Tube material and manufacturing method of tube material, and stent, guide wire and pressure guide wire
The described method improves the inner wall surface roughness and durability of small-diameter Ni-Ti alloy tubes through controlled manufacturing processes, addressing industrial inefficiencies and ensuring compliance with medical device standards.
Patent Information
- Application Number
- JP2023049844
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2043-03-27
AI Technical Summary
Existing methods for manufacturing small-diameter Ni-Ti alloy tubes face challenges in achieving improved inner wall surface roughness and durability against rotational bending, with conventional processes leading to industrial inefficiencies and suboptimal performance.
A manufacturing method involving melting and casting of Ni-Ti alloy, followed by hot working, drawing with a core, and controlled core removal at specific temperature and load conditions to achieve an inner wall surface arithmetic mean height of 0.55 μm or less, ensuring excellent durability against rotational bending.
The method enables the production of Ni-Ti alloy tubes with enhanced inner wall surface roughness and durability, suitable for medical devices like stents, guidewires, and pressure guidewires, while adhering to ASTM F2063-18 standards for carbon and oxygen concentrations.
Smart Images

Figure 2024139059000001_ABST
Abstract
Description
[Technical Field]
[0001] FIELD OF THE DISCLOSURE The present disclosure relates to tubing and methods of making tubing, as well as stents, guidewires and pressure guidewires. [Background technology]
[0002] Ni-Ti alloy materials have excellent corrosion resistance and wear resistance. They are also known to exhibit shape memory and superelastic properties, meaning they can withstand deformations of 5% or more, which would normally cause residual deformation in metals, and return to their original shape without undergoing plastic deformation. Furthermore, Ni-Ti alloy materials are known to be resistant to repeated deformation under a certain strain.
[0003] In recent years, advances in technology for processing Ni-Ti alloy materials into ultra-fine wires and tubes have led to an expansion in the application of Ni-Ti alloy materials to medical devices such as stents, artificial heart valves, and guidewires used to insert stents and catheters into the body.
[0004] Among medical devices, stents and artificial heart valves are known as indwelling devices that are placed inside the body. Because they are subjected to repeated stresses of contraction and expansion caused by the pulsation of blood vessels and other organs within the body, they are devices with many highly demanding characteristics, and are therefore expected to have excellent fatigue durability over a long period of time, such as over 10 years.
[0005] On the other hand, there has been a significant expansion in the use of disposable devices (hereinafter referred to as "disposable"), which are not indwelling devices but are used for purposes different from the above-mentioned medical devices. Disposable devices are often used to target and remove localized blockages in small blood vessels. In particular, there are many cases where wires or other devices are passed through the inside of the tubing.
[0006] In light of this, tubing is particularly required to have fracture resistance even when it is thin. In addition, when other devices are to be passed through the tubing, the condition of the inner wall of the tubing is important because improved operability is required to allow the devices to be passed through smoothly.
[0007] Furthermore, various studies have been conducted on pipe materials made of Ni-Ti alloys.
[0008] For example, Patent Documents 1 and 2 present inventions based on the idea that improving the roughness of the inner wall surface of a pipe is important. Furthermore, based on these technologies, Non-Patent Documents 1 and 2 have succeeded in obtaining pipes with an outer diameter of 4 mm or less that have a good roughness of the inner wall surface.
[0009] However, to summarize Non-Patent Documents 1 and 2, in order to obtain a thin tube with an outer diameter of 4 mm or less and a good condition of the inner wall surface, fixed plug drawing is performed at the stage of outer diameter 4 mm or more, and mandrel drawing is performed at the stage of outer diameter 4 mm or less. As such, since the combination of different processes is required, it is difficult to industrially manufacture long thin-diameter tube materials.
[0010] Furthermore, Patent Document 1, which uses a core made of a shape memory alloy, produces a pipe material with an inner wall surface of 20s (arithmetic mean roughness Ra of about 5 μm) or less, while Patent Document 2, which uses float plug drawing, a known method for producing long pipe materials, produces a pipe material with an inner wall surface of 5s (arithmetic mean roughness Ra of about 1.25 μm).However, to apply the pipe materials of Patent Documents 1 and 2 to the above-mentioned applications, the roughness of the inner wall surface of the pipe material is too high, and there is room for further improvement.
[0011] Here, we will outline prior art methods for manufacturing pipes made of shape memory alloys. Patent Documents 3 and 4 describe manufacturing methods in which a core made of a shape memory alloy is inserted into a metal pipe and processed into an integrated structure. By inserting a cold-worked core into the metal pipe and heating it, the gap between the metal pipe and the core is minimized, resulting in a composite material in which the metal pipe and the core are integrated. This composite material allows for processing of the metal pipe (pipe material) to the target dimensions, enabling industrial production of pipe materials with controlled outer diameter and wall thickness and high dimensional accuracy. To obtain a pipe material processed to the target dimensions, the core must then be removed from the pipe material. Patent Documents 3 and 4 describe the process of heating the entire processed composite material to 750 to 825°C or by applying electrical current to only the core. The heating removes distortion from the core, and the core is then extracted on a draw bench, where it elongates and reduces its diameter, making it possible to remove the core from the pipe material.
[0012] Furthermore, Patent Documents 5 and 6 describe a method of forming a composite material by inserting a core made of mild steel, carbon steel, stainless steel, brass, or the like into a pipe made of a shape memory alloy, and then processing the composite material as an integrated unit. Patent Documents 5 and 6 describe a method of removing the core by heating the composite material after processing, which causes only the seamless pipe material to expand significantly due to thermal expansion, creating a gap (hereinafter also referred to as clearance) between the pipe material and the core. The creation of this clearance makes it possible to remove the core from the pipe material.
[0013] Although Patent Documents 3 to 6 are effective technologies for manufacturing tubing, there is still room for improvement in the manufacturing of small-diameter tubing of 4 mm or less. In particular, in the core removal process, particularly for small-diameter tubing, the precision of the clearance and whether the tubing and the core are securely separated are important industrial points. For example, if the core is removed from the tubing when the clearance is insufficient or the tubing and the core are not sufficiently separated, a problem has been confirmed in which longitudinal streaks appear on the inner wall surface of the tubing.
[0014] Furthermore, all of the above technologies were developed before 2004. Therefore, there is still room for improvement in the conditions for conformance with ASTM F2063-18 (Standard Specification for Wrought Nickel-Titanium Shape Memory Alloys for Medical Devices and Surgical Implants), which specifies Ni-Ti alloys for medical use. When used in medical devices, the above standard is required for both implantable and disposable devices. In particular, the allowable carbon and oxygen concentrations have both been revised to a maximum of 0.04% by mass, further narrowing the ranges within which carbon and oxygen concentrations can be controlled. Therefore, there is a need to develop technology for manufacturing small-diameter tubing while optimizing manufacturing conditions to control the concentrations of these elements.
[0015] Furthermore, in the conventional technology, when the roughness of the inner wall surface is evaluated, the arithmetic mean roughness Ra is measured linearly along the longitudinal direction of the pipe material, so it is not possible to quantitatively determine the effect of roughness on scratches formed in the longitudinal direction of the pipe material. Therefore, there is room for improvement in the technology for evaluating the roughness of the inner wall surface of pipe material.
[0016] For these reasons, there is a demand for a pipe material made of a Ni-Ti alloy with improved inner wall surface roughness that can be manufactured industrially using an easy method. [Prior art documents] [Patent documents]
[0017] [Patent Document 1] Japanese Patent Application Publication No. 10-17963 [Patent Document 2] Japanese Patent Application Publication No. 11-61301 [Patent Document 3] U.S. Patent No. 5,709,021 [Patent Document 4] U.S. Patent No. 6,799,357 [Patent Document 5] Patent No. 3443206 [Patent Document 6] Patent No. 2133478 [Non-patent literature]
[0018] [Non-Patent Document 1] J. Materials Processing Technology, 118(2001), p.251-255 [Non-patent document 2] J. Materials Processing Technology, 153-154(2004), p.145-150 Summary of the Invention [Problem to be solved by the invention]
[0019] The object of the present disclosure is to provide a tubular material that can be easily manufactured industrially, is made of a Ni-Ti alloy material, has improved inner wall surface roughness, and has excellent durability against rotational bending, a method for manufacturing the same, and a stent, guide wire, and pressure guide wire that use the tubular material. [Means for solving the problem]
[0020] [1] A pipe material made of a Ni-Ti alloy, with an arithmetic mean height Sa of the inner wall surface of 0.55 μm or less. [2] The pipe material according to [1] above, containing 54.5 mass% or more and 57.0 mass% or less of Ni, with the remainder consisting of Ti and unavoidable impurities. [3] The pipe material according to [1] or [2] above, wherein the ratio of the outer diameter to the inner diameter of the pipe material (outer diameter / inner diameter) is 1.01 or more and 2.50 or less. [4] A pipe material according to any one of [1] to [3] above, wherein the outer diameter of the pipe material is 0.15 mm or more and 4.00 mm or less, and the inner diameter of the pipe material is 0.10 mm or more and 3.95 mm or less. [5] A pipe material according to any one of [1] to [4] above, which has superelastic properties at 37°C. [6] A stent formed from the tubular material according to any one of [1] to [5] above. [7] A guidewire formed from the tubular material according to any one of [1] to [5] above. [8] A pressure guidewire formed from the tubular material according to any one of [1] to [5] above. [9] A method for producing a tubular material according to any one of [1] to [5] above, comprising: a melting and casting step (step 1) of a Ni-Ti alloy raw material; a hot working step (step 2); a drawing step (step 3) of drawing a composite material obtained by inserting a core into the tubular hot-worked Ni-Ti alloy material obtained in the hot working step (step 2) to obtain a drawn composite material in which the tubular drawn Ni-Ti alloy material and a drawn core material extending inside the drawn Ni-Ti alloy material are integrated; and a core removal step (step 4) of heating the drawn Ni-Ti alloy material to 150°C or more and 800°C or less while applying a tensile load to the drawn core material in the drawn composite material that is large enough to prevent the drawn Ni-Ti alloy material in the drawn composite material from peeling off from the drawn core material.
[10] The method for manufacturing a pipe material described in [9] above, wherein in the core removal step (step 4), the Ni-Ti alloy drawn material is heated to 150°C or more and 800°C or less while applying a tensile load of 4 MPa or more and 300 MPa or less to the drawn core material in the drawn composite material.
[11] A method for manufacturing a pipe material according to [9] or
[10] above, further comprising a superelasticity imparting heat treatment step (step 5) performed after the core removal step (step 4), in which the pipe material is heated to impart superelasticity. [Effects of the Invention]
[0021] According to the present disclosure, it is possible to provide a tubular material that can be easily manufactured industrially, is made of a Ni-Ti alloy material, has improved inner wall surface roughness, and has excellent durability against rotational bending, a method for manufacturing the same, and stents, guidewires, and pressure guidewires that use the tubular material. [Brief explanation of the drawings]
[0022] [Figure 1] FIG. 1 is a perspective view showing an example of a pipe material according to an embodiment. [Figure 2] FIG. 2 is a cross-sectional view showing an example of the tensile load applying step (step 4-1). [Figure 3] FIG. 3 is a cross-sectional view showing another example of the tensile load applying step (step 4-1). [Figure 4] FIG. 4 is a cross-sectional view showing the state after the annealing step (step 4-2) has been performed on the drawn composite material having the configuration shown in FIG. [Figure 5] FIG. 5 is a cross-sectional view showing the state after the annealing step (step 4-2) has been performed on the drawn composite material having the configuration shown in FIG. [Figure 6] FIG. 6 is a cross-sectional view showing an example of the core diameter reducing step (4-3). [Figure 7] FIG. 7 is a cross-sectional view showing an example of the core extraction step (step 4-4). [Figure 8] FIG. 8 is a schematic diagram showing a double-drive type rotating bending fatigue testing machine used in the examples and comparative examples. [Figure 9] FIG. 9 shows the results of observing the inner wall surface of the pipe material produced in Example 1 using a 3D measuring laser microscope. [Figure 10] FIG. 10 shows the results of observing the inner wall surface of the pipe material produced in Example 10 using a 3D measuring laser microscope. [Figure 11] FIG. 11 shows the results of observing the inner wall surface of the pipe material produced in Comparative Example 6 using a 3D measuring laser microscope. DETAILED DESCRIPTION OF THE INVENTION
[0023] Hereinafter, a detailed description will be given based on an embodiment.
[0024] As a result of extensive research, the present inventors have discovered a manufacturing method that can improve the roughness of the inner wall surface of a pipe material without performing conventional processes such as float plug drawing, fixed plug drawing, and mandrel drawing, which are known to improve the roughness of the inner wall surface of a pipe material, or processes that physically or chemically polish the inner wall surface of the pipe material. Furthermore, they have found that improving the roughness of the inner wall surface of a pipe material can result in excellent durability against rotary bending. The present disclosure has been completed based on this finding.
[0025] The pipe material of the embodiment is made of a Ni—Ti alloy, and the arithmetic mean height Sa of the inner wall surface is 0.55 μm or less.
[0026] Fig. 1 is a perspective view showing an example of a pipe material according to an embodiment. The pipe material 1 shown in Fig. 1 is made of a Ni-Ti alloy, and the arithmetic mean height Sa of the inner wall surface 1a is 0.55 µm or less.
[0027] If the arithmetic mean height Sa of the inner wall surface 1a of the pipe material 1 is 0.55 μm or less, the roughness of the inner wall surface 1a is improved, and the pipe material 1 can have excellent durability against rotary bending. From this perspective, the arithmetic mean height Sa of the inner wall surface 1a of the pipe material 1 is 0.55 μm or less, preferably 0.45 μm or less, and the smaller the better. Furthermore, from the perspective of ease of processing, the lower limit of the arithmetic mean height Sa of the inner wall surface 1a is, for example, 0.08 μm or more.
[0028] The arithmetic mean height Sa is a parameter that extends the calculated average roughness Ra, which is used in general roughness evaluations, to a surface. After cutting the pipe material 1 longitudinally, the inner wall surface 1a of the pipe material 1 is measured using a 3D measuring laser microscope, and the arithmetic mean height Sa of the inner wall surface 1a can be obtained.
[0029] The pipe material 1 made of a Ni-Ti alloy is mainly composed of a matrix (not shown) and a plurality of nonmetallic inclusions (not shown) present in the matrix. The pipe material 1 preferably has superelastic properties.
[0030] Furthermore, to improve workability, the pipe material 1 preferably contains 54.5% to 57.0% by mass of Ni (nickel), with the remainder being Ti (titanium) and unavoidable impurities. Among such alloy compositions, if the C (carbon) content in the pipe material 1 is 0.04% by mass or less and the O (oxygen) content is 0.04% by mass or less, the pipe material 1 satisfies the requirements of ASTM F2063-18, which is specified for medical Ni-Ti alloys, and therefore can be used for medical purposes.
[0031] Ni is an element necessary for Ni-Ti alloys to exhibit superelasticity and shape memory properties. If the Ni content is outside the range of 54.5% by mass to 57.0% by mass, it is difficult to process the alloy into a tubular shape. Therefore, when emphasis is placed on processability, the lower limit of the Ni content is preferably 54.5% by mass or more, more preferably 55.6% by mass or more, and the upper limit is preferably 57.0% by mass or less, more preferably 56.7% by mass or less.
[0032] C is an element that forms nonmetallic inclusions. As the C content increases, the number of nonmetallic inclusions present in the matrix increases, and the proportion of nonmetallic inclusions in the pipe material 1 increases, making the pipe material 1 more susceptible to early fracture (fracture after a small number of rotations). For this reason, the lower the C content, the more preferable. In particular, based on the specifications of ASTM F2063-18, the C content is preferably 0.04 mass% or less.
[0033] O is an element that forms nonmetallic inclusions. If the O content is high, the particle size of the nonmetallic inclusions increases, making the pipe material 1 more susceptible to premature fracture. Therefore, the lower the O content, the more preferable. In particular, based on the standard of ASTM 2063-18, the O content is preferably 0.04 mass% or less.
[0034] Furthermore, in order to adjust the superelasticity and shape memory properties, the pipe material 1 may contain at least one element selected from the group consisting of Cu (copper), Ta (tantalum), Zr (zirconium), Nb (niobium), V (vanadium), Mo (molybdenum), Cr (chromium), Fe (iron), and Co (cobalt) in a total amount of more than 0.00% by mass and not more than 0.05% by mass. These elements are included in the pipe material 1 as needed to adjust the superelasticity and shape memory properties. When the concentration of each of the above elements is 0.05% by mass or less, it does not affect the arithmetic mean height Sa of the inner wall surface 1a of the pipe material 1.
[0035] The remainder of the alloy consists of Ti and unavoidable impurities. "Avoidable impurities" refers to impurities that are inevitably mixed in during the manufacturing process. Since the content of unavoidable impurities can affect the properties of the pipe material, the lower the content of unavoidable impurities, the better. For example, the content of N (nitrogen), an unavoidable impurity, is preferably 0.005% by mass or less.
[0036] The parent phase of the pipe material 1 is an austenite phase made of a Ni-Ti alloy, and has a B2 type crystal structure that has a CsCl type body-centered cubic lattice structure.
[0037] The non-metallic inclusions present in the matrix of the Ni-Ti alloy pipe material 1 are mainly TiC-based inclusions, mainly carbides such as TiC, and Ti4Ni2O x The matrix contains a mixture of non-TiC inclusions, primarily oxynitrides such as Ti4Ni2O, and non-TiC inclusions. When the amount of non-metallic inclusions in the matrix increases, premature fractures originating from the non-metallic inclusions become more likely to occur. Of the non-metallic inclusions in the matrix, the ones that are particularly likely to become the starting point for premature fractures are non-TiC inclusions, especially Ti4Ni2O. x is.
[0038] Furthermore, the ratio of the outer diameter R to the inner diameter r of the tubular material 1 (outer diameter R / inner diameter r) is preferably 1.01 or more and 2.50 or less. When the ratio (outer diameter R / inner diameter r) of the tubular material 1 is within the above range, the tubular material 1 has excellent durability against rotary bending even if it has a small diameter, and furthermore, the tubular material 1 can be suitably used in medical devices.
[0039] It is also preferable that the outer diameter R of the tubular material 1 is 0.15 mm or more and 4.00 mm or less, and the inner diameter r of the tubular material 1 is 0.10 mm or more and 3.95 mm or less. When the outer diameter R and inner diameter r of the tubular material 1 are within the above ranges, the tubular material 1 has excellent durability against rotary bending even if it has a small diameter, and furthermore, the tubular material 1 can be suitably used in medical devices.
[0040] Furthermore, if the tubular material 1 has superelastic properties at 37° C., the tubular material 1 can exhibit superelastic properties in vivo, making the tubular material 1 suitable for use in medical devices.
[0041] Next, a method for manufacturing a pipe material according to an embodiment will be described.
[0042] The method for producing a tubular material according to the present embodiment includes a melting and casting step (step 1) of a Ni-Ti alloy material, a hot working step (step 2), a drawing step (step 3) of drawing a composite material obtained by inserting a core into the tubular Ni-Ti alloy hot-worked material obtained in the hot working step (step 2) to obtain a drawn composite material in which the tubular drawn Ni-Ti alloy material and the drawn core material extending inside the drawn Ni-Ti alloy material are integrated, and a core removal step (step 4) of heating the drawn Ni-Ti alloy material to 150°C or higher and 800°C or lower while applying a tensile load to the drawn core material in the drawn composite material that is large enough to prevent the drawn Ni-Ti alloy material from peeling off from the drawn core material. The tubular material produced by this manufacturing method is the tubular material 1 according to the above embodiment.
[0043] In the melting and casting process (Step 1) for the Ni-Ti alloy material, the Ni-Ti alloy material is melted and then cast to obtain a Ni-Ti alloy ingot. Preferably, the carbon concentration ([C]) and oxygen concentration ([O]) in the Ni-Ti alloy ingot are both adjusted to 0.04 mass% or less.
[0044] In addition, in step 1, when the ([C] / [O]) ratio is 0.5 or more, the Ti4Ni2O ingot obtained in step 1 x Since the generation of is suppressed, fatigue durability, which is particularly required for indwelling devices, can be improved.
[0045] As a method for melting the Ni-Ti alloy material, the Ni-Ti alloy material is melted by high-frequency melting in a vacuum atmosphere or an inert gas atmosphere such as Ar gas.
[0046] The carbon concentration (mass%) is adjusted by weighing the raw material so that the total carbon amount, including the amount of carbon eluted from the crucible used, is a predetermined amount. The oxygen concentration (mass%) is adjusted by selecting and weighing the grade of titanium bare metal so that the oxygen amount is a predetermined amount, based on the fact that the amount of oxygen contained in titanium bare metal varies depending on the grade of titanium bare metal used as the raw material.
[0047] The carbon concentration and oxygen concentration can be measured using a conventionally known carbon concentration analyzer and oxygen concentration analyzer, respectively.
[0048] The hot working step (step 2) carried out after step 1 includes a forging step (step 2-1) and may further include an extrusion step (step 2-2).
[0049] In the forging step (step 2-1), the Ni-Ti alloy ingot obtained in step 1 is forged to obtain a hot-worked Ni-Ti alloy material. The heating temperature during forging of the Ni-Ti alloy ingot is preferably 500°C or higher and 950°C or lower, more preferably 600°C or higher and 800°C or lower. In step 2-1, press forging or air hammer forging can be used.
[0050] Next, the hot-worked Ni-Ti alloy material is drilled with a gun drill and then finish-machined on a lathe to obtain a seamless tubular hot-worked Ni-Ti alloy material.
[0051] Alternatively, an extrusion step (step 2-2) may be performed after the forging step (step 2-1). In the extrusion step (step 2-2), the hot-worked Ni-Ti alloy material obtained in step 2-1 is extruded to obtain a seamless tubular hot-worked Ni-Ti alloy material. The heating temperature during extrusion of the hot-worked Ni-Ti alloy material is preferably 500°C or higher and 950°C or lower, more preferably 600°C or higher and 800°C or lower. Patent Document 5 aims to ensure a high area reduction rate from the viewpoint of emphasizing manufacturing efficiency, and therefore the optimal extrusion temperature is set to 800 to 1000°C. On the other hand, in this embodiment, the control of inclusions (metal structure) is important for tubular materials used in medical devices. Therefore, the heating temperature range during the extrusion is different from that of Patent Document 5, in order to maintain both the carbon concentration ([C]) and oxygen concentration ([O]) controlled in step 1 at 0.04 mass% or lower.
[0052] In the drawing process (process 3) carried out after process 2, a composite material obtained by inserting a core into the tubular Ni—Ti-based alloy hot-worked material obtained in process 2 is subjected to drawing.
[0053] First, a core is inserted into the tubular hot-worked Ni-Ti alloy material obtained in step 2 to produce a composite material with the core inserted inside the tubular hot-worked Ni-Ti alloy material. When inserting the core into the tubular hot-worked material, care must be taken to avoid forming insertion scratches along the longitudinal direction of the hot-worked material on the inner wall surface of the hot-worked material, but the difficulty varies depending on the inner diameter of the hot-worked material. Therefore, if inserting the core is difficult, a lubricant may be applied to the inner wall surface of the hot-worked material and the outer wall surface of the core. Preferred lubricants include phosphate coating, graphite, molybdenum disulfide, and boron nitride.
[0054] The tubular hot-worked material before the core is inserted preferably has an outer diameter of 0.75 mm to 51.00 mm, more preferably 2.50 mm to 10.00 mm, and an inner diameter of 0.50 mm to 9.00 mm. The ratio of the inner diameter to the outer diameter of the hot-worked material is preferably 1.01 to 2.50, more preferably 1.15 to 2.00.
[0055] Here, if the dimensional difference between the outer diameter of the core before insertion into the hot-worked material and the inner diameter of the hot-worked material is set to 2% or more and 25% or less, sufficient clearance can be ensured when inserting the core, making it possible to easily assemble the composite material. Furthermore, if the deformation resistance of the core is set to be approximately the same as the deformation resistance of the hot-worked material, buckling of the inner wall surface of the hot-worked material can be suppressed and the hot-worked material can be processed into a small-diameter tubular material in good condition. In this case, the composite material may be subjected to warm working, as described below, in order to adjust the deformation resistance between the core and the hot-worked material.
[0056] The core is preferably cold-worked before being inserted into the hot-worked material. The inventors have discovered that the roughness of the outer wall surface of the core before insertion is important for the arithmetic mean height Sa of the inner wall surface of the pipe material. Therefore, the arithmetic mean height Sa of the outer wall surface of the core, as measured based on the description in "[3] Arithmetic mean height Sa of the outer wall surface of the core" described below, is preferably 0.03 μm or more and 0.30 μm or less, more preferably 0.03 μm or more and 0.20 μm or less. Regarding the annealing conditions for the core, some of the annealing may be performed in an air atmosphere, but finishing is preferably performed in an inert atmosphere.
[0057] Examples of the material for the core include, but are not limited to, SUS304, SUJ2, SS400, SCM415, SUS316, SUS309S, SUS310S, and Ni (54.5 to 56.0 mass%)-Ti (+unavoidable impurities).
[0058] Next, the composite material is subjected to drawing. By performing drawing, the composite material is drawn to obtain a drawn composite material. The drawn composite material is formed by integrating a tubular Ni-Ti-based alloy drawn material obtained by drawing a tubular Ni-Ti-based alloy hot-worked material, and a drawn core material extending inside the drawn Ni-Ti-based alloy material and having a core drawn.
[0059] Drawing can be cold or warm. Cold working involves drawing the composite without placing it in a temperature-controlled furnace. Warm working involves drawing the composite while controlling its temperature, with the aim of adjusting the deformation resistance between the core and the hot-worked material. The warm working temperature is preferably set to a furnace temperature of 100°C or higher and 800°C or lower. The heating atmosphere can be air, as this does not affect the condition of the inner wall surface of the pipe, but an inert atmosphere is preferred in order to maintain the condition of the outer wall surface of the pipe.
[0060] The processing rate in step 3 is at least 10% and less than 60%.
[0061] The composite may also be subjected to multiple draws through dies of ever decreasing diameter.
[0062] Step 3 provides a drawn composite material having an outer diameter of 0.15 mm or more and 4.00 mm or less.
[0063] In the drawing process (process 3), the composite material may be repeatedly subjected to drawing and annealing. Annealing is performed during or after drawing to remove and recover strain that occurs in the composite material (tubular Ni-Ti alloy wrought material) or the drawn composite material (tubular Ni-Ti alloy drawn material) due to drawing.
[0064] The annealing temperature in step 3 is preferably 500° C. or higher and 800° C. or lower, more preferably 600° C. or higher and 800° C. or lower. The heating atmosphere for annealing may be air since this does not affect the condition of the inner wall surface of the pipe material, but an inert atmosphere is preferred in order to maintain the condition of the outer wall surface of the pipe material.
[0065] The composite material is repeatedly drawn and annealed until it reaches the above dimensions.
[0066] In the core removal step (step 4) performed after step 3, only the drawn core material is removed from the drawn composite material obtained in step 3 to obtain a tube material. The core removal step (step 4) includes a tensile load application step (step 4-1), an annealing step (step 4-2), a core diameter reduction step (step 4-3), and a core extraction step (step 4-4). The core diameter reduction step (step 4-3) is an optional step.
[0067] In the tensile load application step (step 4-1), a tensile load is applied to the drawn core material of the drawn composite material such that the tubular Ni-Ti alloy drawn material in the drawn composite material does not peel off from the drawn core material. The tensile load applied to the drawn core material is preferably 4 MPa or more and 300 MPa or less, more preferably 20 MPa or more and 150 MPa or less.
[0068] FIG. 2 is a cross-sectional view showing an example of the tensile load application step (step 4-1), and FIG. 3 is a cross-sectional view showing another example of the tensile load application step (step 4-1). As shown in FIG. 2, score lines 21 may be made in the circumferential direction at both ends of a tubular Ni-Ti alloy drawn material 20 constituting the drawn composite material 10. The score lines 21, for example, penetrate from the outer wall surface to the inner wall surface of the Ni-Ti alloy drawn material 20. In this configuration, a tensile load is applied to the drawn core material 30 while gripping a portion of the drawn composite material 10 closer to the end than the score lines 21. Alternatively, as shown in FIG. 3, both ends of the drawn Ni-Ti alloy drawn material 20 may be scraped to expose the drawn core material 30 at both ends of the drawn composite material 10. In this configuration, a tensile load is applied to the drawn core material 30 while gripping the drawn core material 30 exposed at both ends of the drawn composite material 10.
[0069] If the tensile load applied to the drawn core material 30 of the drawn composite material 10 is greater than the above range, that is, if a tensile load of a magnitude that causes the Ni-Ti alloy drawn material 20 in the drawn composite material 10 to peel off from the drawn core material 30 is applied, plastic deformation occurs in the Ni-Ti alloy drawn material 20, deteriorating the material properties of the tube material 1, including the arithmetic mean height Sa. As a result, the arithmetic mean height Sa of the inner wall surface 1a of the tube material 1 exceeds 0.55 μm.
[0070] In the annealing step (step 4-2) performed after the tensile load application step (step 4-1), the Ni-Ti alloy drawn material 20 is heated while a tensile load of the above magnitude is being applied to the drawn core material 30 of the drawn composite material 10 in the tensile load application step (step 4-1). The heating temperature is 150°C or higher and 800°C or lower, preferably 450°C or higher and 700°C or lower.
[0071] Fig. 4 is a cross-sectional view showing the state after the annealing step (step 4-2) has been performed on the drawn composite material 10 having the configuration shown in Fig. 2, and Fig. 5 is a cross-sectional view showing the state after the annealing step (step 4-2) has been performed on the drawn composite material 10 having the configuration shown in Fig. 3. As shown in Figs. 4 and 5, by performing the annealing step (step 4-2), the drawn core material 30 is peeled from the drawn composite material 10 due to the difference in thermal expansion between the Ni-Ti alloy drawn material 20 and the drawn core material 30, thereby obtaining a tubular material 1. In the annealing step (step 4-2), the drawn Ni-Ti alloy material 20 expands uniformly due to thermal expansion, so that the occurrence of scratches and other damage on the inner wall surface of the tubular drawn Ni-Ti alloy material 20 resulting from the peeling of the drawn core material 30 from the Ni-Ti alloy drawn material 20 can be suppressed. Furthermore, the annealing step (step 4-2) may be performed to peel off the drawn core material 30 from the drawn composite material 10 to obtain the pipe material 1, and at the same time, to impart superelastic properties to the pipe material 1.
[0072] Furthermore, the core diameter reduction step (step 4-3) may be performed after the annealing step (step 4-2). FIG. 6 is a cross-sectional view showing an example of the core diameter reduction step (step 4-3), illustrating the state in which the core diameter reduction step (step 4-3) has been performed on the configuration of FIG. 4. As shown in FIG. 6, in the core diameter reduction step (step 4-3), a tensile load is applied to the annealed drawn core material 30 that is separated from the tube material 1. The tensile load applied to the drawn core material 30 in the core diameter reduction step (step 4-3) is greater than the tensile load applied to the drawn core material 30 in the tensile load application step (step 4-1). Furthermore, the tensile load in the core diameter reduction step (step 4-3) is not applied to the tube material 1.
[0073] In the core diameter reduction step (step 4-3), a large tensile load is applied only to the drawn core material 30, thereby reducing the diameter of the drawn core material 30. Therefore, compared to the configuration after the annealing step (step 4-2), the clearance between the inner wall surface of the tube material 1 and the outer wall surface of the drawn core material 30 can be increased.
[0074] Fig. 7 is a cross-sectional view showing an example of the core extraction step (step 4-4). As shown in Fig. 7, in the core extraction step (step 4-4), which is performed after the annealing step (step 4-2) or the core diameter reduction step (step 4-3), a drawn core material 30 is extracted from a tube material 1, thereby producing a tube material 1. In the core extraction step (step 4-4), the drawn core material 30 is extracted from the tube material 1 while the inner wall surface 1a of the tube material 1 and the outer wall surface 30a of the drawn core material 30 are completely separated. This prevents scratches and abrasions on the inner wall surface 1a of the tube material 1 caused by the extraction of the drawn core material 30, and therefore makes it possible to produce a tube material 1 having an arithmetic mean height Sa of the inner wall surface 1a within the above range.
[0075] 4 and 6, as shown in Fig. 7, one end of the drawn core material 30 is cut to remove the one end of the drawn core material 30 that is integrated with a part of the drawn Ni-Ti alloy material 20, and then the drawn core material 30 is extracted from the tube material 1. Therefore, when the drawn core material 30 is extracted from the tube material 1, it is possible to prevent the part of the drawn Ni-Ti alloy material 20 adhering to one end of the drawn core material 30 from coming into contact with the inner wall surface 1a of the tube material 1, and therefore it is possible to prevent the inner wall surface 1a of the tube material 1 from being scratched or scratched by the worked material 20.
[0076] Furthermore, when the core diameter reduction step (step 4-3) shown in Fig. 6 is performed, the clearance between the inner wall surface 1a of the tube material 1 and the outer wall surface 30a of the drawn core material 30 can be increased compared to the configuration after the annealing step (step 4-2) shown in Figs. 4 and 5. Therefore, in the core removal step (step 4-4), the occurrence of scratches and scrapes on the inner wall surface 1a of the tube material 1 due to the removal of the drawn core material 30 can be further suppressed. As a result, the arithmetic mean height Sa of the inner wall surface 1a of the tube material 1 can be further reduced.
[0077] In this way, a small-diameter tubular member with a good inner wall surface roughness can be manufactured by the above-mentioned industrially easy method without performing special post-processing steps required in the prior art, such as plug drawing, mandrel processing, inner wall surface polishing, etc. Furthermore, the above-mentioned industrially easy method can easily manufacture a tubular member longer than conventional tubular members, for example, a tubular member with a length of about 10 m to 100 m.
[0078] Furthermore, the manufacturing method of the pipe material of the embodiment may further include a superelasticity imparting heat treatment step (step 5) that is carried out after the core removal step (step 4) and involves subjecting the pipe material 1 to superelasticity imparting heating. The conditions for the superelasticity imparting heating, such as the heating atmosphere and heating temperature of the pipe material 1, are not particularly limited as long as they can impart superelasticity properties to the pipe material 1.
[0079] For example, heating the pipe material at a temperature of 600°C or less in an inert gas atmosphere can reduce the amount of nonmetallic inclusions present in the pipe material made of Ni-Ti alloy. The heating temperature is preferably 450°C or higher and 580°C or lower. Furthermore, applying a tensile load to the pipe material and stretching it straight while performing the superelasticity imparting heat treatment step (step 5) can improve the straightness of the pipe material.
[0080] In addition, in the manufacturing method of the pipe material of the embodiment, additional processing may be performed between the core removal step (step 4) and the superelasticity imparting heat treatment step (step 5), or after the core removal step (step 4) if the superelasticity imparting heat treatment step (step 5) is not performed, for the purpose of fine-tuning the dimensions of the pipe material or as a preliminary processing step to the superelasticity imparting heat treatment step (step 5).
[0081] The total area reduction rate of the pipe material due to additional processing is preferably 10% or more and less than 120%, and more preferably 10% or more and less than 84%. As described in JIS H0500:1998, the total area reduction rate of the pipe material is the ratio of the cross-sectional area reduced by processing to the original cross-sectional area, and is expressed as a percentage (%) ((Ao-A) / Ao x 100%) obtained by dividing the difference between the cross-sectional area Ao of the material before processing and the cross-sectional area A of the material after processing by the cross-sectional area Ao of the material before processing. Here, the cross-sectional area Ao of the pipe material before additional processing and the cross-sectional area A of the pipe material after additional processing are measured, and the total area reduction rate is calculated using the above formula.
[0082] The tubular material of the embodiment can be industrially manufactured by a simple method as described above, has improved inner wall surface roughness, and is highly durable against rotational bending, making it suitable for use as a tubular material for medical devices. Suitable medical devices include stents, guidewires, and pressure guidewires. These stents, guidewires, and pressure guidewires are each formed from the tubular material. Furthermore, because the roughness of the inner wall surface of the tubular material is improved, a form in which another device is inserted into the tubular material and used is expected to be a novel medical device.
[0083] According to the embodiment described above, a pipe material made of Ni-Ti alloy material, having improved inner wall surface roughness and excellent durability against rotary bending can be obtained by a simple method.
[0084] Although the embodiments have been described above, the present invention is not limited to the above embodiments, but includes all aspects encompassed by the concept and scope of the claims of the present disclosure, and can be modified in various ways within the scope of the present disclosure. [Example]
[0085] Next, examples and comparative examples will be described, but the present disclosure is not limited to these examples. The compositions (mass%) of each component shown in Tables 1 and 2 were determined by the RIR (Reference Intensity Ratio) method.
[0086] Example 1 In the melting and casting process (step 1), Ni and Ti alloy materials, which were melted in a high-frequency melting furnace, were poured into a molten metal to obtain a Ni-Ti alloy ingot having the alloy composition shown in Table 1. In the hot-working process (step 2), the ingot was forged at 500°C to 950°C to obtain a Ni-Ti alloy forged material. The forged material was then drilled with a gun drill and finish-machined on a lathe to obtain a seamless, tubular Ni-Ti alloy hot-worked material. In the drawing process (step 3), a core shown in Table 3 was inserted into a tubular workpiece, and a composite material was drawn. Thus, a drawn composite material was obtained, in which the tubular Ni-Ti alloy drawn material and the drawn core material extending inside the drawn Ni-Ti alloy were integrated.
[0087] Next, in the core removal step (step 4), score lines were made in the circumferential direction at both ends of the tubular Ni-Ti alloy drawn material constituting the drawn composite material. Subsequently, a tensile load shown in Table 3 was applied to the drawn core material while holding the end portion of the drawn composite material closer to the score lines. Subsequently, while applying the tensile load shown in Table 3 to the drawn core material, the Ni-Ti alloy drawn material was heated at the annealing temperature shown in Table 3. In this way, superelastic properties were imparted, and the drawn core material was peeled from the drawn composite material to obtain a tube. Subsequently, one end of the drawn core material was cut to remove the end of the drawn core material that was integrated with a part of the drawn Ni-Ti alloy drawn material, and the drawn core material was then extracted from the tube. In this way, tubes with lengths of 10 to 100 m and inner wall surfaces with the sizes, arithmetic mean height Sa, and calculated mean roughness Ra shown in Table 3 were produced.
[0088] Example 2 A pipe material having an inner wall surface with the arithmetic mean height Sa and calculated mean roughness Ra shown in Table 3 was manufactured in the same manner as in Example 1, except that the tensile load and annealing temperature before annealing in the core removal process (process 4) were changed to the values shown in Table 3, and the pipe material was subjected to additional processing with the total area reduction rate shown in Table 3.
[0089] Examples 3 to 8 A pipe material having an inner wall surface having the arithmetic mean height Sa and calculated mean roughness Ra shown in Table 3 was manufactured in the same manner as in Example 1, except that the core shown in Table 3 was used and the tensile load before annealing and the annealing temperature in the core removal process (step 4) were changed to the values shown in Table 3.
[0090] (Examples 9 to 16) A pipe material having an inner wall surface with the arithmetic mean height Sa and calculated mean roughness Ra shown in Table 3 was manufactured in the same manner as in Example 1, except that the core shown in Table 3 was used, the tensile load before annealing and the annealing temperature in the core removal process (process 4) were changed to the values shown in Table 3, and the pipe material was subjected to additional processing with a total area reduction rate shown in Table 3.
[0091] (Comparative Examples 1 to 4) Pipe materials having inner wall surfaces with the arithmetic mean height Sa and calculated mean roughness Ra shown in Table 3 were manufactured in the same manner as in Example 1, except that the cores shown in Table 3 were used and the tensile load before annealing and the annealing temperature in the core removal step (step 4) were changed to the values shown in Table 3. In Comparative Examples 1 and 2, annealing was performed without applying a tensile load before annealing and without applying a tensile load to the drawn core material. In Comparative Example 4, annealing was not performed.
[0092] (Comparative Examples 5 to 13) Pipe materials having inner wall surfaces with the arithmetic mean height Sa and calculated mean roughness Ra shown in Table 3 were manufactured in the same manner as in Example 1, except that the cores shown in Table 3 were used, the tensile load before annealing and the annealing temperature in the core removal step (step 4) were changed to the values shown in Table 3, and the pipe material was subjected to additional processing with a total area reduction rate shown in Table 3. In Comparative Examples 6 to 11, annealing was performed without applying a tensile load before annealing and without applying a tensile load to the drawn core material.
[0093] (Examples 17 to 21) In the drawing process (step 3), the core shown in Table 4 was used, the composite material was repeatedly subjected to drawing and annealing at the temperature shown in Table 4, and the tensile load and annealing temperature before annealing in the core removal process (step 4) were changed to the values shown in Table 4. In the same manner as in Example 1, except for this, a pipe material having an inner wall surface having the arithmetic mean height Sa and calculated mean roughness Ra shown in Table 4 was manufactured.
[0094] Examples 22 to 25 In the drawing process (step 3), the core shown in Table 4 was used, and the composite material was repeatedly subjected to drawing and annealing at the temperature shown in Table 4. The tensile load and annealing temperature before annealing in the core removal process (step 4) were changed to the values shown in Table 4. In addition, the tube material was subjected to additional processing with the total area reduction rate shown in Table 4. In the same manner as in Example 1, a tube material having an inner wall surface with the arithmetic mean height Sa and calculated mean roughness Ra shown in Table 4 was manufactured.
[0095] (Examples 26 to 36) Pipe materials having inner wall surfaces with the sizes, arithmetic mean heights Sa, and calculated mean roughnesses Ra shown in Table 5 were manufactured in the same manner as in Example 1, except that the cores shown in Table 5 were used, the tensile load before annealing and the annealing temperature in the core removal step (step 4) were changed to the values shown in Table 5, and the pipe materials were subjected to additional processing with the total area reduction rates shown in Table 5. Note that in Examples 27 and 31, no additional processing was performed.
[0096] (Examples 37 to 48, Comparative Examples 14 to 15) A pipe material having an inner wall surface with the arithmetic mean height Sa and calculated mean roughness Ra shown in Table 6 was manufactured in the same manner as in Example 1, except that a Ni-Ti alloy ingot having the alloy composition shown in Tables 1 to 2 was used, the core shown in Table 6 was used, the tensile load and annealing temperature before annealing in the core removal process (process 4) were changed to the values shown in Table 6, and the pipe material was subjected to additional processing with the total area reduction rate shown in Table 6.
[0097] (Examples 49 to 58) As shown in Table 7, a pipe material having an inner wall surface with the arithmetic mean height Sa and calculated mean roughness Ra shown in Table 7 was manufactured in the same manner as in Example 1, except that a Ni-Ti alloy ingot having the alloy composition shown in Table 2 was used, and the tensile load before annealing and the annealing temperature in the core removal process (step 4) were changed to the values shown in Table 7.
[0098] [Measurement and Evaluation] The pipe materials obtained in the above Examples and Comparative Examples were subjected to the following measurements and evaluations.
[0099] [1] Arithmetic mean height Sa of the inner wall of the tubular The obtained pipe material was cut at least 100 mm from both ends to obtain a tubular sample, which was then split longitudinally. Four locations on the inner wall surface of the pipe material were then measured using a LEXT OLS5100 3D measuring laser microscope.
[0100] As described in ISO 4288 1996E (JIS B0633:2001), when 0.1 < Ra (μm) < 2.0, the evaluation length (mm) of the roughness curve is specified to be at least 4 mm or more, while no detailed measurement length is specified for the arithmetic mean height Sa. Also, conditions regarding three-dimensional surface properties are described in JIS B0681-2:2018 and JIS B0681-3:2019, but there are no regulations regarding the cut-off of λ c and λ s .
[0101] Therefore, in this measurement, the circumferential direction of the pipe material is taken as the X direction, the longitudinal direction of the pipe is taken as the Y direction, and an image (the connected image has overlapping parts, so the length of the connected image in the Y direction is approximately 592 μm) obtained by connecting 5 fields in the Y direction for a measurement surface (1 field) of 35 μm in the X direction and 125 μm in the Y direction is used for analysis, and the cut-off value of each filter at that time is assumed to be none. A fourth-order removal process for the multi-curve is performed, and after converting the curvature in the X direction to a plane, analysis is carried out to obtain the arithmetic mean height. Then, out of the arithmetic mean heights obtained at the 4 measured locations, the smallest value is taken as the arithmetic mean height Sa of the inner wall surface of the pipe material.
[0102] [2] Arithmetic mean roughness Ra of the inner wall surface of the pipe In the image obtained by measuring the inner wall surface of the pipe material using a 3D measurement laser microscope in the same manner as above, seven-line measurements with an evaluation length of 4 mm or more along the Y direction were performed. Then, out of the arithmetic mean roughnesses obtained at the 4 measured locations, the smallest value is taken as the arithmetic mean roughness Ra of the inner wall surface of the pipe material.
[0103] [3] Arithmetic mean height Sa of the outer wall surface of the core The outer wall surface of the core was measured using a 3D measuring laser microscope in the same manner as above for portions of the core at least 100 mm from both ends and the center portion to obtain the arithmetic mean height. The largest of the arithmetic mean heights measured at the three locations was then rounded up to the nearest 0.05 μm, and the resulting value was used to determine the arithmetic mean height Sa of the outer wall surface of the core. Specifically, values between 0.08 μm and 0.10 μm were considered to be 0.10 μm inclusive, values between 0.11 μm and 0.15 μm inclusive were considered to be 0.15 μm inclusive, values between 0.16 μm and 0.20 μm inclusive were considered to be 0.20 μm inclusive, and values between 0.25 μm and 0.30 μm inclusive were considered to be 0.30 μm inclusive. In Table 1, the values of 0.05 μm for Example 18 and 0.03 μm for Example 19 were too small to be grouped together as 0.05 in accordance with the above, so the largest value was used as the arithmetic mean height Sa of the core outer wall surface.
[0104] [4] Break resistance to 1.0% bending strain To measure durability against rotary bending, a rotary bending test was performed with a bending strain of 1.0% applied to the tube material to measure fracture durability against strain. Specifically, a double-drive rotary bending fatigue testing machine 50 shown in Figure 8 was used to test fracture durability against a bending strain of 1.0% on the tube material 1. The maximum bending strain of 1.0% (strain) applied to the tube material was determined using the following formula (1). The chuck distance C was also determined using the following formula (2). R is the outer diameter of the tube material, and L is the length of the tube material.
[0105] In a double-drive rotating bending fatigue tester 50, silicone oil 54 was circulated by a heater power supply 53 with a heater 51 and an agitator motor having an agitator 52, while the temperature of the silicone oil 54 was maintained at 37°C. Then, a tachometer-equipped motor 55 was used to rotate the tube material 1 at 300 revolutions per minute while applying a bending strain of 1.0% to the tube material 1, and the number of revolutions until the tube material 1 broke (the number of revolutions to break) was measured. However, only in Example 48, which had a high transformation temperature, the temperature of the silicone oil 54 was maintained at 100°C. This measurement was performed on three samples (n = 3), and the lowest number of revolutions to break was taken as the number of revolutions to break. The following rankings were given for the break durability.
[0106] ⊚: The number of times of breakage was 9000 or more. Good: The number of times the sample broke was 7,500 or more but less than 9,000. ×: The number of times to break was less than 7,500.
[0107]
number
[0108]
number
[0109] Normally, because the rotary bending test is affected by the physical state of the sample surface (roughness, voids, defects, etc.), the physical state of the sample surface is made constant by electrolytic polishing. However, in the case of high strain bending of pipe material, it has become clear that the state of electrolytic polishing of the pipe material affects the number of times the pipe material breaks. Therefore, in this study, the arithmetic mean height Sa of the outer wall surface of the pipe material was processed to 0.15 μm or more and 0.25 μm or less before the rotary bending test was conducted.
[0110] [5] Evaluation of pipe material properties For the pipe materials manufactured in Examples 1 to 58, when a 6% strain was applied in a tensile test and then unloaded, or when the pipe materials were heated after unloading, the residual strain was 0.5% or less, and therefore the pipe materials in Examples 1 to 58 had superelastic properties and shape memory properties.
[0111] [6] Oxygen and carbon concentrations The oxygen concentration and carbon concentration contained in the pipe materials produced in Examples 1 to 58 were measured using a carbon concentration analyzer and an oxygen concentration analyzer, and both were found to be 0.04 mass % or less.
[0112] [Table 1]
[0113] [Table 2]
[0114] [Table 3]
[0115] [Table 4]
[0116] [Table 5]
[0117] [Table 6]
[0118] [Table 7]
[0119] Fig. 9 shows the results of observation with a 3D measuring laser microscope of the inner wall surface of the tubing produced in Example 1. Fig. 10 shows the results of observation with a 3D measuring laser microscope of the inner wall surface of the tubing produced in Example 10. Fig. 11 shows the results of observation with a 3D measuring laser microscope of the inner wall surface of the tubing produced in Comparative Example 6.
[0120] As shown in Tables 1 to 7 and Figures 9 to 11, in all examples, the pipe materials manufactured using processes under the specified conditions were made of Ni-Ti alloys and had an arithmetic mean height Sa of the inner wall surface of 0.55 μm or less. Therefore, they had excellent durability against rotary bending. On the other hand, in all comparative examples, the pipe materials manufactured using processes outside the specified conditions had an arithmetic mean height Sa of the inner wall surface of more than 0.55 μm, and therefore had poor durability against rotary bending.
[0121] Specifically, the results of Examples 1 to 16 show that even when the core material used was changed, the arithmetic mean height Sa of the inner wall surface could be controlled to 0.55 μm or less by manufacturing the tube material under specified conditions. The results of Examples 17 to 25 show that even when the core outer wall surface Sa was changed in the drawing process (process 3), the arithmetic mean height Sa of the inner wall surface could be controlled to 0.55 μm or less. Furthermore, even when drawing and annealing were repeatedly performed in the drawing process (process 3), the arithmetic mean height Sa of the inner wall surface could be controlled to 0.55 μm or less. The results of Examples 26 to 36 show that for tube materials with different outer and inner diameters, the arithmetic mean height Sa of the inner wall surface could be controlled to 0.55 μm or less. The results of Examples 37 to 58 show that for tube materials with different alloy compositions, the arithmetic mean height Sa of the inner wall surface could be controlled to 0.55 μm or less.
[0122] In Comparative Examples 1 and 2, a tensile load was not applied before annealing, and annealing was performed without applying a tensile load to the drawn core material. As a result, the drawn core material could not be peeled from the drawn composite material, and as a result, a tube material could not be produced. In Comparative Example 3, a tensile load of a magnitude that caused the tubular Ni-Ti alloy drawn core material to peel from the drawn core material was applied to the drawn composite material. This caused the Ni-Ti alloy drawn core material to undergo plastic deformation, and the tube shape could not be controlled. Therefore, it was determined that a tube material could not be produced. In Comparative Example 4, annealing was not performed while a tensile load was being applied to the drawn core material. Therefore, the drawn core material could not be peeled from the drawn composite material, and as a result, a tube material could not be produced. In Comparative Example 5, the annealing temperature was above 800°C, and therefore non-metallic inclusions were not sufficiently controlled. As a result, the Sa of the inner wall surface of the tube material exceeded 0.55 μm, and the durability to rotary bending was inferior to that of the tube materials of the Examples. In Comparative Examples 6 to 11, depending on the core material, pipe materials could be produced even when annealing was performed without applying a tensile load before annealing and without applying a tensile load to the drawn core material. However, when removing the drawn core material from the pipe material, frictional resistance was felt, which did not occur in the Examples. As a result, the Sa of the inner wall surface of the pipe material exceeded 0.55 μm, and the durability against rotary bending was inferior to that of the pipe material of the Examples. In Comparative Examples 12 and 13, the total area reduction rate of the additional processing on the pipe material was too large, so the Sa of the inner wall surface of the pipe material exceeded 0.55 μm, and the durability against rotary bending was inferior to that of the pipe material of the Examples. In Comparative Example 14, the Ni concentration in the alloy composition was low, so cracks occurred during forging, and subsequent processes could not be performed. In Comparative Example 15, the Ni concentration in the alloy composition was high, so cracks occurred as in Comparative Example 14, and subsequent processes could not be performed. [Explanation of symbols]
[0123] 1 Tube material 1a Inner wall surface of pipe material 10 Drawn composite material 20 Tubular Ni-Ti alloy drawn material 21 Scoreline 30 Drawing core material 30a Outer wall surface of drawn core material 50 Double-drive rotating bending fatigue testing machine 51 Heater 52 Stirring device 53 Heater power supply with motor for stirring device 54 Silicone Oil 55 Motor with tachometer
Claims
1. A pipe material made of a Ni-Ti alloy, the arithmetic mean height Sa of the inner wall surface being 0.55 μm or less.
2. The pipe material according to claim 1, containing 54.5 mass% or more and 57.0 mass% or less of Ni, with the balance being Ti and unavoidable impurities.
3. 2. The pipe material according to claim 1, wherein the ratio of the outer diameter to the inner diameter (outer diameter / inner diameter) of the pipe material is 1.01 or more and 2.50 or less.
4. 2. The tube of claim 1, wherein the outer diameter of the tube is greater than or equal to 0.15 mm and less than or equal to 4.00 mm, and the inner diameter of the tube is greater than or equal to 0.10 mm and less than or equal to 3.95 mm.
5. 10. The tubing of claim 1 having superelastic properties at 37°C.
6. A stent formed from the tubular material according to any one of claims 1 to 5.
7. A guidewire formed from the tubular material according to any one of claims 1 to 5.
8. A pressure guidewire formed from the tubular material according to any one of claims 1 to 5.
9. A method for manufacturing a pipe material according to any one of claims 1 to 5, A melting and casting process (step 1) for a Ni-Ti alloy material; A hot working step (step 2); a drawing process (step 3) for performing drawing on the composite material obtained by inserting a core into the tubular Ni-Ti alloy hot-worked material obtained in the hot working process (step 2) to obtain a drawn composite material in which the tubular Ni-Ti alloy drawn material and the drawn core material extending inside the Ni-Ti alloy drawn material are integrated; A core removal step (step 4) of heating the Ni-Ti alloy drawn material to 150°C or more and 800°C or less while applying a tensile load to the drawn core material in the drawn composite material such that the Ni-Ti alloy drawn material in the drawn composite material is not peeled off from the drawn core material; The method for manufacturing a pipe material comprising the steps of:
10. The method for producing a tube material according to claim 9, wherein in the core removal step (step 4), the Ni-Ti based alloy drawn material is heated to 150°C or more and 800°C or less while applying a tensile load of 4 MPa or more and 300 MPa or less to the drawn core material in the drawn composite material.
11. The method for manufacturing a tube material according to claim 9, further comprising a superelasticity imparting heat treatment step (step 5) performed after the core removal step (step 4) of subjecting the tube material to heating to impart superelasticity (step 5).
Citation Information
Patent Citations
Preparation method of high-precision small-diameter thin-wall nickel-titanium alloy pipe
CN114850219A
High-temperature alloy capillary tube and electric auxiliary preparation method thereof
CN115228955A
Manufacture of seamless pipe having ultra-smooth internal surface
JP1989122608A
Method for manufacturing shape memory alloy tube
JP2001096307A
Metal pipe manufacturing method
JP2005502472A