Surface coated cutting tool

A multi-layer coated cutting tool with optimized Ti and Al composite nitride, TiCN, and α-Al2O3 layers addresses chipping issues, enhancing durability and wear resistance during high-speed cutting.

JP2024138692AActive Publication Date: 2024-10-09MITSUBISHI MATERIALS CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023049294
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09
Estimated Expiration
2043-03-27

AI Technical Summary

Technical Problem

Existing surface-coated cutting tools lack sufficient chipping resistance, particularly during high-speed interrupted cutting, despite advancements in coating layer composition and structure.

Method used

A surface-coated cutting tool with a multi-layer structure comprising a lower layer of Ti and Al composite nitride or carbonitride, an intermediate TiCN layer, and an upper layer of α-Al2O3, optimized for thickness, crack density, and crystal structure to enhance chipping resistance.

Benefits of technology

The tool exhibits excellent chipping resistance and durability during high-speed cutting, with improved wear resistance and reduced likelihood of chipping.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138692000001_ABST
    Figure 2024138692000001_ABST
Patent Text Reader

Abstract

To provide a surface coated cutting tool having wear resistance and thermal crack resistance.SOLUTION: In a surface coated cutting tool, a) a coating layer has an upper layer, an intermediate layer, and a lower layer, b) the upper layer has an average thickness of 1.0 to 10.0 μm and contains an α-Al2O3 layer, c) there is a crack on a cross section of the α-Al2O3 layer parallel to a substrate and density of the crack is 0.4 to 6.5 cracks / mm, d) the intermediate layer has an average thickness of 1.5 to 5.0 μm and contains a TiCN layer, e) the lower layer has an average thickness of 3.0 to 10.0 μm and contains a composite nitride layer or a composite carbonitride layer of Ti and Al, f) the composite nitride layer or the composite carbonitride layer of Ti and Al contains crystal grains of a NaCl type face-centered cubic structure of 80 to 100 area% in a longitudinal section of the coating layer, and an average composition thereof is (Ti1-XavgAlXavg)(CYavgN1-Yavg)(0.70≤Xavg≤0.90, 0.000≤Yavg≤0.050).SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a surface-coated cutting tool (hereinafter sometimes referred to as a coated tool). [Background technology]

[0002] Conventionally, in order to extend the life of cutting tools, there have been coated tools in which a coating layer is applied to the surface of a base material such as a tungsten carbide (hereinafter sometimes referred to as WC)-based cemented carbide, and these coated tools have improved wear resistance, etc. In order to further improve the cutting performance of the coated tool, various proposals have been made regarding the composition and structure of the coating layer.

[0003] For example, in Patent Document 1, a coating layer is Ti 1-x Al x N-layer and / or Ti 1-x Al x C layer and / or Ti 1-x Al x A coated tool having an Al2O3 layer on a CN layer (wherein x is 0.65 to 0.95) is described, and the coated tool is said to have excellent durability because the coating layer has heat insulating properties.

[0004] For example, Patent Document 2 discloses a Ti coating layer having an average thickness of 4 to 14 μm. 1-x Al x N inner layer, a TiCN intermediate layer of 0.05-1 μm, and at least one outer layer of α-Al2O3 of 1-9 μm; The texture coefficient TC(hkl) of the α-Al2O3 layer is TC(hkl)=[I(hkl) / I0(hkl)] ×[(1 / n)×Σ(I(hkl) / I0(hkl)] ?1 [where the (hkl) reflections used in the calculation are (0 2 4), (1 1 6), (3 0 0), and (0 0 12); I(hkl) = measured intensity (peak intensity) of the (hkl) reflection, I0(hkl) = Standard intensity according to ICDD PDF card No. 00 - 042 - 1468 n = number of reflections, There is described a coated tool with 3 < TC(0 0 12) < 4, and the coated tool is said to have improved wear resistance and resistance to comb - shaped cracks.

Prior Art Documents

Patent Documents

[0005]

Patent Document 1

Patent Document 2

Summary of the Invention

Problems to be Solved by the Invention

[0006] The present invention has been made in view of the above circumstances and the above proposal, and an object thereof is to obtain a surface - coated cutting tool having excellent chipping resistance in cutting processes including high - speed intermittent cutting.

Means for Solving the Problems

[0007] The surface - coated cutting tool according to an embodiment of the present invention has a substrate and a coating layer on the surface of the substrate, and the coating layer has at least three layers: an upper layer, an intermediate layer, and a lower layer. (a) The upper layer has an average thickness of 1.0 to 10.0 μm and includes an α - Al2O3 layer. (b) Cracks exist in the cross - section parallel to the substrate of the α - Al2O3 layer, and the crack density is 0.4 to 6.5 cracks / mm. (c) The intermediate layer has an average thickness of 1.5 to 5.0 μm and includes a TiCN layer. (d) The lower layer has an average thickness of 3.0 to 10.0 μm and includes a composite nitride layer or a composite carbonitride layer of Ti and Al. (e) The Ti and Al composite nitride layer or composite carbonitride layer contains crystal grains of NaCl type face-centered cubic structure in a longitudinal section of the coating layer at 80 to 100% by area, and the average composition is (Ti 1-Xavg Al Xavg )(C Yavg N 1-Yavg ) (0.70≦Xavg≦0.90, 0.000≦Yavg≦0.050).

[0008] Furthermore, the surface-coated cutting tool according to the embodiment may satisfy at least one of the following (1) to (4).

[0009] (1) The orientation index TC(0 0 12) of the α-Al2O3 layer is 6.0 or more and 7.0 or less, and in a constituent atom sharing lattice point distribution graph, the distribution ratio of Σ3 to the entire ΣN+1 of the α-Al2O3 layer is 40% or more and 100% or less. Where: TC(0 0 12)=[I(0 0 12) / I0(0 0 12)] ×[(1 / 7)×Σ(I(hkl) / I0(hkl)] ?1 however, I(0 0 12): Measured value of X-ray diffraction peak intensity in the (0 0 12) plane I0(0 0 12): Average value of standard X-ray diffraction peak intensity in the (0 0 12) plane of the crystal plane of Al2O3 listed in ICDD card 00-042-1468 Σ(I(hkl) / I0(hkl)): The sum of the values ​​of ([measured X-ray diffraction peak intensity] / [average value of standard diffraction peak intensity of Al2O3 listed on the ICDD card]) for each of the seven faces: (0 1 2), (1 0 4), (1 1 3), (1 1 6), (3 0 0), (2 1 4), and (0 0 12).

[0010] (2) The α-Al2O3 layer has crystals with a residual stress of 0 to +300 MPa. (3) In the α-Al2O3 layer, ρα=[S] / ([Al]+[O]+[S]) ([Q] represents the number of atoms of element Q) is 0.00001 to 0.00050.

[0011] (4) The orientation index TC(422) of the TiCN layer is 2.0 or more and 4.0 or less. Where: TC(422)=[I(422) / I0(422)] ×[(1 / 4)×Σ(I(hkl) / I0(hkl)] ?1 however, I(422): Measured X-ray diffraction peak intensity for the (422) plane I0(422): Average value of standard X-ray diffraction peak intensity on the (422) plane of the TiCN crystal plane listed in ICDD card 00-042-1489 Σ(I(hkl) / I0(hkl)): The sum of the ([measured X-ray diffraction peak intensity] / [average value of standard diffraction peak intensity of TiCN listed on the ICDD card]) values ​​for each of the four faces (111), (200), (420) and (422) It is. Effect of the Invention

[0012] The surface-coated cutting tool according to the embodiment has excellent chipping resistance. [Brief description of the drawings]

[0013] [Figure 1] 1 is a schematic vertical cross-sectional view of a surface-coated cutting tool according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram of a measurement line for measuring crack density. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The present inventors have conducted extensive research into ways to impart better chipping resistance to a coated tool having an α-Al2O3 layer on a coating layer as described in the above-mentioned prior art documents. As a result, it was discovered that while Patent Document 1 states that it is preferable for cracks not to exist, if cracks are present at a predetermined density in the cross section of the α-Al2O3 layer parallel to the substrate surface, the coated tool will exhibit excellent chipping resistance.

[0015] Hereinafter, a coated tool according to an embodiment of the present invention will be described in detail. In this specification and claims, when a numerical range is expressed as "L to M" (L and M are both numerical values), this is synonymous with "L or more, M or less," and the range includes an upper limit (M) and a lower limit (L). When a unit is stated only for the upper limit, the unit for the lower limit is also the same.

[0016] Fig. 1 shows a schematic longitudinal section of a coated tool according to one embodiment of the present invention (a section perpendicular to the surface of the substrate, with the surface of the substrate treated as a horizontal plane, with minute irregularities on the surface of the substrate ignored). As is clear from Fig. 1, the coated tool according to this embodiment has a lower layer (2) in contact with the surface of the substrate (1), an intermediate layer (3) in contact with the lower layer (2) on the tool surface side of the lower layer (2), and an upper layer (4) in contact with the intermediate layer (3) on the tool surface side of the intermediate layer (3). The lower layer (2), intermediate layer (3) and upper layer (4) together constitute a coating layer (5). Each layer will be described in turn below.

[0017] 1. Lower layer The lower layer comprises a composite nitride layer or composite carbonitride layer of Ti and Al (sometimes referred to as (TiAl)(CN)).

[0018] (1) Average thickness The average thickness of the lower layer is preferably 3.0 to 10.0 μm. The reason is that if the average thickness is less than 3.0 μm, excellent wear resistance cannot be exhibited over long-term use, while if the average thickness exceeds 10.0 μm, abnormal damage such as chipping is likely to occur during high-speed interrupted cutting. The average thickness of the lower layer is more preferably 5.0 to 8.0 μm.

[0019] (2) Content of crystal grains with NaCl-type face-centered cubic structure The content of crystal grains having a NaCl type face-centered cubic structure is preferably 80% or more by area in the longitudinal section, because if it is less than 80% by area, the content of the soft wurtzite type hexagonal structure, which is the inherent stable phase of (TiAl)(CN), increases in the lower layer, preventing the coated tool from having sufficient durability;

[0020] (3) Average composition The average composition of the Ti and Al composite nitride layer or carbonitride layer is (Ti 1-Xavg Al Xavg )(C Yavg N 1-Yavg ) (0.70≦Xavg≦0.90, 0.000≦Yavg≦0.050). The reason is that if Xavg is less than 0.70, the high oxidation resistance of (AlTi)CN cannot be obtained sufficiently, while if it exceeds 0.90, sufficient wear resistance cannot be obtained. It is more preferable that Xavg is 0.75 to 0.85.

[0021] In addition, the C component in (AlTi)(CN) has the effect of improving hardness, so C may be contained. However, if Yavg exceeds 0.050, chipping resistance decreases, so it is preferable to make it 0.000≦Yavg≦0.050.

[0022] The film is formed so that the atomic ratio of (AlTi) and (CN) is 1:1, but it may be within the range of 1:0.8 to 1:1.2.

[0023] 2. Middle tier The intermediate layer, which is in contact with the surface of the lower layer and is provided on the tool surface side thereof, contains a TiCN layer and serves as a layer for bonding the lower layer and the upper layer together.

[0024] (1) Average thickness The average thickness of the intermediate layer is preferably 1.5 to 5.0 μm. The reason is that if the average thickness is less than 1.5 μm, the adhesion between the lower layer and the upper layer cannot be sufficiently ensured, and cracks existing in the α-Al2O3 layer contained in the upper layer described later will further progress into the intermediate layer, making chipping likely to occur from the cracks in the intermediate layer, while if it exceeds 5.0 μm, the TiCN layer will break during processing such as high-speed intermittent cutting, making chipping likely to occur. The average thickness of the intermediate layer is more preferably 2.5 to 4.0 μm.

[0025] (2) Composition The composition of the TiCN layer contained in the intermediate layer is not limited to the stoichiometric composition.

[0026] (3) Orientation index It is more preferable that the orientation index TC(422) of the TiCN layer contained in the intermediate layer is 2.0 or more and 4.0 or less. Where: TC(422)=[I(422) / I0(422)] ×[(1 / 4)×Σ(I(hkl) / I0(hkl)] ?1 however, I(422): Measured X-ray diffraction peak intensity for the (422) plane I0(422): Average value of standard X-ray diffraction peak intensity on the (422) plane of the TiCN crystal plane listed in ICDD card 00-042-1489 Σ(I(hkl) / I0(hkl)): The sum of the ([measured X-ray diffraction peak intensity] / [average value of standard diffraction peak intensity of TiCN listed on the ICDD card]) values ​​for each of the four faces (111), (200), (420) and (422) It is.

[0027] The reason why TC(422) is more preferably 2.0 or more is that if it is less than 2.0, cracks in the α-Al2O3 layer contained in the upper layer described later may further progress into the TiCN layer, making chipping more likely to occur starting from cracks in the TiCN layer. Note that the theoretical maximum value for TC(422) is 4.0.

[0028] 3. Upper layer The upper layer, which is provided on the tool surface side and in contact with the surface of the intermediate layer, contains an α-Al2O3 layer and acts as a layer that exhibits excellent high-temperature hardness and high-temperature oxidation resistance.

[0029] (1) Average thickness The average thickness of the upper layer is preferably 1.0 to 10.0 μm. The reason is that if it is less than 1.0 μm, it is not possible to exhibit excellent wear resistance over a long period of time, and furthermore, the crack density in the α-Al2O3 layer contained in the upper layer described later tends to be low, which makes chipping more likely to occur during cutting, while if it exceeds 10.0 μm, chipping is more likely to occur during cutting. The average thickness of the upper layer is more preferably 3.0 to 8.0 μm.

[0030] (2) Composition The composition of the α-Al2O3 layer contained in the upper layer is not limited to the stoichiometric composition.

[0031] (3) Crack density The α-Al2O3 layer contained in the upper layer has cracks in a cross section parallel to the substrate (a cross section parallel to the substrate surface when the substrate surface is treated as a flat surface without minute irregularities on the substrate surface), and the density of the cracks is preferably 0.4 to 6.5 / mm. The reason why a crack density in this range is preferable is that if the crack density is less than 0.4 / mm, the stress applied to the upper layer during cutting is concentrated locally due to the small crack density, making chipping more likely to occur, while if the crack density exceeds 6.5 / mm, the high crack density makes chipping more likely to occur during cutting. The crack density is more preferably 0.8 to 3.6 / mm.

[0032] The crack density is measured as follows. The upper layer is polished to about half its thickness, and a cross section parallel to the substrate surface is obtained, and a field of view with a side length of 1 mm square on this cross section is observed with an optical microscope. Next, as shown in Figure 2, 10 lines, each 1 mm long or longer, are drawn across the square observation area at 11 equal intervals in the vertical direction, and these lines are used as analysis lines. The number of cracks that intersect with each of the 10 analysis lines is counted. The average number of cracks is then used as the crack density.

[0033] (4) Orientation index TC(0 0 12) and the ratio of Σ3 to the total ΣN+1 More preferably, the orientation index TC(0 0 12) of the upper layer is 6.0 or more and 7.0 or less, and the ratio of Σ3 to the entire ΣN+1 of the α-Al2O3 layer is 40% or more and 100% or less. Where: TC(0 0 12)=[I(0 0 12) / I0(0 0 12)] ×[(1 / 7)×Σ(I(hkl) / I0(hkl)] ?1 however, I(0 0 12): Measured value of X-ray diffraction peak intensity in the (0 0 12) plane, I0(0 0 12): average value of standard X-ray diffraction peak intensity in the (0 0 12) plane of the crystal plane of α-Al2O3 described in ICDD card 00-042-1468, Σ(I(hkl) / I0(hkl)): The sum of the values ​​of ([measured X-ray diffraction peak intensity] / [average value of standard diffraction peak intensity of Al2O3 listed on the ICDD card]) for each of the seven faces, (0 1 2), (1 0 4), (1 1 3), (1 1 6), (3 0 0), (2 1 4), and (0 0 12), It is.

[0034] If TC(0 0 12) is 6.0 or more and 7.0 or less (7.0 is the theoretical upper limit), better wear resistance is obtained and welding of the work material is less likely to occur, and if the ratio of Σ3 to the total ΣN+1 in the α-Al2O3 layer is 40% or more, better wear resistance is obtained and the grain boundary strength of the α-Al2O3 layer does not decrease, so that chipping originating from cracks in the α-Al2O3 layer is more reliably suppressed. This ratio of Σ3 may be 100%.

[0035] (5) Residual stress It is more preferable that the residual stress of the α-Al2O3 layer is 0 to +300 MPa. The reason why a residual stress in this range is more preferable is that if it is less than 0 MPa (compressive residual stress exists), the adhesive strength between the α-Al2O3 layer and the TiCN layer decreases, causing the α-Al2O3 layer to peel off, making chipping more likely to occur, whereas if it exceeds 300 MPa, chipping is more likely to occur starting from cracks in the α-Al2O3 layer.

[0036] (6) S (sulfur) atomic ratio In the α-Al2O3 layer, ρα=[S] / ([Al]+[O]+[S]) ([Q] represents the number of atoms of element Q) is more preferably 0.00001 to 0.00050. The reason is that if ρα is less than 0.00001, the α-Al2O3 layer cannot follow the plastic deformation of the substrate, and abnormal damage such as chipping may occur easily, while if it exceeds 0.00050, the grain boundary strength of the α-Al2O3 layer decreases, and chipping may occur easily starting from cracks in the α-Al2O3 layer.

[0037] 4. Other layers The other layers are roughly divided into two types: layers that are intentionally provided and layers that are not intentionally provided (unintended layers). They will be explained in order below.

[0038] 4-1. Intentionally created layers The following layers are intentionally provided.

[0039] (1) Base layer An underlayer may be provided between the substrate and the lower layer. The underlayer may be one or more layers selected from a composite nitride layer or composite carbonitride layer of Ti and Al, a Ti carbide layer, a nitride layer, a carbonitride layer, a carbonate layer, and a carbonitride oxide layer, each having a different composition from the lower layer. The composition of these layers is not limited to a stoichiometric composition.

[0040] (2) Lower adhesion layer A lower adhesion layer may be provided between the lower layer and the intermediate layer. The lower adhesion layer may be one or more layers selected from a Ti carbide layer, a Ti nitride layer, and a Ti carbonitride layer. The composition of these layers is not limited to the stoichiometric composition.

[0041] (3) Upper adhesive layer An upper adhesive layer may be provided between the intermediate layer and the upper layer. The upper adhesive layer may be one or more layers selected from a Ti carbide layer, a nitride layer, a carbonitride layer, a carbonate layer, and a carbonitride oxide layer. The composition of these layers is not limited to a stoichiometric composition.

[0042] 4-2. Unintended layers When switching deposition gases, a Ti and Al composite nitride layer or carbonitride layer as the lower layer, a TiCN layer as the middle layer, an α-Al2O3 layer as the upper layer, and layers other than the underlayer, lower adhesion layer, and upper adhesion layer may be produced in very small amounts unintentionally.

[0043] 5.Base (1) Composition In this embodiment, the substrate may be, for example, a WC-based cemented carbide (containing Co in addition to WC, and further containing carbides or carbonitrides of Ti, Ta, Nb, etc.), a cermet (containing, for example, TiC, TiN, TiCN, etc. as the main component), a ceramic (for example, silicon nitride, sialon, aluminum oxide), or a cBN sintered body, but is not limited to these.

[0044] (2) Shape There are no particular limitations on the shape of the base body as long as it is a shape that can be used as a cutting tool, and examples of the shape include the shape of an insert and the shape of a drill.

[0045] 6. Measurement of average thickness The average thickness of each layer constituting the coating layer can be obtained by, for example, preparing a sample for observation of a vertical cross section at any position of the coating layer using a focused ion beam system (FIB: Focused Ion Beam system), a cross section polisher (CP: Cross section Polisher), etc., observing the vertical cross section at multiple positions (e.g., five positions) using a scanning electron microscope (SEM) or TEM, a scanning transmission electron microscope (STEM: Scanning Transmission Electron Microscope), or an energy dispersive X-ray spectrometer (EDX: Energy Dispersive X-ray spectrometer) attached to the SEM or TEM, determining the thickness, and averaging these.

[0046] 7. Composition Measurement The atomic content of each layer was determined by averaging the measurement results obtained by irradiating an electron beam onto a longitudinal section of a polished cross-section of a sample using Auger Electron Spectroscopy (AES), performing line analysis along the thickness direction of the coating layer using five or more lines.

[0047] 8. Measurement of the proportion of crystal grains with NaCl-type face-centered cubic structure The grain boundaries of the crystal grains constituting the (TiAl)CN layer are obtained and the crystal grains are specified as follows. That is, using a crystal orientation analyzer attached to a transmission electron microscope (TEM), the polished longitudinal section is irradiated with an electron beam tilted, for example, at 0.5 to 1.0 degrees with respect to the normal direction of the polished surface in a precession motion, while the electron beam is scanned at any beam diameter and interval, and electron diffraction patterns are continuously captured to analyze the crystal orientation of each measurement point. The observation field can be exemplified as a width of 50 μm in the direction parallel to the substrate surface (horizontal direction) and the thickness (average thickness) of the coating layer in the vertical direction.

[0048] The conditions for obtaining the electron beam diffraction pattern used in this measurement are, for example, an acceleration voltage of 200 kV, a camera length of 20 cm, a beam size of 2.4 nm, and a measurement step of 5.0 nm. The measured crystal orientation is determined by discretely examining the measurement surface, and the measurement results are used to represent the area up to the middle between adjacent measurement points, thereby obtaining the orientation distribution over the entire measurement surface. The area represented by these measurement points (hereinafter sometimes referred to as a pixel) can be, for example, a regular hexagon.

[0049] If there is an angle difference of 5 degrees or more between the crystal orientations of adjacent pixels, or if only one of the adjacent pixels shows a face-centered cubic structure of NaCl type or a hexagonal structure of wurtzite type, the side of the region where these pixels are in contact is taken as a grain boundary. The part surrounded by the side considered as a grain boundary is defined as one crystal grain. However, a single pixel that has an orientation difference of 5 degrees or more with all adjacent pixels, or that does not have a measurement point with an adjacent NaCl type face-centered cubic structure, is not considered as a crystal grain, and a pixel that is connected with two or more pixels is treated as a crystal grain. In this way, the grain boundary determination is performed and the crystal grain is identified.

[0050] Furthermore, a graph of the distribution of constituent atom-sharing lattice points is created for each of the α-Al2O3 layers by crystal orientation analysis, and the distribution ratio of Σ3 in the entire ΣN+1 is calculated. The constituent atom sharing lattice point distribution graph is obtained by scanning the electron beam at any beam diameter and interval while precessionally irradiating the polished longitudinal section with an electron beam tilted, for example, by 0.5 to 1.0 degrees with respect to the normal direction of the polished surface, measuring the tilt angles made by the normal lines of the (0001) and (10-10) crystal faces of the crystal grains with respect to the normal line of the polished surface, and calculating, based on the measured tilt angles, whether each of the constituent atoms is in contact with the interface between the adjacent crystal grains. The distribution of lattice points that share one constituent atom between each other (constituent atom sharing lattice points) is calculated, and when a constituent atom sharing lattice point form in which there are N lattice points that do not share a constituent atom between the constituent atom sharing lattice points is represented as ΣN+1 (however, N is an even number of 2 or more due to the crystal structure of a corundum-type hexagonal close-packed crystal, if the upper limit of N is set to 28 from the viewpoint of distribution frequency, the even numbers 4, 8, 14, 24, and 26 do not exist), the distribution ratio of each ΣN+1 to the whole ΣN+1 is calculated to create the distribution.

[0051] In the resulting constituent atom-sharing lattice point distribution graph of the α-Al2O3 layer, the distribution ratio of Σ3 in the entire ΣN+1 (the sum of the distribution ratios of Σ3, Σ7, Σ11, Σ13, Σ17, Σ19, Σ21, Σ23, and Σ29 from the above results) is calculated.

[0052] 10. Measurement of TC(hkl) It is not possible to obtain X-ray diffraction results for only the middle layer or only the upper layer, and the X-ray diffraction results for the lower layer, middle layer, and upper layer are shown together (collectively), i.e., the X-ray diffraction results for the coating layer are shown.

[0053] The orientation index TC(0 0 12) of the α-Al2O3 layer is calculated as follows: TC(0 0 12)=[I(0 0 12) / I0(0 0 12)] ×[(1 / 7)×Σ(I(hkl) / I0(hkl)] ?1 however, I(0 0 12): Measured value of X-ray diffraction peak intensity on the (0 0 12) plane of the α-Al2O3 layer, I0(0 0 12): average value of standard X-ray diffraction peak intensity in the (0 0 12) plane of the crystal plane of α-Al2O3 described in ICDD card 00-042-1468, Σ(I(hkl) / I0(hkl)): The sum of the values ​​of ([measured X-ray diffraction peak intensity] / [average value of standard diffraction peak intensity of Al2O3 listed on the ICDD card]) for each of the seven faces of (0 1 2), (1 0 4), (1 1 3), (1 1 6), (3 0 0), (2 1 4), and (0 0 12) in the α-Al2O3 layer, It is.

[0054] The orientation index TC(422) of the TiCN layer is calculated as follows: TC(422)=[I(422) / I0(422)] ×[(1 / 4)×Σ(I(hkl) / I0(hkl)] ?1 however, I(422): Measured X-ray diffraction peak intensity on the (422) plane of the TiCN layer I0(422): Average value of standard X-ray diffraction peak intensity on the (422) plane of the TiCN crystal plane listed in ICDD card 00-042-1489 Σ(I(hkl) / I0(hkl)): The sum of the ([measured X-ray diffraction peak intensity] / [average value of standard diffraction peak intensity of TiCN listed in the ICDD card]) values ​​for each of the four faces of (111), (200), (420), and (422) in the TiCN layer It is.

[0055] In addition, the diffraction lines of the four faces, (111), (200), (420) and (422), in the TiCN layer, and the diffraction lines of the seven faces, (0 1 2), (1 0 4), (1 1 3), (1 1 6), (3 0 0), (2 1 4) and (0 0 12), in the α-Al2O3 layer, are observed separately from the peaks of the upper, middle and lower layers when X-ray diffraction is performed on the coating layers, i.e., the upper, middle and lower layers. X-ray diffraction is measured using Cu-Kα radiation as a radiation source under the conditions of a measurement range (2θ): 15.0 to 135.0 degrees, a scan step: 0.013 degrees, and a measurement time per step: 0.48 sec / step.

[0056] The residual stress of the α-Al2O3 layer is measured using the sin2Ψ method with an X-ray diffractometer using Cu-Kα radiation under the following conditions: measurement range (2θ): 125.7 to 130.1 degrees, scan step: 0.013 degrees, measurement time per step: 359.3 seconds / step. The measurement uses the diffraction peak of the (13_10) plane, and calculations are performed using 386 GPa as the Young's modulus and 0.27 as the Poisson's ratio (Source: B. Eigenmann, B. Scholtes, E. Macherauch, "Grundlagen und Anwendung der rontgenographischen Spannungsermittlung an Keramiken und Metall-Keramik-Verbundwerkstofften, Materialwissenschaft und Werkstofftechnik, vol. 20, pp. 314-325, 1989.).

[0057] 14. Manufacturing method The coating layer of the coated tool of this embodiment can be produced by chemical vapor deposition under the following production conditions, for example.

[0058] That is, the crack density in the α-Al2O3 layer can be controlled by setting the ratio of the HCl amount and the H2S amount in the deposition gas of the α-Al2O3 layer contained in the upper layer to a predetermined value and setting the cooling rate at 400 to 800°C in the cooling process after deposition of all layers to a predetermined value. The film formation conditions for each layer are exemplified as follows.

[0059] (1) Deposition of the lower layer ((TiAl)(CN) layer) Reactant gas composition (volume %): Gas group A: NH3: 0.1-0.8%, H2: 25.0-35.0%, Gas group B: AlCl3: 0.02-0.09%, TiCl4: 0.01-0.03%, N2: 0.0-10.0%, C2H4: 0.0-0.5%, H2: balance Reaction atmosphere pressure: 4.0~5.0kPa Reaction atmosphere temperature: 700~850℃ Gas group A and gas group B supply cycle: 1 to 5 seconds Gas supply time per cycle: 0.15 to 0.25 seconds Phase difference between gas group A supply and gas group B supply: 0.10 to 0.20 seconds

[0060] (2) Deposition of intermediate layer (TiCN layer) Reactant gas composition (volume %): CH3CN: 0.5-1.0%, TiCl4: 1.5-5.0%, N2: 8.0~25.0%, H2: remainder, Reaction atmosphere temperature: 800~900℃ Reaction atmosphere pressure: 4.0~10.0kPa

[0061] (3) Deposition of the upper layer (α-Al2O3 layer) <Initial nucleation conditions> Reactant gas composition (volume %): AlCl3: 1.0-5.0%, CO2: 0.5-2.0%, HCl: 0.3-3.0%, H2: balance Reaction atmosphere pressure: 4.0~10.0kPa Reaction atmosphere temperature: 800~900℃

[0062] <Nucle growth conditions> Reactant gas composition (volume %): AlCl3: 1.0-5.0%, CO2: 3.0-7.0%, HCl: 0.3-3.0%, H2S: 1.0-2.0%, H2: balance Reaction atmosphere pressure: 4.0~10.0kPa Reaction atmosphere temperature: 800~900℃

[0063] (4) Cooling process Cooling rate in the temperature range of 400-800°C: 0.9-1.6°C / min EXAMPLES

[0064] Next, an embodiment will be described. Here, as an example, we will describe an application to an insert cutting tool using a WC-based cemented carbide as the base material, but the same applies when the above-mentioned materials are used as the base material, and also when applied to drills and end mills.

[0065] As raw powders, WC powder, TiC powder, TaC powder, NbC powder, Cr3C2 powder and Co powder were prepared, and these raw powders were blended as shown in Table 1. Wax was added, and the mixture was mixed in a ball mill in acetone for 24 hours, dried under reduced pressure, and then pressed into a green compact of a predetermined shape at a pressure of 98 MPa. This green compact was vacuum sintered under conditions of holding at 1420°C in a vacuum of 5 Pa for 1 hour, to produce WC-based cemented carbide substrates A to C having the ISO standard SEEN1203AFSN shape. Note that each raw powder contained a trace amount of unavoidable impurities.

[0066] Next, a lower layer, an intermediate layer and an upper layer were formed in that order on the surfaces of these substrates A to C according to the manufacturing conditions shown in Tables 2 to 4, respectively, to obtain coated tools 1 to 8 of the examples shown in Table 5 (hereinafter, Examples 1 to 8).

[0067] On the other hand, for comparison, a lower layer, an intermediate layer and an upper layer were formed in that order on the surfaces of bases A to C according to the manufacturing conditions shown in Tables 2 to 4, respectively, to obtain comparative coated tools 1 to 8 (hereinafter, Comparative Examples 1 to 8) shown in Table 5.

[0068] [Table 1]

[0069] [Table 2]

[0070] [Table 3]

[0071] [Table 4]

[0072] [Table 5]

[0073] Next, for the coated tools 1 to 8 of the present invention and the comparative coated tools 1 to 8, the various tool substrates A to C (ISO standard SEEN1203AFSN shape) were all clamped to the tip of an alloy steel cutter with a cutter diameter of 125 mm using a fixture, and the following high-speed dry face milling and center cut cutting tests were carried out on ductile cast iron, and the flank wear width of the cutting edge was measured. Table 7 shows the results of the cutting tests. Note that the comparative coated tools 1 to 8 reached the end of their life before the end of the cutting time due to chipping, so the time until the end of their life is shown.

[0074] Cutting test: Dry high speed face milling, center cut cutting test Cutter diameter: 125mm Work material: JIS FCD700 block material Cutting speed: 300m / min Cutting depth: 2.0mm Feed: 0.2mm / tooth Cutting time: 12 minutes

[0075] [Table 6]

[0076] In Table 6, the cutting time (min) until the end of life in the comparative example indicates the cutting time (min) until the end of life is reached due to the occurrence of chipping.

[0077] As is clear from Table 6, all of the examples had a long maximum machining time, which is the machining time until the cutting edge is chipped, and had excellent durability. [Explanation of symbols]

[0078] 1 Matrix 2 Lower layer 3 Middle Layer 4 Upper Layer 5 Coating layer

Claims

1. A surface-coated cutting tool having a substrate and a coating layer on a surface of the substrate, (a) the coating layer has at least three layers: an upper layer, an intermediate layer, and a lower layer; (b) the upper layer has an average thickness of 1.0 to 10.0 μm and is made of α-Al 2 O 3 layer, (c) the α-Al 2 O 3 Cracks are present in a cross section of the layer parallel to the substrate, and the density of the cracks is 0.4 to 6.5 cracks / mm; (d) the intermediate layer has an average thickness of 1.5 to 5.0 μm and comprises a TiCN layer; (e) the lower layer has an average thickness of 3.0 to 10.0 μm and includes a Ti and Al composite nitride layer or a composite carbonitride layer; (f) The Ti and Al composite nitride layer or composite carbonitride layer contains 80 to 100 area % of crystal grains having a NaCl type face-centered cubic structure in the longitudinal section of the coating layer, and the average composition is (Ti 1-Xavg A Xavg ) (C Yavg N 1-Yavg ) (0.70≦Xavg≦0.90, 0.000≦Yavg≦0.050) A surface-coated cutting tool comprising:

2. The α-Al 2 O 3 The orientation index TC(0 0 12) of the layer is 6.0 or more, and the α-Al 2 O 3 The distribution ratio of Σ3 in the entire ΣN+1 of the layer is 40% or more and 100% or less. Where: TC(0 0 12) = [I(0 0 12) / I0(0 0 12)] ×[(1 / 7)×Σ(I(hkl) / I0(hkl)] ?1 however, I(0 0 12): Measured value of X-ray diffraction peak intensity in the (0 0 12) plane I0 (0 0 12): Al described in ICDD card 00-042-1468 2 O 3 The average value of the standard X-ray diffraction peak intensity in the (0 0 12) plane of the crystal plane of Σ(I(hkl) / I0(hkl)): ([Measured value of X-ray diffraction peak intensity] / [Al listed in ICDD card] for each of the seven faces of (0 1 2), (1 0 4), (1 1 3), (1 1 6), (3 0 0), (2 1 4), and (0 0 12) 2 O 3 The sum of the values ​​of [average of standard diffraction peak intensities of 2. The surface-coated cutting tool according to claim 1,

3. The α-Al 2 O 3 3. The surface-coated cutting tool according to claim 1, wherein the layer has crystals with a residual stress of 0 to +300 MPa.

4. The α-Al 2 O 3 3. The surface-coated cutting tool according to claim 1, wherein in the layer, ρα=[S] / ([Al]+[O]+[S]) ([Q] represents the number of atoms of element Q) is 0.00001 to 0.00050.

5. The TiCN layer has a crystal orientation index TC(422) of 2.0 or more. Where: TC(422) = [I(422) / I0(422)] ×[(1 / 8)×Σ(I(hkl) / I0(hkl)] ?1 however, I(422): Measured value of X-ray diffraction peak intensity in the (422) plane I0(422): Average value of standard X-ray diffraction peak intensity on the (422) plane of the TiCN crystal plane described in ICDD card 00-042-1489 Σ(I(hkl) / I0(hkl)): The sum of the values ​​of ([measured X-ray diffraction peak intensity] / [average value of standard diffraction peak intensity of TiCN listed on the ICDD card]) for each of the eight faces (111), (200), (420) and (422) 2. The surface-coated cutting tool according to claim 1,

Citation Information

Patent Citations

  • Surface coated cemented carbide cutting tool exerting excellent heat-resisting plastic deformation in high- speed cutting

    JP2003071609A

  • Surface coated cutting tool

    JP2011031319A

  • Surface-coated cutting tool in which hard coating layer demonstrates excellent chipping resistance

    JP2012143825A

  • Surface-coated cutting tool

    JP2017024138A

  • Coated Cutting Tools

    JP2020506811A