Cemented carbide alloy for cutting tools and cutting tool substrate using the same

The cemented carbide composition with controlled components and phases addresses the issue of fracture resistance and durability in cutting tools, resulting in improved tool life and reduced wear.

JP2024138925AInactive Publication Date: 2024-10-09MITSUBISHI MATERIALS CORP

Patent Information

Application Number
JP2023049652
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing cemented carbide cutting tools lack sufficient fracture resistance and durability under severe cutting conditions.

Method used

A cemented carbide composition with specific mass percentages of Co, Ni, Ti, Ta, Nb, Zr, Hf, and V, along with controlled GAM values and particle sizes for the hard and γ phases, enhances fracture resistance and durability.

Benefits of technology

The cemented carbide exhibits improved fracture resistance and durability, leading to enhanced tool life and reduced wear during high-speed continuous cutting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138925000004
    Figure 2024138925000004
  • Figure 2024138925000001
    Figure 2024138925000001
  • Figure 2024138925000002
    Figure 2024138925000002
Patent Text Reader

Abstract

To provide a cemented carbide alloy for cutting work with improved defect resistance, and a cutting tool substrate using the alloy.SOLUTION: A cemented carbide alloy for cutting tools comprises: 10.5 to 16.0 mass% in total of one or more of Co and Ni; 4.0 to 12.0 mass% in total of one or more selected from Ti, Ta, Nb, Zr, Hf, and V; 5.8 mass% to 6.2 mass% of C; 0.5 mass% or less of Cr as an optional component; and the balance consisting of W and inevitable impurities. The cemented carbide alloy has a binder phase, a hard phase, and a γ phase. A main component of the binder phase is Co, a main component of the hard phase is W carbide, and the γ phase includes, as a main component, a cubic structure carbide comprising one or more selected from Ti, Ta, Nb, Zr, Hf, and V. In the hard phase, a ratio of (an average GAM value of the hard phase having particle size of 10% or less in cumulative number) / (an average GAM value of the hard phase having particle size of 90% or more in cumulative number) is 1.24 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cemented carbide for cutting tools and a cutting tool substrate (sometimes referred to as a substrate) using the cemented carbide for cutting tools. [Background technology]

[0002] Cemented carbide is used as a cutting tool because of its hardness and toughness. In order to meet the severe cutting conditions required for cutting tools, there have been proposals to improve the cemented carbide for cutting tools and the cutting tool substrate using the cemented carbide.

[0003] For example, Patent Document 1 describes a cemented carbide alloy that includes tungsten carbide particles and a binder phase having at least one element selected from the group consisting of cobalt, nickel and iron, the binder phase being contained in a range of 7% by mass to 13% by mass, and the proportion of tungsten carbide particles having an intragranular orientation difference of 1.5° or more relative to the total number of the tungsten carbide particles being 6% or less, and that is said to have excellent chipping resistance when used as a cutting tool base. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-101746 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention has been made in consideration of the above circumstances and proposals, and has an object to provide a cemented carbide for cutting that has improved fracture resistance when used as a cutting tool base, and a cutting tool base using the cemented carbide for cutting. [Means for solving the problem]

[0006] The cemented carbide for cutting tools according to an embodiment of the present invention is One or more of Co and Ni, total amount of 10.5 mass% or more and 16.0 mass% or less, One or more selected from Ti, Ta, Nb, Zr, Hf, and V, in total, 4.0 mass% or more and 12.0 mass% or less; C: 5.8% by mass or more, 6.2% by mass or less, containing 0.5 mass % or less of Cr as an optional component, The balance is W and unavoidable impurities. having a binder phase, a hard phase and a γ phase; The main component of the binder phase is Co, The main component of the hard phase is W carbide, The γ phase contains, as a main component, carbides having a cubic crystal structure containing one or more elements selected from Ti, Ta, Nb, Zr, Hf, and V, In the hard phase, (Average GAM value of hard phases having a grain size of 10% or less cumulative number) / (Average GAM value of hard phases having a grain size of 90% or more cumulative number) is 1.24 or less.

[0007] The cutting tool base body according to the embodiment of the present invention uses the above-mentioned cemented carbide for cutting tools. Effect of the Invention

[0008] The cemented carbide for cutting tools has excellent chipping resistance when used as a cutting tool substrate, and the cutting tool substrate has durability due to the improved chipping resistance. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is a schematic explanatory diagram of a method for measuring the GAM value of a hard phase according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present inventors have conducted extensive research to obtain a cemented carbide alloy that achieves the above-mentioned object, and have found that the above-mentioned object can be achieved by a cemented carbide alloy for cutting tools that has a specified composition and a specified value for "(average GAM value of hard phases having a grain size of 10% or less by cumulative number) / (average GAM value of hard phases having a grain size of 90% or more by cumulative number)."

[0011] Hereinafter, the cemented carbide for cutting tools and the cutting tool base body using said alloy according to the present invention will be described, particularly focusing on an embodiment in which the cutting tool base body is used as an insert.

[0012] In this specification and claims, when a numerical range is expressed as "M to N" (M and N are both numerical values), this is equivalent to "greater than or equal to M, less than or equal to N," and the range includes the numerical values ​​of the upper limit (N) and the lower limit (M). When a unit is stated only for the upper limit value (N), the unit of the lower limit value (M) is the same as that of the upper limit value (N).

[0013] 1. Composition and structure of cemented carbide for cutting tools The details of the composition and structure of the cemented carbide for cutting tools according to this embodiment are as follows.

[0014] (1) Co and Ni It is preferable that one or both of Co and Ni are contained. The total content of at least one of Co and Ni is preferably 10.5 mass % or more and 16.0 mass % or less. The reason is that if this content is satisfied, the resistance to plastic deformation is excellent when used as a cutting tool base material.

[0015] Here, Co and Ni are mainly present in the binder phase (having crystal grains with an FCC structure), and the total of Co and Ni accounts for 50 atomic % or more of the main components of the binder phase, i.e., all components constituting the binder phase.

[0016] The binder phase may contain W and C, which are hard phase components, one or more of Cr, Ti, Ta, Nb, Zr, Hf, and V, which are contained in the gamma phase, and unavoidable impurities. When these elements are present in the binder phase, they are presumed to be in a solid solution state in the binder phase. The method for identifying the bonded phase will be described later.

[0017] (2), Ti, Ta, Nb, Zr, Hf, V It is preferable to contain at least one selected from Ti, Ta, Nb, Zr, Hf, and V in a total amount of 4.0 mass% or more and 12.0 mass% or less. If the content is less than 4.0 mass%, the oxidation resistance is insufficient, and large wear occurs due to oxidation of the hard phase during cutting, leading to the end of the life. If the content exceeds 12.0 mass%, the toughness is insufficient and chipping is likely to occur.

[0018] These elements are contained as carbides in the gamma phase as the main components. The term "main components" means that the carbides of these elements account for 50 atomic % or more of all the components that make up the gamma phase. In addition to these carbides, the gamma phase may also contain W and C contained in the hard phase, Co and Ni contained in the binder phase, and unavoidable impurities. The method for identifying the γ phase will be described later.

[0019] The average grain size of the γ phase is not particularly limited, but is preferably 1.0 μm or more and 3.0 μm or less. The reason for this is that if the average grain size is less than 1.0 μm, the gamma phases are likely to slip during cutting, resulting in insufficient resistance to plastic deformation and chipping, while if the average grain size exceeds 3.0 μm, sufficient wear resistance cannot be obtained. The average grain size of the γ phase refers to the equivalent circle diameter, that is, the diameter of a circle having an area equal to that of the γ phase, and the method of measuring this will be described later.

[0020] (3) C C is contained to form carbides and is mainly contained in the hard phase and γ phase. Its content is preferably 5.8 mass% or more and 6.2 mass% or less, and within this content range, a sufficient amount of carbides can be formed in the hard phase and γ phase.

[0021] (4)Cr Cr is an optional component and may be contained in an amount of less than 0.5 mass %, that is, the inclusion of Cr is not essential and may not be included. Cr dissolves in the binder phase, inhibits the growth of W carbides contained in the hard phase, refines the W carbides, gives the cemented carbide a fine and uniform grain structure, increases toughness, and improves plastic deformation resistance. This function is impaired when the Cr content exceeds 0.5 mass%, causing composite carbides of Cr and W to precipitate in the binder phase, reducing toughness and potentially becoming the starting point for chipping.

[0022] (5) W W is the main component of the hard phase, that is, W carbides (mostly WC, but not limited to the stoichiometric composition) account for 50 atomic % or more of all the components that make up the hard phase. The hard phase may contain components of the binder phase, components of the gamma phase, Cr, and unavoidable impurities that are inevitably mixed in during the manufacturing process. In addition, the crystal structure of the hard phase is an HCP structure, which is different from the crystal structure of the gamma phase. The method for identifying the hard phase will be described later.

[0023] The average grain size of the hard phase is preferably 3.0 μm or more and 7.0 μm or less. If the average grain size is less than 3.0 μm, the propagation of cracks during cutting cannot be sufficiently suppressed, whereas if the average grain size is 7.0 μm or less, the plastic deformation resistance can be ensured and sufficient plastic deformation resistance is exhibited. Here, the average grain size of the hard phase refers to the equivalent circle diameter, that is, the diameter of a circle having the same area as the hard phase, and the method of measuring this will be described later.

[0024] Regarding the ratio of the GAM values ​​of the hard phase, (Average GAM value of hard phases with a grain size of 10% or less of the total number) / (Average GAM value of hard phases with a grain size of 90% or more of the total number) is 1.24 or less It is preferred.

[0025] If this ratio is 1.24 or less, in high-speed continuous cutting where wear resistance is required, the coarse-grained hard phase contains many dislocations due to low crystallinity even before cutting, so the coarse-grained hard phase breaks and is damaged as it wears as the cutting progresses. As a result, it is possible to suppress the shedding of the coarse-grained hard phase, making it possible to suppress wear due to self-abrasion. On the other hand, since the fine-grained hard phase has few dislocations, it suppresses micro-chipping that occurs especially near the substrate surface, and also has excellent chipping resistance. This ratio is more preferably equal to or less than 1.20.

[0026] Here, the GAM value is the grain average misorientation value (average of local misorientation in crystal grains), which is the average misorientation value of all pixels in the crystal grains that constitute the hard phase. The method for measuring the GAM value will be described later.

[0027] (5) Inevitable impurities As described above, the hard phase, γ phase, and binder phase may contain impurities that are inevitably (unintentionally) mixed in during the manufacturing process, and the amount of such impurities is preferably 0.3% by mass or less, with the total amount of the cemented carbide being 100% by mass.

[0028] 2. Methods for identifying binder phase, hard phase and γ phase and measuring average grain size The binder phase, γ phase, and hard phase are identified and their average grain sizes are measured as follows. (1) Any surface or cross section of a cemented carbide alloy is machined to a smooth surface by removing any fine irregularities that may interfere with EBSD measurement. Multiple fields of view (e.g., 5 fields of view), each with a size of, for example, 24 μm (vertical) × 72 μm (horizontal), are set on the machined surface, and the surface is observed using a field emission scanning electron microscope (SEM) equipped with an energy dispersive X-ray spectrometer (EDS) and a backscattered electron diffraction device (EBSD measurement device (e.g., OIM Data Collection manufactured by EDAX / TSL (now AMETEK))) at an accelerating voltage of 15 kV with a measurement point spacing of 0.1 μm, and the EBSD pattern and EDS data are simultaneously captured.

[0029] The number of phases observed may be the same for distinguishing the binder phase, the γ phase, and the hard phase. For processing the surface or cross section, for example, a focused ion beam device (FIB device) or a cross-section polisher device (CP device) is used.

[0030] (2) Next, the measurement data is read into software for analyzing EBSD measurement results, for example, OIM Analysis ver. 7.3.1 manufactured by EDAX / TSL, and for each crystal grain, the EDS count values ​​obtained from each measurement point inside the crystal grain corresponding to each element are averaged to obtain the EDS measurement value for each element of each crystal grain. The composition of each crystal grain is derived from the obtained measurement values.

[0031] (3) Each phase is identified according to the definition of crystal grains described above. That is, crystal grains identified as hard phases having an HCP structure from the EBSD pattern are defined as hard phases. Next, the average value of the EDS count values ​​of Co and Ni detected is calculated from all measurement points identified as FCC phases, and the measurement points identified as FCC phases having EDS count values ​​of Co and Ni higher than the average value are defined as binder phases, and the remainder of the FCC phase is defined as γ phases.

[0032] (4) When adjacent measurement points are judged to be the same phase, if the difference in orientation between the two measurement points is 5 degrees or more, the boundary between those two measurement points is considered to be the interface of the phase. (5) The average particle size of each phase is determined by determining the area of ​​at least 300 particles (preferably 300 to 1000 particles), calculating the diameter of a circle equal to that area, and averaging the diameters.

[0033] (6) EDS measurement is again performed on each of the phases identified as the hard phase, γ phase, and binder phase in (3) above, and it is confirmed that the particles identified as the hard phase contain 50 atomic % or more of WC, the particles identified as the γ phase contain 50 mass % or more of carbides of M (M is one or more selected from Ti, Ta, Nb, Zr, Hf, and V), and the particles identified as the binder phase contain 50 atomic % or more of the sum of Co and Ni.

[0034] (7) Based on the results of (6) above, a graph is prepared in which the horizontal axis represents the grain size of the hard phase and the vertical axis represents the cumulative percentage of the number of hard phases corresponding to each grain size on the horizontal axis ((cumulative number of hard phases up to each grain size) / (total number of hard phases)×100).

[0035] 3. Measurement of the content of each component The contents of W, Co, Ni, Ti, Ta, Nb, Zr, Hf, V, Cr, C, etc. are measured using an electron beam microanalyzer. An electron beam is irradiated onto the mirror-finished surface of a sample inserted into the electron beam microanalyzer (a surface or cross section of a cemented carbide alloy that has been machined to be smooth by removing minute irregularities so as not to interfere with electron beam microanalyzer measurements), and the components and their amounts are measured from characteristic X-rays obtained from three observation areas each measuring 100 μm (vertical) × 100 μm (horizontal), and the average of the measurement results is used to calculate the content.

[0036] 4. Measurement of GAM value In this embodiment, the hard phase is analyzed at measurement points spaced 0.1 μm apart in the vertical and horizontal directions in the same field of view as that in which the binder phase, hard phase, and γ phase are identified, using the EBSD device described above. When there is an orientation difference of 5 degrees or more between adjacent measurement points (hereinafter referred to as pixels) P, the point is defined as a grain boundary B (see FIG. 1). The area surrounded by the grain boundary is defined as one crystal grain. However, a single pixel with an orientation difference of 5 degrees or more from all adjacent pixels is not considered a crystal grain; two or more connected pixels are treated as crystal grains. A single pixel is replaced with the orientation information of the pixel with the highest CI (Coincidence Index) value among the adjacent pixels using the Cleanup function of the analysis software mentioned above. In FIG. 1, the pixel shape is a regular hexagon, but it may be another shape.

[0037] The GAM value in the present invention is the average value of the misorientation of all adjacent pixels in a crystal grain having an HCP structure. The GAM value can be expressed by the following formula [Equation 1]. Here, m represents the number of boundaries between pixels in the crystal grain, and α i represents the orientation difference at the boundary i between adjacent measurement points.

[0038]

number

[0039] Next, in the graph of the cumulative number ratio of the hard phase mentioned above, the crystal grain size at which the vertical axis is 10% is obtained, and this is set as the 10% grain size. The hard phases with crystal grain sizes of 10% grain size or less are extracted, and the average GAM value of the hard phases with a grain size of 10% or less cumulative by number can be obtained by arithmetically averaging the GAM values ​​of each crystal grain. Similarly, in the graph of the cumulative number ratio, the crystal grain size at which the vertical axis is 90% is obtained, and this is set as the 90% grain size. The hard phases with crystal grain sizes of 90% grain size or more are extracted, and the average GAM value of the hard phases with a grain size of 90% or more cumulative by number can be obtained by arithmetically averaging the GAM values ​​of each crystal grain. EXAMPLES

[0040] The case where the cemented carbide for cutting tools of the present invention is used as a cutting tool base will be specifically described with reference to examples, but the present invention is not limited to these examples.

[0041] 1. Preparation of Examples (1) Raw powder and blending process First, the powders for sintering were WC powder, Co powder, Ni powder, and Cr powder. 3 C 2 Powder, TiC powder, TaC powder, NbC powder, ZrC powder, HfC powder, and VC powder were prepared.

[0042] The WC powder has a particle size range of 1 - 2 μm. When using Cu-Kα rays as the X-ray source and performing θ / 2θ measurement under out-of-plane conditions, the half-value width of the WC(102) plane peak that appears in the range of 2θ = 77.1 - 77.4 degrees is determined. WC powder with high crystallinity and fine particles with a half-value width of 0.8 degrees or less (denoted as fine particles in Table 1) and WC powder with low crystallinity and coarse particles with a particle size range of 7 - 9 μm and an XRD half-value width of the WC(102) plane of 0.9 degrees or more (denoted as coarse particles in Table 1) are mixed at a mass ratio of 1:9 to 9:1, and further mixed with other raw material powders, and then mixed for 6 hours using a ball mill at a rotation speed that results in a surging state.

[0043] Here, the surging state refers to a rotation speed where the rotation speed (N) is smaller than the critical rotation speed (Nc: the rotation speed at which, when increasing the rotation speed of the mill, the grinding medium is pressed against the mill wall by centrifugal force and the contents stop falling), that is, N < Nc.

[0044] (2) Sintering process The obtained powder is dried, press-molded at a pressure of 100 MPa into a predetermined shape so as to become CNMG120408 - MA (tool shape manufactured by Mitsubishi Materials Corporation) after the cutting process, heated to 1180°C at a rate of 20°C / min under an argon atmosphere of 70 Pa, held at 1180°C for 15 minutes, heated from 1180°C to 1350°C at a rate of 5°C / min, held at 1350°C for 20 minutes, cooled (lowered in temperature) from 1350°C to 1180°C at a rate of 10°C / min, and then air-cooled from 1180°C to room temperature.

[0045] (3) Cutting process Following the sintering process, the sintered body is machined and ground to be shaped into CNMG120408 - MA, and cutting substrates 1 - 10 made of cemented carbide of the examples shown in Table 1 (hereinafter referred to as example tool substrates 1 - 10) are produced.

[0046] 2. Production of comparative examples In contrast, for comparison, cutting substrates 1 - 10 made of cemented carbide of comparative examples (hereinafter referred to as comparative example tool substrates 1 - 10) were produced by the following procedure.

[0047] (1) Raw powder and blending process Raw material powders include Co powder, Ni powder, and Cr 3 C 2 Powder, TiC powder, TaC powder, NbC powder, ZrC powder, HfC powder, VC powder, and WC powder were prepared. Unlike the examples, the WC powder was not a mixture of fine and coarse particles, and only WC powder with a particle size range of 4 to 5 μm and low crystallinity with an XRD half-width of 0.9 degrees or more for the WC (102) plane was used.

[0048] Next, these powders were mixed for 6 hours using a ball mill at a rotation speed that caused a surging state.

[0049] (2) Sintering process The obtained powder was dried and press-molded at a pressure of 100 MPa into a specified shape to become CNMG120408-MA after the cutting process. The temperature was raised to 1350°C at a rate of 20°C / min under vacuum, held at 1350°C for 90 minutes, and then air-cooled to room temperature to produce a sintered body.

[0050] (3) Cutting process Following the sintering step, the sintered body was machined and ground to have the shape of CNMG120408-MA, and comparative example tool bases 1' to 10' shown in Table 5 were fabricated.

[0051] The cross sections of the tool substrates 1 to 10 of the examples and the tool substrates 1' to 10' of the comparative examples thus prepared were observed by the above-mentioned method to measure the component contents, the average grain sizes of the hard phase and the γ phase, and the ratio of the GAM values. The results are shown in Table 1. In the embodiment tool substrates 1 to 10 and the comparative example tool substrates 1' to 10', the contents of unavoidable impurities were all within the above-mentioned preferable range.

[0052] The surfaces of the example tool substrates 1 to 10 and the comparative example tool substrates 1' to 10' were provided with a TiN layer having an average thickness of 0.2 μm, a TiCN layer having an average thickness of 4.0 μm, and an Al layer having an average thickness of 3.0 μm. 2 O 3The layer was formed by CVD to produce surface-coated WC-based cemented carbide cutting tools of Examples (hereinafter referred to as "coated tools of Examples") 1 to 10 and surface-coated WC-based cemented carbide cutting tools of Comparative Examples (hereinafter referred to as "coated tools of Comparative Examples") 1' to 10'.

[0053] [Table 1]

[0054] In Table 1, "GAM value ratio" refers to (average GAM value of hard phases having a grain size of 10% or less cumulative number) / (average GAM value of hard phases having a grain size of 90% or more cumulative number).

[0055] The coated tools 1 to 10 of the examples and the coated tools 1' to 10' of the comparative examples were subjected to the following cutting tests.

[0056] Cutting test: Continuous turning of alloy steel Work material: JIS SCM439 (HB330) round bar (4 slits evenly spaced along the length) Cutting speed: 350m / min Cut: 1.5mm Feed: 0.3mm / rev Cutting time: 4 minutes

[0057] After the cutting test, the amount of wear on the flank of the cutting edge was measured, and the state of wear of the cutting edge was observed. Note that, since all of the comparative coated tools did not reach 4 minutes of cutting time and reached the end of their tool life due to chipping during cutting, the time at which the tool life ended was measured. Table 2 shows the results of this test.

[0058] [Table 2]

[0059] "Minor chipping" in the table refers to chipping that has not reached the end of the tool life.

[0060] The cutting test results shown in Table 6 show that the coated tools of the present invention exhibited excellent wear resistance without any chipping, whereas the coated tools of the comparative examples all had a short tool life due to flank wear.

Claims

1. One or more of Co and Ni is 10.5 mass% or more and 16.0 mass% or less in total, one or more selected from Ti, Ta, Nb, Zr, Hf, and V, in total, 4.0 mass% or more and 12.0 mass% or less; C 5.8% by mass or more and 6.2% by mass or less, Contains 0.5 mass % or less of Cr as an optional component, The balance is W and unavoidable impurities, having a binder phase, a hard phase and a γ phase; The main component of the binder phase is Co, The main component of the hard phase is W carbide, The γ phase contains, as a main component, carbides having a cubic crystal structure containing one or more elements selected from Ti, Ta, Nb, Zr, Hf, and V, In the hard phase, (Average GAM value of hard phases having a grain size of 10% or less by number) / (Average GAM value of hard phases having a grain size of 90% or more by number) is 1.24 or less; 1. A cemented carbide for cutting tools, comprising:

2. A cutting tool using the cemented carbide for cutting tools according to claim 1.

Citation Information

Patent Citations

  • Cemented carbide and surface-coated cutting tool prepared using the same

    JP2015101746A

Cited By

  • Surface-coated cutting tool

    WO2025205593A1

  • Surface-coated cutting tool

    WO2025205594A1

  • Cermet member, cutting insert, and cutting tool

    WO2026203771A1

  • Cermet member, cutting insert, and cutting tool

    WO2026203777A1

  • Cermet member, cutting insert, and cutting tool

    WO2026203778A1