Detection method of breakout, operation method of continuous casting facility, and manufacturing method of casting piece

The method of measuring nozzle opening and molten steel level deviations using a linear equation addresses the challenge of immediate breakout detection in continuous steel casting, improving detection accuracy and reducing operational disruptions.

JP2024140166AActive Publication Date: 2024-10-10JFE STEEL CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023051184
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10
Estimated Expiration
2043-03-28

AI Technical Summary

Technical Problem

Existing breakout detection methods in continuous steel casting are inadequate for immediate detection during transient states, particularly at the start of casting when light conditions are insufficient or the mold is transitioning from room temperature, leading to increased damage and operational interruptions.

Method used

A method involving continuous or intermittent measurement of the nozzle opening degree, utilizing a linear equation to determine the allowable upper limit based on casting speed, mold dimensions, and molten steel weight, combined with monitoring molten steel level height and opening deviations, to quickly detect breakouts.

Benefits of technology

Enables rapid breakout detection even in transient states, reducing false positives and operational disruptions, thereby enhancing productivity and minimizing damage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140166000001_ABST
    Figure 2024140166000001_ABST
Patent Text Reader

Abstract

To provide a detection method of breakout, an operation method of a continuous casting facility, and a manufacturing method of a casting piece, which are capable of quickly detecting breakout in a transient state just after starting casting and easily adjustable for optimization.SOLUTION: A detection method of breakout in a continuous casting facility 1 for steel continuously or intermittently measures, at a start timing of casting, a nozzle opening degree of a sliding nozzle 11 for adjusting the supply amount of molten steel 2 to be supplied into a mold 13, compares an opening degree value according to the measured nozzle opening degree with an allowable upper opening degree that is set according to a casting speed, a height change rate of molten steel in a mold, a mold width, a mold thickness and the weight of the molten steel in a tundish, and determines the occurrence of breakout when the opening degree value is greater than the allowable upper opening degree.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for detecting a breakout, a method for operating a continuous casting facility, and a method for producing a cast strip. [Background technology]

[0002] In conventional methods for detecting breakouts in continuous steel casting equipment, as described in Patent Documents 1 and 2, a camera attached directly below the mold is used to detect a breakout by judging the change in the amount of light captured by the camera using a threshold value, and measures such as quickly stopping the supply of molten steel are taken.

[0003] Also, various methods have been proposed for predicting breakout, and Patent Document 3, for example, discloses a method using a temperature measuring device. In the method of Patent Document 3, temperature measuring rows in which multiple temperature measuring devices are arranged horizontally are arranged in multiple stages in the pouring direction below the molten metal surface of the mold of a continuous casting machine, and for any two stages among the multiple stages, the temperature measuring device arranged in the upper temperature measuring row and the temperature measuring device arranged in the lower temperature measuring row are arranged on the same straight line. Then, the measured values ​​of the temperature measuring devices in the upper and lower stages on the same straight line are transmitted to a calculation device, and the breakout is judged using the relationship between these measured values. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-197352 [Patent Document 2] Japanese Patent Application Publication No. 2-235561 [Patent Document 3] JP 2016-39644 A Summary of the Invention [Problem to be solved by the invention]

[0005] In breakout detection technology, a higher detection rate when a breakout occurs is desirable because it reduces the damage caused by the breakout. Also, a lower false positive rate when a breakout does not occur is desirable because it reduces the frequency of interruptions to operations and increases productivity, and a shorter time from breakout occurrence to detection is desirable because it reduces the damage caused by the breakout.

[0006] The problem with detecting breakouts using a camera installed under the mold as in Patent Documents 1 and 2 is that it is difficult to detect a breakout immediately after casting begins, when the amount of molten steel inside the mold is less than normal and the amount of light is insufficient.

[0007] Furthermore, detection of breakout by measuring the temperature of the mold as in Patent Document 3 has the problem that it is difficult to detect a breakout immediately after the start of casting when the mold is in a transitional state in which the temperature is rising from room temperature.

[0008] Therefore, the present invention has been made in consideration of the above-mentioned problems, and has an object to provide a method for detecting a breakout, a method for operating a continuous casting equipment, and a method for manufacturing a cast slab, which are capable of quickly detecting a breakout even in a transient state immediately after the start of casting. [Means for solving the problem]

[0009] (1) According to one aspect of the present invention, there is provided a method for detecting a breakout in a continuous steel casting facility, comprising: continuously or intermittently measuring a nozzle opening of a sliding nozzle that adjusts the amount of molten steel supplied into a mold at the start of casting; comparing an opening value corresponding to the measured nozzle opening with an allowable upper limit opening that is set in accordance with the casting speed, the rate of change of the molten steel level in the mold, the mold width, the mold thickness, and the weight of molten steel in a tundish; and determining that a breakout has occurred when the opening value exceeds the allowable upper limit opening.

[0010] (2) In the above configuration (1), the allowable upper limit opening is expressed by a linear equation with a parameter x consisting of variables including the casting speed, the rate of change of the molten steel level in the mold, the mold width, the mold thickness, and the weight of molten steel in the tundish. (3) In the configuration of (2) above, the parameter x is expressed by the following equation (1).

[0011]

number

[0012] (6) In any one of the configurations (1) to (5) above, at least one of the molten steel level height of the molten steel supplied into the mold at the start of casting and the nozzle opening deviation of the nozzle that adjusts the amount of the molten steel supplied into the mold is monitored, and the occurrence of a breakout is detected when the molten steel level height falls below the lower limit H0 of the allowable height over time after the start of casting and / or the nozzle opening deviation exceeds the upper limit S0 of the allowable deviation over time after the start of casting, and when the opening value exceeds the upper limit of the allowable opening.

[0013] (7) In the above configuration (6), the allowable height lower limit H0 is calculated by equation (8) based on multiple pieces of operation data at the start of past casting, and the allowable deviation upper limit S0 is calculated by equation (9) based on multiple pieces of operation data at the start of past casting. H0 = H-Aσ1 (8) S0 = S + Bσ2 (9) Where: H0: Lower limit of allowable height H: Average value of the mold surface height from multiple past operation data A: Coefficient σ1: Standard deviation of the mold surface height from multiple past operational data S0: Upper limit of allowable deviation S: Average nozzle opening deviation from multiple past operation data B: Coefficient σ2: Standard deviation of nozzle opening deviation from multiple past operational data

[0014] (8) In any one of the configurations (1) to (5) above, at least one of the height of the surface of the molten steel supplied into the mold at the start of casting and the deviation in the opening degree of a nozzle that adjusts the amount of the molten steel supplied into the mold is monitored, The occurrence of a breakout is detected when the molten metal level falls below the lower limit H0 of the allowable height over time after the start of casting, the opening deviation exceeds the upper limit S0 of the allowable deviation over time after the start of casting, and the opening value exceeds the upper allowable opening limit.

[0015] (9) In the above configuration (8), the allowable height lower limit H0 is calculated by formula (8) based on multiple pieces of operation data at the start of past casting, and the allowable deviation upper limit S0 is calculated by formula (9) based on multiple pieces of operation data at the start of past casting. H0 = H-Aσ1 (8) S0 = S + Bσ2 (9) Where: H0: Lower limit of allowable height H: Average value of the mold surface height from multiple past operation data A: Coefficient σ1: Standard deviation of the mold surface height from multiple past operational data S0: Upper limit of allowable deviation S: Average nozzle opening deviation from multiple past operation data B: Coefficient σ2: Standard deviation of nozzle opening deviation from multiple past operational data

[0016] (10) According to one aspect of the present invention, there is provided a method for operating a continuous casting facility that continuously casts steel, comprising the steps of: detecting a breakout at the start of casting using a breakout detection method according to any one of the configurations (1) to (9) above; and interrupting the supply of molten steel to a mold when the breakout is detected. (11) According to one aspect of the present invention, there is provided a method for producing a slab by continuously casting steel using the method for operating a continuous casting facility as described in the configuration of (10) above. Effect of the Invention

[0017] According to one aspect of the present invention, there are provided a method for detecting a breakout, a method for operating a continuous casting system, and a method for producing a cast slab, which are capable of quickly detecting a breakout even in a transient state immediately after the start of casting. [Brief description of the drawings]

[0018] [Figure 1] 1 is a configuration diagram showing a continuous casting facility according to an embodiment of the present invention. FIG. [Diagram 2] FIG. 2 is a schematic diagram showing a state of the continuous casting equipment at the start of casting. [Diagram 3] 1 is a graph showing the relationship between the parameter x and the standardized nozzle opening degree and the allowable upper limit opening degree. [Figure 4] 13 is a graph showing the relationship between the coefficient c and the number of detections. [Diagram 5] 1 is a graph showing the allowable lower limit of height and the molten metal surface height at the time of breakout occurrence in an embodiment. [Figure 6] 11 is a graph showing an allowable upper limit of deviation and an opening deviation when a breakout occurs in an embodiment. [Figure 7] 13 is a graph showing the relationship between the coefficient A and the number of detections in the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] In the following detailed description, an embodiment of the present invention will be described with reference to the drawings. In the description of the drawings, identical or similar parts are given identical or similar symbols, and duplicated explanations are omitted. Each drawing is schematic and may differ from the actual one. In addition, the embodiments shown below are examples of devices and methods for embodying the technical idea of ​​the present invention, and the technical idea of ​​the present invention does not specify the materials, structures, arrangements, etc. of the components as described below. The technical idea of ​​the present invention can be modified in various ways within the technical scope defined by the claims described in the claims.

[0020] First Embodiment (Device configuration) FIG. 1 is a schematic diagram showing a continuous steel casting equipment 1 according to a first embodiment of the present invention. The continuous casting equipment 1 includes a tundish 10, a sliding nozzle 11, a submerged nozzle 12, a mold 13, a plurality of support rolls 14, a molten steel level gauge 15, and a judgment unit 16. In the continuous casting equipment 1, molten steel 2 contained in the tundish 10 is poured into the mold 13 through the sliding nozzle 11 and the submerged nozzle 12, and is cooled to form a solidified shell at the boundary between the mold 13 and the molten steel 2. The solidified shell is then pulled out while being supported by the support rolls 14, and is further cooled by cooling water or the like to form a cast piece having a predetermined cross-sectional shape.

[0021] The sliding nozzle 11 has a plate 110 with holes formed therein, and is a nozzle that controls the supply amount (supply speed) of the molten steel 2 from the tundish 10 to the mold 13 by sliding the plate 110. Specifically, the supply amount of the molten steel 2 is controlled by controlling the overlapping area between the hole of the plate 110 and the hole formed in the bottom of the tundish 10. The ratio of the sliding amount based on the relative position of the plate 110 in the sliding direction with respect to the tundish 10 is called the nozzle opening degree (%). For example, the nozzle opening degree may be 100% when the hole of the plate 110 and the hole in the bottom of the tundish 10 completely overlap in the sliding direction, and 0% when the two holes do not overlap.

[0022] The molten steel level gauge 15 is a measuring device that measures the molten steel level height, which is the height of the bath surface of the molten steel 2 in the mold 13. The measurement method of the molten steel level gauge 15 is not particularly limited as long as it is a known measurement method capable of measuring the molten steel level height. For example, a vortex type molten steel level gauge may be used for the molten steel level gauge 15. The molten steel level height is not particularly limited as long as it is capable of grasping the vertical position of the bath surface of the molten steel 2 in the mold 13, and may be, for example, the height (vertical distance) from the bottom surface of the mold 13 or a predetermined position inside the mold 13.

[0023] In the continuous casting equipment 1, the amount of molten steel 2 supplied to the mold 13 is adjusted by an adjustment mechanism (not shown). The adjustment of the amount of molten steel 2 supplied by this adjustment mechanism is performed by adjusting the nozzle opening based on the measurement result of a molten steel level gauge 15 so that the molten steel level is at a predetermined height.

[0024] The determination unit 16 is a calculation device such as a computer that detects a breakout at the start of casting. A method for detecting a breakout by the determination unit 16 will be described in detail later.

[0025] In the first embodiment, the period during which continuous casting is performed will be described by dividing it into a casting start time and a steady casting time. The casting start time is the period from immediately after the start of continuous casting until the casting speed reaches the steady casting speed. The steady casting time is the period after the casting start time, that is, the period after the casting speed reaches the steady casting speed.

[0026] At the start of casting, continuous casting is started in the state shown in Fig. 2. As shown in Fig. 2, at the start of continuous casting, a dummy bar 17 is inserted into the continuous casting equipment 1, and the tip of the dummy bar 17 (dummy bar head) is placed in the mold 13. Then, with the tip of the dummy bar 17 at the bottom of the mold 13, molten steel 2 is poured into the mold 13, thereby starting continuous casting. Then, after a predetermined time has elapsed since the molten steel 2 was poured, the dummy bar 17 is pulled out. Then, at a predetermined position, the dummy bar 17 is separated from the slab, and the casting speed is increased to a steady casting speed.

[0027] At the start of casting, the judgment unit 16 continuously or intermittently judges whether or not a breakout has occurred, thereby detecting a breakout. Note that since a breakout cannot occur when the dummy bar 17 is present inside the mold 13, the breakout is detected after the dummy bar 17 is pulled out of the mold 13. If a breakout is detected, the supply of molten steel 2 to the mold 13 is stopped, and casting is interrupted. On the other hand, if a breakout is not detected, casting is continued, and the breakout detection is also continued. The steady casting period is not particularly limited, and continuous casting is performed at a steady casting speed using a known continuous casting method.

[0028] (How to detect a breakout) A method for detecting a breakout according to the first embodiment will be described. In the first embodiment, at the start of casting, a nozzle opening value of a sliding nozzle 11 that controls the amount of molten steel 2 supplied into a mold 13 is continuously or intermittently measured.

[0029] Next, the judgment unit 16 compares the opening value according to the measured nozzle opening with the allowable upper limit opening set according to the casting speed, the rate of change of the molten steel level in the mold, the mold width, the mold thickness, and the weight of molten steel in the tundish. If the opening value exceeds the allowable upper limit opening, it is judged that a breakout has occurred, and if the opening value is equal to or less than the allowable upper limit opening, it is judged that a breakout has not occurred. The judgment of whether a breakout has occurred is performed continuously or intermittently depending on the timing of measuring the nozzle opening.

[0030] The allowable upper limit opening is preferably expressed as a linear equation with a parameter x consisting of variables including the casting speed, the rate of change of the molten steel level in the mold, the mold width, the mold thickness, and the weight of molten steel in the tundish. The parameter x can be expressed by the following equation (1). The rate of change of the molten steel level in the mold is the amount of change in the molten steel level per minute (m / min).

[0031]

number

[0032] Specifically, the allowable upper limit opening degree M is expressed by the following formula (2), which is a linear expression of parameter x. In the first embodiment, the judgment unit 16 calculates the parameter x from the casting speed, the rate of change of the molten steel level in the mold, the mold width, the mold thickness, and the weight of molten steel in the tundish at the timing when the nozzle opening degree is measured, and calculates the allowable upper limit opening degree M from the obtained parameter x and formula (2). The judgment unit 16 then judges whether or not a breakout has occurred by judging whether or not the calculated opening degree value exceeds the allowable upper limit opening degree M. This judgment is the same as judging whether or not the nozzle opening degree value satisfies formula (3).

[0033] M = a(xX) + b (2) (sn-SN)-a(xX)-b>0.0 (3) Where: sn: Nozzle opening (%) SN: Average nozzle opening rate for 50 seconds from the start of casting (%) X: Average value of parameter x for 50 seconds from the start of casting a: A constant corresponding to the gradient of the linear expression b: A constant corresponding to the intercept of the linear expression

[0034] In the first embodiment, the nozzle opening value according to the nozzle opening is calculated by subtracting the average value of the nozzle opening for 50 seconds from the start of casting from the measured nozzle opening (also called the standardized nozzle opening or the opening deviation). In addition, the parameter x measured by subtracting the average value of the parameter x for 50 seconds from the start of casting is used as a variable of the linear expression (also called the standardized parameter x). The parameter x and the nozzle opening are not constant due to various conditions such as the difference in the tundish shape and the state of the base metal adhesion in the tundish 10. However, by using standardized values ​​for the nozzle opening and the parameter x and judging the variation from the average value from the start of casting to 50 seconds of the casting chance to be judged, it is possible to detect breakout with the same judgment criteria regardless of the casting conditions. The time from the start of casting for obtaining the average value SN,X of the nozzle opening and the parameter x is preferably 50 seconds. Although the same effect can be obtained even if the time from the start of casting is longer than 50 seconds, it is preferable that the time is shorter so that the breakout can be detected as much as possible.

[0035] Moreover, the constants a and b are preset values, and are preferably set based on a plurality of past operation data in which no breakout has occurred. The operation data preferably includes a plurality of data including a plurality of opening values ​​and a plurality of parameters x at the time of measuring the opening values. Specifically, the constant a is calculated from the plurality of opening values ​​included in the plurality of operation data and the plurality of parameters x at the time of measuring the opening values ​​by a regression equation shown as a linear equation of the following equation (4). The constant b is calculated by equation (5) using the constant b' calculated by equation (4). In addition, the linear relationship between the parameter x and the nozzle opening is not actually constant, but varies within a certain range. In order to evaluate this variation, it is preferable that the number of past operation data is generally 50 or more. On the other hand, in order to deal with changes in the proportional relationship due to long-term fluctuations, it is preferable that the number of past operation data is 200 or less.

[0036] (sn-SN)=a(xX)+b' (4) b = b' + c σ (5) Where: b': A constant corresponding to the intercept of the regression equation c: Coefficient between 5.0 and 10.0 σ: Standard deviation of the regression equation

[0037] Furthermore, as shown in equation (5), the constant b is set to the average value μ b’ The coefficient c is set to 5.0 to 10.0, i.e., 5.0 or more and 10.0 times the standard deviation. In this way, by detecting a breakout only when there is a fluctuation of 5 to 10 times the standard deviation, it becomes possible to determine a breakout without false positives. When the coefficient c is small, less than 5.0, the nozzle opening degree exceeds the upper allowable opening degree M more frequently even when a breakout has not occurred, resulting in more false positives. On the other hand, when the coefficient c is large, more than 10.0, there is a high possibility that a breakout will not be detected even if it has occurred.

[0038] The parameter x corresponds to the ratio of the volume fluctuation of the molten steel 2 in the mold 13 to the volume fluctuation of the molten steel 2 in the tundish 10. The inventors have noticed that when casting is performed normally, the parameter x and the nozzle opening have a linear relationship represented by a first-order equation. They have found that breakout can be detected with high accuracy by determining the allowable upper limit of the nozzle opening, which is set based on the parameter x, as a threshold value.

[0039] Specifically, the inventors came up with the idea of ​​the present invention by approximating the physical model equation shown in equation (6) as being proportional to the head height H and the weight of molten steel in the tundish TD, which results in the proportional equation shown in equation (7). In the physical model shown in equation (6), the molten steel 2 in the tundish 10 falls freely from the head height (H) from the bottom of the tundish 10 to the surface of the molten steel through the sliding nozzle 11 according to the gravitational acceleration g and flows into the mold 13. Then, the molten steel 2 flows from the mold 13 to the casting speed V c The sliding nozzle 11 has a nozzle cross-sectional area of ​​A snThe nozzle opening is sn, and the mold 13 has a width w and a thickness d.

[0040]

number

[0041] When a breakout occurs, the nozzle opening increases so as to keep the molten steel level constant in the mold 13. On the other hand, the slide nozzle of the ladle, which adjusts the supply of molten steel 2 from the ladle to the tundish 10, also opens its nozzle opening as the amount of molten steel in the tundish 10 decreases, so that the weight of molten steel in the tundish is kept constant, and so the parameter x does not change significantly. The detection method in the first embodiment detects a breakout by utilizing this response difference.

[0042] In the first embodiment, the nozzle aperture of the sliding nozzle that adjusts the amount of molten steel supplied to the inside of the mold at the start of casting is continuously or intermittently measured. Then, the allowable upper limit aperture is calculated continuously or intermittently according to the timing of measuring the nozzle aperture, and it is determined that a breakout has occurred when the calculated allowable upper limit aperture exceeds an aperture value corresponding to the nozzle aperture. Since this detection method does not use a camera, it is possible to detect a breakout immediately after the start of casting when the amount of molten steel in the mold 13 is less than in a normal state and the amount of light is insufficient. In addition, since the temperature of the mold 13 is not used, it is possible to detect a breakout immediately after the start of casting when the mold 13 is in a transitional state where the temperature is rising from the normal temperature. Furthermore, since this method can detect a breakout more directly than a method using the mold temperature, etc., it is possible to perform detection without missing any breakouts.

[0043] In the first embodiment, the occurrence of a breakout is determined using equation (3) based on a linear expression of parameter x. This makes it easy to adjust for optimization, since there are only two constants to be set: a and b.

[0044] <Second embodiment> Next, a second embodiment of the present invention will be described. The second embodiment has the same device configuration, the operation method of the continuous casting equipment, and the manufacturing method of the cast slab as the first embodiment, but is different in the method of detecting a breakout. Therefore, in the following description, only the method of detecting a breakout will be described.

[0045] In the second embodiment, in addition to the breakout detection (first detection) in the first embodiment, a breakout detection (second detection) is performed based on at least one of the molten metal level height and the opening deviation at the start of casting. If a breakout is detected in both the first and second detections, it is determined that a breakout has actually occurred.

[0046] [Breakout detection method (secondary detection)] In the second detection in the second embodiment, at the start of casting, the nozzle opening, which is the opening value of the sliding nozzle 11 that controls the amount of molten steel 2 supplied into the mold 13, is measured continuously or intermittently. Furthermore, the judgment unit 16 calculates the opening deviation, which is the difference (fluctuation value) of the nozzle opening thereafter from the average value of the nozzle opening for a certain period from the start of casting. The certain period for calculating the average value of the nozzle opening is not particularly limited, but is preferably about 50 seconds.

[0047] (Detection method based on molten metal surface height) A method of detecting a breakout based on the molten steel level height in the second detection will now be described. In the detection method based on the molten steel level height, first, when continuous casting is started, the molten steel level gauge 15 continuously measures the molten steel level height, and the measurement results are sent to the judgment unit 16, thereby monitoring the molten steel level height. Note that, as the molten steel level height, an actual distance (mm) may be used, or an output value (%) of the molten steel level gauge 15 corresponding to the actual distance may be used.

[0048] Next, the judgment unit 16 judges whether or not the measured molten metal level becomes less than the allowable height lower limit H0 over time after the start of casting. Then, the judgment unit 16 judges that a breakout has occurred when the molten metal level becomes less than the allowable height lower limit H0, and judges that a breakout has not occurred when the molten metal level becomes equal to or greater than the allowable height lower limit H0.

[0049] When a breakout occurs, the molten steel 2 breaks through the solidified shell and leaks out inside the continuous casting equipment 1, and the amount of molten steel 2 discharged from the mold 13 becomes greater than the amount of molten steel 2 supplied from the tundish 10, causing a drop in the molten steel level. For this reason, by setting a lower limit H0 of the allowable height as a threshold value for detecting a breakout, it is possible to detect a breakout in the early stages of casting. The lower limit H0 of the allowable height is a value at the time elapsed after the start of casting, and is set for each elapsed time. For example, the lower limit H0 of the allowable height may be set for each measurement time interval of the molten steel level.

[0050] Furthermore, it is preferable that the allowable height lower limit H0 is calculated by the formula (8) based on multiple operation data from the start of past casting. Note that the multiple operation data from the past are obtained under conditions where no breakout occurs. It is also preferable that the coefficient A is 2.0 or more and 7.0 or less. H0 = H-Aσ1 (8) Where: H0: Lower limit of allowable height H: Average value of the mold surface height from multiple past operation data A: Coefficient σ1: Standard deviation of the mold surface height from multiple past operational data

[0051] The number of past operation data is preferably 50 or more in order to evaluate the variation (standard deviation) of the molten metal level, while the number of past operation data is preferably 200 or less in order to deal with changes in patterns due to long-term fluctuations.

[0052] (Detection method based on opening deviation) Next, a method for detecting a breakout based on the opening deviation in the second detection will be described. In the method for detecting the breakout based on the opening deviation, first, when continuous casting is started, the determination unit 16 continuously obtains the nozzle opening of the sliding nozzle 11 and calculates the opening deviation, thereby monitoring the opening deviation.

[0053] Next, the determination unit 16 determines whether the obtained opening deviation exceeds the upper limit S0 of the allowable deviation over time after the start of casting. If the opening deviation exceeds the upper limit S0 of the allowable deviation, the determination unit 16 determines that a breakout has occurred, and if the opening deviation is equal to or smaller than the upper limit S0 of the allowable deviation, the determination unit 16 determines that a breakout has not occurred.

[0054] When a breakout occurs, the molten steel level drops as described above, and control is performed to increase the nozzle opening to increase the amount of molten steel 2 supplied from the tundish 10. The supply amount at this time is greater than when no breakout occurs, and the nozzle opening and opening deviation are also greater than usual. For this reason, by setting an allowable deviation upper limit S0 as a threshold value for detecting a breakout, it is possible to detect a breakout in the early stages of casting. Furthermore, the allowable deviation upper limit S0 is a value at the time elapsed after the start of casting, and is set for each elapsed time. For example, the allowable deviation upper limit S0 may be set for each measurement time interval of the molten steel level height.

[0055] Furthermore, it is preferable that the allowable deviation upper limit S0 is calculated by the formula (9) based on multiple operation data from the start of past casting. Note that the multiple operation data from the past are obtained under conditions where no breakout occurs. Moreover, it is preferable that the coefficient B is 2.0 or more and 10.0 or less. S0 = S + Bσ2 (9) Where: S0: Upper limit of allowable deviation (%) S: Average value (%) of the opening deviation of multiple past operation data B: Coefficient σ2: Standard deviation of the opening deviation of multiple past operation data

[0056] In addition, the number of past operation data is preferably 50 or more in order to evaluate the variation (standard deviation) of the opening deviation, while the number of past operation data is preferably 200 or less in order to deal with changes in patterns due to long-term fluctuations.

[0057] (Detection method based on melt level and opening deviation) Furthermore, in the second detection, a breakout may be detected based on both the molten metal level height and the opening deviation. In this case, the judgment unit 16 monitors both the molten metal level height and the opening deviation, and judges that a breakout has occurred when the molten metal level height is less than the lower limit H0 of the allowable height and the opening deviation exceeds the upper limit S0 of the allowable deviation. On the other hand, when the molten metal level height is less than the lower limit H0 of the allowable height and the opening deviation does not exceed the upper limit S0 of the allowable deviation, the judgment unit 16 judges that a breakout has not occurred. Note that it is also possible to monitor both the molten metal level height and the opening deviation, and judge that a breakout has occurred when the molten metal level height is less than the lower limit H0 of the allowable height or the opening deviation exceeds the upper limit S0 of the allowable deviation.

[0058] As described above, in the second detection, the occurrence of a breakout is detected by making a judgment based on at least one of the molten metal level height and the nozzle aperture deviation. Since the judgment of the occurrence of a breakout is made based on at least one of the allowable height lower limit H0 and the allowable deviation upper limit S0 over time after the start of casting, it is possible to make a judgment with higher accuracy even in the transient state immediately after the start of casting compared to the case where the judgment is made based on a fixed threshold value for the molten metal level height or the nozzle aperture.

[0059] Furthermore, by setting the allowable height lower limit H0 using a plurality of past operation data and formula (1), or by setting the allowable deviation upper limit S0 using a plurality of past operation data and formula (2), breakout can be detected with high accuracy. The molten metal level is automatically controlled to be a constant value, but in reality it is not constant and varies within a certain range. Since the operation is based on a constant operation immediately after the start of casting, the speed pattern is similar, but the molten metal level is prone to hunting immediately after the casting speed is increased or immediately after the casting speed is made constant, so the average and variation of the molten metal level depend on the passage of time. For this reason, by setting the allowable height lower limit H0 and the allowable deviation upper limit S0 for each elapsed time, breakout can be detected with higher accuracy. Furthermore, by increasing the detection accuracy, false detection can be prevented and productivity can be improved. Furthermore, since breakout can be detected more quickly than with conventional detection methods, the impact on production caused by breakout can be reduced. Furthermore, since breakout can be detected directly compared to detection methods based on the mold temperature, detection can be performed without missing any.

[0060] Furthermore, unlike the molten metal surface height, the nozzle opening degree is not constant, depending on the size (width and thickness) of the mold 13 and various other conditions. For this reason, by making a judgment using the opening deviation, which is the fluctuation value from the average value for a certain period of time from the start of casting during the chance to make the judgment (the unit of continuous casting), it becomes possible to detect breakout using the same judgment criteria regardless of the size of the mold 13.

[0061] Furthermore, by detecting a breakout based on both the molten metal surface height and the opening deviation, it is possible to detect a breakout with higher accuracy.

[0062] Furthermore, in the second detection, it is preferable to set the coefficients A and B in the formulas (8) and (9) to 2.0 or more and 7.0 or less, in other words, to detect a breakout when there is a fluctuation of 5 to 10 times the standard deviation of the mold level height and the opening deviation of the past operation data. By doing so, it is possible to determine a breakout without erroneous detection.

[0063] In the second embodiment, if a breakout is detected in the first detection and then in the second detection, it is detected that a breakout has actually occurred. In this way, it is possible to reduce false positives compared to when a breakout is detected only by the first detection, and since detection can be performed without missing any detections, it is possible to improve detection accuracy.

[0064] Furthermore, in the second embodiment, the number of constants to be set is as small as four at most: a, b, A, and B. This makes adjustments for optimization easier than when there are many constant thresholds to be set.

[0065] <Modification> Although the present invention has been described above with reference to specific embodiments, it is not intended that the invention be limited by these descriptions. By referring to the description of the present invention, other embodiments of the present invention including various modifications in addition to the disclosed embodiments will be apparent to those skilled in the art. Therefore, it should be understood that the embodiments of the invention described in the claims also include embodiments including these modifications described herein, either alone or in combination.

[0066] For example, in the first and second embodiments, the method for detecting a breakout has been described, but the present invention is not limited to such examples. The present invention can also be applied to a method for operating a continuous casting facility and a method for manufacturing a slab. A method for operating a continuous casting facility according to one aspect of the present invention is a method for operating a continuous casting facility 1 that continuously casts steel, and detects a breakout using the method for detecting a breakout according to the first or second embodiment at the start of casting. If a breakout is detected, the supply of molten steel 2 to the mold 13 is interrupted, and if a breakout is not detected, the supply of molten steel 2 to the mold 13 is continued. In addition, a method for manufacturing a slab according to one aspect of the present invention continuously casts steel using the above-mentioned method for operating the continuous casting facility 1.

[0067] In the first embodiment, the standardized nozzle opening and the standardized parameter x are used as the opening value, but the present invention is not limited to this example. If the influence of various conditions such as the difference in tundish shape and the state of ingot adhesion in the tundish 10 among the continuous casting machines is small, the measured nozzle opening may be used as the opening value, and the parameter x calculated by the formula (1) may be used as it is without being standardized. EXAMPLES

[0068] An example carried out by the present inventors will be described. In the example, the allowable upper limit opening was obtained from the past operation data of 200 times. The allowable upper limit opening was obtained by the formula (2). FIG. 3 shows a plot of the past operation data, the obtained allowable upper limit opening (dashed straight line), and the regression equation obtained by the formula (4) (solid straight line). In FIG. 3, the horizontal axis shows the parameter x obtained by the formula (1), and the vertical axis shows the opening value which is the standardized nozzle opening. In the example of FIG. 3, the coefficient c used in the formula (5) when obtaining the allowable upper limit opening was set to 7.

[0069] Furthermore, Figure 3 shows the data of the opening value and parameter x in two charges where a breakout actually occurred as a line plot. In the example shown in Figure 3, it was confirmed that a breakout can be detected 5 to 10 seconds earlier than with the current breakout detection method that relies on the operator.

[0070] Moreover, Figure 4 shows the relationship between the coefficient c used in formula (5) and the number of detections. As can be seen from Figure 4, by making the coefficient c smaller, missed detections are eliminated but false positives increase, resulting in a larger number of detections. On the other hand, by making the coefficient c larger, false positives decrease but missed detections occur. For this reason, it was found that it is preferable to set the coefficient c to be between 5.0 and 10.0.

[0071] Furthermore, in the embodiment, the lower limit of the allowable height H0 and the upper limit of the allowable deviation S0 were calculated from the past operation data of 200 operations using equations (8) and (9), and a comparison was made between the molten metal level height and the aperture deviation when a breakout occurred for two chances.

[0072] FIG. 5 shows the behavior of the molten steel surface height at the time of the occurrence of the breakout for two chances with respect to the elapsed time, the lower limit H0 of the allowable height and the molten steel surface height at the time of the breakout occurrence for two chances. In FIG. 5, the vertical axis is the molten steel surface height, and the horizontal axis is the elapsed time (sec) from the start of the withdrawal of the dummy bar. The molten steel surface height on the vertical axis is the output value (%) of the molten steel level gauge 15 corresponding to the actual distance, and is controlled to be 45%. The elapsed time on the horizontal axis is -50 sec from the start of pouring the molten steel 2 into the mold 13, and 0 sec from the start of the withdrawal of the dummy bar. In the example shown in FIG. 5, the coefficient A is set to 7, that is, the average value of the molten steel surface height is set to 7 times the standard deviation as a threshold value. In the example shown in FIG. 5, the timing when the molten steel surface height falls below the lower limit H0 of the allowable height is 10 to 20 seconds before the breakout detection that is currently dependent on the operator, and it was confirmed that the breakout can be detected quickly and accurately.

[0073] In the example shown in Figure 5, it was confirmed that the threshold value changes over time, reaching a maximum about 20 seconds after the start of casting. This is because the casting speed is changed about 20 seconds after the start of casting, causing large variations in the molten metal surface height, but it was confirmed that the value then falls to about one-third of the peak. Here, with the conventional detection method, detection is performed using a constant threshold value that matches the peak of the variations, so the threshold value must be set large over the entire time period. However, with the second detection method, the optimal threshold value is selected based on the passage of time from past operational data, making it possible to detect breakouts more quickly than with the conventional detection method.

[0074] FIG. 6 shows the behavior of the opening deviation at the time of breakout occurrence for the obtained allowable deviation upper limit S0 and two chances with respect to the elapsed time. In FIG. 6, the vertical axis is the opening deviation, and the horizontal axis is the elapsed time (sec) from the start of pulling out the dummy bar, as in FIG. 3. The opening deviation on the vertical axis is the difference from the average nozzle opening from -50 sec to 0 sec, and is shown after the elapsed time of 0 sec. In addition, in the example shown in FIG. 6, the coefficient B is set to 4, that is, the average opening deviation is given a threshold value of 4 times the standard deviation. Furthermore, the chance of breakout occurrence in FIG. 6 is the same as that in FIG. 5. As is clear from FIG. 6, it was confirmed that breakout can be detected more quickly than the conventional method even when the opening deviation is used, as in the case of using the molten metal level.

[0075] Furthermore, the effect of the coefficients A and B in the formulas (1) and (2) on the detection accuracy and the occurrence of false positives was also investigated. Figure 7 shows the relationship between the coefficients A and B and the number of breakout detections when the coefficients A and B are changed from 1.0 to 10.0. In addition, the graph shown by "Both" in Figure 5 is the case where both the detection methods of the molten metal level and the opening deviation are used, and only when a breakout is detected in both the molten metal level and the nozzle opening, it is detected that a breakout has occurred. In this investigation, the number of breakouts that actually occurred was two. It was confirmed that by decreasing the coefficients A and B, the number of false positives decreased but the number of overdetections increased, while it was confirmed that by increasing the coefficients A and B, the number of overdetections decreased but the number of false positives increased. For this reason, it was confirmed that the coefficients A and B are appropriate for the equipment of this embodiment, from 2.0 to 7.0. Furthermore, in this embodiment, it was confirmed that the number of detections was two under the condition of combining the first detection and the second detection when the coefficients A and B were set to 4 and the coefficient c was set to 7, and there were no overdetections or false positives. In the example shown in Figure 6, it was confirmed that, compared to the current breakout detection method that relies on the operator, the breakout can be detected 9 seconds before the breakout occurrence chance (1) and 4 seconds before the breakout occurrence chance (2). Therefore, it was confirmed that the occurrence of a breakout can be detected with high accuracy by detecting using both the mold surface height and the opening deviation.

[0076] From the above results, it was confirmed that by combining the first and second detections, it is possible to reduce overdetection and erroneous detections and to detect breakouts with high accuracy. [Explanation of symbols]

[0077] 1. Continuous casting equipment 10 Tundish 11 Sliding nozzle 110 Plate 12 Submerged nozzle 13 Mold 14 Support roll 15 Molten Steel Level Gauge 16 Judgment section 17 Dummyba 2. Molten Steel

Claims

1. In continuous steel casting equipment, Continuously or intermittently measure the nozzle opening of a sliding nozzle that adjusts the amount of molten steel supplied into the mold at the start of casting, The method for detecting a breakout comprises comparing a measured nozzle opening value with an allowable upper limit opening value that is set in accordance with the casting speed, the rate of change of the molten steel level in the mold, the mold width, the mold thickness, and the weight of molten steel in the tundish, and determining that a breakout has occurred if the measured nozzle opening value exceeds the allowable upper limit opening value.

2. 2. The method for detecting a breakout according to claim 1, wherein the allowable upper limit opening is expressed by a linear equation of a parameter x consisting of variables including the casting speed, the rate of change of the molten steel level in the mold, the mold width, the mold thickness, and the weight of the molten steel in the tundish.

3. 3. The method for detecting a breakout according to claim 2, wherein the parameter x is expressed by the following equation (1): [0010] Where: V c :Casting speed (m / min) Δh: rate of change of the height of the molten metal surface in the mold (m / min) w: mold width (m) d: mold thickness (m) TD: Weight of molten steel in tundish (t)

4. The method for detecting a breakout according to claim 3, further comprising determining that the breakout has occurred if the following formula (3) is satisfied: (sn-SN)-a(xx-X)-b>0.0...(3) Where: sn: Nozzle opening (%) SN: Average nozzle opening degree (%) for 50 seconds from the start of casting X: Average value of parameter x for 50 seconds from the start of casting a: A constant corresponding to the gradient of the linear expression b: A constant corresponding to the intercept of the linear expression

5. The constants a and b are set based on multiple past operation data from 50 to 200 times, The constant a is calculated from the plurality of opening values ​​included in the plurality of operational data and the plurality of parameters x at the time of measuring the opening values ​​by a regression equation represented by a linear equation of the following formula (4):

5. The method for detecting a breakout according to claim 4, wherein the constant b is calculated by equation (5) using a constant b' calculated by equation (4). (sn-SN)=a(x-X)+b'...(4) b=b'+c・σ...(5) Where: b': A constant corresponding to the intercept of the regression equation c: a constant between 5.0 and 10.0 σ: Standard deviation of the regression equation

6. monitoring at least one of the level of the molten steel supplied into the mold at the start of casting and the opening deviation of a nozzle for adjusting the amount of the molten steel supplied into the mold; The molten metal level is equal to the lower limit H 0 If the opening deviation is less than the allowable deviation upper limit S 0 The method for detecting a breakout according to any one of claims 1 to 5, further comprising detecting that a breakout has occurred when the opening value exceeds the allowable upper limit opening in at least one of the cases where the opening value exceeds the allowable upper limit opening.

7. The allowable height lower limit H 0 is calculated by the formula (8) based on multiple operation data from the start of casting in the past, and the allowable deviation upper limit S 0 The method for detecting a breakout according to claim 6, wherein is calculated using formula (9) based on a plurality of operation data from the start of casting in the past. H 0 = H - Aσ 1 ...(8) S 0 = S + Bσ 2 ...(9) Where: H 0 : Lower limit of allowable height H: Average value of the molten metal level from multiple past operation data A: Coefficient σ 1 : Standard deviation of the mold level height from multiple past operation data S 0 : Upper limit of allowable deviation S: Average value of nozzle opening deviation from multiple past operation data B: Coefficient σ 2 : Standard deviation of nozzle opening deviation from multiple past operation data

8. monitoring at least one of the level of the molten steel supplied into the mold at the start of casting and the opening deviation of a nozzle for adjusting the amount of the molten steel supplied into the mold; The molten metal level is equal to the lower limit H 0 The opening deviation is less than the allowable deviation upper limit S 0 The method for detecting a breakout according to any one of claims 1 to 5, further comprising detecting that a breakout has occurred when the opening value exceeds the allowable upper limit opening.

9. The allowable height lower limit H 0 is calculated by the formula (8) based on multiple operation data from the start of casting in the past, and the allowable deviation upper limit S 0 The method for detecting a breakout according to claim 8, wherein is calculated using formula (9) based on a plurality of operation data from the start of casting in the past. H 0 = H - Aσ 1 ...(8) S 0 = S + Bσ 2 ...(9) Where: H 0 : Lower limit of allowable height H: Average value of the molten metal level from multiple past operation data A: Coefficient σ 1 : Standard deviation of the mold level height from multiple past operation data S 0 : Upper limit of allowable deviation S: Average value of nozzle opening deviation from multiple past operation data B: Coefficient σ 2 : Standard deviation of nozzle opening deviation from multiple past operation data

10. A method for operating a continuous casting facility for continuously casting steel, comprising the steps of: At the start of casting, detecting the breakout using the breakout detection method according to any one of claims 1 to 5; The method for operating a continuous casting facility further comprises interrupting the supply of molten steel to the mold when the breakout is detected.

11. A method for producing a cast slab, comprising the steps of: continuously casting steel using the method for operating a continuous casting facility according to claim 10 to produce the cast slab.

12. A method for operating a continuous casting facility for continuously casting steel, comprising the steps of: Detecting the breakout at the start of casting by using the breakout detection method according to claim 6; The method for operating a continuous casting facility further comprises interrupting the supply of molten steel to the mold when the breakout is detected.

13. A method for producing a slab, comprising the steps of: producing a slab by continuously casting steel using the method for operating a continuous casting facility according to claim 12.

14. A method for operating a continuous casting facility for continuously casting steel, comprising the steps of: Detecting the breakout at the start of casting by using the breakout detection method according to claim 8; The method for operating a continuous casting facility further comprises interrupting the supply of molten steel to the mold when the breakout is detected.

15. A method for producing a cast slab, comprising the steps of: continuously casting steel using the method for operating a continuous casting facility according to claim 14 to produce the cast slab.

16. A method for operating a continuous casting facility for continuously casting steel, comprising the steps of:

10. At the start of casting, detecting the breakout by using the breakout detection method according to claim 9, The method for operating a continuous casting facility further comprises interrupting the supply of molten steel to the mold when the breakout is detected.

17. A method for producing a cast slab, comprising the steps of: continuously casting steel using the method for operating a continuous casting facility according to claim 16 to produce the cast slab.

Citation Information

Patent Citations

  • Casting detect prevention apparatus for continuous casting equipment

    JP1987124055A

  • Casting method at the time of lacking in continuous casting

    JP1993305408A

  • Method for detecting breakout in continuous casting

    JP2013116481A

  • Method for controlling the level of molten metal for a continuous casting machine

    US5913357A

  • Instrument for detecting breakout

    JP1990235561A