Photosensitive resin composition, cured product, organic el display device, and semiconductor device

The photosensitive resin composition addresses the challenge of low water absorption and high flatness by using specific alkali-soluble resins, thermal crosslinking agents, and phenolic resins, enhancing the reliability and performance of organic EL and semiconductor devices.

JP2024138963AInactive Publication Date: 2024-10-09TORAY INDUSTRIES INC

Patent Information

Application Number
JP2023049701
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing photosensitive resin compositions for organic EL display devices and semiconductor devices face challenges in achieving both low water absorption and high flatness, particularly under accelerated conditions, which affect the reliability and performance of these devices.

Method used

A photosensitive resin composition comprising alkali-soluble resins such as polyimide or polybenzoxazole precursors, quinonediazide compounds, thermal crosslinking agents with epoxy and oxetanyl groups, thermal acid generators, and phenolic resins, optimized with specific mass ratios and components to enhance flatness and reduce water absorption.

Benefits of technology

The composition achieves a highly flat and low water absorption cured product, improving the reliability and performance of organic EL display devices and semiconductor devices under various environmental conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138963000001_ABST
    Figure 2024138963000001_ABST
Patent Text Reader

Abstract

To provide a photosensitive resin composition characterized by high flatness and low water absorption in the cured product.SOLUTION: A photosensitive resin composition contains (A) one or more alkali-soluble resins selected from a polyimide precursor, a polybenzoxazole precursor and a copolymer thereof, (B) a quinonediazide compound, (C) a thermal crosslinking agent, (D) a thermal acid generator, and (E) a phenol resin, wherein (C) the thermal crosslinking agent contains (C1) a thermal crosslinking agent having an epoxy group, and (C2) a thermal crosslinking agent having an oxetanyl group.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photosensitive resin composition and a cured product using the same, and an organic EL display device and a semiconductor device each having the cured product. [Background technology]

[0002] Heat-resistant resins such as polyimide and polybenzoxazole have excellent mechanical properties, heat resistance, chemical resistance, and electrical insulation properties, and are therefore used in applications such as surface protection films for semiconductor devices such as LSIs, interlayer insulating films, insulating layers for organic electroluminescence (EL) display devices, and planarizing films for TFT substrates for display devices.

[0003] In general, an organic EL display device has a driving circuit, a planarization layer, a first electrode, a pixel division layer, a light-emitting layer, and a second electrode on a substrate, and can emit light by applying a voltage between the opposing first and second electrodes or by passing a current between them. Of these, photosensitive resin compositions that can be patterned by ultraviolet irradiation are generally used as the materials for the planarization layer and the pixel division layer.

[0004] In recent years, there has been a demand for highly reliable materials whose performance does not deteriorate even after a long period of time. Factors that reduce reliability include the release of gas components from the materials and the release of moisture contained in the materials, and the eluted components corrode wiring and pixels, causing a decrease in reliability.

[0005] Photosensitive resin compositions using polyimide-based or polybenzoxazole-based resins are preferably used because they have high heat resistance and emit small amounts of gas components from the cured product, allowing for the production of highly reliable organic EL display devices (see, for example, Patent Document 1). However, under accelerated conditions such as high temperature, high humidity, and light exposure, it is not enough to simply generate a small amount of gas components; materials with low water absorption are therefore required.

[0006] Furthermore, in organic EL display devices and semiconductor devices, the density of pixels and wiring is increasing, and there is a demand for materials that are suitable for fine pattern processing and for flattening the surfaces of objects with irregularities. In view of this, there is a strong demand for the development of a photosensitive resin composition which provides a cured product with low water absorption and excellent flatness.

[0007] In response to these problems, a method of mixing a novolac resin with a polyimide resin or a polybenzoxazole resin has been investigated as a photosensitive resin composition capable of achieving high flatness (see, for example, Patent Document 2). [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2002-91343 A [Patent Document 2] Patent Publication No. 2022-34533 Summary of the Invention [Problem to be solved by the invention]

[0009] However, the materials proposed in the above-mentioned patent documents have difficulty in achieving both a low water absorption rate of the cured product and high flatness. In view of the above problems, the present invention aims to provide a photosensitive resin composition that has high flatness and a low water absorption rate of the cured product. [Means for solving the problem]

[0010] The object of the present invention is achieved by the following configuration: [1] A photosensitive resin composition comprising (A) one or more alkali-soluble resins selected from the group consisting of polyimide precursors, polybenzoxazole precursors, and copolymers thereof, (B) a quinone diazide compound, (C) a thermal crosslinking agent, (D) a thermal acid generator, and (E) a phenolic resin, wherein the (C) thermal crosslinking agent comprises (C1) a thermal crosslinking agent having an epoxy group, and (C2) a thermal crosslinking agent having an oxetanyl group. [2] The photosensitive resin composition according to [1] above, wherein the (C1) epoxy group-containing thermal crosslinking agent contains one or more types of thermal crosslinking agents selected from the group consisting of an isocyanuric ring structure-containing epoxy thermal crosslinking agent, an alicyclic epoxy thermal crosslinking agent, and an aliphatic epoxy thermal crosslinking agent. [3] The photosensitive resin composition according to [1] or [2] above, wherein the (D) thermal acid generator contains a thermal acid generator having a sulfonate ester structure. [4] The photosensitive resin composition according to any one of [1] to [3] above, wherein the (D) thermal acid generator contains a compound represented by formula (1). [ka] (In formula (1), R 1 R is a divalent to tetravalent group having 1 to 10 carbon atoms. 2 each independently represents an alkyl group having 1 to 10 carbon atoms which may have a substituent, or an aryl group having 6 to 20 carbon atoms which may have a substituent. Examples of the substituent include a hydroxyl group, a halogen atom, a cyano group, a vinyl group, an acetylene group, or a linear or cyclic alkyl group having 1 to 10 carbon atoms. a represents an integer of 2 to 4. [5] The photosensitive resin composition according to any one of the above [1] to [4], wherein the content of the (C1) thermal crosslinking agent having an epoxy group is γ1 (mass) and the content of the (C2) thermal crosslinking agent having an oxetanyl group is γ2 (mass), and the mass ratio γ2 / γ1 is in the range of 1.1≦γ2 / γ1≦5.0. [6] The photosensitive resin composition according to any one of the above [1] to [5], wherein the (A) alkali-soluble resin contains a polybenzoxazole precursor. [7] The photosensitive resin composition according to any one of [1] to [6] above, wherein the (E) phenol resin contains polyhydroxystyrene and / or polyhydroxystyrene / polystyrene copolymer. [8] A cured product obtained by curing the photosensitive resin composition according to any one of [1] to [7] above. [9] An organic electroluminescence display device comprising the cured product according to [8] above.

[10] A semiconductor device comprising the cured product described in [8]. Effect of the Invention

[0011] The photosensitive resin composition of the present invention can provide a photosensitive resin composition having high flatness and low water absorption rate after curing. [Brief description of the drawings]

[0012] [Figure 1] 1 is a cross-sectional view illustrating a TFT substrate on which a planarizing layer and a pixel division layer are formed. [Diagram 2] FIG. 2 is a schematic explanatory view illustrating a cross section of a flatness evaluation sample. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] An embodiment of the present invention will now be described in detail. The photosensitive resin composition of the present invention is a photosensitive resin composition containing (A) one or more alkali-soluble resins selected from the group consisting of polyimide precursors, polybenzoxazole precursors, and copolymers thereof, (B) a quinone diazide compound, (C) a thermal crosslinking agent, (D) a thermal acid generator, and (E) a phenolic resin, wherein the (C) thermal crosslinking agent contains (C1) a thermal crosslinking agent having an epoxy group, and (C2) a thermal crosslinking agent having an oxetanyl group.

[0014] The photosensitive resin composition of the present invention contains (A) an alkali-soluble resin. In the present invention, the term "alkali-soluble" refers to a dissolution rate of 50 nm / min or more calculated from the reduction in film thickness when a solution of a resin dissolved in γ-butyrolactone is applied onto a silicon wafer and dried at 120°C for 4 minutes (the drying of the applied photosensitive resin film by applying heat is sometimes referred to as "prebaking") to form a dried photosensitive resin film having a film thickness of 10 μm±0.5 μm (the dried photosensitive resin film obtained by prebaking is sometimes referred to as "prebaked film"), the prebaked film is immersed in a 2.38 mass% tetramethylammonium hydroxide aqueous solution at 23±1°C for 1 minute, and then rinsed with pure water.

[0015] The alkali-soluble resin (A) is, for example, a polyimide precursor, a polybenzoxazole precursor, or a copolymer thereof. Specifically, it is preferable that the alkali-soluble resin (A) contains a polybenzoxazole precursor, and by containing the polybenzoxazole precursor, the heat resistance of the cured product and film physical properties such as water absorption are excellent.

[0016] In the present invention, one or more types of alkali-soluble resins selected from the group consisting of polyimide precursors, polybenzoxazole precursors, and copolymers thereof that can be used as the alkali-soluble resin (A) preferably have an acidic group in the structural unit of the resin and / or at the end of its main chain in order to impart the above-mentioned alkali solubility. Examples of the acidic group include a carboxyl group, a phenolic hydroxyl group, a sulfonic acid group, and a thiol group. In addition, the alkali-soluble resin preferably has a fluorine atom, which can impart water repellency to the interface between the film and the substrate during development with an alkaline aqueous solution and suppress the penetration of the alkaline aqueous solution into the interface. The fluorine atom content in the alkali-soluble resin is preferably 5% by mass or more from the viewpoint of the effect of preventing the penetration of the alkaline aqueous solution into the interface, and is preferably 20% by mass or less from the viewpoint of solubility in the alkaline aqueous solution.

[0017] The one or more alkali-soluble resins used in the photosensitive resin composition of the present invention selected from the group consisting of polyimide precursors, polybenzoxazole precursors, and copolymers thereof can be synthesized by a known method.

[0018] In the case of polyimide precursors, polyamic acid can be synthesized, for example, by reacting tetracarboxylic dianhydride with a diamine compound at low temperature. Also, polyamic acid ester can be synthesized, for example, by reacting tetracarboxylic dianhydride with a diamine compound at low temperature and then partially esterifying the amide acid structure with N,N-dimethylformamide dimethylacetal, by obtaining a diester from tetracarboxylic dianhydride and alcohol and then reacting it with an amine in the presence of a condensing agent, by obtaining a diester from tetracarboxylic dianhydride and alcohol and then converting the remaining dicarboxylic acid into an acid chloride and reacting it with an amine, or the like.

[0019] In the case of polybenzoxazole precursors, they can be produced by condensation reaction of bisaminophenol compounds with dicarboxylic acids. Specifically, there is a method of reacting a dehydration condensation agent such as dicyclohexylcarbodiimide (DCC) with an acid and adding a bisaminophenol compound to the reaction, or a method of dropping a solution of dicarboxylic acid dichloride into a solution of a bisaminophenol compound to which a tertiary amine such as pyridine has been added.

[0020] Specific examples of the acid dianhydride used as a raw material for the polyimide precursor include pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,2',3,3'-benzophenonetetracarboxylic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 2,2-bis(2,3-dicarboxyphenyl)propane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride, 2,2-bis(2,3-dicarboxyphenyl)hexafluoropropane dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, 1,1-bis(2,3 ... Examples of the tetracarboxylic acid dianhydride include aromatic tetracarboxylic acid dianhydrides such as 9,9-bis(3,4-dicarboxyphenyl)ethane dianhydride, bis(3,4-dicarboxyphenyl)methane dianhydride, bis(2,3-dicarboxyphenyl)methane dianhydride, bis(3,4-dicarboxyphenyl)ether dianhydride, 1,2,5,6-naphthalene tetracarboxylic acid dianhydride, 2,3,6,7-naphthalene tetracarboxylic acid dianhydride, 2,3,5,6-pyridine tetracarboxylic acid dianhydride, 3,4,9,10-perylene tetracarboxylic acid dianhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, and 9,9-bis{4-(3,4-dicarboxyphenoxy)phenyl}fluorene dianhydride, as well as aliphatic tetracarboxylic acid dianhydrides such as butane tetracarboxylic acid dianhydride and 1,2,3,4-cyclopentane tetracarboxylic acid dianhydride. Two or more of these may be used.

[0021] Examples of dicarboxylic acids used as raw materials for polybenzoxazole precursors include terephthalic acid, isophthalic acid, diphenyl ether dicarboxylic acid, bis(carboxyphenyl)hexafluoropropane, biphenyl dicarboxylic acid, benzophenone dicarboxylic acid, and triphenyl dicarboxylic acid. Examples of tricarboxylic acids include trimellitic acid, trimesic acid, diphenyl ether tricarboxylic acid, and biphenyl tricarboxylic acid. Examples of tetracarboxylic acids include pyromellitic acid, 3,3',4,4'-biphenyl tetracarboxylic acid, 2,3,3',4'-biphenyl tetracarboxylic acid, 2,2',3,3'-biphenyl tetracarboxylic acid, 3,3',4,4'-benzophenone tetracarboxylic acid, 2,2',3,3'-benzophenone tetracarboxylic acid, 2,2-bis(3,4-dicarboxyphenyl)propane, 2,2-bis(2,3-dicarboxyphenyl)propane, 2,2-bis(3, Examples of the tetracarboxylic acid include aromatic tetracarboxylic acids such as 4-dicarboxyphenyl)hexafluoropropane, 2,2-bis(2,3-dicarboxyphenyl)hexafluoropropane, 1,1-bis(3,4-dicarboxyphenyl)ethane, 1,1-bis(2,3-dicarboxyphenyl)ethane, bis(3,4-dicarboxyphenyl)methane, bis(2,3-dicarboxyphenyl)methane, bis(3,4-dicarboxyphenyl)ether, 1,2,5,6-naphthalenetetracarboxylic acid, 2,3,6,7-naphthalenetetracarboxylic acid, 2,3,5,6-pyridinetetracarboxylic acid, 3,4,9,10-perylenetetracarboxylic acid, 9,9-bis(3,4-dicarboxyphenyl)fluorene, and 9,9-bis{4-(3,4-dicarboxyphenoxy)phenyl}fluorene, and aliphatic tetracarboxylic acids such as butanetetracarboxylic acid and 1,2,3,4-cyclopentanetetracarboxylic acid. Two or more of these may be used.

[0022] Specific examples of diamines used as raw materials for polyimide precursors include 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 1,4-bis(4-aminophenoxy)benzene, benzidine, m-phenylenediamine, p-phenylenediamine, 1,5-naphthalenediamine, 2,6-naphthalenediamine, bis(4-aminophenoxy)biphenyl, bis{4-(4-aminophenoxy)phenyl}ether, 1,4-bis(4-aminophenoxy)benzene, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-diethyl Examples of the aromatic ring include aryl-4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminobiphenyl, 3,3'-diethyl-4,4'-diaminobiphenyl, 2,2',3,3'-tetramethyl-4,4'-diaminobiphenyl, 3,3',4,4'-tetramethyl-4,4'-diaminobiphenyl, 2,2'-di(trifluoromethyl)-4,4'-diaminobiphenyl, 9,9-bis(4-aminophenyl)fluorene, and compounds in which at least a portion of the hydrogen atoms in these aromatic rings are substituted with alkyl groups or halogen atoms, as well as aliphatic cyclohexyldiamine, methylenebiscyclohexylamine, and diamines having the structures shown below. Two or more of these may be used. [ka] In the above formula, R 2 , R 5 R represents an oxygen atom, C(CF3)2, or C(CH3)2. 3 , R 4 , R 6 ~R 13 each independently represents a hydrogen atom or a hydroxyl group.

[0023] In order to improve the storage stability of the photosensitive resin composition, it is preferable to cap the main chain ends of one or more alkali-soluble resins selected from the group consisting of polyimide precursors, polybenzoxazole precursors, and copolymers thereof with a terminal capping agent such as a monoamine, an acid anhydride, a monocarboxylic acid, a monoacid chloride compound, a monoactive ester compound, etc. For the purpose of improving the chemical resistance of the cured resin obtained by baking, a monoamine, an acid anhydride, a monocarboxylic acid, a monoacid chloride compound, or a monoactive ester compound having at least one alkenyl group or alkynyl group can also be used as the terminal capping agent.

[0024] The content of the terminal blocking agent such as monoamine, acid anhydride, acid chloride, monocarboxylic acid, etc. is preferably 1 mol% or more, more preferably 5 mol% or more, based on the total of all monomer components constituting the resin (100 mol%), from the viewpoint of improving storage stability. Also, from the viewpoint of obtaining a resin with good film properties, the content is preferably 40 mol% or less, more preferably 30 mol% or less, based on the total of all monomer components constituting the resin (100 mol%). A plurality of different terminal groups may be introduced by reacting a plurality of terminal blocking agents.

[0025] The photosensitive resin composition of the present invention contains a quinone diazide compound (B). By containing the quinone diazide compound (B), an acid is generated in the light irradiated area, which increases the solubility of the light irradiated area in an alkaline aqueous solution, thereby making it possible to obtain a positive relief pattern in which the light irradiated area is dissolved.

[0026] Examples of the quinone diazide compound include a polyhydroxy compound to which a sulfonic acid of quinone diazide is bonded via an ester bond, a polyamino compound to which a sulfonic acid of quinone diazide is bonded via a sulfonamide bond, and a polyhydroxy polyamino compound to which a sulfonic acid of quinone diazide is bonded via an ester bond and / or a sulfonamide bond. It is preferable that 50 mol % or more of the functional groups of these polyhydroxy compounds or polyamino compounds are substituted with quinone diazide. The photosensitive resin composition may contain two or more kinds of quinone diazide compounds (B).

[0027] Among (B) quinone diazide compounds, naphthoquinone diazide sulfonic acid ester compounds are preferably used, and can be synthesized by esterification reaction between a compound having a phenolic hydroxyl group and a naphthoquinone diazide sulfonic acid compound, and can be synthesized by a known method. By using these naphthoquinone diazide sulfonic acid ester compounds, resolution, sensitivity, and residual film rate can be further improved.

[0028] The compounds having a phenolic hydroxyl group used herein include Bis-Z, BisP-EZ, TekP-4HBPA, TrisP-HAP, TrisP-PA, TrisP-SA, TrisOCR-PA, BisOCHP-Z, BisP-MZ, BisP-PZ, BisP-IPZ, BisOCP-IPZ, BisP-CP, BisRS-2P, BisRS-3P, BisP-OCHP, methylenetris-FR-CR, BisRS-26X, DML-MBPC, DML-MBOC, DML-OCHP, DML-PCHP, DML-PC, DML-PTBP, DML-34X, DML-EP, DML-POP, dimethylol-BisOC-P, DML-PFP, DML-PSBP, DML-MTrisPC, TriML-P, TriML-35XL, TML-BP, TML-HQ, TM Examples of compounds include L-pp-BPF, TML-BPA, TMOM-BP, HML-TPPHBA, HML-TPHAP (all trade names, manufactured by Honshu Chemical Industry Co., Ltd.), BIR-OC, BIP-PC, BIR-PC, BIR-PTBP, BIR-PCHP, BIP-BIOC-F, 4PC, BIR-BIPC-F, TEP-BIP-A, 46DMOC, 46DMOEP, TM-BIP-A (all trade names, manufactured by Asahi Organic Chemical Industry Co., Ltd.), 2,6-dimethoxymethyl-4-tert-butylphenol, 2,6-dimethoxymethyl-p-cresol, 2,6-diacetoxymethyl-p-cresol, naphthol, tetrahydroxybenzophenone, methyl gallate, bisphenol A, bisphenol E, methylene bisphenol, and BisP-AP (trade name, manufactured by Honshu Chemical Industry Co., Ltd.). As naphthoquinone diazide sulfonic acid ester compounds, those in which naphthoquinone diazide-4-sulfonic acid or naphthoquinone diazide-5-sulfonic acid is introduced via an ester bond can be mentioned as preferred examples, but other compounds can also be used.

[0029] The naphthoquinone diazide sulfonic acid-4-ester compound has an absorption in the i-line region of a mercury lamp and is suitable for i-line exposure, while the naphthoquinone diazide-5-sulfonic acid ester compound has an absorption extending to the g-line region of a mercury lamp and is suitable for g-line exposure. The photosensitive resin composition of the present invention can contain both the naphthoquinone diazide-4-sulfonic acid ester compound and the naphthoquinone diazide-5-sulfonic acid ester compound, can contain a naphthoquinone diazide sulfonic acid ester compound in which a naphthoquinone diazide-4-sulfonyl group and a naphthoquinone diazide-5-sulfonyl group are used in combination in the same molecule, or can contain a mixture of the naphthoquinone diazide-4-sulfonic acid ester compound and the naphthoquinone diazide-5-sulfonic acid ester compound.

[0030] In the photosensitive resin composition, the content of the quinone diazide compound (B) is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, per 100 parts by mass of the alkali-soluble resin (A) from the viewpoint of improving the sensitivity during exposure, and is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, per 100 parts by mass of the alkali-soluble resin (A) from the viewpoint of reducing outgassing from the cured product.

[0031] The photosensitive resin composition of the present invention contains (C) a thermal crosslinking agent. (C) Thermal crosslinking agent refers to a compound having at least two thermally reactive functional groups in the molecule, such as a methylol group, an alkoxymethyl group, an epoxy group, or an oxetanyl group. (C) Thermal crosslinking agent crosslinks with (A) an alkali-soluble resin or other additive components, and can improve the chemical resistance and heat resistance of the cured product.

[0032] The photosensitive resin composition of the present invention contains a thermal crosslinking agent (C) having an epoxy group (C1) (hereinafter, sometimes referred to as "component (C1)"). The component (C1) has at least two epoxy groups in the molecule. By containing component (C1), the photosensitive resin composition of the present invention can crosslink with an alkali-soluble resin or other additive components during curing by heat treatment, thereby suppressing film shrinkage.

[0033] Examples of the (C1) component include those having two epoxy groups in one molecule, such as "Epicoat" (registered trademark) 807, "Epicoat" 828, "Epicoat" 1002, "Epicoat" 1750, "Epicoat" 1007, YX8100-BH30, E1256, E4250, and E4275 (all trade names, manufactured by Japan Epoxy Co., Ltd.), "Epiclon" (registered trademark) EXA-4880, and "Epiclon" EXA-48 22, "Epiclon" EXA-9583, HP4032, HP4770 (all trade names, manufactured by Dainippon Ink and Chemicals, Inc.), "Epolight" (registered trademark) 40E, "Epolight" 100E, "Epolight" 200E, "Epolight" 400E, "Epolight" 70P, "Epolight" 200P, "Epolight" 400P, "Epolight" 1500NP, "Epolight" 80MF, "Epolight" 4000, Epolight" 3002, "Epolight" 1708A, "Epolight" 1608F (all trade names, manufactured by Kyoeisha Chemical Co., Ltd.), "Denacol" (registered trademark) EX-212L, "Denacol" EX-214L, "Denacol" EX-216L, "Denacol" EX-252, "Denacol" EX-850L, "Denacol" EX-201-IM (all trade names, manufactured by Nagase ChemteX Corporation), GAN, GOT (all trade names, manufactured by Examples of such products include "Celloxide" (registered trademark) 2021P (trade name, manufactured by Daicel Corporation), "Licaresin" (registered trademark) DME-100, "Licaresin" BEO-60E (all trade names, manufactured by New Japan Chemical Co., Ltd.), "TBIS" (registered trademark)-GG, "TBIS"-RXG, and "TBIS"-BNEG (all trade names, manufactured by Taoka Chemical Co., Ltd.), and each is available from the respective companies.

[0034] As the component (C1), examples of epoxy resins having three or more epoxy groups in one molecule include VG3101L (trade name, manufactured by Printec Co., Ltd.), "TEPIC" (registered trademark)-S, "TEPIC"-L, "TEPIC"-VL, "TEPIC"-FL, and "TEPIC"-UC (all trade names, manufactured by Nissan Chemical Industries, Ltd.), "Epicron" N660, "Epicron" N695, and HP7200 (all trade names, manufactured by Nissan Chemical Industries, Ltd.). Examples of such inks include "DENACOL" EX-321L (trade name, manufactured by Dainippon Ink and Chemicals Co., Ltd.), "DENACOL" EX-321L (trade name, manufactured by Nagase ChemteX Corporation), NC6000, EPPN502H, NC3000 (all trade names, manufactured by Nippon Kayaku Co., Ltd.), "Epotohto" (registered trademark) YH-434L (trade name, manufactured by Tohto Kasei Co., Ltd.), and EHPE-3150 (trade name, manufactured by Daicel Corporation), each of which is available from the respective companies.

[0035] The (C1) component preferably contains one or more types of thermal crosslinking agents selected from the group consisting of an isocyanuric ring structure-containing epoxy thermal crosslinking agent, an alicyclic epoxy thermal crosslinking agent, and an aliphatic epoxy thermal crosslinking agent. In particular, it is preferable to contain an aliphatic epoxy thermal crosslinking agent. These epoxy thermal crosslinking agents are structured to have no aromatic ring in the molecule, thereby improving the fluidity of the resin and improving flatness. Here, the isocyanuric ring structure-containing epoxy thermal crosslinking agent is an epoxy thermal crosslinking agent containing an isocyanuric ring structure in the compound structure. The alicyclic epoxy thermal crosslinking agent is an epoxy thermal crosslinking agent having one or more alicyclic structures having 3 to 12 carbon atoms, which may have a hetero element or a branched structure, in a compound structure other than an ethylene oxide structure. The aliphatic epoxy thermal crosslinking agent is an epoxy thermal crosslinking agent having a structure having 3 to 24 carbon atoms that is not an alicyclic structure, which may have a hetero element or a branched structure, in a compound structure other than an ethylene oxide structure. In addition, in the present application, an epoxy thermal crosslinking agent having an isocyanuric ring structure, an alicyclic structure, and further an aliphatic structure is classified as an isocyanuric ring structure-containing epoxy thermal crosslinking agent, and in the present application, an epoxy thermal crosslinking agent having an alicyclic structure and further an aliphatic structure is classified as an alicyclic epoxy thermal crosslinking agent.

[0036] Examples of epoxy thermal crosslinking agents containing an isocyanuric ring structure include "TEPIC" (registered trademark)-S, "TEPIC"-L, "TEPIC"-VL, "TEPIC"-FL, and "TEPIC"-UC (all trade names, manufactured by Nissan Chemical Industries, Ltd.), and MA-DGIC (trade name, manufactured by Shikoku Kasei Co., Ltd.). Examples of alicyclic epoxy thermal crosslinking agents include "Denacol" (registered trademark) EX-252 (trade name, manufactured by Nagase ChemteX Corporation), "Epocalic" (registered trademark) THI-DE, "Epocalic" DE-102, and "Epocalic" DE-103 (all trade names, manufactured by ENEOS Corporation), "Shofree" (registered trademark) CDMDG (trade name, manufactured by Showa Denko K.K.), and "Ce Examples of the aliphatic epoxy thermal crosslinking agent include "Denacol" (registered trademark) EX-614B, "Denacol" EX-313, "Denacol" EX-512, "Denacol" EX-321L, "Denacol" EX-810, "Denacol" EX-861, "Denacol" EX-211 (all trade names, manufactured by Nagase ChemteX Corporation), "Epogosey" (registered trademark) BD, "Epogosey" NPG, "Epogosey" HD (trade names, manufactured by Yokkaichi Synthetic Co., Ltd.), and "Showfree" (registered trademark) PETG (trade name, manufactured by Showa Denko K.K.), each of which is available from the respective companies.

[0037] The content of the (C1) component is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and even more preferably 10 parts by mass or more, per 100 parts by mass of the (A) alkali-soluble resin, from the viewpoint of improving the chemical resistance of the cured product, and is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, and even more preferably 20 parts by mass or less, per 100 parts by mass of the (A) alkali-soluble resin, from the viewpoint of enabling pattern processing with high sensitivity.

[0038] The photosensitive resin composition of the present invention contains a thermal crosslinking agent (C) having an oxetanyl group (C2) (hereinafter, sometimes referred to as "component (C2)"). The component (C2) has at least two oxetanyl groups in the molecule. By containing both component (C1) and component (C2), the photosensitive resin composition of the present invention can improve flatness compared to a case where component (C1) or component (C2) is contained alone.

[0039] Although component (C2) has high fluidity when heated and is effective in improving flatness, when used alone, it does not easily progress the crosslinking reaction during heat curing and volatilizes during heat curing, which results in large film shrinkage and may worsen flatness.

[0040] By mixing components (C1) and (C2), thermal crosslinking between components (C1) and (C2) occurs, suppressing the evaporation of component (C2) during thermal curing. As a result, film shrinkage is reduced, which is believed to improve flatness more effectively. In addition, in the present application, a compound having two or more epoxy groups and two or more oxetanyl groups in the molecule is classified as a component (C1).

[0041] Examples of the (C2) component include 3,7-bis(3-oxetanyl)-5-oxa-nonane, 3,3'-(1,3-(2-methyleneyl)propanediylbis(oxymethylene))bis-(3-ethyloxetane), 1,4-bis[(3-ethyl-3-oxetanylmethoxy)methyl]benzene, 1,2-bis[(3-ethyl-3-oxetanylmethoxy)methyl]ethane, 1,3-bis[(3-ethyl-3-oxetanylmethoxy)methyl]propane, ethylene glycol bis(3-ethyl-3-oxetanylmethyl)ether, dicyclopentenyl bis(3-ethyl-3-oxetanylmethyl)ether, and triethylene glycol bis(3-ethyl-3-oxetanylmethyl). ) ether, tetraethylene glycol bis(3-ethyl-3-oxetanylmethyl) ether, tricyclodecanediyldimethylene(3-ethyl-3-oxetanylmethyl) ether, trimethylolpropane tris(3-ethyl-3-oxetanylmethyl) ether, 1,4-bis(3-ethyl-3-oxetanylmethoxy)butane, 1,6-bis(3-ethyl-3-oxetanylmethoxy)hexane, OXT-121, OXT-221, OX-SQ-H (all trade names, manufactured by Toa Gosei Co., Ltd.), "Etanacol" (registered trademark) OXBP, "Etanacol" (registered trademark) OXTP (all trade names, manufactured by Ube Industries, Ltd.), etc., each of which is available from the respective companies.

[0042] The component (C2) preferably contains an oxetanyl thermal crosslinking agent having an aromatic ring in the molecule. Because this oxetanyl thermal crosslinking agent has an aromatic ring in the molecule, it is less likely to volatilize during thermal curing and is effective in improving flatness.

[0043] Examples of oxetanyl thermal crosslinking agents having an aromatic ring in the molecule include 1,4-bis[(3-ethyl-3-oxetanylmethoxy)methyl]benzene, OXT-121 (trade name, manufactured by Toa Gosei Co., Ltd.), "Etanacol" (registered trademark) OXBP, and "Etanacol" (registered trademark) OXTP (all trade names, manufactured by Ube Industries, Ltd.), each of which is available from the respective companies. It is particularly preferable that the component (C2) contains an oxetanyl thermal crosslinking agent represented by formula (2). [ka] (n represents an integer of 1 to 3.) An example of the oxetanyl thermal crosslinking agent represented by formula (2) is "Ethanacol" (registered trademark) OXBP (product name, manufactured by Ube Industries, Ltd.).

[0044] From the viewpoint of improving flatness, the content of the (C2) component is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and even more preferably 10 parts by mass or more, relative to 100 parts by mass of the (A) alkali-soluble resin. Also, from the viewpoint of enabling pattern processing with high sensitivity, the content is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, and even more preferably 20 parts by mass or less, relative to 100 parts by mass of the (A) alkali-soluble resin.

[0045] When the content of the (C1) component is γ1 (mass) and the content of the (C2) component is γ2 (mass), from the viewpoint of achieving both a reduction in water absorption rate and high flatness of the cured product, the mass ratio γ2 / γ1 is preferably in the range of 1.1≦γ2 / γ1≦5.0. From the viewpoint of reducing the water absorption rate of the cured product, the mass ratio γ2 / γ1 is preferably 1.1 or more, more preferably 1.5 or more, and even more preferably 2.0 or more. Moreover, from the viewpoint of flatness, the mass ratio γ2 / γ1 is preferably 5.0 or less, more preferably 4.0 or less, and even more preferably 3.0 or less.

[0046] Within the above range, when component (C1) is an aliphatic epoxy thermal crosslinking agent and component (C2) is an oxetanyl thermal crosslinking agent having an aromatic ring in the molecule, a more effective effect can be obtained.

[0047] The photosensitive resin composition of the present invention may contain a thermal crosslinking agent other than the components (C1) and (C2) within a range that does not impair the sensitivity. Examples of such a thermal crosslinking agent include a thermal crosslinking agent having a methylol group and / or an alkoxymethyl group, a bismaleimide compound, an isocyanate compound, and a blocked isocyanate compound.

[0048] Examples of thermal crosslinking agents having a methylol group and / or an alkoxymethyl group include DML-PC, DML-PEP, DMOM-PC, TriML-P, TriML-35XL, TML-HQ, TML-BP, TML-pp-BPF, TML-BPE, TMOM-BP, TMOM-BPE, TMOM-BPA, TMOM-BPAF, TMOM-BPAP, HML-TPPHBA, HML-TPHAP, HMOM-TPPHBA, HMOM-TPHAP, HMOM-TPPA (all trade names, manufactured by Honshu Chemical Industry Co., Ltd.), 26DMPC, 46DMOC, DM-BIPC-F, DM-BIOC-F, and TM-BIP. Examples of such compounds include NIKALAC-A (all trade names, manufactured by Asahi Yukizai Co., Ltd.), HML-TPPHBA, HML-TPHAP, HMOM-TPPHBA, HMOM-TPHAP, and HMOM-TPPA (all trade names, manufactured by Honshu Chemical Industry Co., Ltd.), "NIKALAC" (registered trademark) MX-290, "NIKALAC" (registered trademark) MX-280, "NIKALAC" (registered trademark) MX-270, "NIKALAC" (registered trademark) MX-279, "NIKALAC" (registered trademark) MW-100LM, and "NIKALAC" (registered trademark) MX-750LM (all trade names, manufactured by Sanwa Chemical Co., Ltd.), and each of these compounds is available from the respective companies.

[0049] Examples of the bismaleimide compound include 1,2-bis(maleimide)ethane, 1,3-bis(maleimide)propane, 1,4-bis(maleimide)butane, 1,5-bis(maleimide)pentane, 1,6-bis(maleimide)hexane, 2,2,4-trimethyl-1,6-bis(maleimide)hexane, N,N'-1,3-phenylenebis(maleimide), 4-methyl-N,N'-1,3 N,N'-1,4-phenylene bis(maleimide), 3-methyl-N,N'-1,4-phenylene bis(maleimide), 4,4'-bis(maleimide)diphenylmethane, 3,3'-diethyl-5,5'-dimethyl-4,4'-bis(maleimide)diphenylmethane, or 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane.

[0050] Examples of the isocyanate compound include aromatic polyisocyanates such as 4,4'-methylenebis(phenylene isocyanate) (MDI) and tolylene diisocyanate (TDI); aliphatic polyisocyanates such as hexamethylene diisocyanate (HDI), trimethylene diisocyanate, 1,4-tetramethylene diisocyanate, pentamethylene diisocyanate and lysine diisocyanate; and alicyclic polyisocyanates such as isophorone diisocyanate (IPDI) and 4,4'-methylenebis(cyclohexyl isocyanate) (H12MDI).

[0051] Examples of the blocked isocyanate compound include compounds obtained by blocking the above-mentioned isocyanate compounds with a blocking agent such as oxime, lactam, or pyrazole, and the crosslinking temperature can be easily adjusted.

[0052] The content of the thermal crosslinking agent other than the components (C1) and (C2) is preferably 3 parts by mass or more per 100 parts by mass of the alkali-soluble resin (A) from the viewpoint of improving the heat resistance and chemical resistance of the cured product, and is preferably 30 parts by mass or less per 100 parts by mass of the alkali-soluble resin (A) from the viewpoint of enabling pattern processing with high sensitivity.

[0053] The photosensitive resin composition of the present invention contains a thermal acid generator (D). A thermal acid generator is a compound that generates an acid by heating, and the thermal decomposition starting temperature of the thermal acid generator (D) is preferably 120°C or higher, more preferably 130°C or higher, and even more preferably 140°C or higher. By setting the thermal decomposition temperature to 120°C or higher, it is possible to prevent acid from being generated in the process of drying the applied photosensitive resin film by applying heat (sometimes referred to as the "pre-baking process") in pattern processing. In addition, the thermal decomposition starting temperature of the thermal acid generator (D) is preferably 250°C or lower, more preferably 240°C or lower, and even more preferably 230°C or lower. By setting the thermal decomposition temperature to 250°C or lower, it is possible to generate sufficient acid in the thermal curing process. In the present invention, the water absorption rate of the cured product can be reduced by generating an acid in the heat treatment process. This is presumably because the (D) thermal acid generator promotes ring closure of the imide precursor structure and / or oxazole precursor structure in the (A) alkali-soluble resin in the cured product during the heat treatment process.

[0054] The (D) thermal acid generator in the photosensitive resin composition of the present invention may have the function of generating an acid by heating, and compounds having the function of generating an acid by light such as ultraviolet light in addition to heat are also included in the definition of (D) thermal acid generator. However, (B) quinone diazide compounds are defined as not being included in the (D) thermal acid generator even if they generate an acid by heating.

[0055] (D) The acid generated from the thermal acid generator is preferably a strong acid, for example, an arylsulfonic acid such as p-toluenesulfonic acid or benzenesulfonic acid, an alkylsulfonic acid such as methanesulfonic acid, ethanesulfonic acid or butanesulfonic acid, or camphorsulfonic acid.

[0056] (D) Examples of the thermal acid generator include the following sulfonium salts and sulfonate esters. Two or more of these may be used. The sulfonium salt preferably has a structure represented by formula (3). [ka] In formula (3), R 14 ~R 16 Each independently represents a monovalent organic group having 1 to 20 carbon atoms. 14 ~R 16 Examples of the monovalent organic group having 1 to 20 carbon atoms that may be represented by include a linear, branched or cyclic alkyl group having 1 to 10 carbon atoms which may have a substituent, and an aryl group having 6 to 20 carbon atoms which may have a substituent. Examples of the substituent include a hydroxyl group, a halogen atom, a cyano group, a vinyl group, an acetylene group, or a linear or cyclic alkyl group having 1 to 10 carbon atoms. Z - is R 17 SO3 - , R 17 SO4 - , R 17 COO - , SbF6 - R represents an anion moiety selected from the group consisting of 17 represents a monovalent organic group having 1 to 20 carbon atoms. 17 Examples of the monovalent organic group having 1 to 20 carbon atoms that can be taken by include an alkyl group, an aryl group, a perfluoroalkyl group, and a structure represented by the formula (4). [ka] In formula (4), * represents a bond.

[0057] In terms of generating heat by heating, the sulfonium salt of formula (3) preferably contains a compound selected from the group consisting of monoarylsulfonium salts and trialkylsulfonium salts.

[0058] Examples of the sulfonate ester include structures represented by formula (5) or formula (6). [ka] In formula (5), R 18 and R 19each independently represents a linear, branched or cyclic alkyl group having 1 to 10 carbon atoms which may have a substituent, or an aryl group having 6 to 20 carbon atoms which may have a substituent. Examples of the substituent include a hydroxyl group, a halogen atom, a cyano group, a vinyl group, an acetylene group, and a linear or cyclic alkyl group having 1 to 10 carbon atoms.

[0059] [ka] In formula (6), R 20 represents a monovalent organic group having 1 to 20 carbon atoms. 20 Examples of the monovalent organic group having 1 to 20 carbon atoms that can be taken by include an alkyl group, an aryl group, a perfluoroalkyl group, and a structure represented by the formula (4). [ka] In formula (4), * represents a bond.

[0060] Among the (D) thermal acid generators, it is preferable to contain a thermal acid generator having a sulfonate structure, since this has a high effect of reducing the water absorption of the cured product. Examples of the compound represented by the above formula (5) include methyl methanesulfonate, ethyl methanesulfonate, propyl methanesulfonate, butyl methanesulfonate, phenyl methanesulfonate, methyl ethanesulfonate, ethyl ethanesulfonate, propyl ethanesulfonate, butyl ethanesulfonate, phenyl ethanesulfonate, methyl propanesulfonate, ethyl propanesulfonate, propyl propanesulfonate, butyl propanesulfonate, phenyl propanesulfonate, methyl butanesulfonate, ethyl butanesulfonate, propyl butanesulfonate, butyl butanesulfonate, phenyl butanesulfonate, methyl octanesulfonate, ethyl octanesulfonate, propyl octanesulfonate, butyl octanesulfonate, phenyl octanesulfonate, methyl p-toluenesulfonate, ethyl p-toluenesulfonate, propyl p-toluenesulfonate, butyl p-toluenesulfonate, phenyl p-toluenesulfonate, methoxyphenyl methanesulfonate, Examples of the compound represented by the above formula (6) include "Irgacure" (registered trademark) PAG103 and PAG121 (all trade names, manufactured by BASF Japan Ltd.), PA-411, and PA-480 (all trade names, manufactured by Heraeus K.K.). Other examples of thermal acid generators having a sulfonate structure include PAI-01, PAI-101, PAI-106, PAI-1001, Examples of such compounds include PAI-1002, PAI-1003, and PAI-1004 (all trade names, manufactured by Midori Chemical Co., Ltd.), SP-082, SP-601, SP-606, SP-607, and SP-612 (all trade names, manufactured by ADEKA Corporation), NIT, MIN, ILP-110, ILP-110N, ILP-118, ILP-113, PA-223, and PA-298 (all trade names, manufactured by Heraeus), and NAI-105, NAI-106, and NAI-109 (all trade names, manufactured by Midori Chemical Co., Ltd.).

[0061] Furthermore, it is particularly preferable that the thermal acid generator (D) contains a compound represented by formula (1). In the study by the present inventors, it was found that the water absorption rate is further reduced when the thermal acid generator (D) contains a compound represented by formula (1). Although the reason is unclear, it is speculated that the water absorption rate is reduced because the thermal acid generator (D) contains a compound represented by formula (1), which reduces the volatility of the thermal acid generator (D) during heat treatment, allowing the thermal acid generator (D) to efficiently generate acid during curing, and increases the effect of promoting ring closure into the imide precursor structure and / or oxazole precursor structure. [ka] In formula (1), R 1 R is a divalent to tetravalent group having 1 to 10 carbon atoms. 2 each independently represents an alkyl group having 1 to 10 carbon atoms which may have a substituent, or an aryl group having 6 to 20 carbon atoms which may have a substituent. Examples of the substituent include a hydroxyl group, a halogen atom, a cyano group, a vinyl group, an acetylene group, or a linear or cyclic alkyl group having 1 to 10 carbon atoms. a represents an integer of 2 to 4.

[0062] From the viewpoint of reducing the water absorption rate of the cured product, R 1 is a divalent to tetravalent group having 1 to 6 carbon atoms, R 2 are preferably each independently a linear, branched or cyclic alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 10 carbon atoms which may have a substituent.

[0063] Examples of the compound represented by the above formula (1) include compounds having a plurality of alcoholic hydroxyl groups (sometimes referred to as "polyhydric alcohol compounds") or compounds having a plurality of phenolic hydroxyl groups (sometimes referred to as "polyhydric phenol compounds") in which the alcoholic hydroxyl groups or the phenolic hydroxyl groups are sulfonated with methanesulfonic acid, ethanesulfonic acid, propanesulfonic acid, butanesulfonic acid, octanesulfonic acid, p-toluenesulfonic acid, benzenesulfonic acid, or the like.

[0064] Among the polyhydric alcohol compounds, specific examples of dihydric alcohol compounds include methanediol, ethanediol, propanediol, butanediol, pentanediol, hexanediol, heptanediol, octanediol, nonanediol, and decanediol. Among the polyhydric alcohol compounds, specific examples of trihydric or higher alcohol compounds include propanetriol, butanetriol, pentanetriol, hexanetriol, heptanetriol, octanetriol, nonanetriol, decanetriol, and pentaerythritol. Specific examples of polyhydric phenol compounds include dihydroxybenzene, trihydroxybenzene, and tetrahydroxybenzene.

[0065] From the viewpoint of reducing the water absorption rate of the cured product, the content of the compound represented by formula (1) is preferably 20% by mass or more, more preferably 50% by mass or more, even more preferably 70% by mass or more, and particularly preferably 100% by mass, based on 100% by mass of the thermal acid generator (D).

[0066] The content of the (D) thermal acid generator is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and even more preferably 3 parts by mass or more, per 100 parts by mass of the (A) alkali-soluble resin, from the viewpoint of reducing the water absorption rate of the cured product. Also, the content of the (D) thermal acid generator is preferably 15 parts by mass or less, more preferably 10 parts by mass or less, and even more preferably 8 parts by mass or less, per 100 parts by mass of the (A) alkali-soluble resin, from the viewpoint of imparting high heat resistance to the cured product.

[0067] The photosensitive resin composition of the present invention contains a phenolic resin (E). By containing the phenolic resin (E) in the photosensitive resin composition, the water absorption rate of the cured product can be reduced. Although the reason is unclear, it is speculated that the phenolic resin (E) serves as a reaction site for the thermal crosslinking reaction of the thermal crosslinking agent having an epoxy group (C1) and the thermal crosslinking agent having an oxetanyl group (C2), thereby suppressing the excessive reaction of the alkali-soluble resin (A) with the components (C1) and (C2), and as a result, the ring closure rate of the imide precursor and / or benzoxazole precursor in the heat treatment process is increased.

[0068] The component (E) used in the photosensitive resin composition of the present invention can be synthesized by a known method. The (E) phenolic resin is preferably a novolak resin, polyhydroxystyrene, or polyhydroxystyrene / polystyrene copolymer. Novolak resins include novolak phenolic resins and resol phenolic resins, which are obtained by polycondensing various phenols alone or a mixture of multiple phenols using aldehydes such as formalin by a known method.

[0069] Examples of phenols constituting the novolak phenolic resin and the resol phenolic resin include phenol, p-cresol, m-cresol, o-cresol, 2,3-dimethylphenol, 2,4-dimethylphenol, 2,5-dimethylphenol, 2,6-dimethylphenol, 3,4-dimethylphenol, 3,5-dimethylphenol, 2,3,4-trimethylphenol, 2,3,5-trimethylphenol, 3,4,5-trimethylphenol, 2,4,5-trimethylphenol, methylenebisphenol, methylenebisp-cresol, and the like. Examples of suitable phenols include phenol, resorcin, catechol, 2-methylresorcin, 4-methylresorcin, o-chlorophenol, m-chlorophenol, p-chlorophenol, 2,3-dichlorophenol, m-methoxyphenol, p-methoxyphenol, p-butoxyphenol, o-ethylphenol, m-ethylphenol, p-ethylphenol, 2,3-diethylphenol, 2,5-diethylphenol, p-isopropylphenol, α-naphthol, and β-naphthol. These may be used alone or in combination.

[0070] Examples of aldehydes include formalin, paraformaldehyde, acetaldehyde, benzaldehyde, hydroxybenzaldehyde, and chloroacetaldehyde, and these can be used alone or in combination.

[0071] It is more preferable that the (E) phenol resin contains polyhydroxystyrene and / or polyhydroxystyrene / polystyrene copolymer. Polyhydroxystyrene can be obtained by addition polymerization of a phenol derivative having an unsaturated bond. Examples of phenol derivatives having an unsaturated bond include hydroxystyrene, dihydroxystyrene, allylphenol, coumaric acid, 2'-hydroxychalcone, N-hydroxyphenyl-5-norbornene-2,3-dicarboxylic acid imide, resveratrol, 4-hydroxystilbene, etc., and two or more of these may be used. In addition, it may be a copolymer with a monomer that does not contain a phenolic hydroxyl group, such as styrene. This makes it easier to adjust the alkali dissolution rate.

[0072] From the viewpoint of sensitivity, the content of the (E) phenolic resin is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, relative to 100 parts by mass of the (A) alkali-soluble resin, and from the viewpoint of development adhesion, the content of the (E) phenolic resin is preferably 90 parts by mass or less, more preferably 80 parts by mass or less, and even more preferably 70 parts by mass or less, relative to 100 parts by mass of the (A) alkali-soluble resin.

[0073] The preferred weight average molecular weight of the (E) phenol resin can be determined in terms of polystyrene by gel permeation chromatography (GPC), and from the viewpoint of sensitivity, it is preferably 1,000 or more, more preferably 2,000 or more, and even more preferably 3,000 or more, and from the viewpoint of development adhesion, it is preferably 10,000 or less, more preferably 8,000 or less, and even more preferably 7,000 or less.

[0074] The content of the (E) phenolic resin is preferably in the range of 0.5≦(γ1+γ2) / γ3≦4.0, where γ1 (mass) is the content of the (C1) epoxy group-containing thermal crosslinking agent, γ2 (mass) is the content of the (C2) oxetanyl group-containing thermal crosslinking agent, and γ3 (mass) is the content of the (E) phenolic resin. When the contents of γ1, γ2, and γ3 are in the above range, the water absorption rate of the cured product after heat treatment decreases. More preferably, it is in the range of 0.8≦(γ1+γ2) / γ3≦3.0, and even more preferably, it is in the range of 1.3≦(γ1+γ2) / γ3≦2.0.

[0075] The photosensitive resin composition of the present invention preferably contains an organic solvent, which can turn the composition into a varnish and improve the coatability. The organic solvent may be a polar aprotic solvent such as γ-butyrolactone, an ether such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, tetrahydrofuran, or dioxane, a ketone such as acetone, methyl ethyl ketone, diisobutyl ketone, cyclohexanone, 2-heptanone, 3-heptanone, or diacetone alcohol, an ethylene glycol monomethyl ether acetate, an ethylene glycol monoethyl ether ... Solvents such as ethyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ethyl lactate, ethyl 2-hydroxy-2-methylpropionate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, 3-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, 3-methyl-3-methoxybutyl propionate, ethyl acetate, n-propyl acetate, i-propyl acetate, n-butyl acetate, i-butyl acetate, methyl acetoacetate, ethyl acetoacetate, and other esters, aromatic hydrocarbons such as toluene and xylene, and amides such as N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide can be used alone or in combination.

[0076] The amount of the organic solvent used is not particularly limited, but is preferably 100 to 3000 parts by mass, more preferably 150 to 2000 parts by mass, based on 100 parts by mass of the total amount of the photosensitive resin composition excluding the solvent. The proportion of the solvent having a boiling point of 180° C. or higher to the total amount of the organic solvent is preferably 20% by mass or less, more preferably 10% by mass or less. By keeping the proportion of the solvent having a boiling point of 180° C. or higher to 20% by mass or less, the amount of outgassing from the cured product can be kept low, and as a result, the reliability of the organic EL device can be improved.

[0077] The photosensitive resin composition of the present invention may contain a colorant. The colorant refers to an organic pigment, an inorganic pigment, or a dye. The colorant is preferably an organic pigment and / or an inorganic pigment.

[0078] Examples of organic pigments include diketopyrrolopyrrole pigments, azo pigments such as azo, disazo, or polyazo, phthalocyanine pigments such as copper phthalocyanine, halogenated copper phthalocyanine, or metal-free phthalocyanine, anthraquinone pigments such as aminoanthraquinone, diaminodianthraquinone, anthrapyrimidine, flavanthrone, anthranthrone, indanthrone, pyranthrone, or violanthrone, quinacridone pigments, dioxazine pigments, perinone pigments, perylene pigments, thioindigo pigments, isoindoline pigments, isoindolinone pigments, quinophthalone pigments, threne pigments, benzofuranone pigments, or organometallic complex pigments.

[0079] Examples of inorganic pigments include titanium oxide, zinc oxide, zinc sulfide, white lead, calcium carbonate, precipitated barium sulfate, white carbon, alumina white, kaolin clay, talc, bentonite, black iron oxide, cadmium red, red iron oxide, molybdenum red, molybdate orange, chrome vermilion, yellow lead, cadmium yellow, yellow iron oxide, titanium yellow, chromium oxide, viridian, titanium cobalt green, cobalt green, cobalt chrome green, Victoria green, ultramarine, Prussian blue, cobalt blue, cerulean blue, cobalt silica blue, cobalt zinc silica blue, manganese violet, and cobalt violet.

[0080] Dyes include, for example, azo dyes, anthraquinone dyes, condensed polycyclic aromatic carbonyl dyes, indigoid dyes, carbonium dyes, phthalocyanine dyes, methine or polymethine dyes.

[0081] For the purpose of improving the contrast of an organic EL display device, the color of the colorant is preferably black, which can block visible light over the entire wavelength range, and it is preferable to include at least one selected from organic pigments, inorganic pigments, and dyes in the photosensitive resin composition, and to include a colorant that will exhibit black color when cured. For this purpose, the above-mentioned black organic pigment and black inorganic pigment may be included, or two or more organic pigments and dyes may be mixed to produce a pseudo-black color. When the pseudo-black color is produced, two or more organic pigments and dyes such as red, orange, yellow, purple, blue, and green may be mixed to produce a pseudo-black color. The photosensitive resin composition of the present invention itself does not necessarily have to be black, and a colorant that changes color when cured by heat treatment to produce a black cured product may be used.

[0082] Among these, from the viewpoint of ensuring high heat resistance, it is preferable to contain an organic pigment and / or an inorganic pigment, and a colorant that will be black when cured. Also, from the viewpoint of ensuring high insulation, it is preferable to contain an organic pigment and / or a dye, and a colorant that will be black when cured. That is, from the viewpoint of achieving both high heat resistance and insulation, it is preferable to contain an organic pigment, and a colorant that will be black when cured.

[0083] The content of the colorant is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, based on the total amount of the photosensitive resin composition excluding the solvent, from the viewpoint of obtaining necessary colorability in the cured product. Also, from the viewpoint of obtaining good storage stability, the content is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, based on the total amount of the photosensitive resin composition excluding the solvent.

[0084] When the photosensitive resin composition contains a pigment, it is preferable to contain a dispersant. By containing a dispersant, the pigment can be uniformly and stably dispersed in the resin composition. The dispersant is not particularly limited, but a polymer dispersant is preferable. Examples of the polymer dispersant include polyester-based polymer dispersants, acrylic-based polymer dispersants, polyurethane-based polymer dispersants, polyallylamine-based polymer dispersants, and carbodiimide-based dispersants. More specifically, the polymer dispersant refers to a polymer compound whose main chain is made of polyamino, polyether, polyester, polyurethane, polyacrylate, etc., and whose side chain or main chain end has a polar group such as amine, carboxylic acid, phosphoric acid, amine salt, carboxylate, or phosphate. The polar group is adsorbed to the pigment, and the steric hindrance of the main chain polymer stabilizes the dispersion of the pigment.

[0085] Dispersants are classified into (polymeric) dispersants having only an amine value, (polymeric) dispersants having only an acid value, (polymeric) dispersants having an amine value and an acid value, and (polymeric) dispersants having neither an amine value nor an acid value. Of these, (polymeric) dispersants having both an amine value and an acid value and (polymeric) dispersants having only an amine value are preferred, and (polymeric) dispersants having only an amine value are more preferred.

[0086] The content of the dispersant is preferably 1 part by mass or more, more preferably 3 parts by mass or more, relative to 100 parts by mass of the pigment in order to obtain good dispersion stability, and is preferably 100 parts by mass or less, more preferably 50 parts by mass or less, relative to 100 parts by mass of the pigment in order to maintain the heat resistance of the cured product.

[0087] The photosensitive resin composition of the present invention may contain an adhesion improver. Examples of the adhesion improver include silane coupling agents such as vinyltrimethoxysilane, vinyltriethoxysilane, epoxycyclohexylethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and N-phenyl-3-aminopropyltrimethoxysilane, titanium chelating agents, aluminum chelating agents, and compounds obtained by reacting aromatic amine compounds with alkoxy group-containing silicon compounds. Two or more of these may be contained. By containing these adhesion improvers, the adhesion to the underlying substrate such as silicon wafer, ITO (transparent electrode), SiO2, and silicon nitride can be improved when developing the photosensitive resin film. In addition, the resistance to oxygen plasma and UV ozone treatment used for cleaning can be improved. The content of the adhesion improver is preferably 0.1 to 10 mass% based on the total amount of the photosensitive resin composition excluding the solvent.

[0088] The photosensitive resin composition of the present invention may contain a surfactant for the purpose of improving wettability with the substrate as necessary. Commercially available compounds can be used as the surfactant. Specifically, silicone surfactants include the SH series, SD series, and ST series from Toray Dow Corning Silicone Co., Ltd., the BYK series from BYK Japan Co., Ltd., the KP series from Shin-Etsu Silicone Co., Ltd., the Disform series from Nippon Oil & Fats Co., Ltd., and the TSF series from Toshiba Silicone Co., Ltd.; fluorine surfactants include the "Megafac (registered trademark)" series from Dainippon Ink Mfg. Co., Ltd., the Fluorard series from Sumitomo 3M Co., Ltd., the "Surflon (registered trademark)" series and "Asahi Guard (registered trademark)" series from Asahi Glass Co., Ltd., the EF series from Shin-Akita Kasei Co., Ltd., and the Polyfox series from OmNova Solutions Co., Ltd.; and surfactants consisting of acrylic and / or methacrylic polymers include the Polyflow series from Kyoeisha Chemical Co., Ltd., and the "Disparon (registered trademark)" series from Kusumoto Chemical Co., Ltd., but are not limited thereto. The content of the surfactant is preferably 0.001 to 1% by mass based on the total amount of the photosensitive resin composition excluding the solvent.

[0089] The photosensitive resin composition of the present invention may contain a compound having a phenolic hydroxyl group, which is different from the component (C1), for the purpose of supplementing the alkaline developability of the photosensitive resin composition as necessary. Examples of such compounds having a phenolic hydroxyl group include Bis-Z, BisOC-Z, BisOPP-Z, BisP-CP, Bis26X-Z, BisOTBP-Z, BisOCHP-Z, BisOCR-CP, BisP-MZ, BisP-EZ, Bis26X-CP, BisP-PZ, BisP-IPZ, BisCRIPZ, BisOCP-IPZ, BisOIPP-CP, Bis26X-IPZ, BisOTBP-CP, TekP-4HBPA (TetrakisP-DO-BPA), TrisPHAP, TrisP-PA, TrisP-PHBA, TrisP-SA, TrisOCR-PA, BisOFP -Z, BisRS-2P, BisPG-26X, BisRS-3P, BisOC-OCHP, BisPC-OCHP, Bis25X-OCHP, Bis26X-OCHP, BisOCHP-OC, Bis23 6T-OCHP, Methylene Tris-FR-CR, BisRS-26X, BisRS-OCHP, (all product names manufactured by Honshu Chemical Industry Co., Ltd.), BIR-OC, BIP-PC, BIR-PC, BIR-PTBP, BIR-PCHP, BIP-BIOC-F, 4PC, BIR-BIPC-F, TEP-BIP-A (trade names, manufactured by Asahi Yokuzai Kogyo Co., Ltd.), 1,4-dihydroxynaphthalene, 1,5-dihydroxynaphthalene Examples of the compounds include 1,6-dihydroxynaphthalene, 1,7-dihydroxynaphthalene, 2,3-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, 2,7-dihydroxynaphthalene, 2,4-dihydroxyquinoline, 2,6-dihydroxyquinoline, 2,3-dihydroxyquinoxaline, anthracene-1,2,10-triol, anthracene-1,8,9-triol, and 8-quinolinol. By containing a compound having a phenolic hydroxyl group, the photosensitive resin composition obtained is almost insoluble in an alkaline developer before exposure, and easily dissolves in an alkaline developer after exposure, so that the film loss due to development is small and development is easy in a short time. Therefore, the sensitivity is easily improved. The content of such a compound having a phenolic hydroxyl group is preferably from 1% by mass to 20% by mass based on the total amount of the photosensitive resin composition excluding the solvent.

[0090] The photosensitive resin composition of the present invention may also contain inorganic particles. Preferred examples include, but are not limited to, silicon oxide, titanium oxide, barium titanate, alumina, and talc. The primary particle size of these inorganic particles is preferably 100 nm or less, more preferably 60 nm or less. The content of the inorganic particles is preferably 5 to 90% by mass based on the total amount of the photosensitive resin composition excluding the solvent.

[0091] Next, a method for producing the photosensitive resin composition of the present invention will be described. For example, the photosensitive resin composition can be obtained by dissolving (A) an alkali-soluble resin, (B) a quinone diazide compound, (C) a thermal crosslinking agent, (D) a thermal acid generator, (E) a phenolic resin, and, if necessary, a solvent, an adhesion improver, a surfactant, a colorant, inorganic particles, etc.

[0092] Examples of dissolving methods include stirring and heating. When heating, the heating temperature is preferably set within a range that does not impair the performance of the photosensitive resin composition, and is usually room temperature to 80°C. The order of dissolving each component is not particularly limited, and examples include a method of dissolving compounds in order starting from the least soluble compound. In addition, for components that are prone to generating bubbles when dissolved by stirring, such as surfactants and some adhesion improvers, the components can be added last after dissolving other components, thereby preventing insufficient dissolution of the other components due to the generation of bubbles.

[0093] The obtained photosensitive resin composition is preferably filtered using a filter to remove dust and particles. The filter pore size is, for example, 0.5 μm, 0.2 μm, 0.1 μm, 0.07 μm, 0.05 μm, 0.02 μm, etc., but is not limited thereto. The material of the filter includes polypropylene (PP), polyethylene (PE), nylon (NY), polytetrafluoroethylene (PTFE), etc., and polyethylene and nylon are preferred.

[0094] The cured product of the present invention is a cured product obtained by curing a photosensitive resin composition. The cured product is obtained by heat-treating the photosensitive resin composition. The heat treatment can be performed by a known method such as a method using a hot plate, an oven, or infrared rays. The preferred heat treatment conditions will be described later in the process for producing a cured product (5) for heat-treating the developed photosensitive resin film.

[0095] Next, a method for producing a cured film using the photosensitive resin composition of the present invention will be described in detail. The method for producing the cured product is as follows: (1) applying the photosensitive resin composition of the present invention to a substrate to form a photosensitive resin film; (2) drying the photosensitive resin film; (3) exposing the dried photosensitive resin film through a photomask; (4) developing the exposed photosensitive resin film; and (5) A process of heat treating the developed photosensitive resin film Includes, in this order.

[0096] (1) In the process of applying the photosensitive resin composition of the present invention to a substrate to form a photosensitive resin film, the photosensitive resin composition of the present invention is applied by a spin coating method, a slit coating method, a dip coating method, a spray coating method, a printing method, or the like to obtain a photosensitive resin film of the photosensitive resin composition on the substrate. Prior to application, the substrate to which the photosensitive resin composition is applied may be pretreated with the adhesion improver described above. For example, a method of treating the substrate surface using a solution in which the adhesion improver is dissolved in a solvent such as isopropanol, ethanol, methanol, water, tetrahydrofuran, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, ethyl lactate, or diethyl adipate at 0.5 to 20% by mass can be used. Examples of the method of treating the substrate surface include spin coating, slit die coating, bar coating, dip coating, spray coating, and steam treatment.

[0097] (2) In the process of drying the photosensitive resin film, the applied photosensitive resin film is subjected to a reduced pressure drying process as necessary, and then heat treatment is performed using a hot plate, oven, infrared rays, etc. at a temperature in the range of 50°C to 180°C for one minute to several hours to obtain a dried photosensitive resin film.

[0098] Next, (3) the step of exposing the dried photosensitive resin film through a photomask will be described. The dried photosensitive resin film is irradiated with actinic radiation through a photomask having a desired pattern. Actinic radiation used for exposure includes ultraviolet rays, visible light, electron beams, X-rays, etc., and in the present invention, it is preferable to use i-rays (365 nm), h-rays (405 nm), and g-rays (436 nm) from a mercury lamp. After irradiation with actinic radiation, post-exposure baking may be performed. By performing post-exposure baking, effects such as improved resolution after development or increased tolerance for development conditions can be expected. For post-exposure baking, an oven, a hot plate, infrared rays, a flash annealing device, a laser annealing device, etc. can be used. The post-exposure baking temperature is preferably 50 to 180°C, more preferably 60 to 150°C. The post-exposure baking time is preferably 10 seconds to several hours. When the post-exposure baking time is within the above range, the reaction proceeds well and the development time may be shortened.

[0099] (4) In the process of developing the exposed photosensitive resin film, the exposed photosensitive resin film is developed using a developer to remove areas other than the exposed area. As the developer, an aqueous solution of an alkaline compound such as tetramethylammonium hydroxide, diethanolamine, diethylaminoethanol, sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, triethylamine, diethylamine, methylamine, dimethylamine, dimethylaminoethyl acetate, dimethylaminoethanol, dimethylaminoethyl methacrylate, cyclohexylamine, ethylenediamine, or hexamethylenediamine is preferred. In some cases, polar solvents such as N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethylsulfoxide, γ-butyrolactone, or dimethylacrylamide, alcohols such as methanol, ethanol, or isopropanol, esters such as ethyl lactate or propylene glycol monomethyl ether acetate, or ketones such as cyclopentanone, cyclohexanone, isobutyl ketone, or methyl isobutyl ketone may be added alone or in combination to these alkaline aqueous solutions. The development method may be spray, paddle, immersion, ultrasonic, or the like.

[0100] Next, the pattern formed by development is preferably rinsed with distilled water. Here, too, the rinsing treatment may be performed by adding alcohols such as ethanol and isopropyl alcohol, or esters such as ethyl lactate and propylene glycol monomethyl ether acetate to the distilled water.

[0101] Next, (5) a step of heat-treating the developed photosensitive resin film is performed. Residual solvents and components with low heat resistance can be removed by heat treatment, so that heat resistance and chemical resistance can be improved. The photosensitive resin composition of the present invention contains a polyimide precursor, a polybenzoxazole precursor, and a copolymer thereof, and can form an imide ring and an oxazole ring by heat treatment, so that heat resistance and chemical resistance can be improved. In addition, since the photosensitive resin composition of the present invention contains a thermal crosslinking agent, a thermal crosslinking reaction can be promoted by heat treatment, and heat resistance and chemical resistance can be improved. From the viewpoint of improving the heat resistance of the cured product, the heat treatment temperature is preferably 200°C or more, more preferably 220°C or more, even more preferably 230°C or more, and particularly preferably 240°C or more. On the other hand, from the viewpoint of avoiding the influence of thermal deterioration of the TFT element, it is preferably 400°C or less, more preferably 350°C or less, and even more preferably 320°C or less. Within this temperature range, the temperature may be raised stepwise or continuously. The heat treatment time is preferably 30 minutes or more, more preferably 45 minutes or more, from the viewpoint of improving the heat resistance of the cured product. Also, from the viewpoint of productivity, it is preferably 180 minutes or less, more preferably 120 minutes or less. For example, a method of heat treating at 150°C and 250°C for 60 minutes each, or a method of heat treating while linearly increasing the temperature from room temperature to 250°C over 2 hours can be mentioned.

[0102] The cured product formed by the photosensitive resin composition of the present invention can be used for a display device including a first electrode formed on a substrate and a second electrode provided opposite to the first electrode, specifically, for example, a planarizing layer of a liquid crystal display device, a planarizing layer and / or a pixel dividing layer of an organic EL display device, etc. The following describes an organic EL display device as an example.

[0103] The organic EL display device of the present invention comprises the cured product. Specifically, it is preferable that the organic EL display device has a driving circuit, a planarization layer, a first electrode, a pixel division layer, an organic EL layer (light-emitting layer), and a second electrode on a substrate, and the planarization layer and / or the pixel division layer contains the cured product. For example, an active matrix type display device has a thin film transistor (hereinafter, sometimes referred to as "TFT") as a driving circuit on a substrate such as glass or a resin film, wiring located on the side of the TFT and connected to the TFT, a planarization layer is provided thereon so as to cover the unevenness, and an organic EL layer is further provided on the planarization layer. The organic EL layer and the wiring are connected via a contact hole and a first electrode formed in the planarization layer. In particular, flexible organic EL display devices have become mainstream in recent years, and it is preferable that the organic EL display device has a substrate having the driving circuit described above made of a resin film.

[0104] The organic EL display device of the present invention preferably has at least a bendable portion and / or a portion fixed in a bent state in a cured product. By using a cured product obtained by curing the photosensitive resin composition or photosensitive resin sheet of the present invention, an organic EL display device having excellent bending resistance can be obtained. The curvature radius of the bendable portion and / or the portion fixed in a bent state is preferably 0.1 mm or more, and preferably 5 mm or less. If the curvature radius is 0.1 mm or more, bending resistance at the bent portion can be ensured, and if it is 5 mm or less, design such as narrowing of the frame can be ensured. The organic EL display device of the present invention can be bent at any appropriate portion. For example, the organic EL display device may be bent at the center like a folding display device, or may be bent at the end from the viewpoint of ensuring design and display screen to the maximum. Furthermore, the organic EL display device may be bent along its longitudinal direction or along its lateral direction. It is sufficient that a specific portion of the organic EL display device is bendable (for example, part or all of the four corners can be bent diagonally) depending on the application.

[0105] FIG. 1 shows a cross-sectional view of an example of a TFT substrate in which a planarization layer and a pixel division layer are formed. On a substrate 1, bottom-gate or top-gate TFTs 2 are arranged in a matrix, and a TFT insulating layer 3 is formed to cover the TFTs 2. Furthermore, a wiring 4 connected to the TFTs 2 is provided on the TFT insulating layer 3. Furthermore, a planarization layer 5 is provided on the TFT insulating layer 3 in a state in which the wiring 4 is embedded. The planarization layer 5 is provided with a contact hole 6 that reaches the wiring 4. Then, an ITO (transparent electrode) is formed as a first electrode 7 on the planarization layer 5 in a state in which it is connected to the wiring 4 through the contact hole 6. Here, the first electrode 7 becomes an electrode of a display element (for example, an organic EL element). Then, a pixel division layer 8 is formed to cover the periphery of the first electrode 7. Furthermore, an organic EL layer 9 is formed on the exposed portion of the first electrode 7, and a second electrode 10 is provided to cover the entire substrate. The organic EL element may be a top emission type that emits emitted light from the side opposite to the substrate 1, or a bottom emission type that extracts light from the substrate 1 side. In this manner, an active matrix type organic EL display device is obtained in which a TFT 2 for driving each organic EL element is connected to each organic EL element.

[0106] As described above, the TFT insulating layer 3, the planarizing layer 5 and / or the pixel dividing layer 8 can be formed by the steps of (1) applying the photosensitive resin composition of the present invention to a substrate to form a photosensitive resin film, (2) drying the photosensitive resin film, (3) exposing the dried photosensitive resin film through a photomask, (4) developing the exposed photosensitive resin film, and (5) heat treating the developed photosensitive resin film. An organic EL display device can be obtained by a manufacturing method having these steps.

[0107] The cured product formed by the photosensitive resin composition of the present invention can be used as an insulating film or a protective film constituting an electronic component. Here, examples of electronic components include active components having semiconductors such as transistors, diodes, integrated circuits (hereinafter, ICs), and memories, and passive components such as resistors, capacitors, and inductors. Electronic components using semiconductors are also referred to as semiconductor devices. That is, the semiconductor device of the present invention includes the cured product. Specific examples of the cured product included in the electronic component include passivation films for semiconductors, surface protective films for semiconductor elements and TFTs, interlayer insulating films in multilayer wiring for high-density mounting of 2 to 10 layers, insulating films for touch panel displays, protective films, and the like, but are not limited thereto and can have various structures. The surface of the substrate on which the cured product is formed can be appropriately selected depending on the application and process, and examples of the material include silicon, ceramics, metals, glass, and epoxy resins, and a plurality of these may be arranged on the same surface. Examples of electronic devices having surface protective films or interlayer insulating films on which the cured product of the present invention is arranged include MRAMs with low heat resistance. That is, the cured product of the present invention is suitable for use as a surface protective film for MRAMs. In addition to MRAM, polymer memory (Polymer Ferroelectric RAM: PFRAM) and phase change memory (Phase Change RAM: PCRAM, or Ovonics Unified Memory: OUM), which are promising next-generation memories, are also likely to use new materials with lower heat resistance than conventional memories. Therefore, the cured product of the present invention is also suitable for use as a surface protection film for these memories. It is also suitable for use in fan-out wafer level packages (hereinafter sometimes referred to as "fan-out WLP"). The fan-out WLP is a semiconductor package in which an extension part is provided around a semiconductor chip using a sealing resin such as epoxy resin, rewiring is performed from the electrodes on the semiconductor chip to the extension part, and solder balls are also mounted on the extension part to ensure the required number of terminals. In the fan-out WLP, wiring is installed so as to straddle the boundary formed by the main surface of the semiconductor chip and the main surface of the sealing resin.That is, an interlayer insulating film is formed on a substrate made of two or more materials, namely, a semiconductor chip provided with metal wiring and a sealing resin, and wiring is formed on the interlayer insulating film. In addition, in a type of semiconductor package in which a semiconductor chip is embedded in a recess formed in a glass epoxy resin substrate, wiring is provided so as to straddle the boundary between the main surface of the semiconductor chip and the main surface of the printed circuit board. In this embodiment, an interlayer insulating film is also formed on a substrate made of two or more materials, and wiring is formed on the interlayer insulating film. The cured product obtained by curing the photosensitive resin composition of the present invention has high adhesion to a semiconductor chip provided with metal wiring and also has high adhesion to sealing resin such as epoxy resin, and is therefore suitably used as an interlayer insulating film provided on a substrate made of two or more materials. EXAMPLES

[0108] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. The photosensitive resin compositions in the examples were evaluated by the following methods. (1) Flatness evaluation (surface step) FIG. 2 shows a schematic explanatory diagram of a cross section of a flatness evaluation sample. The photosensitive resin composition obtained in each of the examples and comparative examples described later was applied by spin coating onto a stepped substrate 11 on which five line patterns of 1.2 μm in thickness and 5 μm in width were patterned in parallel at intervals of 5 μm using a coating and developing apparatus (ACT-8 manufactured by Tokyo Electron Co., Ltd.), and baked at 120° C. for 2 minutes to prepare a pre-baked film so that the film thickness of the part not affected by the line pattern on the substrate was about 2.9 μm. The film thickness was measured using Lambda Ace STM-602 manufactured by Dainippon Screen Mfg. Co., Ltd. under the condition of a refractive index of 1.63. Then, using the developing apparatus of the ACT-8, development was performed using a 2.38 mass % tetramethylammonium aqueous solution (manufactured by Tama Chemicals Co., Ltd.) for a time when the film loss during development was 0.5 μm, followed by rinsing with distilled water and shaking off and drying to obtain a developed film with a film thickness of about 2.4 μm. At this time, the thickness of the developed film in the area not affected by the line pattern on the substrate was measured and used as the thickness before the heat treatment. The developed film was then cured (heat-treated) for 60 minutes in a nitrogen atmosphere at 250°C using a high-temperature inert gas oven (INH-9CD-S; manufactured by Koyo Thermo Systems Co., Ltd.) to produce a cured film (cured product 12). The thickness of the cured film in the area not affected by the line pattern on the substrate was measured and used as the thickness after the heat treatment. For the obtained cured film, the surface step generated on the three line patterns excluding the two outermost lines in the area where the line patterns existed was measured using a surface profiler (P·15; KLA Tencol Co., Ltd.), and the average value of the step (height of the cured film represented by h1 to h3 in Figure 2) was used as the surface step (μm). The baseline of each step was defined as the line connecting the points where the film thickness of the recesses on the left and right of each mountain-like resin film part where h1 to h3 are measured is the smallest, as viewed from Figure 2. A specific example is described below. In FIG. 2, the straight line connecting the bottoms a1 and a2 of the step shape is defined as the baseline, and the length from the top b1 of the step shape to the intersection of the line perpendicular to the substrate surface and the baseline is defined as h1.h2 is defined as the length from the top b2 of the step shape to the intersection of a line drawn perpendicular to the substrate surface and the baseline, with the line connecting a2 and a3 as the baseline, and h3 is defined as the length from the top b3 of the step shape to the intersection of a line drawn perpendicular to the substrate surface and the baseline, with the line connecting a3 and a4 as the baseline.

[0109] (2) Cure shrinkage rate In the above flatness evaluation, the film thickness after the heat treatment was calculated relative to the film thickness before the heat treatment, and this was taken as the cure shrinkage rate (%).

[0110] (3) Evaluation of water absorption rate The photosensitive resin composition obtained in each of the examples and comparative examples described later was applied by spin coating on an 8-inch silicon wafer using a coating and developing apparatus ACT-8 (manufactured by Tokyo Electron Co., Ltd.) to obtain a photosensitive resin film, which was then prebaked on a hot plate at 120°C for 2 minutes to produce a prebaked film with a thickness of 6.5 μm. The film thickness was measured using a Lambda Ace STM-602 manufactured by Dainippon Screen Mfg. Co., Ltd. under a condition of a refractive index of 1.63. No exposure step was performed, and then the film was treated using a 2.38 mass% aqueous solution of tetramethylammonium (manufactured by Tama Chemicals Co., Ltd.) using the developing apparatus of the ACT-8 until the film thickness became 6.0 μm, after which it was rinsed with distilled water and spun off and dried to obtain a developed film. The film was cured (heat-treated) for 60 minutes in an oven at 250°C under a nitrogen atmosphere using an inert oven (CLH-21CD-S manufactured by Koyo Thermo Systems Co., Ltd.) to obtain a silicon wafer substrate provided with a cured product. Thereafter, the silicon wafer substrate having the cured product was immersed in 45% by mass hydrofluoric acid for 5 minutes to peel off the cured product from the silicon wafer. The obtained cured product was thoroughly washed with pure water, then dried in a ventilated oven at 80°C for 5 hours, and the dry weight of the cured product was measured using a precision balance immediately after removal from the oven. Thereafter, the cured product was immersed in pure water at 23°C for 24 hours, and immediately after removal from the pure water, the moisture was wiped off, and the water absorption weight of the cured product was measured using a precision balance after 5 minutes. The water absorption rate (wt%) in the cured product was calculated from the dry weight and water absorption weight of the cured product.

[0111] (4) Compounds used in the Examples and Comparative Examples <(A) Alkali-soluble resin> Synthesis of raw material (phenolic hydroxyl group-containing diamine compound) (Synthesis Example 1) 18.3 g (0.05 mol) of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (hereinafter referred to as "BAHF") was dissolved in 100 mL of acetone and 17.4 g (0.3 mol) of propylene oxide, and cooled to -15°C. A solution of 20.4 g (0.11 mol) of 3-nitrobenzoyl chloride dissolved in 100 mL of acetone was added dropwise to the solution. After the addition was completed, the mixture was reacted at -15°C for 4 hours, and then returned to room temperature. The precipitated white solid was filtered and dried in vacuum at 50°C.

[0112] 30 g of the white solid was placed in a 300 mL stainless steel autoclave and dispersed in 250 mL of methyl cellosolve, and 2 g of 5% palladium-carbon was added. Hydrogen was introduced into the mixture using a balloon, and the reduction reaction was carried out at room temperature. After about 2 hours, the reaction was terminated when it was confirmed that the balloon was no longer deflating. After the reaction was completed, the mixture was filtered to remove the palladium compound catalyst, and the mixture was concentrated using a rotary evaporator to obtain a phenolic hydroxyl group-containing diamine compound represented by the following formula. [ka]

[0113] Synthesis of alkali-soluble resin (P1) (Synthesis Example 2) Under a dry nitrogen stream, 0.16 mol of a mixture of dicarboxylic acid derivatives obtained by reacting 41.3 g (0.16 mol) of diphenyl ether-4,4'-dicarboxylic acid with 43.2 g (0.32 mol) of 1-hydroxy-1,2,3-benzotriazole and 73.3 g (0.20 mol) of BAHF were dissolved in 570 g of NMP, and then reacted at 75 ° C for 12 hours. Next, 13.1 g (0.08 mol) of 5-norbornene-2,3-dicarboxylic anhydride dissolved in 70 g of NMP was added, and the mixture was stirred for another 12 hours to terminate the reaction. After filtering the reaction mixture, the reaction mixture was poured into a solution of water / methanol = 3 / 1 (volume ratio) to obtain a white precipitate. This precipitate was collected by filtration, washed three times with water, and then dried in a vacuum dryer at 80 ° C for 24 hours to obtain the desired polybenzoxazole (PBO) precursor (P1).

[0114] Synthesis of alkali-soluble resin (P2) (Synthesis Example 3) Under a dry nitrogen stream, 62.0 g (0.20 mol) of 3,3',4,4'-diphenylethertetracarboxylic dianhydride (hereinafter referred to as "ODPA") was dissolved in 500 g of N-methyl-2-pyrrolidone (hereinafter referred to as "NMP"). 96.7 g (0.16 mol) of the phenolic hydroxyl group-containing diamine compound obtained in Synthesis Example 1 was added together with 100 g of NMP, and the mixture was reacted at 20°C for 1 hour, and then at 50°C for 2 hours. Next, 8.7 g (0.08 mol) of 3-aminophenol was added as a terminal blocking agent together with 50 g of NMP, and the mixture was reacted at 50°C for 2 hours. Then, a solution obtained by diluting 47.7 g (0.40 mol) of N,N-dimethylformamide dimethylacetal with 100 g of NMP was added dropwise over 10 minutes. After the dropwise addition, the mixture was stirred at 50°C for 3 hours. After stirring, the solution was cooled to room temperature and then poured into 5 L of water to obtain a white precipitate. The precipitate was collected by filtration, washed three times with water, and then dried in a vacuum dryer at 80°C for 24 hours to obtain the desired polyimide precursor (P2).

[0115] <(B) Quinone diazide compound> Synthesis of quinone diazide compound 1 (Synthesis Example 4) Under a dry nitrogen stream, 21.22 g (0.05 mol) of TrisP-PA (trade name, manufactured by Honshu Chemical Industry Co., Ltd.) and 36.27 g (0.135 mol) of 5-naphthoquinone diazide sulfonyl chloride were dissolved in 450 g of 1,4-dioxane and brought to room temperature. 15.18 g of triethylamine mixed with 50 g of 1,4-dioxane was added dropwise so that the temperature in the system did not exceed 35°C. After the dropwise addition, the mixture was stirred at 30°C for 2 hours. The triethylamine salt was filtered, and the filtrate was poured into water. The precipitate was then collected by filtration. The precipitate was dried in a vacuum dryer to obtain quinone diazide compound 1 represented by the following formula. [ka]

[0116] <(C1) Thermal crosslinking agent having an epoxy group> TEPIC-VL; "TEPIC" (registered trademark)-VL (an epoxy thermal crosslinking agent containing an isocyanuric ring structure, a compound represented by the following chemical formula, manufactured by Nissan Chemical Industries, Ltd.) [ka] VG3101L; "Techmore" (registered trademark) VG3101L (thermal crosslinking agent having an aromatic ring and an epoxy group, the compound shown in the chemical formula below, manufactured by Printec Co., Ltd.) [ka] BD: "Epogose" (registered trademark) BD (aliphatic epoxy thermal crosslinking agent, compound shown in the chemical formula below, manufactured by Yokkaichi Chemical Co., Ltd.) [ka]

[0117] <(C2) Thermal crosslinking agent having an oxetanyl group> OXT-221 (Oxetanyl thermal crosslinking agent, compound shown in the chemical formula below, manufactured by Toagosei Co., Ltd.) [ka] OXBP: "Ethanacole" (registered trademark) OXBP (aromatic-containing oxetanyl thermal crosslinking agent, compound shown in the chemical formula below, manufactured by Ube Industries, Ltd.) [ka] (n represents an integer of 1 to 3.)

[0118] <(D) Thermal acid generator> BTS: p-Butyl toluenesulfonate (thermal acid generator with sulfonate structure, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) D1: 1,3-propanediol di-p-toluenesulfonate (thermal acid generator satisfying formula (5), Fujifilm Wako Pure Chemical Industries, Ltd.) [ka]

[0119] <(E) Phenolic resin> Synthesis of polyhydroxystyrene resin (E1) (Synthesis Example 5) 105.75g (0.6 mol) of pt-butoxystyrene was added to a mixture of 2400g of tetrahydrofuran and 2.56g (0.04 mol) of sec-butyl lithium as an initiator, and the mixture was polymerized with stirring for 3 hours, after which 12.82g (0.4 mol) of methanol was added to terminate the polymerization. Next, the reaction mixture was poured into 3L of methanol to purify the polymer, and the precipitated polymer was dried. The obtained polymer was dissolved in 1.6L of acetone, 2g of concentrated hydrochloric acid was added at 60°C, and the mixture was stirred for 7 hours, and pt-butoxystyrene was deprotected and converted to hydroxystyrene. After the reaction was completed, the solution was poured into water to precipitate the polymer, and the obtained precipitate was washed three times with water and then dried in a vacuum dryer at 50°C for 24 hours to obtain the desired polyhydroxystyrene (E1). The weight average molecular weight was 4,500.

[0120] Synthesis of novolac resin (E2) (Synthesis Example 6) Under a dry nitrogen stream, 70.2g (0.65 mol) of m-cresol, 37.8g (0.35 mol) of p-cresol, 75.5g of 37% by weight formaldehyde aqueous solution (0.93 mol of formaldehyde), 0.63g (0.005 mol) of oxalic acid dihydrate, and 264g of methyl isobutyl ketone were charged, and then the flask was immersed in an oil bath, and polycondensation reaction was carried out for 4 hours while refluxing the reaction liquid. After that, the temperature of the oil bath was allowed to cool to room temperature over 3 hours, and then the pressure in the flask was reduced to 4-7 kPa, the volatile matter was removed, and the dissolved resin was cooled to room temperature to obtain a novolac resin (E2). The weight average molecular weight was 3,500. <Solvent> ·PGME; Propylene glycol monomethyl ether GBL; gamma-butyrolactone

[0121] Example 1 Under yellow light, 10.0 g of (P1) obtained in Synthesis Example 2 as (A) an alkali-soluble resin, 2.0 g of quinone diazide compound 1 obtained in Synthesis Example 4 as (B) a quinone diazide compound (20 parts by mass relative to 100 parts by mass of (A)), 1.5 g of VG3101L as (C1) a thermal crosslinking agent having an epoxy group (15 parts by mass relative to 100 parts by mass of (A)), 1.0 g of OXBP as (C2) a thermal crosslinking agent having an oxetanyl group (10 parts by mass relative to 100 parts by mass of (A)), and 0.3 g of BTS as (E) a thermal acid generator (3 parts by mass relative to 100 parts by mass of (A)) were weighed out, and these were dissolved in 40.0 g of PGME and 10.0 g of GBL. Thereafter, the obtained solution was filtered through a filter having a pore size of 1 μm to obtain a photosensitive resin composition A. Using the obtained photosensitive resin composition, the above-mentioned evaluations (1) to (3) were carried out.

[0122] Examples 2 to 17, Comparative Examples 1 to 4 Photosensitive resin compositions B to Q and photosensitive resin compositions a to d were obtained in the same manner as in Example 1, with the types and amounts of compounds being as shown in Tables 1-1, 1-2, and 2. The obtained photosensitive resin compositions were used to carry out the above-mentioned evaluations (1) to (3). The compositions and evaluation results of the examples and comparative examples are shown in Tables 1-1, 1-2 and 2.

[0123] [Table 1-1]

[0124] [Table 1-2]

[0125] [Table 2]

[0126] In all of Examples 1 to 17, good results were obtained in terms of flatness and water absorption. In contrast, Comparative Example 1, which did not use the (C1) component, showed poor flatness. In addition, Comparative Example 3, which did not use the (D) thermal acid generator, and Comparative Example 4, which did not use the (E) phenol resin, showed poor water absorption. Furthermore, Comparative Example 2, which did not use the (C2) component, showed poor results in both flatness and water absorption. [Explanation of symbols]

[0127] 1: Substrate 2: TFT 3: TFT insulating layer 4: Wiring 5: Flattening layer 6: Contact hole 7:First electrode 8: Pixel division layer 9: Organic EL layer 10:Second electrode 11: Stepped board 12: Cured product

Claims

1. A photosensitive resin composition comprising: (A) one or more alkali-soluble resins selected from the group consisting of polyimide precursors, polybenzoxazole precursors, and copolymers thereof; (B) a quinone diazide compound; (C) a thermal crosslinking agent; (D) a thermal acid generator; and (E) a phenolic resin, wherein the (C) thermal crosslinking agent comprises (C1) a thermal crosslinking agent having an epoxy group, and (C2) a thermal crosslinking agent having an oxetanyl group.

2. 2. The photosensitive resin composition according to claim 1, wherein the (C1) epoxy group-containing thermal crosslinking agent contains one or more types of thermal crosslinking agents selected from the group consisting of an isocyanuric ring structure-containing epoxy thermal crosslinking agent, an alicyclic epoxy thermal crosslinking agent, and an aliphatic epoxy thermal crosslinking agent.

3. The photosensitive resin composition according to claim 1 or 2, wherein the thermal acid generator (D) contains a thermal acid generator having a sulfonate structure.

4. The photosensitive resin composition according to claim 1 or 2, wherein the thermal acid generator (D) contains a compound represented by formula (1). 【Chemistry 1】 (In formula (1), R 1 is a divalent to tetravalent group having 1 to 10 carbon atoms. 2 each independently represents an alkyl group having 1 to 10 carbon atoms which may have a substituent, or an aryl group having 6 to 20 carbon atoms which may have a substituent. Examples of the substituent include a hydroxyl group, a halogen atom, a cyano group, a vinyl group, an acetylene group, or a linear or cyclic alkyl group having 1 to 10 carbon atoms. a represents an integer of 2 to 4.

5. 3. The photosensitive resin composition according to claim 1, wherein the content of the thermal crosslinking agent having an epoxy group (C1) is γ1 (mass) and the content of the thermal crosslinking agent having an oxetanyl group (C2) is γ2 (mass), and the mass ratio γ2 / γ1 is in the range of 1.1≦γ2 / γ1≦5.

0.

6. The photosensitive resin composition according to claim 1 or 2, wherein the alkali-soluble resin (A) comprises a polybenzoxazole precursor.

7. 3. The photosensitive resin composition according to claim 1, wherein the (E) phenolic resin comprises polyhydroxystyrene and / or a polyhydroxystyrene / polystyrene copolymer.

8. A cured product obtained by curing the photosensitive resin composition according to claim 1 or 2.

9. An organic electroluminescence display device comprising the cured product according to claim 8 .

10. A semiconductor device comprising the cured product according to claim 8.

Citation Information

Patent Citations

  • Display device

    JP2002091343A

  • Photosensitive resin composition, cured film and organic el display device

    JP2022034533A

Cited By

  • Game machine

    JP2024159845A

  • Positive photosensitive resin composition, method for forming insulating resin film, and method for manufacturing semiconductor packaging

    WO2026210768A1