Method for producing molded product, set of compositions for obtaining optically transparent resin composition, optically transparent resin composition, and kit
Patent Information
- Application Number
- JP2023051658
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-03-28
AI Technical Summary
【0010】 本発明によれば、耐熱性を有しつつ、変色が抑制された成形体の製造方法、組成物セット、光透過性樹脂組成物及びキットを提供することができる。
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a molded article, a set of compositions for obtaining a light-transmitting resin composition, a light-transmitting resin composition, and a kit. [Background technology]
[0002] Laser welding is known as one method for joining thermoplastic resin parts together. In laser welding, a transparent material that transmits laser light is overlapped with an absorbing material that absorbs the laser light, and the laser light is irradiated through the transparent material. The absorbing material then absorbs the laser light, generating heat, melting the resin at the interface between the transparent and absorbing materials, and bonding the transparent and absorbing materials together. Advantages of this method include the reduction in the number of parts and weight reduction compared to fixing with bolts, and the absence of burrs compared to vibration welding.
[0003] As a transparent material to be welded by the laser welding method, Patent Document 1 discloses a thermoplastic resin composition containing a thermoplastic resin and a black colorant having a specific metal azo complex dye. In the examples of this document, polyamide 6 is used as the thermoplastic resin. However, since aliphatic polyamides such as polyamide 6 do not have sufficient heat resistance, the use of semi-aromatic polyamides is being considered.
[0004] Patent Document 2 describes a composition that contains a polyamide resin (A) having a melting point of 300° C. or higher, a light-transmitting dye (C), and a fibrous filler (D), and has a corrected heat of fusion (ΔH R A polyamide resin composition is disclosed in which the melting point of the polyamide resin (A) is adjusted to 10 J / g or more and 70 J / g or less. A semi-aromatic polyamide is used as the polyamide resin (A) having a melting point of 300° C. or more. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Special Publication No. 2003-522269 [Patent Document 2] International Publication No. 2019 / 160117 Summary of the Invention [Problem to be solved by the invention]
[0006] These transparent materials (molded bodies) are usually produced by melt-kneading polyamide resin and light-transmitting dye in a molding machine such as an extruder to form pellets, and then molding the pellets in a molding machine such as an injection molding machine. In the process of molding the molded body, the operation of the molding machine may be temporarily stopped during the production for maintenance of the molding machine, and then the operation may be restarted.
[0007] However, when a polyamide resin having a melting point of 310°C or more is used, the color of the polyamide resin composition is likely to change if the residence time in the molding machine is long, and the color of the molded product may be impaired. This phenomenon was not observed when a polyamide resin having a melting point lower than 310°C was used, and was specific to the use of a polyamide resin having a melting point of 310°C or more.
[0008] The present invention has been made in consideration of the above circumstances, and aims to provide a method for producing a molded body that has heat resistance while suppressing discoloration, a set of compositions for obtaining a light-transmitting resin composition, and a light-transmitting resin composition and a kit. [Means for solving the problem]
[0009] [1] A method for producing a molded product, comprising the steps of: preparing pellets of a polyamide resin composition comprising (A) a polyamide resin having a melting point of 310°C or higher as measured by a differential scanning calorimeter (DSC) and (B) a fibrous filler; dry-blending the pellets of the polyamide resin composition with (C) a light-transmitting dye to obtain a light-transmitting resin composition; and molding the light-transmitting resin composition. [2] The method for producing a molded article according to [1], wherein in the step of preparing pellets of the polyamide resin composition, the polyamide resin (A) and the fibrous filler (B) are melt-kneaded to obtain the pellets. [3] The method for producing a molded article according to [1] or [2], wherein the polyamide resin (A) comprises a structural unit (Aa) derived from a dicarboxylic acid and a structural unit (Ab) derived from a diamine, the structural unit (Aa) derived from the dicarboxylic acid comprises 50 mol % or more of a structural unit derived from terephthalic acid relative to the total number of moles of the structural units (Aa) derived from the dicarboxylic acid, and the structural unit (Ab) derived from the diamine comprises at least one of a structural unit derived from an aliphatic diamine having 4 to 15 carbon atoms and a structural unit derived from an alicyclic diamine having 4 to 20 carbon atoms. [4] The method for producing a molded body according to [3], wherein the diamine-derived structural units (Ab) contain more than 50 mol% of structural units derived from a linear aliphatic diamine having 4 to 15 carbon atoms, based on the total number of moles of the diamine-derived structural units (Ab). [5] The method for producing a molded article according to any one of [1] to [4], wherein in the step of obtaining the light-transmitting resin composition, the polyamide resin composition is dry-blended with a masterbatch containing the light-transmitting dye (C) and a polyamide resin (D) having a melting point lower than 310° C. [6] The method for producing a molded article according to any one of [1] to [5], wherein the light-transmitting dye (C) contains a dye that does not have a maximum absorption wavelength in the wavelength range of 800 nm or more and 1064 nm or less. [7] The method for producing a molded article according to [6], wherein the dye that does not have a maximum absorption wavelength in the wavelength range of 800 nm or more and 1064 nm or less is at least one selected from the group consisting of perylene derivatives, pyrazolone derivatives, perinone derivatives, and anthraquinone derivatives. [8] The method for producing a molded product according to any one of [1] to [7], wherein the content of the light-transmitting dye (C) in the light-transmitting resin composition is 0.1 parts by mass or more and 5 parts by mass or less per 100 parts by mass of the light-transmitting resin composition. [9] A set of compositions for obtaining a light-transmitting resin composition, the set comprising: pellets of a polyamide resin composition comprising a polyamide resin (A) having a melting point of 310°C or higher as measured by a differential scanning calorimeter (DSC) and a fibrous filler (B); and a master batch comprising a light-transmitting dye (C) and a polyamide resin (D) having a melting point lower than 310°C.
[10] A light-transmitting resin composition comprising a dry blend of pellets of a polyamide resin composition comprising a polyamide resin (A) having a melting point of 310°C or higher as measured by a differential scanning calorimeter (DSC) and a fibrous filler (B), and a masterbatch comprising a light-transmitting dye (C) and a polyamide resin (D) having a melting point lower than 310°C.
[11] A kit for obtaining a laser-welded product, comprising the set according to [9], or the light-transmitting resin composition according to
[10] , and a light-absorbing resin composition containing a thermoplastic resin and a light-absorbing dye. Effect of the Invention
[0010] According to the present invention, it is possible to provide a method for producing a molded article that has heat resistance and is suppressed from discoloring, a composition set, a light-transmitting resin composition, and a kit. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] As described above, when pellets of a polyamide resin composition obtained by melt-kneading a polyamide resin having a melting point of 310°C or more and a light-transmitting dye are used to produce a molded article in a molding machine, if the residence time in the molding machine is long, the color of the polyamide resin composition may change, and the color of the molded article may be impaired.
[0012] The reason why this phenomenon occurs is unclear, but is speculated as follows. To melt polyamide resin, which has a melting point of 310°C or higher, it is necessary to heat it to a high temperature. When a light-transmitting dye is exposed to such high temperatures, the aromatic rings and conjugated parts contained in the light-transmitting dye undergo structural changes due to thermal and oxidative degradation at high temperatures, and the absorption wavelength changes. This type of change progresses the longer the exposure to high temperatures (the longer the thermal history), and when the exposure time exceeds a certain time, the change in structure and the change in absorption wavelength become noticeable. It is thought that this causes a decrease in transmittance at specific wavelengths and discoloration.
[0013] In contrast, in the present invention, the molding material is not a pellet obtained by melt-kneading a polyamide resin and a light-transmitting dye, but a blend obtained by dry-blending (non-melt mixing) a pellet obtained by heating and melting a polyamide resin with a light-transmitting dye. As a result, since it is necessary to melt the polyamide resin in a molding process such as injection molding, it is unavoidable that the light-transmitting dye is exposed to high temperatures, but the time during which the light-transmitting dye is exposed to high temperatures in the process prior to the molding process is shortened as much as possible. This makes it possible to prevent the light-transmitting dye from being exposed to high temperatures for a long period of time, and therefore makes it possible to suppress the change in the absorption wavelength associated with the change in the structure of the light-transmitting dye. As a result, discoloration (deterioration in color) of the resulting molded body can be suppressed.
[0014] Hereinafter, a method for producing a molded article according to one embodiment of the present invention and a molding material used therein will be specifically described.
[0015] 1. Manufacturing method of molded body A method for producing a molded product according to one embodiment of the present invention includes the steps of: 1) preparing pellets of a polyamide resin composition containing a polyamide resin (A) having a melting point of 310° C. or higher and a fibrous filler (B); 2) dry-blending the pellets of the polyamide resin composition with a light-transmitting dye (C) to obtain a light-transmitting resin composition; 3) molding the light-transmitting resin composition to obtain a molded product; Includes.
[0016] 1-1. Step of preparing pellets of polyamide resin composition The pellets of the polyamide resin composition may be commercially available or may be manufactured. In this embodiment, the pellets of the polyamide resin composition can be obtained by melt-kneading a polyamide resin (A) having a melting point of 310° C. or more and a fibrous filler (B), followed by granulation or pulverization. Each component contained in the pellets of the polyamide resin composition will be described in detail later.
[0017] The melt kneading can be carried out by a known method, for example, a method of heating and melting the components using an extruder, a kneader, a Banbury mixer, etc. Before the melt kneading, mixing may be carried out using a mixer such as a tumbler or a super mixer, if necessary.
[0018] The melting temperature during melt kneading may be any temperature at which the polyamide resin (A) can be sufficiently melted without decomposing, and may be, for example, from (Tm+5)°C to (Tm+25)°C, inclusive, where Tm (°C) is the melting point of the polyamide resin (A).
[0019] The resulting melt-kneaded product is then granulated or pulverized to obtain pellets of the polyamide resin composition. The size of the pellets is not particularly limited, but may be, for example, about 0.05 mm or more and 10 mm or less in length at the longest portion as measured with a vernier caliper.
[0020] 1-2. Dry blending process The obtained pellets of the polyamide resin composition are dry-blended with the light-transmitting dye (C) to obtain a light-transmitting resin composition. In this specification, the term "dry blend" refers to mixing the pellets of the polyamide resin composition and the light-transmitting dye (C) in a solid phase. More specifically, it refers to mixing the pellets of the polyamide resin composition and the light-transmitting dye (C) at a temperature lower than the melting point of the polyamide resin (A) contained in the pellets of the polyamide resin composition so that the polyamide resin (A) does not melt.
[0021] (Light-transmitting dye (C)) The light-transmitting dye (C) is a component for coloring the polyamide resin composition while suppressing a decrease in the transmittance of the laser light of a specific wavelength used in laser welding. That is, the light-transmitting dye (C) is a dye that is transparent to the laser light of a specific wavelength used in laser welding, and specifically, is a dye that does not have a maximum absorption wavelength in the wavelength range of 800 nm or more and 1064 nm or less.
[0022] The light-transmitting dye (C) preferably contains naphthalocyanine and its derivatives, phthalocyanine and its derivatives, porphyrin and its derivatives, perinone and its derivatives, quaterrylene and its derivatives, anthraquinone and its derivatives, pyrazolone and its derivatives, perylene and its derivatives, chromium complexes, squaric acid and its derivatives, aniline black, azo dyes, and immonium dyes. From the viewpoint of compatibility between transparency and colorability to laser light, the light-transmitting dye (C) preferably contains at least one of perylene derivatives, pyrazolone derivatives, perinone derivatives, and anthraquinone derivatives, more preferably contains at least one of perylene derivatives and anthraquinone derivatives, and particularly preferably contains an anthraquinone derivative.
[0023] The light-transmitting pigment (C) is preferably a black pigment. When the light-transmitting pigment (C) is a black pigment, a black pigment made by mixing two or more chromatic pigments may be used.
[0024] Examples of commercially available light-transmitting dyes (C) include colorants eBind ACW-9871, e-BIND LTW-8731H, and e-BIND LTW-8701H manufactured by Orient Chemical Industries Co., Ltd.
[0025] The amount of the light-transmitting dye (C) to be dry-blended may be set so that the light-transmitting resin composition obtained has a predetermined transmittance at a wavelength of 940 nm or more and exhibits a desired color, and the amount may be set so that the content of the light-transmitting dye (C) in the light-transmitting resin composition falls within the range described below.
[0026] (Dry Blend) The light-transmitting dye (C) may be directly dry-blended with the pellets of the polyamide resin composition obtained in the above step 1), or a masterbatch containing the light-transmitting dye (C) may be dry-blended. Among them, from the viewpoint of further increasing the dispersibility of the light-transmitting dye (C) in the polyamide resin composition, it is preferable to dry-blend a masterbatch containing the light-transmitting dye (C). The composition of the masterbatch will be described in detail later.
[0027] The dry blending may be a dry blending that does not involve heating and melting. The dry blending may be performed using a known mixing means, for example, a mixer such as a tumbler or a super mixer. Heating may be performed during the dry blending. When the melting point of the polyamide resin (A) is Tm (°C), the temperature of the mixture containing the pellets of the polyamide resin composition and the light-transmitting dye (C) in the dry blending step is preferably 0°C or higher (Tm-50)°C or lower, more preferably 0°C or higher (Tm-100)°C or lower, even more preferably 0°C or higher (Tm-200)°C or lower, and particularly preferably 0°C or higher (Tm-250)°C or lower.
[0028] (Light-transparent resin composition) By the above dry blending, a light-transmitting resin composition containing the polyamide resin (A), the fibrous filler (B) and the light-transmitting dye (C) is obtained.
[0029] The content of the polyamide resin (A) in the light-transmitting resin composition is preferably 45 parts by mass or more and 85 parts by mass or less, and more preferably 55 parts by mass or more and 75 parts by mass or less, relative to 100 parts by mass of the light-transmitting resin composition. When the content of the polyamide resin (A) is 45 parts by mass or more, it is easier to ensure moldability during molding. When the content of the polyamide resin (A) is 90 parts by mass or less, for example, the relative amount of the fibrous filler (B) is large, so that the mechanical strength of the molded body is easier to increase.
[0030] The content of the fibrous filler (B) in the light-transmitting resin composition is preferably 10 parts by mass or more and 50 parts by mass or less with respect to 100 parts by mass of the light-transmitting resin composition. When the content of the fibrous filler (B) is 10 parts by mass or more, the mechanical strength of the molded body is more easily increased. When the content of the fibrous filler (B) is 50 parts by mass or less, the laser light transmittance of the molded body is less likely to be impaired, and the resulting decrease in welding strength and excessive increase in viscosity during molding are less likely to occur. The content of the fibrous filler (B) is more preferably 25 parts by mass or more and 45 parts by mass or less.
[0031] The content of the light-transmitting dye (C) in the light-transmitting resin composition may be set so that the light transmittance of the obtained light-transmitting resin composition at a wavelength of 940 nm is a predetermined value or more. Specifically, the content of the light-transmitting dye (C) is preferably 0.1 parts by mass or more and 5 parts by mass or less with respect to 100 parts by mass of the light-transmitting resin composition. When the content of the light-transmitting dye (C) is 0.1 parts by mass or more, it is easier to color the resin, so that the design is more easily improved, and when the content is 5 parts by mass or less, it is possible to more effectively suppress a significant decrease in the transmittance of laser light and a significant decrease in the welding strength due to the same. The content of the light-transmitting dye (C) is preferably 0.1 parts by mass or more and 4 parts by mass or less, and more preferably 0.1 parts by mass or more and 3 parts by mass or less.
[0032] The light-transmitting resin composition may further contain other components other than those described above as necessary. Examples of other components include polymers other than the polyamide resin (A), such as polyamide resin (D) having a melting point lower than 310°C, and other polyamide resins other than the polyamide resin (A) and the polyamide resin (D). The pellets of the polyamide resin composition described above may contain other polymers other than the polyamide resin (A), or may contain the polyamide resin (D) or the other polyamide resins described above. The polyamide resin (D) is a carrier resin contained in the master batch described later, which will be described in detail later.
[0033] The content of the polyamide resin (D) in the light-transmitting resin composition is preferably 0.1 parts by mass or more and 5 parts by mass or less, and more preferably 0.5 parts by mass or more and 2 parts by mass or less, per 100 parts by mass of the total of the polyamide resin (A) and the polyamide resin (D).
[0034] The total amount of other components is preferably 5% by mass or less, and can be 0.4 to 2 parts by mass, based on 100 parts by mass of the light-transmitting resin composition.
[0035] The light-transmitting resin composition can provide a molded article with high transmittance of a laser beam of a specific wavelength used in laser welding. When the light-transmitting resin composition is molded into a molded article with a thickness of 0.7 mm, the transmittance of the molded article with a laser beam of a wavelength of 940 nm is preferably 50% or more, more preferably 60% or more, and even more preferably 70% or more. The upper limit of the transmittance of the laser beam of a wavelength of 940 nm is not particularly limited, but may be, for example, 90%. The transmittance of the laser beam of the molded article can be measured by comparing the laser beam intensity when the sample is transmitted and when the sample is not transmitted using a power meter F300-SH manufactured by Ophir Corporation.
[0036] The transmittance of a laser beam having a wavelength of 940 nm can be adjusted, for example, by the type and content of the light-transmitting dye (C). For example, decreasing the content of the light-transmitting dye (C) tends to increase the transmittance of a laser beam having a wavelength of 940 nm.
[0037] 1-3. Molding process The obtained optically transparent resin composition is molded to obtain a molded article.
[0038] The molding method is not particularly limited, and known molding methods, such as injection molding, blow molding, extrusion molding, and press molding, can be applied. Among them, injection molding is preferred from the viewpoint of good fluidity. In the injection molding method, it is preferable to adjust the resin temperature to 250°C or more and 300°C or less.
[0039] 1-4. Molded body The molded article obtained by molding the above-mentioned light-transmitting resin composition has high transmittance to laser light, and therefore the above-mentioned molded article can be preferably used as a light-transmitting resin member that transmits laser light in a laser welding method.
[0040] 2.Molding material The molding material used in the method for producing the molded article may be a set of compositions obtained by combining pellets of a polyamide resin composition containing a polyamide resin (A) and a fibrous filler (B) with a master batch containing a light-transmitting dye (C); or a light-transmitting resin composition in which pellets of the polyamide resin composition and a master batch are dry-blended in advance in a predetermined ratio.
[0041] 2-1. Composition set The set of compositions includes pellets of a polyamide resin composition and a master batch.
[0042] As described above, the pellets of the polyamide resin composition are pellets (natural pellets) obtained by melt-kneading the polyamide resin (A), the fibrous filler (B), and other components as necessary, and do not substantially contain the light-transmitting dye (C). "Substantially not containing the light-transmitting dye (C)" means that the content of the light-transmitting dye (C) is 0.05% by mass or less, preferably 0% by mass. The master batch is a colorant composition containing the light-transmitting dye (C). In step 2) of the above-mentioned method for producing a molded product, the pellets of the polyamide resin composition and the master batch can be dry-blended to obtain a light-transmitting resin composition. By adjusting the blend ratio of these, a light-transmitting resin composition having an arbitrary laser light transmittance can be prepared. Hereinafter, each composition will be described. The pellets of the polyamide resin composition are also simply called "polyamide resin composition".
[0043] 2-1-1. Pellets of polyamide resin composition The pellets of the polyamide resin composition contain a polyamide resin (A) having a melting point of 310° C. or higher, and a fibrous filler (B).
[0044] (Polyamide resin (A)) The melting point (Tm) of the polyamide resin (A) measured by a differential scanning calorimeter (DSC) is 310° C. or higher, preferably 310° C. or higher and 340° C. or lower, more preferably 310° C. or higher and 330° C. or lower. When the melting point of the polyamide resin (A) is 310° C. or higher, the heat resistance and strength of the polyamide resin composition can be increased. In addition, when the melting point is 340° C. or lower, the thermal decomposition of the polymer and various additives during melt molding of the polyamide resin composition can be further suppressed.
[0045] The melting point (Tm) and glass transition temperature (Tg) of the polyamide resin (A) can be measured, for example, using a differential scanning calorimeter (DSC220C type, manufactured by Seiko Instruments Inc.). Specifically, about 5 mg of the polyamide resin (A) is sealed in an aluminum pan for measurement and heated from room temperature to 350°C at 10°C / min. In order to completely melt the resin, it is held at 350°C for 3 minutes and then cooled to 30°C at 10°C / min. After leaving it at 30°C for 5 minutes, it is heated a second time to 350°C at 10°C / min. The temperature (°C) of the endothermic peak in this second heating is taken as the melting point (Tm). In addition, the transition point corresponding to the glass transition is taken as the glass transition temperature (Tg).
[0046] The melting point (Tm) of the polyamide resin (A) can be adjusted to the above range by adjusting the composition of the polyamide resin. For example, the melting point (Tm) can be increased by increasing the content of the structural unit derived from terephthalic acid, which will be described later.
[0047] The heat of fusion (ΔH) of the polyamide resin (A) measured by differential scanning calorimetry (DSC) is preferably more than 5 J / g. The heat of fusion is an index of the crystallinity of a resin, and the larger the heat of fusion, the higher the crystallinity. When the heat of fusion (ΔH) of the polyamide resin (A) exceeds 5 J / g, the crystallinity is higher, and the strength of the molded article can be further increased.
[0048] The heat of fusion (ΔH) is a value calculated from the area of the endothermic peak during melting in the first heating process in accordance with JIS K7122:2012.
[0049] The polyamide resin (A) preferably contains a structural unit (Aa) derived from a dicarboxylic acid and a structural unit (Ab) derived from a diamine.
[0050] (Structural unit (Aa) derived from dicarboxylic acid) The dicarboxylic acid-derived structural unit (Aa) preferably contains 40 mol% or more of aromatic dicarboxylic acid-derived structural units relative to the total number of moles of the dicarboxylic acid-derived structural units (Aa). If the content of aromatic dicarboxylic acid-derived structural units is 40 mol% or more, the crystallinity of the polyamide resin can be further increased, and the heat resistance, mechanical strength (tensile strength), and water resistance of the resulting molded article can be further increased. From the same viewpoint, the content of aromatic dicarboxylic acid-derived structural units is preferably 60 mol% or more, more preferably 80 mol% or more, even more preferably 95 mol% or more, and particularly preferably 100 mol% relative to the total number of moles of the dicarboxylic acid-derived structural units (Aa).
[0051] The dicarboxylic acid-derived structural unit (Aa) preferably contains at least a structural unit derived from terephthalic acid as an aromatic dicarboxylic acid. The polyamide resin (A) containing a structural unit derived from terephthalic acid has high crystallinity, and therefore can further improve the heat resistance, mechanical strength, and water resistance of the molded product. Examples of terephthalic acid include terephthalic acid and terephthalic acid esters.
[0052] The content of the structural unit derived from terephthalic acid is preferably 50 mol% or more, more preferably 55 mol% or more and 95 mol% or less, and even more preferably 60 mol% or more and 80 mol% or less, based on the total number of moles (Aa) of components derived from dicarboxylic acids in the polyamide resin (A). When the content of the structural unit derived from terephthalic acid is 50 mol% or more, the crystallinity of the polyamide resin (A) can be further increased.
[0053] The dicarboxylic acid-derived structural unit (Aa) may further contain a structural unit derived from a dicarboxylic acid other than the above, within a range that does not impair the effects of the present invention. The other dicarboxylic acid may be an aromatic dicarboxylic acid other than terephthalic acid, an aliphatic dicarboxylic acid, or an alicyclic dicarboxylic acid.
[0054] Examples of aromatic carboxylic acids other than terephthalic acid include isophthalic acid, 2-methylterephthalic acid, naphthalenedicarboxylic acid, etc. Among these, isophthalic acid is preferred.
[0055] The aliphatic dicarboxylic acid is an aliphatic dicarboxylic acid having 4 to 20 carbon atoms, and preferably has 6 to 12 carbon atoms. Examples of such aliphatic dicarboxylic acids include adipic acid, azelaic acid, and sebacic acid. Among these, adipic acid and sebacic acid are preferred.
[0056] Examples of the alicyclic dicarboxylic acid include 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and the like.
[0057] Of these, the other dicarboxylic acid is preferably an aromatic dicarboxylic acid other than terephthalic acid, and isophthalic acid is more preferred.
[0058] The content of the structural units derived from other dicarboxylic acids is, for example, 50 mol% or less, more preferably 5 mol% to 45 mol%, and even more preferably 20 mol% to 40 mol%, based on the total number of moles of the structural units (Aa) derived from dicarboxylic acids. For example, by including structural units derived from aromatic dicarboxylic acids other than terephthalic acid, such as isophthalic acid, in the above-mentioned content, excessive crystallization of the polyamide resin (A) can be suppressed, and the energy required to melt the crystalline portion can be reduced.
[0059] (Structural unit (Ab) derived from diamine) The diamine-derived structural unit (Ab) preferably contains at least one of a structural unit derived from an aliphatic diamine having 4 to 15 carbon atoms and a structural unit derived from an alicyclic diamine having 4 to 20 carbon atoms.
[0060] The aliphatic diamine having 4 to 15 carbon atoms preferably includes a linear aliphatic diamine having 4 to 15 carbon atoms. The linear aliphatic diamine having 4 to 15 carbon atoms may be a linear aliphatic diamine having preferably 4 to 8 carbon atoms, more preferably 6 to 8 carbon atoms. Examples of linear aliphatic diamine having 4 to 15 carbon atoms include 1,4-diaminobutane, 1,6-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane, 1,9-diaminononane, 1,10-diaminodecane, 1,11-diaminoundecane, 1,12-diaminododecane, etc. Among these, 1,6-diaminohexane, 1,9-nonanediamine, and 1,10-diaminodecane are preferred, and 1,6-diaminohexane is more preferred.
[0061] Examples of the alicyclic diamine having 4 to 20 carbon atoms include 1,3-diaminocyclohexane, 1,4-diaminocyclohexane, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, bis(4-aminocyclohexyl)methane, 4,4'-diamino-3,3'-dimethyldicyclohexylmethane, 2,5-bisaminomethylnorbornane, and 2,6-bisaminomethylnorbornane; 1,3-diaminocyclohexane, 1,4-diaminocyclohexane, bis(4-aminocyclohexyl)methane, 1,3-bis(aminocyclohexyl)methane, 2,5-bisaminomethylnorbornane, and 2,6-bisaminomethylnorbornane are preferred; and include 1,3-diaminocyclohexane, 1,4-diaminocyclohexane, bis(4-aminocyclohexyl)methane, 1,3-bis(aminocyclohexyl)methane, 2,5-bisaminomethylnorbornane, and 2,6-bisaminomethylnorbornane.
[0062] Of these, the diamine-derived structural unit (Ab) preferably contains a structural unit derived from a linear aliphatic diamine having 4 or more and 15 or less carbon atoms.
[0063] The total amount of the structural units derived from an aliphatic diamine having 4 to 15 carbon atoms and the structural units derived from an alicyclic diamine having 4 to 20 carbon atoms (preferably the content of the structural units derived from a linear aliphatic diamine having 4 to 15 carbon atoms) is preferably more than 50 mol%, more preferably 60 mol% or more, and even more preferably 90 mol% or more, and may be 100 mol%, based on the total amount of the structural units (Ab) derived from the diamine. When the above total amount exceeds 50 mol%, the heat resistance, mechanical strength, and water resistance of the obtained molded body are more likely to be improved.
[0064] The diamine-derived structural unit (Ab) may further contain a structural unit derived from another diamine other than the above, within a range that does not impair the effects of the present invention. Examples of the other diamine include aromatic diamines. The content of the structural unit derived from the other diamine may be less than 50 mol%, preferably 40 mol% or less, more preferably 10 mol% or less, based on the total number of moles of the diamine-derived structural unit (Ab).
[0065] The respective constituent units of the polyamide resin (A) and the ratio thereof can be calculated from the charge ratio when the polyamide resin (A) is prepared, or can be measured by the NMR method.
[0066] 1 In the case of H-NMR measurement, for example, a nuclear magnetic resonance apparatus (ECX400 manufactured by JEOL Ltd.) is used, the solvent is deuterated orthodichlorobenzene, the sample concentration is 20 mg / 0.6 mL, the measurement temperature is 120° C., and the observation nucleus is 1 The conditions were: H (400 MHz), sequence was single pulse, pulse width was 5.12 μsec (45° pulse), repetition time was 7.0 sec, and the number of integrations was 500 or more. The reference chemical shift was set to 0 ppm for hydrogen in tetramethylsilane, but similar results can also be obtained by setting the peak derived from residual hydrogen in deuterated orthodichlorobenzene at 7.10 ppm as the reference value for the chemical shift. 1 Peaks such as H can be assigned by conventional methods.
[0067] 13 In the case of C-NMR measurement, for example, a nuclear magnetic resonance apparatus (ECP500 manufactured by JEOL Ltd.) is used as the measurement apparatus, a mixed solvent of ortho-dichlorobenzene / heavy benzene (80 / 20% by volume) is used as the solvent, the measurement temperature is 120°C, and the observation nucleus is 13 The conditions are: C (125 MHz), single pulse proton decoupling, 45° pulse, repetition time 5.5 seconds, number of integrations 10,000 or more, and chemical shift reference value 27.50 ppm. Assignment of various signals is performed based on the usual method, and quantification can be performed based on the integration value of signal intensity.
[0068] Specific examples of the polyamide resin (A) include polyamide 6T / 6I (polyhexamethylene terephthalamide / polyhexamethylene isophthalamide copolymer), polyamide 6T / 66 (polyhexamethylene terephthalamide / polyhexamethylene adipamide copolymer), etc. Only one type of polyamide resin (A) may be included, or two or more types may be included.
[0069] The intrinsic viscosity [η] of the polyamide resin (A) measured in concentrated sulfuric acid at a temperature of 25° C. is preferably 0.70 dl / g or more and 1.60 dl / g or less, more preferably 0.80 dl / g or more and 1.20 dl / g or less. When the intrinsic viscosity [η] of the polyamide resin (A) is 0.70 dl / g or more, the mechanical strength of the molded article can be further increased. When the intrinsic viscosity [η] is 1.60 dl / g or less, the flowability of the polyamide resin composition during molding is not easily impaired.
[0070] The intrinsic viscosity [η] of polyamide resin (A) can be measured as follows. 0.5 g of polyamide resin (A) is dissolved in 50 ml of 96.5% sulfuric acid solution to prepare a sample solution. The flow time of the obtained solution at 25°C ± 0.05°C is measured using an Ubbelohde viscometer and calculated based on the following formula. [η]=ηSP / (C*(1+0.205ηSP)) [η]: Intrinsic viscosity (dl / g) ηSP: Specific viscosity C: Sample concentration (g / dl) t: Time required for sample solution to flow (seconds) t0: Number of seconds that blank sulfuric acid flows (seconds) ηSP=(t-t0) / t0
[0071] The polyamide resin (A) can be produced by the same method as known polyamide resins, for example, by polycondensing dicarboxylic acid and diamine in a homogeneous solution. Specifically, the polyamide resin (A) can be produced by heating dicarboxylic acid and diamine in the presence of a catalyst to obtain a low-order condensate as described in WO 03 / 085029, and then applying shear stress to the melt of the low-order condensate to polycondense it.
[0072] The content of the polyamide resin (A) in the polyamide resin composition may be adjusted so that the amount of the polyamide resin (A) in the obtained light-transmitting resin composition falls within the above-mentioned range. For example, the content of the polyamide resin (A) in the polyamide resin composition may be 40 parts by mass or more and 90 parts by mass or less per 100 parts by mass of the polyamide resin composition (the pellets prepared in the step of preparing the polyamide resin composition described above).
[0073] (Fiber filler (B)) Examples of the fibrous filler (B) include glass fiber, wollastonite, potassium titanate whisker, calcium carbonate whisker, aluminum borate whisker, magnesium sulfate whisker, zinc oxide whisker, milled fiber, cut fiber, etc. Among these, one kind may be used alone, or two or more kinds may be used in combination. Among them, wollastonite, glass fiber, and potassium titanate whisker are preferred, and wollastonite or glass fiber is more preferred, because they are easy to increase the mechanical strength of the molded body.
[0074] From the viewpoints of moldability of the polyamide resin composition and mechanical strength and heat resistance of the resulting molded article, the average fiber length of the fibrous filler (B) is preferably 1 μm to 20 mm, more preferably 5 μm to 10 mm, and even more preferably 10 μm to 5 mm. The aspect ratio of the fibrous filler (B) is preferably 5 to 2000, and more preferably 30 to 600.
[0075] The average fiber length and average fiber diameter of the fibrous filler (B) can be measured by the following method. 1) A polyamide resin composition is dissolved in a hexafluoroisopropanol / chloroform solution (0.1 / 0.9% by volume), and then filtered to obtain a filtrate. 2) The filtrate obtained in 1) is dispersed in water, and the fiber length (Li) and fiber diameter (di) of each of 300 random fibers are measured using an optical microscope (magnification: 50x). The number of fibers with fiber length Li is taken as qi, and the weight average length (Lw) is calculated based on the following formula, which is the average fiber length of the fibrous filler (B). Weight average length (Lw) = (Σqi × Li <2> ) / (Σqi×Li) Similarly, the number of fibers having a fiber diameter Di is taken as ri, and the weight average diameter (Dw) is calculated based on the following formula, and this is taken as the average fiber diameter of the fibrous filler (B). Weight average diameter (Dw)=(Σri×Di <2> ) / (Σri×Di)
[0076] The fibrous filler (B) may be surface-treated. If the filler is surface-treated, the adhesion to the polyamide resin (A) which is the matrix resin is likely to be increased. Examples of the surface treatment agent include coupling agents such as silane coupling agents, titanium coupling agents, and aluminate coupling agents; sizing agents, etc. Examples of the sizing agent which is preferably used include epoxy compounds, urethane compounds, carboxylic acid compounds, urethane / maleic acid modified compounds, and urethane / amine modified compounds.
[0077] The content of the fibrous filler (B) in the polyamide resin composition may be adjusted so that the amount of the fibrous filler (B) in the obtained light-transmitting resin composition falls within the above-mentioned range. For example, the content of the fibrous filler (B) in the polyamide resin composition may be 25 parts by mass or more and 40 parts by mass or less per 100 parts by mass of the polyamide resin composition (the pellets prepared in the step of preparing the polyamide resin composition described above).
[0078] (Other ingredients) The polyamide resin composition may further contain other components in addition to those described above, if necessary, provided that the polyamide resin composition does not substantially contain the light-transmitting dye (C).
[0079] 2-1-2.Master batch The master batch preferably contains the above-mentioned light-transmitting dye (C) and a polyamide resin (D) having a melting point lower than 310°C.
[0080] The content of the light-transmitting dye (C) in the masterbatch is preferably 30% by mass or more and 80% by mass or less, and more preferably 40% by mass or more and 70% by mass or less, based on the mass of the masterbatch. When the content of the light-transmitting dye (C) is 30% by mass or more, the polyamide resin composition can be more sufficiently colored.
[0081] (Polyamide resin (D)) When the melting point of the polyamide resin (D) is lower than 310°C, discoloration due to the deterioration of the light-transmitting dye (C) during melt-kneading to obtain the masterbatch can be suppressed. As a result, discoloration of the obtained light-transmitting resin composition can be suppressed even when the masterbatch is used. The melting point of the polyamide resin (D) is preferably 220°C or higher and 310°C or lower. The method for measuring the melting point is the same as the method for measuring the melting point of the polyamide resin (A) described above.
[0082] From the viewpoint of suppressing deterioration of the light-transmitting dye (C) due to heat while further enhancing melt-kneadability with the polyamide resin composition, the difference in melting point between the polyamide resin (D) and the polyamide resin (A) is preferably 10°C or more, more preferably 20°C or more and 150°C or less, and even more preferably 30°C or more and 100°C or less.
[0083] The melting point (Tm) of the polyamide resin (D) can be adjusted by the composition of the polyamide resin. For example, the melting point (Tm) can be lowered by reducing the content of structural units derived from aromatic dicarboxylic acids.
[0084] The polyamide resin (D) is not particularly limited as long as it has a melting point within the above range, but is preferably an aliphatic polyamide. The aliphatic polyamide contains, as a main component, a structural unit that contains an amide bond and does not contain an aromatic ring (an amide bond-containing structural unit that does not contain an aromatic ring). "Containing as a main component" means that the amide bond-containing structural unit contains 80 mol% or more, preferably 90 mol% or more, of the total number of moles of the structural unit.
[0085] The polyamide resin (D) may be a resin obtained by subjecting a dicarboxylic acid and a diamine to a polycondensation reaction, or may be a resin obtained by subjecting an aminocarboxylic acid to a polycondensation reaction, or may be a resin obtained by subjecting a lactam to a ring-opening polymerization reaction.
[0086] For example, the polyamide resin (D) may contain a structural unit (Da) derived from a dicarboxylic acid and a structural unit (Db) derived from a diamine.
[0087] (Structural unit derived from dicarboxylic acid (Da)) The dicarboxylic acid-derived structural unit (Da) preferably contains an aliphatic dicarboxylic acid. The aliphatic dicarboxylic acid is an aliphatic dicarboxylic acid having 4 to 20 carbon atoms, and the number of carbon atoms is preferably 6 to 12. Examples of such aliphatic dicarboxylic acids include oxalic acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, and tetradecanedioic acid. Among them, adipic acid, azelaic acid, and sebacic acid are preferred, and adipic acid is more preferred.
[0088] The content of the structural units derived from aliphatic dicarboxylic acids is, for example, 80 mol% or more, more preferably 90 mol% or more, and may be 100 mol%, based on the total number of moles of the structural units (Da) derived from dicarboxylic acids.
[0089] The dicarboxylic acid-derived structural unit (Da) may further contain a structural unit derived from another dicarboxylic acid other than the above, if necessary. The other dicarboxylic acid includes an aromatic dicarboxylic acid, an alicyclic dicarboxylic acid, etc. The content of the structural unit derived from the other dicarboxylic acid is, for example, 20 mol% or less, more preferably 10 mol% or less, based on the total mole number of the dicarboxylic acid-derived structural unit (Da).
[0090] (Structural unit derived from diamine (Db)) The diamine-derived structural unit (Db) may be the same as the diamine-derived structural unit (Ab).
[0091] Alternatively, the polyamide resin (D) may contain structural units derived from an aminocarboxylic acid or structural units derived from a lactam.
[0092] (Structural unit derived from amino carboxylic acid) The aminocarboxylic acid may be an aminocarboxylic acid having from 6 to 12 carbon atoms, preferably from 6 to 10 carbon atoms. Examples of such aminocarboxylic acids include 6-aminocaproic acid, 7-aminoheptanoic acid, 11-aminoundecanoic acid, 12-aminododecanoic acid, and the like.
[0093] (Structural unit derived from lactam) The lactam may be a lactam having from 6 to 12 carbon atoms, preferably from 6 to 10 carbon atoms. Examples of such lactams include α-pyrrolidone, ε-caprolactam, undecanelactam, ω-laurolactam, ε-enantholactam, and the like.
[0094] Examples of the polyamide resin (D) include polyamide 6, polyamide 66, polyamide 610, polyamide 612, polyamide 92, and polyamide 1010, with polyamide 6, polyamide 66, and polyamide 610 being preferred.
[0095] The content of the polyamide resin (D) in the masterbatch is preferably 20% by mass or more and 70% by mass or less, and more preferably 30% by mass or more and 60% by mass or less, based on the mass of the masterbatch. When the content of the polyamide resin (D) is 20% by mass or more, the light-transmitting dye (C) can be more easily dispersed in the polyamide resin composition, and more uniform coloring can be achieved.
[0096] (Other polyamide resins) As described above, the pellets of the light-transmitting resin composition or the polyamide resin composition may further contain other polyamide resins in addition to the polyamide resin (A) and the polyamide resin (D). Examples of other polyamide resins include polyamide 6T / DT (polyhexamethylene terephthalamide / poly-2-methylpentamethylene terephthalamide copolymer), polyamide 9T (polynonamethylene terephthalamide), polyamide 10T (polydecamethylene terephthalamide), and the like.
[0097] 2-2. Light-transparent resin composition The light-transmitting resin composition according to the present embodiment includes a dry blend of the pellets of the polyamide resin composition and the master batch. The contents of the components (A), (B), and (C) in the light-transmitting resin composition are as described above.
[0098] In the above embodiment, each component including polyamide resin (A) and polyamide resin (D) and all or part of the raw materials used to produce each component may be derived from biomass. For example, the dicarboxylic acid component unit (Aa) derived from a dicarboxylic acid of polyamide resin (A) may contain a component unit derived from a dicarboxylic acid derived from biomass, and the diamine component unit (Ab) derived from a diamine may contain a component unit derived from a diamine derived from biomass. Furthermore, polyamide resin (A) may be a biomass-derived polyamide resin (A) obtained by polymerizing a raw material group including a raw material derived from biomass.
[0099] 3. Manufacturing method for laser welded products In this embodiment, a molded body (first molded body) of the above-mentioned light-transmitting resin composition and a molded body (second molded body) of the light-absorbing resin composition can be irradiated with laser light through the first molded body to weld them together to produce a laser-welded body.
[0100] The first molded body may be one molded using the composition set of the above 2-1, or may be one molded using the light-transmitting resin composition of the above 2-2.
[0101] The second molded body may be one molded from a light-absorbing resin composition, which will be described below.
[0102] 3-1. Light-absorbing resin composition The light-absorbing resin composition contains a thermoplastic resin and a light-absorbing dye, and may further contain a fibrous filler as necessary.
[0103] The thermoplastic resin is not particularly limited, but is preferably a polyamide resin, more preferably the same as the polyamide resin (A), from the viewpoint of easily obtaining good welding strength with the molded body of the light-transmitting resin composition. The fibrous filler is also preferably the same as the fibrous filler (B). In other words, the light-absorbing resin composition can be configured in the same way as the light-transmitting resin composition, except for the type and content of the dye.
[0104] (light absorbing dye) The light-absorbing dye is a dye that has an absorption wavelength in the range of the wavelength of the irradiated laser light, that is, in the range of 800 nm to 1064 nm. Such a light-absorbing dye absorbs the laser light and generates heat, melting the thermoplastic resin. The heat melts and welds the resin component contained in the first molded body.
[0105] The light absorbing pigment may be an inorganic pigment or an organic pigment. Examples of inorganic pigments include black pigments such as carbon black (e.g., acetylene black, lamp black, thermal black, furnace black, channel black, and ketjen black); red pigments such as iron oxide red; orange pigments such as molybdate orange; and white pigments such as titanium oxide. Examples of organic pigments include yellow pigments, orange pigments, red pigments, blue pigments, and green pigments. Among them, inorganic pigments are generally preferred because they have strong hiding power, and black pigments are more preferred.
[0106] From the viewpoint of improving dispersibility, the light-absorbing dye is preferably added as a masterbatch during the production of the light-absorbing resin composition. Examples of the carbon black masterbatch include PA-0896A (masterbatch containing 50% by mass of carbon black) manufactured by Nichiko Bix Co., Ltd.
[0107] The content of the light-absorbing dye in the light-absorbing resin composition is preferably 0.01 part by mass or more and 1 part by mass or less with respect to 100 parts by mass of the resin component.
[0108] 3-2.Kit The light-absorbing resin composition can be used together with the light-transmitting resin composition as a molding material kit for obtaining a laser-welded article. That is, the kit for obtaining a laser-welded article includes 1) the set of the compositions or the light-transmitting resin composition, and 2) the light-absorbing resin composition.
[0109] 3-3. Manufacturing method for laser welded products Next, a method for producing a laser welded product according to this embodiment will be described.
[0110] The manufacturing method of the laser welded body according to this embodiment includes the steps of overlapping a first molded body and a second molded body, and irradiating laser light through the first molded body to weld the first molded body and the second molded body.
[0111] The shapes of the first and second molded bodies are not particularly limited, but since the molded bodies are used by joining them together by laser welding, they usually have at least a surface (flat or curved surface) that can be in surface contact. In laser welding, the laser light that has passed through the first molded body, which is a light-transmitting resin member, is absorbed and melted by the second molded body, which is a light-absorbing resin member, and the two members are welded together. The first molded body obtained by molding the above-mentioned light-transmitting resin composition has high transmittance to laser light despite containing the fibrous filler (B), and therefore can be preferably used as a transparent resin member in the laser welding method.
[0112] The thickness of the first molded body (the thickness in the laser transmission direction at the part through which the laser light passes) can be set appropriately taking into consideration the application and the composition of the light-transmitting resin composition, and is, for example, 5 mm or less, and preferably 4 mm or less.
[0113] The first and second compacts are superimposed on each other, and laser light is applied through the first compact to laser weld the first and second compacts together.
[0114] Specifically, the welded portions of the first and second molded bodies are brought into contact with each other. At this time, it is preferable that the welded portions of the first and second molded bodies are in surface contact. The surface contact may be contact between flat surfaces, contact between curved surfaces, or contact between a flat surface and a curved surface.
[0115] Next, the laser beam is irradiated through the first molded body, which is a light-transmitting resin member. The laser beam is preferably irradiated from an angle of 85° to 95° with respect to the welding surface, from the viewpoint of making it easier for the laser beam to efficiently reach the welding surface. If necessary, the laser beam may be focused on the interface between the first molded body and the second molded body using a lens system. The focused beam passes through the first molded body and is absorbed near the surface of the second molded body, generating heat and melting it. Next, the heat is transferred to the first molded body by thermal conduction, melting it, and a molten pool is formed at the interface between the two. This molten pool is cooled and solidified to become a welded part (joint).
[0116] The laser light source to be used can be selected depending on the light of the light-absorbing dye. For example, a laser light source having a wavelength of 800 nm or more and 1064 nm or less is preferable, and for example, a semiconductor laser can be used.
[0117] The laser welded body obtained by laser welding the first molded body and the second molded body in this manner has high weld strength (bonding strength).
[0118] The obtained laser welded article has good mechanical strength, high weld strength, and little damage to the resin caused by laser irradiation. Therefore, the obtained laser welded article can be applied to various applications, such as various storage containers, electrical and electronic equipment parts, office automation (OA) equipment parts, home appliance parts, machine mechanism parts, vehicle mechanism parts, etc. In particular, it can be suitably used for food containers, pharmaceutical containers, oil and fat product containers, hollow vehicle parts (various tanks, intake manifold parts, temperature control valve parts, thermostat cases, camera housings, etc.), vehicle electrical parts (various control units, ignition coil parts, etc.), motor parts, various sensor parts, connector parts, switch parts, breaker parts, relay parts, coil parts, transformer parts, lamp parts, etc. EXAMPLES
[0119] The present invention will be specifically described below with reference to examples, but the scope of the present invention is not limited to the description of the examples.
[0120] 1. Materials 1-1. Preparation of polyamide resin <Preparation of polyamide resin (A)> 2774g (16.7 mol) of terephthalic acid, 1196g (7.2 mol) of isophthalic acid, 2800g (24.3 mol) of 1,6-hexanediamine, 36.6g (0.3 mol) of benzoic acid, 5.7g of sodium hypophosphite monohydrate and 545g of distilled water were placed in an autoclave with a capacity of 13.6L and substituted with nitrogen. Stirring was started at 190°C, and the internal temperature was raised to 250°C over 3 hours. At this time, the internal pressure of the autoclave was raised to 3.03MPa. After continuing the reaction for 1 hour, the low condensation product was discharged into the atmosphere from a spray nozzle installed at the bottom of the autoclave and extracted. Thereafter, the low condensation product was cooled to room temperature, pulverized to a particle size of 1.5mm or less with a pulverizer, and dried at 110°C for 24 hours. The water content of the obtained low condensate was 4100 ppm, and the intrinsic viscosity [η] was 0.15 dl / g.
[0121] Next, this low condensate was placed in a tray-type solid-phase polymerization reactor, and after replacing with nitrogen, the temperature was raised to 180°C over about 1 hour and 30 minutes. After that, the reaction was continued for 1 hour and 30 minutes, and the temperature was lowered to room temperature. The intrinsic viscosity [η] of the obtained prepolymer was 0.20 dl / g. Thereafter, this prepolymer was melt-polymerized in a twin-screw extruder with a screw diameter of 30 mm and L / D=36 at a barrel set temperature of 330° C., a screw rotation speed of 200 rpm, and a resin supply rate of 6 kg / h to prepare a polyamide resin.
[0122] The composition of the obtained polyamide resin (A) was 6T / 6I (70 / 30 molar ratio). The melting point Tm of the polyamide resin (A) was 330° C., and the glass transition temperature Tg of the polyamide resin (A) was 125° C. The intrinsic viscosity [η] of the polyamide resin (A) was 1.0 dl / g, and the heat of fusion (ΔH) was 55 J / g.
[0123] <Preparation of Polyamide Resin (E)> 1,6-hexanediamine 1312g (11.3 mol), 2-methyl-1,5-pentanediamine 1312g (11.3 mol), terephthalic acid 3655g (22.0 mol), sodium hypophosphite 5.5g (5.2 × 10 -2mol) and 640 ml of ion-exchanged water were charged into a 1-liter reactor, and after replacing with nitrogen, the mixture was heated at 250°C and 35 kg / cm 2 The reaction was carried out for 1 hour under the above conditions. The molar ratio of 1,6-hexanediamine to 2-methyl-1,5-pentanediamine was 50:50. After 1 hour had elapsed, the reaction product produced in the reactor was transferred to a storage tank connected to the reactor and maintained at a pressure of about 10 kg / cm 2 The mixture was discharged into a receiver set at a low temperature to obtain a low-order condensate having an intrinsic viscosity [η] of 0.15 dl / g.
[0124] Next, the obtained low-order condensate was dried and then melt-polymerized at a cylinder set temperature of 330° C. using a twin-screw extruder to obtain a polyamide resin (E).
[0125] The composition of the obtained polyamide resin (E) was 6T / DT (50 / 50 molar ratio). The intrinsic viscosity [η] of the polyamide resin (E) was 1.0 dl / g, the melting point (Tm) was 300°C, and the glass transition temperature (Tg) was 140°C.
[0126] The intrinsic viscosity [η], melting point Tm and heat of fusion ΔH of these polyamide resins were measured by the following methods.
[0127] [Intrinsic viscosity [η]] 0.5 g of polyamide resin was dissolved in 50 ml of 96.5% sulfuric acid solution. The flow time of the obtained solution at 25°C ± 0.05°C was measured using an Ubbelohde viscometer and calculated based on the formula: [η] = ηSP / (C(1 + 0.205ηSP)). [η]: Intrinsic viscosity (dl / g) ηSP: Specific viscosity C: Sample concentration (g / dl) t: Time required for sample solution to flow (seconds) t0: Number of seconds that blank sulfuric acid flows (seconds) ηSP=(t-t0) / t0
[0128] [Melting point Tm] The melting point Tm of the polyamide resin was measured using a differential scanning calorimeter (DSC220C, manufactured by Seiko Instruments Inc.) as follows.
[0129] Approximately 5 mg of polyamide resin was sealed in an aluminum pan for measurement and heated from room temperature to 350°C at 10°C / min. In order to completely melt the resin, it was held at 350°C for 3 minutes and then cooled to 30°C at 10°C / min. Then, after leaving it at 30°C for 5 minutes, it was heated a second time to 350°C at 10°C / min. The temperature (°C) of the endothermic peak during this second heating was taken as the melting point (Tm) of the polyamide resin.
[0130] [Heat of fusion ΔH] The heat of fusion ΔH of the polyamide resin was determined from the area of the endothermic peak during melting in the first heating process using a differential scanning calorimeter (DSC220C type, manufactured by Seiko Instruments Inc.) in accordance with JIS K7121:2012.
[0131] 1-2. Fibrous filler (B) Glass fiber (ECS 03 T-747H, Nippon Electric Glass Co., Ltd., bundling agent: epoxy resin / urethane resin, fiber diameter 10.5 μm)
[0132] 1-3.Masterbatch containing light-transmitting dye (C) Orient Chemical Industry Co., Ltd.'s e-BIND LTW-8701H (a master batch containing 50 mass% of polyamide 66 (melting point 260°C) as polyamide resin (D) and 50 mass% of light-transmitting dye (C) (a black dye containing anthraquinone derivative)) was used.
[0133] 2. Preparation of light-transmitting resin composition (Examples 1 to 3) (1) Preparation of pellets of polyamide resin composition The polyamide resin (A) and the fibrous filler (B) were mixed in a tumbler blender and melt-kneaded in a twin-screw extruder (TEX30α manufactured by Japan Steel Works, Ltd.) at a cylinder temperature (melting point (Tm) of the polyamide resin + 15) °C. The mixture was then extruded into a strand shape and cooled in a water tank. The strand was then taken up and cut by a pelletizer to obtain cylindrical pellets of the polyamide resin composition having a diameter of 2.7 mm and a length of 3.5 mm.
[0134] (2) Preparation of light-transmitting resin composition The resulting polyamide resin composition pellets and the master batch pellets containing the light-transmitting dye (C) were mixed (dry blended) in a tumbler blender to obtain a light-transmitting resin composition in the form of pellets, so as to obtain the composition shown in Table 1. The mixing in the tumbler blender was carried out at room temperature (25° C.).
[0135] (Comparative Examples 1 to 3) The polyamide resin (A), the fibrous filler (B), and the master batch were mixed in a tumbler blender, and melt-kneaded in a twin-screw extruder (TEX30α manufactured by Japan Steel Works, Ltd.) at a cylinder temperature (melting point (Tm) of the polyamide resin + 15) °C. The mixture was then extruded into a strand shape and cooled in a water tank. The strand was then taken up and cut by a pelletizer to obtain a pellet-shaped light-transmitting resin composition.
[0136] (Reference example 1) A light-transmitting resin composition was prepared in the same manner as in Example 2, except that the polyamide resin (A) was changed to the polyamide resin (E).
[0137] (Reference example 2) A light-transmitting resin composition was prepared in the same manner as in Comparative Example 2, except that the polyamide resin (A) was changed to the polyamide resin (E).
[0138] 3. Evaluation For the light-transmitting resin compositions of Examples 1 to 3, Comparative Examples 1 to 3, and Reference Examples 1 to 2 prepared above, the maintenance rate of laser light transmittance was evaluated.
[0139] (Laser light transmittance maintenance rate) The obtained light-transmitting resin composition was molded under the following molding conditions using the following injection molding machine to obtain a test piece having a length of 30 mm, a width of 30 mm and a thickness of 0.7 mm. Molding machine: Toshiba Machine Co., Ltd. EC75N-2A Molding machine cylinder temperature: Melting point (Tm) of polyamide resin composition + 10°C Mold temperature: 160℃ The residence time in the cylinder was set to 1 minute. The transmittance T0 of the obtained test piece to a laser beam with a wavelength of 940 nm was measured using a power meter F300-SH manufactured by Ophir Corporation.
[0140] In addition, the same molding machine was used, and the cooling time was extended so that the residence time in the cylinder was set to 25 minutes, to obtain the above test piece. Similarly, the laser light transmittance T was measured. Then, the maintenance rate relative to the measured laser transmittance T0 was calculated based on the following formula. Maintenance rate of laser light transmittance (%) = (T / T0) x 100
[0141] Table 1 shows the evaluation results of Examples 1 to 3, Comparative Examples 1 to 3, and Reference Examples 1 and 2.
[0142] [Table 1]
[0143] As is clear from Table 1, the molded bodies of Comparative Examples 1 to 3, which used pellets obtained by melt-kneading a master batch containing a polyamide resin (A), a fibrous filler (B), and a light-transmitting dye (C), had a laser light transmittance retention rate of less than 90% and discoloration occurred.
[0144] In contrast, the molded bodies of Examples 1 to 3, which were made using a dry blend of pellets obtained by melt-kneading polyamide resin (A) and fibrous filler (B) and a master batch containing a light-transmitting dye (C), had a high laser light transmittance retention rate of 96% or more and reduced discoloration.
[0145] From these findings, it can be seen that by post-adding a master batch containing the light-transmitting dye (C) by dry blending, the retention rate of the laser light transmittance of the molded body can be increased, and a molded body with little discoloration can be obtained.
[0146] On the other hand, when a polyamide resin (E) having a melting point lower than 310°C was used, there was almost no difference in the maintenance rate of the laser light transmittance between the case where the master batch containing the light-transmitting dye (C) was melt-kneaded from the beginning (Reference Example 2) and the case where it was added later by dry blending (Reference Example 1). That is, even in the case of melt-kneading (Reference Example 2), the maintenance rate of the laser light transmittance was high, at 90% or more. This suggests that the phenomenon of discoloration occurring in the obtained molded article when the light-transmitting dye (C) is melt-kneaded with other components is an issue that becomes apparent in polyamide resins having a melting point of 310°C or more. [Industrial Applicability]
[0147] According to the present invention, it is possible to provide a method for producing a molded article that has heat resistance and is suppressed from discoloring, a composition set, a light-transmitting resin composition, and a kit.
Claims
1. A step of preparing pellets of a polyamide resin composition containing a polyamide resin (A) having a melting point of 310° C. or higher as measured by a differential scanning calorimeter (DSC) and a fibrous filler (B); A step of dry-blending the pellets of the polyamide resin composition with a light-transmitting dye (C) to obtain a light-transmitting resin composition; A step of molding the light-transmitting resin composition; Including, A method for producing a molded body.
2. In the step of preparing pellets of the polyamide resin composition, The polyamide resin (A) and the fibrous filler (B) are melt-kneaded to obtain the pellets. A method for producing the molded article according to claim 1.
3. The polyamide resin (A) contains a structural unit (Aa) derived from a dicarboxylic acid and a structural unit (Ab) derived from a diamine, The structural unit (Aa) derived from a dicarboxylic acid contains a structural unit derived from terephthalic acid in an amount of 50 mol % or more relative to the total number of moles of the structural unit (Aa) derived from a dicarboxylic acid, The diamine-derived structural unit (Ab) includes at least one of a structural unit derived from an aliphatic diamine having 4 to 15 carbon atoms and a structural unit derived from an alicyclic diamine having 4 to 20 carbon atoms. A method for producing the molded article according to claim 1.
4. The diamine-derived structural unit (Ab) contains more than 50 mol% of a linear aliphatic diamine-derived structural unit having 4 to 15 carbon atoms, based on the total number of moles of the diamine-derived structural units (Ab). A method for producing the molded article according to claim 3.
5. In the step of obtaining the light-transmitting resin composition, dry blending the polyamide resin composition with a master batch containing the light transmitting dye (C) and a polyamide resin (D) having a melting point lower than 310°C; A method for producing the molded article according to claim 1.
6. The light-transmitting dye (C) includes a dye that does not have a maximum absorption wavelength in the wavelength range of 800 nm or more and 1064 nm or less. A method for producing the molded article according to claim 1.
7. the dye having no maximum absorption wavelength in the wavelength range of 800 nm or more and 1064 nm or less is at least one selected from the group consisting of perylene derivatives, pyrazolone derivatives, perinone derivatives, and anthraquinone derivatives; A method for producing the molded article according to claim 6.
8. The content of the light-transmitting dye (C) in the light-transmitting resin composition is 0.1 parts by mass or more and 5 parts by mass or less with respect to 100 parts by mass of the light-transmitting resin composition. A method for producing the molded article according to claim 1.
9. A set of compositions for obtaining a light-transmitting resin composition, Pellets of a polyamide resin composition containing a polyamide resin (A) having a melting point of 310° C. or higher as measured by a differential scanning calorimeter (DSC) and a fibrous filler (B); A master batch containing a light-transmitting dye (C) and a polyamide resin (D) having a melting point lower than 310° C.; Including, set.
10. Pellets of a polyamide resin composition containing a polyamide resin (A) having a melting point of 310° C. or higher as measured by a differential scanning calorimeter (DSC) and a fibrous filler (B); A master batch containing a light-transmitting dye (C) and a polyamide resin (D) having a melting point lower than 310° C.; Including a dry blend of Light-transparent resin composition.
11. A kit for obtaining a laser welded product, comprising: The set according to claim 9 or the light-transmitting resin composition according to claim 10, a light absorbing resin composition containing a thermoplastic resin and a light absorbing dye; Including, kit.
Citation Information
Patent Citations
Colored thermoplastic resin compositions for laser welding, specific neutral anthraquinone dyes as colorants therefor, and products molded therefrom.
JP2004534104A
Multilayer container, manufacturing method therefor, and manufacturing method of recycled polyester
JP2021127173A
Polyamide resin composition, molded body thereof, and method for manufacturing laser-welded body
WO2019160117A1
THERMOPLASTIC RESIN COMPOSITION FOR LASER WELDING AND ARTICLES MOLDED THEREOF
JP2003522269A