Method for producing metal-supported carrier and metal-supported carrier precursor

By controlling metal immobilization and reduction processes, the method addresses particle coarsening and clogging issues, achieving efficient and stable production of metal-supported carriers for catalysts.

JP2024140616APending Publication Date: 2024-10-10FURUYA KINZOKU KK

Patent Information

Application Number
JP2023051833
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing methods for synthesizing metal nanoparticles face issues such as particle coarsening, agglomeration, and equipment clogging due to the use of high-boiling reducing agents and hydroxide ions, leading to reduced productivity and inefficiencies in catalyst production.

Method used

A method involving mixing metal compounds with a carrier in a liquid, fixing the metal on the carrier to a specific ratio, and combining with a reducing agent to form a metal-supported carrier, which suppresses particle coarsening and prevents clogging by controlling the metal immobilization and reduction process.

Benefits of technology

The method effectively reduces particle size and enhances metal loading rates while minimizing equipment clogging, resulting in stable and efficient production of metal-supported carriers for catalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000015_0000
    Figure 00000015_0000
Patent Text Reader

Abstract

To provide a method for producing a metal-supported carrier in which nano-metal particles are more suppressed from becoming coarse, and, even in continuous production of nano-metal particles, blocking of piping is difficult to occur, in particular, a metal-supported carrier in which metal of nano particle is supported.SOLUTION: A method for producing a metal-supported carrier, comprising the steps of: mixing one or more metal compounds with a carrier in a liquid; fixing the metal in the metal compound to the carrier; an amount of the metal fixed to the carrier being 0.8 or more and 1 or less relative to the amount of the metal in the metal compound; combining a fluid containing the carrier with the fixed metal and a fluid containing a reducing agent; and recovering a metal-supported carrier in which the metal in the metal compound is supported on the carrier.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a metal-supported carrier and a metal-supported carrier precursor used in the production method. [Background technology]

[0002] Generally, catalysts containing rare metals such as precious metals are widely used in catalysts used for purifying exhaust gas from automobiles, etc., and in various reactions such as compound synthesis. However, rare metals are expensive and produced in small quantities, so there is a demand to reduce their use, and development is underway of nanoparticles, which are small particles of rare metals with a particle size of 100 nm or less that are considered to be highly active.

[0003] A batch synthesis method is known for synthesizing such nanoparticles, in which a high-boiling point reducing agent such as triethylene glycol is heated to a high temperature and then a precious metal salt solution is gradually added to the reducing agent. However, in the batch synthesis, the concentration of the precious metal in the reducing agent solution gradually increases, which causes problems such as particle growth and coarsening, making it difficult to mass-produce alloys with small particle sizes using the batch synthesis method.

[0004] As a means for preventing such coarsening of nanoparticles, for example, Patent Document 1 discloses a flow synthesis method for metal particles using a microreactor. In Patent Document 1, a palladium metal salt solution and a ruthenium metal salt solution are reacted under pressure in a microreactor in the presence of a reducing agent to synthesize solid solution metal nanoparticles of palladium and ruthenium.

[0005] However, extremely small metal nanoparticles are prone to aggregation, and even if metal nanoparticles are synthesized in a microreactor, aggregation of the metal nanoparticles may progress in the solution of the metal nanoparticles during or after synthesis, resulting in coarse metal particles. In addition, when reduction is performed with a reducing agent, it may be necessary to use a large amount of reducing agent due to the reduction rate of the raw metal. The reducing agent is usually an alkali metal hydroxide, but if hydroxide ions are mixed into the metal particles that are coarsened by the alkali metal, it is difficult to remove the mixed hydroxide ions. It is known that hydroxide ions that cannot be completely removed and remain in the metal particles have a negative effect on the reaction apparatus and subsequent reactions.

[0006] In an attempt to suppress this coarsening, Patent Document 2 discloses an apparatus used for synthesizing metal nanoparticles by a flow reaction in which a liquid containing a reducing agent, a liquid containing elements that constitute the single metal microparticles or solid solution microparticles to be supported, and a liquid containing carrier particles are continuously fed and these liquids are merged, resulting in the metal nanoparticles being supported on the carrier. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent Publication No. 2022-109275 [Patent Document 2] WO2020 / 262121 Summary of the Invention [Problem to be solved by the invention]

[0008] According to the method described in Patent Document 2, the metal nanoparticles are supported on a carrier, thereby suppressing the coarsening of the metal nanoparticles. However, the suppression effect is not sufficient, and there are cases in which the piping of the equipment is clogged, resulting in reduced productivity. [Means for solving the problem]

[0009] The present inventors have conducted extensive research to solve the above problems and have completed the present invention.

[0010] [1] A method for producing a metal-loaded carrier, comprising the steps of: mixing one or more metal compounds with a carrier in a liquid; fixing the metal in the metal compound to the carrier; the amount of metal fixed to the carrier being 0.8 or more and 1 or less relative to the amount of metal in the metal compound; combining a fluid containing the carrier with the fixed metal and a fluid containing a reducing agent; and recovering a metal-loaded carrier in which the metal in the metal compound is supported on the carrier. [2] The method for producing a metal-supported carrier according to [1] above, wherein the compound of the metal is a compound of two or more metals. [3] The method for producing a metal-supported carrier according to [1] or [2] above, wherein the metal compound contains at least a platinum group metal compound. [4] The method for producing a metal-supported carrier according to any one of [1] to [3] above, wherein the metal compound contains at least a compound of a base metal. [5] The method for producing a metal-supported carrier according to [3] above, wherein the compound of a platinum group metal is a compound of at least one metal selected from the group consisting of platinum, palladium, iridium, ruthenium and rhodium. [6] The method for producing a metal-supported carrier according to [4] above, wherein the compound of the base metal is a compound of at least one metal selected from the group consisting of iron, cobalt, nickel and copper. [7] The method for producing a metal-supported carrier according to any one of [1] to [6] above, wherein the metal compound contains a compound of at least one metal selected from the group consisting of platinum, palladium, iridium, ruthenium, and rhodium, and a compound of at least one metal selected from the group consisting of iron, cobalt, nickel, and copper. [8] The method for producing a metal-supported carrier according to any one of [1] to [7] above, further comprising a washing step of washing the metal-supported carrier after joining a fluid containing the carrier to which the metal is fixed and a fluid containing a reducing agent.

[0011] The present invention also has the following aspects. [9] A metal-supported carrier precursor having one or more metals fixed to a carrier.

[10] The metal-supported carrier precursor according to the above item [9], in which two or more metals are fixed to the carrier.

[11] The metal-loaded carrier precursor according to [9] or

[10] above, wherein the metal fixed to the carrier contains at least a platinum group metal.

[12] The metal-loaded carrier precursor according to any one of [9] to

[11] above, wherein the metal fixed to the carrier contains at least a base metal. Effect of the Invention

[0012] According to the present invention, a method for producing a metal-loaded support is provided in which the coarsening of nanometal particles is further suppressed and which is less likely to cause blockage of piping, etc., even during continuous production of nanometal particles, in particular a metal-loaded support carrying nanoparticles of metal. The present invention also provides a metal-supported carrier precursor for use in producing the metal-supported carrier. [Brief description of the drawings]

[0013] [Figure 1] 1 is an example of a manufacturing apparatus according to a preferred embodiment for carrying out a part of the manufacturing method of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The present invention will be described in detail below with reference to the embodiments, but the present invention is not limited to these descriptions. Various modifications of the embodiments may be made as long as the effects of the present invention are achieved.

[0015] The method for producing a metal-supported carrier of the present invention (hereinafter also referred to as the present production method) comprises mixing one or more metal compounds with a carrier in a liquid, fixing the metal in the metal compound to the carrier such that the amount of metal fixed to the carrier is 0.8 to 1 relative to the amount of metal in the metal compound, combining a fluid containing the carrier with the fixed metal and a fluid containing a reducing agent, and recovering a metal-supported carrier in which the metal in the metal compound is supported on the carrier. The compound of one or more metals (hereinafter also referred to as the present metal compound) is a compound of one metal or a compound of two or more metals. The present metal compound may be, for example, any of inorganic metal compounds such as metal halides, chalcogen compounds, hydroxides, and inorganic acid salts, and organic metal compounds such as alkoxide compounds, organic acid salts, and organic metal complexes, or a mixture of both. The metal compounds may be different compounds of the same metal, or one compound may contain two or more metals, provided that different compounds of the same metal are a compound of only one metal. Among these compounds, at least one selected from the group consisting of one or more metal halides, chalcogen compounds, hydroxides, inorganic acid salts, alkoxide compounds, carbonyl compounds, organic acid salts, and organometallic complexes is preferred, and from the viewpoint of solubility, halides are more preferred.

[0016] Examples of the halide include iodide, chloride, and bromide, with chloride being preferred from the viewpoint of handling. From the viewpoint of handling, the chalcogen compound is preferably an oxide or a sulfide. Examples of inorganic acid salts include metal salts with sulfuric acid, nitric acid, carbonic acid, phosphoric acid, silicic acid, sulfurous acid, nitrous acid, or phosphorous acid, and among these, sulfates, nitrates, carbonates, and silicates are preferred from the viewpoint of stability, and sulfates are more preferred.

[0017] The alkoxide compound is preferably a metal alkoxide compound with an alkoxy having 1 to 8 carbon atoms or a metal phenoxide compound with phenol, and more preferably a metal methoxy, metal ethoxy, metal propoxy, metal butoxy, or metal phenoxy.

[0018] Examples of organic acid salts include metal salts with carboxylic acids, sulfonic acids, etc., and among these, preferred are carboxylates such as formates, acetates, propionates, butyrates, oxalates, lactates, malonates, succinates, fumarates, maleates, benzoates, isophthalates, terephthalates, salicylates, etc., and sulfonates such as methanesulfonates, trifluoromethanesulfonates, benzenesulfonates, p-toluenesulfonates, etc. The organic acids may be substituted with fluorine or chlorine, etc., and may form an anhydrous salt intramolecularly or intermolecularly. Among these, oxalates, salicylates, formates and lactates are more preferable from the viewpoint of solubility.

[0019] Examples of the organometallic complex include alkyl complexes, carbonyl complexes, olefin complexes, aromatic complexes, and acetylacetonate complexes. Among these organometallic complexes, acetylacetonate complexes and carbonyl complexes are preferred from the viewpoints of reducibility and thermal decomposition properties.

[0020] The one or more metals in the metal compound include metals contained in Groups 3 to 12 of the Periodic Table, including noble or base metals. Examples of the noble metal include gold, silver, platinum, palladium, rhodium, iridium, ruthenium, and osmium. When the metal-supported carrier obtained by the present production method is used as a catalyst for purifying exhaust gas, platinum, palladium, rhodium, iridium, and ruthenium are preferred.

[0021] Examples of the base metal include iron, copper, nickel, aluminum, lead, zinc, tin, tungsten, molybdenum, tantalum, magnesium, cobalt, bismuth, cadmium, titanium, zirconium, antimony, manganese, beryllium, chromium, germanium, vanadium, gallium, hafnium, indium, niobium, rhenium, and thallium. When the metal-supported carrier obtained by the present production method is used as a catalyst for exhaust gas purification, iron, cobalt, copper, and nickel are preferred.

[0022] Examples of the metal compound include chloroplatinic acid, dinitrodiammineplatinum, hexahydroxoplatinic acid, palladium chloride, potassium chloropalladate, palladium sulfate, dinitrodiamminepalladium, chloroiridic acid, iridium chloride, rhodium chloride, rhodium nitrate, ruthenium chloride, and ruthenium iodide. The present metal compound is appropriately selected depending on the above-mentioned use of the obtained metal-supported carrier. For example, potassium chloropalladate, palladium chloride, chloroplatinic acid, iridium chloride, chloroiridic acid, rhodium chloride, and rhodium nitrate are preferred, and potassium chloropalladate, chloroplatinic acid, and chloroiridic acid are more preferred.

[0023] The carrier to be mixed with the present metal compound is appropriately selected depending on the application of the obtained metal-supported carrier, and examples thereof include alumina, silica, silica-alumina, calcia, magnesia, titania, ceria, zirconia, ceria-zirconia, titania-zirconia, lanthana, lanthana-alumina, tin oxide, tungsten oxide, aluminosilicate, aluminophosphate, borosilicate, phosphotungstic acid, hydroxyapatite, hydrotalcite, perovskite, cordierite, mullite, silicon carbide, activated carbon, carbon black, acetylene black, carbon nanotubes, and carbon nanohorns. When the carrier is used as a catalyst for exhaust gas purification, alumina, ceria, zirconia, ceria-zirconia, and magnesia are more preferable. The larger the specific surface area of ​​the carrier, the greater the amount of metal particles that can be adsorbed. 2 / g or more is preferable, and 100m 2 It is more preferable that the molecular weight is 1 / g or more.

[0024] The liquid used when mixing the present metal compound and the carrier in a liquid is usually a compound having a melting point of 80° C. or higher at one atmospheric pressure, and may be a compound that dissolves the present metal compound or a compound that disperses the present metal compound in a colloidal or slurry form. Examples of the liquid used include water or an organic solvent. As described below, in this production method, from the viewpoint of efficiently fixing metal ions or metal complexes to the support, it is preferable that the metal in the metal compound becomes metal ions when mixed with the support in a liquid, and it is preferable that the liquid has the property of dissolving the metal compound.

[0025] Examples of the organic solvent include alcohols having 2 to 6 carbon atoms, alkanes having 3 to 8 carbon atoms, carboxylic acids having 1 to 6 carbon atoms, and polyhydric alcohols having two or more hydroxyl groups (OH groups). Among the organic solvents, alcohols are preferred. The liquid used when mixing the present metal compound with the carrier is appropriately selected depending on the present metal compound used, but is preferably at least one selected from the group consisting of water and organic solvents, and more preferably water.

[0026] When the present metal compound and the carrier are mixed in the liquid, the present metal compound and the liquid may be mixed in advance and the carrier may be added thereto, or the carrier and the liquid may be mixed in advance and the present metal compound may be added thereto, or the present metal compound and the carrier may be added to the liquid simultaneously, or the present metal compound and the liquid may be mixed in advance and the carrier and the liquid may be mixed in advance separately, and then the two may be mixed. The addition may be continuous or intermittent. The metal compound and the support may be mixed either batchwise or continuously.

[0027] From the viewpoint of efficiently fixing the metal in the present metal compound to the support, it is preferable to premix the present metal compound with the liquid and then add the support thereto, or to premix the present metal compound with the liquid, separately premix the support with the liquid, and then mix the two together.

[0028] With respect to the concentration of the present metal compound when mixed in the liquid, from the viewpoint of supporting the metal with a small particle size, the metal concentration is preferably low, preferably 20% by mass or less, more preferably 10% by mass or less, based on 100% by mass of the total mass of the metal in the present metal compound, the support, and the liquid, and further preferably 0.1% by mass or more and 10% by mass or less. From the viewpoint of fluidity of the liquid, the concentration of the carrier when mixed in the liquid is preferably 20% by mass or less, more preferably 10% by mass or less, based on 100% by mass of the total mass of the metal in the metal compound, the carrier, and the liquid, and further preferably 0.1% by mass or more and 10% by mass or less.

[0029] The present metal compound and a carrier are mixed in a liquid to obtain a mixed liquid. In the obtained mixed liquid, the metal in the present metal compound is dissociated and exists in various forms, such as metal ions, metal complexes containing complex ions, and the present metal compound. In the present production method, the metal in the present metal compound, which exists in various forms in the mixed liquid, is fixed to a carrier. The term "fixed to a carrier" means that the metals present in the various forms are adsorbed in an unreduced state on the surface of the carrier or in the pores inside the carrier, as opposed to being supported on a carrier as described below. The metals present in the mixed solution in various forms as described above are fixed to a support to form a metal-supported support precursor in which one or more metals are fixed to a support. In the metal-supported support precursor, the metal in the present metal compound is fixed on the support in the form of a metal ion dissociated from the present metal compound, in the form of a metal complex containing a complex ion, in the form of the present metal compound, or the like. The metal in various forms fixed to the support in this way is also referred to as "metal fixed to a support."

[0030] When this metal-supported carrier precursor is brought into contact with a reducing agent, which will be described later, the metal fixed to the carrier is reduced to a zero-valent metal, thereby forming a metal-supported carrier in which the metal is supported on the carrier.

[0031] On the other hand, some of the metal ions, metal complexes containing complex ions, and the present metal compounds, etc., present in the mixed solution may be present in the mixed solution without being fixed to the carrier. When they come into contact with a reducing agent described later in this state, they are reduced to metals in a state free from the carrier, and when they are subsequently supported on the carrier, the metal particles grow and become coarse on the carrier, making it difficult to reduce the particle size like nanometal particles. In addition, when the metal ions, metal complexes containing complex ions, and the present metal compound, etc., which are not fixed and are present in the mixed liquid, are reduced to become metal particles suspended in the fluid described below, the metal loading rate on the metal-supported carrier decreases, making it difficult to achieve a desired metal loading rate or to increase the metal loading rate. Furthermore, when the metal ions, metal complexes containing complex ions, and the present metal compound, etc., present in the mixed liquid are reduced in the continuously transported fluid to become metal particles, and when they are suspended in the fluid, they adhere to the pipe walls in the transport pipe, etc., and induce clogging of the transport pipe, which may cause a decrease in productivity. In particular, when the amount of the raw metal compound is increased in order to increase the metal loading rate, such clogging of the transport pipe becomes more pronounced.

[0032] In the present production method, the amount of metal fixed to the support is 0.8 to 1 relative to the amount of metal in the present metal compound. The amount of metal fixed to the support is the total amount of metal fixed to the support in the various forms described above. In addition, when the amount of metal fixed to the support is 0.8 or more and 1 or less relative to the amount of metal in the present metal compound, this means that the value obtained by dividing the amount of metal fixed to the support by the amount of metal in the present metal compound used in this production method is 0.8 or more and 1 or less, and a value of 1 means that all of the metal in the present metal compound is fixed to the support. The amount of metal in the metal compound and the amount of metal fixed to the support are both the number of moles of metal atoms, and when the metal is fixed to the support as a metal complex, for example, the number of moles of the metal contained in the metal complex. The amount of metal fixed to the support is the total number of moles of the metal fixed to the support in the various forms.

[0033] By fixing the metal ions, metal complexes containing complex ions, and the present metal compound present in the mixed liquid to a support prior to contact with a reducing agent, the coarsening of the metal particles as described above is suppressed, and the metal loading rate on the support is improved. In addition, the number of metal particles suspended in the continuously transported fluid is reduced, and the precipitation of metal particles on the walls of the transport pipe, etc. is suppressed, thereby preventing blockage of the transport pipe, etc., and as a result, productivity is improved.

[0034] In addition, when the present metal compound contains two or more kinds of metals, the amount of the metal fixed to the support is the sum of the amounts of the fixed metals. When the present metal compound contains two or more kinds of metals, the ratio of the amounts of the metals fixed to the support does not necessarily have to be the same as the ratio of the metals in the present metal compound, but it is preferable that the amount of each metal fixed to the support is 0.8 to 1 relative to the amount of each metal in the present metal compound, and the ratio of each metal in the present metal compound is the same as the ratio of each metal fixed to the support. As described above, the metals present in various forms in the mixed solution are fixed to the support. The ratio of the amount of the metal fixed to the support to the amount of the metal in the metal compound is preferably 0.85 or more, more preferably 0.9 or more, and even more preferably 0.95 or more.

[0035] Methods for measuring the amount of metal fixed to the support include, for example, isolating the support on which the metal is fixed and quantifying the amount of metal fixed to the support by ICP emission spectroscopy or X-ray fluorescence analysis, or a method in which the metal compound and the support are mixed in the liquid, and then the amount of metal in the liquid is quantified by ICP emission spectroscopy or the like, and the amount of metal fixed to the support is calculated by subtracting the amount of metal in the liquid from the total amount of metal.

[0036] By quantifying the concentration of the metal present in various forms in the mixed liquid using the above method while mixing the metal compound and the support in the liquid, the end point of fixation of the metal present in various forms in the mixed liquid to the support can be determined, making it possible to efficiently fix the metal to the support.

[0037] The metal can be fixed to the support by, for example, adjusting the pH of the mixture, concentrating the mixture to reduce the amount of the liquid, introducing the metal into the pores of the support by vacuum impregnation, modifying the surface of the support, etc. The fixation may be performed by any method that, in a mixed liquid obtained by mixing the present metal compound and the support in a liquid, results in a more stable state for the metal in the present metal compound when the amount of metal fixed to the support is 0.8 to 1 relative to the amount of metal in the present metal compound, and is not limited to the above method. The pH of the mixture may be adjusted, for example, by adding a buffer solution, a weakly acidic compound, or a weakly basic compound to the mixture depending on the pH of the mixture. When concentrating the mixture, the liquid may be evaporated by heating, reducing pressure, or a combination of both until the volume of the mixture is reduced to 50% or less, preferably 30% or less, and more preferably 25% or less, or all of the liquid may be removed. When modifying the surface of the support, a support whose surface has been previously modified may be used, or a modifying agent may be added to the mixed solution. Examples of the method for modifying the support include a method for generating cationic ions on the surface of the support, and a method for introducing a group capable of coordinating to a metal onto the surface of the support. As a method for immobilizing the metal on the support, the method of concentrating the mixture is preferable from the viewpoint of simplicity.

[0038] The above steps provide a metal-supported carrier precursor in which the amount of metal fixed on the carrier is 0.8 to 1 relative to the amount of metal in the metal compound. In the following, the metal-supported carrier precursor in which the amount of metal fixed on the carrier is 0.8 to 1 relative to the amount of metal in the metal compound is also referred to as metal-supported carrier precursor A. The obtained metal-supported carrier precursor A may be separated from the process of fixing the metal compound to the carrier and used as a fluid containing the metal-supported carrier precursor described below, or may be used as a fluid containing the metal-supported carrier precursor A as is without separation.

[0039] The obtained fluid containing the metal-supported carrier precursor A and a fluid containing a reducing agent are joined, and the metal ions fixed to the carrier are reduced by the reducing agent to metals with a valence of 0, thereby obtaining a metal-supported carrier in which metal particles are supported on the carrier. The fluid containing the metal-supported carrier precursor A is a gas or liquid containing the metal-supported carrier precursor A, and the fluid containing the reducing agent is a gas or liquid containing the reducing agent.

[0040] Examples of the gas containing the metal-supported carrier precursor A include oxygen, air, and inert gases. The inert gas is a gas that does not react with the metal contained in the metal-supported carrier precursor, and examples of the inert gas include nitrogen, helium, and argon. The liquid containing the metal-supported carrier precursor A includes a liquid that disperses the metal-supported carrier precursor A, and includes water or an organic solvent. The organic solvent includes the same organic solvent used when mixing the present metal compound and the carrier. When the liquid containing the metal-supported carrier precursor A is an organic solvent, it may be the same as or different from the organic solvent used when mixing the present metal compound and the carrier, but it is preferable to use the same organic solvent from the viewpoint of production efficiency. In addition, there may be a plurality of fluids containing the metal-supported carrier precursor A. For example, different fluids may be used for each metal or compound of the metal compound. Each fluid may be merged separately with a fluid containing a reducing agent described later, but from the viewpoint of uniforming the quality of the obtained metal-supported carrier, when there are a plurality of fluids containing the metal-supported carrier precursor A, it is preferable to merge all of the fluids containing the metal-supported carrier precursor A before merging with the fluid containing the reducing agent. When all of the fluids containing the metal-supported carrier precursor A are merged, they may be merged sequentially or all at once.

[0041] The reducing agent is a compound capable of reducing the metal ions in the metal-supported carrier precursor A, and is a compound that makes the metal of the carrier a zero-valent metal. The reducing agent includes inorganic reducing agents and organic reducing agents. Examples of the inorganic reducing agent include hydrazine, sodium borohydride, sodium hypophosphite, lithium aluminum hydride, sodium sulfite, and sodium phosphinate. Examples of the organic reducing agent include ethylene glycol, diethylene glycol, trimethylene glycol, triethylene glycol, propylene glycol, tetraethylene glycol, and 1,2-alkanediols such as 1,2-hexadecanediol.

[0042] The gas containing a reducing agent may be the same as the gas described above, and the liquid containing a reducing agent may be the same as the liquid described above. The fluid may also contain a reducing gas as a reducing agent, such as hydrogen, carbon monoxide, or a hydrocarbon gas.

[0043] The fluid containing the metal-supported carrier precursor A and the fluid containing the reducing agent are joined together. The fluids may be either liquids or gases, or a combination of liquid and gas, but a combination of liquids is preferred from the viewpoint of production efficiency.

[0044] In this manufacturing method, at least one of the fluid containing the metal-supported carrier precursor A and the fluid containing the reducing agent is continuously supplied. Either one of the fluids continuously supplied is joined to the other fluid continuously or intermittently. From the viewpoint of reducing the particle size of the metal particles in the obtained metal-supported carrier, it is preferable to continuously supply both the fluid containing the metal-supported carrier precursor A and the fluid containing the reducing agent and join them.

[0045] The temperature when the fluid containing the metal-supported carrier precursor A and the fluid containing the reducing agent are mixed is preferably 100° C. or higher, more preferably 200° C. or higher, and even more preferably 300° C. or higher, from the viewpoint of promoting the reduction reaction. Moreover, the temperature when the fluid containing the metal-supported carrier precursor A and the fluid containing the reducing agent are mixed is preferably 500° C. or lower, more preferably 400° C. or lower, and even more preferably 374° C. or lower, from the viewpoint of the particle size of the metal particles of the obtained metal-supported carrier. In order to achieve the above-mentioned temperature, the temperature of at least one of the fluid containing the metal-supported carrier precursor A and the fluid containing the reducing agent may be raised to the above-mentioned temperature range before the fluids are joined, or the temperature of the joining point may be set to the above-mentioned temperature range after the two fluids are joined.

[0046] The pressure when the fluid containing the metal-supported carrier precursor A and the fluid containing the reducing agent are mixed is preferably 0.1 MPa or more, more preferably 20 MPa or more, and even more preferably 30 MPa, from the viewpoint of increasing the boiling point. The temperature when the fluid containing the metal-supported carrier precursor A and the fluid containing the reducing agent are mixed is preferably 500° C. or less, more preferably 400° C. or less, and even more preferably 374° C. or less, from the viewpoint of the particle size of the metal particles of the obtained metal-supported carrier. In order to achieve the above-mentioned pressure, the pressure of at least one of the fluid containing the metal-supported carrier precursor A and the fluid containing the reducing agent may be increased to the above-mentioned pressure range before the fluids are joined, or the pressure at the joining point may be set to the above-mentioned pressure range after the two fluids are joined.

[0047] The reaction time for reducing the metal ions contained in the metal-supported carrier precursor A by joining the fluid containing the metal-supported carrier precursor A with the fluid containing the reducing agent is desirably as short as possible so that the metal particles contained in the resulting metal-supported carrier do not become coarse due to thermal aggregation. The reaction time is preferably 1 to 300 minutes, more preferably 10 to 120 minutes, and even more preferably 10 to 60 minutes. The fluid containing the metal-supported carrier precursor A and the fluid containing the reducing agent may be joined once or multiple times. For example, the fluid containing the reducing agent may be joined multiple times to the fluid containing the metal-supported carrier precursor A that is continuously supplied, or the fluid containing the metal-supported carrier precursor A may be joined multiple times to the fluid containing the reducing agent that is continuously supplied. When joining multiple times, the temperature and pressure at the time of joining are the temperature and pressure at the time of first joining. In addition, the reduction reaction time is the time from the time of first joining.

[0048] As described above, the metal ions contained in the metal-supported carrier precursor A are reduced with a reducing agent to generate a metal-supported carrier in which zero-valent metal particles are supported on the carrier (hereinafter also referred to as the present metal-supported carrier). Note that the term "supported" differs from the above-mentioned "fixed" in that the zero-valent metal is attached to the carrier or in the pores of the carrier, and the metal is usually attached to the carrier by a physical force acting between the metal and the carrier. The metal-supported carrier thus produced is separated and recovered from the fluid to obtain the metal-supported carrier. For example, the recovery method includes a method in which a fluid containing a metal-supported carrier precursor A and a fluid containing a reducing agent are joined together, the metal-supported carrier is precipitated by cooling or the like, and the precipitated metal-supported carrier is separated and recovered from the fluid by filtration, sedimentation, centrifugation, or the like. The temperature and pressure at the time of joining are preferably maintained until the present metal-supported carrier is recovered by the above-mentioned method. The reduction reaction time is the time until the present metal-supported carrier is recovered. From the viewpoint of the purity of the obtained metal-supported carrier, it is preferable to further wash the metal-supported carrier with water or an organic solvent, and then recover the metal-supported carrier in the same manner as described above.

[0049] In the present production method, the step of joining the fluid containing the metal-supported carrier precursor A and the fluid containing the reducing agent and recovering the present metal-supported carrier is preferably carried out using a production apparatus such as that shown in FIG. 1, from the viewpoint of being able to control the particle size of the metal particles in the obtained present metal-supported carrier to a small size.

[0050] The manufacturing apparatus 100 has a first fluid supply source 1 that supplies a fluid containing a metal-supported carrier precursor A, and a second fluid supply source 2 that supplies a fluid containing a reducing agent. The manufacturing apparatus 100 may also have a heating unit for heating the fluid containing the metal-supported carrier precursor A supplied from the first fluid supply source 1 and the fluid containing the reducing agent supplied from the second fluid supply source 2, as necessary. The manufacturing apparatus 100 can also adjust the pressure by a pressure adjustment mechanism 9, which will be described later, as necessary. The manufacturing apparatus 100 also has a reaction unit 3 that merges the fluid containing the metal-supported carrier precursor A and the fluid containing the reducing agent. The first fluid supply source 1 and the reaction section 3 are connected by a supply route 4, and a fluid containing a metal-supported carrier precursor A is supplied from the first fluid supply source 1 to the reaction section 3 via the supply route 4. The second fluid supply source 2 and the reaction section 3 are connected by a supply route 5, and a fluid containing a reducing agent is supplied from the second fluid supply source 2 to the reaction section 3 via the supply route 5.

[0051] Furthermore, the reaction section 3 is connected to a recovery section 7 for recovering the generated reaction product by a supply route 6, and a cooling section 8 is disposed around the supply route 6 between the reaction section 3 and the recovery section 7. As a result, the metal-loaded carrier generated in the reaction section 3 is cooled by the cooling section 8 when passing through the supply route 6, and is transported to the recovery section 7. Furthermore, the production apparatus 100 has a pressure adjustment mechanism 9 for the purpose of making the reaction section a high-pressure condition. The pressure adjustment mechanism 9 may be connected to the recovery section 7 as shown in FIG. 1, or may be connected between the cooling section 8 and the recovery section 7 via the supply route 6. The pressure adjustment mechanism may be a plunger, a cylinder, or a regulator, with the cylinder being preferred from the viewpoint of preventing clogging or wear.

[0052] The supply routes 4 to 6 are formed by, for example, piping. The production apparatus 100 makes it possible to stably produce the present metal-loaded carrier.

[0053] In the reaction section 3, a fluid containing the metal-supported carrier precursor A and a fluid containing a reducing agent are joined and mixed together, whereby metal ions in the metal-supported carrier precursor A are reduced to zero-valent metal particles. The pressure adjustment mechanism 9 is located downstream of the production apparatus 100 and is connected to the reaction section 3, the supply route 4, the supply route 5, and the supply route 6, and therefore has a function of adjusting the pressure of the entire production apparatus 100, but may also have a function of adjusting only the pressure of the reaction section 3. In Fig. 1, the pressure adjustment mechanism 9 adjusts the pressure of the reaction section and all of the liquid transfer routes.

[0054] A supply route 4 connecting the first fluid supply source 1 and the reaction section 3 has a supply means. The supply route 4 may be provided with a flow rate adjusting means such as a needle valve or a stop valve for adjusting the flow rate. The supply route 5 connecting the second fluid supply source 2 and the reaction section 3 has a supply means. As with the supply route 4, the supply route 5 may be provided with a means for adjusting the flow rate, such as a needle valve or a stop valve. At least one of the supplying means has a function of continuously supplying a fluid, and it is preferable that both of the supplying means have a function of continuously supplying a fluid.

[0055] The manufacturing apparatus of FIG. 1 may have flow rate adjustment mechanisms 10 and 11 for unidirectionally transferring fluids flowing in either or both of the supply route 4 and the supply route 5. The manufacturing apparatus 100 shown in FIG. 1 has the flow rate adjustment mechanisms 10 and 11 in each of the supply route 4 and the supply route 5 in addition to the first fluid supply source 1, the second fluid supply source 2, the reaction section 3, the supply route 4, the supply route 5, the supply route 6, the recovery section 7, the cooling section 8, and the pressure adjustment mechanism 9. In this embodiment, the flow rate and flow rate of the fluid containing the metal-supported carrier precursor A in the supply route 4 and the flow rate and flow rate of the fluid containing the reducing agent in the supply route 5 can be stably controlled, so that the present metal-supported carrier can be stably manufactured. The flow rate adjustment mechanisms 10 and 11 can be, for example, a plunger, a cylinder, or a regulator.

[0056] There may be a plurality of first fluid supply sources 1. When there are a plurality of first fluid supply sources 1, a plurality of supply routes 4 may be provided accordingly, and each may be connected to the reaction section 3, or the plurality of supply routes 4 may join together before the reaction section 3. When there are multiple first fluid supply sources 1, each first fluid supply source 1 may supply a fluid containing a metal-supported carrier precursor A of a different metal, or may alternately supply a fluid containing a metal-supported carrier precursor A of the same metal.

[0057] There may be a plurality of second fluid supply sources 2. When there are a plurality of second fluid supply sources 2, a plurality of supply routes 5 may be provided accordingly, and each may be connected to the reaction section 3, or the plurality of supply routes 5 may join together before the reaction section 3. When there are a plurality of second fluid supply sources 2, the fluid containing the reducing agent may be supplied alternately.

[0058] A production method using a supply route as shown in FIG. 1 is preferable because it allows the present metal-supported carrier to be produced continuously and also allows the average particle size of the metal particles in the obtained present metal-supported carrier to be small. In the case of a production method using a supply route as shown in FIG. 1, it is possible to control the average particle size of the metal particles in the obtained metal-supported carrier by controlling the metal ion concentration and the reducing agent concentration contained in the metal-supported carrier precursor A of the first fluid supply source 1. In addition, by controlling the supply rate of the fluid containing the metal-supported carrier precursor A, the supply rate of the fluid containing the reducing agent, the temperature or cooling rate of the reaction section, etc., it is possible to control the average particle size of the present oxide to be obtained within the above-mentioned preferred range.

[0059] The metal-supported carrier precursor of the present invention (hereinafter also referred to as "the present metal-supported carrier precursor") has one or more metal ions or metal complexes fixed to the carrier. The present metal-supported carrier precursor becomes a metal-supported carrier by reducing the fixed metal ions or metal complexes, and is therefore suitably used as a precursor of a metal-supported carrier. The term "fixed" is the same as that described above. The metal ions or metal complexes fixed to the carrier may be precious metals or base metals, as in the case of the metal in the metal compound, and are appropriately selected depending on the intended use of the metal-supported carrier. Precious metals include gold, silver, platinum, palladium, rhodium, iridium, ruthenium, and osmium, and base metals include iron, copper, nickel, aluminum, lead, zinc, tin, tungsten, molybdenum, tantalum, magnesium, cobalt, bismuth, cadmium, titanium, zirconium, antimony, manganese, beryllium, chromium, germanium, vanadium, gallium, hafnium, indium, niobium, rhenium, and thallium. The carrier is the same as that used in the present metal-loaded carrier.

[0060] The amount of metal contained in the present metal-supported carrier precursor is appropriately set depending on the metal loading rate of the target metal-supported carrier, etc., but is preferably 0.1 to 20 mass%, and more preferably 0.1 to 10 mass%, based on the mass of the present metal-supported carrier precursor being 100 mass%.

[0061] The present metal-supported carrier precursor can be obtained, for example, by mixing the present metal compound and the carrier in a liquid to prepare a mixed liquid, and then fixing the metal ion or metal complex dissociated from the present metal compound to the carrier. Methods for immobilizing metal ions or metal complexes on a carrier include the methods described above. When immobilized, the amount of metal immobilized on the support is preferably 0.8 or more and 1 or less relative to the amount of metal in the metal compound, more preferably 0.85 or more is immobilized, even more preferably 0.90 or more is immobilized, and particularly preferably 0.95 or more is immobilized. The amount of metal in the present metal compound, the amount of metal fixed to the carrier, and the amount of metal fixed to the carrier relative to the amount of metal in the present metal compound are the same as described above.

[0062] The obtained metal-supported carrier precursor may be separated from the mixed solution, or may be used as it is in the present production method as the metal-supported carrier precursor A. Examples of the method for separation include natural filtration, suction filtration, and cross-flow filtration. The obtained metal-supported carrier precursor may be purified as necessary, for example by washing with pure water to remove impurities.

[0063] The present metal-supported carrier obtained by the present manufacturing method can reduce the particle size of the supported metal particles, and can increase the metal loading rate on the carrier while suppressing the coarsening of the particle size. Therefore, the present metal-supported carrier obtained by the present manufacturing method can be suitably used for chemical catalysts such as catalysts for purifying exhaust gases. Furthermore, according to the present production method, there is little deposition of metal in pipes and the like, and blockage of pipes is suppressed, and loss of metal compounds used as raw materials can be suppressed.

[0064] The present metal-supported carrier precursor can be suitably used in the present production method, and can be an effective precursor for producing a metal-supported carrier, not limited to the present production method.

[0065] The present manufacturing method and the present metal-supported carrier precursor have been described above. However, the present invention is not limited to the configuration of the above embodiment. For example, the configuration of the embodiment shown in Fig. 1 may have any other steps, devices, or functions added thereto, or may be replaced with any other steps that produce the same effect. The metal-supported carrier precursor may also contain other optional components. EXAMPLES

[0066] Examples of the present invention will be described below, but the present invention is not limited to these examples.

[0067] Example 1: Synthesis of metal carrier 1.5 mL of water, palladium chloride (Kojima Chemical, palladium content 32% by mass), platinum chloride (Furuya Metal, platinum content 46.8% by mass) and alumina were mixed in the amounts shown in Table 1, and a dry powder was obtained by distilling the water using a rotary evaporator with the water bath temperature set to 60°C and the vacuum level set to 60 hPa to distill off the water. Thereafter, the amount of pure water shown in Table 1 was added to the dried powder, and the powder was uniformly redispersed by stirring and ultrasonic treatment to obtain a metal support precursor solution as the raw material. Next, a metal carrier was synthesized using the manufacturing apparatus shown in FIG. 1. The metal carrier precursor solution obtained above was stored in the first fluid supply source 1, and the metal carrier precursor solution obtained above was sent from the first fluid supply source 1 to the reaction section 3 at a rate of 30 mL / min. Meanwhile, a reducing agent was stored in the second fluid supply source 2, and an ethanol aqueous solution containing 25 mass% of ethanol as a reducing agent was sent from the second fluid supply source 2 to the reaction section 3 at a rate of 200 mL / min, and the metal carrier precursor solution obtained above and the reducing agent were mixed in the reaction section 3 to obtain a metal carrier dispersion. Thereafter, the mixed metal carrier dispersion was cooled to room temperature and normal pressure of 20° C. at 1 atmosphere in the cooling section 8, and collected in the collection section 7. Thereafter, after filtration with a membrane filter, the filtrate was dried in an electric dryer at 800° C. for 4 hours to obtain 1.8 g of a metal carrier.

[0068] <Comparative Example 1> Synthesis of metal carrier Dispersions containing palladium chloride (manufactured by Kojima Chemical; palladium content 32.3% by mass), platinum chloride (manufactured by Furuya Metal; platinum content 46.8% by mass), and 1% by mass alumina were mixed in the amounts shown in Table 1 to obtain Dispersion 1 containing the raw metals. Next, a metal support was synthesized using the production apparatus shown in FIG. The dispersion liquid 1 containing the metal obtained above was stored in the first fluid supply source 1, and the dispersion liquid 1 containing the metal obtained above was sent from the first fluid supply source 1 to the reaction section 3 at a rate of 30 mL / min. Meanwhile, a reducing agent was stored in the second fluid supply source 2, and an ethanol aqueous solution containing 25 mass% of ethanol as a reducing agent was sent from the second fluid supply source 2 to the reaction section 3 at a rate of 200 mL / min, and the dispersion liquid 1 containing the metal obtained above and the reducing agent were mixed in the reaction section 3 to obtain a metal carrier dispersion liquid. Thereafter, the mixed metal carrier dispersion liquid was cooled to room temperature and normal pressure of 20 ° C. at 1 atmosphere in the cooling section 8, and collected in the collection section 7. Thereafter, after filtration with a membrane filter, the filtrate was dried in an electric dryer at 80 ° C. for 4 hours to obtain 1.7 g of a metal carrier.

[0069] <Comparative Example 2> Synthesis of metal carrier Metal-containing dispersion liquid 2 was prepared by mixing an aqueous solution of palladium chloride (manufactured by Kojima Chemical Co., Ltd., palladium content 32.3 mass%) and platinum chloride (manufactured by Furuya Metals, platinum content 46.8 mass%), and a dispersion liquid containing 1 mass% alumina in the amounts shown in Table 1. The metal concentration in metal-containing dispersion liquid 2 was 15.9 mmol / L. Next, a metal support was synthesized using the production apparatus shown in FIG. The metal carrier precursor solution obtained above was stored in the first fluid supply source 1, and the metal-containing dispersion 2 obtained above was flowed from the first fluid supply source 1 to the reaction section 3 at a rate of 30 mL / min, while the alumina dispersion was also flowed to the reaction section 3 at a rate of 30 mL / min, and the reducing agent was flowed to the reaction section 3 at a rate of 200 mL / min, whereby mixing was performed in the reaction section 3 to obtain a metal carrier dispersion. Thereafter, the mixed metal carrier dispersion was cooled to room temperature and normal pressure (1 atm, 20° C.) in the cooling section 8, and collected in the collection section 7. Thereafter, after filtration with a membrane filter, the filtrate was dried in an electric dryer at 80° C. for 4 hours to obtain 1.7 g of a metal carrier.

[0070] [Table 1]

[0071] TEM observation and particle size evaluation of the catalysts obtained in Example 1, Comparative Example 1, and Comparative Example 2 were performed on at least 100 catalysts using a JEOL transmission electron microscope (JEM-2010). The particle size was evaluated using image analysis software (Image-J) developed by the National Institutes of Health. The results are shown in Table 2.

[0072] [Table 2]

[0073] As is clear from the above results, the catalyst synthesized by the method described in Example 1 showed finer particle size and improved support rate compared to the catalysts synthesized by the methods of Comparative Examples 1 and 2. Therefore, by mixing one or more metal compounds with a support in a liquid, fixing the metal in the metal compound to the support, such that the amount of metal fixed to the support is 0.8 to 1 relative to the amount of metal in the metal compound, combining a fluid containing the support with the metal fixed thereto and a fluid containing a reducing agent, and recovering a metal-supported support in which the metal in the metal compound is supported on the support, the coarsening of nanometal particles can be further suppressed. Furthermore, taking into consideration the improved loading rate on the carrier, it is believed that in this production method, the step of fixing the metal to the carrier in advance suppresses the amount of metal desorbed from the carrier, and less metal adheres to the piping, thereby providing a metal-loaded carrier that is less likely to clog the equipment piping, in particular a metal-loaded carrier carrying nanoparticles of metal. [Explanation of symbols]

[0074] 1: First fluid supply source 2:Second fluid supply source 3: Reaction section 4: Supply route 5: Supply route 6: Supply route 7: Recovery Department 8: Cooling section 9: Pressure adjustment mechanism 10;Flow rate adjustment means 11: Flow rate adjustment means 100: Manufacturing equipment

Claims

1. A method for producing a metal-supported carrier, comprising the steps of: mixing one or more metal compounds with a carrier in a liquid; fixing the metal in the metal compound to the carrier; an amount of the metal fixed to the carrier being 0.8 or more and 1 or less relative to the amount of the metal in the metal compound; combining a fluid containing the carrier with the fixed metal and a fluid containing a reducing agent; and recovering a metal-supported carrier in which the metal in the metal compound is supported on the carrier.

2. 2. The method for producing a metal-supported carrier according to claim 1, wherein the compound of the metal is a compound of two or more metals.

3. 3. The method for producing a metal-supported carrier according to claim 1, wherein the metal compound contains at least a compound of a platinum group metal.

4. 3. The method for producing a metal-supported carrier according to claim 1, wherein the metal compound contains at least a compound of a base metal.

5. 4. The method for producing a metal-supported carrier according to claim 3, wherein the compound of a platinum group metal is a compound of at least one metal selected from the group consisting of platinum, palladium, iridium, ruthenium and rhodium.

6. 5. The method for producing a metal-supported carrier according to claim 4, wherein the compound of the base metal is a compound of at least one metal selected from the group consisting of iron, cobalt, nickel and copper.

7. 7. The method for producing a metal-supported carrier according to claim 5 or 6, wherein the metal compound comprises a compound of at least one metal selected from the group consisting of platinum, palladium, iridium, ruthenium and rhodium, and a compound of at least one metal selected from the group consisting of iron, cobalt, nickel and copper.

8. 3. The method for producing a metal-supported carrier according to claim 1, further comprising a washing step of washing the metal-supported carrier after the fluid containing the carrier having the fixed metal and a fluid containing a reducing agent are joined together.

9. A metal-supported carrier precursor having one or more metals fixed to a carrier.

10. The metal-supported carrier precursor according to claim 9, wherein two or more metals are fixed to the carrier.

11. The metal-supported carrier precursor according to claim 9 or 10, wherein the metal fixed to the carrier contains at least a platinum group metal.

12. The metal-supported carrier precursor according to claim 9 or 10, wherein the metal fixed to the carrier contains at least a base metal.

Citation Information

Patent Citations

  • Method for producing solid solution alloy particles

    JP2022109275A

  • Supported catalyst synthesis device and fine particle synthesis device

    WO2020262121A1

Cited By

  • Preparation method and device of metallized slurry for packaging substrate

    CN119747650A

  • Preparation method and apparatus for metallization slurry for package substrate