Resin composition, pellet, molded article and method for producing resin composition
By integrating iron into the polyethylene terephthalate resin and using recycled carbon fiber with nucleating agents and carbon black, the mold release resistance and mechanical strength of polyester resin compositions are enhanced, addressing the issue of increased mold release in recycled carbon fiber blends.
Patent Information
- Application Number
- JP2023051864
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
The use of recycled carbon fiber in polyester resin compositions leads to increased mold release resistance, which is undesirable in molded products.
Incorporating a specific amount of iron element into the polyethylene terephthalate resin, along with recycled carbon fiber, nucleating agents, and carbon black, to reduce mold release resistance and enhance mechanical strength.
The resin composition achieves low mold release resistance, improved mechanical strength, and reduced shrinkage rates in molded products, while maintaining high impact resistance.
Smart Images

Figure 2024140630000001 
Figure 2024140630000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, a pellet, a molded article, and a method for producing a resin composition, and in particular to a resin composition containing a polyester resin as a main component. [Background technology]
[0002] Polyester resins are widely used in various equipment parts. In particular, reinforcing fibers are widely used to increase the mechanical strength of molded products made from polyester resins. One representative example of such reinforcing fibers is carbon fiber. Patent Document 1 is known as such an example. On the other hand, from the viewpoint of effective use of limited resources, reuse of carbon fibers has been considered. Known examples of recycled carbon fibers include those described in Patent Documents 2 and 3. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Unexamined Patent Publication No. 51-109056 [Patent Document 2] JP 2016-041800 A [Patent Document 3] International Publication No. 2018 / 212016 Summary of the Invention [Problem to be solved by the invention]
[0004] However, it has been found that blending recycled carbon fibers with polyester resin can result in increased mold release resistance when molded using a mold. The present invention aims to solve the above problems, and to provide a resin composition using polyester resin and recycled carbon fibers, which results in a molded article with low demolding resistance, as well as a pellet, a molded article, and a method for producing the resin composition. [Means for solving the problem]
[0005] In view of the above problems, the present inventors have conducted research and found that the above problems can be solved by using a polyester resin containing a predetermined amount of iron element and recycled carbon fibers. Specifically, the above problems were solved by the following means. <1> A resin composition comprising a polyester resin containing a polyethylene terephthalate resin and recycled carbon fibers, wherein the polyethylene terephthalate resin contains elemental iron in a ratio of 1.0 to 100 μg / g. <2> The content of recycled carbon fiber is 5 to 70 parts by mass per 100 parts by mass of polyester resin. <1> The resin composition according to claim 1. <3> The polyethylene terephthalate resin contains a unit derived from isophthalic acid, and the unit derived from isophthalic acid is 0.5 mol % or more and 15 mol % or less of all units derived from a dicarboxylic acid component contained in the polyethylene terephthalate resin. <1> or <2> The resin composition according to claim 1. <4> Polyethylene terephthalate resin contains recycled materials. <1> ~ <3> 10. The resin composition according to claim 9 . <5> Further, the composition contains a nucleating agent in an amount of 0.01 to 10 parts by mass per 100 parts by mass of the polyester resin. <1> ~ <4> 10. The resin composition according to claim 9 . <6> Further, the polyester resin contains carbon black in an amount of 0.01 to 1 part by mass relative to 100 parts by mass of the polyester resin. <1> ~ <5> 10. The resin composition according to claim 9 . <7> The polyester resin further comprises a polybutylene terephthalate resin. <1> ~ <6> 10. The resin composition according to claim 9 . <8> the content of recycled carbon fiber is 5 to 70 parts by mass relative to 100 parts by mass of polyester resin, the polyethylene terephthalate resin contains units derived from isophthalic acid, and among all units derived from dicarboxylic acid components contained in the polyethylene terephthalate resin, the units derived from isophthalic acid account for 0.5 mol % or more and 15 mol % or less, the polyethylene terephthalate resin contains recycled products, and further contains a nucleating agent in a ratio of 0.01 to 10 parts by mass relative to 100 parts by mass of polyester resin, and further contains carbon black in a ratio of 0.01 to 1 part by mass relative to 100 parts by mass of polyester resin, <1> ~ <7> 10. The resin composition according to claim 9 . <9> The polyester resin further comprises a polybutylene terephthalate resin. <1> ~ <8> 10. The resin composition according to claim 9 . <10> <1> ~ <9> 2. A pellet of the resin composition according to claim 1. <11> <1> ~ <9> 2. A molded article formed from the resin composition according to claim 1. <12> A method for producing a resin composition comprising a polyester resin containing a polyethylene terephthalate resin and recycled carbon fibers, the polyethylene terephthalate resin containing iron element in a ratio of 1.0 to 100 μg / g, and further containing carbon black in a ratio of 0.01 to 1 part by mass per 100 parts by mass of the polyester resin, the method comprising blending the carbon black as a master batch premixed with the polyester resin, and melt-kneading the resulting mixture. <13> The polyester resin used in the masterbatch contains a polybutylene terephthalate resin. <12> A method for producing the resin composition according to claim 1. <14> The resin composition <1> ~ <9> The resin composition according to any one of the above items. <12> or <13> A method for producing the resin composition according to claim 1. Effect of the Invention
[0006] INDUSTRIAL APPLICABILITY The present invention makes it possible to provide a resin composition using a polyester resin and recycled carbon fibers, which gives a molded article having low demolding resistance, as well as a pellet, a molded article, and a method for producing the resin composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] Hereinafter, an embodiment of the present invention (hereinafter, simply referred to as "the present embodiment") will be described in detail. Note that the present embodiment is an example for explaining the present invention, and the present invention is not limited to the present embodiment. In this specification, the use of "to" means that the numerical values before and after it are included as the lower limit and upper limit. In this specification, various physical properties and characteristic values are those at 23° C. unless otherwise specified.
[0008] In this specification, unless otherwise specified, the weight average molecular weight is a polystyrene-equivalent value measured by GPC (gel permeation chromatography) using a Tosoh HLC-8320GPC EcoSEC with tetrahydrofuran as a solvent and Shodex KF-G, KF-805L x 3, KF-800D columns at a column temperature of 40°C and a flow rate of 1.2 mL / min, and detected at a detection wavelength of 254 nm. If the measurement methods, etc. described in the standards shown in this specification vary from year to year, they will be based on the standards as of January 1, 2023, unless otherwise stated.
[0009] The resin composition of the present embodiment is a resin composition containing a polyester resin including a polyethylene terephthalate resin and recycled carbon fiber, and is characterized in that the polyethylene terephthalate resin contains an iron element at a ratio of 1.0 to 100 μg / g. By adopting such a configuration, it is possible to reduce the mold release resistance of the obtained molded product. In particular, by blending carbon black into the resin composition and blending polybutylene terephthalate resin in addition to the polyethylene terephthalate resin, a significantly low mold release resistance is achieved. The reason for this is presumably that the polyethylene terephthalate resin contains iron, which increases the solidification rate and improves the mold release resistance. Furthermore, it is presumed that by blending polybutylene terephthalate resin in addition to polyethylene terephthalate resin, the polybutylene terephthalate resin has a faster crystallization rate than polyethylene terephthalate resin, and therefore solidification is further promoted. In addition, the molded product formed from the resin composition of this embodiment can also have a low shrinkage rate. This is presumably because the inclusion of polyethylene terephthalate resin suppresses crystallinity. Furthermore, the molded product formed from the resin composition of this embodiment can also have high mechanical strength. The mechanical strength is achieved by blending recycled carbon fiber, as well as by the polyethylene terephthalate resin having a certain copolymer unit or having a high intrinsic viscosity.
[0010] <Polyester resin> The polyester resin used in the present embodiment contains a polyethylene terephthalate resin, and the polyethylene terephthalate resin contains iron element at a ratio of 1.0 to 100 μg / g. By adopting such a constitution, it is possible to reduce the mold release resistance of the obtained molded article. The resin composition of the present embodiment contains at least a polyethylene terephthalate resin (hereinafter, sometimes referred to as "PET") as a polyester resin. The polyethylene terephthalate resin used in the present embodiment is a resin whose main units are dicarboxylic acid and diol. Furthermore, in the resin composition of the present embodiment, in addition to the polyethylene terephthalate resin, the polyester resin may contain other polyester resins (particularly, alkylene terephthalate resins, preferably polybutylene terephthalate resins).
[0011] <<Polyethylene terephthalate resin>> The resin composition of the present embodiment contains a polyethylene terephthalate resin. Polyethylene terephthalate resin, especially recycled products (such as recycled PET from PET bottles), may contain metal elements as impurities. This may come from a reactor or, in the case of recycled PET, from a cutter. Conventionally, it has been thought that such metal elements, especially iron elements, should not be included because they are magnetic substances. However, in the resin composition of the present embodiment, it has been found that the mold release resistance of the resulting molded product can be reduced by intentionally including a small amount of iron elements.
[0012] In this embodiment, the iron element acts as a crystal nucleating agent in the resin composition of this embodiment, and it is presumed that the iron element in particular contributes to improving the mold releasability of the molded article obtained by molding the resin composition. It goes without saying that in this embodiment, not only recycled PET but also virgin PET containing a predetermined amount of iron element is preferably used. The amount of iron element in the polyethylene terephthalate resin used in this embodiment is 1.0 μg / g or more, preferably 1.2 μg / g or more, more preferably 1.4 μg / g or more, and even more preferably 1.6 μg / g or more, even more preferably 1.8 μg / g or more, and even more preferably 2.4 μg / g or more depending on the application, etc. The amount of iron element in the polyethylene terephthalate resin is 100 μg / g or less, preferably 90 μg / g or less, more preferably 80 μg / g or less, even more preferably 50 μg / g or less, even more preferably 20 μg / g or less, even more preferably 10 μg / g or less, even more preferably 5 μg / g or less, and especially more preferably 4.5 μg / g or less.
[0013] Qualitative / semi-quantitative analysis (μg / g) of iron element in PET is performed by ICP emission spectrometry. Details are as described in the Examples below.
[0014] The polyethylene terephthalate resin used in the present embodiment preferably contains units derived from isophthalic acid, and among all units derived from dicarboxylic acid components contained in the polyethylene terephthalate resin, the units derived from isophthalic acid (hereinafter, sometimes referred to as "isophthalic acid units") are preferably 0.5 mol% or more and 15 mol% or less. By using such a specific polyethylene terephthalate resin, crystallization as a whole can be suppressed, the molding shrinkage rate is reduced, and a molded product with higher impact resistance tends to be obtained.
[0015] The proportion of the isophthalic acid units in all units derived from the dicarboxylic acid component is preferably 0.7 mol% or more, more preferably 0.9 mol% or more, even more preferably 1.1 mol% or more, even more preferably 1.3 mol% or more, and even more preferably 1.5 mol% or more. The proportion of the isophthalic acid units in all units derived from the dicarboxylic acid component is preferably 10 mol% or less, more preferably 8.0 mol% or less, and even more preferably 5.0 mol% or less.
[0016] The intrinsic viscosity of the polyethylene terephthalate resin is preferably 0.50 dL / g or more, more preferably 0.60 dL / g or more. By making it equal to or more than the lower limit, the impact resistance of the obtained molded article tends to be improved and the shrinkage rate tends to be small. The reason for this is presumed to be that the molecular weight increases, which makes it easier for the molecules to become entangled. The intrinsic viscosity of the polyethylene terephthalate resin is preferably 2.0 dL / g or less, more preferably 1.5 dL / g or less, even more preferably 1.2 dL / g or less, even more preferably 0.95 dL / g or less, even more preferably 0.85 dL / g or less, and even more preferably 0.84 dL / g or less. By making it equal to or less than the upper limit, the melt viscosity during melt kneading or molding does not become too high, and the load on the extruder or molding machine tends to be reduced. When the resin composition of the present embodiment contains two or more types of polyethylene terephthalate resins, the intrinsic viscosity refers to the intrinsic viscosity of the mixture. The intrinsic viscosity is measured as described in the Examples section below.
[0017] The melt volume rate (MVR) of polyethylene terephthalate resin measured in accordance with JIS K7210 (temperature 265°C, load 5kgf) is 10 cm 3 / 10 minutes or more is preferable, 20cm 3 / 10 minutes or more is more preferable, and 100 cm 3 / 10 minutes or less is preferable, 50 cm 3 It is more preferable that the time is 10 minutes or less.
[0018] Examples of acid components other than terephthalic acid and isophthalic acid in the polyethylene terephthalate resin used in this embodiment include naphthalenedicarboxylic acid, 4,4'-diphenylsulfonedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 1,3-phenylenedioxydiacetic acid and structural isomers thereof, dicarboxylic acids such as malonic acid, succinic acid, and adipic acid and derivatives thereof, and oxyacids such as p-hydroxybenzoic acid and glycolic acid and derivatives thereof. In the polyethylene terephthalate resin used in this embodiment, terephthalic acid units and isophthalic acid units preferably account for 80 mol % or more of all dicarboxylic acid units, more preferably 95 mol % or more, even more preferably 98 mol % or more, and even more preferably 99 mol % or more.
[0019] Examples of diol components other than ethylene glycol in the polyethylene terephthalate resin used in this embodiment include aliphatic glycols such as 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, pentamethylene glycol, hexamethylene glycol, and neopentyl glycol, alicyclic glycols such as cyclohexanedimethanol, and aromatic dihydroxy compound derivatives such as bisphenol A and bisphenol S. In the polyethylene terephthalate resin used in the present embodiment, ethylene glycol units preferably account for 80 mol % or more of all diol units, more preferably 95 mol % or more, even more preferably 98 mol % or more, and even more preferably 99 mol % or more.
[0020] Furthermore, the polyethylene terephthalate resin may be copolymerized with, for example, 1.0 mol % or less, preferably 0.5 mol % or less, and more preferably 0.3 mol % or less of a branched component, for example, an acid having a trifunctional ester forming ability such as tricarballylic acid, trimellitic acid, trimellitic acid, etc., or a tetrafunctional ester forming ability such as pyromellitic acid, or an alcohol having a trifunctional or tetrafunctional ester forming ability such as glycerin, trimethylolpropane, pentaerythritol, etc.
[0021] In the polyethylene terephthalate resin used in this embodiment, terephthalic acid units, isophthalic acid units, and ethylene glycol units preferably account for 90 mol % or more of all units excluding terminal groups, more preferably 95 mol % or more, even more preferably 98 mol % or more, and even more preferably 99 mol % or more.
[0022] The amount of terminal carboxyl groups in the polyethylene terephthalate resin may be appropriately selected and determined, but is usually 60 eq / ton or less, preferably 50 eq / ton or less, and more preferably 30 eq / ton or less. The lower limit of the amount of terminal carboxyl groups is not particularly determined, but is preferably 5 eq / ton or more in consideration of the productivity of the production of the polyethylene terephthalate resin. The terminal carboxyl group concentration of the polyethylene terephthalate resin is a value determined by dissolving 0.5 g of the polyethylene terephthalate resin in 25 mL of benzyl alcohol and titrating the solution with a 0.01 mol / L benzyl alcohol solution of sodium hydroxide. The amount of terminal carboxyl groups may be adjusted by any conventional method, such as adjusting polymerization conditions such as the raw material charging ratio during polymerization, polymerization temperature, and pressure reduction method, or by reacting a terminal blocking agent.
[0023] As the polyethylene terephthalate resin used in the present embodiment, it is preferable to use recycled PET, particularly recycled PET derived from PET bottles. In addition, polyethylene terephthalate resin (bio-PET) at least a part of the raw material is derived from biological resources (biomass) may be used. Recycled PET includes PET obtained through material recycling, in which collected used PET bottles and films are crushed, washed with water or alkali, and reused as fibers, etc., PET obtained through chemical recycling (chemical decomposition method), and PET obtained through mechanical recycling. Chemical recycling involves chemically breaking down collected used PET bottles and films, returning them to their raw material level and recomposing polyethylene terephthalate resin.Mechanical recycling, on the other hand, is a method that makes it possible to remove dirt from polyethylene terephthalate resin more reliably than with material recycling by carrying out alkaline washing more strictly than in the above-mentioned material recycling, or by vacuum drying at high temperatures. For example, after foreign matter is removed from used PET bottles, the bottles are crushed and washed, then pelletized using an extruder, crystallized in an environment at about 120 to 150°C, and then solid-phase polymerized in an environment at about 210°C under a nitrogen stream or high reduced pressure to obtain recycled PET. Bio-PET is PET produced by replacing the monoethylene glycol, a raw material of PET, with a bio-based raw material derived from sugar cane.
[0024] <<Polybutylene terephthalate resin>> The resin composition of the present embodiment also preferably contains a polybutylene terephthalate resin. By using a polybutylene terephthalate resin, the mold release resistance of the obtained molded article tends to be lower. The polybutylene terephthalate resin used in the resin composition of this embodiment is a polyester resin having a structure in which terephthalic acid units and 1,4-butanediol units are ester-bonded, and includes, in addition to polybutylene terephthalate resin (homopolymer), a polybutylene terephthalate copolymer containing other copolymerization components other than terephthalic acid units and 1,4-butanediol units, and a mixture of a homopolymer and a polybutylene terephthalate copolymer.
[0025] The polybutylene terephthalate resin may contain one or more types of dicarboxylic acid units other than terephthalic acid. Specific examples of other dicarboxylic acids include aromatic dicarboxylic acids such as isophthalic acid, orthophthalic acid, 1,5-naphthalenedicarboxylic acid, 2,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, biphenyl-2,2'-dicarboxylic acid, biphenyl-3,3'-dicarboxylic acid, biphenyl-4,4'-dicarboxylic acid, bis(4,4'-carboxyphenyl)methane, anthracenedicarboxylic acid, and 4,4'-diphenyletherdicarboxylic acid; alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid and 4,4'-dicyclohexyldicarboxylic acid; and aliphatic dicarboxylic acids such as adipic acid, sebacic acid, azelaic acid, and dimer acid. In the polybutylene terephthalate resin used in this embodiment, terephthalic acid units preferably account for 80 mol % or more of all dicarboxylic acid units, more preferably 90 mol % or more, even more preferably 95 mol % or more, and may even account for 99 mol % or more.
[0026] The diol unit may contain one or more other diol units in addition to 1,4-butanediol. Specific examples of other diol units include aliphatic or alicyclic diols having 2 to 20 carbon atoms, bisphenol derivatives, etc. Specific examples include ethylene glycol, propylene glycol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, decamethylene glycol, cyclohexanedimethanol, 4,4'-dicyclohexylhydroxymethane, 4,4'-dicyclohexylhydroxypropane, ethylene oxide adduct diol of bisphenol A, etc. In addition to the above-mentioned bifunctional monomers, a small amount of a trifunctional monomer such as trimellitic acid, trimesic acid, pyromellitic acid, pentaerythritol, trimethylolpropane, etc., can be used in combination to introduce a branched structure, or a monofunctional compound such as a fatty acid, etc., can be used in combination to adjust the molecular weight. In the polybutylene terephthalate resin used in this embodiment, 1,4-butanediol units preferably account for 80 mol % or more of all diol units, more preferably 90 mol % or more, even more preferably 95 mol % or more, and may even be 99 mol % or more.
[0027] In the polyethylene terephthalate resin used in the present embodiment, terephthalic acid units and 1,4-butanediol units preferably account for 90 mol % or more of all units excluding terminal groups, more preferably 95 mol % or more, even more preferably 98 mol % or more, and even more preferably 99 mol % or more. The polybutylene terephthalate resin may also be a polybutylene terephthalate copolymer containing, as the carboxylic acid unit, one or more dicarboxylic acids other than the terephthalic acid and / or, as the diol unit, one or more diols other than the 1,4-butanediol. When the polybutylene terephthalate resin is a polybutylene terephthalate resin modified by copolymerization, specific preferred copolymers include polyester ether resins copolymerized with polyalkylene glycols, particularly polytetramethylene glycol, dimer acid copolymerized polybutylene terephthalate resins, and isophthalic acid copolymerized polybutylene terephthalate resins. Among these, it is preferable to use polyester ether resins copolymerized with polytetramethylene glycol. In addition, when the polybutylene terephthalate resin is a copolymer, the copolymerization amount is 1 mol% or more and less than 50 mol% of all polybutylene terephthalate resin units. In particular, the copolymerization amount is preferably 2 mol% or more and less than 50 mol%, more preferably 3 to 40 mol%, and further preferably 5 to 20 mol%. By setting the copolymerization ratio in this manner, it is preferable because a molded product having a small mold shrinkage rate and high impact resistance can be obtained.
[0028] The amount of terminal carboxyl groups in the polybutylene terephthalate resin may be appropriately selected and determined, but is usually 60 eq / ton or less, preferably 50 eq / ton or less, and more preferably 30 eq / ton or less. By setting it to the above upper limit or less, the alkali resistance and hydrolysis resistance tend to be improved. The lower limit of the amount of terminal carboxyl groups is not particularly set, but considering the productivity of the production of the polybutylene terephthalate resin, it is preferably 5 eq / ton or more.
[0029] The amount of terminal carboxyl groups in the polybutylene terephthalate resin is a value measured by dissolving 0.5 g of the polybutylene terephthalate resin in 25 mL of benzyl alcohol and titrating it with a 0.01 mol / L benzyl alcohol solution of sodium hydroxide. The amount of terminal carboxyl groups can be adjusted by any conventionally known method, such as adjusting the polymerization conditions such as the raw material charge ratio during polymerization, the polymerization temperature, and the pressure reduction method, or by reacting a terminal blocking agent.
[0030] The intrinsic viscosity of the polybutylene terephthalate resin is preferably 0.5 dL / g or more, more preferably 0.6 dL / g or more. The intrinsic viscosity is preferably 2 dL / g or less, more preferably 1.5 dL / g or less, even more preferably 1.4 dL / g or less, even more preferably 1.3 dL / g or less, even more preferably 1.26 dL / g or less, and may be 1.0 dL / g or less, or 0.9 dL / g or less. By making the intrinsic viscosity equal to or less than the upper limit, moldability tends to be further improved. When the resin composition of the present embodiment contains two or more types of polybutylene terephthalate resins, the intrinsic viscosity is the intrinsic viscosity of the mixture. The intrinsic viscosity is measured as described in the Examples section below.
[0031] Polybutylene terephthalate resin can be produced by batch or continuous melt polymerization of a dicarboxylic acid component mainly composed of terephthalic acid or an ester derivative thereof and a diol component mainly composed of 1,4-butanediol. In addition, after producing a low molecular weight polybutylene terephthalate resin by melt polymerization, the degree of polymerization (or molecular weight) can be increased to a desired value by further solid-phase polymerization under a nitrogen gas flow or reduced pressure. The polybutylene terephthalate resin is preferably one obtained by a production method in which a dicarboxylic acid component mainly composed of terephthalic acid and a diol component mainly composed of 1,4-butanediol are melt-polycondensed in a continuous or batch manner.
[0032] The catalyst used in carrying out the esterification reaction may be a conventionally known catalyst, and examples thereof include titanium compounds, tin compounds, magnesium compounds, calcium compounds, etc. Among these, titanium compounds are particularly preferred. Specific examples of titanium compounds as esterification catalysts include titanium alcoholates such as tetramethyl titanate, tetraisopropyl titanate, and tetrabutyl titanate, and titanium phenolates such as tetraphenyl titanate.
[0033] In the polyester resin of the present embodiment, the polyethylene terephthalate resin preferably accounts for 95% by mass or more, more preferably 97% by mass or more, and even more preferably 99% by mass or more, of 100% by mass of the polyethylene resin. The upper limit may be 100% by mass of 100% by mass of the polyethylene resin. In addition, another example of the blend form in which the polyester resin of the present embodiment contains other polyester resins in addition to the polyethylene terephthalate resin is that it contains at least a polybutylene terephthalate resin in addition to the polyethylene terephthalate resin. The mass ratio of the polybutylene terephthalate resin in this blend form is preferably 0.1 mass% or more, more preferably 0.5 mass% or more, and even more preferably 1 mass% or more in 100 mass% of the polyester resin. By making it equal to or more than the lower limit, the mold release resistance of the obtained molded product tends to be small. The mass ratio of the polybutylene terephthalate resin in this blend form may be 90 mass% or less in 100 mass% of the polyester resin contained in the resin composition, or may be 50 mass% or less, 30 mass% or less, 10 mass% or less, 5 mass% or less, or 3 mass% or less depending on the application.
[0034] In this embodiment, the colorant (preferably carbon black) may be blended in the form of a masterbatch with a polyester resin. The polyester resin contained in the masterbatch is also included in the above-mentioned polyester resin. In particular, in this embodiment, it is preferable to blend carbon black in the form of a masterbatch with a polybutylene terephthalate resin.
[0035] The content of the polyester resin in the resin composition of the present embodiment is preferably 30% by mass or more, more preferably 40% by mass or more, even more preferably 50% by mass or more, even more preferably 60% by mass or more, and even more preferably 65% by mass or more, in 100% by mass of the resin composition. By making it equal to or more than the lower limit, the molding processability (releasability) is excellent, and the impact resistance and mechanical properties of the molded article obtained by molding the resin composition are better, which is preferable, and the molded article tends to have better releasability, so that the surface appearance tends to be further improved. In addition, the content of the polyester resin in the resin composition of the present embodiment is preferably 85% by mass or less, more preferably 80% by mass or less, and even more preferably 77% by mass or less, in 100% by mass of the resin composition. By making it equal to or less than the upper limit, the moist heat resistance tends to be further improved. The resin composition of the present embodiment may contain only one type of polyester resin, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0036] <Recycled carbon fiber> The resin composition of the present embodiment contains recycled carbon fibers. Here, recycled carbon fiber refers to carbon fiber recovered from scraps of used carbon fiber reinforced resin (aircraft, vehicles, electrical / electronic devices, etc.) or intermediate products (prepregs) of carbon fiber reinforced resin generated during the manufacturing process of carbon fiber reinforced resin. In contrast, virgin carbon fiber is new carbon fiber that is not recycled carbon fiber, such as that generally sold as carbon fiber. Recycled carbon fibers generally do not contain any surface treatment agents (including bundling agents) on the surface.
[0037] The type of carbon fiber is not particularly limited, but PAN-based carbon fiber is preferred.
[0038] The number average fiber length of the recycled carbon fibers is preferably 50 μm or more, more preferably 100 μm or more, and is preferably 1 mm or less, more preferably 500 μm or less, and even more preferably 300 μm or less. When the number average fiber length of the recycled carbon fibers is within such a range, a resin composition having improved mechanical properties is easily obtained. The number average fiber diameter of the recycled carbon fibers is preferably 3 μm or more, more preferably 4 μm or more, and is preferably 10 μm or less, more preferably 8 μm or less, and even more preferably 5 μm or less. When the number average fiber diameter of the recycled carbon fibers is within such a range, a resin composition having improved mechanical properties is more easily obtained. The number average fiber length and number average fiber diameter of recycled carbon fibers are determined by measuring the fiber length / fiber diameter of 100 random samples and excluding the upper 10% and lower 10% of the samples, and then averaging the measured values. Recycled carbon fiber typically has a circular cross section.
[0039] In this embodiment, the recycled carbon fiber preferably contains a resin (preferably epoxy resin)-derived residue at a ratio of 5% by mass or more, more preferably 8% by mass or more, even more preferably 10% by mass or more, and even more preferably 12% by mass or more. By making the ratio equal to or more than the lower limit, it is presumed that the residue functions as a bundling agent for the recycled carbon fiber, and the mechanical strength of the resulting molded product is further improved. In addition, the recycled carbon fiber preferably contains a resin (preferably epoxy resin)-derived residue at a ratio of 30% by mass or less, more preferably 25% by mass or less, even more preferably 22% by mass or less, even more preferably 19% by mass or less, even more preferably 16% by mass or less, and may be 14% by mass or less. By making the ratio equal to or less than the upper limit, it is easy to obtain the effect of improving productivity while minimizing the decrease in mechanical strength due to the resin residue.
[0040] The resin-derived residue may contain additives as necessary, such as a curing agent, a curing assistant, an internal mold release agent, a flame retardant, an antioxidant, a light stabilizer, an ultraviolet absorbing agent, and a colorant.
[0041] The recycled carbon fiber used in this embodiment is obtained by burning a composite of resin (preferably epoxy resin) and carbon fiber. The amount of residue derived from the resin (preferably epoxy resin) is achieved by burning in a continuous incinerator, burning under a nitrogen atmosphere, burning at a predetermined temperature, etc. For example, the description in International Publication No. 2018 / 212016 can be referred to, the contents of which are incorporated herein by reference.
[0042] The content of the recycled carbon fiber in the resin composition of the present embodiment is usually 5 parts by mass or more, preferably 10 parts by mass or more, more preferably 12 parts by mass or more, and may be 15 parts by mass or more, 18 parts by mass or more, 20 parts by mass or more, or 24 parts by mass or more, depending on the application, etc. By making it equal to or more than the lower limit, the strength of the obtained molded article tends to be further improved. In addition, the content of the recycled carbon fiber in the resin composition of the present embodiment is usually 70 parts by mass or less, preferably 60 parts by mass or less, more preferably 50 parts by mass or less, even more preferably 40 parts by mass or less, and even more preferably 35 parts by mass or less, relative to 100 parts by mass of the polyester resin. By making it equal to or less than the upper limit, it is easy to obtain a molded article with excellent fluidity and better appearance and smoothness.
[0043] Furthermore, the composition of this embodiment preferably contains recycled carbon fiber in an amount of 5 mass% or more, more preferably 10 mass% or more, and even more preferably 15 mass% or more, and preferably 40 mass% or less, more preferably 35 mass% or less, even more preferably 30 mass% or less, and even more preferably 25 mass% or less, calculated as the actual amount of carbon fiber in the composition. The resin composition of the present embodiment may contain only one type of recycled carbon fiber, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0044] The resin composition of this embodiment may or may not contain virgin carbon fiber. One example of the resin composition of this embodiment is an embodiment in which virgin carbon fiber is contained in a proportion of 5 to 50 mass % (preferably 5 to 30 mass %) of the content of recycled carbon fiber. Another example of the composition of this embodiment is an embodiment in which virgin carbon fiber is contained in an amount of less than 5 mass % (preferably less than 3 mass %, more preferably less than 1 mass %) of the content of recycled carbon fiber.
[0045] <Nucleating agent> The resin composition of the present embodiment may contain a nucleating agent. By containing a nucleating agent, the crystallization speed of the resin composition can be adjusted. The type of nucleating agent is not particularly limited, but may be an inorganic nucleating agent or an organic nucleating agent, and an inorganic nucleating agent is more preferable. Examples of inorganic nucleating agents include talc, boron nitride, mica, kaolin, barium sulfate, sodium phosphate, silicon nitride, and molybdenum disulfide. Among these, talc, barium sulfate, sodium phosphate, and boron nitride are preferred, and talc is more preferred because it tends to increase the rigidity of the resin composition.
[0046] As the organic nucleating agent, an organic alkali metal salt is preferable, an alkali metal salt of an aromatic carboxylic acid or a fatty acid is more preferable, and an alkali metal salt of a fatty acid (preferably a fatty acid having 5 to 50 carbon atoms) (preferably a sodium salt or a potassium salt, more preferably a sodium salt) is further preferable. Specific examples of the organic nucleating agent include ionomer, sodium benzoate, sodium palmitate, sodium stearate, sodium behenate, and sodium montanate, among which sodium stearate, sodium behenate, and sodium montanate are more preferable, and sodium montanate is even more preferable because the resin composition tends to have a good balance between rigidity and toughness.
[0047] When the resin composition of the present embodiment contains a nucleating agent, the content is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.1 parts by mass or more, relative to 100 parts by mass of polyester resin. Depending on the application, for example, in applications where releasability is particularly required, it is more preferable to be 0.15 parts by mass or more, and it may be 0.2 parts by mass or more, 1 part by mass or more, 2 parts by mass or more, 2.5 parts by mass or more, 3 parts by mass or more, or 3.5 parts by mass or more. By making it equal to or more than the lower limit, the releasability and mechanical strength of the molded product tend to be improved. In addition, the upper limit of the content of the nucleating agent is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, even more preferably 6 parts by mass or less, and even more preferably 5 parts by mass or less, relative to 100 parts by mass of polyester resin. By making it equal to or less than the upper limit, decomposition of the resin is suppressed, and mechanical strength tends to be improved. The resin composition of the present embodiment may contain only one type of nucleating agent, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0048] <Coloring agent> The resin composition of the present embodiment may contain a colorant. The colorant may be a pigment or a dye, but is preferably a pigment. An example of a colorant that can be used in this embodiment is carbon black. Details of carbon black can be found in paragraph 0021 of JP 2011-57977 A, the contents of which are incorporated herein. In addition, when a colorant such as carbon black is blended into the resin composition of this embodiment, it is preferable to form a master batch and then knead it with a polyester resin or the like. For the master batch, it is preferable to use a polyester resin, and it is more preferable to use a polybutylene terephthalate resin. By using a polybutylene terephthalate resin, the crystallization of the resin composition is more effectively promoted. In particular, when a polybutylene terephthalate resin is present in the vicinity of a colorant such as carbon black, the crystallization promotion effect is more effectively exhibited. The proportion of the colorant in the master batch is preferably 5% by mass or more, more preferably 10% by mass or more, and is preferably 50% by mass or less, more preferably 40% by mass or less. When the resin composition of this embodiment contains a colorant (preferably carbon black), the content thereof is preferably 0.01 part by mass or more, more preferably 0.1 part by mass or more, and preferably 1 part by mass or less, more preferably 0.8 part by mass or less, and even more preferably 0.6 part by mass, relative to 100 parts by mass of the polyester resin. The resin composition of the present embodiment may contain only one type of colorant, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0049] <Other ingredients> The resin composition of the present embodiment may contain other components in addition to the above-mentioned components as necessary, as long as the desired physical properties are not significantly impaired. Examples of other components include various resin additives. The other components may be contained in one type, or in any combination and ratio of two or more types. Specific examples of the additives include reactive compounds, stabilizers, release agents, ultraviolet absorbers, antistatic agents, antifogging agents, antiblocking agents, flow improvers, plasticizers, dispersants, antibacterial agents, etc. The resin composition of the present embodiment preferably contains at least one of the reactive compounds, stabilizers, and release agents. The resin composition of this embodiment is adjusted so that the total of the polyester resin, the recycled carbon fiber, and the other components that are selectively blended is 100% by mass. In the resin composition of this embodiment, the total of the polyester resin and the recycled carbon fiber preferably accounts for 90% by mass or more of the resin composition, and more preferably accounts for 93% by mass or more. In addition, in the resin composition of this embodiment, the total of the polyester resin, the recycled carbon fiber, the reactive compound, the nucleating agent, the stabilizer, the colorant, and the release agent preferably accounts for 99% by mass or more of the resin composition.
[0050] <<Reactive compounds>> The resin composition of the present embodiment may contain a reactive compound. The reactive compound is preferably at least one selected from the group consisting of a carbodiimide compound, an epoxy compound, a compound having an oxazoline group (ring), a compound having an oxazine group (ring), a compound having a carboxylic acid, and a compound having an amide group, and is particularly preferably an epoxy compound, since it tends to improve hydrolysis resistance and suppress outgassing. The epoxy compound may be a monofunctional epoxy compound or a polyfunctional epoxy compound, with the polyfunctional epoxy compound being preferred. Specific examples of polyfunctional epoxy compounds include bisphenol A type epoxy compounds (including bisphenol A diglycidyl ether), bisphenol F type epoxy compounds (including bisphenol F diglycidyl ether), biphenyl type epoxy compounds (including bis(glycidyloxy)biphenyl), resorcin type epoxy compounds (including resorcinol diglycidyl ether), novolac type epoxy compounds, epoxy compounds having an aromatic ring such as benzoic acid glycidyl ester, terephthalic acid diglycidyl ester, orthophthalic acid diglycidyl ester, methyl glycidyl ether, butyl glycidyl ether, 2-ethylhexyl glycidyl ether, decyl glycidyl ether, stearyl glycidyl ether, (di)glycidyl ethers such as glycidyl ether, phenyl glycidyl ether, butylphenyl glycidyl ether, allyl glycidyl ether, neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, glycerin diglycidyl ether, and propylene glycol diglycidyl ether; paraffin-based (e.g., saturated fatty acid-based) or olefin-based (e.g., unsaturated fatty acid-based) (di)glycidyl esters such as sorbic acid glycidyl ester, adipic acid diglycidyl ester, epoxidized linseed oil, and epoxidized soybean oil; alicyclic epoxy compounds such as vinylcyclohexene dioxide and dicyclopentadiene oxide; and epoxy-modified styrene-acrylic copolymers. Among these, styrene-acrylic copolymers containing a glycidyl group in the side chain, bisphenol A type epoxy compounds, novolac type epoxy compounds, bisphenol F type epoxy compounds, and biphenyl type epoxy compounds are preferred.
[0051] In addition to the above, the reactive compounds can be found in paragraphs 0038 to 0050 of JP-A-2020-199755 and paragraph 0043 of JP-A-2020-125468, the contents of which are incorporated herein by reference. Commercially available epoxy compounds include "EP-17" (manufactured by ADEKA), "Joncryl ADR4368C" (manufactured by BASF), Epikote 1003 (manufactured by Mitsubishi Chemical Corporation), and YDCN-704 (manufactured by Nippon Steel Chemical & Material Co., Ltd.).
[0052] The epoxy compound preferably has a weight average molecular weight of 15000 or less, more preferably 10000 or less. There is no particular lower limit, but the weight average molecular weight is preferably 100 or more, more preferably 500 or more. By setting the weight average molecular weight within such a range, the effect of the present embodiment tends to be more effectively exhibited.
[0053] The epoxy compound preferably has an epoxy equivalent of 100 g / eq or more, more preferably 150 g / eq or more, and more preferably 150 g / eq or more. The epoxy compound preferably has an epoxy equivalent of 1500 g / eq or less, more preferably 900 g / eq or less, and even more preferably 800 g / eq or less. By setting the epoxy equivalent to be equal to or more than the above lower limit, the adhesiveness to other members tends to be higher, whereas by setting the epoxy equivalent to be equal to or less than the above upper limit, the fluidity tends to be high and the resin composition tends to be easily molded.
[0054] When the resin composition of the present embodiment contains a reactive compound, the content is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, even more preferably 0.1 parts by mass or more, and even more preferably 0.4 parts by mass or more, relative to 100 parts by mass of polyester resin. By containing the lower limit or more, it is preferable because there is a tendency to improve hydrolysis resistance. In addition, the upper limit of the content of the reactive compound is preferably 15 parts by mass or less, more preferably 10 parts by mass or less, even more preferably 7 parts by mass or less, even more preferably 2 parts by mass or less, and particularly preferably 1 part by mass or less, relative to 100 parts by mass of polyester resin. By containing the upper limit or less, it is preferable because there is a tendency to suppress thickening and improve moldability. The resin composition of the present embodiment may contain only one type of reactive compound, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0055] <<Stabilizer>> The resin composition of the present embodiment may contain a stabilizer. Examples of the stabilizer include hindered phenol compounds, hindered amine compounds, phosphorus compounds, and sulfur stabilizers. Among these, hindered phenol compounds are preferred. As the stabilizer, specifically, the description in paragraphs 0046 to 0057 of JP 2018-070722 A, the description in paragraphs 0030 to 0037 of JP 2019-056035 A, and the description in paragraphs 0066 to 0078 of WO 2017 / 038949 A can be referred to, the contents of which are incorporated herein by reference.
[0056] The resin composition of the present embodiment preferably contains 0.01 parts by mass or more of the stabilizer relative to 100 parts by mass of the polyester resin, more preferably 0.05 parts by mass or more, and even more preferably 0.1 parts by mass or more. The upper limit of the content of the stabilizer is preferably 3 parts by mass or less, more preferably 1 part by mass or less, and even more preferably 0.5 parts by mass or less relative to 100 parts by mass of the polyester resin. The resin composition of the present embodiment may contain only one type of stabilizer, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0057] <<Release agent>> The resin composition of the present embodiment preferably contains a release agent. As the release agent, a wide variety of known release agents can be used. Examples of the release agent include aliphatic carboxylic acid amides, aliphatic carboxylic acids, esters of aliphatic carboxylic acids and alcohols, aliphatic hydrocarbon compounds having a number average molecular weight of 200 to 15,000, and polysiloxane-based silicone oils.
[0058] Examples of the aliphatic carboxylic acid amide include compounds obtained by a dehydration reaction between a higher aliphatic monocarboxylic acid and / or a polybasic acid and a diamine. As the higher aliphatic monocarboxylic acid, saturated aliphatic monocarboxylic acids and hydroxycarboxylic acids having 16 or more carbon atoms are preferred, and examples thereof include palmitic acid, stearic acid, behenic acid, montanic acid, and 12-hydroxystearic acid. Examples of polybasic acids include aliphatic dicarboxylic acids such as malonic acid, succinic acid, adipic acid, sebacic acid, pimelic acid, and azelaic acid; aromatic dicarboxylic acids such as phthalic acid and terephthalic acid; and alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid and cyclohexylsuccinic acid. Examples of diamines include ethylenediamine, 1,3-diaminopropane, 1,4-diaminobutane, hexamethylenediamine, metaxylylenediamine, tolylenediamine, paraxylylenediamine, phenylenediamine, and isophoronediamine. As the carboxylic acid amide compound, a compound obtained by polycondensation of stearic acid, sebacic acid, and ethylenediamine is preferred, and a compound obtained by polycondensation of 2 moles of stearic acid, 1 mole of sebacic acid, and 2 moles of ethylenediamine is more preferred. In addition to bisamide compounds obtained by reacting diamines and aliphatic carboxylic acids, such as N,N'-methylenebisstearamide and N,N'-ethylenebisstearamide, dicarboxylic acid amide compounds, such as N,N'-dioctadecylterephthalamide, can also be suitably used.
[0059] Examples of the aliphatic carboxylic acid include saturated or unsaturated aliphatic mono-, di- or tri-carboxylic acids. Here, the aliphatic carboxylic acid also includes alicyclic carboxylic acids. Among these, preferred aliphatic carboxylic acids are mono- or di-carboxylic acids having 6 to 36 carbon atoms, and more preferred are saturated aliphatic mono-carboxylic acids having 6 to 36 carbon atoms. Specific examples of such aliphatic carboxylic acids include palmitic acid, stearic acid, caproic acid, capric acid, lauric acid, arachic acid, behenic acid, lignoceric acid, cerotic acid, melissic acid, tetralinic acid, montanic acid, adipic acid, and azelaic acid.
[0060] In the ester of an aliphatic carboxylic acid and an alcohol, the aliphatic carboxylic acid may be the same as the aliphatic carboxylic acid. On the other hand, the alcohol may be, for example, a saturated or unsaturated monohydric or polyhydric alcohol. These alcohols may have a substituent such as a fluorine atom or an aryl group. Among these, a monohydric or polyhydric saturated alcohol having 30 or less carbon atoms is preferred, and an aliphatic or alicyclic saturated monohydric alcohol or an aliphatic saturated polyhydric alcohol having 30 or less carbon atoms is more preferred. Specific examples of such alcohols include octanol, decanol, dodecanol, stearyl alcohol, behenyl alcohol, ethylene glycol, diethylene glycol, glycerin, pentaerythritol, 2,2-dihydroxyperfluoropropanol, neopentylene glycol, ditrimethylolpropane, and dipentaerythritol. Specific examples of esters of aliphatic carboxylic acids and alcohols include beeswax (a mixture mainly composed of myricyl palmitate), stearyl stearate, behenyl behenate, stearyl behenate, glycerin monopalmitate, glycerin monostearate, glycerin distearate, glycerin tristearate, pentaerythritol monopalmitate, pentaerythritol monostearate, pentaerythritol distearate, pentaerythritol tristearate, pentaerythritol tetrastearate, and esters of montanic acid and polyfunctional alcohols.
[0061] Examples of the aliphatic hydrocarbons having a number average molecular weight of 200 to 15,000 include liquid paraffin, paraffin wax, microwax, polyethylene wax, Fischer-Tropsch wax, and α-olefin oligomers having 3 to 12 carbon atoms. The aliphatic hydrocarbons herein also include alicyclic hydrocarbons. The number average molecular weight of the aliphatic hydrocarbons is preferably 5,000 or less.
[0062] As for the release agent, in addition to the above, the descriptions in paragraphs 0063 to 0077 of JP 2018-070722 A and the descriptions in paragraphs 0090 to 0098 of JP 2019-123809 A can be referred to, the contents of which are incorporated herein by reference.
[0063] The resin composition of the present embodiment preferably contains 0.01 parts by mass or more of the release agent relative to 100 parts by mass of the polyester resin, more preferably 0.1 parts by mass or more, and even more preferably 0.3 parts by mass or more. The upper limit of the content of the release agent is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, even more preferably 1 part by mass or less, and even more preferably 0.8 parts by mass or less relative to 100 parts by mass of the polyester resin. The resin composition may contain only one type of release agent, or may contain two or more types. When two or more types are contained, the total amount is preferably within the above range.
[0064] <Physical properties of resin composition> The resin composition of the present embodiment preferably has excellent impact resistance. Specifically, the resin composition is molded into a JIS K7139 multipurpose test piece (4 mm thick) and the unnotched Charpy impact strength measured based on the JIS K7111-1 standard is 35 kJ / m 2 It is preferable that the concentration is 38 kJ / m or more. 2 The upper limit of the unnotched Charpy impact strength is not particularly limited, but is preferably 100 kJ / m 2 The following is practical. The resin composition of the present embodiment preferably has a small shrinkage rate. Specifically, the resin composition is molded at a cylinder temperature of 260°C and a mold temperature of 120°C to a length of 100 mm, a width of 100 mm, and a thickness of 2.0 mm, and then conditioned for 24 hours under an environment of 23°C and a humidity of 50% RH. The TD shrinkage rate is preferably 0.72% or less, and more preferably 0.71% or less. The lower limit of the TD shrinkage rate is preferably 0%, but even if it is 0.01% or more, the required performance is sufficiently satisfied. The resin composition of the present embodiment is preferably excellent in releasability. Specifically, the resin composition is molded into a box-shaped molded product having a thickness of 1.5 mmt and outer dimensions of 30×50×15 mm depth under the conditions of a cylinder temperature of 280° C., a mold temperature of 80° C., and a cooling time of 30 seconds, and the maximum release resistance value when the product is released by ejection of an ejector pin is preferably 30 MPa or less, more preferably 25 MPa or less, and even more preferably 19 MPa or less. The lower limit of the maximum release resistance value is preferably 0 MPa, but even if it is 1 MPa or more, the required performance is sufficiently satisfied. The unnotched Charpy impact strength, shrinkage rate, and maximum demolding resistance are measured in accordance with the details described in the Examples section below.
[0065] <Method of producing resin composition> The resin composition of this embodiment can be produced by a conventional method for producing a resin composition containing a polyester resin. For example, the resin composition of this embodiment is produced by a method including feeding a polyester resin containing a polyethylene terephthalate resin, recycled carbon fiber, and other components blended as necessary into an extruder and melt-kneading. The recycled carbon fiber may be side-fed into the extruder. In addition, when the resin composition contains a colorant, it may be blended as a master batch premixed with a thermoplastic resin and melt-kneaded. More specifically, the method for producing a resin composition of the present embodiment is a method for producing a resin composition comprising a polyester resin containing a polyethylene terephthalate resin and recycled carbon fiber, the polyethylene terephthalate resin containing an iron element at a ratio of 1.0 to 100 μg / g, and further containing carbon black at a ratio of 0.01 to 1 part by mass per 100 parts by mass of the polyester resin, and preferably includes blending the carbon black as a master batch in which the carbon black is premixed with the polyester resin, and melt-kneading the blend. Furthermore, it is preferable that the polyester resin used in the master batch contains a polybutylene terephthalate resin. By forming the master batch with the polybutylene terephthalate resin, the mold release resistance of the obtained molded product can be further reduced. The heating temperature during melt kneading can usually be appropriately selected from the range of 220 to 350°C.
[0066] <Application> An example of the resin composition of this embodiment is a pellet. The molded article of the present embodiment is formed from the resin composition of the present embodiment or the pellets of the present embodiment. The molded article of the present embodiment is preferably used for various applications, such as various storage containers, electric and electronic equipment parts, office automation (OA) equipment parts, home appliance parts, machine mechanism parts, vehicle mechanism parts, on-board housing parts, vehicle parts (interior and exterior of automobiles), building materials, various containers, leisure goods and miscellaneous goods, lighting equipment, etc. Among them, it is preferably used for on-board housing parts and vehicle parts (interior and exterior of automobiles), such as door mirrors and wiper parts. Moreover, the molded product of this embodiment is suitable for injection molding. EXAMPLES
[0067] The present invention will be described in more detail below with reference to examples. The materials, amounts, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below. If the measuring instruments used in the examples are difficult to obtain due to discontinuation or the like, measurements can be made using other instruments with equivalent performance.
[0068] 1.Raw materials The following raw materials were used:
[0069] [Table 1]
[0070] <Measurement of intrinsic viscosity> Resin pellets were dissolved in a mixed solvent of phenol / 1,1,2,2-tetrachloroethane (mass ratio 1 / 1) by stirring at 110°C for 1 hour to a concentration of 1.00 g / dL. The solution was then cooled to 30°C. The time it took for the sample solution and the solvent alone to fall at 30°C was measured using a fully automatic solution viscometer, and the intrinsic viscosity was calculated using the following formula (A). Intrinsic viscosity=((1+4K H η sp ) 0.5 -1) / (2K H C) …(A) Here, η sp = η / η0-1, where η is the time it takes for the sample solution to fall, η0 is the time it takes for the solvent alone to fall, C is the concentration of the sample solution (g / dL), and K H is Huggins' constant. K H was set to 0.33. The fully automatic solution viscometer used was a product of Shibayama Scientific Co., Ltd.
[0071] <Amount of iron in polyester resin> Qualitative / semi-quantitative analysis (μg / g) of iron element in polyester resin was performed by ICP emission spectrometry. As a pretreatment, 200 mg of sample was weighed out, Kjeldahl wet digestion (sulfuric acid / nitric acid, sulfuric acid / hydrogen peroxide) was performed, and the volume was adjusted to 50 mL. Then, ICP emission spectrometry was performed by acid concentration matching single point calibration method. ICP emission spectrometry was performed by axial / radial photometry using Thrmo Fisher Scientific's "iCAP7600Duo".
[0072] <Amount of residue> The residue of the recycled carbon fiber in Table 1 indicates the amount of char in the recycled carbon fiber. That is, since the recycled carbon fiber used in this embodiment is a fired product of a composite of resin (e.g., epoxy resin) and carbon fiber, the recycled carbon fiber contains a residue (char) derived from the resin (e.g., epoxy resin). The amount of the resin residue is a value calculated from the carbon fiber content of the carbon fiber mass contained in the carbon fiber reinforced resin before the heat treatment, using formula (X). The unit is % by mass. [B - (A × C) / (B)] × 100 formula (X) A: Mass of carbon fiber reinforced resin before heat treatment B: Mass of heat treatment product C: Carbon fiber content of carbon fiber reinforced resin before heat treatment (ratio, for example, 0.9 for 90% by mass)
[0073] 2. Comparative Example 1, Examples 1 to 4 <Production of Resin Composition (Pellets)> The components shown in Table 1 were fed from the main feed port of the twin-screw extruder in the proportions (parts by mass) shown in Table 2, except for the recycled carbon fiber. The cylinder temperature setting in the first kneading section was set to 265-275°C, and the recycled carbon fiber was fed from a side feeder. The resin composition was melt-kneaded under the conditions of a cylinder temperature setting of 265-285°C after the addition of the recycled carbon fiber and a screw rotation speed of 300-350 rpm. The product was quenched in a water tank and pelletized using a pelletizer to obtain pellets of the resin composition.
[0074] <Unnotched Charpy impact strength> The resin composition pellets obtained above were dried at 120°C for 5 hours, and then injection molded into JIS K7139 multipurpose test pieces (4 mm thick) using an injection molding machine (Japan Steel Works, Ltd., "J-85AD-60H") under conditions of a cylinder temperature of 280°C and a mold temperature of 120°C. Using the above multipurpose test piece (4 mm thick), the unnotched Charpy impact strength (unit: KJ / m 2 ) was measured.
[0075] <Shrinkage rate> The pellets obtained above were dried at 120°C for 5 hours, and then molded into molded products (length 100 mm, width 100 mm, thickness 2.0 mm) using a Nissei Plastic Industrial Co., Ltd. "NEX80-9E" injection molding machine at a cylinder temperature of 280°C and a mold temperature of 120°C. The obtained test pieces were conditioned for 24 hours or more in an environment of 23°C and 50% RH. Then, using the obtained test pieces, the dimensions in the MD (machine direction, also called the flow direction) and TD (transverse direction, also called the perpendicular direction) directions were measured, and the shrinkage rate (unit: %) was calculated based on the dimensions of the mold.
[0076] <Mold release resistance> The pellets obtained above were dried at 120°C for 5 hours, and then a box-shaped molded product with a thickness of 1.5 mmt and external dimensions of 30 x 50 x 15 mm depth was molded using an injection molding machine manufactured by Japan Steel Works (mold clamping force 50T) under conditions of a cylinder temperature of 280°C, a mold temperature of 80°C, and a cooling time of 30 seconds. The maximum mold release resistance value (unit: MPa) when the product was released from the mold by protruding an ejector pin was evaluated as the mold release resistance. For the measurements, a mold-in-mold pressure measurement system called "Mold Margering System (registered trademark)" was used, which uses an ejector pin-shaped pressure sensor "EP Sensor (registered trademark)" with a built-in pressure sensing element manufactured by Futaba Corporation.
[0077] [Table 2]
[0078] As is clear from the above results, the molded articles formed from the resin composition of the present invention had low demolding resistance (Examples 1 to 4). In particular, by blending carbon black and blending the carbon black as a master batch with polybutylene terephthalate resin, remarkably excellent demolding properties were achieved (Examples 2 and 4). Furthermore, the molded article formed from the resin composition of the present invention also had a low shrinkage rate, and in particular, the TD shrinkage rate was reduced. Furthermore, the molded article formed from the resin composition of the present invention also had high mechanical strength. In contrast, when a virgin polyester resin with a low iron content was used, the resulting molded article had high demolding resistance, a high shrinkage rate, and also low mechanical strength (Comparative Example 1).
Claims
1. A resin composition comprising a polyester resin containing a polyethylene terephthalate resin and recycled carbon fibers, wherein the polyethylene terephthalate resin contains iron elements in a ratio of 1.0 to 100 μg / g.
2. The resin composition according to claim 1, wherein the content of the recycled carbon fiber is 5 to 70 parts by mass per 100 parts by mass of the polyester resin.
3. 3. The resin composition according to claim 1, wherein the polyethylene terephthalate resin contains units derived from isophthalic acid, and the units derived from isophthalic acid are 0.5 mol% or more and 15 mol% or less of all units derived from dicarboxylic acid components contained in the polyethylene terephthalate resin.
4. The resin composition according to claim 1 or 2, wherein the polyethylene terephthalate resin comprises a recycled product.
5. The resin composition according to claim 1 or 2, further comprising a nucleating agent in an amount of 0.01 to 10 parts by mass per 100 parts by mass of the polyester resin.
6. The resin composition according to claim 1 or 2, further comprising 0.01 to 1 part by mass of carbon black per 100 parts by mass of the polyester resin.
7. The resin composition of claim 6 , wherein the polyester resin further comprises a polybutylene terephthalate resin.
8. The content of recycled carbon fiber is 5 to 70 parts by mass per 100 parts by mass of polyester resin, the polyethylene terephthalate resin contains units derived from isophthalic acid, and the units derived from isophthalic acid account for 0.5 mol % or more and 15 mol % or less of all units derived from a dicarboxylic acid component contained in the polyethylene terephthalate resin; Polyethylene terephthalate resin contains recycled materials. Further, the composition contains a nucleating agent in an amount of 0.01 to 10 parts by mass per 100 parts by mass of the polyester resin, Further, the polyester resin contains carbon black in an amount of 0.01 to 1 part by mass per 100 parts by mass of the polyester resin. The resin composition according to claim 1.
9. The resin composition of claim 8 , wherein the polyester resin further comprises a polybutylene terephthalate resin.
10. A pellet of the resin composition according to claim 1, 2, 8 or 9.
11. A molded article formed from the resin composition according to claim 1, 2, 8 or 9.
12. A method for producing a resin composition comprising a polyester resin containing a polyethylene terephthalate resin and recycled carbon fibers, the polyethylene terephthalate resin containing an iron element in a ratio of 1.0 to 100 μg / g, and further containing carbon black in a ratio of 0.01 to 1 part by mass per 100 parts by mass of the polyester resin, A method for producing a resin composition, comprising blending carbon black as a master batch premixed with a polyester resin, and melt-kneading the resulting mixture.
13. The method for producing a resin composition according to claim 12, wherein the polyester resin used in the master batch contains a polybutylene terephthalate resin.
14. The method for producing a resin composition according to claim 12 or 13, wherein the resin composition is the resin composition according to claim 1, 2, 8 or 9.
Citation Information
Patent Citations
Taimamoseiseikeizairyono seizohoho
JP1976109056A
Carbon fiber-reinforced polyester resin, and method for manufacturing injection molded object thereof
JP2016041800A
Methods for producing regenerated carbon fiber bundles, regenerated carbon fibers and regenerated milled carbon fibers, apparatus for producing regenerated carbon fiber bundles, method for producing carbon fiber-reinforced resin, and regenerated carbon fiber bundles
WO2018212016A1