Pattern sheet and method for using pattern sheet

The pattern sheet with a thermoplastic resin layer pseudo-adhered to a polyolefin release agent layer addresses the challenge of maintaining adhesive strength loss and improving processability by using a polyolefin resin composition for effective adhesive sheet treatment.

JP2024139493APending Publication Date: 2024-10-09LINTEC CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023050451
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Existing pressure-sensitive adhesive sheets with glue-killing treatments face issues of adhesive strength loss that is difficult to maintain, and the processability is poor due to low adhesive strength in the non-adhesive portions, especially when using silicone films.

Method used

A pattern sheet with a thermoplastic resin layer pseudo-adhered to a release agent layer containing a polyolefin resin composition, where the interface between the layers has a pseudo-adhesive force of 50 mN/50 mm to 1000 mN/50 mm, allowing for effective adhesive strength loss and easy separation.

Benefits of technology

The pattern sheet maintains adhesive strength loss effectively and enhances processability by ensuring the thermoplastic resin layer remains as a non-adhesive portion on the adhesive sheet, preventing adhesive penetration and facilitating easy separation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139493000001_ABST
    Figure 2024139493000001_ABST
Patent Text Reader

Abstract

To provide a pattern sheet which has adequate pseudo adhesion to a release agent layer, is excellent in processability when an adhesive layer is subjected to detackified adhesive treatment, and easily sustains an effect for losing adhesive force.SOLUTION: A pattern sheet 100 is used while being stuck to an adhesive sheet. The pattern sheet 100 includes a release base material 11, a release sheet 10 having a release agent layer 13 provided on one surface of the release base material 11, and a thermoplastic resin layer 20 provided on a surface on a side opposite to the release base material 11 of the release sheet 10, and pseudo-bonded to the release agent layer 13, wherein the release agent layer 13 contains an olefin release agent containing a polyolefin resin composition, the thermoplastic resin layer 20 contains a polyolefin resin, an interface between the release agent layer 13 and the thermoplastic resin layer 20 is a pseudo-bonded interface, and pseudo adhesive force when being released at the pseudo-bonded interface is 50 mN / 50 mm or more and 1,000 mN / 50 mm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pattern sheet and a method for using the pattern sheet. [Background technology]

[0002] In some cases, a part of an adhesive layer provided on the entire surface of one side of an adhesive base material is subjected to a treatment for causing the adhesive layer to lose its adhesive power (so-called glue-killing treatment). A glue-killing treated adhesive sheet has an adhesive part and a non-adhesive part in the adhesive layer. The non-adhesive part is formed by, for example, printing a glue-killing agent such as printing ink or varnish on a part of the adhesive layer to cause the adhesive layer to lose its adhesiveness.

[0003] Patent Document 1 describes a label with release paper, which comprises a release paper having a release agent layer on its surface and a label substrate temporarily attached to the release paper via an adhesive layer, and has an adhesive-blocking surface in which an adhesive-blocking agent is printed on a part of the adhesive layer facing the release agent layer to seal in some of the adhesiveness. The label with release paper described in Patent Document 1 has an equivalent friction resistance of the adhesive-blocking surface against the release agent layer surface and an equivalent friction resistance of the adhesive layer surface against the release agent layer surface, and also has an equivalent peel resistance of the adhesive-blocking surface against the release agent layer surface and an equivalent peel resistance of the adhesive layer surface against the release agent layer surface.

[0004] Patent Document 2 describes a method for producing an adhesive-blocking adhesive sheet, in which a long surface substrate is run together with a long release paper having an adhesive-blocking portion formed on its release agent surface, an adhesive is applied to the inner surface of the surface substrate, and then the inner surface of the surface substrate and the release agent surface of the release paper are bonded together. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2002-099215 A [Patent Document 2] JP 2007-039484 A Summary of the Invention [Problem to be solved by the invention]

[0006] The label with release paper described in Patent Document 1 has a non-adhesive portion formed by printing an adhesive-killing agent containing printing ink on a portion of the adhesive layer to seal in the adhesiveness. Also, the adhesive-killing adhesive sheet described in Patent Document 2 has an adhesive-killing portion formed by applying adhesive-killing printing to the releasable surface (release agent surface) of the release agent layer using commonly used printing ink or varnish, and the adhesive-killing portion is transferred to the adhesive layer to form the non-adhesive portion.

[0007] However, in the label with release paper described in Patent Document 1 and the glue-killing adhesive sheet described in Patent Document 2, the non-adhesive parts formed by the glue-killing agent are difficult to maintain the effect of losing adhesive force because the glue-killing agent easily penetrates into the adhesive layer.

[0008] In addition, the adhesive-killing adhesive sheet described in Patent Document 2 forms an adhesive-killing portion by printing an adhesive directly on a release agent layer made of a silicone film. Therefore, the adhesive-killing portion formed on the release agent layer made of a silicone film appears to be pseudo-adhered to the release agent layer at first glance. However, since the adhesive strength of the adhesive-killing portion to the release agent layer is too low, the adhesive-killing adhesive sheet described in Patent Document 2 is poor in processability when performing adhesive killing treatment on the adhesive layer.

[0009] The object of the present invention is to provide a pattern sheet that has appropriate pseudo-adhesion with a release agent layer, is excellent in processability when applying glue-killing treatment to an adhesive layer, and is easy to maintain the effect of losing adhesive force, and a method for using said pattern sheet. [Means for solving the problem]

[0010] [1] A pattern sheet to be attached to an adhesive sheet, A release sheet including a release substrate and a release agent layer provided on one surface of the release substrate; a thermoplastic resin layer provided on the surface of the release sheet opposite to the release substrate and pseudo-adhered to the release agent layer; Equipped with the release agent layer comprises an olefin release agent containing a polyolefin resin composition, the thermoplastic resin layer contains a polyolefin resin, the interface between the release agent layer and the thermoplastic resin layer is a pseudo-adhesive interface; The pseudo-adhesion strength when peeled off at the pseudo-adhesion interface is 50 mN / 50 mm or more and 1000 mN / 50 mm or less. Pattern sheet.

[0011] [2] In the pattern sheet according to [1], The polyolefin resin composition contains a polyolefin thermoplastic resin having at least one structural unit selected from the group consisting of structural units derived from ethylene, structural units derived from propylene, structural units derived from butene, structural units derived from hexene, structural units derived from octene, and structural units derived from 4-methyl-1-pentene. Pattern sheet.

[0012] [3] In the pattern sheet according to [2], The polyolefin resin composition is a mixture of a copolymer containing a structural unit derived from ethylene and a structural unit derived from butene, and polyethylene, or The polyolefin resin composition is a mixture of a copolymer containing a structural unit derived from ethylene and a structural unit derived from octene, and polyethylene. Pattern sheet.

[0013] [4] [1] to [3], wherein the pattern sheet is The melt flow rate of the polyolefin resin composition is 1 g / 10 min or more and 20 g / 10 min or less. Pattern sheet.

[0014] [5] [1] to [4], wherein the pattern sheet is The polyolefin resin in the thermoplastic resin layer has at least one of a structural unit derived from ethylene and a structural unit derived from propylene. Pattern sheet.

[0015] [6] [1] to [5], wherein the pattern sheet is the thermoplastic resin layer is formed in a pattern so that a portion of the release agent layer is exposed, When the thermoplastic resin layer formed in a pattern and the exposed release agent layer are attached to the pressure-sensitive adhesive sheet, The peel strength of the release agent layer from the pressure-sensitive adhesive sheet is 50 mN / 50 mm or more and 500 mN / 50 mm or less. Pattern sheet.

[0016] [7] [1] to [6], wherein the pattern sheet is The release substrate is one or two of a paper substrate and a resin substrate; Pattern sheet.

[0017] [8] A method for using the pattern sheet according to any one of [1] to [7], providing the pattern sheet; preparing the pressure-sensitive adhesive sheet; a step of attaching the thermoplastic resin layer to the pressure-sensitive adhesive sheet, and laminating the pressure-sensitive adhesive sheet, the thermoplastic resin layer, and the release sheet in this order; having when the pattern sheet is separated from the pressure-sensitive adhesive sheet, the thermoplastic resin layer is separated from the release agent layer and remains on the pressure-sensitive adhesive sheet as a non-adhesive portion that causes the pressure-sensitive adhesive sheet to lose its adhesiveness. How to use the pattern sheet.

[0018] [9] A method for using the pattern sheet according to any one of [1] to [7], providing the pattern sheet; a step of punching the pattern sheet, forming a cut in the thermoplastic resin layer without forming a cut in the release sheet, thereby dividing an unnecessary portion of the thermoplastic resin layer from a patterned portion of the thermoplastic resin layer; a step of removing unnecessary portions of the thermoplastic resin layer to expose a portion of the first release agent layer surface of the release agent layer, thereby forming the thermoplastic resin layer in a pattern; preparing the pressure-sensitive adhesive sheet; a step of attaching the thermoplastic resin layer formed in a pattern to the pressure-sensitive adhesive sheet, and laminating the pressure-sensitive adhesive sheet, the thermoplastic resin layer formed in a pattern, and the release sheet in this order; having when the release sheet is separated from the pressure-sensitive adhesive sheet, the thermoplastic resin layer formed in a pattern is separated from the release agent layer and remains on the pressure-sensitive adhesive sheet as a non-adhesive portion that causes the pressure-sensitive adhesive sheet to lose its adhesiveness. How to use the pattern sheet.

[0019]

[10] A method for using the pattern sheet according to any one of [1] to [7], providing the pattern sheet; a step of punching the pattern sheet, forming a cut in the thermoplastic resin layer without forming a cut in the release sheet, thereby dividing an unnecessary portion of the thermoplastic resin layer from a patterned portion of the thermoplastic resin layer; a step of removing unnecessary portions of the thermoplastic resin layer to expose a portion of the first release agent layer surface of the release agent layer, thereby forming the thermoplastic resin layer in a pattern; preparing the pressure-sensitive adhesive sheet; a step of attaching the thermoplastic resin layer formed in a pattern to the adhesive sheet to form a label sheet in which the adhesive sheet, the thermoplastic resin layer formed in a pattern, and the release sheet are laminated in this order; a step of punching the label sheet, forming a cut in the adhesive sheet alone or in the adhesive sheet and the thermoplastic resin layer formed in a pattern, without forming a cut in the release sheet, to separate a label-free portion from a label portion; a step of removing the unnecessary portion of the label; having when the label portion is separated from the label sheet, the thermoplastic resin layer formed in a pattern is separated from the release agent layer and remains on the adhesive sheet as a non-adhesive portion that causes the adhesive sheet to lose its adhesiveness. How to use the pattern sheet. Effect of the Invention

[0020] According to one aspect of the present invention, there is provided a pattern sheet that has appropriate pseudo-adhesion with a release agent layer, is excellent in processability when applying a glue-killing treatment to an adhesive layer, and is easy to maintain the effect of losing adhesive force, as well as a method for using the pattern sheet. [Brief description of the drawings]

[0021] [Figure 1] FIG. 2 is a schematic cross-sectional view illustrating an example of a pattern sheet according to the present embodiment. [Diagram 2] FIG. 1 is a schematic cross-sectional view illustrating an example of a pressure-sensitive adhesive sheet. [Diagram 3] 1A to 1C are schematic process diagrams illustrating a first embodiment of a method for using a pattern sheet according to the present embodiment. [Figure 4] 1A to 1C are schematic process diagrams illustrating a first embodiment of a method for using a pattern sheet according to the present embodiment. [Diagram 5] 5A to 5C are schematic process diagrams illustrating a second embodiment of a method for using a pattern sheet according to the present embodiment. [Figure 6] 5A to 5C are schematic process diagrams illustrating a second embodiment of a method for using a pattern sheet according to the present embodiment. [Figure 7] 5A to 5C are schematic process diagrams illustrating a second embodiment of a method for using a pattern sheet according to the present embodiment. [Figure 8] 5A to 5C are schematic process diagrams illustrating a second embodiment of a method for using a pattern sheet according to the present embodiment. [Figure 9] 10A to 10C are schematic process diagrams illustrating a third embodiment of a method for using a pattern sheet according to the present embodiment. [Figure 10] 10A to 10C are schematic process diagrams illustrating a third embodiment of a method for using a pattern sheet according to the present embodiment. [Figure 11] 10A to 10C are schematic process diagrams illustrating a third embodiment of a method for using a pattern sheet according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] [Pattern sheet] A preferred embodiment of the pattern sheet according to this embodiment will be described.

[0023] The pattern sheet according to the present embodiment is used by being attached to an adhesive sheet. The pattern sheet includes a release sheet including a release substrate and a release agent layer provided on one side of the release substrate, and a thermoplastic resin layer provided on the side of the release sheet opposite to the release substrate and pseudo-adhered to the release agent layer. The release agent layer includes an olefin release agent containing a polyolefin resin composition, and the thermoplastic resin layer includes a polyolefin resin. The interface between the release agent layer and the thermoplastic resin layer is a pseudo-adhesion interface, and the pseudo-adhesion force when peeled off at the pseudo-adhesion interface is 50 mN / 50 mm or more and 1000 mN / 50 mm or less.

[0024] When the pattern sheet according to this embodiment is attached to the adhesive sheet, the thermoplastic resin layer side of the pattern sheet is attached toward the adhesive layer of the adhesive sheet. When the pattern sheet according to this embodiment is separated from the adhesive body after being attached to the adhesive sheet, the thermoplastic resin layer and the release agent layer in the pattern sheet are separated, and the thermoplastic resin layer remains in the adhesive layer. The part of the thermoplastic resin layer remaining in the adhesive layer becomes a non-adhesive part that has lost its adhesive force. By using the pattern sheet according to this embodiment, the glue killing process for forming the non-adhesive part is performed by transferring the thermoplastic resin, not by using a glue killing agent by printing such as printing ink, so that the glue killing agent does not soak into the adhesive layer. Therefore, by having the above-mentioned configuration, the pattern sheet according to this embodiment is more likely to maintain the effect of losing adhesive force. In addition, the pattern sheet according to this embodiment has excellent adhesive force between the thermoplastic resin and the release agent layer, and the adhesive force is such that the two are easily peeled off when it is desired to peel them off, so that the adhesive force between the thermoplastic resin layer and the release agent layer has moderate pseudo-adhesion. For this reason, the pattern sheet according to the present embodiment has excellent processability when performing glue-killing treatment on the adhesive layer. Since the pattern sheet according to the present embodiment has a suitable pseudo-adhesive property, it has an adhesive strength sufficient for use.

[0025] The pattern sheet according to the present embodiment will be described with reference to the drawings. In the drawings, some parts are shown enlarged or reduced in size to facilitate the description. Referring to Fig. 1, a schematic cross-sectional view of a pattern sheet 100 is shown as an example of the pattern sheet according to the present embodiment.

[0026] The pattern sheet 100 shown in FIG. 1 comprises a release sheet 10 and a thermoplastic resin layer 20 provided on one side of the release sheet 10. The release sheet 10 comprises a release substrate 11 and a release agent layer 13 provided on the release substrate 11. The release substrate 11 comprises a first release substrate surface 111 and a second release substrate surface 112 which is the surface opposite to the first release substrate surface 111, and the release agent layer 13 comprises a first release agent layer surface 131 and a second release agent layer surface 132 which is the surface opposite to the first release agent layer surface 131. The thermoplastic resin layer 20 comprises a first thermoplastic resin layer surface 201 and a second thermoplastic resin layer surface 202 which is the surface opposite to the first thermoplastic resin layer surface 201.

[0027] Specifically, the pattern sheet 100 includes a release substrate 11, a release sheet 10 including a release agent layer 13 laminated directly on one surface (first release substrate surface 111) of the release substrate 11, and a thermoplastic resin layer 20 laminated directly on the surface (first release agent layer surface 131) of the release agent layer 13 on the release sheet 10 opposite to the release substrate 11 side. That is, the pattern sheet 100 includes the release substrate 11, the release agent layer 13, and the thermoplastic resin layer 20 laminated in this order in the thickness direction from the release substrate 11 toward the thermoplastic resin layer 20. The release agent layer 13 contains an olefin release agent containing a polyolefin resin composition. The thermoplastic resin layer 20 contains a polyolefin resin. The thermoplastic resin layer 20 is pseudo-adhered to the release agent layer 13, and the interface between the release agent layer 13 and the thermoplastic resin layer 20 is a pseudo-adhesion interface. Specifically, in the pattern sheet 100, the contact surface between the first release agent layer surface 131 and the second thermoplastic resin layer surface 202 becomes the pseudo-adhesion interface. The pseudo-adhesion strength when peeled at the interface between the release agent layer 13 and the thermoplastic resin layer 20 is in the range of 50 mN / 50 mm or more and 1000 mN / 50 mm or less. When the pattern sheet 100 is attached to an adhesive sheet (not shown), the surface of the thermoplastic resin layer 20 opposite to the release sheet 10 side (first thermoplastic resin layer surface 201) is attached to the adhesive layer (not shown) of the adhesive sheet.

[0028] In the pattern sheet 100 shown in Fig. 1, the release agent layer 13 and the thermoplastic resin layer 20 are not provided on the second release substrate surface 112, which is the surface opposite to the first release substrate surface 111 of the release substrate 11, and the second release substrate surface 112 is exposed. The pattern sheet 100 is used by being attached to an adhesive sheet (not shown). In the release sheet 10 shown in Fig. 1, the release agent layer 13 is firmly adhered to the release substrate 11, not pseudo-adhered.

[0029] Although an example of the pattern sheet according to the present embodiment has been described above with reference to Fig. 1, the pattern sheet according to the present embodiment is not limited to this. The pattern sheet according to the present embodiment may adopt various forms as long as it has the above-mentioned configuration. For example, in the release sheet 10 in the pattern sheet 100 shown in Fig. 1, an intermediate layer (not shown) may be laminated between the release substrate 11 and the release agent layer 13 so as to be in direct contact with both the first release substrate surface 111 of the release substrate 11 and the second release agent layer surface 132 of the release agent layer 13. The intermediate layer may be an intermediate layer formed by extrusion lamination or coating.

[0030] In one aspect, the pattern sheet according to this embodiment preferably has a thermoplastic resin layer provided over the entire surface of the release sheet on the side of the release agent layer opposite the release substrate side.

[0031] In another aspect of the pattern sheet according to the present embodiment, it is also preferable that a thermoplastic resin layer is provided on a part of the surface of the release agent layer opposite the release substrate side of the release sheet. The state in which a thermoplastic resin layer is provided on a part of the surface of the release agent layer opposite the release substrate side has a part on the release agent layer where the thermoplastic resin is provided and a part on which the thermoplastic resin is not provided. That is, in another aspect of the pattern sheet according to the present embodiment, when the pattern sheet is viewed in plan from the thermoplastic resin layer side, the thermoplastic resin layer is intermittently provided on the release agent layer so as to have a part where the thermoplastic resin is exposed and a part where the release agent layer is exposed. In this case, it is also preferable that the pattern sheet according to the present embodiment has a thermoplastic resin layer formed in a pattern on the entire surface of the release agent layer opposite the release substrate side of the release sheet.

[0032] <Release sheet> The release sheet comprises a release substrate and a release agent layer provided on the release substrate.

[0033] (Release substrate) The release substrate is a substrate that supports the release agent layer. The material of the release substrate is not particularly limited, and examples thereof include paper, resin, and metal foil, and these materials may be used alone or in combination of two or more. The release substrate is preferably one or two of a paper substrate and a resin substrate. In this specification, the paper substrate is a substrate formed of paper, and the resin substrate is a resin substrate formed of a resin such as a resin film.

[0034] Examples of the paper used for the paper substrate include kraft paper, fine paper, glassine paper, and coated paper (eg, art paper, clay coated paper, cast coated paper, etc.).

[0035] Examples of resins used for the resin substrate include polyolefin resins (polyethylene, polypropylene, polybutene, polybutadiene, polymethylpentene, ethylene-norbornene copolymers, norbornene resins, and ethylene copolymers (ethylene-vinyl acetate copolymers, ethylene-(meth)acrylic acid copolymers, ethylene-(meth)acrylic acid ester copolymers, etc.)), polyester resins (polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, etc.), polyvinyl chloride resins (polyvinyl chloride, vinyl chloride copolymers, etc.), polyurethane, polystyrene, polycarbonate, polyamide, polyimide, and fluororesins.

[0036] (Middle class) The intermediate layer is a layer that is provided as necessary. When the intermediate layer is provided, the release substrate, the intermediate layer, and the release agent layer are laminated in this order. When the intermediate layer is provided, the intermediate layer may be laminated, for example, on the release substrate by extrusion lamination, or may be laminated on the release substrate by coating an easy adhesive such as a primer, or may be laminated by a combination of these. The intermediate layer is preferably laminated by extrusion lamination.

[0037] The material used for the intermediate layer is not particularly limited as long as it can improve the adhesion between the release substrate and the release agent layer.The material used for the intermediate layer can be, for example, polyolefin resin (polyethylene, polypropylene, etc.), polyurethane resin, polyacrylate, etc. Among these, the material used for the intermediate layer is preferably polyolefin, more preferably at least one of polypropylene and polyethylene, and even more preferably polyethylene.When the material used for the intermediate layer is polyethylene, the polyethylene is preferably low-density polyethylene.

[0038] When the intermediate layer contains, for example, a polyolefin resin, the content of the polyolefin resin is preferably 50% by mass or more and 100% by mass or less. When the intermediate layer contains a polyolefin resin, the content of the polyolefin resin is more preferably 75% by mass or more, even more preferably 90% by mass or more, and even more preferably 100% by mass. The intermediate layer may contain various additives depending on the purpose.

[0039] The thickness of the intermediate layer is not particularly limited, and may be, for example, 1 μm or more and 50 μm or less, or 5 μm or more and 50 μm or less.

[0040] (Release agent layer) When the release agent layer is formed from a silicone-based release agent, the adhesion between the release agent layer and the thermoplastic resin layer becomes too low. Therefore, in order to obtain an appropriate pseudo-adhesion between the release agent layer and the thermoplastic resin layer, an olefin release agent containing a polyolefin resin composition is used for the release agent layer of the release sheet of the pattern sheet according to the present embodiment.

[0041] The polyolefin resin composition contained in the olefin release agent may be, for example, a resin composition containing a polyolefin thermoplastic resin having a structural unit derived from an olefin having 2 to 10 carbon atoms. Specifically, the polyolefin resin composition preferably contains a polyolefin thermoplastic resin having at least one structural unit selected from the group consisting of a structural unit derived from ethylene, a structural unit derived from propylene, a structural unit derived from butene, a structural unit derived from hexene, a structural unit derived from octene, and a structural unit derived from 4-methyl-1-pentene. In this specification, the polyolefin resin composition is composed of a polyolefin thermoplastic resin.

[0042] The polyolefin thermoplastic resin may be a homopolymer having any one of structural units selected from the group consisting of ethylene, propylene, butene, hexene, octene, and 4-methyl-1-pentene, or a copolymer having at least one structural unit selected from the group consisting of ethylene, propylene, butene, hexene, octene, and 4-methyl-1-pentene. The polyolefin resin composition may be a mixture of these homopolymers and copolymers.

[0043] From the viewpoint of easily obtaining an appropriate pseudo-adhesion between the release agent layer and the thermoplastic resin layer, the polyolefin resin composition preferably contains a polyolefin thermoplastic resin having a structural unit derived from ethylene. Examples of the polyolefin thermoplastic resin having a structural unit derived from ethylene include a homopolymer having a structural unit derived from ethylene, and a copolymer having a structural unit derived from ethylene and a structural unit derived from an α-olefin having 3 to 10 carbon atoms. The polyolefin resin composition may be a mixture of these homopolymers and these copolymers.

[0044] From the viewpoint of making it easier to obtain a suitable pseudo-adhesion between the release agent layer and the thermoplastic resin layer, the polyolefin resin composition is preferably a mixture of a copolymer having a structural unit derived from ethylene and a structural unit derived from at least one selected from the group consisting of propylene, butene, hexene, octene, and 4-methyl-1-pentene, and polyethylene. Among these, from the viewpoint of making it easier to obtain a suitable pseudo-adhesion between the release agent layer and the thermoplastic resin layer, the polyolefin resin composition is more preferably a mixture of a copolymer containing a structural unit derived from ethylene and a structural unit derived from butene, and polyethylene. From the same viewpoint, the polyolefin resin composition is also more preferably a mixture of a copolymer containing a structural unit derived from ethylene and a structural unit derived from octene, and polyethylene. When the polyolefin resin composition contains polyethylene, the polyethylene may be any of low density polyethylene, medium density polyethylene, and high density polyethylene. The polyethylene contained in the polyolefin resin composition is preferably low density polyethylene.

[0045] In this specification, a density of 0.91 g / cm 3 More than 0.93g / cm 3 Low density polyethylene is polyethylene with a density of less than 0.93g / cm 3 More than 0.942g / cm 3 Polyethylene with a density of less than 0.942 g / cm is called medium density polyethylene, and 3 More than 0.97g / cm 3 The following polyethylene is referred to as high-density polyethylene. The density of polyethylene can be measured in accordance with JIS K7112:1999.

[0046] The density of a copolymer having a structural unit derived from ethylene and a structural unit derived from at least one selected from the group consisting of propylene, butene, hexene, octene, and 4-methyl-1-pentene is 0.80 g / cm 3 It is preferable that the content is 0.805 g / cm or more. 3 More preferably, it is equal to or greater than this. The density of a copolymer having a structural unit derived from ethylene and a structural unit derived from at least one selected from the group consisting of propylene, butene, hexene, octene, and 4-methyl-1-pentene is 0.91 g / cm 3 Preferably, it is less than 0.905 g / cm 3 More preferably, it is 0.90 g / cm or less. 3 It is even more preferable that: The density of a copolymer having a structural unit derived from ethylene and a structural unit derived from at least one selected from the group consisting of propylene, butene, hexene, octene, and 4-methyl-1-pentene can be measured in accordance with JIS K7112:1999.

[0047] In the pattern sheet according to this embodiment, when the thermoplastic resin layer is a thermoplastic resin layer formed in a pattern as described below, when the pattern sheet according to this embodiment is attached to an adhesive sheet, a part where the adhesive layer and the thermoplastic resin layer are attached and a part where the adhesive layer and the release agent layer are attached are generated. Therefore, from the viewpoint that the release agent layer is more likely to obtain a suitable pseudo-adhesion to the thermoplastic resin layer and is more likely to obtain excellent releasability to the adhesive layer, it is preferable that the polyolefin resin composition contained in the olefin release agent contains a polyolefin thermoplastic resin having at least one structural unit selected from the group consisting of a structural unit derived from ethylene, a structural unit derived from propylene, a structural unit derived from butene, a structural unit derived from hexene, a structural unit derived from octene, and a structural unit derived from 4-methyl-1-pentene.

[0048] From the same viewpoint, the polyolefin resin composition contained in the olefin release agent is preferably a mixture of a copolymer having a structural unit derived from ethylene and a structural unit derived from at least one selected from the group consisting of propylene, butene, hexene, octene, and 4-methyl-1-pentene, and polyethylene. Among these, the polyolefin resin composition is more preferably a mixture of a copolymer containing a structural unit derived from ethylene and a structural unit derived from butene, and polyethylene, or a mixture of a copolymer containing a structural unit derived from ethylene and a structural unit derived from octene, and polyethylene.

[0049] When the polyolefin resin composition is a mixture of a copolymer having a structural unit derived from ethylene and a structural unit derived from at least one selected from the group consisting of propylene, butene, hexene, octene, and 4-methyl-1-pentene, and polyethylene, the mixing ratio of the copolymer and polyethylene (copolymer:polyethylene) is preferably in the range of 10:90 to 90:10, more preferably in the range of 20:80 to 80:20, by mass ratio. If the mixing ratio of the copolymer and polyethylene is in the range of 10:90 to 90:10, the pseudo-adhesion between the release agent layer and the thermoplastic resin layer is more easily obtained. In addition, if the mixing ratio of the copolymer and polyethylene is in the range of 10:90 to 90:10, when it comes into contact with the pressure-sensitive adhesive layer, it has excellent releasability from the pressure-sensitive adhesive layer.

[0050] The polyolefin resin composition preferably has a melt flow rate (MFR) of 1 g / 10 min or more and 20 g / 10 min or less. The polyolefin resin composition more preferably has a MFR of 3 g / 10 min or more. The polyolefin resin composition more preferably has a MFR of 15 g / 10 min or less. The MFR of the polyolefin resin composition used in the release agent layer is measured under the measurement conditions of a temperature of 190° C. and a load of 2.16 kg in accordance with JIS K 7210-1:2011.

[0051] The thickness of the release agent layer is not particularly limited, and is preferably, for example, 3 μm or more and 50 μm or less. The thickness of the release agent layer is more preferably 5 μm or more, and further preferably 10 μm or more. The thickness of the release agent layer is more preferably 40 μm or less, and further preferably 35 μm or less.

[0052] The content of the polyolefin resin composition contained in the olefin release agent is preferably 95% by mass or more and 100% by mass or less based on the total amount of the olefin release agent. The olefin release agent may contain an olefin compound such as a low molecular weight olefin wax in addition to the polyolefin resin composition. From the viewpoint of more easily obtaining pseudo-adhesion between the release agent layer and the thermoplastic resin layer, it is preferable that the olefin release agent does not contain an olefin compound other than the polyolefin resin composition. It is more preferable that the olefin release agent is composed of a polyolefin resin composition.

[0053] The content of the olefin release agent in the release agent layer is preferably 90% by mass or more and 100% by mass or less, more preferably 95% by mass or more, and even more preferably 99% by mass or more, based on the total amount of the release agent layer.

[0054] The release agent layer may contain various additives such as fillers, plasticizers, and stabilizers, as long as the adhesiveness to the release substrate and the pseudo-adhesion between the release agent layer and the thermoplastic resin layer are not impaired. The release agent layer may contain other resins in addition to the polyolefin resin composition, as long as the pseudo-adhesion between the release agent layer and the thermoplastic resin layer is not impaired. An example of the other resin is a silicone resin. From the viewpoint of more easily obtaining the pseudo-adhesion between the release agent layer and the thermoplastic resin layer, the content of the silicone resin in the release agent layer is preferably 0% by mass or more and 1% by mass or less based on the total amount of the release agent layer. From the same viewpoint, it is preferable that the release agent layer does not contain a silicone resin.

[0055] <Thermoplastic resin layer> The thermoplastic resin layer is provided directly on and in contact with the release agent layer of the release sheet. The thermoplastic resin layer is pseudo-adhered to the release agent layer, and the interface between the release agent layer and the thermoplastic resin layer is a pseudo-adhesion interface. The thermoplastic resin layer includes a polyolefin resin. The thermoplastic resin layer may be the same as or different from the polyolefin resin composition contained in the release agent layer, so long as it can pseudo-adhere to the release agent layer and has excellent adhesion to the adhesive layer of the adhesive sheet. In order to more easily obtain pseudo-adhesion between the release agent layer and the thermoplastic resin layer and to have excellent adhesion to the adhesive layer of the adhesive sheet, it is preferable that the thermoplastic resin layer is different from the polyolefin resin composition contained in the release agent layer.

[0056] In the pattern sheet according to this embodiment, the pseudo-adhesion strength when peeled off at the pseudo-adhesion interface, that is, the pseudo-adhesion strength of the thermoplastic resin layer to the release agent layer, is 50 mN / 50 mm or more and 1000 mN / 50 mm or less. The pseudo-adhesion strength of the thermoplastic resin layer to the release agent layer is preferably 60 mN / 50 mm or more, and more preferably 80 mN / 50 mm or more. The pseudo-adhesion strength of the thermoplastic resin layer to the release agent layer is preferably 950 mN / 50 mm or less, more preferably 600 mN / 50 mm or less, and even more preferably 300 mN / 50 mm or less.

[0057] If the pseudo-adhesion strength of the thermoplastic resin layer to the release agent layer is 50 mN / 50 mm or more, the thermoplastic resin layer can be prevented from unintentionally peeling off from the release agent layer. In addition, since the thermoplastic resin layer has an appropriate adhesion strength to the release agent layer, the adhesive layer of the adhesive sheet has excellent processability when the adhesive layer is subjected to a glue-killing treatment. Therefore, the non-adhesive portion can be easily formed on the adhesive layer. If the pseudo-adhesion strength of the thermoplastic resin layer to the release agent layer is 1000 mN / 50 mm or less, the thermoplastic resin layer has excellent releasability when separated from the release agent layer of the release sheet, and therefore the adhesive layer of the adhesive sheet has excellent processability when the adhesive layer is subjected to a glue-killing treatment, and a non-adhesive portion can be easily formed in the adhesive layer. The pseudo-adhesion strength of the thermoplastic resin layer to the release agent layer can be measured by the method described in the examples below.

[0058] The polyolefin resin is not particularly limited, and examples of the polyolefin resin include polymers obtained by polymerizing monomers containing an olefin monomer having 2 to 18 carbon atoms.

[0059] Examples of the polyolefin resin include homopolymers of olefin monomers such as ethylene, propylene, butene, hexene, octene, decene, and 4-methyl-1-pentene. Examples of the polyolefin resin include copolymers of olefin monomers selected from the group consisting of ethylene, propylene, butene, hexene, octene, decene, and 4-methylpentene. Examples of the copolymers of olefin monomers include copolymers of ethylene and α-olefins having 3 to 18 carbon atoms (for example, at least one olefin monomer selected from the group consisting of propylene, butene, hexene, octene, decene, and 4-methylpentene). The copolymers of olefin monomers may be a combination of two or more olefin monomers. The polyolefin resin may be a single resin or a combination of two or more resins.

[0060] Examples of polyolefin resins include copolymers of one or more olefin monomers such as ethylene, propylene, butene, hexene, octene, and 4-methyl-1-pentene with one or more monomers having a hydroxyl group, a carboxyl group, a vinyl acetate structure, an acid anhydride structure, or the like.

[0061] Specific examples of the polyolefin resin include at least one selected from the group consisting of polyethylene (low density polyethylene, medium density polyethylene, high density polyethylene, etc.), polypropylene, poly-1-butene, poly-2-butene, poly-1-hexene, poly-1-octene, poly(4-methyl-1-pentene), ethylene-propylene copolymer, ethylene-vinyl acetate copolymer, ethylene-(meth)acrylic acid copolymer, and ethylene-(meth)acrylic acid ester copolymer.

[0062] Among these, the polyolefin resin is preferably a resin having at least one of a structural unit derived from ethylene and a structural unit derived from propylene. Specifically, the polyolefin resin is more preferably at least one selected from the group consisting of polyethylene, polypropylene, and an ethylene-vinyl acetate copolymer, and further preferably at least one selected from the group consisting of polyethylene and polypropylene. When polyethylene is used as the polyolefin resin, the polyolefin resin is preferably low-density polyethylene.

[0063] When the polyolefin resin contained in the thermoplastic resin layer and the polyolefin resin composition contained in the release agent layer are different, the polyolefin resin contains either a homopolymer of an olefin monomer or a copolymer polymerized from a monomer containing an olefin monomer, and the polyolefin resin composition may contain both a copolymer polymerized from a monomer containing an olefin monomer and a homopolymer of an olefin monomer. The polyolefin resin contains a homopolymer of an olefin monomer, and the polyolefin resin composition may contain both a copolymer polymerized from a monomer containing an olefin monomer and a homopolymer of an olefin monomer. The olefin monomer of the polymer contained in the polyolefin resin may be an olefin monomer having a carbon number of 2 or more and 18 or less. The olefin monomer of the polymer contained in the polyolefin resin composition may be an olefin monomer having a carbon number of 2 or more and 10 or less. Specific combinations of the polyolefin resin and the polyolefin resin composition are preferably, for example, the following combinations.

[0064] The polyolefin resin is preferably a resin having at least one of a structural unit derived from ethylene and a structural unit derived from propylene, and the polyolefin resin composition is preferably a mixture of polyethylene and a copolymer having a structural unit derived from ethylene and a structural unit derived from at least one selected from the group consisting of propylene, butene, hexene, octene, and 4-methyl-1-pentene. The polyolefin resin is at least one selected from the group consisting of polyethylene, polypropylene, and ethylene-vinyl acetate copolymer, and the polyolefin resin composition is more preferably a mixture of a copolymer containing structural units derived from ethylene and structural units derived from butene and polyethylene, or a mixture of a copolymer containing structural units derived from ethylene and structural units derived from octene and polyethylene. It is more preferable that the polyolefin resin is low-density polyethylene or polypropylene, and the polyolefin resin composition is a mixture of an ethylene-1-butene copolymer and low-density polyethylene or a mixture of an ethylene-1-hexene copolymer and low-density polyethylene.

[0065] In addition, when the release sheet has an intermediate layer, for example, the intermediate layer may contain low-density polyethylene, the release agent layer may contain a mixture of an ethylene-1-butene copolymer and low-density polyethylene or a mixture of an ethylene-1-hexene copolymer and low-density polyethylene, and the thermoplastic resin layer may contain low-density polyethylene or polypropylene.

[0066] The density of the polyolefin resin is not particularly limited and is, for example, 0.85 g / cm 3 More than 0.97g / cm 3 It is preferable that the density of the polyolefin resin is not more than 1. The density of the polyolefin resin can be measured in accordance with JIS K7112:1999.

[0067] The thermoplastic resin layer is a layer for forming a non-adhesive portion in the adhesive layer of the adhesive sheet by being attached to the adhesive layer of the adhesive sheet and then peeled off from the release layer of the release sheet. From the viewpoint of providing an appropriate thickness for the non-adhesive portion, the thickness of the thermoplastic resin layer is not particularly limited, and is preferably, for example, 3 μm or more and 50 μm or less. The thickness of the thermoplastic resin layer is more preferably 5 μm or more, and further preferably 10 μm or more. The thickness of the thermoplastic resin layer is more preferably 40 μm or less, and further preferably 35 μm or less.

[0068] The content of the polyolefin resin in the thermoplastic resin layer is preferably 90 mass% or more, more preferably 95 mass% or more, even more preferably 99 mass% or more, and even more preferably 100 mass%, based on the total amount of the thermoplastic resin layer.

[0069] The thermoplastic resin layer may contain additives, if necessary, in addition to the polyolefin resin. Examples of additives include antioxidants, lubricants, ultraviolet absorbers, colorants, and antiblocking agents. When the thermoplastic resin layer contains an additive, the additive may be contained alone or may contain two or more types. The thermoplastic resin layer may be required to have low visibility as a non-adhesive part. In this case, the thermoplastic resin layer is preferably transparent. For this reason, the thermoplastic resin layer preferably does not contain additives that reduce transparency. Here, transparency means that at least visible light is transmitted, and specifically, for example, means that the thermoplastic resin layer has a total light transmittance of 50% or more as specified in JIS K7361-1:1997.

[0070] The thermoplastic resin layer is preferably formed in a pattern so that a part of the release agent layer is exposed (for example, see FIG. 6 described later as an example of a pattern sheet having a thermoplastic resin layer formed in a pattern). When the thermoplastic resin layer formed in a pattern and the exposed release agent layer are attached to an adhesive sheet, the peel force of the release agent layer to the adhesive sheet (i.e., the peel force of the release agent layer to the adhesive layer in the adhesive sheet) is preferably 50 mN / 50 mm or more and 500 mN / 50 mm or less. The peel strength of the release agent layer from the pressure-sensitive adhesive sheet is more preferably 60 mN / 50 mm or more, even more preferably 100 mN / 50 mm or more, and even more preferably 110 mN / 50 mm or more. The peel strength of the release agent layer from the pressure-sensitive adhesive sheet is more preferably 500 mN / 50 mm or less, and even more preferably 200 mN / 50 mm or less. The peel strength of the release agent layer from the pressure-sensitive adhesive sheet can be measured by the method described in the Examples section below.

[0071] When the patterned sheet according to the present embodiment has a thermoplastic resin layer formed in a pattern, it has a portion where the pressure-sensitive adhesive layer and the thermoplastic resin layer are attached and a portion where the pressure-sensitive adhesive layer and the release agent layer are attached. Therefore, if the peel strength of the release agent layer from the pressure-sensitive adhesive sheet is 50 mN / 50 mm or more and 500 mN / 50 mm or less, the release property of the release agent layer from the pressure-sensitive adhesive layer is excellent.

[0072] The pattern shape of the thermoplastic resin layer formed in a pattern is not particularly limited, and may be a pattern shape corresponding to the shape of the intended non-adhesive portion. The pattern shape may be a rectangle, a circle, an ellipse, a polygon, or a combination thereof. The number of pattern shapes may also be provided according to the purpose.

[0073] <Manufacturing method of patterned sheet> An example of a preferred method for producing the pattern sheet according to the present embodiment will be described. The preferred method for producing the pattern sheet according to the present embodiment includes the steps of: obtaining a release sheet having a release agent layer provided thereon by melt-extrusion laminating an olefin release agent containing a polyolefin resin composition on a release substrate; and providing a thermoplastic resin layer containing a polyolefin resin on the surface of the release agent layer of the release sheet opposite to the release substrate by melt-extrusion laminating a polyolefin resin.

[0074] When an intermediate layer is provided between the release substrate and the release agent layer of the release sheet, the process for obtaining the release sheet may include a process for forming an intermediate layer on the release substrate by performing at least one of melt extrusion lamination and coating, and a process for obtaining a release sheet provided with a release agent layer by melt extrusion laminating an olefin release agent containing a polyolefin resin composition on the intermediate layer.

[0075] The step of obtaining the release sheet includes a step of preparing a release substrate and a step of preparing an olefin release agent containing a polyolefin resin composition. The release substrate may be prepared as described above for the release substrate. The release substrate may be obtained by a known manufacturing method. The polyolefin resin composition may be prepared as described above for the release agent layer. The polyolefin resin composition may be obtained by a known manufacturing method. When the polyolefin resin composition includes a copolymer having a structural unit derived from ethylene and a structural unit derived from at least one selected from the group consisting of propylene, butene, hexene, octene, and 4-methyl-1-pentene, the copolymer is preferably a copolymer polymerized using a multi-site catalyst.

[0076] In the process of obtaining a release sheet, the method of melt extrusion laminating the olefin release agent containing the polyolefin resin composition on the release substrate is not particularly limited, and a known method can be adopted. The conditions for providing the release agent layer are not particularly limited as long as the temperature conditions are such that the release agent layer can be formed. For example, the polyolefin resin composition is put into the hopper of an extruder equipped with a T-die, the cylinder temperature and the die temperature are appropriately adjusted according to the type of the polyolefin resin composition, and the film-like melt kneaded product of the polyolefin resin composition is extruded from the T-die and cooled by a cooling roll, thereby forming a release agent layer on the release substrate.

[0077] In the process of obtaining a release sheet, when an intermediate layer is provided by melt extrusion lamination, the intermediate layer can be provided on the release substrate by adjusting the conditions for melt extrusion lamination according to the type of resin used for the intermediate layer, similar to the case of providing a release agent layer. When the intermediate layer is provided by coating, for example, the material used for the intermediate layer can be provided on the release substrate by a known coating method such as bar coating, knife coating, roll knife coating, roll coating, blade coating, die coating, curtain coating, or gravure coating.

[0078] The step of obtaining a release sheet may be a step of providing a release agent layer after subjecting the surface of a release substrate to an easy-adhesion treatment such as corona treatment, plasma treatment, or flame treatment. When an intermediate layer is provided, the step may be a step of providing a release agent layer after subjecting the intermediate layer to an easy-adhesion treatment on the surface of the release substrate to form the intermediate layer, and then subjecting the intermediate layer to an easy-adhesion treatment.

[0079] The step of providing the thermoplastic resin layer includes a step of preparing a polyolefin resin. The polyolefin resin may be the polyolefin resin described above for the thermoplastic resin layer. The polyolefin resin may be obtained by a known manufacturing method.

[0080] In the step of providing a thermoplastic resin layer, the method of melt extrusion laminating a polyolefin resin on the surface of the release agent layer opposite to the release substrate side is not particularly limited, and a known method can be adopted. The conditions for providing a thermoplastic resin layer are not particularly limited as long as the temperature conditions are such that a thermoplastic resin layer can be formed. For example, a thermoplastic resin layer can be obtained as follows. First, a polyolefin resin is charged into a hopper of an extruder equipped with a T-die, and the cylinder temperature and die temperature are appropriately adjusted according to the type of polyolefin resin. Next, a film-like melt kneaded product of the polyolefin resin is extruded from the T-die and cooled by a cooling roll, thereby forming a thermoplastic resin layer on the release agent layer in the release sheet.

[0081] In the step of providing the thermoplastic resin layer, when the thermoplastic resin layer is formed, the surface of the release agent layer in the release sheet may be subjected to an adhesion enhancing treatment such as a corona treatment, a plasma treatment, or a flame treatment.

[0082] When the thermoplastic resin layer is formed in a pattern, a preferred manufacturing method of the patterned sheet according to the present embodiment includes a step of exposing a part of the release agent layer and forming the thermoplastic resin layer in a pattern. The step of forming the thermoplastic resin layer in a pattern can be, for example, a step of forming the thermoplastic resin layer in a pattern by dividing the unnecessary thermoplastic resin layer part and the patterned thermoplastic resin layer part without providing a cut in the release sheet and removing the unnecessary thermoplastic resin layer part. When the thermoplastic resin layer is formed in a pattern, the patterned sheet before the thermoplastic resin layer is formed in a pattern becomes a raw sheet for obtaining a patterned sheet provided with a thermoplastic resin layer formed in a pattern. The patterned sheet provided with a thermoplastic resin layer formed in a pattern can be processed by a roll-to-roll method.

[0083] By going through the above steps, the pattern sheet according to this embodiment is obtained.

[0084] [Adhesive sheet] An example of an adhesive sheet to which the pattern sheet according to the present embodiment is attached will be described below. The adhesive sheet has an adhesive base and an adhesive layer provided on the adhesive base.

[0085] The adhesive sheet to which the pattern sheet according to the present embodiment is attached will be described with reference to the drawings. In the drawings, some parts are illustrated enlarged or reduced in size to facilitate the description. Referring to Fig. 2, a schematic cross-sectional view of an adhesive sheet 30 is shown as an example of the adhesive sheet.

[0086] The adhesive sheet 30 shown in FIG. 2 includes an adhesive base 31 and an adhesive layer 33. The adhesive base 31 has a first adhesive base surface 311 and a second adhesive base surface 312, which is the surface opposite to the first adhesive base surface 311. The adhesive layer 33 is laminated on one surface (first adhesive base surface 311) of the adhesive base 31. In the adhesive sheet 30, the adhesive layer 33 is directly laminated on the adhesive base 31, and the adhesive layer 33 is firmly attached to the adhesive base 31. In the adhesive sheet 30 shown in FIG. 2, the adhesive layer 33 is not provided on the second adhesive base surface 312, and the second adhesive base surface 312 is exposed. The first adhesive layer surface 331 of the adhesive layer 33 is the surface to be attached to a thermoplastic resin layer of a pattern sheet according to this embodiment, not shown.

[0087] Although an example of the adhesive sheet attached to the pattern sheet according to the present embodiment has been described above with reference to Fig. 2, the adhesive sheet is not limited to this. The adhesive sheet may take various forms as long as it has the above-mentioned configuration. For example, the adhesive sheet 30 shown in FIG. 2 may be provided with a printed layer (not shown) on at least one surface of the adhesive substrate 31 (one or both of the first adhesive substrate surface 311 and the second adhesive substrate surface 312). Specifically, for example, the adhesive sheet 30 may be provided with a printed layer on the surface (second adhesive substrate surface 312) opposite to the surface (first adhesive substrate surface 311) of the adhesive substrate 31 on the adhesive layer 33 side. When the printed layer is provided on the adhesive substrate 31, the printed layer may be composed of information such as letters, numbers, figures, symbols, patterns, illustrations, photographs, graphs, and combinations thereof. The printing for forming the printed layer may be monochromatic or multicolor printing. The printed layer is printed by a known printing method. In addition, in the adhesive sheet 30 shown in Figure 2, in order to improve the adhesion between the adhesive substrate 31 and the adhesive layer 33, an easy-adhesion layer (not shown) or the like may be provided between the adhesive substrate 31 and the adhesive layer 33 so as to be in contact with both the first adhesive substrate surface 311 of the adhesive substrate 31 and the second adhesive layer surface 332 of the adhesive layer 33.

[0088] (adhesive base material) The adhesive substrate is a substrate that supports the adhesive layer. The material of the adhesive substrate is not particularly limited, and examples thereof include paper, resin, and metal foil. The adhesive substrate may be one of these materials alone or a combination of two or more. The adhesive substrate may be a resin substrate. The resin substrate is a resin substrate formed of a resin film or the like. The resin substrate also includes a resin substrate called a synthetic paper, such as a foamed plastic film having properties similar to those of paper.

[0089] Examples of resins used in the resin substrate include polyester resins (polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, etc.), polyolefin resins (polyethylene, polypropylene, polybutene, polybutadiene, polymethylpentene, ethylene-norbornene copolymers, norbornene resins, and ethylene copolymers (ethylene-vinyl acetate copolymers, ethylene-(meth)acrylic acid copolymers, and ethylene-(meth)acrylic acid ester copolymers, etc.), polyvinyl chloride resins (polyvinyl chloride and vinyl chloride copolymers, etc.), (meth)acrylic acid ester copolymers, polyurethane, polyamide, polyimide, polystyrene, polycarbonate, fluororesins, and ionomers. The substrate may be a single-layer film of the above resins, or a laminated film in which two or more layers are laminated. When the substrate is a laminated film, the resins of each layer may be the same type of resin or different types of resins.

[0090] The thickness of the adhesive substrate is preferably 5 μm or more, more preferably 10 μm or more, even more preferably 30 μm or more, and even more preferably 50 μm or more. The thickness of the adhesive substrate is preferably 500 μm or less, more preferably 450 μm or less, even more preferably 300 μm or less, even more preferably 250 μm or less, and even more preferably 200 μm or less.

[0091] The adhesive substrate may be printed on a second adhesive substrate surface (the surface opposite to the surface on which the adhesive layer is provided). In order to improve the adhesion of the print, the adhesive substrate may be surface-treated on the second adhesive substrate surface (the surface on which the print is applied).

[0092] (Adhesive layer) The adhesive layer is not particularly limited, and is formed from an adhesive composition containing an adhesive. Examples of the adhesive include acrylic, rubber, silicone, urethane, polyester, and polyvinyl ether adhesives. The adhesive may be selected depending on the application. The adhesive is preferably an acrylic adhesive.

[0093] Acrylic pressure-sensitive adhesives include, for example, polymers or copolymers mainly composed of (1) a main monomer component with a low glass transition temperature (low Tg) that imparts adhesiveness, (2) a comonomer component with a high glass transition temperature (high Tg) that imparts at least one of adhesive properties and cohesive strength, and (3) a functional group-containing monomer component for crosslinking or improving adhesiveness.

[0094] (1) Main monomer component Examples of the main monomer component include (meth)acrylic acid esters. Specific examples of the (meth)acrylic acid esters include methyl acrylate, ethyl acrylate, butyl acrylate, amyl acrylate, 2-ethylhexyl acrylate, octyl acrylate, cyclohexyl acrylate, benzyl acrylate, butyl methacrylate, 2-ethylhexyl methacrylate, cyclohexyl methacrylate, and benzyl methacrylate.

[0095] In this specification, "(meth)acrylic" refers to both acrylic and methacrylic, as well as other similar terms.

[0096] (2) Comonomer component The comonomer components include methyl (meth)acrylate, ethyl (meth)acrylate, vinyl acetate, styrene, and acrylonitrile.

[0097] (3) Functional group-containing monomer component Examples of functional group-containing monomer components include carboxyl group-containing monomers such as (meth)acrylic acid, maleic acid, and itaconic acid; hydroxyl group-containing monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and N-methylol acrylamide; (meth)acrylamide; and glycidyl (meth)acrylate.

[0098] By selecting the type of monomer, molecular weight, etc., it is possible to obtain qualities and characteristics suited to the application.

[0099] The acrylic adhesive may be either a crosslinked type or a non-crosslinked type. When the acrylic adhesive is a crosslinking type, examples of the crosslinking agent include various crosslinking agents such as epoxy compounds, isocyanate compounds, metal chelate compounds, metal alkoxides, metal salts, amine compounds, hydrazine compounds, and aldehyde compounds. When the acrylic adhesive is a crosslinking type, examples of the crosslinking agent include a method of crosslinking by irradiation with radiation.

[0100] The pressure-sensitive adhesive layer may contain various additives, such as a tackifier, a plasticizer, a filler, an antioxidant, a dye, and a pigment, as required.

[0101] The thickness of the pressure-sensitive adhesive layer is not particularly limited, and is, for example, preferably 5 μm or more and 200 μm or less, and more preferably 10 μm or more and 100 μm or less.

[0102] The adhesive sheet can be obtained, for example, by a manufacturing method including a step of preparing an adhesive substrate and a step of providing an adhesive layer on the adhesive substrate. The step of providing an adhesive layer on the adhesive substrate can be, for example, by applying an adhesive composition to the adhesive substrate to form an adhesive layer. In addition, the step of providing an adhesive layer on the adhesive substrate can be, first, by preparing a release sheet for preparing an adhesive sheet. Next, the adhesive composition is applied to the releasable surface of the release sheet for preparing an adhesive sheet to form an adhesive layer, and then the adhesive substrate is laminated on the adhesive layer. Next, the adhesive layer is transferred to the adhesive substrate. In such a step, an adhesive layer can also be formed on the adhesive substrate.

[0103] The method for applying the pressure-sensitive adhesive composition is not particularly limited, and known methods such as gravure coating, bar coating, spray coating, spin coating, knife coating, roll coating, and die coating can be used.

[0104] [Pattern sheet usage] According to the pattern sheet of this embodiment, the pattern sheet has a suitable pseudo-adhesion with the release agent layer, has excellent processability when performing glue-killing treatment on the adhesive layer, and is easy to maintain the effect of losing adhesive force. Therefore, the pattern sheet of this embodiment can be applied to various applications requiring glue-killing treatment. Examples of applications requiring glue-killing treatment include various labels such as tag labels, protective labels, and POP (Point Of Purchase) labels (POP labels are also called eye-catching labels and attention labels, etc.), sticky note sheets, and process papers for temporarily fixing parts. The applications of the pattern sheet of this embodiment are not limited to the applications requiring glue-killing treatment listed above, but can also be applied to other applications requiring glue-killing treatment. In addition, the pattern sheet of this embodiment is not limited to applications requiring glue-killing treatment, but can also be applied to various applications not requiring glue-killing treatment.

[0105] [How to use the pattern sheet] A preferred embodiment of a method for using the pattern sheet according to this embodiment will now be described.

[0106] <First aspect> A first aspect of the method for using the pattern sheet according to this embodiment includes the following steps. (Step P1-1) A step of preparing a pattern sheet according to this embodiment. (Step P1-2) A step of preparing an adhesive sheet. (Step P1-3) A step of attaching the thermoplastic resin layer of the pattern sheet to the adhesive sheet, and laminating the adhesive sheet, the thermoplastic resin layer, and the release sheet of the pattern sheet in this order. In a first aspect of the method of using the pattern sheet according to this embodiment, when the pattern sheet is separated from the adhesive sheet, the thermoplastic resin layer is separated from the release agent layer and remains on the adhesive sheet as a non-adhesive portion that causes the adhesive sheet to lose its adhesiveness.

[0107] Hereinafter, a first embodiment of the method for using the pattern sheet according to the present embodiment will be described with reference to the drawings. In the drawings, some parts are shown enlarged or reduced in size to facilitate explanation. Referring to Figures 3 and 4, Figures 3 and 4 show a schematic process diagram of one embodiment using the pattern sheet according to the present embodiment.

[0108] In step P1-1, a pattern sheet according to this embodiment is prepared. The pattern sheet according to this embodiment may be the pattern sheet described above in the pattern sheet section. In FIG. 3, the pattern sheet 100 described in FIG. 1 is prepared, and the pattern sheet 100 is used. The pattern sheet 100 includes a release sheet 10 including a release substrate 11 and a release agent layer 13 provided on the release substrate 11, and a thermoplastic resin layer 20 provided on the release sheet 10.

[0109] In step P1-2, an adhesive sheet to which the pattern sheet according to the present embodiment is attached is prepared. The adhesive sheet may be the adhesive sheet described above in the adhesive sheet. In FIG. 3, the adhesive sheet 30 described in FIG. 2 is prepared, and the adhesive sheet 30 is used. The adhesive sheet 30 includes an adhesive base material 31 and an adhesive layer 33 provided on the adhesive base material 31. The adhesive sheet 30 may have a printed layer on at least one surface of the adhesive base material 31. The adhesive sheet 30 may have a printed layer, for example, on the surface (second adhesive base surface 312) on which the adhesive layer 33 is not provided.

[0110] In step P1-3, the pattern sheet according to the present embodiment prepared in step P1-1 is attached to the adhesive sheet prepared in step P1-2. FIG. 3 shows an adhesive body 400 in a state in which the pattern sheet 100 and the adhesive sheet 30 are attached to each other. The adhesive body 400 shown in FIG. 3 is obtained by attaching the thermoplastic resin layer 20 to the adhesive layer 33 so that the first thermoplastic resin layer surface 201 of the thermoplastic resin layer 20 in the pattern sheet 100 faces the first adhesive layer surface 331 of the adhesive layer 33 in the adhesive sheet 30. In the adhesive body 400, the pattern sheet 100 is attached to a part of the first adhesive layer surface 331 of the adhesive layer 33. When the pattern sheet 100 is attached to the adhesive sheet 30, the adhesive body 400 is laminated in the order of the adhesive sheet 30, the thermoplastic resin layer 20, and the release sheet 10. Specifically, the adhesive body 400 has an adhesive substrate 31, an adhesive layer 33, a thermoplastic resin layer 20, a release agent layer 13, and a release substrate 11 laminated in this order in the thickness direction.

[0111] In the adhesive body 400, the thermoplastic resin layer 20 is pseudo-adhered to the release agent layer 13 of the release sheet 10, and the interface between the release agent layer 13 and the thermoplastic resin layer 20 is a pseudo-adhesion interface. Therefore, the adhesive body 400 can be separated between the thermoplastic resin layer 20 and the release agent layer 13 in the pattern sheet 100. When the adhesive body 400 is separated in the direction of the arrow R1 shown in FIG. 3, the adhesive body 400 is separated between the second thermoplastic resin layer surface 202 of the thermoplastic resin layer 20 and the first release agent layer surface 131 of the release agent layer 13. The separated thermoplastic resin layer 20 remains on the adhesive layer 33 of the adhesive sheet 30 with the first thermoplastic resin layer surface 201 still attached to the first adhesive layer surface 331 of the adhesive layer 33.

[0112] FIG. 4 shows an adhesive body 401 in a state where the thermoplastic resin layer 20 remains on the adhesive layer 33 after the pattern sheet 100 shown in FIG. 3 is separated from the adhesive sheet 30. The adhesive body 401 shown in FIG. 4 includes an adhesive sheet 30 and a thermoplastic resin layer 20 remaining on the adhesive layer 33 of the adhesive sheet 30. The adhesive layer 33 has an adhesive portion 333 where the first adhesive layer surface 331 is exposed, and a non-adhesive portion 335 where the second thermoplastic resin layer surface 202 of the thermoplastic resin layer 20 is exposed. The thermoplastic resin layer 20 functions as the non-adhesive portion 335 that causes the adhesive sheet 30 to lose its adhesiveness by remaining on the adhesive layer 33 of the adhesive sheet 30. In FIG. 4, the thickness of the adhesive layer 33 in the adhesive portion 333 is shown to be equal to the thickness of the adhesive layer 33 in the non-adhesive portion 335, but is not limited thereto. The thickness of the adhesive layer 33 in the adhesive portion 333 may be thicker than the thickness of the adhesive layer 33 in the non-adhesive portion 335. For example, the thickness of the adhesive layer 33 in the adhesive portion 333 may be approximately the sum of the thickness of the thermoplastic resin layer 20 and the thickness of the adhesive layer 33 in the non-adhesive portion 335.

[0113] The pattern sheet 100 used in the first embodiment has a pseudo-adhesion with an appropriate adhesive strength between the thermoplastic resin layer 20 and the release agent layer 13. Therefore, according to the first embodiment of the method for using the pattern sheet according to the present embodiment, the adhesive layer 33 of the adhesive sheet 30 has excellent processability when the adhesive layer 33 is subjected to a glue-killing treatment, and the adhesive layer 33 can be easily provided with a non-adhesive portion 335. Furthermore, since the non-adhesive portion 335 provided on the adhesive layer 33 is provided by the thermoplastic resin layer 20, the effect of losing the adhesive force is likely to be sustained.

[0114] <Second aspect> A second aspect of the method for using the pattern sheet according to this embodiment includes the following steps. (Step P2-1) A step of preparing a pattern sheet according to this embodiment. (Step P2-2) A step of punching out the pattern sheet, leaving no cuts in the release sheet of the pattern sheet, and cutting the thermoplastic resin layer of the pattern sheet, thereby separating the unnecessary thermoplastic resin layer portion from the thermoplastic resin layer pattern portion. (Step P2-3) A step of removing unnecessary portions of the thermoplastic resin layer to expose a part of the first release agent layer surface of the release agent layer, thereby forming the thermoplastic resin layer in a pattern. (Step P2-4) A step of preparing an adhesive sheet. (Step P2-5) A step of attaching the thermoplastic resin layer formed in a pattern to the adhesive sheet, and laminating the adhesive sheet, the thermoplastic resin layer formed in a pattern, and the release sheet in that order. In a second aspect of the method of using the patterned sheet according to this embodiment, when the release sheet is separated from the adhesive sheet, the thermoplastic resin layer formed in a pattern is separated from the release agent layer and remains on the adhesive sheet as a non-adhesive portion that causes the adhesive sheet to lose its adhesiveness.

[0115] In step P2-2, "no slits are provided in the release sheet" means that no slits are provided in the release sheet, and also includes slits that are unavoidable when punching. For example, slits are provided from the first release agent layer surface toward the release substrate in the thickness direction of the release agent layer, in an area of ​​about 1 / 10 or less of the entire thickness of the release agent layer, to the extent that they do not affect the releasability between the thermoplastic resin layer and the release agent layer and do not cause the release sheet to break.

[0116] The second embodiment differs from the first embodiment in that the pattern sheet used in the first embodiment is punched to separate the unnecessary thermoplastic resin layer portion from the patterned thermoplastic resin layer portion, and the unnecessary thermoplastic resin layer portion is removed to form the thermoplastic resin layer in a pattern shape. Steps P2-1 and P2-4 in the second embodiment are similar to steps P1-1 and P1-2 in the first embodiment, and therefore will not be described.

[0117] Hereinafter, a second embodiment of the method for using the pattern sheet according to the present embodiment will be described with reference to the drawings. In the drawings, some parts are shown enlarged or reduced in size to facilitate explanation. With reference to Fig. 5 to Fig. 8, Fig. 5 to Fig. 8 show a schematic process diagram of one embodiment using the pattern sheet according to the present embodiment.

[0118] In step P2-2, the pattern sheet 100 prepared in step P2-1 is punched. As shown in FIG. 5, when the pattern sheet 100 is punched, the thermoplastic resin layer 20 of the pattern sheet 100 has a slit 20X. On the other hand, after the punching, the release sheet 10 of the pattern sheet 100 does not have a slit 20X. The pattern sheet 100 is punched in the thickness direction of the thermoplastic resin layer 20 from the first thermoplastic resin layer surface 201 toward the release sheet 10. The slit 20X reaches the second thermoplastic resin layer surface 202 and extends from the first thermoplastic resin layer surface 201 to the second thermoplastic resin layer surface 202. The punching may be performed using a known processing device equipped with a punching means.

[0119] By punching the thermoplastic resin layer 20, an unnecessary thermoplastic resin layer portion 20Z and a thermoplastic resin layer pattern portion 20A are partitioned by a cut 20X. The dimensions of the thermoplastic resin layer pattern portion 20A and the dimensions of the unnecessary thermoplastic resin layer portion 20Z may be determined according to the desired dimensions.

[0120] In step P2-3, a scrap is removed to remove the unnecessary portion 20Z of the thermoplastic resin layer partitioned in step P2-2. By performing this scrap removal, a part of the first release agent layer surface 131 of the release agent layer 13 is exposed, and the thermoplastic resin layer 20 is formed in a pattern. The scrap removal may be performed using a known processing device equipped with a scrap removal means. Steps P2-2 and P2-3 may be performed using a processing device equipped with a punching means and a scrap removal means.

[0121] FIG. 6 shows the patterned sheet 101 after the step P2-3. The patterned sheet 101 shown in FIG. 6 shows a patterned sheet 101 in which a thermoplastic resin layer 21 formed in a pattern is laminated on a release sheet 10 having a release agent layer 13 provided on a release substrate 11. The thermoplastic resin layer 21 formed in a pattern is laminated in direct contact with the first release agent layer surface 131 of the release agent layer 13. The contact surface between the first release agent layer surface 131 of the release agent layer 13 and the second thermoplastic resin layer surface 212 of the thermoplastic resin layer 21 is a pseudo-adhesive surface. The thermoplastic resin layer 21 has thermoplastic resin layer pattern portions 20A provided intermittently at intervals. The first release agent layer surface 131 is exposed between adjacent thermoplastic resin layer pattern portions 20A.

[0122] Step P2-5 is substantially the same as step P1-3 in the first embodiment, but differs from the first embodiment in that a patterned sheet 101 having a thermoplastic resin layer 21 formed in a pattern is used. In step P2-5, the patterned sheet 101 is attached such that the first thermoplastic resin layer surface 211 of the thermoplastic resin layer 21 formed in a pattern faces the adhesive layer 33 of the adhesive sheet 30 prepared in step P2-4. When the patterned sheet 101 is attached to the adhesive sheet 30, it may be attached by being pressed, or may be attached without being pressed.

[0123] FIG. 7 shows an adhesive body 403 in a state where the pattern sheet 101 and the adhesive sheet 30 are attached. The adhesive body 403 shown in FIG. 7 is obtained by attaching the thermoplastic resin layer 21 toward the adhesive layer 33 so that the first thermoplastic resin layer surface 211 and the first release agent layer surface 131 of the thermoplastic resin layer 21 formed in a pattern shape in the pattern sheet 101 face the first adhesive layer surface 331 of the adhesive layer 33 in the adhesive sheet 30. In the adhesive body 403, when the thermoplastic resin layer 21 is attached toward the adhesive layer 33, it is attached by being pressed. When the pattern sheet 101 is attached to the adhesive sheet 30, the adhesive body 403 is formed by laminating the adhesive sheet 30, the thermoplastic resin layer 21, and the release sheet 10 in this order. Specifically, the adhesive body 403 is formed by sequentially laminating an adhesive substrate 31, an adhesive layer 33, a thermoplastic resin layer 21 formed in a pattern, a release agent layer 13, and a release substrate 11 in this order in the thickness direction.

[0124] In the adhesive body 403, the thermoplastic resin layer 21 is pseudo-adhered to the release agent layer 13 of the release sheet 10, and the interface between the release agent layer 13 and the thermoplastic resin layer 21 is a pseudo-adhesion interface. Therefore, the adhesive body 403 can be separated between the thermoplastic resin layer 21 formed in a pattern and the release agent layer 13. When the adhesive body 403 is separated, the adhesive body 403 is separated between the second thermoplastic resin layer surface 212 of the thermoplastic resin layer 21 and the first release agent layer surface 131 of the release agent layer 13. The separated thermoplastic resin layer 21 remains on the adhesive layer 33 of the adhesive sheet 30 with the first thermoplastic resin layer surface 211 still attached to the first adhesive layer surface 331 of the adhesive layer 33. The thermoplastic resin layer 21 is formed by the thermoplastic resin layer pattern portion 20A.

[0125] FIG. 8 shows an adhesive body 405 in a state where the thermoplastic resin layer 21 remains on the adhesive layer 33 after the pattern sheet 101 shown in FIG. 7 is separated from the adhesive sheet 30. The adhesive body 405 shown in FIG. 8 includes an adhesive sheet 30 and a thermoplastic resin layer 21 formed in a pattern shape remaining on the adhesive layer 33 of the adhesive sheet 30. The adhesive layer 33 has an adhesive portion 333 where the first adhesive layer surface 331 is exposed, and a non-adhesive portion 335 where the second thermoplastic resin layer surface 212 of the thermoplastic resin layer 21 formed in a pattern shape is exposed. The separated thermoplastic resin layer 21 remains on the adhesive layer 33 of the adhesive sheet 30, thereby functioning as a non-adhesive portion 335 that causes the adhesive sheet 30 to lose its adhesiveness. In FIG. 8, the thickness of the adhesive layer 33 in the adhesive portion 333 is shown as the total thickness of the adhesive layer 33 and the thermoplastic resin layer 21 in the non-adhesive portion 335, but is not limited thereto. The thickness of the adhesive layer 33 in the adhesive portion 333 may be smaller than the total thickness of the adhesive layer 33 in the non-adhesive portion 335 and the thickness of the thermoplastic resin layer 21 .

[0126] The pattern sheet 101 used in the second embodiment has pseudo-adhesion, which is an appropriate adhesive strength between the thermoplastic resin layer 21 and the release agent layer 13. Therefore, according to the second embodiment of the method of using the pattern sheet according to the present embodiment, the non-adhesive portion 335 can be easily provided in the adhesive layer 33 of the adhesive sheet 30, similarly to the above-described first embodiment. Moreover, similarly to the first embodiment described above, the non-adhesive portion 335 tends to maintain the effect of losing adhesive force. Furthermore, since the pattern sheet 101 used in the second embodiment includes the thermoplastic resin layer 21 formed in a pattern, the release agent layer 13 and the adhesive layer 33 come into contact with each other in the adhesive body 405 in which the pattern sheet 101 is attached to the adhesive sheet 30. When the release agent layer 13 is peeled off from the adhesive layer 33 at the location where the release agent layer 13 and the adhesive layer 33 come into contact with each other, the release agent layer 13 has excellent releasability with respect to the adhesive layer 33.

[0127] <Third Aspect> A third aspect of the method for using the pattern sheet according to this embodiment includes the following steps. (Step P3-1) A step of preparing a pattern sheet according to this embodiment. (Step P3-2) A step of punching out the pattern sheet, leaving no cuts in the release sheet of the pattern sheet, and cutting the thermoplastic resin layer of the pattern sheet, thereby separating the unnecessary thermoplastic resin layer portion from the thermoplastic resin layer pattern portion. (Step P3-3) A step of removing unnecessary portions of the thermoplastic resin layer to expose a part of the first release agent layer surface of the release agent layer, thereby forming the thermoplastic resin layer in a pattern. (Step P3-4) A step of preparing an adhesive sheet. (Step P3-5) A step of attaching the thermoplastic resin layer formed in a pattern to the adhesive sheet to form a label sheet in which the adhesive sheet, the thermoplastic resin layer formed in a pattern, and the release sheet are laminated in this order. (Step P3-6) A step of punching out the label sheet, leaving no cuts in the release sheet, and cutting only the adhesive sheet, or the adhesive sheet and the thermoplastic resin layer formed in a pattern, to separate the label-free area from the labeled area. (Step P3-7) A step of removing waste to remove the unnecessary portion of the label. In a third aspect of the method of using the patterned sheet according to this embodiment, when the label portion is separated from the label sheet, the thermoplastic resin layer formed in a pattern is separated from the release agent layer and remains on the adhesive sheet as a non-adhesive portion that causes the adhesive sheet to lose its adhesiveness.

[0128] In step P3-2, the release sheet has no cuts, which means the same as described in step 2-2 in the second embodiment. In step P3-6, the release sheet has no cuts, which means that the release sheet has no cuts at all, and also means that cuts that are unavoidable when punching are allowed. For example, it is allowed that cuts are allowed in the thickness direction of the release layer from the first release layer surface toward the release substrate, for example, in a range of about 1 / 10 or less of the entire thickness of the release layer, so long as they do not affect the releasability between the thermoplastic resin layer and the release agent layer, and between the pressure-sensitive adhesive layer and the release agent layer, and do not break the release sheet.

[0129] The third embodiment differs from the second embodiment in that the adhesive body formed by attaching the thermoplastic resin layer formed in a pattern to the adhesive sheet used in the second embodiment is a label sheet. The third embodiment also differs from the second embodiment in that the label sheet is punched, no cuts are made in the release sheet, and cuts are made only in the adhesive sheet or in the adhesive sheet and the thermoplastic resin layer formed in a pattern, and after separating the label-unnecessary portion from the label portion, a waste removal is performed to remove the label-unnecessary portion. Steps P3-1 to P3-4 in the third embodiment are the same as steps P2-1 to P2-4 in the second embodiment, and therefore will not be described here.

[0130] Moreover, step P3-5 is substantially the same as step P2-5 in the second embodiment. In step P3-5, the thermoplastic resin layer formed in a pattern is attached to the adhesive sheet to form a laminated adhesive body, which is a label sheet. When the pattern sheet is attached to the adhesive sheet, it may be attached by pressing or may not be pressed. In step P3-5, the label sheet laminated by attaching the pattern sheet to the adhesive sheet has the same laminated structure as that described for the adhesive body 403 shown in FIG. 7. Therefore, a description of the label sheet obtained in step P3-5 will be omitted.

[0131] Hereinafter, a third embodiment of the method for using the pattern sheet according to the present embodiment will be described with reference to the drawings. In the drawings, some parts are shown enlarged or reduced in size to facilitate the description. With reference to Figs. 9 to 11, Figs. 9 to 11 show a schematic process diagram of one embodiment using the pattern sheet according to the present embodiment.

[0132] In step P3-6, the label sheet obtained in step P3-5 is punched. When the label sheet is punched, no cuts are made in the release sheet, but cuts are made only in the adhesive sheet, or in the adhesive sheet and the thermoplastic resin layer formed in a pattern. By making these cuts, the label-free portion and the label portion are separated. Below, a case where cuts are made only in the adhesive sheet will be described.

[0133] 9 shows label sheet 407 after punching the label sheet obtained in step P3-5. As shown in FIG. 9, in the punched label sheet 407, a slit 407X is provided in the adhesive sheet 30. On the other hand, in the punched label sheet 407, no slit 407X is provided in the release sheet 10. The label sheet 407 obtained in step P3-5 is punched in the thickness direction of the adhesive sheet 30, from the second adhesive base surface 312 toward the release sheet 10. The slit 407X reaches the first adhesive layer surface 331, and extends from the second adhesive base surface 312 to the first adhesive layer surface 331. The punching may be performed using a known processing device equipped with a punching means.

[0134] By punching the label sheet 407, a label-free portion 407Z and a label portion 407A are separated by a cut 407X. The dimensions of the label portion 407A and the dimensions of the label-free portion 407Z may be determined according to the desired dimensions. As shown in Fig. 9, in step 3-6, the thermoplastic resin layer 21 is divided into each label portion 407A such that one thermoplastic resin layer pattern portion 20A is arranged for one label portion 407A.

[0135] In step P3-7, waste removal is performed to remove the unnecessary label portion 407Z defined in step P3-6. Figure 10 shows label sheet 409 after waste removal is performed on label sheet 407 shown in Figure 9, thereby removing unnecessary label portion 407Z from label sheet 407. As shown in Figure 10, in label sheet 409 after waste removal, part of first release agent layer surface 131 of release agent layer 13 is exposed, and a large number of label portions 407A are attached intermittently at a distance from one another on release sheet 10. Waste removal may be performed using a known processing device equipped with waste removal means. Steps P3-6 and P3-7 may be performed using a processing device equipped with a punching means and waste removal means. Furthermore, steps P3-2 and P3-3, as well as steps P3-6 and P3-7, may be performed in a processing device that is equipped with a punching means and a waste removal means for performing steps P3-2 and P3-3, and further equipped with a punching means and a waste removal means for performing steps P3-6 and P3-7. Furthermore, steps P3-2 and P3-3, as well as steps P3-5 to P3-7, may be performed in a label production device that is equipped with a punching means and a waste removal means for performing steps P3-2 and P3-3, as well as steps P3-6 and P3-7.

[0136] Since the interface between the release agent layer 13 and the thermoplastic resin layer 21 (i.e., the contact surface between the first release agent layer surface 131 of the release agent layer 13 and the second thermoplastic resin layer surface 212 of the thermoplastic resin layer 21) is a pseudo-adhesive interface, the label sheet 409 can be separated between the thermoplastic resin layer 21 formed in a pattern and the release agent layer 13. FIG. 11 shows a state in which the label portion 407A is separated from the label sheet 409 in the direction of the arrow R2. The label portion 407A separated from the label sheet 409 is a label 410. When the label portion 407A is separated from the label sheet 409, the label sheet 409 is separated between the second thermoplastic resin layer surface 212 and the first release agent layer surface 131 in the pattern sheet 101. The separated thermoplastic resin layer 21 remains as a thermoplastic resin layer pattern portion 20A on the adhesive layer 33 of the adhesive sheet 30 with the first thermoplastic resin layer surface 211 still attached to the first adhesive layer surface 331 of the adhesive layer 33. The label portion 407A may be separated from the label sheet 409 using, for example, an automatic labeling device.

[0137] The label 410 shown in FIG. 11 includes an adhesive sheet 30 and a thermoplastic resin layer pattern portion 20A which is a part of the thermoplastic resin layer 21 remaining on the adhesive layer 33 of the adhesive sheet 30. The adhesive layer 33 has an adhesive portion 333 where the first adhesive layer surface 331 is exposed, and a non-adhesive portion 335 where the second thermoplastic resin layer surface 212 of the thermoplastic resin layer 21 formed in a pattern shape is exposed. The adhesive portion 333 is a portion of the adhesive layer 33 where the thermoplastic resin layer 21 formed in a pattern shape is not attached. The separated thermoplastic resin layer 21 remains on the adhesive layer 33 of the adhesive sheet 30, thereby functioning as a non-adhesive portion 335 which causes the adhesive sheet 30 to lose its adhesiveness. In FIG. 11, the thickness of the adhesive layer 33 in the adhesive portion 333 is shown as a thickness approximately equal to the sum of the thickness of the adhesive layer 33 and the thickness of the thermoplastic resin layer 21 in the non-adhesive portion 335, but is not limited thereto. The thickness of the adhesive layer 33 in the adhesive portion 333 may be smaller than the total thickness of the adhesive layer 33 in the non-adhesive portion 335 and the thickness of the thermoplastic resin layer 21 .

[0138] The pattern sheet 101 used in the third embodiment has pseudo-adhesion, which is an appropriate adhesive strength between the thermoplastic resin layer 21 and the release agent layer 13. Therefore, according to the third embodiment of the method of using the pattern sheet according to the present embodiment, the non-adhesive portion 335 can be easily provided in the adhesive layer 33 of the adhesive sheet 30, similarly to the first and second embodiments described above. Moreover, similarly to the first and second embodiments described above, the effect of losing adhesive force tends to last. Furthermore, since the pattern sheet 101 used in the third embodiment has a thermoplastic resin layer 21 formed in a pattern, when the release agent layer 13 is peeled off from the adhesive layer 33, similarly to the second embodiment, the release agent layer 13 has excellent releasability with respect to the adhesive layer 33.

[0139] The present invention is not limited to the above-described embodiment, and may include modifications and improvements within the scope of the present invention. EXAMPLES

[0140] Examples will be described below, but the present invention is not limited to these examples in any way.

[0141] The following raw materials were prepared as raw materials for producing each of the Examples and Comparative Examples.

[0142] [Materials for making release sheets] (Release substrate) "RB-1": High-quality paper (manufactured by Nippon Paper Industries Co., Ltd., "WM Seal 64.0G", basis weight 64g / m 2 ). "RB-2": Polyethylene terephthalate film (manufactured by Mitsubishi Chemical Corporation, "T-100", thickness 38 μm).

[0143] (Middle class) "M-1": Low-density polyethylene (manufactured by Japan Polyethylene Co., Ltd., "LC605Y", MFR: 7.3 g / 10 min, density: 0.918 g / cm 3 ).

[0144] (Release agent layer) "RA-1": Olefin release agent [Polyolefin resin composition (ethylene-1-butene copolymer (manufactured by Sumitomo Chemical Co., Ltd., "Excellen VL EUL731", density: 0.895 g / cm 3 ) 75% by mass and low-density polyethylene (Novatec LD LC604, manufactured by Japan Polyethylene Co., Ltd., density: 0.918 g / cm 3 ) 25 mass% mixture), MFR of polyolefin resin composition: 8.5 g / 10 min. "RA-2": Olefin release agent [Polyolefin resin composition (ethylene-1-octene copolymer (manufactured by Dow Corporation, "ENGAGE8200", density: 0.870 g / cm 3 ) 75% by mass and low-density polyethylene (Novatec LD LC604, manufactured by Japan Polyethylene Co., Ltd., density: 0.918 g / cm 3 ) 25 mass% mixture), MFR of polyolefin resin composition: 5.0 g / 10 min. "RA-3": Silicone-based release agent (manufactured by Shin-Etsu Chemical Co., Ltd., "KS847").

[0145] [Thermoplastic resin layer forming material] "PE-1": Low-density polyethylene (manufactured by Japan Polyethylene Co., Ltd., "Novatec LD LC605Y", MFR: 7.3 g / 10 min, density: 0.918 g / cm 3 ) "PE-2": Low-density polyethylene (manufactured by Japan Polyethylene Co., Ltd., "Novatec LD LC8001", MFR: 20g / 10min, density: 0.917g / cm 3 ) "PE-3": Low-density polyethylene (manufactured by Sumitomo Chemical Co., Ltd., "Sumikasen L405", MFR: 3.7 g / 10 min, density: 0.924 g / cm 3 ) "PP-1": Polypropylene (manufactured by SunAllomer Co., Ltd., "PHA03A", MFR: 42g / 10min, density: 0.90g / cm 3 )

[0146] <Example 1> (Preparation of release sheet) The low-density polyethylene (M-1) for forming the intermediate layer was heated and melted, and the melted polyethylene was extruded from a T-die at an extrusion resin temperature of 280°C to form an intermediate layer having a thickness of 15 μm on one side of the release substrate (RB-1). Next, the olefin release agent (RA-1) for forming the release agent layer was heated and melted on the intermediate layer, and extruded at an extrusion resin temperature of 280°C so as to have a thickness of 20 μm to form a release agent layer. In this way, a release sheet was obtained in which the release substrate, the intermediate layer, and the release agent layer were laminated in this order.

[0147] (Creating pattern sheets) After corona treatment was performed on the surface of the release agent layer of the release sheet obtained above on which the thermoplastic resin layer was to be formed, low-density polyethylene (PE-1) for forming the thermoplastic resin layer was heated and melted, and the melted polyethylene was extruded from a T-die at an extrusion resin temperature of 280° C. to form a thermoplastic resin layer with a thickness of 13 μm on the release agent layer. In this way, a pattern sheet of Example 1 was obtained in which the thermoplastic resin layer was pseudo-adhered to the release agent layer of the release sheet.

[0148] <Examples 2 to 14> The pattern sheets of each example were obtained in the same manner as in Example 1, except that at least one of the conditions listed in Table 1 was changed: the type of release substrate, the type of release agent layer, the type of thermoplastic resin layer-forming material, the thickness of the thermoplastic resin layer, and whether or not corona treatment was performed when providing the thermoplastic resin layer.

[0149] <Comparative Examples 1 to 4> At least one of the conditions of the type of release agent layer, the type of thermoplastic resin layer forming material, and the thickness of the thermoplastic resin layer was changed according to Table 1, and further, corona treatment was omitted when providing the thermoplastic resin layer. Except for this, pattern sheets of each comparative example were obtained in the same manner as in Example 1.

[0150] <Comparative Example 5> A release sheet was obtained in the same manner as in Example 1, except that a release agent layer was not provided in the preparation of the release sheet. Next, using the obtained release sheet, a pattern sheet of Comparative Example 5 was obtained in the same manner as in Example 1, except that the type of thermoplastic resin layer-forming material was changed according to Table 1, and further, corona treatment was not performed when providing the thermoplastic resin layer.

[0151] [Adhesion evaluation] The adhesion between the release agent layer and the thermoplastic resin layer in the patterned sheet produced in each example was visually evaluated according to the following evaluation criteria. "A": No defects such as lifting were observed, and the release agent layer and the thermoplastic resin layer were adhered to each other. "F": Defects such as lifting are observed, and adhesion is insufficient.

[0152] [Measurement of pseudo-adhesion force] The pseudo-adhesion strength at the interface between the release agent layer and the thermoplastic resin layer of the release sheet was measured. The pseudo-adhesive strength was measured according to the 180° peel adhesion measurement specified in JIS Z0237:2022. Specifically, first, the thermoplastic resin layer side of the pattern sheet produced in each example was fixed to a stainless steel plate using double-sided tape. Then, the release sheet of the pattern sheet was peeled off from the thermoplastic resin layer under the conditions of a peel speed of 0.3 m / min and a peel angle of 180°. The magnitude of the force (peel force) required for this peeling was measured, and the measured peel force was taken as the pseudo-adhesive strength (unit: mN / 50 mm). In addition, the pseudo-adhesion strength of Comparative Example 5 could not be measured because the thermoplastic resin layer could not be peeled off from the intermediate layer due to the absence of a release agent layer. In the table, the pseudo-adhesion strength of Comparative Example 5 is represented as F.

[0153] [Peeling force of release layer from adhesive layer] The peel strength was measured according to the 180° peel adhesion test specified in JIS Z0237:2022. Specifically, a release sheet was first prepared according to the procedure of "Preparation of Release Sheet" above. Next, an acrylic adhesive (an adhesive solution containing 100 parts by mass of an acrylic acid ester copolymer having a weight average molecular weight of 800,000, obtained by copolymerizing 90 parts by mass of butyl acrylate and 10 parts by mass of acrylic acid, and 2 parts by mass of an isocyanate-based crosslinking agent (Takenate D-101E, manufactured by Mitsui Chemicals, Inc.)) was coated on the surface of the release layer of the obtained release sheet to a thickness of 20 μm to form an adhesive layer. Then, a PET film having a thickness of 50 μm was attached to the adhesive layer. Then, a 2 kg roller was moved back and forth once to prepare an adhesive body. After leaving this adhesive body for one day under conditions of a temperature of 23°C and a relative humidity of 50%, the release agent layer was peeled off from the adhesive body and the peel force was measured under conditions of a peel speed of 0.3 m / min and a peel angle of 180°. In addition, the peel strength of Comparative Example 5 was not measurable because the release agent layer was not provided and the thermoplastic resin layer could not be peeled from the adhesive body. In the table, the peel strength of Comparative Example 5 was indicated as F.

[0154] [Table 1]

[0155] In each Example, pseudo-adhesion was obtained, and therefore peeling was possible at the interface between the release agent layer of the release sheet and the thermoplastic resin layer. On the other hand, in Comparative Examples 1 to 4, since the release agent layer was formed from a silicone-based release agent, the pseudo-adhesion strength between the interface of the release agent layer of the release sheet and the thermoplastic resin layer was too low, resulting in poor adhesion. In Comparative Example 5, since there was no release agent layer, the thermoplastic resin layer could not be peeled off from the intermediate layer.

[0156] From the above results, it can be seen that the pattern sheet according to this embodiment has a suitable pseudo-adhesion between the release agent layer and the thermoplastic resin layer. In addition, since the pattern sheet according to this embodiment has a suitable pseudo-adhesion between the release agent layer and the thermoplastic resin layer, it has excellent processability when performing glue-killing treatment on the adhesive layer, and can easily form a non-adhesive part on the adhesive layer of the adhesive sheet. Furthermore, since the pattern sheet according to this embodiment has a non-adhesive part formed by the thermoplastic resin, the effect of losing adhesive force is easily sustained. [Explanation of symbols]

[0157] 10...release sheet, 11...release substrate, 13...release agent layer, 20, 21...thermoplastic resin layer, 20A...thermoplastic resin layer pattern portion, 20X...slit, 20Z...unnecessary portion of thermoplastic resin layer, 30...adhesive sheet, 31...adhesive substrate, 33...adhesive layer, 100, 101...pattern sheet, 111...first release substrate surface, 112...second release substrate surface, 131...first release agent layer surface, 132...second release agent layer surface, 201, 211... First thermoplastic resin layer surface, 202, 212...second thermoplastic resin layer surface, 311...first adhesive substrate surface, 312...second adhesive substrate surface, 331...first adhesive layer surface, 332...second adhesive layer surface, 333...adhesive portion, 335...non-adhesive portion, 400, 401, 403, 405...adhesive body, 407...label sheet, 407A...label portion, 407X...slit, 407Z...no label required portion, 409...label sheet, 410...label.

Claims

1. A pattern sheet to be attached to an adhesive sheet, A release sheet including a release substrate and a release agent layer provided on one surface of the release substrate; a thermoplastic resin layer provided on the surface of the release sheet opposite to the release substrate and pseudo-adhered to the release agent layer; Equipped with the release agent layer comprises an olefin release agent containing a polyolefin resin composition, the thermoplastic resin layer contains a polyolefin resin, the interface between the release agent layer and the thermoplastic resin layer is a pseudo-adhesive interface; The pseudo-adhesion strength when peeled off at the pseudo-adhesion interface is 50 mN / 50 mm or more and 1000 mN / 50 mm or less. Pattern sheet.

2. The pattern sheet according to claim 1 , The polyolefin resin composition contains a polyolefin thermoplastic resin having at least one structural unit selected from the group consisting of structural units derived from ethylene, structural units derived from propylene, structural units derived from butene, structural units derived from hexene, structural units derived from octene, and structural units derived from 4-methyl-1-pentene. Pattern sheet.

3. The pattern sheet according to claim 2, The polyolefin resin composition is a mixture of a copolymer containing a structural unit derived from ethylene and a structural unit derived from butene, and polyethylene, or The polyolefin resin composition is a mixture of a copolymer containing a structural unit derived from ethylene and a structural unit derived from octene, and polyethylene. Pattern sheet.

4. The pattern sheet according to any one of claims 1 to 3, The melt flow rate of the polyolefin resin composition is 1 g / 10 min or more and 20 g / 10 min or less. Pattern sheet.

5. The pattern sheet according to any one of claims 1 to 3, The polyolefin resin in the thermoplastic resin layer has at least one of a structural unit derived from ethylene and a structural unit derived from propylene. Pattern sheet.

6. The pattern sheet according to any one of claims 1 to 3, the thermoplastic resin layer is formed in a pattern so that a portion of the release agent layer is exposed, When the thermoplastic resin layer formed in a pattern and the exposed release agent layer are attached to the pressure-sensitive adhesive sheet, The peel strength of the release agent layer from the pressure-sensitive adhesive sheet is 50 mN / 50 mm or more and 500 mN / 50 mm or less. Pattern sheet.

7. The pattern sheet according to any one of claims 1 to 3, The release substrate is one or two of a paper substrate and a resin substrate; Pattern sheet.

8. A method for using the pattern sheet according to any one of claims 1 to 3, comprising the steps of: providing the pattern sheet; preparing the pressure-sensitive adhesive sheet; a step of attaching the thermoplastic resin layer to the pressure-sensitive adhesive sheet, and laminating the pressure-sensitive adhesive sheet, the thermoplastic resin layer, and the release sheet in this order; having when the pattern sheet is separated from the pressure-sensitive adhesive sheet, the thermoplastic resin layer is separated from the release agent layer and remains on the pressure-sensitive adhesive sheet as a non-adhesive portion that causes the pressure-sensitive adhesive sheet to lose its adhesiveness. How to use the pattern sheet.

9. A method for using the pattern sheet according to any one of claims 1 to 3, comprising the steps of: providing the pattern sheet; a step of punching the pattern sheet, forming a cut in the thermoplastic resin layer without forming a cut in the release sheet, thereby dividing an unnecessary portion of the thermoplastic resin layer from a patterned portion of the thermoplastic resin layer; a step of removing unnecessary portions of the thermoplastic resin layer to expose a portion of the first release agent layer surface of the release agent layer, thereby forming the thermoplastic resin layer in a pattern; preparing the pressure-sensitive adhesive sheet; a step of attaching the thermoplastic resin layer formed in a pattern to the pressure-sensitive adhesive sheet, and laminating the pressure-sensitive adhesive sheet, the thermoplastic resin layer formed in a pattern, and the release sheet in this order; having when the release sheet is separated from the pressure-sensitive adhesive sheet, the thermoplastic resin layer formed in a pattern is separated from the release agent layer and remains on the pressure-sensitive adhesive sheet as a non-adhesive portion that causes the pressure-sensitive adhesive sheet to lose its adhesiveness. How to use the pattern sheet.

10. A method for using the pattern sheet according to any one of claims 1 to 3, comprising the steps of: providing the pattern sheet; a step of punching the pattern sheet, leaving no cuts in the release sheet and providing cuts in the thermoplastic resin layer to separate an unnecessary portion of the thermoplastic resin layer from a patterned portion of the thermoplastic resin layer; a step of removing unnecessary portions of the thermoplastic resin layer to expose a portion of the first release agent layer surface of the release agent layer, thereby forming the thermoplastic resin layer in a pattern; preparing the pressure-sensitive adhesive sheet; a step of attaching the thermoplastic resin layer formed in a pattern to the adhesive sheet to form a label sheet in which the adhesive sheet, the thermoplastic resin layer formed in a pattern, and the release sheet are laminated in this order; a step of punching the label sheet, forming a cut in the adhesive sheet alone or in the adhesive sheet and the thermoplastic resin layer formed in a pattern, without forming a cut in the release sheet, to separate a label-free portion from a label portion; a step of removing the unnecessary portion of the label; having when the label portion is separated from the label sheet, the thermoplastic resin layer formed in a pattern is separated from the release agent layer and remains on the adhesive sheet as a non-adhesive portion that causes the adhesive sheet to lose its adhesiveness. How to use the pattern sheet.

Citation Information

Patent Citations

  • Composite display label

    JP1996262979A

  • Pressure sensitive adhesive label from which part of substrate is peelable

    JP2001051606A

  • Self-adhesive temper-proof label

    JP2008298988A

  • Vacuum transfer film for electroless plating

    JP2020090717A

  • Recovering prevention label

    JP3056012U