Tube container, and article contained in container

A tube container using a combination of plant-derived polyethylene resins through compression molding addresses stress crack issues, enhancing production efficiency and durability while reducing environmental impact.

JP2024140279APending Publication Date: 2024-10-10DAIWA CAN
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023051342
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing tube containers made from petroleum-derived polyethylene resin face issues with stress cracks and are not suitable for compression molding, which limits production efficiency and resin color change capabilities.

Method used

A tube container formed by compression molding using a combination of plant-derived low-density polyethylene resin and linear low-density polyethylene resin, with specific mass ratios and layer structures, to enhance moldability and prevent stress cracks.

Benefits of technology

The solution allows for high production efficiency and ease of resin color change while preventing stress cracks, contributing to reduced CO2 emissions and improved durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140279000001_ABST
    Figure 2024140279000001_ABST
Patent Text Reader

Abstract

To provide a tube container comprising a head part whose stress crack is prevented from being generated, that is formed from a material containing a plant-derived polyethylene resin by compression-molding.SOLUTION: A tube container comprises: a tube-shaped trunk part; and a head part provided with a spout, that is connected to one end of the trunk part. The head part comprises a plant-derived low-density polyethylene resin, and a linear low-density polyethylene resin. The head part is a molded product obtained by performing molding and connection to the trunk part by compression-molding.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a tube container and a containerized article. [Background technology]

[0002] Currently available tube containers for toothpaste, cosmetics, etc. are mainly made of petroleum-derived polyethylene resin. In recent years, in order to reduce the environmental impact, the use of biomass-derived polyethylene resin, which is a carbon-neutral material, has been increasing instead of petroleum-derived polyethylene resin.

[0003] A tube container is composed of a body having a tube shape and a head having a pouring outlet. There are two known methods for forming the head of a tube container: injection molding and compression molding. In these methods, the head is molded by injection molding or compression molding so as to be joined to one end of a preformed body, and molding of the head and joining to the body are performed simultaneously. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2018-167860 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a tubular container which is formed by compression molding from a material containing a plant-derived polyethylene resin and has a head which is less susceptible to stress cracks. [Means for solving the problem]

[0006] According to one aspect, A body portion having a tube shape; a head portion having a spout and joined to one end of the body portion; Equipped with The head portion contains a plant-derived low-density polyethylene resin and a linear low-density polyethylene resin, The head portion is a molded product formed and joined to the body portion by compression molding, thereby providing a tube container.

[0007] According to another aspect, there is provided the tube container according to the above aspect, wherein the linear low-density polyethylene resin is a petroleum-derived linear low-density polyethylene resin.

[0008] According to still another aspect, there is provided the tube container according to any one of the above aspects, wherein the head portion contains the low-density polyethylene resin and the linear low-density polyethylene resin in a mass ratio of 5:95 to 95:5.

[0009] According to yet another aspect, there is provided a tube container according to any one of the above aspects, wherein the body portion is an extrusion molding.

[0010] According to yet another aspect, there is provided a tube container according to any of the above aspects, wherein the body has a five-layer structure in which an innermost layer containing a polyethylene resin, a first adhesive layer, an intermediate layer, a second adhesive layer, and an outermost layer containing a polyethylene resin are laminated in this order from the inside of the body to the outside of the body.

[0011] According to yet another aspect, there is provided a tube container according to any one of the above aspects, wherein the intermediate layer contains an ethylene-vinyl alcohol copolymer resin.

[0012] According to yet another aspect, there is provided a tube container according to any one of the above aspects, wherein each of the innermost layer and the outermost layer contains a plant-derived polyethylene resin as the polyethylene resin.

[0013] According to yet another aspect, A tube container according to any one of the above aspects; The contents filled in the tube container; and wherein the other end of the body is sealed.

[0014] According to yet another aspect, there is provided a method for producing a tube container, the method including compression molding a material containing a plant-derived low-density polyethylene resin and a linear low-density polyethylene resin at one end of a body portion having a tube shape to form a head portion having a pouring outlet and joined to the one end of the body portion.

[0015] According to yet another aspect, Manufacturing a tube container by the method according to the above aspect; Filling the tube container with a content; sealing the other end of the body after said filling; A method for manufacturing a containerized article is provided, comprising: Effect of the Invention

[0016] According to the present invention, there is provided a tube container which is formed by compression molding from a material containing a plant-derived polyethylene resin and has a head portion which is less susceptible to stress cracks. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a plan view showing a configuration of a tube container according to an embodiment of the present invention. [Diagram 2] Cross-sectional view showing the five-layer structure of the body. [Diagram 3] FIG. 4 is a cross-sectional view showing an example of a compression molding process for a tube container. [Figure 4] FIG. 4 is a cross-sectional view showing an example of a compression molding process for a tube container. [Diagram 5] 4 is a cross-sectional view showing another example of a compression molding process for a tube container. FIG. [Figure 6] 4 is a cross-sectional view showing another example of a compression molding process for a tube container. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, embodiments of the present invention will be described. The embodiments described below are more specific embodiments of any of the above aspects. The following items can be incorporated into each of the above aspects alone or in combination.

[0019] As described above, two types of methods are known for molding the head of a tube container: injection molding and compression molding. Compression molding is superior in that it can increase the production speed with fewer molds, so that production efficiency per mold is high, and that it is easy to change the color of the resin. Therefore, the present inventors tried to form the head of a tube container at one end of the body of a tube container by compression molding using a plant-derived polyethylene resin, but encountered problems such as the body (extrusion molded product) not being able to maintain its shape and being unable to be molded, or even if it was possible to mold it, there was a large molding distortion, and cracks occurred immediately after molding or after storage.

[0020] The present inventors have solved the above problems by using a plant-derived low-density polyethylene resin in combination with a linear low-density polyethylene resin, and have thus completed the present invention.

[0021] 1. Tube container According to one aspect, A body portion having a tube shape; a head portion having a spout and joined to one end of the body portion; Equipped with The head portion contains a plant-derived low-density polyethylene resin and a linear low-density polyethylene resin, The head portion is a molded product formed and joined to the body portion by compression molding, thereby providing a tube container.

[0022] In this specification, the term "tube container" refers to a tube container before being filled with a content, i.e., a tube container before the other end of the body (i.e., the end on the side where the head is not joined) is sealed. In this specification, a tube container after being filled with a content is referred to as a "container-packed article."

[0023] 1-1.Structure The structure of a tube container according to one embodiment of the present invention will be described below with reference to Fig. 1. Fig. 1 is a plan view showing the configuration of a tube container according to one embodiment of the present invention.

[0024] As shown in FIG. 1, the tube container 10 includes a body 11 and a head 12 joined to one end of the body 11. As described above, the tube container 10 is a tube container before being filled with the contents. The tube container 10 is used by filling the body 11 with the contents, sealing the other end of the body 11, and fitting a cap onto the head 12. Here, the contents may be a high-viscosity liquid or a semi-solid. The contents are, for example, cosmetics. Specific examples of the contents include moisturizing cream, face wash, cleansing agent, sunscreen, shaving agent, hair styling agent, hair care agent, and foundation.

[0025] The body 11 has a tubular shape. The body 11 is, for example, an extrusion molded product. The body 11 is preferably an extrusion molded product having a multi-layer structure. The layer structure and resin composition of the body 11 will be described later.

[0026] The head 12 is joined to one end of the body 11, and the other end of the body 11 is open and not sealed. The unsealed end of the body 11 has a circular or elliptical cylindrical shape when viewed from the opening. The body 11 has a circumferential length of, for example, 30 to 190 mm, preferably 40 to 160 mm. The circumferential length refers to the outer periphery of the tube container 10.

[0027] The head 12 is a molded product formed by compression molding and joining to the body 11. The resin composition of the head 12 and the method of compression molding will be described later. The head 12 may be a screw-type, or a stopper-type, which is driven in.

[0028] The head 12 has a shoulder 31 that is integrally continuous with one end of the body 11, and a cylindrical mouth 32 provided in the center of the shoulder 31. The head 12 has a spout at the cylindrical mouth 32.

[0029] The shoulder 31 has an outer surface facing the exterior space of the tube container 10 and an inner surface facing the interior space of the tube container 10, each of which has a truncated cone shape tapering from the interior space to the exterior space. The outer peripheral edge of the shoulder 31 is continuous with the body 11. The mouth 32 is provided at the center of the shoulder 31 so as to protrude outward.

[0030] 1-2. Resin composition of the head The head portion 12 includes a plant-derived low-density polyethylene resin (biomass LDPE) and a linear low-density polyethylene resin (L-LDPE). The linear low-density polyethylene resin (L-LDPE) may be a plant-derived linear low-density polyethylene resin (biomass L-LDPE) or a petroleum-derived linear low-density polyethylene resin (petroleum L-LDPE). According to one embodiment, the linear low-density polyethylene resin is a petroleum-derived linear low-density polyethylene resin (petroleum L-LDPE).

[0031] The head 12 can contain a plant-derived low-density polyethylene resin (biomass LDPE) and a linear low-density polyethylene resin (L-LDPE) in a mass ratio of, for example, 5:95 to 95:5, preferably 10:90 to 90:10, and more preferably 30:70 to 70:30.

[0032] When the linear low-density polyethylene resin (L-LDPE) is a petroleum-derived linear low-density polyethylene resin (petroleum L-LDPE), in order to increase the biomass content, the plant-derived low-density polyethylene resin (biomass LDPE) and petroleum-derived linear low-density polyethylene resin (petroleum L-LDPE) can be contained in a mass ratio of preferably 50:50 to 95:5, more preferably 50:50 to 90:10, and even more preferably 50:50 to 70:30.

[0033] The proportion of polyethylene resin in the head 12 is, for example, 51% by mass or more, and preferably 70% by mass or more. In this manner, the head 12 is mainly composed of polyethylene resin, but may contain known additives in addition to the polyethylene resin as necessary.

[0034] As the additive, various additives known as resin additives can be used. Examples of the additive include antioxidants, ultraviolet absorbers, weathering agents, antistatic agents, fillers, crystal nucleating agents, color pigments, matting agents, coloring inhibitors, anti-fogging agents, flame retardants, anti-blocking agents, lubricants (including slip agents and release agents), and CO2 absorbers. The total content of the additives can be, for example, 0.01 to 10 parts by mass relative to 100 parts by mass of the polyethylene resin.

[0035] Below, we will explain the structural differences between "low-density polyethylene resin (LDPE)" and "linear low-density polyethylene resin (L-LDPE)", and then provide specific explanations about "plant-derived low-density polyethylene resin (biomass LDPE)", "plant-derived linear low-density polyethylene resin (biomass L-LDPE)", and "petroleum-derived linear low-density polyethylene resin (petroleum L-LDPE)".

[0036] Low-density polyethylene resin (LDPE) and linear low-density polyethylene resin (L-LDPE) are structurally different due to differences in the manufacturing methods. That is, low-density polyethylene resin (LDPE) is a polymer of ethylene, and has a structure in which ethylene is randomly branched and bonded. For this reason, low-density polyethylene resin (LDPE) has side chains with various carbon numbers bonded to the main chain, and the side chains include short-chain branches (e.g., short-chain branches with about 20 carbon atoms or less) and long-chain branches (e.g., long-chain branches with more than about 20 carbon atoms). On the other hand, linear low-density polyethylene resin (L-LDPE) is a copolymer of ethylene and α-olefin. For this reason, linear low-density polyethylene resin (L-LDPE) does not have long-chain branches (e.g., long-chain branches with more than about 20 carbon atoms) bonded to the main chain, but only short-chain branches (e.g., short-chain branches with about 20 carbon atoms or less) bonded.

[0037] "Plant-derived low-density polyethylene resin (biomass LDPE)" "Plant-derived low-density polyethylene resin (biomass LDPE)" is an ethylene polymer produced using plants as a raw material, and has a structure in which ethylene is randomly branched and bonded. "Plant-derived low-density polyethylene resin (biomass LDPE)" is, for example, a low-density polyethylene resin derived from sugarcane. Sugarcane-derived low-density polyethylene resin is an ethylene polymer produced using sugarcane as a raw material, and has a structure in which ethylene is randomly branched and bonded.

[0038] The density of "plant-derived low-density polyethylene resin (biomass LDPE)" is 0.91 g / cm 3 ~0.93g / cm 3 and preferably in the range of 0.915 g / cm 3 ~0.93g / cm 3 It is more preferable that the density of the resin described in this specification is a measured value obtained by a method in accordance with JIS K7112:1999.

[0039] The melt flow rate (MFR) of the "plant-derived low density polyethylene resin (biomass LDPE)" is preferably within the range of 0.1 g / 10 min to 10 g / 10 min, and more preferably within the range of 1 g / 10 min to 5 g / 10 min. The melt flow rate (MFR) of the resin described in this specification is a measured value obtained by a method conforming to JIS K7210:1999. Specifically, the melt flow rate is a measured value of the weight of the resin extruded in 10 minutes when a load of 21.18 N is applied to the resin at 190°C.

[0040] As the "plant-derived low-density polyethylene resin (biomass LDPE)", for example, plant-derived low-density polyethylene sold by Braskem can be used, and examples of such resins include those sold under the trade names SEB853, SBC818, SBF0323HC, STN7006, and SPB618.

[0041] "Plant-derived linear low-density polyethylene resin (biomass L-LDPE)" "Plant-derived linear low-density polyethylene resin (biomass L-LDPE)" is a copolymer of ethylene and α-olefin produced using plants as a raw material. "Plant-derived linear low-density polyethylene resin (biomass L-LDPE)" is, for example, a linear low-density polyethylene resin derived from sugarcane. Sugarcane-derived linear low-density polyethylene resin is a copolymer of ethylene and α-olefin produced using sugarcane as a raw material.

[0042] The "α-olefin" is at least one compound selected from the group consisting of α-olefins having 3 to 20 carbon atoms, and examples thereof include 1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene.

[0043] The density of "plant-derived linear low-density polyethylene resin (biomass L-LDPE)" is 0.91 g / cm 3 ~0.93g / cm 3 and preferably in the range of 0.915 g / cm 3 ~0.93g / cm 3 In addition, the melt flow rate (MFR) of the "plant-derived linear low-density polyethylene resin (biomass L-LDPE)" is preferably in the range of 0.1 g / 10 min to 10 g / 10 min, and more preferably in the range of 1 g / 10 min to 5 g / 10 min.

[0044] As the "plant-derived linear low-density polyethylene resin (biomass L-LDPE)", for example, plant-derived linear low-density polyethylene sold by Braskem can be used, and examples thereof include resins sold under the trade names SLL118, SLL118 / 21, SLL218, SLL218 / 21, SLL318, SLH118, SLH218, and SLH0820 / 30AF.

[0045] "Petroleum-derived linear low-density polyethylene resin (petroleum L-LDPE)" "Petroleum-derived linear low-density polyethylene resin (petroleum L-LDPE)" is a copolymer of ethylene and α-olefins produced using petroleum as a raw material.

[0046] The "α-olefin" is at least one compound selected from the group consisting of α-olefins having 3 to 20 carbon atoms, and examples thereof include 1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene.

[0047] The density of "petroleum-derived linear low-density polyethylene resin (petroleum L-LDPE)" is 0.91 g / cm 3 ~0.93g / cm 3 and preferably in the range of 0.915 g / cm 3 ~0.93g / cm 3 In addition, the melt flow rate (MFR) of the "petroleum-derived linear low-density polyethylene resin (petroleum L-LDPE)" is preferably within a range of 0.1 g / 10 min to 10 g / 10 min, and more preferably within a range of 1 g / 10 min to 5 g / 10 min.

[0048] The "petroleum-derived linear low-density polyethylene resin (petroleum L-LDPE)" can be a commercially available petroleum-derived linear low-density polyethylene resin, examples of which include resins sold under the trade names EVOLUE (registered trademark), NEOZEX (registered trademark), or ULTOZEX (registered trademark) by Prime Polymer Co., Ltd., and resins sold under the trade name NOVATEC (registered trademark) by Japan Polyethylene Co., Ltd.

[0049] 1-3. Layer structure and resin composition of the body The body 11 may be a product obtained by rolling laminated sheets into a tube shape, or may be an extrusion molded product. The body 11 is preferably an extrusion molded product.

[0050] When the body 11 is an extrusion molded product, there are no overlapping parts (i.e., seams) as seen in the body of a laminated tube, and a seamless appearance can be achieved. Furthermore, when the body 11 is an extrusion molded product, it is easier to make it thicker than the body of a laminated tube, and even a tube container with a large diameter can maintain sufficient strength.

[0051] In this specification, the term "extrusion molded product" refers to a product formed into a tubular shape by extrusion molding. In other words, the term "extrusion molded product" refers to a product that has a tubular shape immediately after extrusion molding. Therefore, the term "extrusion molded product" does not include a product that is extruded into a sheet shape and then rolled into a tubular shape.

[0052] The following describes the layer structure and resin composition of the body 11. There are no particular limitations on the layer structure and resin composition of the body 11. The body 11 may have a single-layer structure or a multi-layer structure.

[0053] In a preferred embodiment, the body 11 has a five-layer structure. Fig. 2 is a cross-sectional view showing the five-layer structure of the body 11. As shown in Fig. 2, the body 11 has a five-layer structure in which an innermost layer 1a containing a polyethylene resin, a first adhesive layer 1b, an intermediate layer 1c, a second adhesive layer 1d, and an outermost layer 1e containing a polyethylene resin are laminated in this order from the inside of the body 11 to the outside of the body 11. In the body 11 shown in Fig. 2, the surface on the innermost layer 1a side is adjacent to the internal space of the tube container 10, and the surface on the outermost layer 1e side is adjacent to the external space of the tube container 10.

[0054] The body 11 has a thickness of, for example, 190 to 550 μm, and preferably 240 to 500 μm. The thickness refers to the thickness of the wall of the tube container 10, and is the average value of thicknesses measured at three points set at approximately equal intervals along the longitudinal direction of the body 11.

[0055] The innermost layer 1a has a thickness of, for example, 120 to 250 μm. The first adhesive layer 1b has a thickness of, for example, 1 to 30 μm. The intermediate layer 1c has a thickness of, for example, 10 to 100 μm. The second adhesive layer 1d has a thickness of, for example, 1 to 30 μm. The outermost layer 1e has a thickness of, for example, 60 to 200 μm.

[0056] (Innermost layer 1a) The innermost layer 1a contains a plant-derived polyethylene resin. In a preferred embodiment, the innermost layer 1a contains a plant-derived low-density polyethylene resin (biomass LDPE) and a plant-derived linear low-density polyethylene resin (biomass L-LDPE). The innermost layer 1a contains the plant-derived low-density polyethylene resin (biomass LDPE) and the plant-derived linear low-density polyethylene resin (biomass L-LDPE) in a mass ratio of, for example, 9:1 to 4:6.

[0057] (1st adhesive layer 1b) The first adhesive layer 1b serves to bond the innermost layer 1a to the intermediate layer 1c. The first adhesive layer 1b contains a petroleum-derived adhesive polyethylene resin (adhesive PE), for example, a petroleum-derived maleic anhydride-modified polyethylene resin (MA-modified PE).

[0058] (middle layer 1c) The intermediate layer 1c preferably contains a resin having gas barrier properties, for example, an ethylene-vinyl alcohol copolymer resin (EVOH).

[0059] (2nd adhesive layer 1d) The second adhesive layer 1d serves to bond the outermost layer 1e to the intermediate layer 1c. The second adhesive layer 1d contains a petroleum-derived adhesive polyethylene resin (adhesive PE), for example, a petroleum-derived maleic anhydride-modified polyethylene resin (MA-modified PE). The second adhesive layer 1d may have the same resin composition as the first adhesive layer 1b, or may have a different resin composition from the first adhesive layer 1b.

[0060] (outermost layer 1e) The outermost layer 1e contains a plant-derived polyethylene resin. In a preferred embodiment, the outermost layer 1e contains a plant-derived low-density polyethylene resin (biomass LDPE) and a plant-derived linear low-density polyethylene resin (biomass L-LDPE). The outermost layer 1e contains the plant-derived low-density polyethylene resin (biomass LDPE) and the plant-derived linear low-density polyethylene resin (biomass L-LDPE) in a mass ratio of, for example, 9:1 to 4:6. The outermost layer 1e may have the same resin composition as the innermost layer 1a, or may have a different resin composition from the innermost layer 1a.

[0061] (Additives) The innermost layer 1a, the first adhesive layer 1b, the intermediate layer 1c, the second adhesive layer 1d, and the outermost layer 1e are mainly composed of resin, but may contain known additives in addition to the resin as necessary. As the additives, various additives known as resin additives can be used. Examples of the additives include antioxidants, ultraviolet absorbers, weathering agents, antistatic agents, fillers, crystal nucleating agents, color pigments, matting agents, coloring inhibitors, anti-fogging agents, flame retardants, anti-blocking agents, lubricants (including slip agents and release agents), and CO2 absorbers. The total content of the additives can be, for example, 0.01 to 10 parts by mass with respect to 100 parts by mass of the resin of each layer.

[0062] The above-mentioned five-layer structure is collectively described below as Layer Structure A: Layer structure A (5 layer structure) Innermost layer: A mixture of plant-derived low-density polyethylene resin (plant LDPE) and plant-derived linear low-density polyethylene resin (biomass L-LDPE) First adhesive layer: Petroleum-derived adhesive polyethylene resin (adhesive PE) Middle layer: Ethylene-vinyl alcohol copolymer resin (EVOH) Second adhesive layer: Petroleum-derived adhesive polyethylene resin (adhesive PE) Outermost layer: A mixture of plant-derived low-density polyethylene resin (plant-LDPE) and plant-derived linear low-density polyethylene resin (biomass L-LDPE).

[0063] The body portion 11 is not limited to the above-mentioned layer structure A, and may have any of the following layer structures B to H. In the following layer structures B to H, in the case of a multi-layer structure, the resins constituting each layer are described in the order of lamination from the inside of the body portion 11 to the outside of the body portion 11.

[0064] Layer structure B (3 layer structure) Inner layer: A mixture of petroleum-derived adhesive low-density polyethylene resin (adhesive LDPE) and plant-derived linear low-density polyethylene resin (biomass L-LDPE) Middle layer: Ethylene-vinyl alcohol copolymer resin (EVOH) Outer layer: A mixture of petroleum-derived adhesive low-density polyethylene resin (adhesive LDPE) and plant-derived linear low-density polyethylene resin (biomass L-LDPE).

[0065] Layer structure C (2 layer structure) Inner layer: Petroleum-derived high-density polyethylene resin (petroleum HDPE) Outer layer: A mixture of petroleum-derived linear low-density polyethylene resin (petroleum L-LDPE) and plant-derived low-density polyethylene resin (biomass LDPE).

[0066] Layer structure D (single layer structure) Single layer: A mixture of petroleum-derived low-density polyethylene resin (petroleum LDPE), petroleum-derived linear low-density polyethylene resin (petroleum L-LDPE), and plant-derived low-density polyethylene resin (biomass LDPE).

[0067] Layer structure E (5 layer structure) Innermost layer: Low density polyethylene resin (LDPE) First adhesive layer: Petroleum-derived adhesive polyethylene resin (adhesive PE) Middle layer: Ethylene-vinyl alcohol copolymer resin (EVOH) Second adhesive layer: Petroleum-derived adhesive polyethylene resin (adhesive PE) Outermost layer: Low density polyethylene resin (LDPE) In the layer structure E, the low density polyethylene resin (LDPE) may be any one of petroleum LDPE, biomass LDPE, and a mixture of petroleum LDPE and biomass LDPE.

[0068] Layer structure F (3 layer structure) Inner layer: A mixture of petroleum-derived adhesive low-density polyethylene resin (adhesive LDPE) and petroleum-derived adhesive linear low-density polyethylene resin (adhesive L-LDPE) Middle layer: Ethylene-vinyl alcohol copolymer resin (EVOH) Outer layer: A mixture of petroleum-derived adhesive low-density polyethylene resin (adhesive LDPE) and petroleum-derived adhesive linear low-density polyethylene resin (adhesive L-LDPE).

[0069] Layer structure G (2 layer structure) Inner layer: High density polyethylene resin (HDPE) Outer layer: Low density polyethylene resin (LDPE) In the layer structure G, the high density polyethylene resin (HDPE) may be any of petroleum HDPE, biomass HDPE, and a mixture of petroleum HDPE and biomass HDPE. In the layer structure G, the low density polyethylene resin (LDPE) may be any of petroleum LDPE, biomass LDPE, and a mixture of petroleum LDPE and biomass LDPE.

[0070] Layer structure H (single layer structure) Single layer: Low density polyethylene resin (LDPE) In layer structure H, the low density polyethylene resin (LDPE) may be any one of petroleum LDPE, biomass LDPE, and a mixture of petroleum LDPE and biomass LDPE.

[0071] Of the above-mentioned layer structures A to H, from the viewpoint of increasing the biomass ratio, it is preferable to employ a layer structure containing a polyethylene resin derived from plants.

[0072] When the body 11 is an extrusion molded product having a multi-layer structure, the extrusion molded product can be manufactured according to a known co-extrusion method, that is, by extruding resin materials for each layer into a single die using separate extruders and forming a multi-layered tubular shape within the die.

[0073] The body 11 may further include one or more additional layers on the outer surface of the tube-shaped resin molded product (e.g., extrusion molded product). The additional layers can be formed according to known decoration techniques, for example, by printing (e.g., offset printing, screen printing), painting (e.g., clear coating for protecting the surface of the printed layer, UV coating), labeling, hot stamping, shrink film application, vapor deposition, or film transfer.

[0074] 2. Manufacturing method of tube containers The above-mentioned tube container 10 can be manufactured by compression molding a resin material for forming the head 12 at one end of the body 11 to form the head 12 joined to one end of the body 11. Therefore, according to another aspect, there is provided a method for manufacturing a tube container, which includes compression molding a material containing a plant-derived low-density polyethylene resin and a linear low-density polyethylene resin at one end of a body having a tube shape to form a head having a pouring outlet and joined to the one end of the body.

[0075] 2-1. An example of the compression molding process for tube containers An example of a compression molding process for the tube container 10 will be described below with reference to Figures 3 and 4. Figure 3 shows the state before compression molding, and Figure 4 shows the state after compression molding.

[0076] As shown in FIG. 3, the compression molding apparatus includes a convex die 50, a concave die 60, an orifice 70, and a moving mechanism 80.

[0077] The convex die 50 includes a mandrel 51, a punch 52, and a pressing shaft 53. The mandrel 51 has a tip that tapers to correspond to the inner peripheral edge of the head 12, and has a through hole extending from the tip to the other end. The mandrel 51 is installed so as to be movable up and down so that the tip faces downward. The pressing shaft 53 is installed in the through hole of the mandrel 51. The pressing shaft 53 is movable in its axial direction within the through hole of the mandrel 51. The punch 52 is supported by one end of the pressing shaft 53 on the tip side of the mandrel 51, and is movable together with the pressing shaft 53 in its axial direction within the through hole of the mandrel 51. The lower surface of the punch 52 has a shape in which the center portion protrudes downward in correspondence with the inner central portion of the head 12.

[0078] The concave die 60 has a cavity having a shape corresponding to the outer surface of the head 12. The concave die 60 is placed directly below the convex die 50 with the cavity facing upward.

[0079] The orifice 70 is a rod-like member having a cylindrical shape, and the tip side surface has a shape corresponding to the inner surface of the mouth portion 32. The orifice 70 is installed so that the tip is located within the cavity of the concave die 60. The orifice 70 is vertically movable and is biased upward.

[0080] The movement mechanism 80 moves the convex die 50 up and down. In addition, the movement mechanism 80 moves the pressing shaft 53 relatively to the mandrel 51 in the axial direction.

[0081] Prior to compression molding using the compression molding device shown in FIG. 3, a cylindrical body portion 11 is molded by extrusion molding.

[0082] 3, the cylindrical body 11 is placed so as to cover the periphery of a cylindrical mandrel 51 and so that the lower end face is positioned slightly below the lower end of the mandrel 51. At this time, the relative position of the punch 52 with respect to the mandrel 51 is set, for example, above the lowest point.

[0083] Furthermore, the resin material 12a for forming the head 12 is placed in the cavity of the concave mold 60. Here, the resin material 12a is doughnut-shaped and placed so that the cylindrical orifice 70 passes through its hole. Here, the resin material 12a is preheated to a temperature of, for example, 200 to 300°C. The resin material 12a is used in an amount of, for example, 0.3 to 5.0 g. Furthermore, the temperature of the concave mold 60 is set to a temperature of, for example, 10 to 40°C.

[0084] Next, the moving mechanism 80 operates to move the convex die 50 downward. Specifically, the moving mechanism 80 operates to move the mandrel 51, the punch 52, and the pressing shaft 53 downward as one body. When the convex die 50 moves downward, the lower end of the body 11 is bent along the shape of the cavity. Also, when the convex die 50 moves downward, the punch 52 brings the center of its lower surface into contact with the upper end surface of the orifice 70, and then presses the orifice 70 down.

[0085] Next, the moving mechanism 80 operates to move the punch 52 downward while keeping the position of the mandrel 51 fixed. This causes the punch 52 to further press down the orifice 70 and to flow the resin material 12a so that it spreads between the convex die 50 and the concave die 60. A part of the flowed resin material 12a melts the inner surface of the lower end portion of the body portion 11. The resin material 12a is then cooled and solidified, thereby obtaining the head portion 12 made of the resin material 12a and integrated with the body portion 11, as shown in FIG. 3.

[0086] Next, the moving mechanism 80 operates to move the convex die 50 upward. After that, the molded product is removed from the convex die 50. In this manner, a tube container without a step at the joint between the head part 12 and the body part 11 is obtained.

[0087] 2-2. Another example of compression molding process for tube containers Another example of the compression molding process for the tube container 10 is shown in Figures 5 and 6. Figure 5 shows the state before compression molding, and Figure 6 shows the state after compression molding.

[0088] In the compression molding apparatus shown in Fig. 5, the convex die 50 and the concave die 60 are arranged upside down compared to the compression molding apparatus shown in Fig. 3. At this time, in the convex die 50, the punch 52 is set to be, for example, at the uppermost position relative to the mandrel 51. Also, in the compression molding apparatus shown in Fig. 5, the movement mechanism 80 moves the concave die 60 up and down, not the convex die 50. Except for these points, the compression molding apparatus shown in Fig. 5 has the same structure as the compression molding apparatus shown in Fig. 3.

[0089] Regarding the operation of the compression molding apparatus shown in FIG. 5, only the points that differ from the operation of the compression molding apparatus shown in FIG. 3 will be explained below.

[0090] In this example, after the cylindrical body 11 is placed around a mandrel 51, as shown in FIG. 5, a doughnut-shaped resin material 12a is placed so that the protruding part of a punch 52 passes through the hole of the doughnut-shaped resin material 12a.

[0091] Next, the movement mechanism 80 operates to move the concave die 60 downward. When the concave die 60 moves downward, the upper end of the body portion 11 is bent along the shape of the cavity. Furthermore, when the concave die 60 moves downward, the resin material 12a flows so as to spread between the convex die 50 and the concave die 60. A portion of the flowing resin material 12a melts the inner surface of the upper end portion of the body portion 11.

[0092] Thereafter, the resin material 12a is cooled and solidified to obtain a head 12 made of the resin material 12a and integrated with the body 11, as shown in Fig. 6. The tube container thus obtained also has no step at the joint between the head 12 and the body 11.

[0093] 3. Containerized goods and their manufacturing method A containerized article can be obtained by filling the above-mentioned tube container 10 with contents and sealing the other end of the body 11 of the tube container (i.e., the end on the side where the head 12 is not joined). Therefore, according to another aspect, there is provided a containerized article comprising the above-mentioned tube container and contents filled in the tube container, and the other end of the body is sealed. According to yet another aspect, there is provided a method for manufacturing a containerized article, including manufacturing a tube container by the method described in the section "2. Method for manufacturing tube container", filling the tube container with contents, and sealing the other end of the body after the filling.

[0094] As described above, the contents may be a high-viscosity liquid or a semi-solid. The contents may be, for example, cosmetics. Specific examples of the contents include moisturizing cream, face wash, cleansing agent, sunscreen, shaving agent, hair styling agent, hair care agent, foundation, etc.

[0095] The sealing can be performed by a known method for end sealing of tube containers, for example, a heat sealing method, an ultrasonic sealing method, or a hot air sealing method, thereby sealing the other end of the body portion 21.

[0096] 4.Effects As described above, the plant-derived polyethylene resin has a problem that it cannot be molded when compression molded, or even if it can be molded, the molding distortion is large, and cracks occur immediately after molding or after storage. In contrast, the tube container of the present invention is manufactured by forming a head part at one end of a body part by compression molding using a plant-derived polyethylene resin, but the problem of not being able to perform compression molding can be solved by using a combination of two specific types of plant-derived polyethylene resins. Therefore, the present invention can enjoy the advantages of the compression molding method, such as high production efficiency per mold because the production speed can be increased with a small number of molds, and easy color change of the resin. In addition, the tube container of the present invention can prevent cracks from occurring immediately after compression molding or after storage by using a combination of two specific types of plant-derived polyethylene resins as the resin material for the head part, and can achieve the effect of making stress cracks less likely to occur. Furthermore, since the tube container of the present invention contains a plant-derived polyethylene resin, it can contribute to reducing CO2 emissions compared to the case of a petroleum-derived polyethylene resin. EXAMPLES

[0097] [1] Manufacturing of tube containers [1-1] Example 1 A tube container having the structure shown in FIG. 1 was manufactured by the following procedure.

[0098] First, a body portion having the following five-layer structure (see Figure 2) was manufactured. Innermost layer 1a: Plant-derived low-density polyethylene resin (density: 0.923 g / cm 3 , MFR: 2.7g / 10min (190℃, 21.18N load)) and plant-derived linear low-density polyethylene resin (density: 0.916g / cm 3 , MFR: 2.3 g / 10 min (190°C, 21.18 N load)) in a mass ratio of 50:50. First adhesive layer 1b: petroleum-derived maleic anhydride-modified low-density polyethylene (density: 0.93 g / cm 3, MFR: 1.0g / 10min (210℃, 21.18N load) Intermediate layer 1c: Ethylene-vinyl alcohol copolymer (density: 1.14 g / cm 3 , MFR: 12.0g / 10min (210℃, 21.18N load) Second adhesive layer 1d: petroleum-derived maleic anhydride-modified low-density polyethylene (density: 0.93 g / cm 3 , MFR: 1.0g / 10min (210℃, 21.18N load) Outermost layer 1e: Plant-derived low-density polyethylene resin (density: 0.923 g / cm 3 , MFR: 2.7g / 10min (190℃, 21.18N load)) and plant-derived linear low-density polyethylene resin (density: 0.916g / cm 3 , MFR: 2.3 g / 10 min (190°C, 21.18 N load)) in a mass ratio of 50:50.

[0099] Specifically, the resin material (pellets) for each layer was fed into five hoppers of a single-screw tube extruder. The extruder and die temperatures were set to 170-200°C, and a tube with a five-layer structure of innermost layer / first adhesive layer / middle layer / second adhesive layer / outermost layer was molded under molding conditions of a production speed of 60 tubes / min and a take-up speed of 9.1 m / min.

[0100] The resulting tube (i.e., the body) had a circumference of 108 mm, a length of 150 mm, and an average wall thickness of 0.46 mm. The thicknesses of the innermost layer, the first adhesive layer, the intermediate layer, the second adhesive layer, and the outermost layer were 0.225 mm, 0.01 mm, 0.04 mm, 0.01 mm, and 0.175 mm, respectively.

[0101] Next, a head was molded at one end of the body using the compression molding device shown in Figure 3. The following resins were used as the resin material for forming the head.

[0102] Plant-derived low-density polyethylene resin (density: 0.923 g / cm 3, MFR: 2.7g / 10min (190℃, 21.18N load)) (hereinafter referred to as biomass LDPE) and petroleum-derived linear low-density polyethylene resin (density: 0.922g / cm 3 A mixture obtained by dry blending petroleum L-LDPE in a mass ratio of 95:5 with petroleum L-LDPE (hereinafter referred to as petroleum L-LDPE) (MFR: 1.2g / 10min (190℃, 21.18N load)).

[0103] Compression molding was performed as described above in the section "2-1. An example of a compression molding process for a tube container." The resin material was used in an amount of 1.4 g. Before compression molding, the resin material was preheated to a temperature of 260°C. The temperature of the concave mold was set to a temperature of 20°C.

[0104] [1-2] Examples 2-7 The tube containers of Examples 2 to 7 were manufactured according to the same procedure as in Example 1, except that the resin material for forming the head portion was changed to the following resin material. The "biomass LDPE" and "petroleum L-LDPE" used in Examples 2 to 7 were the same as those used in Example 1. Example 2: Mixture obtained by dry blending biomass LDPE and petroleum L-LDPE in a mass ratio of 90:10 Example 3: Mixture obtained by dry blending biomass LDPE and petroleum L-LDPE in a mass ratio of 70:30 Example 4: Mixture obtained by dry blending biomass LDPE and petroleum L-LDPE in a mass ratio of 50:50 Example 5: Mixture obtained by dry blending biomass LDPE and petroleum L-LDPE in a mass ratio of 30:70 Example 6: Mixture obtained by dry blending biomass LDPE and petroleum L-LDPE in a mass ratio of 10:90 Example 7: A mixture obtained by dry blending biomass LDPE and petroleum L-LDPE in a mass ratio of 5:95.

[0105] [1-3] Comparative Example 1 The tube container of Comparative Example 1 was produced by molding a head part by injection molding at one end of the body part produced in Example 1. Biomass LDPE was used as the resin material for forming the head part. The "biomass LDPE" used in Comparative Example 1 was the same as that used in Example 1.

[0106] [1-4] Comparative Example 2 A tube container of Comparative Example 2 was manufactured according to the same procedure as in Example 1, except that the resin material for forming the head portion was changed to biomass LDPE. The "biomass LDPE" used in Comparative Example 2 was the same as that used in Example 1.

[0107] [1-5] Comparative Example 3 A tube container of Comparative Example 3 was produced in the same manner as in Example 1, except that the resin material for forming the head portion was changed to the following biomass L-LDPE. Plant-derived linear low-density polyethylene resin (density: 0.916 g / cm 3 , MFR: 2.3g / 10min (190℃, 21.18N load).

[0108] [2] Evaluation method [2-1] Can the head be molded? The moldability of the head was evaluated as follows. Evaluation criteria ○: Molding was possible ×: Unable to mold

[0109] [2-2] Stress crack test A 10% Igepal (poly(oxyethylene) nonylphenyl ether) aqueous solution was applied to the top of the resulting tube container, and the cap was sealed with a torque of 3.2 N·cm times the cap diameter, and then the container was stored in a 65°C thermostatic chamber for a specified period of time. Tests were performed for 6 hours, 24 hours, and 30 hours of storage. After each storage period, the presence or absence of cracks was visually determined and evaluated according to the following criteria: Evaluation criteria AA: No cracks were observed after 30 hours of storage. A: No cracks were observed after 24 hours of storage, but cracks were observed after 30 hours of storage. B: No cracks were observed after 6 hours of storage, but cracks were observed after 24 hours of storage. C: Cracks were observed after 6 hours of storage.

[0110] [3] Evaluation results The evaluation results are shown in Table 1. [Table 1]

[0111] The tube container of Example 1 could be manufactured without any defects during compression molding. In addition, the tube container of Example 1 showed no cracks in a stress crack test after storage for 6 hours. The tube containers of Examples 2 to 7 could be manufactured without any defects during compression molding. In addition, the tube containers of Examples 2 to 7 showed no cracks in a stress crack test after storage for 30 hours.

[0112] On the other hand, the tube container of Comparative Example 1 had no problems in the evaluation results, but since it was manufactured by injection molding, it could not enjoy the advantages of compression molding. The tube container of Comparative Example 2 showed cracks in the stress crack test after storage for 6 hours. The tube container of Comparative Example 3 had sticky resin material that stuck to the mold during compression molding.

[0113] These results show that when biomass LDPE and biomass L-LDPE are used in combination as the resin material for the head of a tube container, it is possible to obtain a tube container with a head that can be formed by compression molding and is less susceptible to stress cracks.

[0114] Regarding the methods for mixing biomass LDPE and biomass L-LDPE, there are two methods: blending pellets and re-pelletizing after melt kneading. It was confirmed that either method can obtain the above-mentioned effect. It was also confirmed that the above-mentioned effect can be obtained when additives and colorants are mixed into the resin material used to form the head. Furthermore, regarding the methods for adding additives and colorants, there are two methods: blending master batches and re-pelletizing after melt kneading. It was also confirmed that the above-mentioned effect can be obtained with either method. [Explanation of symbols]

[0115] Reference Signs List 1a...innermost layer, 1b...first adhesive layer, 1c...middle layer, 1d...second adhesive layer, 1e...outermost layer, 10...tube container, 11...body portion, 12...head portion, 12a...resin material, 31...shoulder portion, 32...mouth portion, 50...convex die, 51...mandrel, 52...punch, 53...pressing shaft, 60...concave die, 70...orifice, 80...moving mechanism

Claims

1. A body portion having a tube shape; a head portion having a spout and joined to one end of the body portion; Equipped with The head portion contains a plant-derived low-density polyethylene resin and a linear low-density polyethylene resin, The head portion of the tube container is a molded product that is formed and joined to the body portion by compression molding.

2. 2. The tube container according to claim 1, wherein the linear low-density polyethylene resin is a petroleum-derived linear low-density polyethylene resin.

3. 2. The tube container according to claim 1, wherein the head portion contains the low-density polyethylene resin and the linear low-density polyethylene resin in a mass ratio of 5:95 to 95:

5.

4. 2. The tube container according to claim 1, wherein the body portion is an extrusion molding.

5. 2. The tube container according to claim 1, wherein the body portion has a five-layer structure in which an innermost layer containing a polyethylene resin, a first adhesive layer, an intermediate layer, a second adhesive layer, and an outermost layer containing a polyethylene resin are laminated in this order from the inside of the body portion to the outside of the body portion.

6. 6. The tube container according to claim 5, wherein the intermediate layer contains an ethylene-vinyl alcohol copolymer resin.

7. 6. The tube container according to claim 5, wherein each of the innermost layer and the outermost layer contains a plant-derived polyethylene resin as the polyethylene resin.

8. A tube container according to any one of claims 1 to 7; The contents filled in the tube container; and the other end of the body is sealed.

9. A method for manufacturing a tube container includes compression molding a material containing a plant-derived low-density polyethylene resin and a linear low-density polyethylene resin at one end of a body portion having a tube shape to form a head portion having a pouring outlet and joined to the one end of the body portion.

10. Producing a tube container according to the method of claim 9; Filling the tube container with a content; sealing the other end of the body after said filling; A method for manufacturing a containerized article, comprising:

Citation Information

Patent Citations

  • Tube container

    JP2018167860A