenness of the back surface of the wafer by concave and convex detection means 7. In addition, if a concave and convex height Z1 detected is within a permission range, a step of positioning a focal point of a laser beam of a wavelength having a transmissivity to the wafer at an inner part of the wafer corresponding to the division schedule line for irradiation, and forming a modified layer. If the concave and convex height detected is out of the permission range, a step of cleaning the holding surface of the chuck table and a protection tape distributed to the wafer by fetching out the wafer from the chuck table, and removing a foreign material, and a step of holding the wafer again after the removing of the foreign material, and detecting the unevenness.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for processing a wafer having a surface on which a plurality of devices are defined by dividing lines. [Background technology]

[0002] Wafers, on whose surface multiple devices such as ICs and LSIs are formed, are divided along division lines. These are then separated into individual device chips using a dicing machine or laser processing machine. These are then used in electrical devices such as mobile phones and personal computers.

[0003] The laser processing equipment has a chuck table having a holding surface that holds the tape side arranged on the front surface of the wafer, and irradiates the back surface of the wafer held on the chuck table with a laser beam having a wavelength that is transparent to the wafer, positioning the focal point inside the wafer corresponding to the intended division line to form a modified layer that serves as the starting point for division.The tape is then expanded to apply an external force to the wafer, dividing the wafer into individual device chips along the modified layer (see, for example, Patent Document 1).

[0004] Alternatively, after forming a modified layer along the intended division line by a laser processing device as described above, the tape side can be held on a chuck table of a grinding device that grinds the back surface of the wafer, and the back surface of the wafer can be ground to thin the wafer and divide the wafer along the modified layer into individual device chips (see, for example, Patent Document 2). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2005-251986 A [Patent Document 2] Patent Publication No. 2021-068872 Summary of the Invention [Problem to be solved by the invention]

[0006] However, when forming a modified layer along the planned dividing lines of the wafer, if foreign matter adheres to the surface of the protective tape that is held by the chuck table or to the holding surface of the chuck table, the foreign matter will cause the wafer to partially lift up, and the focal point of the laser beam will not be positioned at the correct position inside the wafer, resulting in an insufficient modified layer, which will result in the wafer not being divided into individual device chips as intended or will cause chips to form in the device chips.

[0007] The present invention has been made in consideration of the above-mentioned facts, and its main technical object is to provide a wafer processing method capable of forming an appropriate modified layer along the planned dividing lines of the wafer, thereby dividing the wafer into individual device chips. [Means for solving the problem]

[0008] In order to solve the above-mentioned main technical problem, according to the present invention, there is provided a wafer processing method for processing a wafer having a surface into which a plurality of devices are partitioned by planned dividing lines, the method including a protective tape applying step of applying a protective tape to the surface of the wafer, a wafer holding step of holding the protective tape side on a holding surface of a chuck table and exposing the back surface of the wafer, and an unevenness detection step of detecting unevenness on the back surface of the wafer, in which, if the unevenness detected in the unevenness detection step is within an allowable range, a modified layer forming step is carried out in which a focal point of a laser beam having a wavelength that is transparent to the wafer is positioned inside the wafer corresponding to the planned dividing lines and the laser beam is irradiated to form a modified layer, and if the unevenness detected in the unevenness detection step is outside the allowable range, a foreign matter removal step is carried out in which the wafer is removed from the chuck table, and the holding surface of the chuck table and the protective tape disposed on the wafer are cleaned to remove foreign matter, and after the foreign matter removal step, the wafer holding step and the unevenness detection step are carried out again.

[0009] In the unevenness detection step, it is preferable to detect unevenness by measuring the height of the back surface of the wafer corresponding to the planned dividing line by a laser measuring device. Also, it is preferable to include a grinding step after the modified layer formation step, in which the protective tape side of the wafer is held on a chuck table of a grinding device to grind and thin the back surface of the wafer, and the wafer is divided into individual device chips along the modified layer. Effect of the Invention

[0010] The wafer processing method of the present invention is a method for processing a wafer having a surface into which a plurality of devices are partitioned by planned dividing lines, and includes a protective tape applying step of applying a protective tape to the surface of the wafer, a wafer holding step of holding the protective tape side on a holding surface of a chuck table and exposing the back surface of the wafer, and an unevenness detecting step of detecting unevenness on the back surface of the wafer, and if the unevenness detected in the unevenness detecting step is within an allowable range, a modified layer is formed by irradiating the wafer with a focused point of a laser beam having a wavelength that is transparent to the wafer, positioned inside the wafer corresponding to the planned dividing lines. A modified layer forming step is carried out, and if the unevenness detected by the unevenness detection step is outside the allowable range, a foreign matter removal step is carried out in which the wafer is removed from the chuck table and the holding surface of the chuck table and the protective tape placed on the wafer are cleaned to remove any foreign matter. After the foreign matter removal step, the wafer holding step and the unevenness detection step are carried out again. This eliminates the problem that the modified layer forming step is carried out with the back surface of the wafer in a proper state, resulting in an insufficient modified layer, which makes it impossible to properly divide the wafer into individual device chips or causes chips to form in the device chips. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is an overall perspective view of the laser processing device. [Diagram 2] FIG. 11 is a perspective view showing an embodiment of a protective tape disposing step. [Diagram 3] FIG. 13 is a perspective view showing an embodiment of a wafer holding step. [Figure 4] FIG. 11 is a perspective view showing an embodiment of an unevenness detection step. [Diagram 5] 1A is a perspective view showing how a thermo-compression sheet is pressed onto a chuck table in a foreign matter removal step, and FIG. 1B is a perspective view showing how the thermo-compression sheet is peeled off from the chuck table. [Figure 6] 1 is a perspective view showing a mode of removing foreign matter from a protective tape disposed on a wafer. FIG. [Figure 7] FIG. 2A is a perspective view showing an embodiment of a modified layer forming step, and FIG. 2B is a partially enlarged cross-sectional view of a wafer in the modified layer forming step shown in FIG. [Figure 8] FIG. 1 is a perspective view showing an embodiment of a grinding process. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, an embodiment of the wafer processing method of the present invention will be described in detail with reference to the accompanying drawings.

[0013] 1 shows an overall perspective view of a laser processing apparatus 1 suitable for carrying out the wafer processing method of this embodiment. The laser processing apparatus 1 is provided with a holding means 3 arranged on a base 2 and holding a wafer 10 (see FIG. 2) which is a workpiece, a feed means 4 for moving the holding means 3 in the X-axis direction and the Y-axis direction in the figure, a frame 5 consisting of a vertical wall portion 5a erected on the side of the feed means 4 of the base 2 and a horizontal wall portion 5b extending horizontally from the upper end of the vertical wall portion 5a, an alignment means 6 for imaging the wafer 10 held by the holding means 3 and performing alignment, an unevenness detection means 7 for detecting unevenness on the back surface 10b of the wafer 10, a laser beam application means 8 for applying a laser beam having a wavelength that is transparent to the wafer 10, a display means 9, and a control means 20.

[0014] An optical system constituting the above-mentioned laser beam application means 8 is housed inside the horizontal wall 5b of the frame 5. A condenser 81 that constitutes part of the optical system of the laser beam application means 8 and condenses and irradiates the laser beam on the wafer 10 held by the holding means 3 is disposed on the underside of the tip of the horizontal wall 5b. The alignment means 6 and the unevenness detection means 7 are disposed at positions adjacent to the condenser 81 in the X-axis direction indicated by the arrow X in the figure.

[0015] As shown in FIG. 1, the holding means 3 includes a rectangular X-axis direction movable plate 31 mounted on the base 2 so as to be movable in the X-axis direction, a rectangular Y-axis direction movable plate 32 mounted on the X-axis direction movable plate 31 so as to be movable in the Y-axis direction, a cylindrical support 33 fixed to the upper surface of the Y-axis direction movable plate 32, and a rectangular cover plate 34 fixed to the upper end of the support 33. A chuck table 35 is disposed on the cover plate 34 and extends upward through an elongated hole formed in the cover plate 34. The chuck table 35 is configured to be rotatable by a rotation drive means (not shown) housed in the support 33. A circular suction chuck formed of a porous material having air permeability and extending substantially horizontally is disposed on the upper surface of the chuck table 35 to form a holding surface 35a. The holding surface 35a is connected to a suction means (not shown) by a flow path passing through the support 33.

[0016] The feed means 4 includes an X-axis feed means 41 and a Y-axis feed means 42. The X-axis feed means 41 converts the rotational motion of the motor 43 into linear motion via a ball screw 44, transmits the motion to the X-axis movable plate 31, and moves the X-axis movable plate 31 forward and backward in the X-axis direction along a pair of guide rails 2a, 2a arranged on the base 2 along the X-axis direction. The Y-axis feed means 42 converts the rotational motion of the motor 46 into linear motion via a ball screw 45, transmits the motion to the Y-axis movable plate 32, and moves the Y-axis movable plate 32 forward and backward in the Y-axis direction along a pair of guide rails 31a, 31a arranged on the X-axis movable plate 31 along the Y-axis direction.

[0017] The alignment means 6 includes a conventional imaging element (CCD) that uses visible light to capture an image of the workpiece held on the chuck table 35, an infrared irradiation means that irradiates the workpiece with infrared rays, an optical system that captures the infrared rays irradiated by the infrared irradiation means, and an imaging element (infrared CCD) that outputs an electrical signal corresponding to the infrared rays captured by the optical system (all of which are omitted from the illustration).

[0018] The unevenness detection means 7 is, for example, a generally known laser distance measuring device. The laser distance measuring device can detect the distance to the object to be measured, i.e., unevenness, by irradiating the object with a laser beam that is amplitude-modulated at a predetermined fundamental frequency. Note that the unevenness detection means 7 is not limited to the above-mentioned laser distance measuring device, and any known measuring device can be used.

[0019] The control means 20 is configured by a computer and includes a central processing unit (CPU) that performs calculations according to a control program, a read-only memory (ROM) that stores the control program, etc., a readable / writable random access memory (RAM) for temporarily storing detected values, calculation results, etc., an input interface, and an output interface (details are not shown in the drawings). The control means 20 is connected to each operating unit of the laser processing device 1, the alignment means 6, the unevenness detection means 7, and the display means 9. The height of the surface of the measurement object measured by the unevenness detection means 7 is displayed on the display means 9 and stored in the control means 20 together with the XY coordinates of the position where the unevenness is detected.

[0020] The laser processing apparatus 1 has a configuration generally as described above, and a wafer processing method configured according to the present invention and carried out using this laser processing apparatus 1 will be described below.

[0021] The workpiece to be processed by the wafer processing method of this embodiment is, for example, a wafer 10 shown in Fig. 2. The wafer 10 is a silicon (Si) wafer having a plurality of devices 12 formed on a surface 10a and partitioned by planned division lines 14. Once the wafer 10 is prepared, a protective tape disposing step is performed in which a protective tape T1 is attached and disposed on the surface 10a of the wafer 10, as shown in Fig. 2.

[0022] Next, the above-mentioned wafer 10 is transported to the laser processing device 1, and as shown in FIG. 3, the wafer 10 is flipped over so that the protective tape T1 side faces downward and the back surface 10b of the wafer 10 faces upward, and placed on the holding surface 35a of the chuck table 35. A suction means (not shown) is activated to hold the wafer by suction, thereby exposing the back surface 10b of the wafer 10 upward, thereby carrying out a wafer holding process.

[0023] After the above-mentioned wafer holding step is performed, the feed means 4 is operated to position the wafer 10 below the alignment means 6. Then, the alignment means 6 is operated to irradiate the back surface 10b of the wafer 10 with infrared rays to capture an image of the dividing lines 14 formed on the front surface 10a, and alignment is performed to detect the positions of the dividing lines 14 based on the captured image information. Based on the position information of the dividing lines 14 detected by the alignment, the chuck table 35 is rotated to align the dividing lines 14 formed in a predetermined direction with the X-axis direction, and the feed means 4 is operated to position the unevenness detection means 7 above the dividing lines 14 as shown in FIG.

[0024] When the unevenness detection means 7 is positioned above the planned dividing lines 14, the unevenness detection means 7 is operated and the feed means 4 is operated to appropriately move the chuck table 35 in the X-axis direction, the Y-axis direction, and the rotation direction indicated by the arrow R1 while irradiating the laser beam LB1 of the laser length measuring device constituting the unevenness detection means 7 to detect unevenness at the position of the rear surface 10b corresponding to the planned dividing lines 14 of the wafer 10. As shown in FIG. 4, the unevenness detection means 7 is connected to the control means 20, and displays the height of the planned dividing lines 14 indicated by the dashed line 100 where the unevenness is detected on the display means 9 and stores the XY coordinates of the position. As can be seen from the display means 9 shown in FIG. 4, when the rear surface 10b of the wafer 10 is flat, it is displayed as a solid line H0, and when the rear surface 10b of the wafer 10 is convex, it is displayed as a dashed line H1.

[0025] Here, with regard to the unevenness detected by the unevenness detection means 7, it is judged whether the unevenness on the back surface 10b of the wafer 10 is within the allowable range or outside the allowable range. More specifically, in the display means 9 of FIG. 4, if the height Z1 of the convex part indicated by the broken line H1 with respect to the reference height of the back surface 10b of the wafer 10 indicated by the solid line H0 is less than a judgment standard (e.g., 10 μm) defined as the allowable range, it is judged to be within the allowable range, and if it is equal to or greater than the judgment standard, it is judged to be outside the allowable range. This completes the unevenness detection process. Note that the judgment standard is appropriately set depending on the thickness of the wafer 10 and the depth position where the modified layer is formed in the modified layer formation process described later, and is not limited to the above-mentioned 10 μm.

[0026] If the height Z1 of the protrusions indicated by the dashed line H1 is determined to be within the allowable range in the unevenness detection process described above, the modified layer formation process described below is carried out. In contrast, if the height Z1 of the protrusions is determined to be outside the allowable range, it is determined that foreign matter is attached to at least one of the surface of the protective tape T1 held by the chuck table 35 and the holding surface 35a of the chuck table 35, and the foreign matter removal process described below is carried out.

[0027] The foreign matter removing step will be described with reference to FIGS. 5 and 6. When performing the foreign matter removing step, first, the wafer 10 is removed from the chuck table 35. Next, as shown in FIG. 5(a), a foreign matter removing sheet T2 having a size at least larger than the holding surface 35a of the chuck table 35 is placed on the holding surface 35a of the chuck table 35. The foreign matter removing sheet T2 is a sheet having adhesive force on the surface placed on the holding surface 35a, but for example, a thermocompression sheet is used that does not have a separate adhesive layer (glue layer) formed on the surface placed on the holding surface 35a and that softens and exerts adhesive force when heated to near the melting temperature. The thermocompression sheet is, for example, selected from a polyolefin-based sheet or a polyester-based sheet. Examples of polyolefin-based sheets that can be used as the thermocompression sheet T include a polyethylene (PE) sheet, a polypropylene (PP) sheet, and a polystyrene (PS) sheet. Examples of polyester-based sheets that can be used as the thermocompression sheet T include a polyethylene terephthalate sheet (PET) and a polyethylene naphthalate (PEN) sheet. In this embodiment, a polyethylene sheet is selected as the thermocompression sheet T.

[0028] As described above, after the foreign substance removing sheet T2 is placed, a pressure roller 51 as shown in FIG. 5(a) is prepared. The pressure roller 51 is equipped with a heater and a temperature sensor (not shown) inside. After the pressure roller 51 is prepared, the heater is operated to heat the surface 52 of the pressure roller 51 to a temperature close to the melting temperature (for example, 120°C to 140°C) at which the polyethylene sheet constituting the foreign substance removing sheet T2 exerts its adhesive force, and the surface 52 is pressed against the foreign substance removing sheet T2 placed on the holding surface 35a of the chuck table 35. Next, the pressure roller 35 is rotated in the direction indicated by the arrow R2 and moved in the direction indicated by the arrow R3 to press the foreign substance removing sheet T2, which has exerted its adhesive force by the heating, against the holding surface 35a of the chuck table 35. The surface 52 of the pressure roller 51 is coated with a fluororesin so as not to roll in the foreign substance removing sheet T2, which has exerted its adhesive force. The pressure roller 51 is not limited to having a built-in heater, and the foreign matter removing sheet T2 may be heated to a required temperature by a separately prepared heating means while being pressure-bonded by the pressure roller 51.

[0029] As described above, after the foreign matter removing sheet T2 is pressed against the holding surface 35a of the chuck table 35, the foreign matter removing sheet T2 is pulled in the direction indicated by the arrow R4 as shown in Fig. 5(b) to be peeled off from the holding surface 35a. As a result, if any foreign matter is attached to the holding surface 35a, the foreign matter is removed and the holding surface 35a is cleaned.

[0030] In the above embodiment, a polyethylene sheet is selected as the foreign matter removing sheet T2, but the present invention is not limited to this, and the above-mentioned polypropylene sheet, polystyrene sheet, polyethylene terephthalate sheet, and polyethylene naphthalate sheet may be selected. Note that the temperature at which adhesive force is exerted by heating (temperature near the melting temperature) differs for each sheet, and the target temperature when heating and pressing is appropriately adjusted according to the melting temperature.

[0031] Further, the wafer 10 removed from the holding surface 35a of the chuck table 35 is transported to a plasma device 60 (only a part of which is shown) shown in FIG. 6. The illustrated plasma device 60 is, for example, an atmospheric pressure plasma device, and includes a plasma electrode 64 forming a positive electrode, and a table portion 62 having a surface 62a that forms an electrode facing the plasma electrode 64 and capable of earthing the wafer 10 and capable of holding the wafer 10. The atmosphere is arranged to flow between the plasma electrode 64 and the table portion 62. After the wafer 10 is transported to the plasma device 60, it is placed on the surface 62a of the table portion 62 with the side to which the protective tape T1 is attached facing upward. Next, a high voltage is applied to the plasma electrode 64 and the table portion 62, thereby generating plasma P (plasmaized oxygen, nitrogen, etc.) between the lower surface 64a of the plasma electrode 64 and the surface 62a of the table portion 62. By operating the plasma device 60 in this manner, the plasma P acts on the surface of the protective tape T1 of the wafer 10, and if any foreign matter such as organic matter is attached to the protective tape T1, the foreign matter is destroyed and cleaned. This completes the foreign matter removal process.

[0032] As described above, after the foreign matter removal step is performed and the holding surface 35a of the chuck table 35 and the surface of the protective tape T1 disposed on the wafer 10 are cleaned, the wafer is transported to the laser processing device 1 again and the above-mentioned wafer holding step and unevenness detection step are performed. This determines whether unevenness that falls outside the allowable range detected in the previously performed unevenness detection step remains, and if unevenness outside the allowable range is not detected, the modified layer formation step described below is performed. Note that if unevenness outside the allowable range is detected after the wafer holding step and unevenness detection step are performed, and unevenness outside the allowable range continues to be detected despite the above-mentioned foreign matter removal step being repeatedly performed, the details of the holding surface 35a of the chuck table 35 and the surface of the protective tape T1 on the wafer 10 are checked and replaced as necessary.

[0033] The specific method for carrying out the foreign matter removal step is not limited to the above embodiment, and foreign matter may be removed by other methods. As another method for removing foreign matter from the holding surface 35a of the chuck table 35, for example, cleaning water may be sprayed from the inside of the holding surface 35a and brushing may be performed from the front side to remove the foreign matter. As another method for removing foreign matter from the surface of the protective tape T1 disposed on the wafer 10, for example, high-pressure cleaning water may be sprayed onto the surface of the protective tape T1 to remove the foreign matter.

[0034] When the modified layer forming step is performed after the unevenness detection step, the condenser 81 of the laser beam application means 8 is positioned at a processing position corresponding to the dividing line 14 where the modified layer is to be formed, as shown in Fig. 7(a), based on the position information of the dividing line 14 detected in the unevenness detection step. Then, as can be understood from Fig. 7(b) in addition to Fig. 7(a), the condensing point of the laser beam LB2 having a wavelength that is transparent to the wafer 10 is positioned at a predetermined depth position inside the wafer 10 where the modified layer is to be formed, and the wafer 10 is processed and fed in the X-axis direction to form a modified layer 110 that is the starting point of division along the dividing line 14. After the modified layer 110 is formed, the wafer 10 is indexed and fed in the Y-axis direction by the interval of the dividing line 14, and the unprocessed dividing line 14 adjacent in the Y-axis direction is positioned directly under the condenser 81. Then, in the same manner as described above, the focal point of the laser beam LB2 is positioned inside the wafer 10 corresponding to the planned dividing lines 14 of the wafer 10 and irradiated, and the wafer 10 is processed and fed in the X-axis direction to form the modified layer 110. By repeating these steps, the wafer 10 is processed and fed in the X-axis direction and the Y-axis direction to form the modified layer 110 along the inside of the wafer 10 corresponding to all the planned dividing lines 14 along the X-axis direction.

[0035] Next, the wafer 10 is rotated 90 degrees in the direction indicated by the arrow R1 to align the unprocessed dividing lines 14 perpendicular to the dividing lines 14 on which the modified layers 110 have already been formed, in the X-axis direction. Then, the focal point of the laser beam LB2 is positioned and irradiated in the same manner as described above to the inside of the wafer 10 corresponding to each of the remaining dividing lines 14, thereby forming modified layers 110 in the inside of the wafer 10 corresponding to all of the dividing lines 14 formed on the front surface 10a of the wafer 10. This completes the modified layer forming process.

[0036] The laser processing conditions when carrying out the modified layer forming step are set, for example, as follows. Wavelength: 1342nm Repetition frequency: 90kHz Average output: 1.2W Machining feed speed: 700mm / sec

[0037] After the modified layer forming step described above has been carried out, a grinding step is carried out to divide the wafer 10 into individual device chips along the modified layer 110 formed in the modified layer forming step described above.

[0038] When carrying out the above-mentioned grinding step, the wafer 10 on which the modified layer 110 has been formed is transferred to a grinding device 70 (only a part of which is shown) shown in Fig. 8. The grinding device 70 includes a grinding means 72 and a chuck table 77 that suction-holds the wafer 10. The grinding means 72 includes a rotating spindle 73 that is rotated by a rotation drive mechanism (not shown), a wheel mount 74 attached to the lower end of the rotating spindle 73, and a grinding wheel 75 equipped with a plurality of grinding stones 76 attached to the lower surface of the wheel mount 74 and arranged in a ring shape on the lower surface side.

[0039] The wafer 10 is transported to the grinding device 70, and placed on the chuck table 77 with the protective tape T1 side facing downward and the back surface 10b side facing upward, and held by suction. Next, the rotating spindle 73 of the grinding means 72 is rotated to rotate the grinding wheel 75 in the direction indicated by the arrow R5 in Fig. 8 at, for example, 6000 rpm, while rotating the chuck table 77 in the direction indicated by the arrow R6 at, for example, 300 rpm. Then, while supplying grinding water onto the back surface 10b of the wafer 10 by a grinding water supplying means (not shown), the grinding stone 76 is lowered in the direction indicated by the arrow R7 to contact the back surface 10b of the wafer 10, and the grinding wheel 75 is fed for grinding at a grinding feed speed of, for example, 1.0 µm / sec. At this time, grinding can be carried out while measuring the thickness of the wafer 10 with a contact or non-contact measuring gauge (not shown), and the back surface 10b of the wafer 10 is ground to a predetermined thickness. As a result, dividing grooves 120 are formed along the modified layer 110 described above, and the wafer 10 is divided into individual device chips 12'.

[0040] The wafer processing method of this embodiment includes the wafer holding process, unevenness detection process, and foreign matter removal process described above, and since the modified layer formation process is carried out with the back surface 10b of the wafer 10 in a proper state, problems such as the modified layer being insufficient and therefore the wafer 10 being unable to be properly divided or chips being formed in the device chips when being divided into individual device chips 12' are eliminated.

[0041] In the above embodiment, after the modified layer forming step, the wafer 10 is transported to the grinding device 70 to divide the wafer 10 into individual device chips, and the grinding step is performed, but the modified layer forming step is not limited to the above-mentioned grinding step. For example, after the modified layer forming step, the wafer 10 may be held by an adhesive tape in an annular frame having an opening in the center capable of accommodating the wafer 10, and the adhesive tape may be expanded to apply an external force to the wafer 10, thereby dividing the wafer 10 into individual device chips 12'. [Explanation of symbols]

[0042] 1: Laser processing equipment 2: Base 2a: Guide rail 3: Holding means 31:X-axis movable plate 32: Y-axis direction movable plate 35: Chuck table 35a: Holding surface 4:Feeding means 41: X-axis feed means 42: Y-axis feed means 5:Frame body 6: Alignment method 7: Irregularity detection means 8: Laser beam irradiation means 81: Concentrator 9:Display means 10: Wafer 10a: surface 10b: Back side 12: Device 14: Planned division line 20: Control means 51: Pressure roller 60: Plasma device 62: Table section 64: Plasma electrode 70: Grinding equipment 72: Grinding means 75: Grinding wheel 76: Grinding wheel 77: Chuck table 110: Modified layer 120: Dividing groove T1: Protective tape T2: Foreign object removal sheet

Claims

1. A method for processing a wafer having a surface on which a plurality of devices are defined by dividing lines, comprising the steps of: a protective tape applying step of applying a protective tape to a front surface of the wafer; a wafer holding step of holding the protective tape side on a holding surface of a chuck table and exposing the back surface of the wafer; An unevenness detection step of detecting unevenness on the back surface of the wafer, If the irregularities detected by the irregularity detection step are within an allowable range, a modified layer formation step is carried out in which a focused point of a laser beam having a wavelength that is transparent to the wafer is positioned inside the wafer corresponding to the planned division line, and a modified layer is formed by irradiating the focused point of the laser beam, If the unevenness detected by the unevenness detection step is outside the allowable range, a foreign matter removal step is carried out in which the wafer is removed from the chuck table, and the holding surface of the chuck table and the protective tape placed on the wafer are cleaned to remove foreign matter; After the foreign matter removing step, the wafer holding step and the irregularity detecting step are carried out again.

2. 2. The wafer processing method according to claim 1, wherein in the unevenness detecting step, the height of the rear surface of the wafer corresponding to the intended dividing lines is measured by a laser length measuring device to detect the unevenness.

3. 2. The wafer processing method according to claim 1, further comprising a grinding step of holding the protective tape side on a chuck table of a grinding apparatus to grind and thin the back surface of the wafer after the modified layer forming step, and dividing the wafer along the modified layer into individual device chips.

Citation Information

Patent Citations

  • Method for processing wafer

    JP2014056889A

  • Method for processing wafer

    JP2014139964A

  • Dicing tape integral type adhesive sheet

    JP2019111775A

  • Holder

    JP2020189384A

  • Method of processing wafer

    JP2021068872A