Cemented carbide alloy for cutting tool and cutting tool substrate using the same
The cemented carbide composition with controlled Co, Ni, Ti, Ta, Nb, Zr, Hf, and V content, and optimized GAM values, addresses the issue of fracture resistance and durability in cutting tools, resulting in improved performance and longevity.
Patent Information
- Application Number
- JP2023049651
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
Existing cemented carbide cutting tools lack sufficient fracture resistance and durability under severe cutting conditions.
A cemented carbide composition with specific mass percentages of Co, Ni, Ti, Ta, Nb, Zr, Hf, and V, along with controlled GAM values for hard phase particle size distribution, enhances fracture resistance and durability.
The cemented carbide exhibits improved fracture resistance and durability, leading to enhanced cutting tool performance with reduced chipping and extended tool life.
Smart Images

Figure 2024138924000004 
Figure 2024138924000001 
Figure 2024138924000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a cemented carbide for cutting tools and a cutting tool substrate (sometimes referred to as a substrate) using the cemented carbide for cutting tools. [Background technology]
[0002] Cemented carbide is used as a cutting tool because of its hardness and toughness. In order to meet the severe cutting conditions required for cutting tools, there have been proposals to improve the cemented carbide for cutting tools and the cutting tool substrate using the cemented carbide.
[0003] For example, Patent Document 1 describes a cemented carbide alloy that includes tungsten carbide particles and a binder phase having at least one element selected from the group consisting of cobalt, nickel and iron, the binder phase being contained in a range of 7% by mass to 13% by mass, and the proportion of tungsten carbide particles having an intragranular orientation difference of 1.5° or more relative to the total number of the tungsten carbide particles being 6% or less, and that is said to have excellent chipping resistance when used as a cutting tool base. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2015-101746 A Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention has been made in consideration of the above circumstances and proposals, and has an object to provide a cemented carbide for cutting that has improved fracture resistance when used as a cutting tool base, and a cutting tool base using the cemented carbide for cutting. [Means for solving the problem]
[0006] The cemented carbide for cutting tools according to an embodiment of the present invention is One or more of Co and Ni, total of 4.0 mass% or more and 10.0 mass% or less, One or more selected from Ti, Ta, Nb, Zr, Hf, and V, in total, 4.0 mass% or more and 12.0 mass% or less; C: 6.0% by mass or more, 6.5% by mass or less, Contains 0.5 mass% or less of Cr as an optional component; The balance is W and unavoidable impurities. having a binder phase, a hard phase and a γ phase; The main component of the binder phase is Co, The main component of the hard phase is W carbide, The γ phase contains, as a main component, carbides having a cubic crystal structure containing one or more elements selected from Ti, Ta, Nb, Zr, Hf, and V, In the hard phase, (Average GAM value of hard phases having a grain size of 10% or less cumulative number) / (Average GAM value of hard phases having a grain size of 90% or more cumulative number) is 1.3 or more.
[0007] The cutting tool base body according to the embodiment of the present invention uses the above-mentioned cemented carbide for cutting tools. Effect of the Invention
[0008] The cemented carbide for cutting tools has excellent chipping resistance when used as a cutting tool substrate, and the cutting tool substrate has durability due to the improved chipping resistance. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a schematic explanatory diagram of a method for measuring the GAM value of a hard phase according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present inventors have conducted extensive research to obtain a cemented carbide alloy that achieves the above-mentioned object, and have found that the above-mentioned object can be achieved by a cemented carbide alloy for cutting tools that has a specified composition and a specified value for "(average GAM value of hard phases having a grain size of 10% or less by cumulative number) / (average GAM value of hard phases having a grain size of 90% or more by cumulative number)."
[0011] Hereinafter, the cemented carbide for cutting tools and the cutting tool base body using said alloy according to the present invention will be described, particularly focusing on an embodiment in which the cutting tool base body is used as an insert.
[0012] In this specification and claims, when a numerical range is expressed as "M to N" (M and N are both numerical values), this is equivalent to "greater than or equal to M, less than or equal to N," and the range includes the numerical values of the upper limit (N) and the lower limit (M). When a unit is stated only for the upper limit value (N), the unit of the lower limit value (M) is the same as that of the upper limit value (N).
[0013] 1. Composition and structure of cemented carbide for cutting tools The details of the composition and structure of the cemented carbide for cutting tools according to this embodiment are as follows.
[0014] (1) Co and Ni It is preferable that one or both of Co and Ni are contained. The total content of at least one of Co and Ni is preferably 4.0 mass % or more and 10.0 mass % or less. The reason is that if this content is satisfied, the resistance to plastic deformation is excellent when used as a cutting tool base.
[0015] Here, Co and Ni are mainly present in the binder phase (having crystal grains with an FCC structure), and the total of Co and Ni accounts for 50 atomic % or more of the main components of the binder phase, i.e., all components constituting the binder phase.
[0016] The binder phase may contain W and C, which are hard phase components, one or more of Cr, Ti, Ta, Nb, Zr, Hf, and V, which are contained in the gamma phase, and unavoidable impurities. When these elements are present in the binder phase, they are presumed to be in a solid solution state in the binder phase. The method for identifying the bonded phase will be described later.
[0017] (2), Ti, Ta, Nb, Zr, Hf, V It is preferable to contain at least one selected from Ti, Ta, Nb, Zr, Hf, and V in a total amount of 4.0 mass% or more and 12.0 mass% or less. If the content is less than 4.0 mass%, the oxidation resistance is insufficient, and large wear occurs due to oxidation of the hard phase during cutting, leading to the end of the life. If the content exceeds 12.0 mass%, the toughness is insufficient and chipping is likely to occur.
[0018] These elements are contained as carbides in the gamma phase as the main components. The term "main components" means that the carbides of these elements account for 50 atomic % or more of all the components that make up the gamma phase. In addition to these carbides, the gamma phase may also contain W and C contained in the hard phase, Co and Ni contained in the binder phase, and unavoidable impurities. The method for identifying the γ phase will be described later.
[0019] The average grain size of the γ phase is not particularly limited, but is preferably 1.0 μm or more and 3.0 μm or less. The reason for this is that if the average grain size is less than 1.0 μm, the gamma phases are likely to slip during cutting, resulting in insufficient resistance to plastic deformation and chipping, while if the average grain size exceeds 3.0 μm, sufficient wear resistance cannot be obtained. The average grain size of the γ phase refers to the equivalent circle diameter, that is, the diameter of a circle having an area equal to that of the γ phase, and the method of measuring this will be described later.
[0020] (3) C C is contained to form carbides and is mainly contained in the hard phase and γ phase. Its content is preferably 6.0 mass% or more and 6.5 mass% or less, and within this content range, a sufficient amount of carbides can be formed in the hard phase and γ phase.
[0021] (4)Cr Cr is an optional component and may be contained in an amount of 0.5 mass % or less. In other words, the inclusion of Cr is not essential and may not be included. Cr dissolves in the binder phase, inhibits the growth of W carbides contained in the hard phase, refines the W carbides, gives the cemented carbide a fine and uniform grain structure, increases toughness, and improves plastic deformation resistance. This function is impaired when the Cr content exceeds 0.5 mass%, causing composite carbides of Cr and W to precipitate in the binder phase, reducing toughness and potentially becoming the starting point for chipping.
[0022] (5) W W is the main component of the hard phase, that is, W carbides (mostly WC, but not limited to the stoichiometric composition) account for 50 atomic % or more of all the components that make up the hard phase. The hard phase may contain components of the binder phase, components of the gamma phase, Cr, and unavoidable impurities that are inevitably mixed in during the manufacturing process. In addition, the crystal structure of the hard phase is an HCP structure, which is different from the crystal structure of the gamma phase, which has an FCC crystal structure. The method for identifying the hard phase will be described later.
[0023] The average grain size of the hard phase is preferably 1.0 μm or more and 6.0 μm or less. If the average grain size is less than 1.0 μm, the propagation of cracks during cutting cannot be sufficiently suppressed, whereas if the average grain size is 6.0 μm or less, the plastic deformation resistance can be ensured and sufficient plastic deformation resistance is exhibited. Here, the average grain size of the hard phase refers to the equivalent circle diameter, that is, the diameter of a circle having the same area as the hard phase, and the method of measuring this will be described later.
[0024] Regarding the ratio of the GAM values of the hard phase, (Average GAM value of hard phases with a grain size of 10% or less of the total number) / (Average GAM value of hard phases with a grain size of 90% or more of the total number) is 1.3 or more It is preferable.
[0025] If this ratio is less than 1.3, the amount of dislocations already present before cutting to prevent the movement of dislocations inside the fine hard phase is insufficient, so that when cutting accompanied by large plastic deformation is performed, dislocations move easily, causing accumulation of dislocations and making the hard phase more likely to fracture. In other words, the material is not durable in cutting accompanied by large plastic deformation. It is more preferable that this ratio is 1.4 or more.
[0026] Here, the GAM value is the grain average misorientation value (average of local misorientation in crystal grains), which is the average misorientation value of all pixels in the crystal grains that constitute the hard phase. The method for measuring the GAM value will be described later.
[0027] (5) Inevitable impurities As described above, the hard phase, γ phase, and binder phase may contain impurities that are inevitably (unintentionally) mixed in during the manufacturing process, and the amount of such impurities is preferably 0.3% by mass or less, with the total amount of the cemented carbide being 100% by mass.
[0028] 2. Methods for identifying binder phase, hard phase and γ phase and measuring average grain size The binder phase, γ phase, and hard phase are identified and their average grain sizes are measured as follows. (1) Any surface or cross section of the cemented carbide is machined to a smooth surface by removing any fine irregularities that may interfere with EBSD measurement, and multiple fields of view (e.g., 5 fields of view), each with a size of, for example, 24 μm (vertical) × 72 μm (horizontal), are set on the machined surface. The surface is observed using a field emission scanning electron microscope (SEM) equipped with an energy dispersive X-ray spectrometer (EDS) and an electron backscattered diffraction device (EBSD measurement device (e.g., OIM Data Collection manufactured by EDAX / TSL (now AMETEK))) at an accelerating voltage of 15 kV with a measurement point spacing of 0.1 μm, and the EBSD pattern and EDS data are simultaneously captured.
[0029] The number of phases observed may be the same for distinguishing the binder phase, the γ phase, and the hard phase. For processing the surface or cross section, for example, a focused ion beam device (FIB device) or a cross-section polisher device (CP device) is used.
[0030] (2) Next, the measurement data is read into software for analyzing EBSD measurement results, for example, OIM Analysis ver. 7.3.1 manufactured by EDAX / TSL, and for each crystal grain, the EDS count values obtained from each measurement point inside the crystal grain corresponding to each element are averaged to obtain the EDS measurement value for each element of each crystal grain. The composition of each crystal grain is derived from the obtained measurement values.
[0031] (3) Each phase is identified according to the definition of crystal grains described above. That is, crystal grains identified as hard phases having an HCP structure from the EBSD pattern are defined as hard phases. Next, the average value of the EDS count values of Co and Ni detected is calculated from all measurement points identified as FCC phases, and the measurement points identified as FCC phases having EDS count values of Co and Ni higher than the average value are defined as binder phases, and the remainder of the FCC phase is defined as γ phases.
[0032] (4) When adjacent measurement points are judged to be the same phase, if the difference in orientation between the two measurement points is 5 degrees or more, the boundary between those two measurement points is considered to be the interface of the phase. (5) The average particle size of each phase is determined by determining the area of at least 300 particles (preferably 300 to 1000 particles), calculating the diameter of a circle equal to that area, and averaging the diameters.
[0033] (6) EDS measurement is again performed on each of the phases identified as the hard phase, γ phase, and binder phase in (3) above, and it is confirmed that the particles identified as the hard phase are composed of 50 atomic % or more of WC, the particles identified as the γ phase are composed of 50 mass % or more of M carbides (M is one or more selected from Ti, Ta, Nb, Zr, Hf, and V), and the particles identified as the binder phase are composed of 50 atomic % or more of Co and Ni combined.
[0034] (7) Based on the results of (6) above, a graph is prepared in which the horizontal axis represents the grain size of the hard phase and the vertical axis represents the cumulative percentage of the number of hard phases corresponding to each grain size on the horizontal axis ((cumulative number of hard phases up to each grain size) / (total number of hard phases)×100).
[0035] 3. Measurement of the content of each component The contents of W, Co, Ni, Ti, Ta, Nb, Zr, Hf, V, Cr, C, etc. are measured using an electron beam microanalyzer. An electron beam is irradiated onto the mirror-finished surface of a sample inserted into the electron beam microanalyzer (a surface or cross section of a cemented carbide alloy that has been machined to be smooth by removing minute irregularities so as not to interfere with electron beam microanalyzer measurements), and the components and their amounts are measured from characteristic X-rays obtained from three observation fields each measuring 100 μm (vertical) × 100 μm (horizontal), and the average of the measurement results is calculated.
[0036] 4. Measurement of GAM value In this embodiment, the hard phase is analyzed at measurement points spaced 0.1 μm apart in the vertical and horizontal directions in the same field of view as that in which the binder phase, hard phase, and γ phase are identified, using the EBSD device described above. When there is an orientation difference of 5 degrees or more between adjacent measurement points (hereinafter referred to as pixels) P, the point is defined as a grain boundary B (see FIG. 1). The area surrounded by the grain boundary is defined as one crystal grain. However, a single pixel with an orientation difference of 5 degrees or more from all adjacent pixels is not considered a crystal grain; two or more connected pixels are treated as crystal grains. A single pixel is replaced with the orientation information of the pixel with the highest CI (Coincidence Index) value among the adjacent pixels using the Cleanup function of the analysis software mentioned above. In FIG. 1, the pixel shape is a regular hexagon, but it may be another shape.
[0037] The GAM value in the present invention is the average value of the misorientation of all adjacent pixels in a crystal grain having an HCP structure. The GAM value can be expressed by the following formula [Equation 1]. Here, m represents the number of boundaries between pixels in the crystal grain, and α i represents the orientation difference at the boundary i between adjacent measurement points.
[0038]
number
[0039] Next, in the graph of the cumulative number ratio of the hard phase mentioned above, the crystal grain size at which the vertical axis is 10% is obtained, and this is set as the 10% grain size. The hard phases with crystal grain sizes of 10% grain size or less are extracted, and the average GAM value of the hard phases with a grain size of 10% or less cumulative by number can be obtained by arithmetically averaging the GAM values of each crystal grain. Similarly, in the graph of the cumulative number ratio, the crystal grain size at which the vertical axis is 90% is obtained, and this is set as the 90% grain size. The hard phases with crystal grain sizes of 90% grain size or more are extracted, and the average GAM value of the hard phases with a grain size of 90% or more cumulative by number can be obtained by arithmetically averaging the GAM values of each crystal grain. EXAMPLES
[0040] The case where the cemented carbide for cutting tools of the present invention is used as a cutting tool base will be specifically described with reference to examples, but the present invention is not limited to these examples.
[0041] 1. Preparation of Examples (1) Raw powder and blending process First, the powders for sintering were WC powder, Co powder, Ni powder, and Cr powder. 3 C 2 Powder, TiC powder, TaC powder, NbC powder, ZrC powder, HfC powder, and VC powder were prepared.
[0042] WC powder was used to determine the full width at half maximum (FWHM) of the WC (102) plane peak that appears in the range of 2θ = 77.1 - 77.4 degrees when θ / 2θ measurement was performed under out-of-plane conditions using Cu-Kα radiation with a particle size range of 2 - 3 μm. WC powder with high crystallinity and fine particles with an FWHM of 0.8 degrees or less (denoted as fine particles in Table 1) and WC powder with high crystallinity and coarse particles with a particle size range of 5 - 9 μm and an XRD FWHM of the WC (102) plane of 0.8 degrees or less (denoted as coarse particles in Table 1) were mixed at a mass ratio of 1:9 to 9:1 and further mixed with other raw material powders, and then mixed for 24 hours using a ball mill at a rotational speed in a surging state.
[0043] Here, the surging state refers to a rotational speed where the rotational speed (N) is smaller than the critical rotational speed (Nc: the rotational speed at which the grinding medium is pressed against the mill wall by centrifugal force and the contents do not fall when the rotational speed of the mill is increased), that is, N < Nc.
[0044] (2) Sintering process The obtained powder was dried and press-molded into a predetermined shape at a pressure of 100 MPa so as to become CNMG120408 - MA (tool shape manufactured by Mitsubishi Materials Corporation) after the cutting process. The temperature was raised to 1180 °C at a rate of 10 °C / min under vacuum, then raised from 1180 °C to 1350 °C at a rate of 2 °C / min, held at 1350 °C for 30 minutes, cooled (lowered the temperature) to 1180 °C at a rate of 5 °C / min, and air-cooled from the time it reached 1180 °C until it cooled to room temperature.
[0045] (3) Cutting process Following the sintering process, the sintered body was machined and ground to obtain the shape of CNMG120408 - MA, and cemented carbide cutting substrates 1 - 10 of the examples shown in Table 1 (hereinafter referred to as example tool substrates 1 - 10) were produced.
[0046] 2. Production of comparative examples In contrast, cemented carbide cutting substrates 1 - 10 of comparative examples (hereinafter referred to as comparative example tool substrates 1' - 10') were produced by the following procedure for comparison.
[0047] (1) Raw material powder and compounding process Raw material powders include Co powder, Ni powder, and Cr 3 C 2 Powder, TiC powder, TaC powder, NbC powder, ZrC powder, HfC powder, VC powder, and WC powder were prepared. Unlike the examples, the WC powder was not a mixture of fine and coarse particles, and only WC powder with a particle size range of 3 to 4 μm and high crystallinity with an XRD half-width of 0.8 degrees or less for the WC (102) plane was used.
[0048] Next, these powders were mixed for 24 hours using a ball mill rotating at a speed that caused a surging state.
[0049] (2) Sintering process The obtained powder was dried and press-molded at a pressure of 100 MPa into a specified shape to become CNMG120408-MA after the cutting process. The temperature was raised to 1350°C at a rate of 20°C / min under vacuum, held at 1350°C for 90 minutes, and then air-cooled to room temperature to produce a sintered body.
[0050] (3) Cutting process Following the sintering step, the sintered body was machined and ground to have the shape of CNMG120408-MA, and comparative example tool bases 1' to 10' shown in Table 1 were fabricated.
[0051] The cross sections of the thus-prepared Example tool substrates 1 to 10 and Comparative Example tool substrates 1' to 10' were observed by the above-mentioned method to measure the component contents, the average grain sizes of the hard phase and the γ phase, and the ratio of the GAM values. The results are shown in Table 1. In the embodiment tool substrates 1 to 10 and the comparative example tool substrates 1' to 10', the contents of unavoidable impurities were all within the above-mentioned preferable range.
[0052] The surfaces of the tool substrates 1 to 10 of the examples and the tool substrates 1' to 10' of the comparative examples were coated with a Ti layer having an average thickness of 2.0 μm. 0.5 Al 0.5The N layer was coated by PVD to produce surface-coated WC-based cemented carbide cutting tools of the embodiments (hereinafter referred to as example coated tools) 1 to 10 and surface-coated WC-based cemented carbide cutting tools of the comparative examples (hereinafter referred to as comparative example coated tools) 1' to 10'.
[0053] [Table 1]
[0054] In Table 1, "GAM value ratio" refers to (average GAM value of hard phases having a grain size of 10% or less cumulative number) / (average GAM value of hard phases having a grain size of 90% or more cumulative number).
[0055] The coated tools 1 to 10 of the examples and the coated tools 1' to 10' of the comparative examples were subjected to the following cutting tests.
[0056] Cutting test: Intermittent turning of an alloy steel round bar with four equally spaced slits along its length Work material: JIS SCM440 (HB325) round bar (4 slits evenly spaced along the length) Cutting speed: 100m / min Cutting depth: 2.0mm Feed: 0.5mm / rev Cutting time: 4 minutes
[0057] Cutting under the above conditions was performed four times for each Example and Comparative Example, and the number of times chipping occurred during cutting is shown in Table 2. Some of the coated tools of the Examples did not reach the end of their tool life, but chipping with a long side length of 10 μm or less occurred on the flank after cutting. This chipping is called mild chipping, and the number of times mild chipping occurred is shown in Table 2.
[0058] [Table 2]
[0059] The cutting test results shown in Table 2 show that the coated tools of the Examples exhibited excellent cutting performance without any chipping, whereas the coated tools of the Comparative Examples all suffered chipping and had a short tool life.
Claims
1. One or more of Co and Ni is 4.0 mass% or more and 10.0 mass% or less in total, one or more selected from Ti, Ta, Nb, Zr, Hf, and V, in total, 4.0 mass% or more and 12.0 mass% or less; C 6.0% by mass or more and 6.5% by mass or less, Contains 0.5 mass % or less of Cr as an optional component, The balance is W and unavoidable impurities, having a binder phase, a hard phase and a γ phase; The main component of the binder phase is Co, The main component of the hard phase is W carbide, The γ phase contains, as a main component, carbides having a cubic crystal structure containing one or more elements selected from Ti, Ta, Nb, Zr, Hf, and V, In the hard phase, (Average GAM value of hard phases having a grain size of 10% or less in cumulative number) / (Average GAM value of hard phases having a grain size of 90% or more in cumulative number) is 1.3 or more; 1. A cemented carbide for cutting tools, comprising:
2. A cutting tool using the cemented carbide for cutting tools according to claim 1.
Citation Information
Patent Citations
Cbn tool
JP2007030096A
Cutting tool made of WC-group cemented carbide alloy excellent in Anti-plastic deformation and Anti-chipping and cutting tool made of surface-coating WC-group cemented carbide
JP2020110891A
WC-based hard metal-made cutting tool excellent in plastic deformation resistance and defect resistance, and surface-coated WC-based hard metal-made cutting tool
JP2021134364A
Powder material for additive manufacturing and manufacturing method for molding using the powder material
JP2022155986A
Cemented carbide material and method of making same
US20150376744A1