Manufacturing method for CFRP product
The method of using amorphous thermoplastic resin films in a press molding process with elevated mold temperatures addresses the issue of wrinkles in CFRP products, resulting in efficient, wrinkle-free resin layers and improved appearance without additional surface treatments.
Patent Information
- Application Number
- JP2023051731
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for manufacturing CFRP products with a resin protective layer often result in wrinkles and require additional surface treatments like spray painting, which can be inefficient and affect the appearance.
A method involving the use of amorphous thermoplastic resin films in a press molding process where the mold temperature exceeds the glass transition temperature of the resin, allowing for wrinkle-free resin protective layers on CFRP products without pre-shaping, and enabling direct demolding at high temperatures.
This approach produces CFRP articles with a smooth resin layer and good appearance, eliminating wrinkles and potentially eliminating the need for additional surface treatments like spray painting, enhancing production efficiency and product quality.
Smart Images

Figure 2024140548000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a CFRP product. [Background technology]
[0002] Carbon fiber reinforced plastics (CFRP) have strength and elastic modulus comparable to metals, but have a smaller specific gravity than metals, so they are increasingly being used in aircraft and automobiles to reduce fuel consumption.
[0003] Carbon fiber prepreg sheets are used to efficiently manufacture CFRP products. Carbon fiber prepreg sheets are sheet-shaped intermediate materials in which reinforcing material made of carbon fibers is pre-impregnated with a thermosetting matrix resin. Patent Document 1 reports that a CFRP plate having an acrylic resin layer on the surface was obtained by disposing an acrylic resin film on the surface of a carbon fiber prepreg sheet when the sheet was cured in an autoclave. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-1411 A Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention aims to provide a technique for efficiently producing a three-dimensional CFRP article with a good appearance and having a wrinkle-free resin protective layer on its surface, by heating and pressurizing a carbon fiber prepreg sheet and a resin film in a molding die. [Means for solving the problem]
[0006] According to one aspect of the present invention, there is provided a method for producing a three-dimensional CFRP product having a resin protective layer on at least a portion of its surface, the method comprising: molding the CFRP product by heating and pressurizing a laminate including at least one carbon fiber prepreg sheet and a film made of an amorphous thermoplastic resin superimposed thereon, in a molding die without pre-shaping, wherein the temperature of the molding die during the molding and when the CFRP product is released from the molding die is higher than the glass transition temperature of the amorphous thermoplastic resin. According to one aspect of the present invention, there is provided a three-dimensional CFRP product having a CFRP part and a resin protective layer covering at least a portion of a surface of the CFRP part, the protective layer being made of an amorphous thermoplastic resin, and the glass transition temperature of the CFRP part being higher than the glass transition temperature of the amorphous thermoplastic resin. Effect of the Invention
[0007] According to a preferred embodiment of the present invention, there is provided a technique for efficiently producing a three-dimensional CFRP article with a good appearance and having a wrinkle-free resin protective layer on its surface, by heating and pressurizing a carbon fiber prepreg sheet and a resin film in a molding die. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a schematic diagram showing a press molding apparatus. [Diagram 2] FIG. 2 is a cross-sectional view of the mold. [Diagram 3] FIG. 3 is a cross-sectional view for explaining a manufacturing process of a CFRP product. [Figure 4] FIG. 4 is a cross-sectional view for explaining a manufacturing process of a CFRP product. [Diagram 5] FIG. 5 is a cross-sectional view for explaining a manufacturing process of a CFRP product. [Figure 6] FIG. 6 is a cross-sectional view for explaining the manufacturing process of a CFRP product. [Figure 7] FIG. 7 is a diagram showing the appearance of the tray. [Figure 8] FIG. 8 is a diagram showing an example of the arrangement of carbon fiber prepreg sheets and thermoplastic resin films in a laminate. [Figure 9] FIG. 9 is a diagram showing another example of the arrangement of carbon fiber prepreg sheets and thermoplastic resin films in a laminate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the present invention will be described with reference to the accompanying drawings. 1. Manufacturing method of CFRP products An embodiment of the present invention relates to a method for manufacturing a CFRP product, and more particularly to a method for manufacturing a three-dimensional CFRP product having a resin protective layer on at least a portion of its surface.
[0010] The manufacturing method according to the embodiment is typically carried out using a press molding apparatus. In the manufacturing method according to the embodiment, for example, a press molding apparatus having a configuration shown in Fig. 1 can be used. Referring to Fig. 1, the press molding apparatus 100 has a press machine 10, a molding die 20, and a vacuum pump 30. The press 10 comprises a main frame 11, a bolster 12 fixed to the lower part of the main frame 11, a slide 13 that can be raised and lowered vertically, and a lifting mechanism 14 that raises and lowers the slide 13.
[0011] The forming die 20 is composed of a lower die 20L fixed to the upper surface of the bolster 12 and an upper die 20U fixed to the lower surface of the slide 13. Each of upper mold 20U and lower mold 20L has a built-in heater (not shown), which may be, for example, a steam heater, an oil heater, or an electric heater, making it possible to heat forming mold 20 to a predetermined temperature.
[0012] FIG. 2 is a cross-sectional view showing an example of a molding die 20 in an open state. The lower mold 20L and the upper mold 20U have a molding surface 21L and a molding surface 21U, respectively. Both the molding surface 21L and the molding surface 21U are three-dimensional. The lower die 20L has a vertical outer peripheral surface, and a seal ring 22 is fitted into a groove that goes around the outer peripheral surface. The upper die 20U is provided with an annular vertical wall 23 so that the lower die 20L and the upper die 20U can be fitted together via the seal ring 22. The airtight space formed between the lower mold 20L and the upper mold 20U when they are mated can be evacuated by operating a vacuum pump 30 connected through a hole provided in the upper mold 20U.
[0013] In the manufacturing method according to the embodiment, as shown in Fig. 3, a laminate 3 including at least one carbon fiber prepreg sheet 1 and a thermoplastic resin film 2 laminated thereon is placed between a lower mold 20L and an upper mold 20U without being pre-shaped. It is preferable that the lower mold 20L and the upper mold 20U are already heated to the same temperature as the molding temperature Tm at this point. The molding temperature Tm will be described later.
[0014] The laminate 3 may include two or more carbon fiber prepreg sheets 1 laminated together. In FIG. 3, one thermoplastic resin film 2 is overlaid on the carbon fiber prepreg sheet 1, but in other examples, one carbon fiber prepreg sheet 1 or two or more carbon fiber prepreg sheets 1 laminated to each other may be sandwiched between two thermoplastic resin films 2 on both sides. When two or more carbon fiber prepreg sheets 1 are laminated, films having various functions may be interposed between the carbon fiber prepreg sheets 1, or a configuration in which only carbon fiber prepreg sheets 1 are laminated, i.e., a configuration in which no films other than carbon fiber prepreg sheets are present between the carbon fiber prepreg sheets 1, may be used.
[0015] The carbon fiber prepreg sheet 1 and the thermoplastic resin film 2 are cut into a predetermined shape as necessary, but are not pre-shaped. In other words, they are laminated together in a flat state and placed between the lower mold 20L and the upper mold 20U.
[0016] Next, the lower die 20L and the upper die 20U are brought close to each other, and the molding die 20 is closed as shown in Fig. 4. The carbon fiber prepreg sheet 1 and the thermoplastic resin film 2, which were flat before the molding die 20 was closed, are deformed to conform to the shapes of the molding surfaces 21L and 21U after the molding die 20 is closed. As a result, wrinkles are generated in the thermoplastic resin film 2.
[0017] In the process of closing the molding die 20, as shown in Fig. 5, an airtight space 24 sealed by a seal ring 22 is formed between the lower die 20L and the upper die 20U. In a preferred embodiment, the airtight space 24 may be evacuated by operating a vacuum pump 30 to expel air bubbles from between the carbon fiber prepreg sheet 1 and the thermoplastic resin film 2. In order to sufficiently expel air bubbles, the movement of the lower die 20L and the upper die 20U toward each other may be stopped when the airtight space 24 is formed, or the speed at which the lower die 20L and the upper die 20U are brought toward each other may be reduced.
[0018] The mold 20 is kept closed for a certain period of time in order to heat and pressurize the laminate 3 of the carbon fiber prepreg sheet 1 and the thermoplastic resin film 2 within the mold 20. In this specification, this period (the period from when the mold 20 is closed to when it is opened) is referred to as the "molding time." The pressure applied to the carbon fiber prepreg sheet 1 in the mold 20 is preferably within a range of 3 MPa to 10 MPa. The pressure here is a value obtained by dividing the pressing force of the press machine 10 by the area of the carbon fiber prepreg sheet 1. The molding time is set to a length sufficient for the carbon fiber prepreg sheet 1 to harden.
[0019] The higher the temperature of the mold 20 between when it is closed and when it is opened (herein, this temperature is referred to as the "molding temperature Tm"), the shorter the time it takes for the carbon fiber prepreg sheet 1 to harden. Therefore, the molding temperature Tm is preferably 120°C or higher, more preferably 130°C or higher, and even more preferably 135°C or higher. When the molding temperature Tm is 120°C or higher, the molding time can be within 2 hours.
[0020] From the viewpoint of reducing the frequency of molding defects caused by too early curing of the carbon fiber prepreg sheet 1, the molding temperature Tm is preferably 170°C or lower, more preferably 160°C or lower, and even more preferably 150°C or lower. Not setting the molding temperature Tm too high is advantageous in that it reduces the difference between the molding temperature Tm and a temperature Td, which will be described later, and shortens the time required for temperature control of the molding die 20.
[0021] Once the carbon fiber prepreg sheet 1 has hardened, the molding die 20 is opened as shown in FIG. 6, and the CFRP product 4 molded into a three-dimensional shape is removed from the molding die 20. The CFRP product 4 has a CFRP part 41 made of a cured carbon fiber prepreg sheet 1, and a protective layer 42 that covers the surface of the CFRP part 41. The protective layer 42 is formed by adhering a thermoplastic resin film 2 to the surface of the CFRP part 41. Therefore, the material of the protective layer 42 is a thermoplastic resin.
[0022] In the manufacturing method according to the embodiment, the thermoplastic resin constituting the thermoplastic resin film 2 is amorphous. In other words, the thermoplastic resin constituting the thermoplastic resin film 2 has a glass transition temperature Tg2 and exhibits fluidity at temperatures equal to or higher than the glass transition temperature Tg2. Tg2 is determined by the properties of the amorphous main polymer that forms a continuous phase in the thermoplastic resin.
[0023] In the manufacturing method according to the embodiment, the molding temperature Tm is higher than the glass transition temperature Tg2 of the thermoplastic resin. Therefore, wrinkles that occur in the thermoplastic resin film 2 when the molding die 20 is closed disappear during molding, and the protective layer 42 can become completely wrinkle-free. This is thought to be because, in the molding die 20, the thermoplastic resin film 2 is continuously subjected to high pressure and exposed to a temperature higher than the glass transition temperature Tg2, so that the resin around the wrinkles fuses to each other.
[0024] On the other hand, when the CFRP product 4 is released from the molding die 20, it is not necessary to lower the temperature of the molding die 20 to a temperature equal to or lower than the glass transition temperature Tg2 of the thermoplastic resin. This is because, as long as the temperature Td of the molding die 20 at the time of release does not greatly exceed the glass transition temperature Tg2, there is no problem that part of the thermoplastic resin film 2 remains on the molding surface 21L at the time of release. The reason for this is believed to be that the thermoplastic resin is amorphous. Amorphous thermoplastic resins have a high degree of elastic properties, since their viscosity does not become extremely low compared to when they are in a glassy state, even at temperatures higher than the glass transition temperature Tg2.
[0025] The properties of amorphous thermoplastics contrast with crystalline thermoplastics, which have a much lower viscosity when they become flowable, i.e., when they reach their melting point. For example, in the manufacturing method according to the embodiment, it is possible to set the molding temperature Tm so as to obtain a wrinkle-free protective layer 42, and at the same time, to demold the CFRP product 4 while maintaining the temperature of the mold 20 at the molding temperature Tm, because the material of the thermoplastic resin film 2 is amorphous.
[0026] The glass transition temperature Tg1 of the CFRP part 41 of the CFRP product 4 can be a factor to be considered when determining the temperature Td of the molding die 20 when the CFRP product 4 is released from the molding die 20. This is because if the temperature Td of the molding die when the CFRP product 4 is released is too high compared with the glass transition temperature Tg1 of the CFRP part 41, there is a risk that the CFRP product 4 will be distorted when released from the molding die.
[0027] The temperature Td of the molding die when demolding may be equal to or higher than the glass transition temperature Tg1 of the CFRP part 41, but in that case, the difference between these two temperatures (Td-Tg1) is preferably 20° C. or less, and more preferably 10° C. or less. It is even more preferable that the temperature Td of the molding die 20 when demolding is lower than the glass transition temperature Tg1 of the CFRP part 41.
[0028] The temperature Td of the mold at the time of demolding is preferably the same as or lower than the molding temperature Tm. In a particularly preferred embodiment, the temperature of the mold 20 is kept constant from before the mold 20 is closed until the CFRP product 4 is demolded from the mold 20 (hereinafter, this embodiment will be referred to as "embodiment A"). When embodiment A is applied in the case where molding cycles are performed continuously, the time required to change the temperature of the mold 20 is not required, which is extremely advantageous in terms of production efficiency.
[0029] In embodiment A, since the molding temperature Tm and the temperature Td of the molding mold 20 at the time of demolding are the same, it is desirable not to make the molding temperature Tm too high in order to prevent distortion of the CFRP product 4 at the time of demolding and to suppress thermal shrinkage of the CFRP product 4 after demolding. Therefore, also in embodiment A, the molding temperature Tm is preferably 170° C. or lower, more preferably 160° C. or lower, and even more preferably 150° C. or lower.
[0030] In embodiment A, when a molding temperature Tm within the range of 120°C or higher and 170°C or lower, particularly 130°C or higher and 160°C or lower, and even more particularly 135°C or higher and 150°C or lower, is adopted, a film made of an amorphous thermoplastic resin having a glass transition temperature between 80°C and 100°C can be preferably used as the thermoplastic resin film 2.
[0031] 2.Material The materials that can be used in the manufacturing method of CFRP products described above in 1 are explained below.
[0032] 2.1.Carbon fiber prepreg sheet A carbon fiber prepreg sheet is a sheet-shaped molding material consisting of a reinforcing material made of carbon fiber and an uncured thermosetting matrix resin, and is produced by impregnating the reinforcing material with the matrix resin. Typical examples of carbon fiber prepreg sheets include carbon fiber UD prepreg, carbon fiber woven prepreg and carbon fiber sheet molding compound.
[0033] In carbon fiber UD prepregs, the carbon fibers contained as reinforcing material are aligned in one direction. In the carbon fiber woven prepreg, a woven fabric made of carbon fibers is used as a reinforcement material. Examples of the weave include, but are not limited to, plain weave, twill weave, and satin weave. The fabric may be a non-crimp fabric. In carbon fiber sheet molding compounds, random mats formed by scattering chopped carbon fiber bundles are used as reinforcing materials.
[0034] Carbon fiber prepreg sheets that can be preferably used in the manufacturing method according to the embodiment are carbon fiber UD prepregs and carbon fiber woven prepregs, particularly carbon fiber woven prepregs, because they are less likely to flow during molding. When using two or more carbon fiber prepreg sheets, only one of the carbon fiber UD prepregs and the carbon fiber woven prepregs may be used, or both of the carbon fiber UD prepregs and the carbon fiber woven prepregs may be used.
[0035] Carbon fiber UD prepregs, carbon fiber woven prepregs, and carbon fiber sheet molding compounds have been widely used in the past, and publicly known information can be appropriately referred to for their types, specifications, manufacturing methods, etc. Examples of commercially available carbon fiber UD prepregs and carbon fiber woven prepregs include Pyrofil (registered trademark) from Mitsubishi Chemical Corporation, Torayca (registered trademark) from Toray Industries, Inc., and Tenax (registered trademark) from Teijin Limited, and those skilled in the art can purchase and use these.
[0036] To find the glass transition temperature Tg1 of the CFRP part of a CFRP product, dynamic viscoelasticity measurements are performed using test pieces obtained by curing the carbon fiber prepreg sheet used as the material under conditions simulating actual molding conditions, and G'Tg, which is determined based on the temperature dependence of the storage rigidity G', is used as the glass transition temperature Tg1. More specifically, a carbon fiber prepreg sheet is cured to produce a CFRP plate with a thickness of about 1 mm, and then a test piece with a length of 55 mm and a width of 12.5 mm is cut out from the sheet. The storage modulus G' of this test piece is measured using a rheometer ARES-RDA manufactured by TA Instruments under the conditions of torsion mode, measurement frequency of 1 Hz, and heating rate of 5°C / min. In a graph plotting logG' against temperature, the temperature at the intersection of the approximation line of the plateau region of logG' and the approximation line of the region where logG' drops rapidly is G'Tg.
[0037] For example, International Publication WO2013 / 081058 discloses that CFRPs having various G'Tg values within a range from about 100°C to about 170°C can be obtained by curing a carbon fiber prepreg sheet, along with a method for producing the carbon fiber prepreg sheet, which can be used as a reference.
[0038] 2.2.Thermoplastic resin film The material of the thermoplastic resin film used in the manufacturing method of the CFRP product according to the embodiment is a non-crystalline thermoplastic resin. The type of the non-crystalline thermoplastic resin is not particularly limited, but suitable examples include acrylic resin, ABS resin, and polycarbonate resin.
[0039] In the manufacturing method of the CFRP product according to the embodiment, the molding temperature Tm is set to be higher than the glass transition temperature Tg2 of the thermoplastic resin, thereby eliminating wrinkles that are formed in the thermoplastic resin film when the mold is closed. In order to eliminate wrinkles in a shorter molding time, the difference (Tm-Tg2) between the glass transition temperature Tg2 of the thermoplastic resin and the molding temperature Tm is preferably 10°C or more, more preferably 20°C or more, and even more preferably 30°C or more.
[0040] In the manufacturing method of a CFRP product according to the embodiment, the temperature Td of the mold when the CFRP product is released from the mold is higher than the glass temperature Tg2 of the thermoplastic resin that is the material of the thermoplastic resin film. To prevent part of the thermoplastic resin film from remaining on the molding surface when the CFRP product is released from the mold, the difference (Td-Tg2) between the glass transition temperature Tg2 of the thermoplastic resin and the temperature Td of the mold when the CFRP product is released from the mold is preferably 60°C or less, more preferably 50°C or less.
[0041] The glass transition temperature Tg2 of a thermoplastic resin is measured by the following method. Using a differential scanning calorimeter (e.g., DSC6200, manufactured by Seiko Instruments Inc.), the thermoplastic resin is heated from room temperature at a heating rate of 10°C / min until it reaches 150°C, and then rapidly cooled to 20°C. The difference in heat flow with the reference is measured while heating again to 150°C at a heating rate of 10°C / min, and in the obtained chart, the temperature of the intersection between the baseline on the lower side of the temperature range where the baseline shifts downward and the tangent to the DSC curve at the inflection point within that temperature range is obtained. The temperature of this intersection is taken as the glass transition temperature.
[0042] When a thermoplastic resin contains multiple amorphous thermoplastic polymer phases, a DSC curve having multiple temperature ranges where the baseline shifts is obtained. In that case, the glass transition temperature of the main polymer forming the continuous phase is taken as the glass transition temperature Tg2 of the thermoplastic resin.
[0043] At the stage of selecting candidate materials for the thermoplastic resin film, instead of measured values based on differential scanning calorimetry, it is also possible to use estimated glass transition temperatures calculated from the FOX equation using values listed in the Polymer Handbook (J. Brandrup, Interscience, 1989) or catalog values from monomer manufacturers.
[0044] The higher the glass transition temperature Tg2 of the thermoplastic resin that is the material of the thermoplastic resin film, the higher the protective effect that the protective layer provides in the CFRP product manufactured by the method according to the embodiment. From this viewpoint, the glass transition temperature Tg2 of the thermoplastic resin is preferably 80°C or higher, more preferably 90°C or higher, and may be 100°C or higher. A resin film made of an amorphous thermoplastic resin with a glass transition temperature Tg2 of 80° C. or higher does not undergo plastic deformation at the temperature (usually less than 80° C.) at which the carbon fiber prepreg sheet is preshaped. Therefore, it is often difficult to preshape a laminate of a carbon fiber prepreg sheet and such a resin film before press molding.
[0045] The thickness of the thermoplastic resin film is not limited, but is usually 25 μm or more, preferably 50 μm or more, more preferably 75 μm or more, and is usually 300 μm or less, preferably 250 μm or less, more preferably 200 μm or less.
[0046] The surface of the thermoplastic resin film may be a mirror surface or a matte surface. When the surface of the thermoplastic resin film is a matte surface, the surface roughness is not particularly limited, and the arithmetic mean roughness (Ra) may be, for example, 0.2 μm or more and less than 0.5 μm, 0.5 μm or more and less than 1.0 μm, or 1.0 μm or more and 2.0 μm or less. The maximum height (Rz) is preferably within a range of 4 to 8 times the arithmetic mean roughness (Ra).
[0047] The arithmetic mean roughness and maximum height are calculated based on roughness measurements performed using a stylus surface roughness meter equipped with a 60° cone tip probe with a tip radius of 1 μm, in accordance with JIS B0601-2001 under the conditions of a measurement length of 4.0 mm, an evaluation length of 4.0 mm, a cutoff wavelength of 0.8 mm, and a measurement speed of 0.3 mm / s. When the thermoplastic resin film has a machine direction (MD) and a transverse direction (TD), the measurement direction is parallel to the TD. For the measurements, a surface roughness meter SURFCOM 1400D manufactured by Tokyo Seimitsu Co., Ltd. can be used, but is not limited thereto.
[0048] When at least one surface of the thermoplastic resin film is a matte surface, if the thermoplastic resin film and the carbon fiber prepreg sheet are superimposed in the above-described production method so that the matte surface faces the surface of the carbon fiber prepreg sheet, air bubbles are less likely to be trapped between the thermoplastic resin film and the carbon fiber prepreg sheet, and even if air bubbles are trapped, they are easily removed during molding.
[0049] There is no limitation on the method for producing the thermoplastic resin film, and any of melt extrusion methods including a T-die method and an inflation method, a calendar method, and other melt casting methods may be used.
[0050] One example of the thermoplastic resin film may be a laminated film having a layer containing a matting agent and a layer not containing a matting agent. The method for manufacturing a laminated film may involve forming single-layer films and then laminating the films together, but from an economical standpoint, a co-extrusion lamination method using a T-die with a multi-manifold or feed block is preferred.
[0051] When the thermoplastic resin film is a laminated film, it may include only layers formed of the same type of thermoplastic resin, or may include layers formed of different types of thermoplastic resin, provided that the thermoplastic resin forming each layer is amorphous and has a glass transition temperature Tg2 lower than the molding temperature in the manufacturing method according to the embodiment.
[0052] Among the amorphous thermoplastic resins exemplified above as materials for the thermoplastic resin film, acrylic resin is particularly preferred. The acrylic resin is a composition containing a polymer of alkyl (meth)acrylate as the main component.
[0053] The acrylic resin according to a preferred embodiment contains an acrylic rubber-containing polymer and a thermoplastic alkyl (meth)acrylate polymer as main components. The ratio of the content of the acrylic rubber-containing polymer and the thermoplastic alkyl (meth)acrylate polymer in the acrylic resin is preferably 10 / 90 or more by weight, more preferably 20 / 80 or more and 95 / 5 or less.
[0054] The acrylic rubber-containing polymer is produced by polymerizing a monomer component containing 30% by mass or more of alkyl acrylate to obtain rubber particles, and then polymerizing a monomer component containing 51% by mass or more of alkyl methacrylate in the presence of the rubber particles.
[0055] The monomer residues in the thermoplastic alkyl (meth)acrylate polymer may be all alkyl methacrylate monomer residues, or 50 to 99.9 mass%, 85 to 99.9 mass%, or 92 to 99.9 mass% may be alkyl methacrylate monomer residues. The content of alkyl acrylate monomer residues in the thermoplastic alkyl (meth)acrylate polymer is preferably 50 mass% or less, more preferably 0.1 to 15 mass%, and even more preferably 0.1 to 8 mass%. The thermoplastic alkyl (meth)acrylate polymer may contain 49 mass% or less of residues of monomers other than alkyl (meth)acrylate having one double bond per molecule.
[0056] The acrylic resin may be blended with additives such as matting agents, stabilizers, lubricants, processing aids, plasticizers, impact resistance aids, foaming agents, fillers, colorants, and ultraviolet absorbing agents, as required.
[0057] 2.3.Other films In the manufacturing method of a CFRP product according to the embodiment, as described above in 1, when two or more carbon fiber prepreg sheets are laminated, films having various functions can be interposed between the carbon fiber prepreg sheets. Examples of such films include, but are not limited to, foamed films and elastomeric films.
[0058] The expected effects of using foamed film are weight reduction of CFRP products and provision of sound insulation properties to CFRP products. The expected effect of using the elastomer film is to impart impact resistance to the CFRP product. Examples of the elastomer film include, but are not limited to, nitrile rubber films.
[0059] 3.CFRP products A CFRP product manufactured using the method according to the embodiment has a portion made of CFRP that has a three-dimensional shape, and has a resin protective layer on at least a portion of the surface of the portion. As will be understood from the above description of the manufacturing method, the resin protective layer is made of an amorphous thermoplastic resin, and its glass transition temperature Tg2 is lower than the molding temperature Tm of the CFRP product. Therefore, when the glass transition temperature Tg1 of the portion made of CFRP is higher than the molding temperature Tm, the glass transition temperature Tg1 is higher than the glass transition temperature Tg2 of the thermoplastic resin constituting the protective layer.
[0060] Depending on the application, the resin protective layer on the surface of the CFRP product can serve as an alternative to spray painting. In other words, depending on the application, the CFRP product manufactured using the method according to the embodiment can be used without further spray painting. From the viewpoint of enhancing the protective effect provided by the protective layer, the glass transition temperature of the amorphous thermoplastic resin which is the material of the protective layer is preferably 80°C or higher, more preferably 90°C or higher, and may be 100°C or higher.
[0061] 4. Topcoat painting In one example, a topcoat may be applied on the resin protective layer of the CFRP product manufactured using the method according to the embodiment. In other words, the resin protective layer may serve as a primer coating. In such an example, the protective layer may be polished to flatten the surface before the topcoat is applied. The amount of polishing required to flatten the surface of the protective layer is usually less than the amount of polishing required to flatten the CFRP surface without the protective layer.
[0062] In the topcoat application, at least one coating film including a pigmented coating film is formed. The coating film formed by topcoating is preferably a baked coating film, and is formed by drying the applied paint at a temperature of 80°C or higher, typically 100°C or higher. The coating film formed by overcoating may include a colored coating film and a clear coating film formed thereon. The clear coating film may be formed as a top coat. The coating film formed by topcoating may include a colored coating film and an undercoat coating film formed thereunder. When a plurality of coating films are formed by overlaying with topcoats, the plurality of coatings are preferably overlaid wet-on-wet and then baked simultaneously in one step.
[0063] 5. Summary of the embodiment Embodiments of the present invention include, but are not limited to, the following. [Embodiment 1] A method for producing a three-dimensional CFRP product having a resin protective layer on at least a portion of its surface, the method comprising: molding the CFRP product by heating and pressurizing a laminate comprising at least one carbon fiber prepreg sheet and a film made of amorphous thermoplastic resin superimposed thereon, in a molding die without pre-shaping; the temperature of the molding die during the molding and when the CFRP product is removed from the molding die is higher than the glass transition temperature of the amorphous thermoplastic resin. [Embodiment 2] The method of embodiment 1, wherein the laminate comprises two or more of the carbon fiber prepreg sheets laminated together. [Embodiment 3] The method according to embodiment 2, wherein the laminate does not include any film other than the carbon fiber prepreg sheets interposed between the carbon fiber prepreg sheets. [Embodiment 4] The method according to any one of embodiments 1 to 3, wherein the temperature of the mold during the molding is 120°C or more, preferably 130°C or more, more preferably 135°C or more, and preferably 170°C or less, more preferably 160°C or less, and even more preferably 150°C or less. [Embodiment 5] The method according to any one of embodiments 1 to 4, wherein the pressure applied to the carbon fiber prepreg sheet during the molding is 3 MPa or more and 10 MPa or less. [Embodiment 6] The method according to any one of embodiments 1 to 5, wherein the temperature of the molding die at the time of demolding is lower than the glass transition temperature of the CFRP contained in the CFRP product. [Embodiment 7] The method according to any one of embodiments 1 to 6, wherein the temperature of the mold during the demolding is the same as or lower than the temperature of the mold during the molding. [Embodiment 8] The method according to any one of embodiments 1 to 7, wherein the difference between the temperature of the mold during the molding and the glass transition temperature of the amorphous thermoplastic resin is 10°C or more, preferably 20°C or more, and more preferably 30°C or more. [Embodiment 9] The method according to any one of embodiments 1 to 8, wherein the difference between the temperature of the mold and the glass transition temperature of the amorphous thermoplastic resin when the mold is removed is 60°C or less, preferably 50°C or less. [Embodiment 10] The method according to any one of embodiments 1 to 9, wherein the amorphous thermoplastic resin has a glass transition temperature of 80°C or higher, preferably 90°C or higher, and may further be 100°C or higher. [Embodiment 11] The method of embodiment 7, wherein the temperature of the mold at the time of demolding is the same as the temperature of the mold during molding. [Embodiment 12] The method of embodiment 11, wherein the temperature of the mold during molding is 170°C or less, preferably 160°C or less, more preferably 150°C or less. [Embodiment 13] The method according to embodiment 12, wherein the amorphous thermoplastic resin has a glass transition temperature of 80°C or higher and 100°C or lower. [Embodiment 14] The method according to any one of embodiments 1 to 13, wherein the at least one carbon fiber prepreg sheet includes either or both of a carbon fiber UD prepreg and a carbon fiber woven prepreg. [Embodiment 15] The method according to any one of embodiments 1 to 14, wherein the amorphous thermoplastic resin comprises one or more resins selected from an acrylic resin, an ABS resin, and a polycarbonate resin. [Embodiment 16] The method of embodiment 15, wherein the amorphous thermoplastic resin comprises an acrylic resin. [Embodiment 17] The method according to any one of the first to sixth embodiments, wherein the amorphous thermoplastic resin film is an acrylic resin film. [Embodiment 18] A three-dimensional CFRP product having a CFRP part and a resin protective layer covering at least a portion of the surface of the CFRP part, the protective layer being made of an amorphous thermoplastic resin, and the glass transition temperature of the CFRP part being higher than the glass transition temperature of the amorphous thermoplastic resin. [Embodiment 19] A CFRP product according to embodiment 18, wherein the amorphous thermoplastic resin comprises one or more resins selected from acrylic resin, ABS resin, and polycarbonate resin. [Embodiment 20] A CFRP product according to embodiment 19, wherein the amorphous thermoplastic resin comprises an acrylic resin. EXAMPLES
[0064] 6. Experimental Results 6.1. Prototyping of CFRP products The results of the prototype CFRP products produced by the inventors are described below.
[0065] The prototype CFRP product is a tray with a rounded rectangular opening measuring 155 mm × 205 mm and a height of 25 mm, as shown in Fig. 7. In Fig. 7, the tray is placed with the bottom facing up, and Fig. 7(a) shows a perspective view of the bottom side, (b) shows a bottom view, and (c) shows a side view.
[0066] <Material> The materials used are as follows: [Carbon fiber prepreg sheet] Either a carbon fiber UD prepreg made by lining up carbon fibers in one direction and densely arranging them and impregnating them with an epoxy resin composition, or a carbon fiber woven prepreg made by impregnating a plain woven carbon fiber fabric with an epoxy resin composition was used. In either case, the material was cut into a 176 mm x 228 mm rectangle with rounded corners before use. All carbon fiber prepregs have a glass transition temperature of 170°C when cured under conditions of 140°C, 4 MPa, and 5 minutes.
[0067] [Thermoplastic resin film] The seven types of acrylic resin films shown in Table 1 were cut into rounded rectangles measuring 205 mm x 260 mm and used.
[0068] [Table 1]
[0069] The estimated glass transition temperatures shown in Table 1 are those of the acrylic resins that are the materials of the acrylic resin films. The estimated glass transition temperatures were calculated from the FOX formula using values given in the Polymer Handbook (J. Brandrup, Interscience, 1989) or values in the catalogues of monomer manufacturers.
[0070] The surface roughness of the acrylic resin film shown in Table 1 is the average value of the arithmetic mean roughness Ra and the maximum height Rz obtained from roughness measurements performed at three locations. A stylus-type surface roughness meter (SURFCOM 1400D, Tokyo Seimitsu Co., Ltd.) was used to measure the roughness. The probe was a Tokyo Seimitsu Co., Ltd. replaceable roughness shape probe (for high magnification measurement) (model number 010 2506), with a tip radius of 1 μm and a tip shape of a 60° cone. The measurement conditions were in accordance with JIS B0601-2001, with a measurement length of 4.0 mm, evaluation length of 4.0 mm, cutoff wavelength of 0.8 mm, and measurement speed of 0.3 mm / s. The measurement direction was parallel to the TD.
[0071] The acrylic resin films A, B, C, and G were laminated films having a layer made of a first acrylic resin containing a matting agent and a layer made of a second acrylic resin not containing a matting agent. In Table 1, the estimated glass transition temperatures of acrylic resin films A, B, C, and G are such that the value before the slash is that of the first acrylic resin and the value after the slash is that of the second acrylic resin, i.e., (estimated glass transition temperature of the first acrylic resin) / (estimated glass transition temperature of the second acrylic resin). In Table 1, the surface roughness of the acrylic resin films A, B, C, and G is the surface roughness on the side of the layer made of the first acrylic resin. The method for producing each acrylic resin will be described later.
[0072] <Tray molding> Prototypes were made for the 10 combinations shown in Table 2 below. For each prototype, a laminate was first created by layering two acrylic resin films on multiple carbon fiber prepreg sheets. When using carbon fiber UD prepregs, six carbon fiber UD prepregs (five for Prototype 10, described later) were placed between two acrylic resin films, as shown in Fig. 8. Of the six (five for Prototype 10, described later), the two at the ends had their fiber direction parallel to the long side of the rounded rectangle, and the remaining four (three for Prototype 10, described later) sandwiched between the two had their fiber direction parallel to the short side of the rounded rectangle. When carbon fiber woven prepregs were used, four carbon fiber woven prepregs were placed between two acrylic resin films as shown in FIG.
[0073] When the acrylic resin film was a laminated film, the surface of the layer containing the matting agent was brought into contact with the carbon fiber prepreg sheet. When acrylic resin films A, B, C, D, and G were used, air bubbles that formed between the carbon fiber prepreg sheets and the acrylic resin films during lamination could be easily expelled by manually pressing the surface of the laminate.
[0074] Next, the laminate was heated and pressed in a mold of a press molding machine without preforming to form a tray at a molding temperature of 140° C., a molding pressure of 4 MPa, and a molding time of 5 minutes. In prototypes 1 to 9, a release agent (liquid release agent Chemlease (registered trademark) AF-7 from Chemtrend Japan Inc.) was applied to the surface of the mold. In prototype 10, no release agent was used. When the mold was closed, degassing was performed for 90 seconds using a vacuum pump so that the vacuum pressure inside the mold became 0.1 MPa. The molded tray was demolded without lowering the temperature of the mold.
[0075] The results are shown in Table 2 below.
[0076] [Table 2]
[0077] As shown in Table 2, in all of the prototypes 1 to 10, the molded trays could be easily removed from the mold without lowering the temperature of the mold from 140°C. In all of the trays obtained from prototypes 1 to 10, the surface was covered with a protective layer made of acrylic resin, and no wrinkles were observed in the protective layer.
[0078] 6.2. Manufacturing method of acrylic resin film The acrylic resin films A to G used in the prototype experiments described in 6.1 above were produced by the following methods.
[0079] [Acrylic resin film A] The ingredients shown in Table 3 below are mixed in the ratio shown in column A-1 of the table using a Henschel mixer, fed into a twin-screw extruder, and extruded into strands while removing impurities with a screen mesh (stainless steel 200 mesh plain weave, nominal filtration diameter 77 μm) under conditions of a cylinder temperature of 170 to 260°C and a die head temperature of 220 to 240°C. The strands are cooled in a water tank and then cut to obtain pellets of the first acrylic resin. Similarly, a second acrylic resin pellet is obtained by blending the components in the following Table 3 in the blending ratio shown in column A-2 of the same table.
[0080] The pellets of the first acrylic resin and the pellets of the second acrylic resin are dehumidified and dried at 85° C. overnight before use. The first acrylic resin is plasticized using a 30mmφ non-vent screw extruder at a cylinder temperature of 200-240°C, and the second acrylic resin is plasticized using a 40mmφ non-vent screw extruder at a cylinder temperature of 220-240°C, and then fed into a 500mm wide two-type two-layer multi-manifold T-die set at 245°C to extrude a laminated film. When the laminated film is cooled, the first acrylic resin side is brought into contact with an embossed silicone roll, and the second acrylic resin side is brought into contact with a nip roll of a mirror-finished stainless steel roll.
[0081] [Acrylic resin film B] The composition of the first acrylic resin is the composition shown in column B-1 of Table 3 below, and the composition of the second acrylic resin is the composition shown in column B-2 of Table 3 below, except that the composition is the same as acrylic resin film A.
[0082] [Acrylic resin film C] The laminated film was cooled in the same manner as for Acrylic Resin Film B, except that the second acrylic resin side was brought into contact with a mirror-finish cooling roll instead of the nip roll.
[0083] [Acrylic resin film D] Acrylic resin pellets having the composition shown in column D of Table 3 below are used after drying and dehumidifying overnight at 85°C. Using a 40 mmφ non-vented screw extruder equipped with a 300 mm wide T-die, a monolayer film is extruded under conditions of a cylinder temperature of 200 to 240° C. and a T-die temperature of 245° C. When cooling the film, the surface is brought into contact with a mirror-finished cooling roll.
[0084] [Acrylic resin film E] The composition of the acrylic resin is the same as that of acrylic resin film D, except that the composition is the composition shown in column E of Table 3 below.
[0085] [Acrylic resin film F] The composition of the acrylic resin is the same as that of acrylic resin film D, except that the composition is the composition shown in column F of Table 3 below.
[0086] [Acrylic resin film G] The composition of the first acrylic resin is the composition shown in column G-1 of Table 3 below, and the composition of the second acrylic resin is the composition shown in column G-2 of Table 3 below, except that the composition is the same as acrylic resin film C.
[0087] [Table 3]
[0088] The acrylic rubber-containing polymer (G) shown in Table 3 was produced by the following method. The rubber-containing multistage polymer (I) is produced by the method of Preparation Example 1 described in International Publication WO2019 / 244791. The rubber-containing multistage polymer (II) is produced by the method of Preparation Example 2 described in International Publication WO2019 / 244791.
[0089] The rubber-containing multistage polymer (III) is produced in the same manner as in Preparation Example 2 described in International Publication WO2019 / 244791, except that the amount of n-OM in the monomer component (ii-c) is changed to 0.186 parts.
[0090] The rubber-containing multistage polymer (IV) is produced by the method of Preparation Example 3 described in International Publication WO2019 / 244791. The matting agent (D1) shown in Table 3 is produced by the method of Preparation Example 5 described in International Publication WO2019 / 244791. [Industrial Applicability]
[0091] Resin-coated CFRP molded articles can be used for a variety of purposes, including parts for mobile objects such as aircraft and automobiles, housings for electronic devices such as mobile PCs, digital video cameras, and mobile phones, and housings for large flat panel displays. [Explanation of symbols]
[0092] 1 Carbon fiber prepreg sheet 2 Thermoplastic resin film 3 Laminate 4. CFRP products 10 Press machine 11. Mainframe 12 Bolster 13 Slides 14 Lifting mechanism 20 mold 20L lower mold 20U upper type 21L molding surface 21U molding surface 22 Seal ring 23 vertical wall 24 Airtight Space 30 Vacuum Pump 41 CFRP section 42 Protective layer 100 Press equipment
Claims
1. A method for producing a three-dimensional CFRP product having a resin protective layer on at least a portion of its surface, comprising the steps of: The method includes molding the CFRP product by heating and pressurizing a laminate including at least one carbon fiber prepreg sheet and a film made of an amorphous thermoplastic resin laminated thereon in a molding die without preforming the laminate, The method wherein the temperature of the mold during said molding and when said CFRP article is demolded from said mold is greater than the glass transition temperature of said amorphous thermoplastic resin.
2. The method of claim 1 , wherein the laminate comprises two or more of the carbon fiber prepreg sheets laminated together.
3. The method according to claim 2 , wherein the laminate does not include any film other than the carbon fiber prepreg sheets interposed between the carbon fiber prepreg sheets.
4. 4. The method of claim 1, wherein the temperature of the mold during molding is 120° C. or higher.
5. The method according to any one of claims 1 to 4, wherein a pressure applied to the carbon fiber prepreg sheet during the molding is 3 MPa or more and 10 MPa or less.
6. The method according to claim 1 , wherein the temperature of the mold at the time of demolding is lower than the glass transition temperature of the CFRP contained in the CFRP product.
7. 7. The method of claim 1, wherein the temperature of the mold at the time of demolding is the same as or lower than the temperature of the mold during molding.
8. 8. The method according to claim 1, wherein the difference between the temperature of the mold during the molding and the glass transition temperature of the amorphous thermoplastic resin is 10°C or more.
9. The method according to any one of claims 1 to 8, wherein the difference between the temperature of the mold and the glass transition temperature of the amorphous thermoplastic resin when the mold is removed is 60°C or less.
10. The method according to any one of claims 1 to 9, wherein the amorphous thermoplastic resin has a glass transition temperature of 80°C or higher.
11. 8. The method of claim 7, wherein the temperature of the mold at the time of demolding is the same as the temperature of the mold during molding.
12. 12. The method of claim 11, wherein the temperature of the mold during said molding is 170°C or less.
13. The method according to claim 12, wherein the amorphous thermoplastic resin has a glass transition temperature of 80° C. or more and 100° C. or less.
14. 14. The method of claim 1, wherein the at least one carbon fiber prepreg sheet comprises either or both of a carbon fiber UD prepreg and a carbon fiber woven prepreg.
15. The method according to any one of claims 1 to 14, wherein the amorphous thermoplastic resin comprises one or more resins selected from an acrylic resin, an ABS resin, and a polycarbonate resin.
16. The method of claim 15 , wherein the amorphous thermoplastic resin comprises an acrylic resin.
17. The method according to any one of claims 1 to 16, The amorphous thermoplastic resin film is an acrylic resin film.
18. A CFRP part and a resin protective layer covering at least a part of a surface of the CFRP part, the protective layer is made of an amorphous thermoplastic resin, A three-dimensional CFRP product, wherein the glass transition temperature of the CFRP portion is higher than the glass transition temperature of the amorphous thermoplastic resin.
19. 19. The CFRP product according to claim 18, wherein the amorphous thermoplastic resin comprises one or more resins selected from acrylic resins, ABS resins, and polycarbonate resins.
20. 20. The CFRP product of claim 19, wherein the amorphous thermoplastic resin comprises an acrylic resin.
Citation Information
Patent Citations
Coated molded article and production method therefor
JP2018001411A