Electrostatic chuck
By matching the thermal expansion coefficients and adjusting material content in the via and conductor layers, the electrostatic chuck addresses disconnection issues, providing stable power supply and reducing wire breakage.
Patent Information
- Application Number
- JP2023049637
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2043-03-27
AI Technical Summary
The difference in thermal expansion coefficients between the conductor layer and the dielectric substrate in electrostatic chucks can lead to disconnections in the electrical path, preventing stable power supply to the conductor layer.
The electrostatic chuck design includes a dielectric substrate with a via portion containing a material matching the dielectric substrate's thermal expansion coefficient, and the conductor layer has varying material content to minimize thermal stress, with increased thickness near the via portion to further stabilize the connection.
This design stabilizes power supply to the conductor layer by reducing the likelihood of wire breakage due to thermal expansion, ensuring reliable operation of the electrostatic chuck.
Smart Images

Figure 2024138915000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrostatic chuck. [Background technology]
[0002] For example, in semiconductor manufacturing equipment such as a CVD device or an etching device, an electrostatic chuck is provided as a device for attracting and holding a substrate such as a silicon wafer to be processed. The electrostatic chuck includes a dielectric substrate provided with an attracting electrode and a base plate for supporting the dielectric substrate, which are joined together. When a voltage is applied to the attracting electrode, an electrostatic force is generated, and the substrate placed on the dielectric substrate is attracted and held.
[0003] A conductor layer is embedded inside the dielectric substrate. The conductor layer is, for example, the above-mentioned chucking electrode, but may also be an electric heater, an RF electrode, or the like. An electrode portion (e.g., an electrode terminal) for supplying power to the conductor layer is provided on the dielectric substrate at a position opposite to the mounting surface. As shown in Patent Document 1 below, the conductor layer and the electrode portion are electrically connected by an electric path provided inside the dielectric substrate.
[0004] The electric path is often configured by filling a conductive material such as tungsten inside a hole (via) formed in the dielectric substrate 100 so as to extend in a direction perpendicular to the mounting surface. Hereinafter, an electric path configured in this manner is also referred to as a "via portion." [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 7184034 Summary of the Invention [Problem to be solved by the invention]
[0006] The thermal expansion coefficient of the material constituting the conductor layer and the via portion is different from that of the material constituting the dielectric substrate, and therefore, when the dielectric substrate is fired or when an electrostatic chuck is used, the difference in the thermal expansion coefficient between the two materials may cause a defect such as a disconnection in the electric path from the conductor layer to the electrode portion, which may result in an inability to supply power to the conductor layer properly.
[0007] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide an electrostatic chuck that can stably supply power to a conductor layer embedded in a dielectric substrate. [Means for solving the problem]
[0008] In order to solve the above problems, the electrostatic chuck according to the present invention includes a dielectric substrate having a mounting surface on which an object to be attracted is placed, a conductor layer embedded in the dielectric substrate, an electrode portion provided on the dielectric substrate at a position opposite to the mounting surface, and a via portion electrically connecting the conductor layer and the electrode portion. The dielectric substrate includes a predetermined material. The content of the predetermined material per unit volume of the via portion is greater than the content of the predetermined material per unit volume of a portion of the conductor layer excluding a portion to which the via portion is connected and an area adjacent thereto.
[0009] In an electrostatic chuck having such a configuration, the via portion contains a "predetermined material" common to the dielectric substrate. The predetermined material may also be contained in the conductor layer, but in any case, the via portion contains a larger amount of the predetermined material than the conductor layer. The thermal expansion coefficient of the via portion, which is the portion most susceptible to breakage due to thermal expansion, is close to the thermal expansion coefficient of the surrounding dielectric substrate, so that the occurrence of breakage can be suppressed. In addition, since it is not necessary to make the conductor layer contain an excessive amount of the predetermined material, the performance of the conductor layer is not deteriorated.
[0010] In order to solve the above problems, an electrostatic chuck according to the present invention includes a dielectric substrate having a mounting surface on which an object to be attracted is placed, a conductor layer embedded in the dielectric substrate, an electrode portion provided on the dielectric substrate at a position opposite to the mounting surface, and a via portion electrically connecting the conductor layer and the electrode portion. The dielectric substrate includes a predetermined material. When a portion of the conductor layer including a portion to which the via portion is connected and its vicinity is defined as a first portion, and a portion of the conductor layer surrounding the first portion is defined as a second portion, the content of the predetermined material per unit volume of the first portion is greater than the content of the predetermined material per unit volume of the second portion.
[0011] In the electrostatic chuck having such a configuration, a first portion including a portion of the conductor layer to which the via portion is connected and its vicinity contains the "predetermined material" common to the dielectric substrate. The predetermined material may also be contained in a second portion, which is another portion of the conductor layer, but in any case, the first portion contains a larger amount of the predetermined material than the second portion.
[0012] The thermal expansion coefficient of the first portion, which is the portion of the conductor layer most susceptible to breakage due to thermal expansion, is close to the thermal expansion coefficient of the surrounding dielectric substrate, making it possible to suppress the occurrence of breakage, etc. Furthermore, since it is not necessary to include an excessive amount of a specific material in the entire conductor layer including the second portion, the performance of the conductor layer is not degraded.
[0013] In the electrostatic chuck according to the present invention, it is also preferable that the thickness of the conductor layer in the first portion is increased toward the via portion. By making the conductor layer thicker in the vicinity of the via portion, where breakage or the like due to thermal expansion is most likely to occur, the occurrence of breakage or the like can be further suppressed.
[0014] In the electrostatic chuck according to the present invention, the predetermined material is preferably alumina. By including alumina, which is widely used as a material for dielectric substrates, in both the dielectric substrate and the via portion (or the dielectric substrate and the first portion), it is possible to suppress the occurrence of disconnection and the like. Effect of the Invention
[0015] According to the present invention, it is possible to provide an electrostatic chuck capable of stably supplying power to a conductor layer embedded in a dielectric substrate. [Brief description of the drawings]
[0016] [Figure 1] 1 is a cross-sectional view illustrating a schematic configuration of an electrostatic chuck according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a perspective view showing a specific configuration of a via portion and the like. [Diagram 3] 4 is a cross-sectional view showing a specific configuration of a via portion, etc. FIG. [Figure 4] 11A to 11C are diagrams for explaining a method of forming a via portion and the like. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, the present embodiment will be described with reference to the accompanying drawings. In order to facilitate understanding of the description, the same components in each drawing are denoted by the same reference numerals as much as possible, and duplicated description will be omitted.
[0018] The electrostatic chuck 10 according to this embodiment is configured to electrostatically attract and hold a substrate W to be processed inside a semiconductor manufacturing apparatus (not shown), such as a CVD film forming apparatus. The substrate W is, for example, a silicon wafer. The electrostatic chuck 10 may be used in an apparatus other than a semiconductor manufacturing apparatus.
[0019] 1 shows, in a schematic cross-sectional view, the configuration of an electrostatic chuck 10 in a state in which the electrostatic chuck 10 attracts and holds a substrate W. The electrostatic chuck 10 includes a dielectric substrate 100, a base plate 200, and a bonding layer 300.
[0020] The dielectric substrate 100 is a substantially disk-shaped member made of a sintered ceramic body. The dielectric substrate 100 contains, for example, high-purity alumina (Al2O3), but may contain other materials. The purity, type, and additives of the ceramics in the dielectric substrate 100 can be appropriately set in consideration of the plasma resistance and other properties required of the dielectric substrate 100 in semiconductor manufacturing equipment.
[0021] 1 of the dielectric substrate 100 is a "mounting surface" on which a substrate W, which is an object to be attracted, is placed. Also, a lower surface 120 of the dielectric substrate 100 in FIG. 1 (i.e., the surface 120 opposite to the surface 110) is a "bonded surface" that is bonded to a base plate 200 via a bonding layer 300 described below. The viewpoint when the electrostatic chuck 10 is viewed from the surface 110 side along a direction perpendicular to the surface 110 is hereinafter also referred to as a "top view".
[0022] An adsorption electrode 130 is embedded inside the dielectric substrate 100. The adsorption electrode 130 is a thin, flat conductive layer made of a metal material such as tungsten, and is arranged so as to be parallel to the surface 110. The material of the adsorption electrode 130 may be molybdenum, platinum, palladium, or the like, in addition to tungsten. The adsorption electrode 130 may be generally parallel to the surface 110 as a whole, and may include a portion that is not parallel to the surface 110. When a voltage is applied to the adsorption electrode 130 from the outside through a via portion 40 described later, an electrostatic force is generated between the surface 110 and the substrate W, thereby adsorbing and holding the substrate W. The adsorption electrode 130 may be provided in two pieces as a so-called "bipolar" electrode as in this embodiment, or may be provided with only one as a so-called "monopolar" electrode.
[0023] Electrode terminals 50 are embedded in the surface 120 corresponding to the respective chucking electrodes 130. The electrode terminals 50 and the chucking electrodes 130 are electrically connected to each other by via portions 40 provided inside the dielectric substrate 100. One end of a power supply path 13 is connected to each electrode terminal 50. The power supply path 13 is a conductive metal member (e.g., a bus bar) and is drawn out to the outside through a through hole (not shown) provided in the base plate 200. For example, a cylindrical insulating member may be provided between the inner surface of the through hole and the power supply path 13. The electrode terminals 50 are located on the opposite side of the dielectric substrate 100 from the surface 110, and are portions that receive power from the outside. The electrode terminals 50 correspond to the "electrode portion" in this embodiment.
[0024] The via portion 40, the electrode terminal 50, and the power supply path 13 constitute an electric path for applying a voltage to the chucking electrode 130. The configuration of the via portion 40 and the like is illustrated in a simplified manner in Fig. 1. The specific configuration of the via portion 40 will be described later.
[0025] A space SP is formed between the dielectric substrate 100 and the substrate W. When a process such as film formation is performed in the semiconductor manufacturing apparatus, helium gas for temperature adjustment is supplied from the outside to the space SP through a gas hole (not shown) formed in the dielectric substrate 100. By providing helium gas between the dielectric substrate 100 and the substrate W, the thermal resistance between them is adjusted, and the temperature of the substrate W is thereby maintained at an appropriate temperature. The temperature adjustment gas supplied to the space SP may be a type of gas other than helium.
[0026] A seal ring 111 and dots 112 are provided on a surface 110 which is an adsorption surface, and a space SP is formed around these.
[0027] The seal ring 111 is a wall that divides the space SP at the outermost position. The upper end of each seal ring 111 forms part of the surface 110 and abuts against the substrate W. Note that a plurality of seal rings 111 may be provided to divide the space SP. With this configuration, it is possible to individually adjust the pressure of the helium gas in each space SP and make the surface temperature distribution of the substrate W during processing more uniform.
[0028] 1 and the like, the portion marked with the reference symbol "116" is the bottom surface of the space SP. Hereinafter, this portion will also be referred to as the "bottom surface 116." The seal ring 111, together with the dots 112 described below, is formed as a result of digging down a part of the surface 110 to the position of the bottom surface 116. The bottom surface 116 may have grooves formed therein to quickly diffuse the helium gas within the space SP.
[0029] The dots 112 are circular protrusions protruding from the bottom surface 116. A plurality of dots 112 are provided and are distributed approximately evenly on the attraction surface of the dielectric substrate 100. The upper end of each dot 112 forms part of the surface 110 and abuts against the substrate W. By providing a plurality of such dots 112, bending of the substrate W is suppressed.
[0030] The base plate 200 is a substantially disk-shaped member that is bonded to the surface 120 of the dielectric substrate 100 in order to support the dielectric substrate 100. The base plate 200 is formed of a metal such as aluminum. A surface 210 of the base plate 200 on the upper side in FIG. 1 is a "bonded surface" that is bonded to the dielectric substrate 100 via a bonding layer 300. The surface of the base plate 200 including the surface 210 may be covered with an insulating film such as an alumina sprayed film.
[0031] The bonding layer 300 is a layer provided between the dielectric substrate 100 and the base plate 200, and bonds them together. The bonding layer 300 is formed by curing an adhesive made of an insulating material. For example, a silicone-based adhesive can be used as such an adhesive.
[0032] A coolant flow path 250 for flowing a coolant is formed inside the base plate 200. When a process such as film formation is performed in the semiconductor manufacturing apparatus, a coolant is supplied to the coolant flow path 250 from the outside, thereby cooling the base plate 200. Heat generated in the substrate W during the process is transferred to the coolant via the helium gas in the space SP, the dielectric substrate 100, and the base plate 200, and is discharged to the outside together with the coolant.
[0033] A specific configuration of the via portion 40 and its neighboring portion in the dielectric substrate 100 will be described. Fig. 2 shows the configuration of this portion as a schematic perspective view. Fig. 3 shows the configuration of this portion as a schematic cross-sectional view.
[0034] 2, in this embodiment, one electrode terminal 50 and the chucking electrode 130 are connected by two via portions 40. Instead of this embodiment, the number of via portions 40 connected to one electrode terminal 50 may be only one, or may be three or more.
[0035] Each via portion 40 is formed by filling the inside of a hole (via) formed in the dielectric substrate 100 with a conductive material such as tungsten. The hole is also referred to as a "via 150" below. The via 150 is a substantially cylindrical hole, and is formed to extend in a direction perpendicular to the surface 110. The via portion 40 is configured as a conductive member disposed inside the via 150.
[0036] A recess (not shown) is formed on the surface 120 of the dielectric substrate 100, and the electrode terminal 50 is held in a state of being embedded in the recess. The electrode terminal 50 is a metal terminal having a substantially cylindrical shape. The central axis of the electrode terminal 50 is perpendicular to the surface 110 and the surface 120. In FIG. 2, the reference numeral "51" denotes a brazing material provided so as to cover the bottom surface of the recess, and is, for example, silver brazing. The electrode terminal 50 is fixed to the recess of the dielectric substrate 100 via the brazing material 51. The brazing material 51, together with the via portion 40 and the like, constitutes a part of an electric path for supplying power to the chucking electrode 130.
[0037] Instead of the electrode terminal 50, a thin metal plate may be provided at the position of the brazing material 51, and a rod-shaped pin inserted from the outside may be brought into contact with the metal plate. In this case, the metal plate corresponds to the "electrode portion."
[0038] 3 shows a cross section of the via portion 40 and its vicinity of the dielectric substrate 100, taken along a plane including the central axis of the via portion 40. As shown in the figure, the thickness of the chucking electrode 130 is not uniform throughout. The thickness of the chucking electrode 130 is locally larger in the portion where the via portion 40 is connected and in its vicinity. Note that the "thickness" here refers to the dimension along the direction perpendicular to the surface 110.
[0039] For ease of explanation, the portion of the chucking electrode 130 surrounded by the dotted line DL1 in Fig. 3 is also referred to as the "connected portion 130A" below. The portion of the chucking electrode 130 surrounded by the dotted line DL2 in Fig. 3 is also referred to as the "middle portion 130B" below. Furthermore, the portion of the chucking electrode 130 surrounded by the dotted line DL3 in Fig. 3 is also referred to as the "periphery portion 130C" below.
[0040] The connected portion 130A is a portion of the chucking electrode 130 to which the via portion 40 is connected. The connected portion 130A can also be said to be a portion of the chucking electrode 130 that overlaps with the via portion 40 in a top view.
[0041] The intermediate portion 130B is a portion of the chucking electrode 130 near the connected portion 130A. In a top view, the intermediate portion 130B surrounds the connected portion 130A in a circular shape. As shown in Fig. 3, in the intermediate portion 130B, the chucking electrode 130 becomes gradually thicker as it approaches the connected portion 130A.
[0042] The peripheral portion 130C is a portion of the chucking electrode 130 excluding the connected portion 130A and the intermediate portion 130B. In the peripheral portion 130C, the thickness of the chucking electrode 130 is generally uniform throughout. The thickness of the chucking electrode 130 in the peripheral portion 130C is smaller than the thickness of the chucking electrode 130 in the connected portion 130A. The intermediate portion 130B described above smoothly connects the connected portion 130A and the peripheral portion 130C, which have different thicknesses, by varying the thickness depending on the position.
[0043] As described above, the dielectric substrate 100 is a ceramic sintered body containing high-purity alumina. The chucking electrode 130 and the via portion 40 built into the dielectric substrate 100 are both formed of a metal material such as tungsten. In such a configuration, the thermal expansion coefficients of the materials constituting the chucking electrode 130 and the via portion 40 are generally different from the thermal expansion coefficients of the materials constituting the dielectric substrate 100. For this reason, when the dielectric substrate 100 is fired or when the electrostatic chuck 10 is used (i.e., when the substrate W is processed), there is a concern that a defect such as a break in the electrical path from the conductor layer to the electrode portion may occur due to the difference in the thermal expansion coefficient between the dielectric substrate 100 and the via portion 40, etc.
[0044] Therefore, in this embodiment, the same material as that contained in the dielectric substrate 100 is contained in the via portion 40 and the attraction electrode 130. This makes the thermal expansion coefficient of the via portion 40 etc. closer to that of the dielectric substrate 100, thereby suppressing the occurrence of disconnection and the like as described above.
[0045] The above-mentioned material contained in the via portion 40, etc., i.e., "the same material as that contained in the dielectric substrate 100", refers to a material having the same composition as the material constituting the dielectric substrate 100, and in this embodiment, specifically, is alumina.
[0046] As described above, the material contained in the chucking electrode 130 etc. for the purpose of adjusting the thermal expansion coefficient and also contained in the dielectric substrate 100 is hereinafter also referred to as an "adjustment material." For example, a member made of the same material as the dielectric substrate 100 may be formed into particles of a predetermined size, and a plurality of such particles may be contained in each of the chucking electrode 130 and the via portion 40 as the adjustment material.
[0047] The content of the adjustment material per unit volume is not uniform throughout the chucking electrode 130 and the via portion 40, but varies from place to place. The "content" here refers to, for example, mass, but may also refer to volume.
[0048] In this embodiment, the content of the adjustment material per unit volume of the via portion 40 is greater than the content of the adjustment material per unit volume of the portion of the chucking electrode 130 excluding the portion to which the via portion 40 is connected and its vicinity. The "portion of the chucking electrode 130 excluding the portion to which the via portion 40 is connected and its vicinity" refers to the peripheral portion 130C.
[0049] In a configuration in which the content of the adjusting material is adjusted as described above, the via portion 40 contains a large amount of the adjusting material (alumina) that is common to the dielectric substrate 100. The content of the adjusting material in the peripheral portion 130C may be 0, or the peripheral portion 130C may contain a small amount of the adjusting material. In either case, the via portion 40 contains a larger amount of the adjusting material than the peripheral portion 130C.
[0050] The thermal expansion coefficient of the via portion 40, which is the portion most susceptible to breakage due to thermal expansion, is close to the thermal expansion coefficient of the surrounding dielectric substrate 100, so that it is possible to suppress the occurrence of breakage, etc. Note that the peripheral portion 130C, which occupies the majority of the chucking electrode 130, does not need to contain an excessive amount of adjustment material, so that the performance of the chucking electrode 130 is not degraded.
[0051] Hereinafter, the combined whole of the connected portion 130A, which is the portion of the chucking electrode 130 to which the via portion 40 is connected, and the intermediate portion 130B, which is the portion adjacent thereto, will be referred to as the "first portion." The portion of the chucking electrode 130 surrounding the first portion, i.e., the peripheral portion 130C, will be referred to as the "second portion." In this embodiment, the content of the adjustment material per unit volume of the first portion (connected portion 130A, intermediate portion 130B) is greater than the content of the adjustment material per unit volume of the second portion (peripheral portion 130C). The content of the adjustment material per unit volume of the first portion (connected portion 130A, intermediate portion 130B) is approximately equal to the content of the adjustment material per unit volume of the via portion 40.
[0052] In the configuration in which the content of the adjusting material is adjusted as described above, the first portion (connected portion 130A, intermediate portion 130B) of the attraction electrode 130 contains a large amount of the adjusting material (alumina) that is common to the dielectric substrate 100. As described above, the content of the adjusting material in the peripheral portion 130C may be 0, or the peripheral portion 130C may contain a small amount of the adjusting material. In either case, the first portion (connected portion 130A, intermediate portion 130B) contains a larger amount of the adjusting material than the second portion (peripheral portion 130C).
[0053] The thermal expansion coefficient of the first portion of the chucking electrode 130, which is the portion most susceptible to breakage and other problems due to thermal expansion, is close to the thermal expansion coefficient of the surrounding dielectric substrate 100, thereby preventing breakage and other problems from occurring.
[0054] As described above, this embodiment employs both (1) a configuration in which the content of the adjusting material in the via portion 40 is greater than the content of the adjusting material in the peripheral portion 130C, and (2) a configuration in which the content of the adjusting material in the first portion is greater than the content of the adjusting material in the second portion. Instead of this embodiment, only one of the above (1) and (2) may be employed.
[0055] For example, the content of the adjustment material per unit volume of the via portion 40 may be greater than the content of the adjustment material per unit volume of the peripheral portion 130C, while the content of the adjustment material per unit volume of the first portion (connected portion 130A, intermediate portion 130B) may be approximately the same as the content of the adjustment material per unit volume of the peripheral portion 130C. In this case, the effect of suppressing disconnection and the like is reduced compared to the present embodiment, but a certain degree of suppression effect can be obtained compared to the conventional art.
[0056] As described above, the thickness of the chucking electrode 130 in the intermediate portion 130B of the first portion becomes thicker toward the via portion 40. By making the portion of the chucking electrode 130 near the via portion 40, which is the portion most susceptible to breakage due to thermal expansion, thicker, it is possible to further suppress the occurrence of breakage.
[0057] A method for forming the attraction electrode 130, the via portion 40, and the like having the above-mentioned configuration will be described with reference to Fig. 4. The dielectric substrate 100 of this embodiment is manufactured by stacking and pressing a plurality of green sheets 101 to obtain a molded body, and then firing the molded body.
[0058] As shown in FIG. 4(A), some of the green sheets 101 have vias 150 formed in advance, and the green sheets 101 are stacked so that the positions of the vias 150 are vertically overlapped. Then, the inside of the lined up vias 150 is filled with a conductive paste, which is the material of the via portion 40. The paste is made to be in a state of being raised further upward than the upper surface S of the uppermost green sheet 101. In FIG. 4(A), the part of the conductive paste that is raised above the upper surface S is given the reference symbol "41". This part is also referred to as the "raised portion 41" below. A predetermined amount of an adjustment material (alumina) is uniformly contained in the entire conductive paste including the raised portion 41 in advance. When viewed from above, the raised portion 41 extends to the outside of the vias 150.
[0059] Of the green sheet 101A to be laminated on the upper surface S of Fig. 4(A), a conductive paste to become the chucking electrode 130 is applied in advance to the surface facing the upper surface S. This conductive paste does not contain an adjusting material (alumina), but may contain a small amount. In either case, it is preferable that the content of the adjusting material per unit volume of the conductive paste to become the via portion 40 is greater than the content of the adjusting material per unit volume of the conductive paste to become the chucking electrode 130.
[0060] Thereafter, the green sheet 101A is placed on the upper surface S, and the entire laminate is pressed. Fig. 4(B) shows a cross section of the laminate in a state where pressing has been completed.
[0061] At this time, the portion of the upper surface S that was covered by the raised portion 41 is deformed into a concave shape as shown by the arrow AR1 as a result of the raised portion 41 being sandwiched and pressed, thereby forming an intermediate portion 130B above it.
[0062] When pressure is applied, the conductive paste applied to the green sheet 101A (the portion that becomes the attraction electrode 130) becomes integrated with the raised portion 41. Therefore, the content of the adjusting material in the conductive paste becomes locally higher in the portion that becomes integrated with the raised portion 41, and becomes approximately the same as the content of the adjusting material in the via portion 40.
[0063] As a result, as described above, in this embodiment, the content of the adjusting material per unit volume of the first portion (connected portion 130A, intermediate portion 130B) is greater than the content of the adjusting material per unit volume of the second portion (peripheral portion 130C). Also, the content of the adjusting material per unit volume of the via portion 40 is greater than the content of the adjusting material per unit volume of the peripheral portion 130C.
[0064] The "conductor layer" that receives power through the via portion 40 may be the attraction electrode 130 as in this embodiment, but may also be a layer provided for another purpose. For example, the conductor layer may be an RF electrode, an electric heater, or the like.
[0065] The present embodiment has been described above with reference to specific examples. However, the present disclosure is not limited to these specific examples. Any design modifications made by a person skilled in the art to these specific examples are also included within the scope of the present disclosure as long as they have the features of the present disclosure. The elements of each of the above-mentioned specific examples and their arrangements, conditions, shapes, etc. are not limited to those exemplified and can be changed as appropriate. The combination of each of the elements of each of the above-mentioned specific examples can be changed as appropriate as long as no technical contradiction occurs. [Explanation of symbols]
[0066] W: Substrate 10: Electrostatic chuck 40:Beer section 50: Electrode terminal 100: Dielectric substrate 110,120: face 130: Adsorption electrode 130A: Connected part 130B: Middle part 130C: Periphery
Claims
1. a dielectric substrate having a mounting surface on which an object to be attached is placed; A conductor layer embedded in the dielectric substrate; an electrode portion provided on the dielectric substrate at a position opposite to the mounting surface; a via portion electrically connecting the conductor layer and the electrode portion, the dielectric substrate includes a predetermined material; The content of the predetermined material per unit volume of the via portion is a portion of the conductor layer excluding a portion to which the via portion is connected and a portion adjacent thereto, the portion having a content of the predetermined material per unit volume being greater than the content of the predetermined material.
2. a dielectric substrate having a mounting surface on which an object to be attached is placed; A conductor layer embedded in the dielectric substrate; an electrode portion provided on the dielectric substrate at a position opposite to the mounting surface; a via portion electrically connecting the conductor layer and the electrode portion, the dielectric substrate includes a predetermined material; A portion of the conductor layer including a portion to which the via portion is connected and a vicinity thereof is defined as a first portion, When a portion of the conductor layer surrounding the first portion is defined as a second portion, The content of the predetermined material per unit volume of the first portion is a content of the predetermined material per unit volume of the second portion being greater than the content of the predetermined material.
3. 3. The electrostatic chuck according to claim 2, wherein the thickness of the conductor layer in the first portion increases toward the via portion.
4. 4. The electrostatic chuck according to claim 1, wherein the predetermined material is alumina.
Citation Information
Patent Citations
Wafer holder
JP7184034B2
Cited By
Retaining member and method for manufacturing the retaining member
JP7866117B1
Retaining member
JP7909664B1