Coating composition having self-repair function, laminated coating film, structure with coating film, and coating system
A self-healing coating composition with a polymer and boronic acid enhances the durability and adhesion of metal structures, addressing the limitations of catechol-based paints by naturally repairing scratches and preventing rust, thereby extending the lifespan of metal structures.
Patent Information
- Application Number
- JP2023049529
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
Existing paints for metal structures, particularly those containing a catechol group, suffer from poor weather resistance, limited workability, and rapid deterioration due to physical impact, necessitating frequent manual repairs, especially on structures like power transmission towers where safety is a concern.
A coating composition with a self-healing function is developed, comprising a polymer with a 3,4-dihydroxyphenyl group and 1,4-phenylene diboronic acid, using organic solvents with high boiling points and a silane coupling agent, forming a laminated coating film with an undercoat, intermediate, and top coat to enhance adhesion and durability.
The coating composition provides excellent self-healing properties, significantly reducing deterioration and corrosion, extending the lifespan of metal structures by naturally repairing scratches and preventing rust, while maintaining weather resistance and adhesion, thus reducing maintenance needs.
Smart Images

Figure 2024138827000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a coating composition, a coating film laminate, a coated structure, and a coating system having a self-repairing function. [Background technology]
[0002] Metal materials used in power facilities are painted to prevent corrosion caused by the external environment. When the paint becomes scratched or peels off due to damage from physical impact or deterioration from the external environment, it is usually repaired or repainted, but this requires manual labor. In particular, when painting transmission towers, the work is done at high altitudes and is dangerous. Therefore, from the standpoints of cost and safety, it is desirable to extend the painting treatment cycle.
[0003] So far, we have developed a paint that can self-repair while scratches are still small by using a resin that contains a catechol group in the side chain, which forms a complex between metal ions, as the main component (see Patent Document 1 and Non-Patent Document 1).
[0004] However, existing paints are damaged by physical impacts and deteriorated by external factors, leading to scratches and peeling in a relatively short period of time. In addition, when a paint composed of a self-repairing resin containing a catechol group disclosed in Patent Document 1 is used outdoors alone, the occurrence of scratches can be prevented more effectively than with existing paints, but there are issues with the performance of the paint product, such as workability including ease of application and appearance. Since the catechol group has poor weather resistance, it also has the disadvantage of causing deterioration in a short period of time compared to other existing paints. Therefore, there has been a demand for a paint that takes advantage of the paint properties that have a self-repairing function. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 6850973 [Non-patent literature]
[0006] [Non-Patent Document 1] Jincai Li, Hirotaka Ejima, Naoko Yoshie: “Seawater-assisted self-healing of catechol polymers via hydrogen bonding and coordination interactions”, ACS Appl. Mater. Interfaces, 2016,8(29),pp19047-19053.) Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention has been made in consideration of the above problems, and aims to provide a coating composition having a self-repairing function, which uses a self-repairing resin containing a catechol group, a laminated coating film containing the coating composition, a structure with a coating film, and a coating system. [Means for solving the problem]
[0008] In order to solve the above problems, the inventors investigated the properties (adhesion to zinc-plated steel sheets, self-repairing function, and UV resistance) of a paint having a self-repairing function in which a catechol group has been introduced into the side chain, and discovered that a paint composition having a self-repairing function that is useful as an undercoat paint can be obtained, thus arriving at the present invention. That is, the present invention is as follows.
[0009] (1) A self-repairing polymer composed of a polymer (A) having a 3,4-dihydroxyphenyl group in a side chain and 1,4-phenylenediboronic acid (B), and an organic solvent; The coating composition has a self-repairing function, and the organic solvent contains at least one selected from glycol ether-based solvents and alcohol-based solvents having a boiling point of 80°C or higher. (2) The coating composition having a self-repairing function described in (1) above, further comprising a silane coupling agent. (3) The coating composition having the self-repairing function described in (1) above, further comprising one or more coating additives selected from a pigment, a thickener, an anti-settling agent, a dispersant, a thixotropic agent, an anti-sagging agent, and an anti-color separation agent. (4) The coating composition having a self-repairing function according to (1) above, wherein the polymer (A) is a copolymer of 5 to 90 mol % of a vinyl monomer (a) containing a 3,4-dihydroxyphenyl group and 10 to 95 mol % of another polymerizable unsaturated monomer (b), and the other polymerizable unsaturated monomer (b) is at least one type selected from acrylic monomers. (5) The coating film formed by the coating composition is A coating composition having a self-repairing function as described in (1) above, which has a network structure formed by crosslinking the 3,4-dihydroxyphenyl groups of the polymer (A) with 1,4-phenylenediboronic acid (B). (6) A laminated coating film comprising an undercoat coating film formed from a coating composition having a self-repairing function described in any one of (1) to (5) above, an epoxy resin-based intermediate coating film, and a topcoat coating film. (7) A structure having the multilayer coating film described in (6) above. (8) A coating system comprising the following steps 1, 2 and 3. Step 1: A step of applying a coating composition having a self-repairing function described in any one of (1) to (5) above to a structure to form an undercoat coating film. Step 2: Applying an epoxy resin paint onto the undercoat to form a middle coat. Step 3: Applying weather-resistant paint to the undercoat to form a topcoat Effect of the Invention
[0010] The coating composition having a self-repairing function of the present invention has a self-repairing function for naturally repairing scratches that have occurred, and a function for naturally stopping corrosion reactions due to excellent metal adhesion, and since the main component of the coating is a resin having a catechol group, the coating film has excellent self-repairing properties. Therefore, by using the coating composition as an undercoat paint for various structures, particularly metal structures such as steel towers, the progress of deterioration of the structures due to rust, etc. can be significantly suppressed. Furthermore, by combining the coating composition having self-repairing properties of the present invention with durable coating materials such as epoxy resin coating materials and silicone-based coating materials, it is possible to provide a long-life laminated coating film and a long-life coating system that have higher weather resistance and rust prevention properties than conventional anti-rust coating materials and are expected to reduce the number of times that coating repairs are required. [Brief description of the drawings]
[0011] [Figure 1] FIG. 13 shows the results of tensile tests on a coating film before and after self-repair. [Diagram 2] FIG. 13 shows the results of a test to confirm the repairability of a self-repairing coating film. [Diagram 3] FIG. 1 shows the results of measuring the adhesion of a coating film before and after an accelerated aging test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The coating composition having a self-repairing function of the present invention includes a polymer having a self-repairing function composed of a polymer (A) having a 3,4-dihydroxyphenyl group in a side chain and 1,4-phenylenediboronic acid (B), and an organic solvent, the organic solvent including at least one selected from a propylene glycol ether-based solvent and an alcohol-based solvent having a boiling point of 80° C. or more. The coating composition further preferably includes a silane coupling agent. That is, the polymer having a self-repairing function of the present invention has a structure in which the polymer (A) is crosslinked by boronic acid to form a network. JPEG2024138827000002.jpg50139
[0013] The polymer (A) constituting the coating composition having a self-repairing function of the present invention is described in Japanese Patent No. 6850973. As long as the side chain has a 3,4-dihydroxyphenyl group (catechol group), its structure is not particularly limited. As the polymer (A), a homopolymer of a vinyl monomer (a) containing a 3,4-dihydroxyphenyl group (catechol group) or a copolymer of the monomer (a) and another polymerizable unsaturated monomer (b) is mentioned. Among them, it is described that the polymer P(DA-co-BA) containing N-(2-(3,4-dihydroxyphenyl)ethyl)acrylamide (a) as a constituent unit is preferable in terms of ease of synthesis and availability as a raw material.
[0014] The above-mentioned N-(2-(3,4-dihydroxyphenyl)ethyl)acrylamide (dopamine acrylamide) has been reported in Non-Patent Document 1 and the like. According to Non-Patent Document 1, it can be obtained by reacting acrylic acid with acrylic chloride in the presence of triethylamine to obtain acrylic anhydride, and then reacting the acrylic anhydride with 2-(3,4-dihydroxyphenyl)ethylamine hydrochloride. In addition, as the 2-(3,4-dihydroxyphenyl)ethylamine hydrochloride, a commercially available product known as dopamine hydrochloride can also be used.
[0015] JPEG2024138827000003.jpg59139
[0016] The polymer (A) is preferably obtained as a copolymer of a vinyl monomer (a) containing a 3,4-dihydroxyphenyl group (catechol group), such as N-(2-(3,4-dihydroxyphenyl)ethyl)acrylamide, and another polymerizable unsaturated monomer (b). A homopolymer of N-(2-(3,4-dihydroxyphenyl)ethyl)acrylamide (a) is difficult to form a good coating film because the polymer is denatured at a temperature lower than the glass transition temperature (differential scanning calorimetry (DSC) method), crosslinking occurs, and the polymer is thermally cured. However, by copolymerizing it with another polymerizable unsaturated monomer having a low glass transition temperature, coating film formability can be imparted.
[0017] The ratio of the vinyl monomer (a) containing a 3,4-dihydroxyphenyl group in the polymer (A) is preferably 5 to 90 mol%, more preferably 10 to 50 mol%, and particularly preferably 10 to 30 mol%. If the ratio of (a) is 5 mol% or more, it is possible to impart a self-repairing function to the polymer (A) by adding a boron compound (boronic acid), and if it is 90 mol% or less, it is possible to impart a coating film-forming property to the polymer (A).
[0018] The proportion of the other polymerizable unsaturated monomer (b) in the polymer (A) is preferably 10 to 95 mol %, more preferably 50 to 90 mol %, particularly preferably 70 to 90 mol %. The other polymerizable unsaturated monomer (b) may be used alone or in combination of two or more.
[0019] Examples of the other polymerizable unsaturated monomer (b) that can be used include C1-22 alkyl esters of (meth)acrylic acid, C2-18 alkoxyalkyl esters of (meth)acrylic acid, aminoacrylic monomers, acrylamide monomers, epoxy group-containing monomers, hydroxyl group-containing monomers, and alkylene oxide group-containing monomers. Examples of the alkyl esters of (meth)acrylic acid having 1 to 22 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, lauryl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, etc. Examples of the alkoxyalkyl esters of (meth)acrylic acid having 2 to 18 carbon atoms include methoxybutyl (meth)acrylate, methoxyethyl (meth)acrylate, etc. Examples of aminoacrylic monomers include N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, Nt-butylaminoethyl (meth)acrylate, and N,N-dimethylaminopropyl (meth)acrylate. Examples of acrylamide monomers include acrylamide, methacrylamide, N-methylacrylamide, N-methylmethacrylamide, N-ethylacrylamide, N-ethylmethacrylamide, N-butylacrylamide, N-butylmethacrylamide, N,N-dimethylacrylamide, and N,N-dimethylmethacrylamide. Examples of epoxy group-containing monomers include glycidyl acrylate and glycidyl methacrylate. Examples of the hydroxyl group-containing monomer include hydroxyl group-containing monomers having one or more hydroxyl groups and one or more polymerizable unsaturated bonds in one molecule, such as monoesters of glycols having 2 to 20 carbon atoms and (meth)acrylic acid, such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxybutyl (meth)acrylate. Examples of the alkylene oxide group-containing monomer include monomers having one or more ethylene oxide and / or propylene oxide groups and one or more polymerizable unsaturated bonds in one molecule, such as polyoxyethylene alkoxy(meth)acrylate and polyoxypropylene alkoxy(meth)acrylate. In addition, as monomers other than the above acrylic monomers, for example, carboxyl group-containing monomers such as acrylic acid, methacrylic acid, maleic acid, itaconic acid, fumaric acid, mesaconic acid, and anhydrides and half esters thereof can also be used. Furthermore, other polymerizable unsaturated monomers such as styrene, α-methylstyrene, vinyltoluene, acrylonitrile, vinyl acetate, and vinyl chloride can also be used. Among the above unsaturated monomers, acrylic monomers are preferred in terms of reactivity with dopamine acrylamide, ease of availability, etc., and one or more types selected from acrylic monomers can be used. Among them, n-butyl acrylate is particularly preferred in terms of film-forming properties.
[0020] The polymer (A) can be produced by a known polymerization method, for example, solution polymerization, etc. The number average molecular weight (Mn) of the polymer (A) is preferably in the range of 10,000 to 1,000,000, more preferably in the range of 30,000 to 500,000.
[0021] The glass transition temperature of the polymer (A), as determined by differential scanning calorimetry (DSC), is preferably 20° C. or lower, more preferably −10° C. or lower. When 1,4-phenylenediboronic acid (B) is added to the polymer (A), the boron compound acts as a crosslinking agent, and the polymer (A) exhibits elastic mechanical strength, thereby obtaining a self-repairing function. However, when the glass transition temperature exceeds 20° C., the polymer (A) no longer exhibits elastic behavior. The lower limit of the glass transition temperature of the polymer (A) is not particularly limited, but is preferably −60° C. or higher.
[0022] By mixing a polymer (A) having a 3,4-dihydroxyphenyl group (catechol group) in the side chain with 1,4-phenylenediboronic acid (chemical formula 1) as a boron compound (B), a bonding state similar to the complex formation reaction occurring between a catechol group and a metal ion is generated by the interaction between the catechol group and a boron atom or a diboronic acid compound, and a polymer having a self-repairing function can be obtained. Specifically, the polymer (A) and 1,4-phenylenediboronic acid (chemical formula 1) are each dissolved in an organic solvent, and the two are thoroughly stirred at room temperature to prepare the polymer. 1,4-phenylenediboronic acid (chemical formula 1) is a solid powder at 20°C, and is a substance that is soluble in methanol and poorly soluble in water (solubility 2.5%), but is available from Fujifilm Wako Pure Chemical Industries, Ltd., Tokyo Chemical Industry Co., Ltd., etc. [ka]
[0023] The ratio (molar ratio) of 1,4-phenylenediboronic acid (B) to polymer (A) is preferably in the range of 0.01 to 0.2, more preferably 0.01 to 0.1, and particularly preferably 0.05 to 0.1, relative to the 3,4-dihydroxyphenyl groups in polymer (A). By setting the ratio of polymer (A) to 1,4-phenylenediboronic acid (B) within the above range, it is possible to impart a good self-repairing function to the coating film.
[0024] The coating composition having a self-repairing function of the present invention can be prepared by mixing a polymer having a self-repairing function, which is composed of a polymer (A) and 1,4-phenylenediboronic acid (B), with an organic solvent and other components according to a known method. For example, a method in which a solution of 1,4-phenylenediboronic acid (B) dissolved in an organic solvent and a basic compound such as triethylamine as a catalyst are added to a solution of a polymer (A) dissolved in an organic solvent, and the mixture is stirred; Alternatively, a method in which a basic compound such as triethylamine is added to a solution in which a polymer (A) and 1,4-phenylenediboronic acid (B) are dissolved in an organic solvent, and the solution is stirred; etc. When the components are mixed, an organic solvent may be added, if necessary.
[0025] The stirring time is preferably about 12 to 24 hours, and if it is too short, a polymer having a sufficiently uniform self-repairing function cannot be obtained, and if it is too long, the workability deteriorates. The basic compound may be a compound other than triethylamine, for example, N,N-diisopropylethylamine. The amount of the basic compound to be added is preferably 0.3 to 0.5 moles per mole of the catechol content of the polymer (A).
[0026] In the self-repairing coating composition of the present invention, the content of the organic solvent is preferably determined taking into consideration the drying properties of the resulting coating film and the appearance and physical properties of the coating film.
[0027] Examples of organic solvents that dissolve the polymer (A) and 1,4-phenylenediboronic acid (B) include ether solvents such as ethylene glycol monoethyl ether, ethylene glycol monoisopropyl ether, ethylene glycol mono-n-propyl ether, ethylene glycol mono-n-butyl ether, ethylene glycol mono-t-butyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, propylene glycol mono-n-butyl ether, and dioxane; and alcohol solvents such as methanol, ethanol, n-propanol, isopropanol, n-butanol, sec-butanol, isobutanol, and n-pentanol. By using these organic solvents, the coating properties, film-forming properties, and coating film properties (self-repairing properties) of the coating composition having a self-repairing function are improved. Preparation of a polymer with a self-repairing function takes time (12 hours or more). Therefore, by using an organic solvent with as low volatility as possible at room temperature and allowing the reaction between the polymer (A) and 1,4-phenylenediboronic acid (B) to proceed sufficiently, a polymer with a high self-repairing function can be synthesized. From this viewpoint, glycol ether-based solvents are preferred, and propylene glycol ether-based solvents are more preferred, in that they have a high boiling point (100°C or more) and excellent solubility of the polymer (A). In addition, when using an alcohol-based solvent, a solvent with a high boiling point is preferred, and propanol, butanol, etc., with a boiling point of 80°C or more, are more preferred.
[0028] The coating composition having a self-repairing function of the present invention preferably contains a silane coupling agent within a range that does not impair the effects of the present invention. By containing a silane coupling agent, the adhesion of the coating composition to a substrate and the water resistance of the coating film can be improved.
[0029] Examples of the silane coupling agent include methyltrimethoxysilane, ethyltriethoxysilane, dimethyldimethoxysilane, trimethylmethoxysilane, vinyltrimethoxysilane, 3-(glycidyloxy)propyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-trimethoxysilylpropyl isocyanate, 3-triethoxysilylpropyl isocyanate, and methyltris(ethylmethylketoxime)silane. Among the silane coupling agents, those having a reactive group such as an isocyanate group are preferred because they can react with the amino group of the self-repairing resin. In particular, compounds containing an isocyanate group such as 3-trimethoxysilylpropyl isocyanate and 3-triethoxysilylpropyl isocyanate are preferred because they have excellent adhesion to epoxy resin paints. The silane coupling agents may be used alone or in combination of two or more.
[0030] The amount of the silane coupling agent in the coating composition having a self-repairing function of the present invention is preferably 0.1 to 10 parts by mass relative to 100 parts by mass of the coating composition. From the viewpoint of improving water resistance and anticorrosive properties, it is more preferably 0.2 to 6 parts by mass, and particularly preferably 0.5 to 4 parts by mass. By adding the silane coupling agent, the performance of the anticorrosive coating film, such as the adhesion of the coating film to the structure, can be improved.
[0031] In addition to the above-mentioned components, the coating composition having a self-repairing function of the present invention may further contain, as necessary, organic solvents, pigments, thickeners, anti-sagging agents, anti-settling agents, dispersants, thixotropic agents, color separation inhibitors, and other additives (defoamers, viscosity regulators, surface conditioners, plasticizers, film-forming assistants, ultraviolet absorbers, antioxidants, leveling agents, etc.) within the range that does not impair the effects of the present invention. These additives may be used alone or in combination of two or more.
[0032] Examples of organic solvents include aromatic solvents such as toluene and xylene; ester solvents such as ethyl acetate, propyl acetate, butyl acetate, methoxybutyl acetate, amyl acetate, methyl cellosolve acetate, cellosolve acetate, diethylene glycol monomethyl ether acetate, and carbitol acetate; and ketone solvents such as dioxane, acetone, methyl ethyl ketone, and methyl isobutyl ketone. These organic solvents can be used alone or in combination. The amount of the solvent is not particularly limited.
[0033] Examples of the extender pigment include calcium carbonate, magnesium carbonate, barium sulfate, kaolin, clay, talc, mica, silica, etc. Examples of the coloring pigment include inorganic pigments such as titanium oxide, red iron oxide, carbon black, iron black, zinc oxide, etc.; and organic pigments such as molybdenum red, Prussian blue, cobalt blue, azo pigments, phthalocyanine pigments, quinacridone pigments, isoindoline pigments, threne pigments, perylene pigments, dioxazine pigments, diketopyrrolopyrrole pigments, etc. Among the above coloring pigments, inorganic pigments are preferred, and titanium oxide is preferred, because they can be used in a relatively small amount to provide coloring and because of the ease of polishing and the finish when used as a putty. The amount of pigment in the coating composition having self-repairing function of the present invention is not particularly limited, but from the viewpoint of the coloring power and appearance of the resulting coating film, it is preferably 1 to 30 parts by mass, more preferably 5 to 25 parts by mass, per 100 parts by mass of the coating composition.
[0034] Examples of the anti-sagging agent (anti-settling agent) include organic thixotropic agents such as amide wax, hydrogenated castor oil, and polyethylene oxide, and inorganic thixotropic agents such as clay minerals such as bentonite, and synthetic fine silica powder. The amount of the anti-sagging agent (anti-settling agent) in the coating composition having a self-repairing function of the present invention is preferably 0.1 to 10 parts by mass relative to 100 parts by mass of the coating composition, and more preferably 0.5 to 10 parts by mass from the viewpoint of stability. By blending one or more types of anti-sagging agents, the coatability, film formability, and film performance (flexibility, etc.) of the coating material can be improved. It is preferable to blend an anti-sagging agent.
[0035] The self-repairing coating composition of the present invention can be obtained by the above method. The coating composition is an organic solvent-based coating composition, and the solid content of the coating composition is usually about 15 to 80 mass %, preferably 15 to 50 mass %.
[0036] Examples of the object to be coated include steel towers (especially steel towers for electricity transmission) or their components, various structures such as automobiles, etc. Also, the coating may be applied to metal substrates such as cold-rolled steel plates, galvanized steel plates, zinc alloy-plated steel plates, stainless steel plates, tin-plated steel plates, etc., aluminum plates, aluminum alloy plates, etc., which form these steel towers, etc.; various plastic substrates; etc. In particular, the coating is suitable for steel plates, and is particularly suitable for galvanized steel plates. Furthermore, the object to be coated may be a metal substrate whose metal surface has been subjected to a chemical conversion treatment such as phosphate treatment or chromate treatment.
[0037] In the present invention, it is preferable to scrape a rust-free steel plate or rust-containing steel plate, and then apply the self-repairing coating composition of the present invention to the steel plate. The self-repairing coating composition is preferably applied by brush coating, roller coating, or spray coating. The wet film thickness at the time of application is preferably 50 to 200 μm, more preferably 50 to 100 μm. If the coating is applied thinly, a coating film having sufficient self-repairing function cannot be formed, and if the coating is applied thickly, when a difference in surface tension occurs due to brush marks, etc., the surface tends to break from the part with weak surface tension and cause a running-off phenomenon.
[0038] By applying the paint to the surface of the galvanized steel sheet and leaving it for about 1 to 8 hours, the organic solvent contained in the paint evaporates and a dry coating film is formed, and a coating film suitable for subsequent painting can be obtained. The thickness of the dry coating film thus obtained is preferably about 10 to 100 μm, more preferably 15 to 80 μm, and particularly preferably 15 to 60 μm. If the thickness is less than 10 μm, there is a risk that sufficient self-repairing function will not be obtained, and if the thickness exceeds 100 μm, the drying property of the coating film will decrease, which will not only decrease workability but also worsen economic efficiency.
[0039] On the surface of a steel plate or the like on which a coating film of a coating composition having a self-repairing function has been formed, it is desirable to apply a corrosion-resistant and weather-resistant coating (undercoat and topcoat) in order to prevent the catechol group from being decomposed by ultraviolet light. As the anticorrosive and weather-resistant paint, generally used anticorrosive paints such as fluororesin-based, acrylic resin-based, acrylic silicone resin-based, silicone resin-based, urethane resin-based, and epoxy resin-based paints can be used. The total thickness of the dried coating film (laminated coating film) after applying these multi-layer coatings is not particularly limited, but is usually 50 to 500 μm, preferably 100 to 400 μm. The coating method may be a conventional method. The coating method may be a conventional method.
[0040] As the undercoat paint, an epoxy resin paint is preferred because of its excellent adhesion to the self-repairing coating film. As the topcoat paint, a weather-resistant paint containing a fluororesin, an acrylic resin, an acrylic silicone resin, or a silicone resin is preferred in terms of weather resistance and ultraviolet light resistance.
[0041] The laminated coating film according to the present invention is a laminated coating film consisting of an undercoat coating film formed from the coating composition having a self-repairing function of the present invention, an epoxy resin-based intermediate coating film, and a topcoat coating film. Such a laminated coating film can be produced by forming an undercoat coating film using a coating composition having a self-repairing function, and then forming an intermediate coating film and a topcoat coating film in that order on the undercoat coating film. Specifically, it can be prepared by a method including the steps of painting a structure with a paint composition having a self-repairing function and drying the painted paint to form an undercoat coating film, painting an epoxy resin paint on the undercoat coating film, then drying and curing it to form an intermediate coating film, and painting a weather-resistant paint on the intermediate coating film to form a topcoat coating film.
[0042] The coating method of the coating composition having a self-repairing function and other coatings is not particularly limited, and conventionally known methods such as spray coating, brush coating, and roller coating can be used. When coating, the coating composition may be diluted with various solvents as necessary before coating. In addition, depending on the application and the conditions of the coating site, a base anticorrosive coating film may be formed before coating the coating composition having a self-repairing function.
[0043] The coating composition and coating system having a self-repairing function of the present invention can also be used for repair work of steel towers for electric power transmission. Not only does it eliminate the need for scraping treatment for steel towers for electric power transmission, but it is also possible to stop the occurrence and progression of rust by applying the coating of the present invention to deteriorated parts that were previously replaced because the progression of rust was at a level where it was impossible to prevent, thereby extending the life of electric power transmission facilities, shortening the period of line outages, and reducing costs. EXAMPLES
[0044] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples.
[0045] (Production Example 1) N-(2-(3,4-dihydroxyphenyl)ethyl)acrylamide (hereinafter referred to as "dopamine acrylamide") was produced by the method described in (Reference Production Example) of Japanese Patent No. 6850973. JPEG2024138827000005.jpg68145
[0046] A copolymer of dopamine acrylamide and n-butyl acrylate (hereinafter abbreviated as "P(DA-co-n-BA)") was prepared as follows. That is, 8.0 g of dopamine acrylamide (38.6 mmol), 222 mg of 2,2'-azobis(methyl isobutyrate) (0.964 mmol), 22.0 mL of butyl acrylate (19.8 g, 154 mmol), and 96 mL of ethanol (dehydrated) were added to a nitrogen-substituted 200 mL Schlenk flask. The mixture was degassed by repeating a freeze-vacuum-thaw cycle three times, and nitrogen was introduced again. The mixture was heated in a 75 ° C oil bath for 24 hours to react. The reaction was stopped by immersing the reaction vessel in liquid nitrogen, and the mixture was concentrated to about 50 mL using a rotary evaporator. After adding 30 mL of tetrahydrofuran to dissolve well, the mixture was added to hexane at 0 ° C in a Teflon (registered trademark) beaker and reprecipitated. The precipitate was collected by filtration and dried under reduced pressure to obtain 26.4 g (95% yield) of pale yellow solid P(DA-co-n-BA). The obtained P(DA-co-n-BA) was confirmed to have a molar ratio of dopamine acrylamide and butyl acrylate of 1:4 by 1H-NMR analysis. In addition, gel permeation chromatography (GPC) measurements (eluent: DMF with 10 mM lithium chloride dissolved, standard substance: polystyrene) showed that the number average molecular weight Mn was 78,000, and the ratio of the weight average molecular weight Mw to the number average molecular weight Mn was Mw / Mn = 2.1.
[0047] Example 1 4.7 g of P(DA-co-n-BA) obtained in Production Example 1 (3,4-dihydroxyphenyl groups present in the polymer are 6.5 mmol) was dissolved in 40.0 ml of propylene glycol monomethyl ether (Solution A). 108 mg (0.65 mmol) of 1,4-phenylenediboronic acid was dissolved in 6.6 ml of propylene glycol monomethyl ether (Solution B). Solutions A and B were thoroughly stirred to prepare a solvent solution of the self-repairing resin.
[0048] <Self-repairability evaluation> A cast film (thickness: approximately 60 μm) was produced from a solvent solution of the prepared self-repairing resin. After cutting the film, the ends of the cut films were overlapped, and 100 μL of water or seawater was dropped onto the cut film and left for 24 hours. After drying under reduced pressure for another 24 hours, the film was subjected to a tensile test. The results are shown in Figure 1. As shown in Figure 1, the elongation of the film before it was cut was 330%, while the elongation of the film restored after water was dropped was 230%, and the elongation of the film restored after seawater was dropped was 130%, confirming that the film properties were restored even when seawater was attached.
[0049] In addition, when a film was applied to a glass plate, a cut was made with a knife, water was dripped onto the film, and the film was left at room temperature. After 24 hours, the scratch disappeared, confirming the film's self-repairing properties.
[0050] Example 2 A coating composition having a self-repairing function (hereinafter, a self-repairing coating composition) was prepared by mixing the components shown in Table 1 in predetermined amounts with the self-repairing resin solutions A and B prepared in Example 1.
[0051] [Table 1]
[0052] <Self-repairability evaluation> When the self-repairing paint composition was applied to a steel plate and a thin scratch of 0.38 mm width was made on the surface with a cutter blade, self-repairing properties were confirmed after two days in an environment of 50°C and 99% humidity. The results of the repairability confirmation test are shown in Figure 2.
[0053] <Painting performance evaluation> The self-repairing paint composition was applied to a zinc-plated steel sheet (150 x 70 x 3 mm) using a brush (Laboran Brush, Cat. No. 9-829-01) and left to dry overnight. The thickness of the resulting coating was measured. The thickness was measured at six points along the length of each test piece using an electromagnetic coating thickness meter (SDM-3000, Sanko Electronics Laboratory Co., Ltd.) to calculate the average thickness (film thickness: approximately 30 μm).
[0054] The paint-coated test pieces were subjected to a cyclic corrosion test and a weathering test to evaluate the coating performance, and after the evaluation of the coating performance was completed, the adhesion of the coating to the galvanized steel sheet was evaluated by the following method. Boronic acid, sodium, calcium, magnesium, and nickel were used as the metal cations that form the crosslinked network structure of the resin.
[0055] (1) Cyclic corrosion test The test was conducted in accordance with JIS K5600-7-9 cyclic corrosion test method - salt spray / dry / wet cycle A. A 50±10g / L sodium chloride aqueous solution, pH 6.0-7.0 (25°C), was used as salt water, and the following cycle was repeated twice (total 16 hours): 2 hours of salt spray at 35±1°C, 4 hours of drying at 60±1°C and 20-30% RH, and 2 hours of wetting at 50±1°C and 95% RH or higher. The coating film in the cyclic corrosion test was evaluated for (a) rust formation, (b) swelling of the coating film, (c) cracking of the coating film, and (d) peeling of the coating film.
[0056] (a) Rust formation; The rust area and size were evaluated in accordance with JIS K5600-8-3. (b) Blistering of the coating; In accordance with JIS K5600-8-2 and with reference to the calibration images in Appendix A (regulations), the amount of blister (density) was evaluated on a six-point scale from 0 to 5, and the size of the blister was evaluated on a six-point scale from S0 to S5. (c) Paint cracking; The density and size of the cracks were evaluated in accordance with JIS K5600-8-4. (d) peeling of coating; The peeling area and size were evaluated in accordance with JIS K5600-8-5.
[0057] (2) Weather resistance test The adhesion was evaluated after 500 hours in accordance with JIS A6909, xenon lamp method.
[0058] (3) Measurement of adhesive strength Measurements were performed in accordance with JIS K5600-5-7 (pull-off method). For each test piece, the adhesion strength was measured at three points along the length and the average value was calculated. A solvent-free two-liquid epoxy resin was used as the adhesive to bond the test cylinder to the test piece, and an automatic adhesion tester (POSITEST AT-A, manufactured by DeFelsko Corporation) was used as the measuring device. Figure 3 shows the adhesion strength before the test, after the cyclic corrosion test (16 hours), and after the weather resistance test.
[0059] The self-repairing paint was tested for rust formation before and after accelerated aging tests, and although it showed a higher degree of rust formation than the current undercoat paint (not shown), the adhesion strength of the coating film was found to be high, with the self-repairing paint using boronic acid (bonded with B) showing the highest value both before and after the cycle test and after the weather resistance test, as shown in Figure 3. In other words, the adhesion strength of the self-repairing resin bonded with B was 97% of the adhesion strength before the test, whereas the adhesion strength of the self-repairing resin bonded with Na, Ca, and Mg had decreased to about 70% of the adhesion strength before the test for Na and Ca, and about 93% of the adhesion strength before the test for Mg, as shown in Figure 3.
[0060] (Example 3; Painting System 1) The self-repairing paint prepared in Example 2 was applied to two galvanized steel sheets (150 x 70 x 3 mm) using a brush (Laboran Brush, Cat. No. 9-829-01) and left to dry overnight. After measuring the thickness of the resulting coating, one sheet was used as a test piece (Specification 1). The remaining piece was coated with a modified epoxy paint, and then with a topcoat (urethane resin paint) on top of that, and then dried to create a test specimen (specification 2). As a comparative example, the modified epoxy paint was similarly applied to two zinc-plated steel sheets and left to dry overnight. After measuring the thickness of the resulting coating film, one sheet was used as a test piece (comparative specification 1). The remaining piece was coated with a modified epoxy paint, then coated with a topcoat (urethane resin paint) on top of that, and dried to prepare a test specimen (comparative specification 2).
[0061] Each test piece was scratched in the center of the coating before undergoing a cyclic corrosion test, and the self-repair function was evaluated based on how the scratch healed after the test. The coating was scratched with a cutter, with a depth of about 7 mm and no depth reaching the zinc-plated steel sheet.
[0062] The test results are shown in Table 2.
[0063] [Table 2]
[0064] From Table 2, it can be seen that the corrosion resistance of the test piece coated with the self-repairing paint (specification 1) is inferior to that of the modified epoxy single film (comparison specification 1). However, it can be seen that the self-repairing system film (specification 2), which is made by coating the self-repairing paint with a modified epoxy paint and a urethane resin paint, shows better corrosion resistance than the modified epoxy system film (comparison specification 2), which is made by coating the modified epoxy paint with a urethane paint.
[0065] (Example 4; Painting System 2) The self-repairing paints (two types, one with and one without adhesion promoter) prepared in Example 2 were applied to the surface of the substrate in a dry film thickness of 60 μm, and then epoxy resin paints (three types) were overcoated on top in a dry film thickness of 300 μm to prepare test pieces, and a cyclic corrosion test was carried out. As in Example 3, the coating film was scratched, and the degree of repair was evaluated based on the appearance of the coating film (adhesion, presence or absence of blistering) and the maximum blister width on one side of the scratch (water resistance) after 30 cycles (240 hours) and 90 cycles (720 hours).
[0066] The substrate was a mild steel plate "SPCC-SB" (product name, manufactured by Nippon Test Panel Co., Ltd., planar dimensions 150 mm x 75 mm, thickness 3.2 mm), and the surface was lightly polished with waterproof paper #240 to prepare the substrate surface.
[0067] The results are shown in Table 3.
[0068] [Table 3]
[0069] From Table 3, it can be seen that by using a self-repairing paint with an adhesion promoter (silane coupling agent) added as a primer, a significant difference in water resistance is observed for high-solid epoxy resin paints. A clear difference is observed in appearance and water resistance for glass flake-containing epoxy resin paints (heavy duty anti-corrosion paints). No significant difference is observed for solventless epoxy resin paints. Also, among epoxy resin paints, it can be seen that the combination of a self-repairing paint and a high-solid type epoxy resin paint, and the combination of a self-repairing paint and a solvent-free epoxy resin paint show good results.
[0070] Example 5 The self-repairing paint prepared in Example 2 (containing 0.5% by mass of the same adhesion promoter as in the Example) was applied to the surface of a substrate in a dry film thickness of 360 μm, and then the four types of commercially available epoxy resin paints listed below (Paints 1 to 4; Reference Examples) were overcoated on top in dry film thicknesses of 100 to 300 μm each to prepare test pieces (three pieces each).
[0071] Paint 1: Epoxy fluorine paint Paint 2: Epoxy silicone paint Paint 3: Epoxy silicone paint Paint 4: Epoxy urethane polyurea ion sealing paint
[0072] The substrate was a mild steel plate "SPCC-SB" (product name, manufactured by Nippon Test Panel Co., Ltd., planar dimensions 150 mm x 75 mm, thickness 3.2 mm), and the surface was lightly polished with waterproof paper #240 to prepare the substrate surface. Two sheets were without crosscuts: normal parts (No. 1, 2), and one sheet was with crosscuts: cut part (No. 3).
[0073] <Accelerated rust prevention test> The cyclic corrosion test was carried out in accordance with JIS K5600-7-9 cyclic corrosion test method - salt spray / dry / wet cycle A. A 5% aqueous solution of sodium chloride was used as the salt water, and a cycle test was conducted in which the salt water was sprayed at 35±1°C for 2 hours, dried at 60±1°C and 20-30% RH for 4 hours, and then wetted at 50±2°C and 95% RH for 2 hours.
[0074] Each test piece was evaluated for surface rust, blistering, cracking, and peeling.
[0075] <Corrosion prevention of coating film> The area and size of rust were evaluated in accordance with JIS K 5600-8-3 and in accordance with the following evaluation criteria. (Evaluation Criteria) Ri0(0); Rust area 0% Ri1: Rust area 0.05% Ri2; Rust area 0.5% Ri3: Rust area 1% Ri4; Rust area 8% Ri5: Rust area 40-50%
[0076] <Paint film swelling> In accordance with JIS K5600-8-2, the amount (density) of the blister and the size of the blister were evaluated by referring to the calibration images in Appendix A (normative). (Evaluation Criteria) 0: No blistering occurs on the coating after testing
[0077] <Cracks in the coating> According to JIS K5600-8-4, the crack density (1-2 dm 2 The crack size and crack surface area were evaluated. (Evaluation Criteria) It cannot be seen even at 0;10x magnification.
[0078] <Paint peeling> The peeling area and size were evaluated in accordance with JIS K5600-8-5. (Evaluation Criteria) 0; peeling area 0%.
[0079] The evaluation results are summarized in Table 4.
[0080] [Table 4]
[0081] From Table 4, in general areas without cross cuts, there is a tendency for rust to occur in the following order: self-repairing paint = Paint 3 ≦ Paint 4 < Paint 1 < Paint 2. Furthermore, in cut areas with cross cuts, there is a tendency for rust to occur more frequently with self-repairing paints in the following order: Paint 4 < Paint 3 < Paint 1 < Paint 2. In other words, the self-repairing paint exhibited better rust prevention properties than conventional epoxy-, silicone-, and urethane-based paints, and it was confirmed that it was able to suppress rust formation around the crosscuts, especially in test pieces with crosscuts.
[0082] <Weatherability evaluation of coating film> The weather resistance test was conducted in accordance with JIS K5400 using a Sunshine Weatherometer (manufactured by Suga Test Instruments Co., Ltd.), and after a 600-hour accelerated weather resistance test, the appearance was observed.
[0083] The results are shown in Table 5.
[0084] [Table 5]
[0085] From Table 5, it can be seen that the self-repairing coating material of the present invention (containing a silane coupling agent) shows good results in the weather resistance test.
[0086] In other words, the results of the rust prevention and weather resistance tests (Tables 4 and 5) show that by using a resin containing catechol groups, which has both a self-repairing function that allows scratches to naturally heal and an excellent metal adhesion function that allows corrosion reactions to naturally stop, as the raw material for the paint, and combining it with epoxy- or silicone-based paints, it is possible to achieve a paint with higher weather resistance and rust prevention properties than conventional rust prevention paints, and a longer life, which is expected to reduce the number of times the paint needs to be repaired. [Industrial Applicability]
[0087] The self-repairing paint and coating system of the present invention can be widely applied to undercoat coatings for steel towers, repair materials for tunnels, various coating materials, chimney coatings for thermal power plants, exterior and interior coatings for hydraulic (seawater) piping, etc. The self-repairing paint of the present invention is particularly useful as an undercoat coating.
Claims
1. A self-repairing polymer composed of a polymer (A) having a 3,4-dihydroxyphenyl group in a side chain and 1,4-phenylenediboronic acid (B), and an organic solvent; The coating composition has a self-repairing function, and the organic solvent contains at least one selected from glycol ether-based solvents and alcohol-based solvents having a boiling point of 80°C or higher.
2. The coating composition having a self-repairing function according to claim 1 , further comprising a silane coupling agent.
3. The coating composition having a self-repairing function according to claim 1, further comprising one or more coating additives selected from the group consisting of pigments, thickeners, anti-settling agents, dispersants, thixotropic agents, anti-sagging agents, and anti-color separation agents.
4. The coating composition having a self-repairing function according to claim 1, wherein the polymer (A) is a copolymer of 5 to 90 mol % of a vinyl monomer (a) containing a 3,4-dihydroxyphenyl group and 10 to 95 mol % of another polymerizable unsaturated monomer (b), and the other polymerizable unsaturated monomer (b) is at least one selected from acrylic monomers.
5. The coating film formed by the coating composition is 2. The coating composition having a self-repairing function according to claim 1, which has a network structure formed by crosslinking the 3,4-dihydroxyphenyl group of the polymer (A) with the 1,4-phenylenediboronic acid (B).
6. A laminated coating film comprising an undercoat coating film formed from the coating composition having a self-repairing function according to any one of claims 1 to 5, an epoxy resin-based intermediate coating film, and a topcoat coating film.
7. A structure having the multilayer coating film according to claim 6.
8. A coating system comprising the following steps 1, 2 and 3. Step 1: A step of applying a coating composition having a self-repairing function according to any one of claims 1 to 5 to a structure to form an undercoat coating film. Step 2: Applying an epoxy resin paint onto the undercoat to form a middle coat. Step 3: A step of applying a weather-resistant paint onto the undercoat to form a topcoat.
Citation Information
Patent Citations
Composition for peeling adhesive
JP1994080940A
Anticorrosive coating composition, coated film, shipment and marine structure
JP2017088824A
Coating having self-repairing function
JP2018076395A
Active energy ray-curable composition and method of manufacturing coated article
JP2020169269A
Coating composition, coating film, and article
JP2022050830A
Cited By
Silsesquioxane-based inorganic-organic hybrid material, self-healing composition, self-healing molded article, and self-healing film, and method for producing silsesquioxane-based inorganic-organic hybrid material
JP2026165085A