Method for manufacturing high-strength aluminum alloy extruded material having excellent SCC resistance, and aluminum alloy used for the same
A controlled cooling and extrusion process for an Al-Zn-Mg alloy addresses the SCC resistance issue in high-strength alloys, achieving enhanced tensile and yield strengths with improved SCC resistance.
Patent Information
- Application Number
- JP2024047122
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-09
AI Technical Summary
Existing high-strength Al-Zn-Mg alloys suffer from decreased stress corrosion cracking (SCC) resistance when attempting to achieve higher strength levels.
A specific Al-Zn-Mg-based alloy composition with controlled cooling and extrusion conditions, including a casting speed of 50 mm/min, homogenization at 480-520°C for 1-12 hours, and controlled cooling rates after extrusion, is used to produce an extruded material with an average grain size of 250 μm or less, followed by aging treatment.
The method achieves a tensile strength of 500 MPa or more and a 0.2% yield strength of 470 MPa or more, while maintaining excellent SCC resistance.
Smart Images

Figure 2024139746000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an extruded material made of an Al-Zn-Mg aluminum alloy having high strength and excellent SCC resistance, and to an aluminum alloy used in the method. [Background technology]
[0002] In the field of vehicles and the like, there is a demand for high-strength aluminum alloy extrusion materials for the purpose of reducing weight. Among aluminum alloys, Al-Zn-Mg alloys are known to have high strength, but there was a technical issue of decreasing stress corrosion cracking resistance (SCC resistance) when trying to achieve even higher strength.
[0003] For example, in Patent Document 1, the thickness of the surface recrystallization is set to 7% or less of the wall thickness, and the average grain size of the surface recrystallization is set to 150 μm or less, thereby improving SCC resistance, but the tensile strength is at the level of approximately 450 MPa. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 2928445 Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention aims to obtain a high-strength aluminum alloy extrusion material with excellent SCC resistance by using an Al-Zn-Mg alloy having a specified component composition and obtaining the extrusion material under specified extrusion conditions. [Means for solving the problem]
[0006] The high-strength aluminum alloy extrusion material with excellent SCC resistance according to the present invention uses an aluminum alloy having an average crystal grain size after casting of 250 μm or less, comprising, in mass%, Zn: 6.0 to 10.0%, Mg: 1.5 to 3.5%, Cu: 0.20 to 2.50%, Zr: 0.10 to 0.25%, Ti: 0.005 to 0.05%, Mn: 0.30 or less, Cr: 0.25% or less, a total of [Mn + Cr + Zr] of 0.10 to 0.50%, and the balance being Al and unavoidable impurities. To obtain a cast structure with an average crystal grain size of 250 μm or less, a molten aluminum alloy having the above alloy composition is cast at a casting speed of 50 mm / min or more, and then homogenized at 480 to 520°C for 1 to 12 hours (HOMO treatment), followed by cooling at a cooling speed of 50°C or more.
[0007] The manufacturing method of the high-strength aluminum alloy extrusion material excellent in SCC resistance according to the present invention is characterized in that the above-mentioned aluminum alloy is extruded so that the temperature of the extrusion material immediately after the extrusion processing is 440°C or higher, the extrusion material is allowed to cool in the atmosphere at a cooling rate of less than 100°C / min for 1.0 to 3.4 minutes until the temperature of the extrusion material reaches 250 to 400°C from immediately after the extrusion processing, and then the extrusion material is cooled at a cooling rate of 100 to 2000°C / min until the temperature of the extrusion material reaches 150°C or lower, followed by aging treatment. This provides a tensile strength of 500 MPa or more and a 0.2% yield strength of 470 MPa or more. Here, natural cooling refers to extruding so that the temperature of the extruded material immediately after extrusion is 440° C. or higher, and then allowing it to cool naturally in the air at a cooling rate of less than 100° C. / min over 1.0 to 3.4 minutes. The forced cooling is performed by forced air cooling using a fan or water cooling at a cooling rate in the range of 100 to 2000°C. Furthermore, once the extruded material cools to 150°C or below, its strength and SCC resistance are not affected.
[0008] Also preferably, after the extrusion process, the extruded material is allowed to cool in air over a period of 1 minute or more until the temperature of the extruded material reaches 300 to 400 °C, and then, until the extrusion temperature becomes 150 °C or lower, it is forcibly cooled at a cooling rate of 200 to 2000 °C / min and then age-treated.
[0009] The reasons for selecting the aluminum alloy composition used in the present invention are as follows. <Zn and Mg components> Even at relatively high concentrations, Zn does not reduce the extrudability and contributes to the improvement of strength. By adding Mg, MgZn2 precipitates in the structure, increasing the strength. However, when the addition amount of Mg increases, the extrudability decreases, and the precipitation amount of MgZn2 may become too large, possibly reducing the toughness. Therefore, a combination in the range of Zn: 6.0 to 10.0% and Mg: 1.5 to 3.5% is preferable. <Cu component> The addition of the Cu component is effective for improving strength by the solid solution effect. However, when the addition amount increases, the general corrosion resistance decreases. Therefore, a range of Cu: 0.20 to 2.50% is preferable. <Zr, Mn and Cr components> All of these components are transition elements. They suppress the recrystallization depth formed on the surface of the extruded material during the extrusion process and are effective in refining the crystal grains. Thereby, the stress corrosion cracking resistance is improved. Among these, the Cr component has the most acute hardening sensitivity. Although the Mn component has a lower hardening sensitivity than Cr, its influence is greater than that of Zr. Therefore, in the present invention, Zr is set to 0.10 to 0.25%. When adding Mn, it is suppressed to 0.30% or less, and when adding Cr, it is suppressed to 0.25% or less, and the total of [Mn + Cr + Zr] is preferably suppressed to the range of 0.10 to 0.50%. <Ti component> The Ti component is effective in refining the crystal grains when casting the billet used for the extrusion process. Generally, a very small amount of B is also added. A small addition amount of Ti: 0.005 to 0.05% is sufficient. <Other ingredients> In the casting process of 7000 series aluminum alloys, Fe and Si are often included as impurities. If the amount of these impurities is large, they affect the extrudability and stress corrosion cracking resistance, etc., so it is preferable to limit the Fe content to 0.2% or less and the Si content to 0.1% or less. Effect of the Invention
[0010] By extruding an aluminum alloy of a specified composition and controlling the cooling conditions immediately after extrusion (die edge quenching), a high-strength extruded material can be obtained while maintaining excellent SCC resistance. [Brief description of the drawings]
[0011] [Figure 1] The composition of the aluminum alloy used in the evaluation is shown, with the remainder being Al and unavoidable impurities. [Diagram 2] The casting conditions and homogenization treatment (HOMO treatment) conditions for the extrusion billet are shown below. [Diagram 3] The extrusion conditions and the cooling conditions immediately after extrusion of the extruded material are shown below. [Figure 4] The evaluation results of the extruded material are shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Molten aluminum alloys having the compositions shown in the table of FIG. 1 were prepared, and billets were cast and homogenized (HOMO) under the conditions shown in the table of FIG. Next, as shown in Figure 3, the billet (BLT) was preheated to 440°C or higher, and extruded at a speed of 5 m / min or higher to produce hollow or solid extrusions with a thickness of 2 to 3 mm, height of 50 to 60 mm, and width of 110 to 120 mm. The temperature of the extruded material immediately after extrusion is shown in the table in FIG. All of the temperatures were above 440°C.
[0013] As shown in the table of FIG. 3, the cooling conditions immediately after extrusion were varied and evaluated for Examples 1 to 14 and Comparative Examples 1 to 16. The target range for each condition is shown in the table in Figure 3, with conditions that fall within that range marked with an "O" and conditions that fall outside that range marked with an "X".
[0014] The evaluation results are shown in Figure 4. The evaluation conditions are as follows: <Mechanical properties> Based on JIS-Z2241, JIS-5 test pieces were prepared and the tensile strength, σ, was measured using a tensile testing machine conforming to the JIS standard. 0.2 The yield strength and elongation were measured. <Billet grain size and microstructure of extruded material> The sample surface was mirror-polished and etched with Keller's reagent. The metal structure was observed by optical microscopy, and the image at 100 times magnification was processed to determine the average crystal grain size. <Stress corrosion cracking resistance (SCC resistance)> The test piece was subjected to a stress of 80% of its yield strength, with the following conditions being one cycle, and the target was met if no cracks occurred after 720 cycles. If cracks occurred during testing, the number of cycles at which they occurred was recorded. [1 cycle] Immerse in a 3.5% NaCl aqueous solution at 25°C for 10 minutes, then leave at 25°C and 40% humidity for 50 minutes, and then air dry.
[0015] As can be seen from the table in FIG. 4, Examples 1 to 14 all had excellent SCC resistance because the cooling conditions immediately after extrusion were controlled within the target range, whereas Comparative Examples 1 to 14 had a tensile strength of 500 MPa or more, a 0.2% yield strength of 470 MPa or more, and an elongation of 8% or more, but all of them did not achieve the target SCC resistance.
[0016] When examining the evaluation results in detail, the following can be stated: In the table of Figure 3, the cooling start extrusion temperature indicates that the extrusion material immediately after extrusion was allowed to cool naturally in the air, and once it reached the cooling start extrusion temperature shown in the table of Figure 3, it was forced to cool at a cooling rate of 100 to 2000°C / min. In addition, in the table of FIG. 3, the time to reach the cooling start point refers to the above-mentioned time for natural cooling in the atmosphere.
[0017] As shown in the table of FIG. 3, in Examples 1 to 10, the extrusion material cooling rate was 279 to 350° C. / min, which indicates forced air cooling by a fan. In contrast, in Examples 11 to 14, the extrusion material cooling rate was 1500° C. / min, which indicates that forced cooling was performed by water cooling. This shows that the temperature of the extruded material immediately after extrusion is 440°C or higher, and by providing a process for slowly cooling the material naturally in the air over a period of 1.0 to 3.4 minutes, it is possible to achieve excellent SCC resistance, regardless of whether the subsequent forced cooling is air-cooling or water-cooling. In addition, Comparative Example 15 was allowed to cool naturally in the air for 5.02 minutes, and Comparative Example 16 was allowed to cool naturally in the air for 3.45 minutes. Although elongation and SCC resistance were ensured, the tensile strength and yield strength did not reach the target.
[0018] The cooling rate by natural cooling immediately after extrusion can be calculated by the formula: (temperature of extruded material after extrusion)-(extrusion temperature at which cooling starts) / (time to reach cooling start). For example, the cooling rate in Example 1 when allowed to cool in the air is (470-382) / 1.24 = approximately 70°C / min. Moreover, the cooling rate in Example 12 is (500-350) / 2.40=about 62.5°C / min. As explained above, in Comparative Examples 15 and 16, although SCC resistance was ensured, the strength did not reach the target. This shows that, although SCC resistance can be ensured if the material is allowed to cool naturally in the air immediately after extrusion slowly at less than 100°C / min, in order to ensure strength, it is necessary to limit the cooling time in the air to between 1.0 and 3.4 minutes. From the viewpoint of ensuring strength, the cooling start temperature is preferably in the range of 300 to 400°C. Furthermore, it is preferable that the forced cooling by a fan or water cooling is 200° C. / min or more.
[0019] In Comparative Example 1, the cooling start time was short at 0.10 minutes, and the forced cooling was fast at 2300° C. / min, so that the SCC resistance was not achieved.
Claims
1. An aluminum alloy having, in mass %, Zn: 6.0 to 10.0%, Mg: 1.5 to 3.5%, Cu: 0.20 to 2.50%, Zr: 0.10 to 0.25%, Ti: 0.005 to 0.05%, Mn: 0.30 or less, Cr: 0.25% or less, a total of [Mn + Cr + Zr] of 0.10 to 0.50%, with the balance being Al and unavoidable impurities, and having an average crystal grain size after casting of 250 μm or less, The extrusion is performed so that the temperature of the extruded material immediately after the extrusion is 440° C. or higher. A method for producing a high-strength aluminum alloy extrusion material with excellent SCC resistance, comprising the steps of: cooling the extrusion material in the atmosphere at a cooling rate of less than 100°C / min for 1.0 to 3.4 minutes until the temperature of the extrusion material reaches 250 to 400°C immediately after extrusion; and then forcibly cooling the extrusion material at a cooling rate of 100 to 2000°C / min until the temperature of the extrusion material reaches 150°C or less, followed by aging treatment.
2. Immediately after the extrusion process, the extruded material is cooled in the air for at least 1 minute until the temperature of the extruded material reaches 300 to 400 ° C. The method for producing a high strength aluminum alloy extrusion material having excellent SCC resistance according to claim 1, characterized in that the extrusion temperature is then forcedly cooled at a cooling rate of 200 to 2000°C / min until the extrusion temperature becomes 150°C or less, and then aging treatment is performed.
3. 3. The method for producing a high-strength aluminum alloy extrusion material having excellent SCC resistance according to claim 2, characterized in that the extrusion material has a tensile strength of 500 MPa or more and a 0.2% yield strength of 470 MPa or more.
Citation Information
Patent Citations
High-strength aluminum alloy extruded material and its manufacturing method
JP2928445B2