Magnet, article, and manufacturing method for magnet

By incorporating fluororesin particles in the gaps between hard magnetic powders and applying a magnetic field during compression molding, the method addresses the density and magnetic performance issues of binderless magnets, achieving high-density magnets with enhanced magnetic properties.

JP2024140526APending Publication Date: 2024-10-10CANON KK
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023051701
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing methods for manufacturing binderless magnets using metal soap-based lubricants fail to achieve sufficient density and magnetic properties due to the limitations of these lubricants, leading to insufficient magnetic performance.

Method used

A magnet comprising a mixture of hard magnetic powders and fluororesin particles, where the volume ratio of hard magnetic powder is 85% or more, with fluororesin particles present in the gaps between the powders, and a manufacturing process involving compression molding under a magnetic field without heating, to enhance magnetic orientation and density.

Benefits of technology

The method produces a binderless magnet with improved magnetic properties by preventing damage to the magnetic powder during compression and enhancing orientation, resulting in higher residual magnetic flux density and orientation efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140526000001_ABST
    Figure 2024140526000001_ABST
Patent Text Reader

Abstract

To provide a binderless magnet with sufficient magnetic properties.SOLUTION: A magnet 10 includes multiple magnetic powders 1 and fluorine resin particles 2. The volume ratio of the magnetic powders 1 to the magnet 10 is 85% or more. The fluorine resin particles 2 exist in a gap 8 in the multiple magnetic powders 1.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to magnets, articles and methods of making magnets. [Background technology]

[0002] Magnets are broadly divided into sintered magnets and bonded magnets. Compared to sintered magnets, which are dense and have high magnetic properties, bonded magnets have poor magnetic properties because they contain a lot of resin binder. However, binderless magnets, which do not use resin binders and are made by compressing and molding only magnetic powder, are expected to have better magnetic properties than bonded magnets, although they do not reach the level of sintered magnets. In addition, because sintering is not required, there are advantages such as not needing large equipment such as sintering furnaces and being able to use magnetic powder for bonded magnets that is available on the market.

[0003] When magnetic powder with magnetic anisotropy is used, the magnetic properties of binderless magnets can be improved by applying a magnetic field and performing compression molding. In order to further improve the magnetic properties, it is necessary to create a dense compact, but if the pressure applied during molding is too high, the magnetic powder may be damaged or the orientation of the oriented magnetic powder may change due to frictional forces, resulting in a loss of orientation.

[0004] Patent Document 1 discloses that when producing a binderless magnet, a lubricant is added and then magnetic powder is molded to increase the density of the molded body. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2016-207711 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, the method disclosed in Patent Document 1 uses a metal soap-based lubricant as the lubricant, so that the density of the compact cannot be made sufficient, and the magnetic properties are insufficient. [Means for solving the problem]

[0007] A first aspect for solving the above problem is a magnet comprising a plurality of hard magnetic powders and fluororesin particles, wherein the volume ratio of the hard magnetic powder to the magnet is 85% or more, and the fluororesin particles are present in the gaps between the plurality of hard magnetic powders.

[0008] A second aspect for solving the above problem is a manufacturing method for a magnet, comprising: a preparation step of preparing a mixed powder in which a plurality of hard magnetic powders and fluororesin particles are mixed; and a molding step of compression molding the mixed powder while applying a magnetic field to the mixed powder, characterized in that in the compression molding step, molding is performed at a pressure such that the volume ratio of the hard magnetic powder to the magnet is 85% or more. Effect of the Invention

[0009] According to the present disclosure, it is possible to provide a binderless magnet having sufficient magnetic properties. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a conceptual diagram showing the structure of a magnet in one embodiment of the present disclosure. [Diagram 2] FIG. 2 is a schematic diagram showing a molding apparatus used in manufacturing an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] (magnet) The present disclosure will now be described in detail with reference to the drawings.

[0012] 1 is a conceptual diagram showing the structure of a magnet 10 according to one embodiment of the present disclosure. The magnet 10 has a plurality of hard magnetic powders 1 and fluororesin particles 2.

[0013] The magnet 10 can be applied to various articles. The magnet 10 can be used by being attached to a base material such as a housing or a wiring board of the article. Examples of the article include rotating devices such as motors, home appliances, office automation equipment, and medical equipment. The shape of the magnet 10 when used in an article is not particularly limited. It may be a hexahedron such as a rectangular parallelepiped or cube, a cylinder, a sphere, a prism, a cone, a ring shape, a plate shape, or a sheet shape.

[0014] Magnet 10 is a so-called binderless magnet. Unlike bonded magnets, which are made by melting a binder made of organic components such as resin to mold magnetic powder, binderless magnets are magnets that are manufactured without heating to a temperature above the binder melting point (melting point of the binder). In other words, they are magnets that do not contain molten resin.

[0015] The hard magnetic powder 1, which is a magnetic powder, is a ferromagnetic material with high saturation magnetic flux density, coercive force, and residual magnetic flux density, which is used as a permanent magnet. For example, ferrite-based compounds, samarium-cobalt-based compounds, and RTB-based compounds are known as hard magnetic powders 1. In particular, permanent magnets using RTB-based compounds are known to have high performance. Here, R is a rare earth element containing at least one of Nd and Pr, T is a transition metal element containing at least Fe, and B is boron. Those containing Nd in R are called neodymium magnets, and Dy is often added.

[0016] As the RTB compound, neodymium magnets, which are Nd-Fe-B compounds, are preferred. Commercially available Nd-Fe-B compounds include, for example, MF15P, MF18P (manufactured by Aichi Steel Corporation), MQP-12-8HD, MQP-10-8.5HD, MQP-12.5-8.5, MQP-11-8, MQP-8-5 (manufactured by Magnequench), YMM13-9, YMM9-6, YMM8-4 (manufactured by Yuhong Magnetic Materials Co. Ltd.), ZRK B-12M, ZRK B-10M, and ZRK-B-8.5M (manufactured by Zhe Jiang Zhao-Ri-Ke Magnet Industries Co., Ltd.). These magnetic powders may be used alone or in combination of two or more.

[0017] From the viewpoint of enhancing the magnetic properties of the magnet 10, the hard magnetic powder 1 is preferably a crystal having magnetic anisotropy. This is because by applying a magnetic field to perform molding, the crystals are aligned (oriented) in the direction of the easy magnetization axis, which facilitates magnetization, making it easier to obtain a magnet with high magnetic properties. Commercially available crystals having magnetic anisotropy include, for example, MF15P and MF18P (both manufactured by Aichi Steel Corporation).

[0018] In the magnet 10 of the present disclosure, the volume ratio of the hard magnetic powder 1 in the magnet 10 is 85% or more. In other words, the magnet 10 is a dense compact with a small volume ratio of pores, less than 15%. Therefore, the magnet 10 of the present disclosure can exhibit higher magnetic properties than conventional binderless magnets. Here, the magnetic properties are, for example, the degree of orientation, which is the ratio of the residual magnetic flux density to the saturation magnetic flux density. A magnet with a high degree of orientation has a small change in magnetic flux density when a magnetic field is applied, which means that it is excellent as a permanent magnet. The preferred degree of orientation is 0.88 or more.

[0019] The hard magnetic powder particles 1 are bonded to each other at the bonding surfaces 7. The inventors believe that this mechanism is as follows. A very thin oxide layer exists on the surface of the hard magnetic powder particles 1, but when the hard magnetic powder particles 1 are compression molded with strong pressure, the oxide layer breaks and new surfaces are exposed. Since the new surfaces are active, they bond with each other to form the bonding surfaces 7.

[0020] The fluororesin particles 2 are present in the gaps 8 between the multiple hard magnetic powder particles 1. In magnet 10 after compression molding, it is preferable that no fluororesin particles 2 are present on bonding surfaces 7 where the hard magnetic powder particles 1 are bonded.

[0021] The fluororesin particles 2 play a role of providing a lubricating effect that relieves the pressure applied to the hard magnetic powder 1 when the mixed powder with the hard magnetic powder 1 is compression molded. When the mixed powder of the hard magnetic powder 1 and the fluororesin particles 2 is compression molded, the fluororesin particles 2 move into the gaps 8 and assist in the generation of the binding surface 7 of the hard magnetic powder 1. When attempting to compression mold only the hard magnetic powder 1 without the fluororesin particles 2, the hard magnetic powder may be damaged and the magnetic properties may not be sufficient. In addition, the hard magnetic powder may rotate due to frictional force during compression molding, so even if a magnetic field is applied, a strong magnetic field may be required to align the crystals in the direction of the easy axis of magnetization.

[0022] The content of the fluororesin particles 2 in the magnet 10 is preferably in the range of 0.5% by volume or more and 2.0% by volume or less. If it is less than 0.5% by volume, the above-mentioned assist effect is not fully exerted, and a strong magnetic field may be required to increase the magnetic properties of the hard magnetic powder 1. On the other hand, if it is more than 2.0% by volume, the fluororesin particles 2 are more likely to overflow from the gaps 8, and the fluororesin particles 2 may be present on the bonding surfaces 7, requiring a large pressure force to increase the relative density of the hard magnetic powder 1. A more preferable content is in the range of 0.6% by volume or more and 1.3% by volume or less.

[0023] The average particle diameter of the fluororesin particles 2 is preferably smaller than that of the hard magnetic powder 1. This is because the fluororesin particles 2 are more likely to be present in the gaps 8 between a plurality of hard magnetic powders. The average particle diameter of the fluororesin particles 2 is preferably ¼ or less, more preferably 1 / 20 or less, of the average particle diameter of the hard magnetic powder 1. For example, if the average particle diameter of the hard magnetic powder 1 is 100 μm, the average particle diameter of the fluororesin particles 2 is preferably 25 μm or less, and more preferably 5 μm or less.

[0024] The fluorine-based resin particles 2 may be, for example, at least one selected from the group consisting of tetrafluoroethylene resin (PTFE), tetrafluoroethylene-perfluoroalkoxyethylene copolymer resin (PFA), tetrafluoroethylene-hexafluoropropylene copolymer resin (FEP), tetrafluoroethylene-hexafluoropropylene-perfluoroalkoxyethylene copolymer resin (EPE), tetrafluoroethylene-ethylene copolymer resin (ETFE), trifluorochloroethylene copolymer resin (PCTFE), trifluorochloroethylene-ethylene copolymer resin (ECTFE), vinylidene fluoride resin (PVDF), and vinyl fluoride resin (PVE). From the viewpoint of commercial availability, tetrafluoroethylene resin (PTFE) is particularly preferable. Two or more of the above-mentioned types may be mixed and used.

[0025] The melting point of the fluororesin particles 2 is preferably equal to or higher than the Curie temperature of the hard magnetic powder 1. The Curie temperature is the temperature at which the ferromagnetic properties of a ferromagnetic material are lost. If the melting point of the fluororesin particles 2 is equal to or higher than the Curie temperature of the hard magnetic powder 1, it is possible to heat the magnet 10 at a temperature lower than the Curie temperature of the hard magnetic powder 1 when manufacturing the magnet 10 by compression molding. This is because heating may make it easier to make the volume ratio of the hard magnetic powder 1 85% or more. More preferably, the melting point of the fluororesin particles 2 is 10 degrees or higher than the Curie temperature of the hard magnetic powder 1.

[0026] As described above, the magnet disclosed herein contains fluorine-based resin particles, which reduces the pressure applied to the hard magnetic powder during compression molding and prevents the hard magnetic powder from being damaged or rotating due to frictional forces during compression molding. As a result, the proportion of anisotropic powder oriented in the direction of the easy axis of magnetization can be increased, making it possible to provide a binderless magnet with excellent magnetic properties.

[0027] (Magnet manufacturing method) A method for manufacturing the magnet of the present disclosure will now be described.

[0028] First, a mixed powder in which a plurality of hard magnetic powders 1 and fluororesin particles 2 are mixed is prepared (preparation step). In the preparation step, a premixed mixed powder may be prepared, or a mixed powder may be obtained by mixing a plurality of hard magnetic powders 1 and fluororesin particles 2. The method for mixing a plurality of hard magnetic powders 1 and fluororesin particles 2 is not particularly limited, and may be dry mixing or wet mixing.

[0029] Next, the mixed powder is compression molded while applying a magnetic field to the mixed powder (molding process). FIG. 2 is a schematic diagram of a molding device 20 that can be used in the molding process. The molding device 20 has a molding die and a coil 5. The molding die has a die 3, an upper punch 4a, and a lower punch 4b. The mixed powder 11 can be compression molded by pressing the mixed powder 11 with the upper punch 4a and the lower punch 4b inside the die. A current can be passed through the coil 5 by applying a voltage by a control device (not shown), and a magnetic field can be generated at the same time. The function of generating a magnetic field in the molding device 20 does not require special specifications, and is a function that can also be used in the manufacture of sintered magnets and bonded magnets.

[0030] In the molding process, first, the mixed powder 11 is fed into a molding die. Before feeding, a release agent may be applied to the surface of the die as necessary. This is because the application of the release agent makes it easier to remove the molded body. The type of release agent is not particularly limited, and for example, a material having a lubricating effect such as boron nitride, magnesium stearate, calcium stearate, molybdenum disulfide, etc. can be used. In addition, the method of applying the release agent is also not particularly limited. For example, the release agent can be dispersed in a quick-drying liquid and applied directly or sprayed with a spray gun to adhere to the die surface.

[0031] Next, a current is passed through the coil 5 to generate a magnetic field, which is then applied to the mixed powder. The magnetic field generated by the coil 5 is preferably 1 T or more at the center of the molding die in order to sufficiently orient the hard magnetic powder 1 contained in the mixed powder 11. However, the strength of the magnetic field can be changed depending on the average particle size of the hard magnetic powder 1 and the shape of the molded body.

[0032] Next, the mixed powder 11 is pressed and molded using the upper punch 4a and the lower punch 4b. Pressurization may be performed by moving the upper punch 4a downward and the lower punch 4b upward, or the lower punch 4b may be fixed and the upper punch 4a moved downward. At this time, it is necessary to apply pressure with such a large force that the relative density of the hard magnetic powder 1 in the molded magnet 10 is 85% or more. Specifically, it is preferable to pressurize the mixed powder 11 with a pressure of 500 MPa or more. However, the magnitude of the pressing force can be changed depending on the average particle size of the hard magnetic powder 1 and the shape of the molded body.

[0033] The pressure is then removed, the application of the magnetic field is terminated, and the compact is then removed. The removed compact is then subjected to a magnetization process to obtain magnet 10 of the present disclosure. There are no particular limitations on the means of magnetization, and any known method can be used, such as pulse magnetization, in which a pulse is applied using a magnetization power supply.

[0034] As described above, according to the magnet manufacturing method of the present disclosure, in the compression molding step, the mixed powder containing fluorine-based resin particles is molded at a pressure such that the relative density of the hard magnetic powder in the magnet is 85% or more. This reduces the pressure applied to the hard magnetic powder during compression molding, and prevents the hard magnetic powder from being damaged or rotating due to frictional force during compression molding. This makes it possible to obtain a high-density magnet without the step of heating to a temperature that melts the binder. This makes it possible to provide a binderless magnet with high magnetic properties.

[0035] In the above embodiment, the magnetic field is applied to the mixed powder before compression molding, but the magnetic field may be applied to the mixed powder after compression molding. Similarly, the application of the magnetic field is terminated after the applied pressure is released, but the applied pressure may be released after the application of the magnetic field is terminated.

[0036] In the above embodiment, the compression molding is performed without heating, but heating may be performed at a temperature lower than the Curie temperature of the hard magnetic powder 1. However, from the viewpoint of increasing production efficiency, it is preferable to perform the compression molding without heating. EXAMPLES

[0037] The effects of the present disclosure will be described below with reference to examples and comparative examples. First, prior to the examples, the evaluation methods of the examples will be described.

[0038] [Magnetic properties] The magnetic properties were measured using a high-sensitivity vibrating sample magnetometer (VSM, Tamagawa Seisakusho, TM-VSM311483-HGC type). The maximum magnetic field applied during the measurement was 3.2 T.

[0039] [Fluorine-based resin particle content] The volume ratio of the fluororesin particles (PTFE) shown in Table 1 below was determined by cutting the magnet in half and analyzing the cut surface with a scanning X-ray photoelectron spectroscopy analyzer (XPS, ULVAC-PHI, Inc., Quantera II).14 Based on the molecular weights of B and PTFE, the volume ratio of each was calculated from the detected element ratios of Fe and F. Next, the volume ratio of PTFE was calculated when the total amount of hard magnetic powder and PTFE was taken as 100%. The diameter of the XPS analysis area was 100 μm, and the average value of 10 points was used.

[0040] [Volume ratio of hard magnetic powder] The volume ratio of the hard magnetic powder was calculated by dividing the density calculated from the weight of the hard magnetic powder and the volume of the magnet by the theoretical density of the hard magnetic powder. The weight was calculated by measuring the weight of the magnet with an electronic balance (Shinko Denshi, ALE623H) and subtracting the weight of the fluororesin particles from that value. The volume was calculated with a micrometer (Mitutoyo, MDQ-30MX).

[0041] Example 1 First, we used NdFeB anisotropic magnetic powder as the hard magnetic powder. 14 B (MF15P, manufactured by Aichi Steel Corporation, average particle size 100 μm, Curie temperature 315° C.) was prepared. In addition, PTFE particles (KTL-1N, manufactured by Kitamura Corporation, average particle size 2 μm, melting point 327° C.) were prepared as fluororesin particles. Next, dry mixing was performed using a ball mill to obtain a mixed powder for molding.

[0042] Next, the mixed powder was compression molded using an experimental molding machine capable of applying a magnetic field, which has the same configuration as that shown in Figure 2. The mold used for molding was made of non-magnetic cemented carbide material, with a cavity area of ​​6 mm x 6 mm. The mold surface was sprayed with boron nitride as a mold release agent.

[0043] After 1.0 g of the mixed powder was placed in the mold, a magnetic field was applied by a coil placed around the mold. The magnetic field strength applied by the coil was measured in advance at the center of the mold, and a current was passed through the coil so that the magnetic field strength was 2.6 T.

[0044] Thirty seconds after the magnetic field was applied, the upper punch was lowered and pressure was started to reach a predetermined pressure (2000 MPa to 2500 MPa) for the cavity area. At this time, the lower punch was held stationary and pressure was applied by moving only the upper punch. When the target pressure was reached, the pressure was immediately released and the sample was demagnetized to remove the magnetic force. After demagnetization was completed, the compact was taken out and magnetized to obtain the magnet of Example 1.

[0045] (Examples 2 to 4) Magnets of Examples 2 to 4 were produced in the same manner as in Example 1, except that the content of the fluorine-based resin particles was changed to the value shown in Table 1.

[0046] Comparative Example 1 First, we used NdFeB anisotropic magnetic powder as the hard magnetic powder. 14 B (MF15P, average particle size 100 μm, manufactured by Aichi Steel Corporation) was prepared. No fluorine-based resin particles were included.

[0047] Next, the hard magnetic powder was compression molded using an experimental molding machine capable of applying a magnetic field, which has the same configuration as that shown in Figure 2. The mold used for molding was made of non-magnetic cemented carbide, with a cavity area of ​​6 mm x 6 mm. The mold surface was sprayed with boron nitride as a mold release agent.

[0048] After placing 1.0 g of hard magnetic powder in the mold, a magnetic field was applied by a coil placed around the mold. The magnetic field strength applied by the coil was measured in advance at the center of the mold, and a current was passed through the coil so that the magnetic field strength was 2.6 T.

[0049] Thirty seconds after the magnetic field was applied, the upper punch was lowered and pressure was started to reach the specified pressure (2300 MPa) for the cavity area. At this time, the lower punch was held stationary and pressure was applied by moving only the upper punch. When the target pressure was reached, the pressure was immediately released and the sample was demagnetized to remove the magnetic force. After demagnetization was completed, the compact was removed and magnetized to obtain the magnet of Comparative Example 1.

[0050] Comparative Example 2 A magnet of Comparative Example 2 was produced in the same manner as in Comparative Example 1, except that the molding pressure was changed to 2200 MPa.

[0051] Comparative Example 3 A magnet of Comparative Example 3 was produced in the same manner as in Comparative Example 1, except that the molding pressure was changed to 2250 MPa.

[0052] Table 1 shows the type and volume ratio of hard magnetic powder, the type and content of fluorine-based resin particles, saturation magnetic flux density, residual magnetic flux density, and degree of orientation in Examples 1 to 4 and Comparative Examples 1 to 3.

[0053] [Table 1]

[0054] As can be seen from Table 1, the magnets of Examples 1 to 4, in which PTFE was mixed, had higher residual magnetic flux density than the magnets of Comparative Examples 1 to 3, and as a result showed a high degree of orientation. When the magnets of Examples 1 to 4 were cut in half and the cross section was observed under an electron microscope, it was confirmed that the hard magnetic powder particles were bonded together as shown in Figure 1. It was also confirmed that the structure had PTFE particles scattered in the gaps between the hard magnetic powder particles.

[0055] In Examples 1 to 4, the pressure applied to the hard magnetic powder during compression molding was reduced by using PTFE particles, and it is considered that the hard magnetic powder was prevented from being damaged or rotated by frictional force during compression molding. As a result, the proportion of anisotropic powder oriented in the direction of the easy magnetization axis was increased, and the degree of orientation was higher than that of the comparative example. On the other hand, since PTFE particles were not used in Comparative Examples 1 to 3, it is considered that the hard magnetic powder was damaged or rotated by frictional force during compression molding. Therefore, it is considered that the proportion of anisotropic powder oriented in the direction of the easy magnetization axis was less than that of the examples, and the degree of orientation was lower than that of the examples.

[0056] The present disclosure includes the following embodiments.

[0057] (Configuration 1) A magnet comprising a plurality of magnetic powders and fluorine-based resin particles, The volume ratio of the magnetic powder to the magnet is 85% or more, The magnet is characterized in that the fluororesin particles are present among the plurality of magnetic powder particles.

[0058] (Configuration 2) 2. The magnet according to claim 1, wherein the content of the fluorine-based resin particles in the magnet is in the range of 0.5% by volume to 2.0% by volume.

[0059] (Configuration 3) 2. The magnet according to claim 1, wherein the content of the fluorine-based resin particles in the magnet is in the range of 0.6 volume % to 1.3 volume %.

[0060] (Configuration 4) 4. The magnet according to any one of configurations 1 to 3, wherein the average particle size of the fluororesin particles is smaller than the average particle size of the magnetic powder.

[0061] (Configuration 5) 5. The magnet according to claim 4, wherein the average particle size of the fluororesin particles is less than or equal to one-fourth the average particle size of the magnetic powder.

[0062] (Configuration 6) 6. The magnet according to any one of configurations 1 to 5, wherein the fluorine-based resin particles are not present on the bonding surfaces of the plurality of magnetic powder particles.

[0063] (Configuration 7) 7. The magnet according to any one of configurations 1 to 6, wherein the melting point of the fluorine-based resin particles is higher than the Curie temperature of the magnetic powder.

[0064] (Configuration 8) The magnet according to any one of configurations 1 to 7, wherein the magnetic powder is an RTB compound (wherein R is a rare earth element including at least one of Nd and Pr, and T is a transition metal element including at least Fe).

[0065] (Configuration 9) 9. The magnet according to any one of configurations 1 to 8, having a degree of orientation, which is the ratio of residual magnetic flux density to saturation magnetic flux density, of 0.88 or more.

[0066] (Configuration 10) An article having a substrate on which the magnet according to any one of configurations 1 to 9 is provided.

[0067] (Method 1) A preparation step of preparing a mixed powder in which a plurality of magnetic powders and fluorine-based resin particles are mixed; and a molding step of compression-molding the mixed powder while applying a magnetic field to the mixed powder, A method for manufacturing a magnet, wherein in the compression molding step, molding is performed at a pressure such that the volume ratio of the magnetic powder to the magnet is 85% or more.

[0068] (Method 2) In the preparation step, A manufacturing method for a magnet according to method 1, comprising mixing a plurality of magnetic powders and fluororesin particles to obtain a mixed powder so that the content of the fluororesin particles in the magnet is in the range of 0.5 volume % or more and 2.0 volume % or less. [Explanation of symbols]

[0069] 1 Hard magnetic powder (magnetic powder) 2. Fluorine-based resin particles 8 Gap 9 Bonding surface 10. Magnets

Claims

1. A magnet comprising a plurality of magnetic powders and fluorine-based resin particles, The volume ratio of the magnetic powder to the magnet is 85% or more, The magnet is characterized in that the fluororesin particles are present among the plurality of magnetic powder particles.

2. 2. The magnet according to claim 1, wherein the content of the fluorine-based resin particles in the magnet is in the range of 0.5% by volume to 2.0% by volume.

3. 2. The magnet according to claim 1, wherein the content of the fluorine-based resin particles in the magnet is in the range of 0.6 volume % to 1.3 volume %.

4. 2. The magnet according to claim 1, wherein the average particle size of the fluororesin particles is smaller than the average particle size of the magnetic powder.

5. 5. The magnet according to claim 4, wherein the average particle size of the fluororesin particles is equal to or less than one-fourth the average particle size of the magnetic powder.

6. 2. The magnet according to claim 1, wherein the fluororesin particles are not present on the bonding surfaces of the plurality of magnetic powder particles.

7. 2. The magnet according to claim 1, wherein the melting point of the fluororesin particles is higher than the Curie temperature of the magnetic powder.

8. 2. The magnet according to claim 1, wherein the magnetic powder is an R-T-B type compound (wherein R is a rare earth element including at least one of Nd and Pr, and T is a transition metal element including at least Fe).

9. 2. The magnet according to claim 1, wherein the degree of orientation, which is the ratio of the residual magnetic flux density to the saturation magnetic flux density, is 0.88 or more.

10. An article comprising a substrate provided with the magnet according to any one of claims 1 to 9.

11. A preparation step of preparing a mixed powder in which a plurality of magnetic powders and fluorine-based resin particles are mixed; and a molding step of compression-molding the mixed powder while applying a magnetic field to the mixed powder, A method for manufacturing a magnet, characterized in that in the compression molding step, molding is performed at a pressure such that the volume ratio of the magnetic powder to the magnet is 85% or more.

12. In the preparation step, 12. The method for producing a magnet according to claim 11, wherein a mixed powder is obtained by mixing a plurality of magnetic powders and fluororesin particles so that the content of the fluororesin particles in the magnet is in the range of 0.5 volume % or more and 2.0 volume % or less.

Citation Information

Patent Citations

  • Manufacturing method of magnet and magnet

    JP2016207711A