Method for producing electrode active material for lithium-sulfur battery
The manufacturing method for lithium-sulfur battery electrode active material, involving the deposition of metal sulfides on porous carbon-sulfur composites, addresses the outflow of lithium polysulfide, improving the battery's cycle and discharge capacity.
Patent Information
- Application Number
- JP2023050319
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2043-03-27
AI Technical Summary
Existing lithium-sulfur batteries face challenges in maintaining cycle capacity retention and charge/discharge capacity, particularly in large-scale power equipment and aviation applications, due to the outflow of lithium polysulfide from the porous carbon material.
A method for manufacturing an electrode active material for lithium-sulfur batteries involves mixing a porous carbon material with sulfur and a metal source in a liquid medium, followed by heat-treatment to precipitate and deposit a metal compound and subsequently a metal sulfide on the surface of the composite material, enhancing the retention of lithium polysulfide.
The method improves the cycle characteristics of lithium-sulfur batteries by effectively suppressing the outflow of lithium polysulfide, thereby enhancing the battery's capacity retention and discharge performance.
Smart Images

Figure 2024139403000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing an electrode active material for a lithium-sulfur battery. [Background technology]
[0002] Lithium-sulfur batteries are secondary batteries with high energy density per unit mass, and for example, mesoporous carbon-sulfur composites with sulfur arranged in mesopores are used. Lithium-sulfur batteries are lighter than conventional lithium-ion batteries, and are expected to be used in large power equipment applications such as electric vehicles and aviation applications such as drones. For these applications, improvements in cycle capacity retention and charge / discharge capacity are required.
[0003] In relation to the above, for example, Patent Document 1 proposes a positive electrode material containing iron sulfide that adsorbs lithium polysulfides. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special Publication No. 2021-531228 Summary of the Invention [Problem to be solved by the invention]
[0005] One aspect of the present disclosure aims to provide a method for producing an electrode active material for a lithium-sulfur battery that can form a battery with improved cycle characteristics. [Means for solving the problem]
[0006] The first aspect is a method for producing an electrode active material for a lithium-sulfur battery, the method comprising: mixing a composite material including a porous carbon material and sulfur supported on the porous carbon material, a metal source, and a liquid medium to obtain a first modified composite material having a metal compound derived from the metal source attached thereto; and heat-treating the first modified composite material to obtain a second modified composite material having a metal sulfide attached thereto. The metal source includes at least one specific metal selected from the group consisting of Ti, V, Mn, Fe, Co, Ni, Cu, Zn, Ge, Zr, In, Sn, Nb, Mo, Ta, and W.
[0007] In one embodiment, a method for producing an electrode active material for a lithium-sulfur battery may include heat-treating a mixture containing a composite material including a porous carbon material and sulfur supported on the porous carbon material, a metal source, and a liquid medium under pressure to precipitate a metal compound derived from the metal source on a surface of the composite material to obtain a first modified composite material having the metal compound adhered thereto, and heat-treating the first modified composite material to obtain a second modified composite material having a metal sulfide derived from the metal source adhered thereto.
[0008] In one embodiment, a method for producing an electrode active material for a lithium-sulfur battery may include adjusting a pH of a mixture including a composite material including a porous carbon material and sulfur supported on the porous carbon material, a metal source, and a liquid medium to precipitate a metal compound derived from the metal source on a surface of the composite material to obtain a first modified composite material having the metal compound adhered thereto, and heat-treating the first modified composite material to obtain a second modified composite material having a metal sulfide derived from the metal source adhered thereto.
[0009] In one embodiment, a method for producing an electrode active material for a lithium-sulfur battery may include adding a sulfur source to a mixture including a composite material including a porous carbon material and sulfur supported on the porous carbon material, a metal source, and a liquid medium, thereby precipitating a metal compound derived from the metal source on a surface of the composite material to obtain a first modified composite material having the metal compound attached thereto, and heat-treating the first modified composite material to obtain a second modified composite material having a metal sulfide derived from the metal source attached thereto.
[0010] The second aspect is a positive electrode active material for a lithium-sulfur battery, comprising a composite material containing a porous carbon material and sulfur supported on the porous carbon material, and a metal sulfide containing a specific metal. The positive electrode active material for a lithium-sulfur battery has a ratio of the mass ratio of the specific metal to the total amount of carbon, sulfur, oxygen, nitrogen, and the specific metal in the vicinity of the surface of the positive electrode active material for a lithium-sulfur battery measured by energy dispersive spectroscopy to the mass-based content of the specific metal in the positive electrode active material for a lithium-sulfur battery measured by inductively coupled plasma optical emission spectroscopy of 0.3 or more. The specific metal includes at least one selected from the group consisting of Ti, V, Mn, Fe, Co, Ni, Cu, Zn, Ge, Zr, In, Sn, Nb, Mo, Ta, and W. Effect of the Invention
[0011] According to one aspect of the present disclosure, it is possible to provide a method for producing an electrode active material for a lithium-sulfur battery, which is capable of forming a battery with improved cycle characteristics. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a diagram showing an example of an X-ray diffraction spectrum of the electrode active material according to Example 1. [Diagram 2] FIG. 4 is a diagram showing an example of an X-ray diffraction spectrum of an electrode active material according to Example 2. [Diagram 3] FIG. 10 is a diagram showing an example of an X-ray diffraction spectrum of an electrode active material according to Example 3. [Figure 4] FIG. 10 is a diagram showing an example of an X-ray diffraction spectrum of an electrode active material according to Example 4. [Diagram 5] FIG. 2 is a diagram showing an example of an X-ray diffraction spectrum of an electrode active material according to Comparative Example 1. [Figure 6] FIG. 13 is a diagram showing an example of an X-ray diffraction spectrum of an electrode active material according to Comparative Example 2. [Figure 7] FIG. 2 is a diagram showing an example of a scanning electron microscope image of the electrode active material according to Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] In this specification, the term "step" includes not only an independent step, but also a step that cannot be clearly distinguished from other steps, as long as the intended purpose of the step is achieved. In addition, "the content of each component in the composition means the total amount of the multiple substances present in the composition when multiple substances corresponding to each component are present in the composition, unless otherwise specified. Furthermore, the upper and lower limits of the numerical ranges described in this specification can be arbitrarily selected and combined from the numerical values exemplified as the numerical ranges. Hereinafter, the embodiments of the present invention will be described in detail. However, the embodiments shown below are examples of methods for producing electrode active materials for lithium-sulfur batteries to embody the technical ideas of the present invention, and the present invention is not limited to the methods for producing electrode active materials for lithium-sulfur batteries shown below.
[0014] Method for producing electrode active material for lithium-sulfur battery The method for producing an electrode active material for a lithium-sulfur battery (hereinafter also simply referred to as the "production method") includes a first modification step of mixing a porous carbon material, a composite material containing sulfur supported on the porous carbon material, a metal source, and a liquid medium to obtain a first modified composite material having a metal compound derived from the metal source attached thereto, and a second modification step of heat-treating the first modified composite material to obtain a second modified composite material having a metal sulfide derived from the metal source attached thereto. In addition to the first modification step and the second modification step, the production method may further include other steps as necessary.
[0015] In the presence of a liquid medium, a metal compound containing a metal derived from a metal source is precipitated on the surface of a composite material containing a porous carbon material carrying sulfur, thereby obtaining a first modified composite material, which is a composite material having a metal compound uniformly attached to the surface. The obtained first modified composite material is heat-treated to obtain a second modified composite material having a metal sulfide derived from a metal source uniformly attached to the surface of the composite material. The metal sulfide disposed on the surface can suppress the outflow of lithium polysulfide generated during discharge of the lithium-sulfur battery from the porous carbon material. This improves the cycle characteristics of the lithium-sulfur battery. This can be considered to be due to the fact that the metal sulfide present on the surface of the composite material can suppress the passage of the electrolyte while allowing lithium ions to pass through.
[0016] In the first modification step, a composite material, a metal source, and a liquid medium are mixed to obtain a mixture, and a first modified composite material is obtained in which a metal compound derived from the metal source is precipitated on the surface of the composite material. The composite material used in the preparation of the mixture may be purchased and prepared, or a desired composite material may be prepared by preparing it by a conventional method. The composite material can be prepared, for example, by heat-treating a mixture of a porous carbon material and sulfur.
[0017] The porous carbon material used in the preparation of the composite material may have a shape of a sphere or the like. It may also be a sphere formed by agglomeration of fibrous carbon such as carbon nanotubes. The porous carbon material may have a volume average particle size of, for example, 0.5 μm or more and 50 μm or less, 1 μm or more, or 2 μm or more, and 40 μm or less, or 30 μm or less. When the volume average particle size of the porous carbon material is within the above range, an electrode with less coating unevenness tends to be produced. The volume average particle size (D50) of the porous carbon material is measured as a particle size corresponding to 50% of the cumulative volume from the small diameter side in the volume-based particle size distribution. The volume-based particle size distribution is measured by a laser diffraction particle size distribution measuring device.
[0018] The aspect ratio (major axis / minor axis) of the porous carbon material may be, for example, 1 or more and 3 or less. The major axis and minor axis of the porous carbon material are measured by a method of calculating the length of the major axis and minor axis from an image obtained from an optical microscope, an electron microscope, or the like, or by using an image-type particle size distribution measuring device. Specifically, for example, the volume average particle size D50 is measured with a laser diffraction type particle size distribution measuring device, and 30 to 50 porous carbon material particles having a particle size, which is the arithmetic average value of the major axis and minor axis measured from a scanning electron microscope (SEM) image, are arbitrarily selected, and the aspect ratio of each particle is calculated, and the aspect ratio of the porous carbon material is calculated as the arithmetic average value thereof. The aspect ratio is calculated according to the Japanese Industrial Standards (JIS Z8900-1:2008), by measuring the maximum major axis and the minor axis, which is the width perpendicular to the maximum major axis, and determining the ratio of the major axis to the minor axis, and the arithmetic average value is taken as the aspect ratio. For example, automated analysis can be performed using software such as Image J.
[0019] The peak pore diameter of the porous carbon material may be, for example, 0.5 nm or more and 10 nm or less, 1.5 nm or more, 2.0 nm or more, or 2.5 nm or more, and may be 8 nm or less, 6 nm or less, or 4 nm or less. When the peak pore diameter of the porous carbon material is within the above range, the reaction between the metal source and sulfur tends to be appropriately suppressed, and the decrease in the charge / discharge capacity of the lithium-sulfur battery tends to be more effectively suppressed. Here, the peak pore diameter means the pore diameter showing the maximum peak in the pore distribution curve obtained by the quenched solid density functional theory (QSDFT method) from the nitrogen adsorption isotherm obtained by nitrogen gas adsorption / desorption measurement.
[0020] Porous carbon materials have a specific surface area of, for example, 1000 m 2 / g or more, preferably 1500m 2 / g or more, 2000m 2 / g or more, or 2500m 2 / g or more. The specific surface area may be, for example, 3500 m 2 / g or less, or 3300m 2The specific surface area of the porous carbon material may be 1 / g or less. The specific surface area of the porous carbon material is measured by a BET method based on the Brunauer Emmett Teller (BET) theory. Specifically, for example, it is measured by a multipoint method using nitrogen gas.
[0021] The pore volume of the porous carbon material may be, for example, 0.8 ml / g or more and 4 ml / g or less, 1.0 ml / g or more, or 1.2 ml / g or more, and 3 ml / g or less, 2.5 ml / g or less, or 2.3 ml / g or less. In particular, it is preferable that the pore volume of pores having a diameter of 0.5 nm or more and 4.0 nm or less is within the above range. When the pore volume of the porous carbon material is within the above range, a large amount of sulfur can be packed into the pores of the porous carbon material, which tends to increase the energy density of the lithium-sulfur battery. The pore volume of the porous carbon material is measured, for example, by nitrogen gas adsorption / desorption measurement.
[0022] The carbon content in the porous carbon material may be, for example, 80% by mass or more, preferably 90% by mass or more, or 95% by mass or more, and may be substantially composed of carbon alone. Here, "substantially" does not mean to exclude other elements that are inevitably mixed in.
[0023] Specific examples of the porous carbon material include carbon nanotubes, graphene, and carbon materials obtained by carbonizing and activating resins, petroleum pitch, or compounds made from plants. The porous carbon material may contain at least activated carbon. One type of porous carbon material may be used alone, or two or more types may be used in combination.
[0024] The composite material includes sulfur supported on a porous carbon material. At least a part of the sulfur may be disposed in the pores of the porous carbon material, or may be disposed on the surface of the porous carbon material. The purity of the sulfur supported on the porous carbon material may be, for example, 50% by mass or more, 90% by mass or more, or 100% by mass or less.
[0025] By using a porous carbon material having sulfur disposed on the surface as a composite material, metal sulfide is more uniformly disposed on the surface of the composite material, and the outflow of lithium polysulfide generated during discharge from the porous carbon material can be more effectively suppressed.
[0026] The sulfur content in the composite material may be, for example, 100% by mass or more and 500% by mass or less, or 150% by mass or more, or 200% by mass or more, relative to the porous carbon material.
[0027] The composite material can be prepared by heat-treating a mixture containing a porous carbon material and sulfur. In addition to the porous carbon material and sulfur, the mixture may further contain compounds containing phosphorus, boron, nitrogen, etc., transition metals, polymer compounds, etc. as necessary. The heat treatment of the mixture can be performed, for example, in a sealed container at a heat treatment temperature of 100°C or more and 450°C or less. The heat treatment temperature may be 100°C or more or 400°C or less. The pressure during the heat treatment may be atmospheric pressure or more and may be 15 MPa or less as a gauge pressure. The heat treatment time may be, for example, 1 hour or more and 72 hours or less, or 1.5 hours or more, or 36 hours or less.
[0028] The content of the composite material in the mixture containing the composite material, the metal source, and the liquid medium in the first modification step may be, for example, 1% by mass or more and 70% by mass or less, 5% by mass or more, 7% by mass or more, or 10% by mass or more, and 50% by mass or less, or 40% by mass or less, based on the total mass of the mixture. If the content of the composite material is within the above range, the wet dispersion treatment can be performed more efficiently.
[0029] The metal contained in the metal source constituting the mixture may include at least one specific metal selected from the group consisting of titanium (Ti), vanadium (V), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), germanium (Ge), zirconium (Zr), indium (In), tin (Sn), niobium (Nb), molybdenum (Mo), tantalum (Ta) and tungsten (W), and may include at least Zn. It is considered that the specific metal reacts with sulfur to form a metal sulfide that is permeable to lithium ions but not permeable to the electrolyte. The metal source may include a simple substance of the specific metal, an alloy, a compound containing the specific metal, and the like. Examples of the compound containing the specific metal include metal salts such as sulfates, nitrates, oxalates, phosphates, and borates, oxides, nitrides, carbides, borides, sulfides, phosphides, composite oxides, composite oxynitrides, and the like. The purity of the compound containing the specific metal used as the metal source may be, for example, 30% by mass or more, 60% by mass or more, or 90% by mass or more. The purity of the compound containing the specific metal may be, for example, less than 100% by mass.
[0030] The metal source may be a substance soluble in the liquid medium described below. By using a metal source soluble in the liquid medium, a modified composite material can be obtained more efficiently. Here, soluble in the liquid medium means that the solubility in 100 g of the liquid medium at room temperature (e.g., 25°C) or the temperature of the heat treatment is 0.01 g or more. The solubility may be 0.02 g or more.
[0031] The content of the metal source in the mixture containing the composite material, the metal source, and the liquid medium may be, for example, 0.1 mass % or more and 50 mass % or less, 1 mass % or more, 1.5 mass % or more, 2 mass % or more, or 3 mass % or more, and 30 mass % or less, 20 mass % or less, 10 mass % or less, or 5 mass % or less, based on the total mass of the mixture. When the content of the metal source is within the above range, the metal source can be added homogeneously to the composite material.
[0032] The mixture may have a mass ratio of the metal source content to the composite material content of, for example, 0.1 mass% or more and 20 mass% or less, 0.5 mass% or more, 1 mass% or more, or 15 mass% or less. When the mass ratio of the metal source to the composite material is within the above range, it tends to be possible to produce a positive electrode material for a lithium-sulfur battery while suppressing a decrease in the energy density of the lithium-sulfur battery.
[0033] The liquid medium constituting the mixture containing the composite material, the metal source, and the liquid medium may be a substance capable of dissolving at least a part of the metal source, and may contain at least water. When the liquid medium contains water, the water content in the liquid medium may be 20 mass% or more, 40 mass% or more, or 60 mass% or more, based on the total mass of the liquid medium. The water content in the liquid medium may be 100 mass% or less, or less than 100 mass%. The liquid medium may contain a liquid medium other than water. Examples of liquid media other than water include water-soluble organic solvents such as ethanol.
[0034] The content of the liquid medium in the mixture containing the composite material, the metal source, and the liquid medium may be, for example, 10% by mass or more and 99% by mass or less, 20% by mass or more, or 30% by mass or more, and 95% by mass or less, or 90% by mass or less, based on the total mass of the mixture. If the content of the liquid medium is within the above range, the wet dispersion treatment can be performed more efficiently.
[0035] The pH of the mixture containing the composite material, the metal source, and the liquid medium may be, for example, 1 to 14, preferably 1.5 or more or 2 or more, and preferably 13.5 or less, 7 or less, or 5 or less. The pH of the mixture may be set depending on the type of the metal source.
[0036] The mixture is obtained by mixing the composite material, the metal source, and the liquid medium. The mixing method for obtaining the mixture may be appropriately selected from commonly used wet dispersion processing methods. Specific examples include a method using a propeller type agitator, a method using beads, and a method using a homogenizer. The temperature during mixing may be, for example, 0°C or higher and 100°C or lower. The mixing time may be, for example, 1 minute or higher and 72 hours or lower.
[0037] In the first modification step, a first modified composite material is obtained in which a metal compound derived from a metal source is precipitated on the surface. Examples of the precipitated metal compound include metal oxides, metal hydroxides, metal sulfides, metal phosphates, and metal borates. Methods for precipitating the metal compound include heat treatment of the mixture, adjusting the pH of the liquid medium constituting the mixture, removing the liquid medium from the mixture, and adjusting the ion concentration of the ions constituting the precipitated metal compound.
[0038] In one embodiment, the manufacturing method may be a first manufacturing method in which the first modification step includes a first heat treatment step of heat-treating the mixture. In the first heat treatment step, the resulting mixture may be heat-treated in a sealed and pressurized state. This allows a first modified composite material to be obtained. By reacting the sulfur contained in the composite material with the metal source in the presence of a liquid medium, a deposit containing, for example, a metal sulfide is precipitated on the surface of the composite material to form the first modified composite material. In addition, by precipitating the metal sulfide in the liquid medium, the metal sulfide can be precipitated uniformly on the surface of the composite material.
[0039] The first heat treatment step may be performed under a sealed condition. Specifically, the mixture may be heated in a pressure-resistant sealed container. The pressurization condition in the first heat treatment step may be the vapor pressure of the liquid medium in the first heat treatment step. For example, when the liquid medium is water and the temperature in the first heat treatment step is 230°C, the absolute pressure is 2.8 MPa. The pressurization condition may be, for example, 2.0 MPa or more and 15 MPa or less, 4.7 MPa or more, or 7.4 MPa or less.
[0040] The temperature of the first heat treatment step may be, for example, a temperature equal to or higher than the boiling point of the liquid medium. The first heat treatment step may include a temperature increase step in which the mixture is heated to a predetermined temperature, and a maintenance step in which the predetermined temperature is maintained for a predetermined time. The temperature increase rate in the temperature increase step may be adjusted so that the maximum temperature during the temperature increase does not exceed the target temperature, and may be, for example, 1°C / min to 20°C / min. The predetermined heat treatment temperature in the first heat treatment step may be, for example, 120°C to 300°C, 150°C to 200°C, and 270°C or less, or 250°C or less. The predetermined time in the maintenance step may be, for example, 30 minutes or more, 1 hour or more, or 3 hours or more. The predetermined time in the maintenance step may be, for example, 72 hours or less, 48 hours or less, or 24 hours or less. The predetermined heat treatment time in the maintenance step is set to the time when the temperature set in the above-mentioned temperature range is reached, and the time when the operation for lowering the temperature is performed is set to the time.
[0041] The atmosphere in the first heat treatment step may be, for example, any of an air atmosphere, a nitrogen atmosphere, an argon atmosphere, and the like.
[0042] The first heat treatment step may include a cooling step of lowering the temperature of the dispersion liquid containing the obtained first modified composite material following the above-mentioned maintaining step. The cooling step starts when an operation for lowering the temperature is performed and ends when the temperature is lowered to 50° C. or less. The temperature lowering rate may be, for example, 1° C. / min or more and 10° C. / min or less.
[0043] The first manufacturing method may further include a separation step of separating the obtained first modified composite material from the mixture, and may further include a purification step as necessary. In the separation step, for example, the mixture containing the first modified composite material may be subjected to solid-liquid separation to extract the first modified composite material. In the purification step, the first modified composite material may be washed with pure water or the like. The extracted first modified composite material may be dried, for example, by heat drying, vacuum degassing, natural drying, or a combination thereof.
[0044] The first manufacturing method includes a second modification step of heat-treating the first modified composite material to obtain a second modified composite material having a metal sulfide derived from a metal source attached thereto. In the second modification step, the first modified composite material, which is a composite material having a metal sulfide attached thereto, is re-heat-treated to obtain a second modified composite material having a more stable sulfur state, the second modified composite material having a metal sulfide attached to its surface. The metal sulfide contained in the second modified composite material may be a metal sulfide containing a specific metal, and may contain at least zinc sulfide. The heat treatment in the second modification step of the first manufacturing method may include removing at least a portion of the liquid medium attached to the first modified composite material to obtain a dried product.
[0045] The heat treatment in the second modification step of the first manufacturing method may include a temperature increase step in which the first modified composite material is heated to a predetermined temperature, and a maintenance step in which the predetermined temperature is maintained for a predetermined time. The temperature increase rate in the temperature increase step may be, for example, 1°C / min or more and 20°C / min or less. The predetermined heat treatment temperature in the heat treatment may be, for example, 100°C or more and 450°C or less, 120°C or more, or 150°C or more, and 430°C or less, or 400°C or less. The predetermined time in the maintenance step may be, for example, 30 minutes or more, 1 hour or more, or 3 hours or more. The predetermined time in the maintenance step may be, for example, 72 hours or less, 48 hours or less, or 24 hours or less. The predetermined heat treatment time in the maintenance step is set to start when the temperature set in the above-mentioned temperature range is reached, and end when the operation for lowering the temperature is performed. The atmosphere of the heat treatment may be, for example, any of air atmosphere, nitrogen atmosphere, argon atmosphere, etc.
[0046] The heat treatment in the second modification step may include a cooling step of lowering the temperature of the first modified composite material following the above-mentioned maintaining step. The cooling step starts when an operation for lowering the temperature is performed and ends when the temperature is lowered to 50° C. or less. The temperature lowering rate may be, for example, 1° C. / min or more and 10° C. / min or less.
[0047] In one embodiment, the production method may be a second production method in which the first modification step includes a pH adjustment step of adjusting the pH of the liquid medium constituting the mixture. By adjusting the pH of the liquid medium, the metal compound with reduced solubility is precipitated on the surface of the composite material, and a first modified composite material is obtained, which is a composite material with the metal compound attached to the surface. By precipitating the metal compound in the liquid medium, the metal compound can be uniformly precipitated on the surface of the composite material. Examples of the metal compound precipitated in the pH adjustment step include metal hydroxides, metal oxides, metal sulfides, metal phosphates, metal borates, etc., and may include at least one selected from the group consisting of these.
[0048] In the pH adjustment step, it is sufficient if a metal compound containing a metal derived from a metal source can be precipitated by adjusting the pH of the liquid medium. Specifically, for example, a basic compound or an acidic compound may be added to the mixture to adjust the pH of the liquid medium. Examples of basic compounds used for pH adjustment include hydroxide salts such as hydroxides of alkali metals and hydroxides of alkaline earth metals, and aqueous ammonia solutions. Examples of acidic compounds include nitric acid, sulfuric acid, phosphoric acid, and boric acid. The adjustment range of the pH in the pH adjustment step may be, for example, 2 to 14, and preferably 2.5 or more, or 13.5 or less. In the pH adjustment step, for example, the pH of the liquid medium may be increased, and preferably increased by 1 or more, or 2 or more. The increase range of the pH may be 12 or less. In the pH adjustment step, for example, the pH of the liquid medium may be decreased, and preferably decreased by 1 or more, or 2 or more. The decrease range of the pH may be 14 or less.
[0049] After adjusting the pH of the liquid medium, a precipitation step of precipitating the metal compound may be included. In the precipitation step, the metal compound may be precipitated while stirring the mixture, or may be precipitated in a stationary state. The temperature in the precipitation step may be, for example, 0°C or higher and 100°C or lower, and preferably 10°C or higher or 90°C or lower. The precipitation time in the precipitation step may be, for example, 1 minute or higher and 72 hours or lower, and preferably 5 minutes or higher or 48 hours or lower.
[0050] The second manufacturing method may further include a separation step of separating the obtained first modified composite material from the mixture, and may further include a purification step as necessary. In the separation step, for example, the mixture containing the first modified composite material may be subjected to solid-liquid separation to extract the first modified composite material. In the purification step, the first modified composite material may be washed with pure water or the like. The extracted first modified composite material may be dried, for example, by heat drying, vacuum degassing, natural drying, or a combination thereof.
[0051] The second manufacturing method includes a second modification step of heat-treating the first modified composite material to obtain a second modified composite material to which a metal sulfide derived from a metal source is attached. In the second modification step, the first modified composite material, which is a composite material to which a metal compound is attached, is heat-treated, so that, for example, the metal compound reacts with sulfur contained in the composite material to generate a metal sulfide, and a second modified composite material, which is a composite material to which the metal sulfide is attached, is obtained. The metal sulfide contained in the second modified composite material may be a metal sulfide containing a specific metal, and may contain at least zinc sulfide. The heat treatment in the second modification step of the second manufacturing method may include removing at least a part of the liquid medium attached to the first modified composite material to obtain a dried product.
[0052] The heat treatment in the second modification step of the second manufacturing method may include a temperature increase step in which the first modified composite material is heated to a predetermined temperature, and a maintenance step in which the predetermined temperature is maintained for a predetermined time. The temperature increase rate in the temperature increase step may be, for example, 1°C / min or more and 20°C / min or less. The predetermined heat treatment temperature in the heat treatment may be, for example, 50°C or more and 450°C or less, 100°C or more, or 150°C or more, and 400°C or less, or 350°C or less. The predetermined time in the maintenance step may be, for example, 30 minutes or more, 1 hour or more, or 3 hours or more. The predetermined time in the maintenance step may be, for example, 72 hours or less, 48 hours or less, or 24 hours or less. The predetermined heat treatment time in the maintenance step is set to the time when the temperature set in the above-mentioned temperature range is reached, and the time when the operation for lowering the temperature is performed is set to the time. The atmosphere of the heat treatment may be, for example, any of an air atmosphere, a nitrogen atmosphere, an argon atmosphere, etc.
[0053] The heat treatment in the second modification step may include a cooling step of lowering the temperature of the first modified composite material following the above-mentioned maintaining step. The cooling step starts when an operation for lowering the temperature is performed and ends when the temperature is lowered to 50° C. or less. The temperature lowering rate may be, for example, 1° C. / min or more and 10° C. / min or less.
[0054] In one embodiment, the production method may be a third production method in which the first modification step includes a sulfur source addition step of adding a sulfur source to the mixture. By adding a sulfur source to the mixture, a metal compound with reduced solubility is precipitated on the surface of the composite material, and a first modified composite material is obtained, which is a composite material having a metal compound attached to the surface. By precipitating the metal compound in a liquid medium, the metal compound can be uniformly precipitated on the surface of the composite material. Examples of the metal compound precipitated in the sulfur source addition step include metal sulfides, metal hydroxides, metal oxides, etc., and may include at least one selected from the group consisting of these.
[0055] The sulfur source added to the mixture may be, for example, a compound capable of generating sulfide ions. Specific examples of sulfur sources include hydrogen sulfide, carbon disulfide, silicon disulfide, nitrogen sulfide, phosphorus sulfide, and arsenic sulfide. The amount of sulfur source added may be, for example, 0.5 times or more by mol, and preferably 0.8 times or more by mol, in terms of sulfide ions, relative to the content of metal ions contained in the metal source constituting the mixture. The amount of sulfur source added in terms of sulfide ions may be, for example, 3.0 times or less by mol, and preferably 2.5 times or less by mol, or 2.0 times or less by mol.
[0056] The sulfur source addition step may further include adjusting the pH of the mixture. The pH adjustment may be performed prior to the start of the addition of the sulfur source, or may be performed in parallel during the addition of the sulfur source. The pH adjustment may suppress the pH change of the mixture accompanying the addition of the sulfur source. Specifically, the pH adjustment of the mixture may be performed, for example, by adding a basic compound or an acidic compound to the mixture. Examples of the basic compound used for the pH adjustment include hydroxide salts such as hydroxides of alkali metals and hydroxides of alkaline earth metals, and aqueous ammonia solutions. Examples of the acidic compound include nitric acid, sulfuric acid, phosphoric acid, and boric acid. The pH adjustment range in the pH adjustment may be, for example, 2 or more and 14 or less, and may be preferably 2.5 or more. The pH adjustment may be, for example, by increasing the pH of the mixture, preferably by increasing it by 1 or more or 2 or more. The pH adjustment may be, for example, by decreasing the pH of the mixture, preferably by decreasing it by 1 or more or 2 or more. Further, the pH may be adjusted, for example, to suppress the pH fluctuation of the mixture, and the pH fluctuation accompanying the addition of the sulfur source may be suppressed, for example, to 13.5 or less, preferably 12 or less.
[0057] After the sulfur source is added, a precipitation step of precipitating the metal compound may be included. In the precipitation step, the metal compound may be precipitated while stirring the mixture, or the metal compound may be precipitated in a stationary state. The temperature in the precipitation step may be, for example, 0°C or higher and 100°C or lower, and preferably 10°C or higher or 90°C or lower. The precipitation time in the precipitation step may be, for example, 1 minute or higher and 72 hours or lower, and preferably 5 minutes or higher or 48 hours or lower.
[0058] The third manufacturing method may further include a separation step of separating the obtained first modified composite material from the mixture, and may further include a purification step as necessary. In the separation step, for example, the mixture containing the first modified composite material may be subjected to solid-liquid separation to extract the first modified composite material. In the purification step, the first modified composite material may be washed with pure water or the like. The extracted first modified composite material may be dried, for example, by heat drying, vacuum degassing, natural drying, or a combination thereof.
[0059] The third manufacturing method includes a second modification step of heat-treating the first modified composite material to obtain a second modified composite material having a metal sulfide derived from a metal source attached thereto. The details of the second modification step in the third manufacturing method are the same as those of the second modification step in the first manufacturing method.
[0060] Electrode active material for lithium-sulfur batteries The electrode active material for lithium-sulfur batteries includes a composite material containing a porous carbon material and sulfur supported on the porous carbon material, and a metal sulfide containing a specific metal arranged on the surface of the composite material. The positive electrode active material for lithium-sulfur batteries has a ratio (Cx / Ci) of 0.3 or more of the mass ratio (Cx) of the specific metal to the total amount of carbon, sulfur, oxygen, nitrogen and the specific metal in the vicinity of the surface of the positive electrode active material for lithium-sulfur batteries measured by energy dispersive X-ray spectroscopy relative to the mass-based content (Ci) of the specific metal in the positive electrode active material for lithium-sulfur batteries measured by inductively coupled plasma optical emission spectroscopy. Here, the specific metal may include at least one selected from the group consisting of Ti, V, Mn, Fe, Co, Ni, Cu, Zn, Ge, Zr, In, Sn, Nb, Mo, Ta and W. Preferably, the specific metal may include at least Zn. That is, the metal sulfide may include at least zinc sulfide.
[0061] The electrode active material for lithium-sulfur batteries may include a coated composite material in which at least a part of the surface of the composite material is coated with a metal sulfide, and the coated composite material may be, for example, the second modified composite material in the above-mentioned manufacturing method. By disposing the metal sulfide on the surface of the composite material, it is possible to more effectively suppress the outflow of lithium polysulfide generated during charging and discharging of the lithium-sulfur battery from the porous carbon material. The presence of the metal sulfide can be detected, for example, by X-ray diffraction (XRD) spectrum or transmission electron microscope (TEM). For example, when the specific metal is zinc, the presence of ZnS can be confirmed by the presence of a peak derived from the (111) plane of ZnS at around 28.5° in XRD measurement. In addition, the (111) plane of ZnS can also be assigned from the diffraction point in the electron beam diffraction image by TEM observation.
[0062] In the electrode active material for lithium-sulfur batteries, the metal sulfide is arranged on the surface of the composite material. The arrangement state of the metal sulfide on the surface of the composite material can be evaluated, for example, by the ratio of the content of the specific metal present in a partial region of the surface of the electrode active material for lithium-sulfur batteries to the total content of the specific metal contained in the electrode active material for lithium-sulfur batteries (hereinafter, also referred to as the dispersion index of the specific metal). The larger the dispersion index value, the more uniformly the specific metal is dispersed and present on the entire surface of the composite material.
[0063] The total content of the specific metals contained in the electrode active material for lithium-sulfur batteries can be evaluated as the mass-based content (Ci) of the specific metals in the positive electrode active material for lithium-sulfur batteries measured by inductively coupled plasma (ICP) atomic emission spectrometry.
[0064] In addition, the contents of carbon, sulfur, oxygen, nitrogen and specific metals in the vicinity of the surface of the electrode active material for lithium-sulfur batteries, which is composed of carbon, sulfur and specific metals, can be evaluated by energy dispersive spectroscopy (EDX). That is, the content of the specific metal present on the surface of the electrode active material for lithium-sulfur batteries can be evaluated by the mass ratio (Cx) of the specific metal to the total mass of carbon, oxygen, nitrogen, sulfur and specific metal in the vicinity of the surface of the positive electrode active material for lithium-sulfur batteries measured by energy dispersive X-ray (EDX) spectroscopy. The measurement conditions of SEM-EDX vary depending on the size of the particles, but the magnification may be such that at least 100 particles, preferably 500 particles, more preferably 1000 particles are present in the observation area. For example, when D50 is about 2 μm, the magnification can be selected to be 1500 times.
[0065] Here, the surface vicinity measured by EDX spectroscopy is a depth that varies depending on the element being measured, even under the same measurement conditions. For example, for carbon, sulfur, etc., the depth is several μm (10 -6 Even under measurement conditions that allow detection to a depth of several hundred nm (10 -7It is considered that the metal is only detected to a depth of about 1000 nm (order of m). In this case, when the metal compound is localized with a certain thickness near the surface of the electrode active material for lithium-sulfur batteries, the content of the metal atoms contained in the metal compound is detected as a content that is smaller than that of carbon, sulfur, etc. Therefore, when the dispersion index (Cx / Ci) of the specific metal is evaluated for the electrode active material for lithium-sulfur batteries, when the specific metal is uniformly distributed near the surface of the electrode active material for lithium-sulfur batteries, the value is close to 1. On the other hand, when the specific metal is localized near the surface of the electrode active material for lithium-sulfur batteries, the value is smaller than when the specific metal is uniformly distributed.
[0066] In the electrode active material for lithium-sulfur batteries, the dispersion index of the specific metal may be 0.3 or more, preferably 0.5 or more, or 0.7 or more. The dispersion index of the specific metal may be 1.2 or less. When the dispersion index of the specific metal is within the above range, there is a tendency that the outflow of lithium polysulfide generated during the discharge of the lithium-sulfur battery from the porous carbon material can be more effectively suppressed. The dispersion index of the specific metal is evaluated as the arithmetic average value of the measured values measured in any three regions.
[0067] When the electrode active material for lithium-sulfur batteries contains zinc sulfide as a metal sulfide, the intensity ratio of the peak intensity of the (220) plane to the peak intensity of the (111) plane of zinc sulfide in the X-ray diffraction (XRD) pattern may be 0.42 or more, preferably 0.421 or more, or 0.422 or more. The peak intensity ratio may be 0.5 or less. When the peak intensity ratio in the XRD pattern is within the above range, the cycle retention rate tends to be further improved. Here, the peak originating from the (111) plane of zinc sulfide is observed at about 28.5°, and the peak originating from the (220) plane is observed at about 47.5°.
[0068] The content of the specific metal contained in the electrode active material for lithium-sulfur batteries may be, for example, 0.1% by mass or more and 30% by mass or less, 0.5% by mass or more, or 20% by mass or less. In addition, the mass ratio of the content of the metal sulfide to the content of the composite material in the electrode active material for lithium-sulfur batteries may be, for example, 0.15% by mass or more and 30% by mass or less, 0.75% by mass or more, or 40% by mass or less. Furthermore, the mass ratio of the content of the metal sulfide to the total content of sulfur in the electrode active material for lithium-ion batteries may be, for example, 0.2% by mass or more and 60% by mass or less, 1% by mass or more, or 30% by mass or less. When the content of the specific metal is within the above range, there is a tendency that the outflow of lithium polysulfide generated during discharge of the lithium-sulfur battery from the porous carbon material can be more effectively suppressed.
[0069] Positive electrode for lithium-sulfur batteries A positive electrode for a lithium-sulfur battery (hereinafter, simply referred to as "positive electrode") includes a current collector and a positive electrode active material layer disposed on the current collector. The positive electrode active material layer may include the above-mentioned electrode active material for a lithium-sulfur battery. The positive electrode is manufactured, for example, by applying an electrode composition containing the above-mentioned electrode active material for a lithium-sulfur battery, a liquid medium, a binder, a conductive assistant, and the like, onto a current collector, followed by drying and pressure molding to form a positive electrode active material layer on the current collector.
[0070] The liquid medium may be an organic solvent, water, or the like, depending on the application. Examples of the organic solvent include amide-based solvents such as N-methyl-2-pyrrolidone (NMP), ketone-based solvents such as diisopropyl ketone, diisobutyl ketone, and methyl ethyl ketone, hydrocarbon-based solvents such as heptane, ether-based solvents such as tetrahydrofuran, dimethoxyethane, and dioxolane, amine-based solvents such as diethylenetriamine, and ester-based solvents. The organic solvent may be used alone or in combination of two or more. The content of the liquid medium may be, for example, 10% by mass or more and 90% by mass or less with respect to the total mass of the electrode composition.
[0071] The binder is a material that aids in adhesion between the electrode active material and the conductive assistant, and adhesion of the electrode composition to the current collector. Examples of the binder include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene-butylene rubber, fluororubber, and various copolymers. The content of the binder may be, for example, 0.05% by mass or more and 50% by mass or less with respect to the total mass of the electrode composition.
[0072] The conductive assistant is, for example, a material that improves the electrical conductivity of the positive electrode composition layer. Examples of the conductive assistant include graphite such as modified graphene, natural graphite, and artificial graphite, carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black, conductive fibers such as carbon fibers and metal fibers, and carbon materials such as graphene and carbon nanotubes. The content of the conductive assistant may be, for example, 0.5% by mass or more and 30% by mass or less with respect to the total mass of the electrode composition.
[0073] Examples of the current collector include metals such as copper, stainless steel, aluminum, nickel, and titanium, composite materials in which the surface of copper or stainless steel is treated with carbon, nickel, titanium, silver, and the like, and carbon foil. When manufacturing a lightweight lithium-sulfur battery, for example, aluminum and carbon foil are preferable as lightweight current collectors. The current collector can also increase the adhesive strength of the positive electrode composition layer by forming fine irregularities on its surface. In addition, various forms such as films, sheets, foils, nets, porous bodies, foams, and nonwoven fabrics are possible. The thickness of the current collector may be, for example, 3 μm or more and 500 μm or less.
[0074] The positive electrode active material layer formed by including the above-mentioned electrode active material for lithium-sulfur batteries may be formed as a dense layer with few voids. The porosity of the positive electrode active material layer in the positive electrode may be, for example, 75% or less, preferably 60% or less, 55% or less, or 50% or less. The lower limit of the porosity of the positive electrode active material layer may be, for example, 1% or more. The porosity of the positive electrode active material layer may be calculated from the ratio of the theoretical density of the positive electrode composition layer calculated from the material constituting the positive electrode composition layer to the pressed density calculated from the thickness measured when the positive electrode composition layer is pressed. Alternatively, it may be calculated by specifying a predetermined range from a cross-sectional SEM image of the positive electrode active material layer and measuring the area ratio of the void portion using image analysis software.
[0075] Lithium-sulfur secondary battery The lithium-sulfur battery includes the positive electrode for the lithium-sulfur battery. The lithium-sulfur battery includes a positive electrode for the lithium-sulfur battery, a negative electrode, and an electrolyte disposed between the positive electrode and the negative electrode. The lithium-sulfur battery may include a separator as necessary. The electrolyte may be included in the positive electrode, the negative electrode, and the separator for the lithium-sulfur battery.
[0076] negative electrode A known material may be used as the negative electrode constituting the lithium-sulfur battery. Examples of the negative electrode material constituting the negative electrode include Li metal, Li-Si alloy, Li-Al alloy, Li-In alloy, and lithium titanate (e.g., Li4Ti5O 12 and LiTi2O4), lithium titanium composite oxides (e.g., Li4Ti 5-x Mn x O 12 ;0 <x≦0.3)、Li x C(x≦6) and the like. In these negative electrode materials, a part of the lithium may be replaced by other alkali metals. The negative electrode materials include Li metal, Li-Si alloy, Li-Al alloy, Li-In alloy, Li x C(x≦6) is preferred. These materials allow high voltage to be obtained from lithium-sulfur batteries.
[0077] Separator The separator may be made of a known material, such as porous polyethylene, polypropylene, etc. Also, a known separator may be used after being coated.
[0078] electrolyte The electrolyte may contain a lithium salt and may be appropriately selected from lithium salts used in conventional lithium ion batteries. The lithium salt may contain an anion having a fluorine element, for example. Specific examples of lithium salts containing an anion having a fluorine element include LiPF6, LiBF4, LiSbF6, LiAsF6, LiSO3CF3, LiN(SO2CF3)2 (LiTFSI), and LiN(SO2F)2 (LiFSI). The electrolyte may also contain a lithium salt that does not contain a fluorine element, such as lithium nitrate or LiClO4. The electrolyte may be one of these electrolytes, or two or more of them may be used in combination.
[0079] The electrolyte may contain an organic solvent. As the organic solvent, a carbonate-based solvent, an ether-based solvent, an ester-based solvent, an amide-based solvent, a nitrile-based solvent, or a sulfur-containing solvent may be used, or an organic solvent in which some elements of the above organic solvents are replaced with fluorine may be used. As the organic solvent, for example, carbonate-based solvents such as propione carbonate, ethylene carbonate, dimethyl carbonate, ethyl methyl carbonate, and fluoroethylene carbonate, ether-based solvents such as 1,3-dioxolane, 1,2-dimethoxyethane, 1,3-dimethoxypropane, 2,2,3,3-tetrafluoropropyl difluoromethyl ether, and tetrahydrofuran, ester-based solvents such as methyl formate, methyl acetate, and γ-butyl lactone, amide-based solvents such as N,N-dimethylacetamide and N,N-dimethylformamide, sulfolane, dimethyl sulfoxide, and 1,3-propane sultone, and the like can be mentioned.
[0080] The invention according to the present disclosure may include, for example, the following aspects. [1] A method for producing an electrode active material for a lithium-sulfur battery, comprising: mixing a composite material comprising a porous carbon material and sulfur supported on the porous carbon material, a metal source, and a liquid medium to obtain a first modified composite material having a metal compound derived from the metal source attached thereto; and heat-treating the first modified composite material to obtain a second modified composite material having a metal sulfide attached thereto, wherein the metal source contains at least one specific metal selected from the group consisting of Ti, V, Mn, Fe, Co, Ni, Cu, Zn, Ge, Zr, In, Sn, Nb, Mo, Ta, and W.
[0081] [2] The method for producing an electrode active material for a lithium-sulfur battery according to [1], wherein obtaining the first modified composite material includes heat-treating a mixture containing the composite material, the metal source, and the liquid medium under pressure to precipitate the metal compound on a surface of the composite material.
[0082] [3] The method for producing an electrode active material for a lithium-sulfur battery according to [2], wherein the heat treatment under pressure is carried out at a temperature equal to or higher than the boiling point of the liquid medium.
[0083] [4] The method for producing an electrode active material for a lithium-sulfur battery according to [2] or [3], wherein the heat treatment under pressure is carried out in a closed system.
[0084] [5] The method for producing an electrode active material for a lithium-sulfur battery according to [1], wherein obtaining the first modified composite material includes adjusting a pH of a mixture containing the composite material, a metal source, and a liquid medium to precipitate the metal compound on a surface of the composite material.
[0085] [6] The method for producing an electrode active material for a lithium-sulfur battery according to [1], wherein obtaining the first modified composite material includes adding a sulfur source to a mixture containing the composite material, a metal source, and a liquid medium, and precipitating the metal compound on a surface of the composite material.
[0086] [7] The method for producing an electrode active material for a lithium-sulfur battery according to [6], wherein obtaining the first modified composite material further comprises adjusting a pH of the mixture.
[0087] [8] The method for producing an electrode active material for a lithium-sulfur battery according to any one of [1] to [7], wherein the porous carbon material has a peak pore size of 0.5 nm or more and 10 nm or less.
[0088] [9] The method for producing an electrode active material for a lithium-sulfur battery according to any one of [1] to [8], wherein the porous carbon material has a volume average particle size of 0.5 μm or more and 20 μm or less.
[0089]
[10] The method for producing an electrode active material for a lithium-sulfur battery according to any one of [1] to [9], wherein the porous carbon material has an aspect ratio of 1 or more and 3 or less.
[0090]
[11] The method for producing an electrode active material for a lithium-sulfur battery according to any one of [1] to
[10] , wherein the heat treatment of the first modified composite material includes removing at least a portion of the liquid medium to obtain a dried product.
[0091]
[12] The method for producing an electrode active material for a lithium-sulfur battery according to
[11] , wherein the heat treatment of the first modified composite material further comprises heat treating the dried material at 50°C or higher and 400°C or lower.
[0092]
[13] A positive electrode active material for a lithium-sulfur battery comprising a porous carbon material, sulfur supported on the porous carbon material, and a metal sulfide containing a specific metal, wherein a ratio of a mass ratio of the specific metal to a total amount of carbon, sulfur, oxygen, nitrogen, and the specific metal in the vicinity of a surface of the positive electrode active material for a lithium-sulfur battery as measured by X-ray photoelectron spectroscopy relative to a mass content of the specific metal in the positive electrode active material for a lithium-sulfur battery as measured by inductively coupled plasma atomic emission spectroscopy is 0.3 or more, and the specific metal is at least one selected from the group consisting of Ti, V, Mn, Fe, Co, Ni, Cu, Zn, Ge, Zr, In, Sn, Nb, Mo, Ta, and W.
[0093]
[14] The electrode active material for a lithium-sulfur battery according to
[13] , wherein the porous carbon material has a peak pore size of 0.5 nm or more and 10 nm or less.
[0094]
[15] The electrode active material for a lithium-sulfur battery according to
[13] or
[14] , wherein the porous carbon material has a volume average particle size of 0.5 μm or more and 20 μm or less.
[0095]
[16] The electrode active material for a lithium-sulfur battery according to any one of
[13] to
[15] , wherein the porous carbon material has an aspect ratio of 1 or more and 3 or less.
[0096]
[17] The positive electrode active material for a lithium-sulfur battery according to any one of
[13] to
[16] , wherein the metal sulfide includes zinc sulfide.
[0097]
[18] The electrode active material for a lithium-sulfur battery according to
[17] , wherein in an X-ray diffraction pattern, the intensity ratio of a peak originating from a (220) plane of zinc sulfide to a peak originating from a (111) plane of zinc sulfide is 0.42 or more.
[0098]
[19] The positive electrode active material for a lithium-sulfur battery according to any one of
[13] to
[18] , wherein the content of the specific metal in the positive electrode active material for a lithium-sulfur battery is 0.1 mass% or more and 20 mass% or less.
[0099]
[20] The positive electrode active material for a lithium-sulfur battery according to any one of
[13] to
[19] , wherein the ratio of the mass ratio of the specific metal to the total amount of carbon, sulfur, oxygen, nitrogen and the specific metal in the vicinity of the surface of the positive electrode active material for a lithium-sulfur battery measured by X-ray photoelectron spectroscopy to the mass content of the specific metal in the positive electrode active material for a lithium-sulfur battery measured by inductively coupled plasma atomic emission spectroscopy is 0.5 or more.
[0100]
[21] The positive electrode active material for a lithium-sulfur battery according to any one of
[13] to
[20] , wherein the ratio of the mass ratio of the specific metal to the total amount of carbon, sulfur, oxygen, nitrogen and the specific metal in the vicinity of the surface of the positive electrode active material for a lithium-sulfur battery measured by X-ray photoelectron spectroscopy to the mass content of the specific metal in the positive electrode active material for a lithium-sulfur battery measured by inductively coupled plasma atomic emission spectroscopy is 0.7 or more. EXAMPLES
[0101] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0102] Example 1 Preparation of ZnS-containing sulfur-carbon positive electrode active material A mixture was obtained by mixing 12 g of a porous carbon material (AT Electrodes, AP20-0001HC) and 18 g of sulfur powder (weight ratio of 40:60). The mixture was placed in a pressure vessel and heat-treated at 150°C for 3 hours to obtain a composite material as a sulfur-carbon composite. The physical properties of the porous carbon material used are shown in Table 1. The nitrogen adsorption isotherm was measured using Quantachrome's "Novatouch," and the BET specific surface area and pore size distribution were analyzed using the QSDFT method (quenched solid density functional theory). The aspect ratio was calculated as follows.
[0103] Aspect ratio calculation The porous carbon material before impregnation with sulfur was mounted on a carbon tape, and the shape of the porous carbon material was observed using an electron microscope (Hitachi High-Technologies Corporation, FLEXSEM1000II). The observation conditions were an acceleration voltage of 5 kV and a magnification of 10,000 times. Any particle whose particle shape could be confirmed (the arithmetic mean of the long and short diameters as observed by SEM) was 50 The aspect ratio of each of the 47 particles (which are 0.1 to 1.5 times larger than the particle size) was calculated using Image J, and the average aspect ratio was found to be 1.15.
[0104] Particle size distribution measurement The volumetric particle size distribution was measured using a laser diffraction particle size distribution analyzer (Malvern MASTERSIZER 2000). For the measurement sample, an appropriate amount of carbon material was dispersed in 170 mL of ethanol solvent so that the laser intensity of the measurement device was within the appropriate range. The stirring process was performed at 2500 rpm for 60 seconds. The volume average particle size was calculated as the 50% particle size D 50 The 10% particle size D was calculated as the value at which the volume accumulated value from the small particle size side becomes 10% and 90%. 10 and 90% particle size D 90 The results are shown in Table 1.
[0105] [Table 1]
[0106] 4 g of the composite material was mixed with 0.3 g of zinc oxide. 8 g of pure water was added to the mixture of zinc oxide and the composite material and mixed to obtain a slurry as a dispersion of zinc oxide and the composite material. The obtained slurry was placed in a pressure-resistant container and heat-treated at 230°C for 3 hours in a closed system. The heat-treated slurry was suction-filtered, and the filtered product was dried at 50°C for 30 minutes to obtain a dried product. The above-mentioned dried product was placed in a closed container and heat-treated at 300°C for 3 hours to obtain the ZnS-containing sulfur-carbon positive electrode active material of Example 1 as a coated composite material.
[0107] Example 2 A ZnS-containing sulfur-carbon positive electrode active material of Example 2 was prepared in the same manner as in Example 1, except that the amount of zinc oxide added to the mixture was changed to 0.15 g.
[0108] Example 3 A ZnS-containing sulfur-carbon positive electrode active material of Example 3 was prepared in the same manner as in Example 1, except that the amount of zinc oxide added to the mixture was changed to 0.6 g.
[0109] Example 4 1.05 g of zinc sulfate heptahydrate (Fujifilm Wako Pure Chemical Industries, Ltd.) was added with 36 g of pure water to obtain an aqueous zinc sulfate solution. 4.0 g of the composite material was mixed with the obtained solution to obtain a slurry of a dispersion. 0.58 g of sodium hydroxide (Fujifilm Wako Pure Chemical Industries, Ltd.) was added with 40 g of pure water and dissolved to obtain an aqueous sodium hydroxide solution. The aqueous sodium hydroxide solution was added to the dispersion slurry obtained above and stirred for 10 minutes. The pH of the slurry was 12.8 to 12.9. After stirring, the slurry was suction filtered and the filtered product was heated at 50°C for 30 minutes to obtain a dried product. The steam-dried product was placed in a sealed heating chamber and heat-treated at 300°C for 3 hours to obtain a ZnS-containing sulfur-carbon positive electrode material of Example 4 as a coated composite material.
[0110] Comparative Example 1: Preparation of sulfur-carbon positive electrode active material 12 g of a porous carbon material (manufactured by AT Electrode Co., Ltd., AP20-0001HC) was mixed with 18 g of sulfur powder (weight ratio of 40:60). The mixture of the porous carbon material and the sulfur powder was placed in a pressure-resistant container and heat-treated at 150°C for 3 hours. After that, the mixture was returned to room temperature and then heat-treated at 350°C for 3 hours to obtain a sulfur-carbon positive electrode active material of Comparative Example 1.
[0111] Comparative Example 2 A composite material was obtained as a sulfur-carbon composite in the same manner as in Example 1. 4.0 g of the obtained composite material and 0.36 g of zinc sulfide (Kishida Chemical) were mixed, placed in a sealed container, and heat-treated at 300° C. for 3 hours to obtain a ZnS-containing sulfur-carbon positive electrode active material of Comparative Example 2.
[0112] X-ray diffraction (XRD) analysis XRD analysis (Rigaku miniflex) was performed on the ZnS-containing sulfur-carbon positive electrode active materials produced in Examples 1, 2, 3, 4, Comparative Example 1, and Comparative Example 2. Figures 1 to 4 show the XRD analysis results for the ZnS-containing sulfur-carbon positive electrode active materials produced in Examples 1 to 4. Figure 5 shows the XRD analysis result for the sulfur-carbon positive electrode active material of Comparative Example 1, and Figure 6 shows the XRD analysis result for the positive electrode active material of Comparative Example 2.
[0113] In Fig. 1, a peak derived from the (111) plane of ZnS was observed around 28.5°, confirming that crystalline ZnS was formed in the sulfur-carbon positive electrode active material to which ZnS was added produced in Example 1. In addition, a peak derived from the (220) plane of ZnS was also observed around 47.5°. Furthermore, a peak derived from the (311) plane of ZnS was also observed around 56.5°.
[0114] ICP analysis The positive electrode active material obtained above was subjected to inductively coupled plasma (ICP) atomic emission spectroscopy to determine the mass-based content (Ci) of Zn, a specific metal contained in the positive electrode active material. Specifically, a sample was prepared using nitric acid and heated and dissolved by microwaves, and the Zn content was determined using an inductively coupled plasma (ICP) atomic emission spectroscopy analyzer (ICP-AES; Optima 8300: manufactured by Perkin Elmer). The results are shown in Table 2.
[0115] Surface composition analysis The ratio (Cx) of zinc to the total amount of carbon, sulfur, oxygen, nitrogen, and zinc near the surface of the positive electrode active material was determined for three locations using a scanning electron microscope (SEM) / energy dispersive X-ray analyzer (EDX) (Hitachi High-Technologies Corporation; accelerating voltage 5 kV, magnification 1500 times, spectrum area count number >2500000), and the arithmetic average was calculated. Furthermore, Cx / Ci was calculated as the dispersion index of a specific metal. The results are shown in Table 2. FIG. 7 shows the SEM image used in the EDX analysis of Example 1.
[0116] Manufacturing of positive electrodes for lithium-sulfur secondary batteries A positive electrode slurry composition was prepared by mixing 85 parts by mass of the sulfur-carbon positive electrode active material prepared in Example 1 and Comparative Example 1, 10 parts by mass of carbon black, and 5 parts by mass of styrene-butadiene rubber (SBR) / carboxymethyl cellulose (CMC) / polyvinylpyrrolidone (PVP) (SBR / CMC / PVP=2.0 / 2.5 / 0.5).
[0117] The obtained positive electrode slurry composition was applied to a current collector and dried at 50° C. for 30 minutes. The current collector was an aluminum foil coated with carbon. The dried product was pressed with a roll press to obtain an active material layer with a density of 1.0 g / cm. 3 After that, the positive electrode for a lithium-sulfur secondary battery of Example 1 was obtained by cutting into a predetermined size.
[0118] Preparation of non-aqueous electrolyte Fluoroethylene carbonate (FEC) and dimethyl carbonate (DMC) were mixed in a volume ratio of 71:100 to obtain a mixed solution. Lithium hexafluorophosphate (LiPF6) was dissolved in the resulting mixed solution to a concentration of 1.0 mol / L to prepare a non-aqueous electrolyte solution.
[0119] Assembly of lithium-sulfur secondary batteries A lead electrode was attached to the positive electrode obtained above, a separator made of porous polypropylene (Celgard 2400) was placed, and the resultant was stored in a bag-shaped laminate pack. After storage, the material was vacuum dried at 50°C to remove moisture adsorbed on each component. After vacuum drying, the metallic lithium of the negative electrode placed on the SUS foil was placed in the laminate pack facing the positive electrode via the porous polypropylene, and the nonaqueous electrolyte prepared above was poured in and sealed to obtain a laminate-type lithium-sulfur secondary battery as an evaluation battery. The following battery characteristics were evaluated using the obtained evaluation battery.
[0120] Capacity retention rate during charge / discharge cycles The evaluation battery obtained as described above was placed in a thermostatic chamber at 25°C, and an evaluation test of the cycle capacity retention rate was performed. The charge and discharge voltage was in the range of 1.0V to 3.0V. The discharge current was the current value when 0.1C capacity was extracted. The discharge capacity per mass of sulfur in the second cycle immediately after the start of discharge, Qcyc(2), was measured. Next, charging and discharging were repeated, and the discharge capacity in the 30th cycle, Qcyc(30), was measured. The capacity retention rate after 30 cycles, Pcyc (=100×Qcyc(30) / Qcyc(2)) (%) was calculated by dividing Qcyc(30) by the obtained Qcyc(2). The results are shown in Table 2.
[0121] [Table 2]
[0122] In the evaluation batteries containing the ZnS-containing sulfur-carbon positive electrode active material in Examples 1 to 4, the cycle characteristics were improved compared to Comparative Example 1. In Comparative Example 2, the cycle characteristics were deteriorated. This is considered to be because the dispersion index was low and ZnS was segregated, so that the effect of suppressing the side reaction between sulfur and the electrolyte by the coating was not sufficiently obtained. In addition, the peak intensity ratio (220 / 111) of ZnS in Examples 1 to 4 was higher than that of the comparative examples. When (220 / 111) is low, it is considered that the occupancy rate of S sites in ZnS is low and there are S defects in the structure. Therefore, it is considered that the crystal structure of ZnS becomes unstable when charging and discharging is repeated, resulting in poor cycle characteristics.
Claims
1. mixing a composite material including a porous carbon material and sulfur supported on the porous carbon material, a metal source, and a liquid medium to obtain a first modified composite material having a metal compound derived from the metal source attached thereto; and heat treating the first modified composite material to obtain a second modified composite material having attached thereto a metal sulfide derived from the metal source; The metal source includes at least one specific metal selected from the group consisting of Ti, V, Mn, Fe, Co, Ni, Cu, Zn, Ge, Zr, In, Sn, Nb, Mo, Ta and W.
2. 2. The method for producing an electrode active material for a lithium-sulfur battery according to claim 1, wherein obtaining the first modified composite material comprises heat-treating a mixture containing the composite material, the metal source and the liquid medium under pressure to precipitate the metal compound on a surface of the composite material.
3. The method for producing an electrode active material for a lithium-sulfur battery according to claim 2 , wherein the heat treatment under pressure is carried out at a temperature equal to or higher than the boiling point of the liquid medium.
4. The method for producing an electrode active material for a lithium-sulfur battery according to claim 3, wherein the heat treatment under pressure is carried out in a closed system.
5. 2. The method for producing an electrode active material for a lithium-sulfur battery according to claim 1, wherein obtaining the first modified composite material comprises adjusting a pH of a mixture containing the composite material, the metal source, and the liquid medium to precipitate the metal compound on a surface of the composite material.
6. 2. The method for producing an electrode active material for a lithium-sulfur battery according to claim 1, wherein obtaining the first modified composite material comprises adding a sulfur source to a mixture containing the composite material, the metal source, and the liquid medium, and precipitating the metal compound on a surface of the composite material.
7. 7. The method for preparing an electrode active material for a lithium-sulfur battery according to claim 6, wherein obtaining the first modified composite material further comprises adjusting a pH of the mixture.
8. The method for producing an electrode active material for a lithium-sulfur battery according to any one of claims 1 to 7, wherein the porous carbon material has a peak pore size of 0.5 nm or more and 10 nm or less.
9. The method for producing an electrode active material for a lithium-sulfur battery according to any one of claims 1 to 7, wherein the porous carbon material has a volume average particle size of 0.5 µm or more and 20 µm or less.
10. The method for producing an electrode active material for a lithium-sulfur battery according to any one of claims 1 to 7, wherein the porous carbon material has an aspect ratio of 1 or more and 3 or less.
11. The method for producing an electrode active material for a lithium-sulfur battery according to claim 1 , wherein the heat treatment of the first modified composite material includes removing at least a portion of the liquid medium to obtain a dried product.
12. 12. The method of claim 11, wherein the heat treatment of the first modified composite material further comprises heat treating the dried material at 50°C to 400°C.
13. A positive electrode active material for a lithium-sulfur battery, comprising: a porous carbon material; sulfur supported on the porous carbon material; and a metal sulfide containing a specific metal, Relative to the mass-based content of the specific metal in the positive electrode active material for lithium-sulfur batteries measured by inductively coupled plasma optical emission spectrometry, a mass ratio of the specific metal to the total amount of carbon, sulfur, oxygen, nitrogen, and the specific metal in the vicinity of the surface of the positive electrode active material for a lithium-sulfur battery measured by X-ray photoelectron spectroscopy is 0.3 or more; The specific metal is at least one selected from the group consisting of Ti, V, Mn, Fe, Co, Ni, Cu, Zn, Ge, Zr, In, Sn, Nb, Mo, Ta and W.
14. The electrode active material for a lithium-sulfur battery according to claim 13, wherein the porous carbon material has a peak pore size of 0.5 nm or more and 10 nm or less.
15. The electrode active material for a lithium-sulfur battery according to claim 13, wherein the porous carbon material has a volume average particle size of 0.5 μm or more and 20 μm or less.
16. The electrode active material for a lithium-sulfur battery according to claim 13 , wherein the porous carbon material has an aspect ratio of 1 or more and 3 or less.
17. The positive electrode active material for a lithium-sulfur battery according to claim 13, wherein a ratio of a mass ratio of the specific metal to a total amount of carbon, sulfur, oxygen, nitrogen and the specific metal in the vicinity of a surface of the positive electrode active material for a lithium-sulfur battery measured by X-ray photoelectron spectroscopy to a mass-based content of the specific metal in the positive electrode active material for a lithium-sulfur battery measured by inductively coupled plasma atomic emission spectroscopy is 0.5 or more.
18. The positive electrode active material for a lithium-sulfur battery according to claim 17, wherein a ratio of a mass ratio of the specific metal to a total amount of carbon, sulfur, oxygen, nitrogen and the specific metal in the vicinity of a surface of the positive electrode active material for a lithium-sulfur battery measured by X-ray photoelectron spectroscopy to a mass-based content of the specific metal in the positive electrode active material for a lithium-sulfur battery measured by inductively coupled plasma atomic emission spectroscopy is 0.7 or more.
19. The positive electrode active material for a lithium-sulfur battery according to claim 13 , wherein the metal sulfide comprises zinc sulfide.
20. 20. The positive electrode active material for a lithium-sulfur battery according to claim 19, wherein the intensity ratio of a peak derived from a (220) plane of zinc sulfide to a peak derived from a (111) plane of zinc sulfide in an X-ray diffraction pattern is 0.42 or more.
21. The positive electrode active material for a lithium-sulfur battery according to claim 13, wherein the content of the specific metal in the positive electrode active material for a lithium-sulfur battery is 0.1% by mass or more and 20% by mass or less.
Citation Information
Patent Citations
Composite material, positive electrode for lithium sulfur battery, lithium sulfur battery, and method for manufacturing composite material
JP2021136126A
Positive electrode material for lithium ion batteries, and lithium ion battery
WO2012086196A1
Method for producing iron sulfide, positive electrode for lithium secondary battery containing the iron sulfide produced by the method, and lithium secondary battery including the same
JP2021531228A
Cited By
Positive electrode material for lithium sulfur battery and method for manufacturing same
WO2026094691A1