Polishing pad
The polishing pad with optimized viscoelasticity and groove ratios in a polyurethane resin layer addresses the challenge of high polishing performance and defect reduction in semiconductor manufacturing, achieving improved scratch and deposit performance.
Patent Information
- Application Number
- JP2024048760
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-09
AI Technical Summary
Existing polishing pads for semiconductor manufacturing face challenges in achieving high polishing performance while minimizing defects such as scratches and deposits, with the relationship between circumferential and cross grooves on the polishing surface and dynamic viscoelasticity of the polishing layer not adequately addressed.
A polishing pad with a polyurethane resin layer featuring concentric holding grooves and intersecting discharge grooves, with specific viscoelasticity and groove area ratios defined by loss tangent tan δ and area ratio (Sc/Sr), optimized to balance slurry retention and discharge, thereby enhancing defect reduction and polishing rate.
The optimized polishing pad achieves excellent defect reduction and high polishing rates by balancing viscoelasticity and groove functions, effectively reducing scratches and deposits during chemical mechanical polishing.
Smart Images

Figure 2024139754000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a polishing pad, and more particularly to a polishing pad having a circumferential groove for holding and an intersecting groove for discharging formed on a polishing surface. [Background technology]
[0002] Conventionally, chemical mechanical polishing (CMP) has been performed in the process of forming insulating films and metal wiring in semiconductor manufacturing, and for such polishing, a polishing pad having a polishing layer made of polyurethane resin is used. Today's polishing requires not only high polishing performance but also a reduction in defects (scratches and deposits), and there are known polishing pads in which circumferential grooves and intersecting grooves are formed along the circumferential direction on the polishing surface of the polishing layer, with the circumferential grooves functioning as holding grooves for holding slurry and the intersecting grooves functioning as discharge grooves for discharging polishing waste and used slurry (Patent Document 1), as well as a polishing pad in which the dynamic viscoelasticity of the polishing layer is specified (Patent Document 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 5706178 [Patent Document 2] Patent No. 4959901 Summary of the Invention [Problem to be solved by the invention]
[0004] As such, many proposals have been made regarding polishing performance and defect reduction, but now, by discovering a relationship between the circumferential grooves and intersecting grooves formed on the polishing surface and the dynamic viscoelasticity of the polishing layer, it has been possible to obtain a polishing pad with excellent defect reduction and polishing rate. [Means for solving the problem]
[0005] That is, the polishing pad according to the invention of claim 1 has a polishing layer made of polyurethane resin, and a polishing surface formed on the surface of the polishing layer has a retaining groove formed of a circumferential groove and a discharge groove formed of an intersecting groove that intersects the retaining groove and penetrates to the outer periphery of the polishing layer, Regarding the above-mentioned polishing layer, the loss tangent tanδ (=E″ / E′) obtained by dividing the loss modulus E″ by the storage modulus E′ at 40°C is as follows: 0.073≦tan δ≦0.130 (1) 0.158≦0.0072×(Sc / Sr)+tanδ≦0.258 (2) (In the above formula 2, Sr represents the area of the discharge groove on the polishing surface, and Sc represents the area of the holding groove excluding the area of the intersection with the discharge groove.) It is characterized by satisfying the following. Effect of the Invention
[0006] In the above invention, the loss tangent tan δ (E″ / E′) in formula 1 is a parameter related to the viscosity and elasticity of the polishing layer, and the area ratio (Sc / Sr) in formula 2 is a parameter related to the ability of the discharge groove to discharge the slurry and the ability of the retention groove to retain the slurry. The present invention provides a polishing pad with reduced defects and an excellent removal rate by focusing on the relationship between the viscosity and elasticity of the polishing layer and the slurry discharge and retention capabilities of the discharge grooves and retention grooves. [Brief description of the drawings]
[0007] [Figure 1] FIG. 2 is a side view showing the polishing apparatus according to the embodiment. [Diagram 2] FIG. [Diagram 3] Graphs for Equations 1 and 2. [Figure 4] 1 is a table showing experimental results for examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The present invention will now be described with reference to the illustrated embodiment. FIG. 1 shows a side view of a polishing apparatus 2 equipped with a polishing pad 1 according to the present invention, which polishes an object 3 to be polished using the polishing pad 1. The polishing apparatus 2 includes a polishing platen 4 provided on the lower side for supporting the polishing pad 1, a support platen 5 provided on the upper side for supporting the workpiece 3, and a slurry supply means 6 for supplying a liquid slurry S. The polishing pad 1 and the workpiece 3 each have a substantially disk shape, and in this embodiment, the diameter of the polishing pad 1 is larger than the diameter of the workpiece 3. The lower surface of the polishing pad 1 is fixed to a polishing platen 4 with double-sided tape or the like, and the workpiece 3 is vacuum-adsorbed to a supporting platen 5. In addition, the polishing platen 4 and the support platen 5 are rotated relative to each other by a driving means not shown, and the support platen 5 is arranged to be able to move back and forth in the radial direction from the center position of the polishing platen 4, so that the polishing pad 1 and the workpiece 3 slide against each other while rotating relative to each other. A slurry supplying means 6 supplies a liquid slurry S, which is a mixture of abrasive grains and a required chemical, between the polishing pad 1 and the object to be polished 3, whereby the object to be polished 3 is polished. The polishing apparatus 2 having such a configuration is conventionally known, and a more detailed description will be omitted. In addition to the polishing apparatus 2 having the above configuration, polishing apparatuses 2 having other configurations, such as a polishing apparatus 2 in which the support platen 5 is not driven and is rotated by the rotation of the polishing platen 4, can also be used.
[0009] 2, the polishing surface 1A of the polishing pad 1 for polishing the workpiece 3 is formed with concentric holding grooves 1B made of circumferential grooves and a plurality of discharge grooves 1C made of intersecting grooves that intersect with the holding grooves 1B. In the following description, the portion of the polishing surface 1A where the holding grooves 1B and discharge grooves 1C are not formed is called a land portion 1D. The cross-sectional shapes of the holding groove 1B and the discharge groove 1C are not particularly limited, but may be, for example, a U-shaped or V-shaped cross section, or a trapezoidal shape expanding toward the polishing surface 1A. The cross-sectional shapes of the holding groove 1B and the discharge groove 1C may be different. The holding groove 1B is composed of a plurality of concentric circles formed concentrically from the center, and each holding groove 1B itself does not directly penetrate to the outer periphery of the polishing pad 1, but has a closed shape. The holding groove 1B thus formed holds the slurry S therein when the object 3 to be polished is polished, thereby achieving the effect of improving the polishing rate. In this embodiment, the holding grooves 1B are formed concentrically at equal pitches, but the intervals (pitch) between adjacent holding grooves 1B may be made different.
[0010] On the other hand, the discharge groove 1C is composed of multiple linear grooves formed radially from the center, and the ends of each discharge groove 1C reach the outer peripheral edge of the polishing pad 1 and penetrate into the side of the polishing pad 1. The discharge groove 1C thus formed is designed so that when polishing debris or the like gets into the discharge groove 1C during polishing of the workpiece 3, the debris or the like is discharged from the outer peripheral edge of the polishing pad 1 together with the slurry S as the polishing pad 1 rotates, thereby serving to reduce defects (the occurrence of scratches and deposits) on the workpiece 3. In this embodiment, the discharge grooves 1C are formed at equal angles, but the angles of adjacent discharge grooves 1C may be different. The groove depth of the holding groove 1B and the discharge groove 1C may be the same or different, but from the viewpoint of preventing the accumulation of polishing debris and the like, it is preferable that the groove depth is the same.
[0011] Furthermore, some of the bubbles formed in the polishing layer are open on the polishing surface 1A. In this embodiment, the average pore size of the bubbles opening on the polishing surface 1A is preferably within a range of 11.0 μm to 17.0 μm, more preferably 12.0 μm to 16.0 μm, and particularly preferably 12.0 μm to 15.5 μm. When the average pore size is 11.0 μm or more, clogging of the pores with aggregates of abrasive grains in the slurry, polishing debris, etc., which cause scratches, can be easily suppressed. On the other hand, when the average pore size is 17.0 μm or less, clogging of the pores with aggregates of abrasive grains in the slurry, polishing debris, etc., at the bottom of the pores is difficult, and scratches and deposits are difficult to occur. However, even if the average opening diameter is within the above range, if the conditions relating to the groove area ratio and the dynamic viscoelasticity tan δ of the polishing layer are not satisfied, as described below, the retention / discharge performance of the abrasive grains and polishing debris will not be balanced, or the viscosity and elasticity of the polishing surface will not be balanced, resulting in scratches and adhesions being more likely to occur and a decrease in the polishing rate.
[0012] A method for producing a polishing pad 1 having the above-mentioned configuration may include, for example, a preparation step of preparing at least a polyurethane bond-containing isocyanate compound as a prepolymer, a curing agent, and a hollow body; a mixing step of mixing at least the polyurethane bond-containing isocyanate compound and the curing agent to obtain a mixture for molding a molded body; a molded body forming step of molding a polyurethane resin molded body from the mixture for molding a molded body; and a polishing layer forming step of forming a polishing layer having the above-mentioned polishing surface 1A from the polyurethane resin molded body. The steps are divided into a preparation step, a mixing step, a compact forming step, and an abrasive layer forming step, and each step will be described below.
[0013] In the preparation step, for example, a polyurethane bond-containing isocyanate compound, a curing agent, and a hollow body are used as raw materials for the polyurethane resin molded body in the manufacture of the polishing pad 1. Furthermore, a polyol compound may be used together with the above components, and components other than the above may be used together within a range that does not impair the effects of the present invention.
[0014] The polyurethane bond-containing isocyanate compound prepared in the preparation step is a compound obtained by reacting the following polyisocyanate compound with a polyol compound under commonly used conditions, and contains a polyurethane bond and an isocyanate group in the molecule. In addition, other components may be contained in the polyurethane bond-containing isocyanate compound within the range that does not impair the effects of the present invention. The polyurethane bond-containing isocyanate compound may be a commercially available product, or may be a product synthesized by reacting a polyisocyanate compound with a polyol compound. The reaction is not particularly limited, and addition polymerization may be performed using a method and conditions known in the art for producing polyurethane resins. For example, the polyisocyanate compound heated to 50°C is added to a polyol compound heated to 40°C while stirring in a nitrogen atmosphere, and the mixture is heated to 80°C after 30 minutes and then reacted at 80°C for 60 minutes.
[0015] First, the polyisocyanate compound means a compound having two or more isocyanate groups in the molecule. The polyisocyanate compound is not particularly limited as long as it has two or more isocyanate groups in the molecule. For example, diisocyanate compounds having two isocyanate groups in the molecule include m-phenylene diisocyanate, p-phenylene diisocyanate, 2,6-tolylene diisocyanate (2,6-TDI), 2,4-tolylene diisocyanate (2,4-TDI), naphthalene-1,4-diisocyanate, diphenylmethane-4,4'-diisocyanate (MDI), 4,4'-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI), 3,3'-dimethoxy-4,4'-biphenyl diisocyanate, 3,3'-dimethyl Examples of the diisocyanate include diphenylmethane-4,4'-diisocyanate, xylylene-1,4-diisocyanate, 4,4'-diphenylpropane diisocyanate, trimethylene diisocyanate, hexamethylene diisocyanate, propylene-1,2-diisocyanate, butylene-1,2-diisocyanate, cyclohexylene-1,2-diisocyanate, cyclohexylene-1,4-diisocyanate, p-phenylene diisothiocyanate, xylylene-1,4-diisothiocyanate, and ethylidine diisothiocyanate. Furthermore, as the polyisocyanate compound, a diisocyanate compound is preferable, among which 2,4-TDI, 2,6-TDI and MDI are more preferable, and 2,4-TDI and 2,6-TDI are particularly preferable. These polyisocyanate compounds may be used alone, or a plurality of polyisocyanate compounds may be used in combination.
[0016] Next, the above-mentioned polyol compound means a compound having two or more alcoholic hydroxyl groups (OH) in the molecule. Examples of the polyol compound used in the synthesis of the polyurethane bond-containing isocyanate compound include diol compounds, triol compounds, and the like, such as ethylene glycol, diethylene glycol (DEG), butylene glycol, and the like; polyether polyol compounds, such as poly(oxytetramethylene) glycol (or polytetramethylene ether glycol) (PTMG), polypropylene glycol (PPG), and polyether polycarbonate diol (PEPCD), and the like; polyester polyol compounds, such as the reaction product of ethylene glycol and adipic acid, and the reaction product of butylene glycol and adipic acid, and the like; polycarbonate polyol compounds, polycaprolactone polyol compounds, and the like. Also, trifunctional propylene glycol with ethylene oxide added thereto can be used. Among these, PTMG, PPG, a mixture of PTMG and a polyester polyol compound, a mixture of PPG and PEPCD, or a combination of these with DEG is preferred. The above polyol compounds may be used alone or in combination of two or more.
[0017] Here, the NCO equivalent of the prepolymer, which indicates the molecular weight of the polyurethane bond-containing isocyanate compound (prepolymer) per NCO group, is preferably 200 to 800, more preferably 300 to 700, and even more preferably 400 to 600. Specifically, the NCO equivalent of the prepolymer can be determined as follows. NCO equivalent of prepolymer = (parts by mass of polyisocyanate compound + part by mass of polyol compound) / [(number of functional groups per molecule of polyisocyanate compound x parts by mass of polyisocyanate compound / molecular weight of polyisocyanate compound) - (number of functional groups per molecule of polyol compound x parts by mass of polyol compound / molecular weight of polyol compound)]
[0018] As the curing agent (also called a chain extender), for example, a polyamine compound and / or a polyol compound can be used. The polyamine compound means a compound having two or more amino groups in the molecule, and an aliphatic or aromatic polyamine compound, particularly a diamine compound, can be used. Examples of such compounds include ethylenediamine, propylenediamine, hexamethylenediamine, isophoronediamine, dicyclohexylmethane-4,4'-diamine, 3,3'-dichloro-4,4'-diaminodiphenylmethane (methylenebis-o-chloroaniline) (hereinafter abbreviated as MOCA), and polyamine compounds having a similar structure to MOCA. Furthermore, the polyamine compound may have a hydroxyl group, and examples of such amine compounds include 2-hydroxyethylethylenediamine, 2-hydroxyethylpropylenediamine, di-2-hydroxyethylethylenediamine, di-2-hydroxyethylpropylenediamine, 2-hydroxypropylethylenediamine, and di-2-hydroxypropylethylenediamine. As the polyamine compound, a diamine compound is preferable, MOCA, diaminodiphenylmethane, and diaminodiphenylsulfone are more preferable, and MOCA is particularly preferable. The polyamine compound may be used alone or in combination of two or more polyamine compounds. In order to facilitate mixing with other components and / or to improve the uniformity of the bubble diameter in the subsequent molding process, the polyamine compound is preferably degassed under reduced pressure while being heated as necessary. As a method for degassing under reduced pressure, a method known in the art for producing polyurethanes may be used, and for example, degassing can be performed using a vacuum pump at a vacuum degree of 0.1 MPa or less. When a solid compound is used as the curing agent (chain extender), it can be melted by heating and degassed under reduced pressure.
[0019] The polyol compound used as the curing agent is not particularly limited as long as it is a diol compound, a triol compound, etc. The polyol compound may be the same as or different from the polyol compound used to form the prepolymer. Specific examples include low molecular weight diols such as ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, pentanediol, 3-methyl-1,5-pentanediol, and 1,6-hexanediol, and high molecular weight polyol compounds such as poly(oxytetramethylene) glycol, polyethylene glycol, and polypropylene glycol. The above polyol compounds may be used alone or in combination of two or more.
[0020] Here, the components are mixed so that the R value, which is the equivalent ratio of the active hydrogen groups (amino groups and hydroxyl groups) present in the curing agent to the isocyanate groups present at the ends of the polyurethane bond-containing isocyanate compound, is 0.60 to 1.40. The R value is preferably 0.65 to 0.130, and more preferably 0.70 to 1.20.
[0021] The hollow body means a microsphere having a void. The microsphere includes those having a spherical shape, an elliptical shape, and shapes similar thereto. An example of a hollow body is one obtained by thermally expanding unfoamed heat-expandable microspheres having an outer shell (polymer shell) made of a thermoplastic resin and a low-boiling point hydrocarbon contained in the outer shell. As disclosed in JP-A-57-137323, etc., the polymer shell may be made of a thermoplastic resin such as an acrylonitrile-vinylidene chloride copolymer, an acrylonitrile-methyl methacrylate copolymer, or a vinyl chloride-ethylene copolymer. Similarly, the low-boiling point hydrocarbon encapsulated in the polymer shell may be, for example, isobutane, pentane, isopentane, petroleum ether, etc. In addition to using the hollow bodies, bubbles may be formed by chemical foaming such as water foaming or foaming due to mechanical stirring, or these methods may be combined.
[0022] Next, the mixing step will be described. In the mixing step, the polyurethane bond-containing isocyanate compound as a prepolymer, the curing agent, and the hollow bodies prepared in the preparation step are fed into a mixer and stirred and mixed. The mixing step is performed in a state where the components are heated to a temperature at which the fluidity of each component can be ensured. Although there is no particular restriction on the order of mixing, it is preferable to prepare a mixed liquid obtained by mixing a polyurethane bond-containing isocyanate compound and a hollow body, and a mixed liquid obtained by mixing a curing agent and other components as necessary, and to supply both mixed liquids into a mixer and mix and stir them. In this way, a mixed liquid for molding a molded body is prepared.
[0023] Next, in the molding process, the mixture for molding prepared in the mixing process is poured into a mold at 80 to 120° C. and cured to form a polyurethane resin molded body. At this time, the prepolymer and the curing agent react to form a polyurethane resin, and the mixture is cured.
[0024] In the abrasive layer forming process, the polyurethane resin molded body obtained in the above-mentioned molded body forming process is sliced into sheets, and the sliced resin sheets are cut into circles to obtain disc-shaped abrasive layers. One surface of the polishing layer becomes the polishing surface 1A, and the holding groove 1B and the discharge groove 1C are machined on the polishing surface 1A as shown in Fig. 2. Also, double-sided tape for mounting on the polishing device 2 is attached to the opposite surface of the polishing layer.
[0025] A polishing pad 1 having a retaining groove 1B and a discharge groove 1C formed on the polishing surface 1A as shown in Figure 2 is conventionally known as shown in Patent Documents 1 and 2 above, and by achieving both the function of retaining the slurry S by the retaining groove 1B and the function of discharging the slurry S by the discharge groove 1C, it is possible to obtain a defect reduction function and a high polishing rate. However, there is still a demand for improvements in these functions, and the present invention provides a polishing pad 1 having the above-mentioned retaining groove 1B and discharge groove 1C formed therein, which has superior defect reduction function and a high polishing rate.
[0026] The polishing layer of the polishing pad 1 of the present invention is configured to satisfy the conditions shown in the following equations 1 and 2, and more specifically, is configured to satisfy the conditions defined on the sides and in the inner area of the approximately parallelogram shown in the graph of Figure 3. In FIG. 3, the vertical axis represents the loss tangent tan δ of Equation 1 described below, and the horizontal axis represents the area ratio (Sc / Sr) between the discharge groove 1C and the holding groove 1B. The formula 1 is as follows: 0.073≦tan δ≦0.130 (1) In the above formula 1, tan δ represents the loss tangent tan δ (=E″ / E′) obtained by dividing the loss modulus E″ of the polishing layer by the storage modulus E′ at 40°C. The storage modulus E' and loss modulus E" can be measured using a conventional method (e.g., dynamic mechanical properties test (DMA) according to JIS K7244-4). In the present invention, the storage modulus E' and loss modulus E" of the polishing pad were measured at 40°C, assuming the temperature of the polishing layer surface during polishing, and the loss tangent tanδ was calculated. Tangent delta is an index of viscoelasticity under certain temperature conditions. Storage modulus E' is a measure of the energy stored and completely recovered per cycle when a sinusoidally varying stress is applied. On the other hand, loss modulus E" refers to the magnitude of the stress component that is n / 2 out of phase with the strain when a sinusoidal strain of a characteristic frequency is applied. This loss tangent tan δ is a parameter that indicates the relationship between the viscosity and elasticity of the polishing surface 1A when the polishing pad 1 is pressed against the workpiece, and generally, the larger the tan δ, the more viscous the surface is, and the smaller the tan δ, the more elastic the surface is. If the viscosity of the polishing surface 1A is high, the abrasive grains in the slurry tend to sink and scratches are less likely to occur, but the polishing rate (especially in the case of mechanical polishing) tends to decrease. In addition, polishing debris generated by polishing is easily taken up by the polishing surface, causing an increase in adhesion. On the other hand, if the elasticity of the polishing surface 1A is high, the hardness of the polishing surface 1A increases, making it difficult for the abrasive grains in the slurry to sink, which tends to improve the polishing rate (especially in the case of mechanical polishing), but makes scratches more likely to occur. That is, in formula 1, if tan δ is less than 0.073, the elasticity of the polishing surface becomes too high, resulting in a deterioration in the scratch value, and if tan δ exceeds 0.130, the viscosity of the polishing surface becomes too high, resulting in a decrease in the removal rate. In the above formula 1, tan δ is set to 0.073 or more and 0.130 or less, more preferably 0.073 or more and 0.125 or less, and particularly preferably 0.073 or more and 0.120 or less.
[0027] And the formula 2 is as follows: 0.158≦0.0072×(Sc / Sr)+tanδ≦0.258···(2) In the above formula 2, Sr is the area (mm 2 ), Sc is the area (mm 2 ) and Sc / Sr represents the area ratio between the holding groove 1B and the discharge groove 1C. The above area ratio (Sc / Sr) is a parameter that indicates the relationship between the slurry S retention function of the holding groove 1B and the slurry S discharge function of the discharge groove 1C. If the retention function of the holding groove 1B is increased, the slurry S can be retained in the holding groove, but polishing debris will also be contained in the holding groove 1B, causing an increase in scratches and adhesions. On the other hand, if the discharge function of the discharge groove 1C is improved, the polishing waste can be quickly discharged to the outside of the polishing pad 1, but the slurry S is difficult to retain, resulting in a problem of a decrease in the polishing rate. And, formula 2 shows the relationship between the area ratio (Sc / Sr) of the holding groove 1B to the discharge groove 1C and the loss tangent tan δ in formula 1 above. In the above formula 2, the value in formula 2 is set to 0.158 or more and 0.258 or less, more preferably 0.158 or more and 0.250 or less, and particularly preferably 0.158 or more and 0.242 or less. The term (0.0072 × (Sc / Sr) + tan δ) in formula (2) is a parameter value that combines the dynamic viscoelasticity of the polishing layer and the retention / discharge performance of the retention groove and discharge groove. By keeping this parameter value within the above range, a high defect reduction effect and polishing rate can be obtained.
[0028] In Fig. 3, the loss tangent tan δ in formula 1 corresponds to the value on the vertical axis, and defines the upper and lower opposite sides of the parallelogram shown in Fig. 3. In contrast, formula 2 defines the left and right opposite sides of the parallelogram shown in Fig. 3. The polishing pad of the present invention is defined as being located on the sides and inside the area consisting of the parallelogram described above, in other words, on the sides and inside the rectangular area formed by connecting the vertices (3.9, 0.130), (17.8, 0.130), (11.8, 0.073), and (25.7, 0.073) of the parallelogram described above. Polishing pad 1 having a polishing layer defined on the sides and inside of the region has been confirmed to have an excellent defect reduction function and polishing rate based on the following experimental results.
[0029] As shown in FIGS. 3 and 4, the following experiments were carried out using the polishing pads 1 according to the above embodiment, the polishing pads 1 of Examples 1 to 13 and the polishing pads 1 of Comparative Examples 1 to 5. The polishing pad 1 used in the above Examples 1 to 3, 9 to 10 and Comparative Examples 1 to 2 was produced as follows. First, 100 parts of a urethane prepolymer having an NCO equivalent of 460, obtained by reacting 2,4-tolylene diisocyanate (TDI), poly(oxytetramethylene) glycol (PTMG), poly(1,4-butylene adipate) having a molecular weight of 2000, and diethylene glycol (DEG), were mixed with 1.2 parts of unexpanded hollow bodies having an outer shell made of acrylonitrile-vinylidene chloride copolymer and containing isobutane gas within the shell, to obtain a urethane prepolymer mixture. The obtained urethane prepolymer mixed liquid was charged into a first liquid tank and kept at 60°C. Separately from the first liquid tank, 25.5 parts of 3,3'-dichloro-4,4'-diaminodiphenylmethane (methylene bis-o-chloroaniline) (MOCA) was charged into a second liquid tank as a curing agent and kept at 120°C.
[0030] Next, the liquids in the first liquid tank and the second liquid tank were poured into a mixer equipped with two injection ports, and mixed and stirred to obtain a mixed liquid. At this time, the mixing ratio was adjusted so that the R value, which represents the equivalent ratio of the amino group and hydroxyl group in the curing agent to the isocyanate group at the end of the urethane prepolymer, was 0.90.
[0031] The resulting mixture was poured into a mold preheated to 90°C and heated for 30 minutes for primary curing. The resulting block-shaped molded product was removed from the mold and secondary cured in an oven at 120°C for 4 to 8 hours to obtain a polyurethane resin molded product. The resulting polyurethane resin molded product was allowed to cool to 25°C, and then heated again in an oven at 120°C for 5 hours, after which it was sliced to a thickness of 1.3 mm or 1.6 mm to obtain a disk-shaped polyurethane foam sheet (polishing layer). Here, one surface of the obtained polishing layer constitutes the polishing surface 1A, and the diameter of the polishing surface 1A is 740 mm, and the area of the polishing surface 1A is 430084 mm. 2 It was. Thereafter, concentric holding grooves 1B and radial discharge grooves 1C were formed on the surface of the polishing layer as in Examples 1 to 11 or Comparative Examples 1 to 5 shown below, and a cushion layer and double-sided tape were attached to the back surface not used for polishing to obtain a polishing pad 1. Here, in this experiment, the depths of the holding grooves 1B and discharge grooves 1C were set to 0.6 mm. The cushion layer can be made of a resin-impregnated nonwoven fabric, a flexible material such as synthetic resin or rubber, or a foam having a cellular structure. In the above examples and comparative examples, a 1.3 mm-thick impregnated nonwoven fabric impregnated with polyurethane resin was used as the cushion layer.
[0032] Dynamic viscoelasticity tests were conducted on the polishing layer under the following measurement conditions. A dry polishing layer that had been kept in a thermohygrostat at a temperature of 23°C (±2°C) and a relative humidity of 50% (±5%) for 40 hours was used as a sample, and measurements were performed in tension mode under normal atmospheric conditions (dry conditions). The measurement results are shown in Figure 3. (Measurement conditions) Measuring device: RSA-G2 (TA Instruments) Sample size: length 5cm x width 0.5cm x thickness 0.16cm Test length: 1cm Test mode: Tensile mode Frequency: 10rad / s(1.6Hz) Measurement temperature: 40℃ Heating rate: 5℃ / min Distortion range: 0.10% Initial load: 148g Measurement interval: 2 points / ℃
[0033] The average pore size of the abrasive layer was calculated using the pores formed on a cut surface obtained by slicing the abrasive layer. A laser microscope (VK-X1000, manufactured by KEYENCE) was used to observe the cut surface of the polishing layer at a magnification of 400 times within an area of approximately 0.6 mm square (excluding the grooves) on the surface of the polishing layer, and the obtained image was binarized using image processing software (WinRooF2018 Ver4.0.2, manufactured by Mitani Shoji) to confirm the holes formed on the cut surface. The circle equivalent diameter of each hole was then calculated from the area of each hole, and the average value (average hole diameter) was calculated as the average hole diameter.
[0034] Example 1 In the polishing pad of Example 1, the storage modulus E' was 274.2 MPa, the loss modulus E'' was 32.7 MPa, and the loss tangent tan δ according to formula 1 was 0.1191. The discharge grooves 1C formed on the polishing surface 1A have a groove pitch angle of 15°, a groove width of 1.5 mm, and 24 grooves (hereinafter, in the radial direction). As a result, the area Sr of the discharge grooves 1C is 13320 mm 2 It became. On the other hand, the holding groove 1B has a groove pitch of 1.7 mm, a groove width of 0.4 mm, and 209 grooves. As a result, the area Sc of the holding groove 1B, obtained by subtracting the area of the intersection with the discharge groove 1C from the area of the holding groove 1B, is 97843 mm 2 It became. As a result, the area ratio Sc / Sr of the area Sc of the holding groove 1B to the area Sr of the discharge groove 1C in the above formula 2 was 7.3, and the value in formula 2 taking into account the above loss tangent tan δ was 0.1720. The average pore size on the polished surface A was 12.6 μm.
[0035] Example 2 The polishing layer of the polishing pad of Example 2 was the same as that of the polishing pad of Example 1, and therefore the loss tangent tan δ according to Equation 1 was 0.1191. The discharge grooves 1C formed on the polished surface 1A have a groove pitch angle of 11.25°, a groove width of 1.0 mm, and 32 grooves. As a result, the area Sr of the discharge grooves 1C is 11840 mm 2 It became. On the other hand, the holding groove 1B has the same configuration as the holding groove 1B in the first embodiment, and the area Sc of the holding groove 1B obtained by subtracting the area of the intersection with the discharge groove 1C from the area of the holding groove 1B is 98177 mm 2 It became. As a result, the area ratio Sc / Sr of the area Sc of the holding groove 1B to the area Sr of the discharge groove 1C in the above formula 2 was 8.3, and the value in formula 2 taking into account the above loss tangent tan δ was 0.1788.
[0036] Example 3 The polishing layer of the polishing pad of Example 3 was the same as that of the polishing pad of Example 1, and therefore the loss tangent tan δ according to Equation 1 was 0.1191. The discharge grooves 1C formed on the polished surface 1A have a groove pitch angle of 22.5°, a groove width of 1.5 mm, and 16 grooves. As a result, the area Sr of the discharge grooves 1C is 8880 mm 2 It became. On the other hand, the holding groove 1B has the same configuration as the holding groove 1B in the first embodiment, and the area Sc of the holding groove 1B obtained by subtracting the area of the intersection with the discharge groove 1C from the area of the holding groove 1B is 98846 mm 2 It became. As a result, the area ratio Sc / Sr of the area Sc of the holding groove 1B to the area Sr of the discharge groove 1C in the above formula 2 was 11.1, and the value in formula 2 taking into account the above loss tangent tan δ was 0.1933. Here, in Examples 1 to 3, the polishing pads have the same polishing layer, but the configuration of the discharge grooves 1C is different.
[0037] Example 4 The polishing layer of the polishing pad according to Example 4 was different from those of Examples 1 to 3 and 9 to 10 and Comparative Examples 1 and 2. Specifically, the polishing layer was made using a urethane prepolymer with an NCO equivalent of 420 obtained by reacting poly(1,4-butylene adipate) with a lower molecular weight (molecular weight 800). In the polishing pad of Example 4, the storage modulus E' was 361.5 MPa, the loss modulus E'' was 33.8 MPa, and the loss tangent tan δ according to formula 1 was 0.0935. The holding groove 1B and the discharge groove 1C formed on the polishing surface 1A have the same configuration as in Example 3, and the area Sr of the discharge groove 1C is 8880 mm 2 The area Sc of the holding groove 1B, obtained by subtracting the area of the intersection with the discharge groove 1C from the area of the holding groove 1B, is 98846 mm 2 It became. The area ratio Sc / Sr of the area Sc of the holding groove 1B to the area Sr of the discharge groove 1C in the above formula 2 was 11.1, and the value related to formula 2 was 0.1736. The average pore size on polished surface A was 13.4 μm.
[0038] Example 5 The polishing layer of the polishing pad according to Example 5 was different from those of Examples 1 to 3 and 9 to 10 and Comparative Examples 1 and 2. Specifically, poly(1,4-butylene adipate) was not mixed into the urethane prepolymer mixture, and hollow bodies with large particle diameters were used to prepare the polishing layer. In the polishing pad of Example 5, the storage modulus E' was 322.0 MPa, the loss modulus E'' was 29.9 MPa, and the loss tangent tan δ according to formula 1 was 0.0928. The holding groove 1B and the discharge groove 1C formed on the polishing surface 1A have the same configuration as in Example 3, and the area Sr of the discharge groove 1C is 8880 mm 2 The area Sc of the holding groove 1B, obtained by subtracting the area of the intersection with the discharge groove 1C from the area of the holding groove 1B, is 98846 mm 2 It became. The area ratio Sc / Sr of the area Sc of the holding groove 1B to the area Sr of the discharge groove 1C in the above formula 2 was 11.1, and the value related to formula 2 was 0.1730. The average pore size on the polished surface A was 15.0 μm.
[0039] Example 6 The polishing layer of the polishing pad according to Example 6 was different from those of Examples 1 to 3 and 9 to 10 and Comparative Examples 1 and 2. Specifically, the polishing layer was produced using a urethane prepolymer with an NCO equivalent of 420 obtained by reacting poly(1,4-butylene adipate) with a lower molecular weight (molecular weight 800), and hollow bodies with a large particle size. In the polishing pad of Example 6, the storage modulus E' was 370.9 MPa, the loss modulus E'' was 32.8 MPa, and the loss tangent tan δ according to formula 1 was 0.0884. The holding groove 1B and the discharge groove 1C formed on the polishing surface 1A have the same configuration as in Example 3, and the area Sr of the discharge groove 1C is 8880 mm 2 The area Sc of the holding groove 1B, obtained by subtracting the area of the intersection with the discharge groove 1C from the area of the holding groove 1B, is 98846 mm 2 It became. The area ratio Sc / Sr of the area Sc of the holding groove 1B to the area Sr of the discharge groove 1C in the above formula 2 was 11.1, and the value related to formula 2 was 0.1685. The average pore size on polished surface A was 14.9 μm.
[0040] Example 7 The polishing layer of the polishing pad according to Example 7 was different from those of Examples 1 to 3 and 9 to 10 and Comparative Examples 1 and 2. Specifically, a urethane prepolymer obtained by reacting 2,4-tolylene diisocyanate (TDI), poly(oxytetramethylene) glycol (PTMG) and diethylene glycol (DEG) was used without mixing poly(1,4-butylene adipate), and hollow bodies with large particle diameters were used to prepare a polishing layer with a lower density. In the polishing pad of Example 7, the storage modulus E' was 249.2 MPa, the loss modulus E'' was 21.5 MPa, and the loss tangent tan δ according to formula 1 was 0.0862. The holding groove 1B and the discharge groove 1C formed on the polishing surface 1A have the same configuration as in Example 3, and the area Sr of the discharge groove 1C is 8880 mm 2 The area Sc of the holding groove 1B, obtained by subtracting the area of the intersection with the discharge groove 1C from the area of the holding groove 1B, is 98846 mm2 It became. The area ratio Sc / Sr of the area Sc of the holding groove 1B to the area Sr of the discharge groove 1C in the above formula 2 was 11.1, and the value related to formula 2 was 0.1664. The average pore size on polished surface A was 14.6 μm.
[0041] Example 8 The polishing layer of the polishing pad according to Example 8 was different from those of Examples 1 to 3 and 9 to 10 and Comparative Examples 1 and 2. Specifically, a urethane prepolymer with an NCO equivalent of 420 obtained by reacting poly(1,4-butylene adipate) with a lower molecular weight (molecular weight 800) was used, and the polishing layer was produced using hollow bodies with large particle diameters and different compositions. In the polishing pad of Example 8, the storage modulus E' was 577.7 MPa, the loss modulus E'' was 46.9 MPa, and the loss tangent tan δ according to formula 1 was 0.0812. The holding groove 1B and the discharge groove 1C formed on the polishing surface 1A have the same configuration as in Example 3, and the area Sr of the discharge groove 1C is 8880 mm 2 The area Sc of the holding groove 1B, obtained by subtracting the area of the intersection with the discharge groove 1C from the area of the holding groove 1B, is 98846 mm 2 It became. The area ratio Sc / Sr of the area Sc of the holding groove 1B to the area Sr of the discharge groove 1C in the above formula 2 was 11.1, and the value related to formula 2 was 0.1613. The average pore size on polished surface A was 13.6 μm. Here, in Examples 3 to 8, the polishing pads have discharge grooves 1C and holding grooves 1B of the same configuration formed on the polishing surface 1A, but the loss tangent tan δ of the polishing layer is made different.
[0042] Example 9 The polishing layer of the polishing pad of Example 9 was the same as that of the polishing pad of Example 1, and therefore the loss tangent tan δ according to Equation 1 was 0.1191. The discharge grooves 1C formed on the polished surface 1A have a groove pitch angle of 15°, a groove width of 1.0 mm, and 24 grooves. As a result, the area Sr of the discharge grooves 1C is 8880 mm 2 It became. On the other hand, the holding groove 1B has the same configuration as the holding groove 1B in the first embodiment, and the area Sc of the holding groove 1B obtained by subtracting the area of the intersection with the discharge groove 1C from the area of the holding groove 1B is 98846 mm 2 It became. As a result, the area ratio Sc / Sr of the area Sc of the holding groove 1B to the area Sr of the discharge groove 1C in the above formula 2 was 11.1, and the value in formula 2 taking into account the above loss tangent tan δ was 0.1993. Here, Example 9 differs from Example 1 in the groove width of the discharge groove 1C, and as a result, the area Sr of the discharge groove 1C is the same as that of Example 3. Furthermore, since the same polishing layer is used in Example 9 and Example 3, Equation 1 and Equation 2 show the same values.
[0043] Example 10 The polishing layer of the polishing pad of Example 10 was the same as that of the polishing pad of Example 1, and therefore the loss tangent tan δ according to Equation 1 was 0.1191. The discharge grooves 1C formed on the polishing surface 1A have a groove pitch angle of 22.5°, a groove width of 1.0 mm, and 16 grooves. As a result, the area Sr of the discharge grooves 1C is 5920 mm 2 It became. On the other hand, the holding groove 1B has the same configuration as the holding groove 1B in the first embodiment, and the area Sc of the holding groove 1B obtained by subtracting the area of the intersection with the discharge groove 1C from the area of the holding groove 1B is 99515 mm 2 It became. As a result, the area ratio Sc / Sr of the area Sc of the holding groove 1B to the area Sr of the discharge groove 1C in the above formula 2 was 16.8, and the value in formula 2 taking into account the above loss tangent tan δ was 0.2402. Here, the tenth embodiment is different from the third embodiment in that the groove width of the discharge groove 1C is different.
[0044] Example 11 The polishing layer of the polishing pad according to Example 11 was different from those of Examples 1 to 3 and 9 to 10 and Comparative Examples 1 and 2. Specifically, the polishing layer was prepared using a urethane prepolymer having an NCO equivalent of 400, which was obtained by reacting poly(1,4-butylene adipate) having a lower molecular weight (molecular weight 800). In the polishing pad of Example 11, the storage modulus E' was 468.7 MPa, the loss modulus E'' was 35.4 MPa, and the loss tangent tan δ according to formula 1 was 0.0755. The discharge grooves 1C formed on the polished surface 1A have a groove pitch angle of 30°, a groove width of 1.0 mm, and 12 grooves in number. As a result, the area Sr of the discharge grooves 1C is 4440 mm 2 It became. On the other hand, the holding groove 1B has the same configuration as the holding groove 1B in the first embodiment, and the area Sc of the holding groove 1B obtained by subtracting the area of the intersection with the discharge groove 1C from the area of the holding groove 1B is 99849 mm 2 It became. As a result, the area ratio Sc / Sr of the area Sc of the holding groove 1B to the area Sr of the discharge groove 1C in the above formula 2 was 22.5, and the value in formula 2 taking into account the above loss tangent tan δ was 0.2374. The average pore size on polished surface A was 14.8 μm.
[0045] Example 12 The polishing layer of the polishing pad according to Example 12 was different from those of Examples 1 to 3 and 9 to 10 and Comparative Examples 1 and 2. Specifically, polypropylene glycol (PPG) and polyether polycarbonate diol (PEPCD) were used instead of poly(oxytetramethylene) glycol (PTMG), and a urethane prepolymer with an NCO equivalent of 420 was used to prepare the polishing layer. In the polishing pad of Example 12, the storage modulus E' was 247.6 MPa, the loss modulus E'' was 22.5 MPa, and the loss tangent tan δ according to formula 1 was 0.0908. The discharge grooves 1C formed on the polished surface 1A have a groove pitch angle of 22.5°, a groove width of 1.5 mm, and 16 grooves. As a result, the area Sr of the discharge grooves 1C is 8880 mm 2 It became. On the other hand, the holding groove 1B has the same configuration as the holding groove 1B in the first embodiment, and the area Sc of the holding groove 1B obtained by subtracting the area of the intersection with the discharge groove 1C from the area of the holding groove 1B is 99849 mm 2 It became. As a result, the area ratio Sc / Sr of the area Sc of the holding groove 1B to the area Sr of the discharge groove 1C in the above formula 2 was 11.1, and the value in formula 2 taking into account the above loss tangent tan δ was 0.1709. The average pore size on polished surface A was 14.0 μm.
[0046] Example 13 The polishing layer of the polishing pad of Example 13 was different from those of Examples 1 to 3 and 9 to 10 and Comparative Examples 1 and 2. Specifically, the same resin was used, and the amount of hollow bodies added was 3.3 parts to prepare the polishing layer. In the polishing pad of Example 13, the storage modulus E' was 221.9 MPa, the loss modulus E'' was 22.5 MPa, and the loss tangent tan δ according to formula 1 was 0.1016. The discharge grooves 1C formed on the polished surface 1A have a groove pitch angle of 22.5°, a groove width of 1.5 mm, and 16 grooves. As a result, the area Sr of the discharge grooves 1C is 8880 mm 2 It became. On the other hand, the holding groove 1B has the same configuration as the holding groove 1B in the first embodiment, and the area Sc of the holding groove 1B obtained by subtracting the area of the intersection with the discharge groove 1C from the area of the holding groove 1B is 99849 mm 2 It became. As a result, the area ratio Sc / Sr of the area Sc of the holding groove 1B to the area Sr of the discharge groove 1C in the above formula 2 was 11.1, and the value in formula 2 taking into account the above loss tangent tan δ was 0.1818. The average pore size on the polished surface A was 13.2 μm.
[0047] Comparative Example 1 The polishing layer of the polishing pad of Comparative Example 1 was the same as that of the polishing pad of Example 1, and therefore the loss tangent tan δ according to Equation 1 was 0.1191. The discharge grooves 1C formed on the polishing surface 1A have a groove pitch angle of 20°, a groove width of 2.0 mm, and 18 grooves. As a result, the area Sr of the discharge grooves 1C is 13320 mm 2 It became. On the other hand, the holding groove 1B has a groove pitch of 2.82 mm, a groove width of 0.4 mm, and 126 grooves. As a result, the area Sc of the holding groove 1B, obtained by subtracting the area of the intersection with the discharge groove 1C from the area of the holding groove 1B, is 58813 mm 2 It became. As a result, the area ratio Sc / Sr of the area Sc of the holding groove 1B to the area Sr of the discharge groove 1C in the above formula 2 was 4.4, and the value in formula 2 taking into account the above loss tangent tan δ was 0.1509.
[0048] Comparative Example 2 The polishing layer of the polishing pad of Comparative Example 2 was the same as that of the polishing pad of Example 1, and therefore the loss tangent tan δ according to Equation 1 was 0.1191. The discharge grooves 1C formed on the polished surface 1A have a groove pitch angle of 22.5°, a groove width of 2.0 mm, and 16 grooves. As a result, the area Sr of the discharge grooves 1C is 11840 mm 2 It became. On the other hand, the holding groove 1B has the same configuration as the holding groove 1B of Comparative Example 1, and the area Sc of the holding groove 1B obtained by subtracting the area of the intersection with the discharge groove 1C from the area of the holding groove 1B is 59014 mm 2 It became. As a result, the area ratio Sc / Sr of the area Sc of the holding groove 1B to the area Sr of the discharge groove 1C in the above formula 2 was 5.0, and the value in formula 2 taking into account the above loss tangent tan δ was 0.1550.
[0049] Comparative Example 3 The polishing layer of the polishing pad of Comparative Example 3 was the same as that of the polishing pad of Example 11, and therefore the loss tangent tan δ according to Equation 1 was 0.0755. The holding groove 1B and the discharge groove 1C formed on the polishing surface 1A have the same configuration as in Example 3, and the area Sr of the discharge groove 1C is 8880 mm 2The area Sc of the holding groove 1B, obtained by subtracting the area of the intersection with the discharge groove 1C from the area of the holding groove 1B, is 98846 mm 2 It became. From the above, the area ratio Sc / Sr of the area Sc of the holding groove 1B to the area Sr of the discharge groove 1C in the above formula 2 was 11.1, and the value for formula 2 was 0.1557. Here, in Comparative Example 3, a different polishing layer was used compared to Example 3.
[0050] Comparative Example 4 The polishing layer of the polishing pad according to Comparative Example 4 was different from those of the above-mentioned Examples 1 to 3 and 9 to 10 and Comparative Examples 1 and 2. Specifically, polypropylene glycol (PPG) was used in the urethane prepolymer mixture instead of poly(oxytetramethylene) glycol (PTMG) and poly(1,4-butylene adipate), and the polishing layer was prepared using hollow bodies with large particle sizes. In the polishing pad of Comparative Example 4, the loss tangent tan δ according to Equation 1 was 0.1747. The holding groove 1B and the discharge groove 1C formed on the polishing surface 1A have the same configuration as in Example 10, and the area Sr of the discharge groove 1C is 5920 mm 2 The area Sc of the holding groove 1B, obtained by subtracting the area of the intersection with the discharge groove 1C from the area of the holding groove 1B, is 99515 mm 2 It became. As a result, the area ratio Sc / Sr of the area Sc of the holding groove 1B to the area Sr of the discharge groove 1C in the above formula 2 was 16.8, and the value in formula 2 taking into account the above loss tangent tan δ was 0.2957. The average pore size on polished surface A was 15.1 μm. Here, in Comparative Example 4, a different polishing layer was used compared to that in Example 10.
[0051] Comparative Example 5 The polishing layer of the polishing pad according to Comparative Example 5 was different from those of the above-mentioned Examples 1 to 3 and 9 to 10 and Comparative Examples 1 and 2. Specifically, the polishing layer was produced using a urethane prepolymer with an NCO equivalent of 400, which was obtained by increasing the mixing ratio of poly(oxytetramethylene) glycol (PTMG) and decreasing the mixing ratio of low molecular weight poly(1,4-butylene adipate) and reacting them. In the polishing pad of Comparative Example 5, the storage modulus E' was 446.1 MPa, the loss modulus E'' was 32.1 MPa, and the loss tangent tan δ according to formula 1 was 0.0720. The holding groove 1B and the discharge groove 1C formed on the polishing surface 1A have the same configuration as in Example 11, and the area Sr of the discharge groove 1C is 4440 mm 2 The area Sc of the holding groove 1B, obtained by subtracting the area of the intersection with the discharge groove 1C from the area of the holding groove 1B, is 99849 mm 2 It became. As a result, the area ratio Sc / Sr of the area Sc of the holding groove 1B to the area Sr of the discharge groove 1C in the above formula 2 was 22.5, and the value in formula 2 taking into account the above loss tangent tan δ was 0.2339. The average pore size on polished surface A was 14.7 μm. Here, in Comparative Example 5, a different polishing layer was used compared to that in Example 11.
[0052] As shown in FIG. 3, the polishing characteristics (polishing rate and defect performance (scratches and deposits)) of each of the polishing pads of Examples 1 to 11 and Comparative Examples 1 to 5 were evaluated under the following polishing conditions. (polishing conditions) Polishing machine used: F-REX300X (manufactured by Ebara Corporation) Disk: KINIK 34R Abrasive temperature: 20℃ Polishing platen rotation speed: 90 rpm Polishing head rotation speed: 81 rpm Grinding pressure: 1.7psi Polishing slurry (positively charged): CES-5003-2.5 (CES-5003-2.5 stock solution: pure water = mixed solution of 1:3 by weight) (AGC Inc.) Polishing slurry flow rate: 250ml / min Polishing time: 60 seconds Object to be polished: TEOS film substrate Pad break: 32N 30 minutes Conditioning: Ex-situ, 32N, 4 scans
[0053] (polishing rate) For the polished object 3, the average value was calculated from the thickness measurements of 121 points before and after polishing, and the polishing rate (Å / min) was calculated by dividing the thickness measured at each shop from the average value by the polishing time. The thickness was measured using the DBS mode of an optical film thickness and film quality measuring device (KLA Tencor, ASET-F5x). The measurement results of the polishing rate of each polishing pad are summarized in Figure 4. (Defect) For the polished object 3, defects of 60 nm or more were detected using the high sensitivity measurement mode of a surface inspection device (KLA Tencor, Surfscan SP5). For each defect detected, SEM images taken with a review SEM were analyzed, and the number of "scratches" representing surface damage and the total number of "particles," "pad debris," and "organic residues" representing surface deposits were measured and averaged. The measurement results of defects for each polishing pad are summarized in Figure 4. If the number of scratches was less than 4 on average and the total number of deposits was less than 50 on average, the evaluation was made as a circle, and if the number of scratches was 4 or more on average or the total number of deposits was 50 or more on average, the evaluation was made as a cross. As a result of the measurement, as shown in Fig. 4, in Examples 1 to 13, all of them had a high polishing rate of 900 Å / min or more, and an average of 4 or more scratches and an average of 50 or more deposits were not detected on the polished object 3, showing good defect performance. On the other hand, in Comparative Examples 3 to 5, an average of 4 or more scratches or an average of 50 or more deposits were detected, showing inferior defect performance compared to the Examples. Also, in Comparative Examples 1, 2, and 4, the polishing rate was insufficient.
[0054] In the above embodiment, a concentric groove is used as the holding groove 1B, but it is believed that the same effect can be obtained with a spiral holding groove 1B. In addition, when a spiral holding groove 1B is used, the outer peripheral end needs to be formed so as not to penetrate the outer periphery of the polishing pad 1. [Explanation of symbols]
[0055] 1 Polishing pad 1A Polishing surface 1B Holding groove 1C Discharge groove
Claims
1. A polishing pad having a polishing layer made of polyurethane resin, and a polishing surface formed on the surface of the polishing layer, in which a retaining groove consisting of a circumferential groove and a discharge groove consisting of an intersecting groove that intersects the retaining groove and penetrates to the outer periphery of the polishing layer, Regarding the loss tangent tan δ (=E″ / E′) obtained by dividing the loss modulus E″ by the storage modulus E′ at 40° C. in the above polishing layer, 0.073≦tan δ≦0.130 (1) 0.158≦0.0072×(Sc / Sr)+tanδ≦0.258...(2) (In the above formula 2, Sr represents the area of the discharge groove on the polishing surface, and Sc represents the area of the holding groove excluding the area of the intersection with the discharge groove.) A polishing pad characterized by satisfying the above.
2. 2. The polishing pad of claim 1, wherein said retention grooves are concentric grooves and said discharge grooves are radial grooves.
3. 2. The polishing pad according to claim 1, wherein the groove depth of the retaining groove and the groove depth of the discharge groove are the same.
4. 2. The polishing pad according to claim 1, wherein the number of said discharge grooves is 12 to 32.
5. In the above formula 2, Sc / Sr is 7≦Sc / Sr≦12 (3) The polishing pad of claim 1 ,
6. 2. The polishing pad according to claim 1, wherein the polishing layer has hollow bodies in a polyurethane resin, and the average pore size is 11.0 μm or more and 17.0 μm or less.
7. The polishing pad according to claim 1, wherein the polyurethane resin constituting the polishing layer contains a polyurethane bond-containing isocyanate compound synthesized by reacting a polyisocyanate compound and a polyol compound as raw materials, the polyol compound being a polyether polyol compound and / or a polyester polyol compound, the polyether polyol compound being poly(oxytetramethylene) glycol or polypropylene glycol, and the polyester polyol compound being poly(1,4-butylene adipate).
Citation Information
Patent Citations
JP1974059901A
Vibration preventing device
JP1982006178A
Cited By
Polishing pads and polishing methods
JP2026113391A